Binder for secondary battery, separator, secondary battery, and electrical apparatus
By using an annular structure acrylic copolymer adhesive to increase the contact area between the pole piece and the separator, the problem of battery cell openings is solved, and the battery performance and cycle life are improved.
Patent Information
- Application Number
- PCT/CN2023/099995
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2023-06-13
- Publication Date
- 2024-10-31
AI Technical Summary
There is an opening problem in the battery cell, and a gap is easily formed between the pole piece and the separator, resulting in poor battery cycle performance.
An acrylic copolymer with a ring structure is used as the adhesive. Its hollow through-hole structure increases the contact area with the pole piece and separator, improves the bonding performance, and reduces the amount of adhesive used.
The hardness of the battery core and the cycle performance of the large clamp are improved, the cycle life of the battery is extended, the internal resistance and polarization loss are reduced, and the utilization rate of the secondary battery is enhanced.
Smart Images

Figure CN2023099995_31102024_PF_FP_ABST
Abstract
Description
Binder for secondary battery, separator, secondary battery and electrical device
[0001] Related applications
[0002] This application claims priority to Chinese patent application No. 202310447240.5 filed on April 24, 2023, the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The present application relates to the technical field of secondary batteries, and in particular to a binder for secondary batteries, a separator, a secondary battery, and an electrical device. Background Art
[0004] With the rapid growth of portable electronic devices and electric vehicles, the demand for power batteries is also growing. Among them, the electrochemical performance of batteries is also attracting more and more attention.
[0005] At present, there is an opening problem in battery cells, that is, a gap is easily formed between the electrode and the diaphragm, resulting in poor battery cycle performance.
[0006] Summary of the Invention
[0007] The main purpose of this application is to provide a binder for secondary batteries, which aims to improve the adhesion between the electrode and the separator through the binder, thereby improving the battery performance.
[0008] To achieve the above-mentioned purpose, the present application provides a binder for a secondary battery, wherein the binder includes an acrylic copolymer and has a ring shape.
[0009] Acrylate copolymers have good adhesion, and the use of acrylic copolymers can improve the adhesion between the diaphragm and the electrode.
[0010] The adhesive with an annular structure has a bonding site with a larger area. For example, when the adhesive with an annular structure contacts the electrode, the contact point is the ring line of the annular adhesive, while the contact site of the spherical adhesive is point contact. For annular structures and spherical adhesives of the same size, the adhesive with an annular structure has better bonding performance; and the adhesive with an annular structure has a hollow through hole. For annular structures and spherical adhesives of the same size, the adhesive with an annular structure has a smaller mass. In this way, better bonding performance can be achieved while reducing the amount of adhesive used in the annular structure.
[0011] Optionally, the specific surface area of the binder is in the range of 0.4 m 2 / g to 1.2m 2 / g, preferably, the specific surface area of the binder is in the range of 0.6m 2 / g to 0.9m 2 / g.
[0012] Specific surface area refers to the total area per unit mass of a material. The ring-shaped binder has a hollow through-hole. Compared with the spherical structure binder of the same size, the ring-shaped binder has a larger specific surface area. The range of the specific surface area of the binder is 0.4m 2 / g to 1.2m 2 / g, preferably, the specific surface area of the binder is in the range of 0.6m 2 / g to 0.9m 2 / g, which is beneficial to improving the contact between the annular adhesive and the diaphragm and electrode, and improving the bonding performance.
[0013] Optionally, the ratio of the surface area to volume of the binder is 0.1×10 6 m -1 to 20×10 6 m -1 Preferably, the ratio of the surface area to volume of the binder is 0.5×10 6 m -1 to 16×10 6 m -1 .
[0014] The ratio of surface area to volume is the ratio of the total area of the material to the total volume of the material. The ring-shaped adhesive has a hollow through hole. Compared with the spherical structure adhesive of the same size, the surface area to volume ratio of the ring-shaped adhesive is larger. The surface area to volume ratio of the adhesive is 0.1×10 6 m -1 to 20×10 6 m -1 Preferably, the ratio of the surface area to volume of the binder is 0.5×10 6 m -1 to 16×10 6 m -1 This shows that the annular adhesive has a higher surface area than the spherical adhesive, which is beneficial to improving the contact between the annular adhesive and the diaphragm and electrode, and improving the bonding performance.
[0015] Optionally, the bulk density of the binder is in the range of 0.3 g / cm 3 to 0.8g / cm 3 Preferably, the bulk density of the binder is in the range of 0.4 g / cm 3 to 0.7g / cm 3 .
[0016] Bulk density is the mass per unit volume measured when powder is freely filled in a container. Ring-shaped binders have hollow through-holes. When a ring-shaped binder is filled in a container, the through-holes form gaps, resulting in a lower bulk density than when a spherical binder of the same size is filled. The bulk density range of the binder is 0.3 g / cm 3 to 0.8g / cm 3 Preferably, the bulk density of the binder is in the range of 0.4 g / cm 3 to 0.7g / cm 3 This shows that under certain conditions, reducing the mass of the ring adhesive can also improve the bonding performance of the adhesive.
[0017] Optionally, the shape of the adhesive includes a ring shape.
[0018] According to experimental experience and the surface tension of materials, a ring shape is easier to achieve.
[0019] Optionally, the volume particle size distribution Dv50 of the binder is in the range of 1 μm to 15 μm. Preferably, the volume particle size distribution Dv50 of the binder is in the range of 3 μm to 12 μm.
[0020] In order to improve the adhesion of the adhesive and improve the gap between the diaphragm and the pole piece, the volume particle size distribution Dv50 of the adhesive ranges from 1 μm to 15 μm. Preferably, the volume particle size distribution Dv50 of the adhesive ranges from 3 μm to 12 μm.
[0021] Optionally, the monomers constituting the acrylic ester copolymer include a first polymerizable monomer, and the structure of the first polymerizable monomer includes:
[0022] Wherein, R1 includes hydrogen or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.
[0023] The first polymerized monomer structure contains an ester group, which can improve the compatibility of the acrylic copolymer with the electrolyte, enhance the ion conductivity, and improve the anti-swelling ability of the acrylic copolymer. In addition, as a flexible monomer segment in the molecular chain segment, it can adjust the glass transition temperature of the acrylic copolymer, improve the toughness of the adhesive during application, and help to exert a good bonding effect.
[0024] Optionally, the first polymerizable monomer includes one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.
[0025] Theoretically, this application does not limit the type of the first polymerized monomer. The first polymerized monomer satisfies the above structure, that is, the first polymerized monomer includes the above-listed substances and substances not listed in this application.
[0026] By using any one or more of the above-mentioned first polymerizable monomers, the glass transition temperature of the acrylic ester copolymer can be adjusted, and the anti-swelling ability of the acrylic ester copolymer can be improved.
[0027] Optionally, the monomers constituting the acrylic ester copolymer include a second polymerizable monomer, and the structure of the second polymerizable monomer includes:
[0028] Wherein, R3 includes hydrogen or an alkyl group of 1 to 6 carbon atoms.
[0029] The structure of the second polymerized monomer contains carboxyl groups, which have the characteristics of strong polarity and can improve the adhesion and flexibility of the adhesive. For example, the carboxyl groups can form a binding force with the functional groups on the electrode and the diaphragm material to improve the bonding effect.
[0030] Optionally, the second polymerizable monomer includes one or more of acrylic acid, methacrylic acid, crotonic acid, and heptenoic acid.
[0031] Theoretically, this application does not limit the type of the second polymerized monomer. The second polymerized monomer satisfies the above structure, that is, the second polymerized monomer includes the above-listed substances and substances not listed in this application.
[0032] The use of any one or more of the above-mentioned second polymerizable monomers can improve the bonding properties of the acrylic copolymer.
[0033] Optionally, the monomers constituting the acrylic ester copolymer include a third polymerizable monomer, and the structure of the third polymerizable monomer includes:
[0034] Wherein, R4 includes a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0035] The structure of the third polymer monomer contains an unsaturated nitrile group. The highly polar cyano group helps to improve the ionic conductivity and also has the effects of anti-swelling and high adhesion.
[0036] Optionally, the third polymerizable monomer includes one or more of acrylonitrile and methacrylonitrile.
[0037] Theoretically, this application does not limit the type of the third polymerized monomer. The third polymerized monomer satisfies the above structure, that is, the third polymerized monomer includes the above-listed substances and substances not listed in this application.
[0038] The use of any one or more third polymerizable monomers mentioned above can improve the ionic conductivity of the acrylic ester copolymer and enhance its adhesiveness.
[0039] Optionally, the monomers constituting the acrylic ester copolymer include a fourth polymerizable monomer, and the structure of the fourth polymerizable monomer includes:
[0040] Wherein, R5 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R6 includes a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.
[0041] The structure of the fourth polymerizable monomer contains an unsaturated amide group, which plays a role in improving swelling and enhancing adhesion.
[0042] Optionally, the fourth polymerizable monomer includes one or more of acrylamide, N-hydroxymethyl acrylamide and N-butoxymethyl acrylamide.
[0043] Theoretically, this application does not limit the type of the fourth polymerized monomer. The fourth polymerized monomer satisfies the above structure, that is, the fourth polymerized monomer includes the above-listed substances and substances not listed in this application.
[0044] The use of any one or more fourth polymerizable monomers mentioned above can improve the adhesion of the acrylic copolymer.
[0045] It is understood that the bonding effect is better when at least two of the above four monomers are included. For example, the constituent monomers of the acrylic ester copolymer include at least the first polymerized monomer and the second polymerized monomer, or the constituent monomers of the acrylic ester copolymer include at least the first polymerized monomer and the third polymerized monomer, or the constituent monomers of the acrylic ester copolymer include at least the first polymerized monomer and the fourth polymerized monomer. When the constituent monomers of the acrylic ester copolymer include all four of the above monomers, the adhesive performance is better.
[0046] Optionally, the constituent monomers of the acrylic ester copolymer include a first polymerized monomer, a second polymerized monomer, a third polymerized monomer and a fourth polymerized monomer, and the mass ratio of the first polymerized monomer, the second polymerized monomer, the third polymerized monomer and the fourth polymerized monomer is 1: (0.01~0.8): (0.01~0.5): (0.01~0.3), preferably, the mass ratio of the first polymerized monomer, the second polymerized monomer, the third polymerized monomer and the fourth polymerized monomer is 1: (0.1~0.5): (0.15~0.45): (0.1~0.22).
[0047] The constituent monomers of the acrylic ester copolymer include the above four monomers at the same time, and when the content of each monomer component is within the above range, the comprehensive performance is better.
[0048] The present application also provides a separator, which includes a substrate and an adhesive layer provided on at least one side of the substrate, wherein the adhesive layer includes the adhesive for secondary batteries as described above.
[0049] Optionally, the surface density of the adhesive layer on the substrate is in the range of 0.7 g / m 2 Up to 3g / m 2 , preferably 0.8 g / m 2 Up to 2g / m 2 .
[0050] The adhesive based on the ring structure can increase the contact area between the adhesive and the electrode and the diaphragm. That is, better bonding performance can be achieved while reducing the amount of the adhesive used. In this way, the surface density of the adhesive layer on the substrate is in the range of 0.7g / m 2 Up to 3g / m 2 Preferably, the surface density of the adhesive layer on the substrate is in the range of 0.8 g / m 2 Up to 2g / m 2 .
[0051] The present application also provides a secondary battery, which includes the separator.
[0052] The present application also provides an electrical device, which includes the secondary battery as described above. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0054] FIG1 is a scanning electron microscope image of the adhesive provided in Example 1 of the present application;
[0055] FIG2 is a scanning electron microscope image of the adhesive provided in Example 1 of the present application;
[0056] FIG3 is a schematic flow chart of a method for preparing an adhesive provided in an embodiment of the present application;
[0057] FIG4 is a schematic diagram of a secondary battery provided in an embodiment of the present application;
[0058] FIG5 is an exploded view of the secondary battery provided by the embodiment of the present application shown in FIG4 ;
[0059] FIG6 is a schematic diagram of a battery module provided in an embodiment of the present application;
[0060] FIG7 is a schematic diagram of a battery pack provided in an embodiment of the present application;
[0061] FIG8 is an exploded view of the battery pack provided by the embodiment of the present application shown in FIG7 ;
[0062] FIG9 is a schematic diagram of an electrical device using a secondary battery provided in an embodiment of the present application as a power source;
[0063] FIG10 is a schematic diagram of the adhesive provided in Example 1 of the present application.
[0064] Description of Figure Numbers:
[0065] The realization of the objectives, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0066] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0067] Below, the binder and its preparation method of the present application, as well as the embodiments of the diaphragm, electrode assembly, battery cell, battery and electrical device containing the binder are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0068] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0069] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0070] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0071] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0072] There is an opening problem in the battery cell, that is, a gap is easily formed between the electrode and the diaphragm, resulting in poor battery cycle performance.
[0073] For example, the bonding strength between the positive and negative electrodes and the separator is insufficient, which often leads to problems such as cell opening, and the secondary battery's requirements for the performance of the coated separator cannot be met.
[0074] The battery cell is formed by bonding the positive and negative electrode sheets and the separator. The battery cell has a certain hardness. That is, because the bonded positive and negative electrode sheets and the separator adhere to each other and support each other, a structure with a certain thickness is formed. A structure with a certain thickness has a certain hardness. The negative electrode will expand during the charge and discharge process. If the bonding force is weak, a gap will form between the positive and negative electrode sheets and the separator. The positive and negative electrode sheets and the separator cannot adhere to each other and support each other, resulting in a loose battery cell and a lower hardness. At this time, the power performance of the battery cell will deteriorate. For example, the rate performance will be reduced, and the cycle performance will also deteriorate. For example, in electric vehicles, loose battery cells will cause the battery charging speed to slow down, and the battery cycle performance will deteriorate, which will directly shorten the battery life. Electric vehicles need to frequently replace batteries, and consumers' costs for electric vehicles increase.
[0075] Based on this, the present application provides an adhesive for a secondary battery, the adhesive including an acrylic copolymer, and the shape of the adhesive including a ring.
[0076] Binder refers to a material with adhesive properties that is used to bond different substances together.
[0077] The ring-shaped adhesive has a through hole formed in its structure, wherein the through hole refers to a hole that passes through two opposite surfaces of the adhesive, as shown in Figures 1 and 2, which is an adhesive with a ring structure.
[0078] The annular ring line, as shown in Figure 10, is formed in the structure of the annular adhesive with a through hole 61, and a ring line 60 is formed around the through hole 61. It can be understood that when the adhesive is placed on the diaphragm in the direction toward the through hole 61 (that is, the opening of the through hole 61 faces the diaphragm), the periphery of the through hole 61 will contact the diaphragm, and the contact portion is a ring line. Compared with setting the spherical adhesive on the diaphragm, the spherical adhesive is in point contact with the diaphragm, and the annular adhesive can contact the diaphragm through the ring line, thereby increasing the contact area.
[0079] Acrylate copolymers, acrylic copolymers are a general term for polymers produced by copolymerization of acrylic monomers and other comonomers.
[0080] The acrylic ester monomer has an acrylate group in its structure, for example, methyl acrylate, ethyl acrylate, and n-butyl acrylate.
[0081] Acrylate copolymers have good adhesion, and the use of acrylic copolymers can improve the adhesion between the diaphragm and the electrode.
[0082] The adhesive with an annular structure has a bonding site with a larger area. For example, when the adhesive with an annular structure contacts the electrode, the contact point is the ring line of the annular adhesive, while the contact site of the spherical adhesive is point contact. The annular structure and the spherical adhesive of the same size have better bonding performance based on the larger contact site of the annular structure. In addition, the adhesive with an annular structure has a hollow through hole. The annular structure adhesive and the spherical adhesive of the same size have a smaller mass. In this way, better bonding performance can be achieved while reducing the amount of annular structure adhesive used.
[0083] Coating the ring-shaped adhesive on the diaphragm can increase the contact area between the adhesive and the electrode and diaphragm, reduce the amount of adhesive used, and meet the cold pressing bonding force between the diaphragm and the positive and negative electrode sheets during the cold pressing process, thereby increasing the hardness of the battery cell and improving problems such as battery cell opening and soft battery cells. At the same time, the adhesive coated on the diaphragm is applied to the secondary battery, which can improve the large-clamp cycle performance of the secondary battery.
[0084] Among them, the large clamp cycle performance is a cyclic functional test performance of the battery cell. During the test, a clamp is added to the battery cell and a certain force is applied to the clamp to squeeze the battery cell. When the battery cell is full, it will expand. Due to the dual squeezing of the clamping force and the expansion force, the battery cell will deform. This test is used to test the shape retention performance and compressive performance of the battery cell. The adhesive of this solution is used. Due to its good bonding performance, the expansion of the battery cell is reduced, and the shape of the battery cell is well maintained. The battery cell using the adhesive of this application maintains good performance under the test conditions of the large clamp, indicating that the battery cell obtained by using the adhesive of this solution has good deformation retention. After the battery cell is assembled into a battery, since the battery cell is not easily deformed, the space used to install the battery cell can be saved, so that the battery volume can be made smaller. Because if the battery cell is easily deformed, it will squeeze the structure near the battery cell. In order to improve this phenomenon, a larger space is required to accommodate the deformed battery cell. That is, space needs to be reserved in the battery to accommodate the deformed part of the battery cell, thereby occupying more space inside the battery.
[0085] At the same time, the good cycle performance of the large clamp of the battery cell also indicates that the cycle performance of the battery cell is good. For example, when the battery cell expands, the gap between the electrode and the diaphragm becomes larger, and the path of lithium ions (taking lithium-ion batteries as an example, of course it can also be other types of secondary batteries) through the positive and negative electrodes becomes longer, resulting in poor cycle performance.
[0086] The adhesive of the present application can improve the close fit between the diaphragm and the electrode, improve the discharge capacity of the battery, reduce the internal resistance, reduce the polarization loss, extend the cycle life of the battery, and improve the utilization rate of the secondary battery.
[0087] In one embodiment, the specific surface area of the binder is in the range of 0.4 m2 / g to 1.2m 2 / g, preferably, the specific surface area of the binder is in the range of 0.6m 2 / g to 0.9m 2 / g.
[0088] Specific surface area refers to the total area per unit mass of material, measured in m 2 / g.
[0089] Specific surface area test: BET specific surface area was determined by the BET method with N2 adsorption.
[0090] A NOVA 2000 surface area and pore analyzer from Quantachrome was used, and high-purity nitrogen greater than or equal to 99.999% was used as the adsorbent. A spherical sample tube with a diameter of 20 mm was selected, and 1.4000 g ± 0.2000 g of the binder sample was weighed. A heating pack was placed on the tube, and a vacuum pump was used to evacuate the tube to a pressure of 10 -2 Above torr, slowly heat up to a certain temperature after the pressure stabilizes, control the pretreatment time, cool for 30 minutes after pretreatment, and weigh the sample mass; conduct full-process adsorption and desorption tests on the pretreated samples to obtain the isothermal adsorption and desorption curves of the samples, and use the instrument's built-in software to process the data and obtain the specific surface area parameters of the binder.
[0091] Specific surface area refers to the total area per unit mass of a material. The ring-shaped binder has a hollow through-hole. Compared with the spherical structure binder of the same size, the ring-shaped binder has a larger specific surface area. The range of the specific surface area of the binder is 0.4m 2 / g to 1.2m 2 / g, preferably, the specific surface area of the binder is in the range of 0.6m 2 / g to 0.9m 2 / g, which is beneficial to improving the contact between the annular adhesive and the diaphragm and electrode, and improving the bonding performance.
[0092] Above 0.4m 2 / g to 1.2m 2 / g, the value includes the minimum and maximum values of the range, and each value between the minimum and maximum values, and specific examples include but are not limited to the point value in the embodiment and 0.4m 2 / g,,0.5m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g1.2m 2 / g, etc., as well as the range value between any two of the above point values.
[0093] Above 0.6m 2 / g to 0.9m 2 / g, the value includes the minimum and maximum values of the range, and each value between the minimum and maximum values, and specific examples include but are not limited to the point value in the embodiment and 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, etc., as well as the range value between any two of the above point values.
[0094] In one embodiment, the ratio of the surface area to volume of the adhesive is 0.1×10 6 m -1 to 20×10 6 m -1 Preferably, the ratio of the surface area to volume of the binder is 0.5×10 6 m -1 to 16×10 6 m -1 .
[0095] The surface area to volume ratio is the ratio of the total area of a material to the total volume of the material.
[0096] The test method for the ratio of surface area to volume can be used to test the surface area and volume of a certain mass of binder respectively, and then divide the surface area by the volume to obtain the ratio of surface area to volume. Define the test m1 gram of binder, the surface area test method can be obtained using the above specific surface area test method, and define the above specific surface area value as am 2 / g, then the surface area of m1 gram of binder is (m1*a), the unit is m 2 ; Use the drainage method to test the volume of m1 gram of binder. Take water with a volume of V1 and put it into a container. Then put 1 gram of binder into the container to obtain a mixed solution of binders. The volume of the mixed solution is measured to be V2. Then, the volume of m1 gram of binder is V2-V1; the surface area to volume ratio is calculated as follows: (m1*a) / (V2-V1) The unit is m -1 .
[0097] The ring-shaped adhesive has hollow through-holes. Compared with the spherical adhesive of the same size, the surface area to volume ratio of the ring-shaped adhesive is larger. The surface area to volume ratio of the adhesive is 0.1×10 6 m -1 to 20×10 6 m -1Preferably, the ratio of the surface area to volume of the binder is 0.5×10 6 m -1 to 16×10 6 m -1 This shows that the annular adhesive has a higher surface area than the spherical adhesive, which is beneficial to improving the contact between the annular adhesive and the diaphragm and electrode, and improving the bonding performance.
[0098] The above 0.1×10 6 m -1 to 20×10 6 m -1 In the example, the value includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and 0.1×10 6 m -1 , 1×10 6 m -1 , 2×10 6 m -1 , 3×10 6 m -1 , 4×10 6 m -1 , 5×10 6 m -1 , 6×10 6 m -1 , 7×10 6 m -1 , 8×10 6 m -1 , 9×10 6 m -1 , 10×10 6 m -1 , 11×10 6 m -1 , 12×10 6 m -1 , 13×10 6 m -1 , 14×10 6 m -1 , 15×10 6 m -1 , 16×10 6 m -1 , 17×10 6 m -1 , 18×10 6 m -1 , 19×10 6 m -1 , 20×10 6 m -1 etc., as well as the range values between any two of the above point values.
[0099] The above 0.5×10 6 m -1 to 16×10 6 m -1 In the example, the value includes the minimum and maximum values of the range, and each value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and 0.5×10 6 m -1 , 1×10 6 m -1 , 2×10 6 m -1 , 3×10 6 m -1 , 4×10 6 m -1 , 5×10 6 m -1 , 6×10 6 m -1 , 7×10 6 m -1 , 8×10 6 m -1 , 9×10 6 m -1 , 10×10 6 m -1 , 11×10 6 m -1 , 12×10 6 m -1 , 13×10 6 m -1 , 14×10 6 m -1 , 15×10 6 m -1 , 16×10 6 m -1 etc., as well as the range values between any two of the above point values.
[0100] In one embodiment, the bulk density of the binder is in the range of 0.3 g / cm 3 to 0.8g / cm 3 Preferably, the bulk density of the binder is in the range of 0.4 g / cm 3 to 0.7g / cm 3 .
[0101] Bulk density is the mass per unit volume measured when powder is freely filled in a container immediately after filling is completed.
[0102] The specific test steps are as follows: using the vibration instrument method, the sample is placed in a 100mL measuring cylinder of the vibration instrument, the equipment is started, and the vibration device of the vibration instrument vibrates the measuring cylinder to compact the sample. During the experiment, the sample is continuously added until the sample volume no longer decreases. Finally, the mass of the sample is weighed, and the bulk density is obtained by dividing the sample mass by the sample volume.
[0103] The ring-shaped adhesive has a hollow through-hole. After the ring-shaped adhesive is filled in the container, the through-holes of the ring-shaped adhesive form a gap, which reduces the bulk density of the ring-shaped adhesive compared to the spherical adhesive of the same size. The bulk density range of the adhesive is 0.3g / cm 3 to 0.8g / cm 3 Preferably, the bulk density of the binder is in the range of 0.4 g / cm 3 to 0.7g / cm 3 This shows that under certain conditions, reducing the mass of the ring adhesive can also improve the bonding performance of the adhesive.
[0104] Above 0.3g / cm 3 to 0.8g / cm 3 In the range, the values include the minimum and maximum values of the range, and each value between the minimum and maximum values, and specific examples include but are not limited to the point values in the embodiment and 0.3g / cm 3 , 0.4g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 , 0.7g / cm 3 , 0.8g / cm 3 etc., as well as the range values between any two of the above point values.
[0105] Above 0.4g / cm 3 to 0.7g / cm 3 The values include the minimum and maximum values of the range, and each value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment with 0.4 g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 , 0.7g / cm 3 etc., as well as the range values between any two of the above point values.
[0106] In one embodiment, the shape of the adhesive comprises a ring shape.
[0107] According to experimental experience and the surface tension of materials, a circular ring is a shape that is relatively easy to achieve. The shape of the adhesive in this application includes a circular ring. It should also be understood that the circular ring in this application can be an approximate circular ring. For example, as shown in Figure 1, the structure of some adhesives is not a perfect circular ring. For example, some parts are flattened to form a structure that is approximately circular.
[0108] In one embodiment, the volume particle size distribution Dv50 of the binder is in a range of 1 μm to 15 μm. Preferably, the volume particle size distribution Dv50 of the binder is in a range of 3 μm to 12 μm.
[0109] Dv50: Among the sample particles, 50% of the total volume of the particles have a particle size larger than this value, and another 50% of the total volume of the particles have a particle size smaller than this value; Dv50 can represent the median particle size of the sample.
[0110] The volume particle size distribution Dv50 of the binder can be measured using methods known in the art. For example, GB / T 19077-2016 can be used for characterization testing using a Malvern laser particle size analyzer, such as a Malvern Mastersizer-3000.
[0111] In order to improve the adhesion of the adhesive and improve the gap between the diaphragm and the pole piece, the volume particle size distribution Dv50 of the adhesive ranges from 1 μm to 15 μm. Preferably, the volume particle size distribution Dv50 of the adhesive ranges from 3 μm to 12 μm.
[0112] In the above-mentioned 1μm to 15μm, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc., as well as the range values between any two of the above-mentioned point values.
[0113] In the above-mentioned 3μm to 12μm, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, etc., as well as the range values between any two of the above-mentioned point values.
[0114] In one embodiment, the monomers constituting the acrylic ester copolymer include a first polymerizable monomer, and the structure of the first polymerizable monomer includes: Wherein, R1 includes hydrogen or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.
[0115] The first polymerized monomer structure contains an ester group, which can improve the compatibility of the acrylic copolymer with the electrolyte, enhance the ion conductivity, and improve the anti-swelling ability of the acrylic copolymer. In addition, as a flexible monomer segment in the molecular chain segment, it can adjust the glass transition temperature of the acrylic copolymer, improve the toughness of the adhesive during application, and help to exert a good bonding effect.
[0116] In one embodiment, the first polymerizable monomer includes one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.
[0117] Theoretically, this application does not limit the type of the first polymerized monomer. The first polymerized monomer satisfies the above structure, that is, the first polymerized monomer includes the above-listed substances and substances not listed in this application.
[0118] By using any one or more of the above-mentioned first polymerizable monomers, the glass transition temperature of the acrylic ester copolymer can be adjusted, and the anti-swelling ability of the acrylic ester copolymer can be improved.
[0119] In one embodiment, the monomers constituting the acrylic ester copolymer include a second polymerizable monomer, and the structure of the second polymerizable monomer includes: Wherein, R3 includes hydrogen or an alkyl group of 1 to 6 carbon atoms.
[0120] The structure of the second polymerized monomer contains carboxyl groups, which have the characteristics of strong polarity and can improve the adhesion and flexibility of the adhesive. For example, the carboxyl groups can form a binding force with the functional groups on the electrode and the diaphragm material to improve the bonding effect.
[0121] In one embodiment, the second polymerizable monomer includes one or more of acrylic acid, methacrylic acid, butenoic acid, and heptenoic acid.
[0122] Theoretically, this application does not limit the type of the second polymerized monomer. The second polymerized monomer satisfies the above structure, that is, the second polymerized monomer includes the above-listed substances and substances not listed in this application.
[0123] The use of any one or more of the above-mentioned second polymerizable monomers can improve the bonding properties of the acrylic copolymer.
[0124] In one embodiment, the monomers constituting the acrylic ester copolymer include a third polymerizable monomer, and the structure of the third polymerizable monomer includes: Wherein, R4 includes a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0125] The structure of the third polymer monomer contains an unsaturated nitrile group. The highly polar cyano group helps to improve the ionic conductivity and also has the effects of anti-swelling and high adhesion.
[0126] In one embodiment, the third polymerizable monomer includes one or more of acrylonitrile and methacrylonitrile.
[0127] Theoretically, this application does not limit the type of the third polymerized monomer. The third polymerized monomer satisfies the above structure, that is, the third polymerized monomer includes the above-listed substances and substances not listed in this application.
[0128] The use of any one or more third polymerizable monomers mentioned above can improve the ionic conductivity of the acrylic ester copolymer and enhance its adhesiveness.
[0129] In one embodiment, the monomers constituting the acrylic ester copolymer include a fourth polymerizable monomer, and the structure of the fourth polymerizable monomer includes: Wherein, R5 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R6 includes a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.
[0130] The structure of the fourth polymerizable monomer contains an unsaturated amide group, which plays a role in improving swelling and enhancing adhesion.
[0131] In one embodiment, the fourth polymerizable monomer includes one or more of acrylamide, N-methylol acrylamide, and N-butoxymethyl acrylamide.
[0132] Theoretically, this application does not limit the type of the fourth polymerized monomer. The fourth polymerized monomer satisfies the above structure, that is, the fourth polymerized monomer includes the above-listed substances and substances not listed in this application.
[0133] The use of any one or more fourth polymerizable monomers mentioned above can improve the adhesion of the acrylic copolymer.
[0134] It is understood that the bonding effect is better when at least two of the above four monomers are included. For example, the constituent monomers of the acrylic ester copolymer include at least the first polymerized monomer and the second polymerized monomer, or the constituent monomers of the acrylic ester copolymer include at least the first polymerized monomer and the third polymerized monomer, or the constituent monomers of the acrylic ester copolymer include at least the first polymerized monomer and the fourth polymerized monomer. When the constituent monomers of the acrylic ester copolymer include all four of the above monomers, the adhesive performance is better.
[0135] In one embodiment, the constituent monomers of the acrylic ester copolymer include a first polymerized monomer, a second polymerized monomer, a third polymerized monomer, and a fourth polymerized monomer, and the mass ratio of the first polymerized monomer, the second polymerized monomer, the third polymerized monomer, and the fourth polymerized monomer is 1: (0.01-0.8): (0.01-0.5): (0.01-0.3). Preferably, the mass ratio of the first polymerized monomer, the second polymerized monomer, the third polymerized monomer, and the fourth polymerized monomer is 1: (0.1-0.5): (0.15-0.45): (0.1-0.22).
[0136] The constituent monomers of the acrylic ester copolymer include the above four monomers at the same time, and when the content of each monomer component is within the above range, the comprehensive performance is better.
[0137] The mass ratio test method is as follows: during the preparation of the acrylic ester copolymer, the mass of each monomer used to prepare the acrylic ester copolymer input during the reaction is recorded, the mass of the first polymerized monomer is recorded as m1, the mass of the second polymerized monomer is recorded as m2, the mass of the third polymerized monomer is recorded as m3, and the mass of the fourth polymerized monomer is recorded as m4. The mass ratio of the four monomers is m1:m2:m3:m4.
[0138] In the above 1: (0.01~0.8): (0.01~0.5): (0.01~0.3), the values include the minimum and maximum values of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and 1: 0.01: 0.01: 0.01, 1: 0.5: 0.25: 0.15, 1: 0.8: 0.5: 0.3, etc., as well as the range values between any two of the above point values.
[0139] In the above 1: (0.1~0.5): (0.15~0.45): (0.1~0.22), the values include the minimum and maximum values of the range, and every value between this minimum and maximum value. Specific examples include but are not limited to the point values in the embodiments and 1: 0.1: 0.15: 0.1, 1: 0.3: 0.3: 0.15, 1: 0.5: 0.45: 0.22, etc., as well as the range values between any two of the above point values.
[0140] In one embodiment, the present application further provides a method for preparing an adhesive, comprising: preparing an acrylic copolymer emulsion; and spray-drying the acrylic copolymer emulsion to obtain a ring-shaped adhesive.
[0141] Spray drying, through mechanical action, disperses the material to be dried (acrylate copolymer emulsion) into very fine mist-like particles (increasing the water evaporation area and accelerating the drying process). When in contact with hot air, most of the water is removed instantly, and the solid matter in the material is dried into powder.
[0142] An acrylic copolymer emulsion is prepared by emulsion polymerization and spray-dried to obtain a ring-shaped adhesive. The mechanism is that due to the evaporation of water, the primary emulsion particles of the acrylic copolymer are tightly stacked together to form a ring-shaped adhesive.
[0143] In one embodiment, the steps of preparing an acrylic copolymer emulsion include: adding water, an emulsifier, and monomers constituting the acrylic copolymer into a container, stirring and emulsifying, and obtaining a pre-emulsion of the monomers; adding an emulsifier and water into a reaction container, stirring and emulsifying, adding the pre-emulsion and an initiator solution under heating conditions, and heating the reaction to obtain an acrylic copolymer emulsion.
[0144] Pre-emulsion is a solution obtained by pre-emulsifying the monomers. Emulsification is the process of evenly dispersing a liquid in another immiscible liquid in the form of extremely small droplets. Water, an emulsifier, and the monomers constituting the acrylic copolymer are blended and stirred so that the monomers constituting the acrylic copolymer are dispersed in water under the action of the emulsifier.
[0145] Emulsion polymerization is a process in which monomers are dispersed in water with the help of emulsifiers and mechanical stirring to form an emulsion, and then an initiator is added to initiate monomer polymerization.
[0146] Emulsifiers are substances that can transform mutually incompatible oil and water into an emulsion that is difficult to separate. Emulsifiers are usually surfactants that have both hydrophilic polar groups and hydrophobic (lipophilic) non-polar groups.
[0147] Initiators are substances that can initiate polymerization reactions of monomers. For example, free radical initiators are compounds that readily decompose into free radicals (i.e., primary free radicals) upon exposure to heat. They can be used to initiate free radical polymerization and copolymerization reactions of olefins and dienes.
[0148] In the preparation of the acrylic copolymer emulsion, pre-emulsification followed by polymerization allows for more uniform monomer mixing, resulting in more uniform acrylic copolymer particles with more stable performance, and facilitates the formation of a ring-shaped binder during the spray drying process.
[0149] Polyvinylidene fluoride (PVDF), the most commonly used binder, is widely used in separators. However, its price has risen sharply, and market supply is tight. Coating PVDF polymer on the surface of lithium battery separators can partially address the separator's high-temperature shrinkage problem. After winding, battery cells are cold-pressed, but conventional PVDF is a homopolymer with a crystallinity of approximately 50%. This results in insufficient adhesion to the positive and negative electrodes, often leading to cell opening problems and failing to meet the performance requirements of coated separators for secondary batteries.
[0150] Specifically, coating the battery separator with polyvinylidene fluoride (PVDF) polymer can partially address the separator's high-temperature shrinkage problem. After winding, the battery cell undergoes cold pressing, but conventional PVDF is a homopolymer with a crystallinity of approximately 50%, resulting in insufficient adhesion to the positive and negative electrode sheets, often leading to cell openings. These openings create gaps between the electrode sheets and the separator, loosening the overall cell structure and reducing its rigidity, leading to poor cycling performance.
[0151] Applying the annular adhesive of the present application to the diaphragm and spraying it on the diaphragm can increase the contact area between the adhesive and the electrode and diaphragm, reduce the amount used, and meet the cold pressing bonding force between the diaphragm and the positive and negative electrode sheets during the cold pressing process, thereby improving the hardness of the battery cell and avoiding problems such as battery cell opening and soft battery cells. At the same time, the adhesive is coated on the diaphragm and applied to the secondary battery, which can improve the large clamp cycle performance of the secondary battery.
[0152] In one embodiment, the present application also provides a diaphragm, which includes a substrate and an adhesive layer provided on at least one side of the substrate, the adhesive layer includes the adhesive for secondary batteries as described above; or, the adhesive layer includes an adhesive prepared by the preparation method of the adhesive for secondary batteries as described above.
[0153] The adhesive layer is a structure formed by an adhesive applied on the diaphragm.
[0154] Before applying the adhesive to the diaphragm, adhesive slurry is prepared first. The adhesive is dissolved in water to prepare slurry. The slurry is applied to the diaphragm and dried to obtain an adhesive layer.
[0155] It can be understood that the adhesive has no adhesive force at room temperature (room temperature is about 23±2°C) and without pressure after drying, that is, when no pressure is applied to the diaphragm, the side of the adhesive layer facing away from the diaphragm is non-sticky, which can meet the needs of winding and unwinding the diaphragm. When a certain pressure is applied, the adhesive shows pressure sensitivity and better adhesion, which meets the adhesion requirements between the diaphragm and the positive and negative electrode sheets. At the same time, the adhesion also forms intermolecular forces with the molecules on the diaphragm and the electrode sheets, and the diaphragm and the electrode sheets are effectively bonded through the adhesive.
[0156] It is also understandable that after cold pressing, the hollow through-holes of the annular adhesive are not completely blocked, thereby forming gaps. These gaps help the infiltration of the electrolyte and improve the transmission of lithium ions (taking lithium-ion batteries as an example, of course, other types of secondary batteries can also be used)).
[0157] The binder powder prepared by the spray drying process achieves non-adhesiveness when there is no pressure at room temperature.
[0158] Pressure sensitivity means that after the adhesive is squeezed, the adhesive can deform under force and penetrate into the pores of the diaphragm and electrode to play a mechanical interlocking role, thereby achieving a bonding effect.
[0159] In one embodiment, the surface density of the adhesive layer on the substrate is in the range of 0.7 g / m 2 Up to 3g / m 2 , preferably 0.8 g / m 2 Up to 2g / m 2 .
[0160] Areal density refers to the mass of the adhesive layer applied on one side of the diaphragm.
[0161] The test method for surface density is: take a certain area of diaphragm, obtain the diaphragm area S, weigh the weight M1 of the diaphragm plus the adhesive, weigh the mass M2 of the diaphragm without adhesive coating of the same area S, and the surface density of the adhesive is calculated as (M1-M2) / S.
[0162] The adhesive based on the ring structure can increase the contact area between the adhesive and the electrode and the diaphragm. That is, better bonding performance can be achieved while reducing the amount of the adhesive used. In this way, the surface density of the adhesive layer on the substrate is in the range of 0.7g / m 2 Up to 3g / m 2 , preferably 0.8 g / m 2 Up to 2g / m 2 .
[0163] Above 0.7g / m 2 Up to 3g / m 2 In the range, the value includes the minimum and maximum values of the range, and each value between the minimum and maximum values, and specific examples include but are not limited to the point values in the embodiment and 0.7g / m 2 , 0.8g / m 2 , 0.9g / m 2 , 1g / m 2 , 1.5g / m 2 , 2g / m 2 , 2.5g / m 2 , 3g / m 2 etc., as well as the range values between any two of the above point values.
[0164] Above 0.8g / m 2 Up to 2g / m 2 In the range, the value includes the minimum and maximum values of the range, and each value between the minimum and maximum values, and specific examples include but are not limited to the point values in the embodiment and 0.8g / m 2 , 0.9g / m 2 , 1g / m 2 , 1.2g / m 2 , 1.5g / m 2 , 1.7g / m 2 , 1.9g / m 2 , 2g / m 2 etc., as well as the range values between any two of the above point values.
[0165] An embodiment of the present application further provides a secondary battery, which includes the separator as described above.
[0166] Secondary batteries include battery modules, battery cells, battery packs, and other forms. When the secondary battery is a battery cell, the battery cell includes the aforementioned separator; when the secondary battery is a battery module, the battery module includes the aforementioned separator; and when the secondary battery is a battery pack, the battery pack includes the aforementioned separator.
[0167] An embodiment of the present application further provides an electrical device, which includes the above-mentioned battery cell or the above-mentioned battery.
[0168] In addition, the electrode assembly, battery cell, battery, and electric device of the present application will be described below with reference to the accompanying drawings as appropriate.
[0169] In one embodiment of the present application, an electrode assembly is provided.
[0170] Typically, an electrode assembly includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery's charge and discharge process, active ions are embedded in and released from the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator is located between the positive and negative electrodes, primarily preventing a short circuit between the positive and negative electrodes while allowing ions to pass through. The separator is the separator described above in this application.
[0171] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.
[0172] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0173] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0174] In some embodiments, when the electrode assembly is a lithium-ion battery, the positive electrode active material may be a positive electrode active material for lithium-ion batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0175] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0176] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0177] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0178] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0179] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0180] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0181] In some embodiments, the negative electrode active material may adopt the negative electrode active material for batteries known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may include at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0182] In some embodiments, the negative electrode film layer may further optionally include a binder. The binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0183] In some embodiments, the negative electrode film layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0184] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0185] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0186] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. This application has no specific restrictions on the type of electrolyte, and it can be selected according to needs.
[0187] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0188] In some embodiments, the electrolyte salt may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0189] In some embodiments, the solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0190] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0191] In some embodiments, the electrode assembly further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0192] In some embodiments, the material of the separator may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0193] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0194] In some embodiments, the electrode assembly may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0195] In some embodiments, the outer packaging of the electrode assembly may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the electrode assembly may be a soft shell, such as a bag-type soft shell. The soft shell may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0196] The present application has no particular limitation on the shape of the electrode assembly, which may be cylindrical, square, or any other shape. For example, FIG4 shows a secondary battery 5 having a square structure as an example.
[0197] In some embodiments, referring to Figure 5, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the diaphragm can be formed into a secondary battery 52 through a winding process or a lamination process. The secondary battery 52 is encapsulated in the receiving cavity. The electrolyte is immersed in the secondary battery 52. The number of secondary batteries 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0198] In some embodiments, the electrode assemblies may be assembled into a battery module. The number of electrode assemblies contained in the battery module may be one or more. The specific number may be selected by those skilled in the art based on the application and capacity of the battery module.
[0199] Figure 6 shows an example battery module 4. Referring to Figure 6 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured using fasteners.
[0200] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0201] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0202] Figures 7 and 8 illustrate an example battery pack 1. Referring to Figures 7 and 8 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0203] In addition, the present application also provides an electrical device, which includes at least one of the electrode assembly, battery module, or battery pack provided in the present application. The electrode assembly, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0204] As an electrical device, an electrode assembly, battery module or battery pack can be selected according to its usage requirements.
[0205] Figure 9 shows an example of an electric device. This device can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the electrode assembly, a battery pack or battery module can be used.
[0206] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use an electrode assembly as a power source.
[0207] Example
[0208] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0209] Example 1
[0210] Preparation of acrylic copolymers
[0211] (1) 150 g of deionized water and 3.6 g of sodium lauryl sulfate were added to a 500 ml three-necked flask, and the mixture was stirred for 15 min for emulsification. Then, 76.34 g of the first polymerizable monomer, ethyl acrylate, 0.76 g of the second polymerizable monomer, acrylic acid, 15.27 g of the third polymerizable monomer, and 7.63 g of the fourth polymerizable monomer, N-hydroxymethyl acrylamide, were added in a mass ratio of 1:0.01:0.2:0.1, totaling 100 g of monomers. The mixture was stirred for 60 min to obtain a pre-emulsion of the monomers, which was then taken out for later use.
[0212] (2) To a 500 ml four-necked flask equipped with a condenser, a stirrer, a peristaltic pump, and a thermometer, add 100 ml of deionized water and 0.15 g of sodium dodecylbenzenesulfonate, heat to 75 ° C, and emulsify at a speed of 2000 r / min for 15 min to fully emulsify the system. Then, slowly dropwise add the pre-emulsion prepared in the previous step and the initiator solution (0.2 g of potassium persulfate is dissolved in 30 g of deionized water to form a solution). After the addition is complete, heat to 90 ° C and keep the temperature for reaction for 1 h. Cool to below 40 ° C, adjust the pH of the system to neutral with an ammonia solution, stop stirring, filter the material, and obtain a polymer emulsion.
[0213] The volume particle size distribution Dv50 of the acrylic ester copolymer is 0.1 μm±0.01 μm (the volume particle size distribution Dv50 of the acrylic ester copolymer in each example is 0.1 μm±0.01 μm).
[0214] Preparation of binder
[0215] The acrylic copolymer emulsion prepared above was spray-dried to obtain a ring-shaped adhesive. The spray-drying parameters were: inlet air temperature 115° C., outlet air temperature 65° C., and air pressure 2200 Pa.
[0216] Example 2 to Example 27
[0217] Based on Example 1, the types and mass ratios of the monomers input were changed, the monomer composition of the acrylic copolymer and the volume particle size distribution Dv50 of the binder, as well as the surface density of the binder coated on the substrate were adjusted to obtain Examples 2 to 27.
[0218] Comparative Example 1
[0219] Spherical binder is obtained by emulsion polymerization
[0220] (1) 150 g of deionized water and 3.6 g of sodium lauryl sulfate were added to a 500 ml three-necked flask, and the mixture was stirred for 15 min for emulsification. Then, 76.34 g of the first polymerizable monomer, ethyl acrylate, 22.9 g of the second polymerizable monomer, acrylic acid, 15.27 g of the third polymerizable monomer, and 7.63 g of the fourth polymerizable monomer, N-hydroxymethyl acrylamide, were added in a mass ratio of 1:0.3:0.2:0.1, totaling 100 g of the monomers. The mixture was stirred for 60 min to obtain a pre-emulsion of the monomers, which was then taken out for later use.
[0221] (2) To a 500 ml four-necked flask equipped with a condenser, a stirrer, a peristaltic pump, and a thermometer, 100 ml of deionized water and 0.15 g of sodium dodecylbenzenesulfonate were added, and the mixture was heated to 75 ° C. and emulsified at a speed of 2000 r / min for 15 min to fully emulsify the system. Then, the pre-emulsion prepared in the previous step and the initiator solution (0.2 g of potassium persulfate was dissolved in 30 g of deionized water to form a solution) were slowly added dropwise. After the addition was completed, the temperature was raised to 90 ° C. and the reaction was kept at this temperature for 1 h. The mixture was cooled to below 40 ° C. After the pH of the system was adjusted to neutral with an ammonia solution, stirring was stopped, and the material was filtered to obtain a first polymer emulsion.
[0222] (3) Repeat step (1) to obtain a second pre-emulsion, add the second pre-emulsion and an initiator solution (0.2 g of potassium persulfate is dissolved in 30 g of deionized water to form a solution) to the first polymer emulsion obtained in step (2), raise the temperature to 90°C after the addition is complete, keep the temperature to react for 1 hour, cool to below 40°C, adjust the pH of the system to neutral with an ammonia solution, stop stirring, filter the material, and obtain a second polymer emulsion.
[0223] Preparation of battery cells and batteries
[0224] (1) Preparation of diaphragm
[0225] A commercially available PE microporous film with a thickness of 7 μm and an average pore size of 80 nm (from Zhuogao Electronic Technology Co., Ltd.) was used as the substrate. The membrane adhesive prepared as described above was stirred and mixed uniformly in deionized water to obtain a slurry (solid content of 20%). The slurry was sprayed onto both surfaces of the substrate and dried to remove the solvent to obtain an adhesive layer. The surface density of the adhesive layer on the substrate was 1.35 g / m 2 , and obtain a diaphragm.
[0226] (2) Preparation of positive electrode sheet
[0227] Polyvinylidene fluoride (PVDF), lithium iron phosphate (LFP), conductive carbon black, and N-methylpyrrolidone (NMP) were mixed in a mass ratio of 1.2:58.38:0.42:40 and stirred thoroughly to prepare a positive electrode slurry. 2 The loading amount is evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed and cut to obtain the positive electrode sheet.
[0228] (3) Preparation of negative electrode sheet
[0229] Artificial graphite, conductive agent acetylene black, binder styrene butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na) were added into deionized water in a mass ratio of 96.2:1.0:1.6:1.2, and stirred thoroughly to prepare a negative electrode slurry (solid content of 63%). 2 The loading amount is coated on the negative electrode current collector copper foil, and then dried, cold pressed and cut to obtain the negative electrode sheet.
[0230] (4) Preparation of electrolyte
[0231] At 25°C, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a mixed solvent, and then LiPF6 is dissolved in the above mixed solvent to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0232] (5) Preparation of secondary batteries
[0233] The positive electrode sheets, separators, and negative electrode sheets are stacked in sequence, wound, and cold-pressed (during which the separators and the electrodes are bonded) to obtain a battery cell; the battery cell is placed in an outer package, and the above-prepared electrolyte is added. After packaging, standing, formation, aging, and other processes, a secondary battery is obtained.
[0234] Performance Testing
[0235] (1) Cold press adhesion test steps
[0236] The battery negative electrode and separator were stacked together and placed on a hot press. Pressing parameters were set at 25°C, 7t, and 15s to produce a bonded separator / negative electrode sample. The separator / electrode sample was cut into 150mm x 20mm rectangular strips. The electrode side of the strip was affixed to a steel plate using double-sided tape. At one end of the strip, the separator and electrode were separated by 2cm along the length to produce the test specimen.
[0237] The steel plate was held horizontally and secured with the lower clamp of a universal testing machine (Xie Qiang Instrument Manufacturing (Shanghai) Co., Ltd., Model CTM2100). The peeled end of the separator, as described above, was secured with the upper clamp of the universal testing machine and connected to a tensile testing machine. The test conditions were set to a tensile rate of 20 mm / min and a horizontal pull of 10 cm. Once the tension stabilized, the force was recorded. The ratio of the force to the sample width was used to determine the adhesion strength between the separator and the electrode.
[0238] (2) Battery cell hardness test steps
[0239] Place the battery cell on a table with both ends level, with a 12cm wide hollowed-out area in the middle. Allow the cell to lie naturally flat and measure the deviation of the cell center from the horizontal reference line to assess the cell's hardness. The greater the deviation of the cell center from the horizontal reference line, the lower the cell's hardness.
[0240] (3) Large fixture cycle performance test steps
[0241] A clamping force of 10,000 N was applied to the battery cell, and a cycling test was performed under this condition. The test steps were as follows: At 25°C, the battery prepared in Example 1 was charged at a constant current of 1 / 3C to 3.8V, then charged at a constant voltage of 3.8V to a current of 0.05C, left for 5 minutes, and then discharged at 1 / 3C to 2.0V. The resulting discharge capacity was recorded as the initial capacity C0. The above steps were repeated for the same battery, and the discharge capacity Cn of the battery after the nth cycle was recorded. The battery capacity retention rate after each cycle, Pn, = (Cn / C0) × 100%. The battery capacity retention rate after 500 cycles can be used to reflect the difference in cycling performance.
[0242] Table 1 Preparation parameters of adhesive and bonding layer
[0243] Table 2 Battery Performance
[0244] Table 3 Adhesive parameters
[0245] From the above data, it can be seen that the adhesive based on the ring structure has a larger contact area with the diaphragm and the electrode, and better bonding performance can be achieved while reducing the amount of adhesive used in the ring structure.
[0246] The above is only a preferred embodiment of the present application and does not limit the patent scope of the present application. All equivalent structural transformations made based on the contents of the present application specification and drawings, or direct / indirect application in other related technical fields, are included in the patent protection scope of the present application.
Claims
1. A binder for a secondary battery, in, The adhesive includes an acrylic copolymer, and the shape of the adhesive includes a ring shape.
2. The binder for secondary batteries according to claim 1, in, The specific surface area of the binder is in the range of 0.4 m 2 / g to 1.2m 2 / g, preferably, the specific surface area of the binder is in the range of 0.6m 2 / g to 0.9m 2 / g.
3. The binder for secondary batteries according to claim 1 or 2, in, The ratio of the surface area to volume of the binder is 0.1×10 6 m -1 Up to 20×10 6 m -1 Preferably, the ratio of the surface area to volume of the binder is 0.5×10 6 m -1 Up to 16×10 6 m -1 .
4. The secondary battery binder according to any one of claims 1 to 3, in, The bulk density of the binder is in the range of 0.3 g / cm 3 Up to 0.8g / cm 3 Preferably, the bulk density of the binder is in the range of 0.4 g / cm 3 Up to 0.7g / cm 3 .
5. The secondary battery binder according to any one of claims 1 to 4, in, The shape of the adhesive includes a ring shape.
6. The secondary battery binder according to any one of claims 1 to 5, in, The volume particle size distribution Dv50 of the binder is in the range of 1 μm to 15 μm. Preferably, the volume particle size distribution Dv50 of the binder is in the range of 3 μm to 12 μm.
7. The binder for secondary batteries according to any one of claims 1 to 6, in, The constituent monomers of the acrylic ester copolymer include a first polymerizable monomer, and the structure of the first polymerizable monomer includes: Among them, R1 includes hydrogen or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.
8. The binder for secondary batteries according to claim 7, in, The first polymerizable monomer includes one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.
9. The binder for secondary batteries according to any one of claims 1 to 8, in, The constituent monomers of the acrylic ester copolymer include a second polymerizable monomer, and the structure of the second polymerizable monomer includes: Wherein, R3 includes hydrogen or an alkyl group of 1 to 6 carbon atoms.
10. The binder for secondary batteries according to claim 9, in, The second polymerizable monomer includes one or more of acrylic acid, methacrylic acid, butenoic acid, and heptenoic acid.
11. The secondary battery binder according to any one of claims 1 to 10, in, The constituent monomers of the acrylic ester copolymer include a third polymerizable monomer, and the structure of the third polymerizable monomer includes: Here, R4 includes a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
12. The binder for secondary batteries according to claim 11, in, The third polymerizable monomer includes one or more of acrylonitrile and methacrylonitrile.
13. The secondary battery binder according to any one of claims 1 to 12, in, The monomers constituting the acrylic ester copolymer include a fourth polymerizable monomer, and the structure of the fourth polymerizable monomer includes: Among them, R5 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R6 includes a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.
14. The binder for secondary batteries according to claim 13, in, The fourth polymerizable monomer includes one or more of acrylamide, N-hydroxymethyl acrylamide and N-butoxymethyl acrylamide.
15. The secondary battery binder according to any one of claims 1 to 14, in, The constituent monomers of the acrylic ester copolymer include a first polymerized monomer, a second polymerized monomer, a third polymerized monomer and a fourth polymerized monomer, and the mass ratio of the first polymerized monomer, the second polymerized monomer, the third polymerized monomer and the fourth polymerized monomer is 1: (0.01-0.8): (0.01-0.5): (0.01-0.3), preferably, the mass ratio of the first polymerized monomer, the second polymerized monomer, the third polymerized monomer and the fourth polymerized monomer is 1: (0.1-0.5): (0.15-0.45): (0.1-0.22).
16. A diaphragm, in, The separator includes a substrate and an adhesive layer provided on at least one side of the substrate, wherein the adhesive layer includes the binder for a secondary battery according to any one of claims 1 to 15.
17. The diaphragm according to claim 16, in, The surface density of the bonding layer on the substrate is in the range of 0.7 g / m 2 Up to 3g / m 2 Preferably, the surface density of the adhesive layer on the substrate is in the range of 0.8 g / m 2 Up to 2g / m 2 .
18. A secondary battery, in, The secondary battery includes the separator according to claim 16 or 17.
19. An electrical device, in, The electric device comprises the secondary battery as claimed in claim 18.
Citation Information
Patent Citations
Hollow microsphere and its preparation method
CN102764616A
Aqueous adhesive for lithium ion secondary battery
CN103509500A
Acrylonitrile binder powder and preparation method thereof
CN114736632A
Pressure-sensitive adhesive comprising hollow tacky microspheres and macromonomer-containing binder copolymer
US4994322A