Positive electrode composite material and preparation method therefor, positive electrode sheet, and battery
By forming a coherent phase boundary coating layer on the surface of the high-nickel layered cathode material, the problem of poor electrode/electrolyte interface stability is solved, the battery cycle performance is improved, side reactions are suppressed, and the battery life is extended.
Patent Information
- Application Number
- PCT/CN2023/114169
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2023-08-22
- Publication Date
- 2024-10-31
AI Technical Summary
In practical applications, high-nickel layered cathode materials have poor electrode/electrolyte interface stability, leading to side reactions and structural failure. The existing inert coating layer is easy to dissociate during the charge and discharge process, and cannot effectively solve the interface stability and structural stability. question.
Using a cathode composite material with a coherent phase boundary, a coating layer with good electrochemical activity is formed on the surface of the high-nickel layered cathode material, and a topological transformation reaction is used to prepare the coherent coating layer to ensure that the connection between the coating layer and the bulk material is Chemical combination to improve interface stability and structural stability.
It effectively reduces battery capacity loss, inhibits the side reaction between Ni4+ and electrolyte, extends battery cycle life, reduces battery gas production, and improves battery cycle performance.
Smart Images

Figure CN2023114169_31102024_PF_FP_ABST
Abstract
Description
Positive electrode composite material and preparation method thereof, positive electrode sheet and battery
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application number 202310452631.6 filed with the State Intellectual Property Office of China on April 25, 2023, entitled “Positive electrode composite material, preparation method thereof, positive electrode sheet and battery,” the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The present application relates to the technical field of lithium batteries, and in particular to a positive electrode composite material and a preparation method thereof, a positive electrode sheet and a battery. Background Art
[0004] Under the background of carbon neutrality, the rapid development of the new energy vehicle industry has driven the rapid growth of power lithium-ion batteries.
[0005] High nickel layered cathode materials have the advantages of high gram capacity, excellent cycle performance and low production cost, which can achieve a single charge mileage of more than 300km for electric vehicles and have received widespread attention in the market. High nickel layered cathode materials are usually faced with complex electrode / electrolyte interface problems in actual application: on the one hand, the residual lithium compounds such as LiOH and Li2CO3 on the surface of the high nickel layered cathode material are relatively high, which easily aggravates the gelation and gas production of the electrode slurry; on the other hand, when the high nickel layered cathode material is in a high charge state, the H2→H3 phase transition causes the crystal structure to anisotropically shrink or expand, and mechanical stress is continuously accumulated at the grain boundaries, inducing microcracks and particle breakage. The electrolyte will penetrate into the active particles along the cracks, aggravating the high activity Ni in the high nickel layered cathode material. 4+ The side reactions with the electrolyte eventually lead to the failure of the high-nickel layered positive electrode material.
[0006] By preparing a coating layer on the surface of the high nickel layered cathode material (also known as the bulk material), the high nickel layered cathode material can be separated from the electrolyte to reduce the reactivity between the two. In the highly delithiation state, the coating layer can also prevent the highly oxidized Ni 4+ The irreversible phase transition from layered to disordered spinel and rock salt structures caused by electrolyte side reactions improves the cycle life of the positive electrode material. However, current coating materials are electrochemically inert compounds or, although the coating materials have electrochemical properties, the coating material and the bulk material are physically bonded and easily dissociate or fall off during charge and discharge. Therefore, the interface stability between the bulk material and the electrolyte is still poor.
[0007] Summary of the Invention
[0008] Based on this, the present application provides a positive electrode composite material and a preparation method thereof, a positive electrode sheet and a battery, which are used to solve the problem of poor interface stability and structural stability between the coating layer and the main material in the related art.
[0009] In a first aspect, a positive electrode composite material is provided, comprising a bulk material and a coating layer;
[0010] The bulk material includes the general formula Li w Ni a Co b Mn c X 1-a-b-c O2 material, wherein X includes one or more of Al, Ti, Zr, Mg and W, and 0.95≤w≤1.1, 0.6≤a≤1, b≥0, and c≥0;
[0011] The general formula of the coating material includes Li α Ni β Co γ Mn δ O2 materials, wherein 0 < α ≤ 1, 0 ≤ β ≤ 0.6, 0 ≤ γ ≤ 1, 0 ≤ δ ≤ 1, and β, γ, and δ are not all 0 at the same time;
[0012] The interface between the bulk material and the cladding layer is a coherent phase boundary.
[0013] Optionally, in the crystal structures of the bulk material and the coating layer material, oxygen ions are closely packed structures;
[0014] and / or,
[0015] The material of the coating layer belongs to one or more space groups of Fd-3m, Fm-3m, R-3m and C2 / m.
[0016] Optionally, the thickness of the coating layer is ≤200 nm.
[0017] In a second aspect, a method for preparing the positive electrode composite material according to the first aspect is provided, comprising:
[0018] preparing or providing the bulk material;
[0019] The bulk material is mixed with a coating additive, and the positive electrode composite material is prepared through a topological conversion reaction.
[0020] Optionally, the bulk material is mixed with a coating additive, and the cathode composite material is prepared by a topoconversion reaction, comprising:
[0021] Mixing the bulk material and the coating additive;
[0022] calcining the mixed two materials in steps to prepare the positive electrode composite material;
[0023] The stepwise calcination includes two steps, wherein the first step calcination temperature is 400-600°C and the time is 1-5 hours; the second step calcination temperature is 600-800°C and the time is 3-10 hours, and the atmosphere of the stepwise calcination is an oxygen-containing atmosphere.
[0024] The coating additive includes a first precursor and a reaction aid, wherein the first precursor includes: Ni x Co y Mn z (OH)2、Ni x Co y Mn z OOH、Ni x Co y Mn z O, wherein 0≤x≤0.6, 0≤y≤1, 0≤z≤1, and x, y and z are not 0 at the same time; the reaction auxiliary agent includes one or more of lithium carbonate, lithium oxide and lithium hydroxide;
[0025] Optionally, in the stepwise calcination, the first precursor has an oxygen close-packed structure, and the space group includes one or more of Fd-3m, Fm-3m, R-3m and C2 / m;
[0026] Optionally, the first precursor satisfies one of the following conditions:
[0027] (1) The specific surface area of the first precursor is ≥ 20m 2 / g;
[0028] (2) the molar ratio of the first precursor to the bulk material is 0.5 mol% to 10 mol%;
[0029] (3) The total number of metal atoms in the first precursor is M, the total number of residual lithium atoms in the reaction aid and the bulk material is L, and the M and L satisfy 0.8 <L / M<1.2。
[0030] Optionally, preparing the bulk material comprises:
[0031] In an oxygen-containing atmosphere, a high-nickel material precursor and a lithium salt are mixed, calcined at a high temperature, cooled with the furnace, and crushed and sieved;
[0032] Optionally, the preparation of the bulk material satisfies at least one of the following conditions:
[0033] (1) The high nickel material precursor includes: one or more of oxides and hydroxides;
[0034] (2) The lithium salt includes one or more of lithium carbonate and lithium hydroxide;
[0035] (3) The molar ratio of lithium atoms in the high nickel material precursor and the reaction aid is 1.0:(0.9-1.1);
[0036] (4) The heating rate is 2-8°C / min, the calcination temperature is 700-1100°C, and the calcination time is 12h-24h.
[0037] In a third aspect, a positive electrode sheet is provided, comprising: a positive electrode current collector, and a positive electrode material layer formed on at least one surface of the positive electrode current collector;
[0038] The positive electrode material layer includes the positive electrode composite material as described in the first aspect or the positive electrode composite material prepared by the preparation method as described in the second aspect.
[0039] In a fourth aspect, a battery is provided, comprising: the positive electrode sheet as described in the third aspect.
[0040] Compared with the prior art, this application has the following beneficial effects:
[0041] By forming a coating layer on the surface of the high-nickel layered positive electrode material (i.e., the main material), since the coating layer has good electrochemical activity, the battery capacity loss caused by the inert coating layer in the related art can be effectively reduced. At the same time, since the interface between the main material and the coating layer is a coherent phase boundary, on the one hand, the coating layer and the main material are chemically bonded, and therefore, the bonding stability between the coating layer and the main material can be effectively improved; on the other hand, the interface between the two is a coherent phase boundary, which can effectively improve the interface stability and structural stability between the coating layer and the main material. Therefore, the coating layer can relieve the stress accumulation of the high-nickel layered positive electrode material during the battery cycle, avoid direct contact between the high-nickel layered positive electrode material and the electrolyte, thereby effectively inhibiting the Ni on the surface of the high-nickel layered positive electrode material. 4+ The side reactions between the coating and the electrolyte can effectively improve the battery cycle performance. On the other hand, the formation of the coating can consume the residual lithium compounds on the surface of the high-nickel layered positive electrode material, thereby reducing the residual lithium compounds on the surface of the high-nickel layered positive electrode material and effectively reducing battery gas production. This solves the problem of poor interface stability and structural stability between the coating layer and the main material in related technologies. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] FIG1 is an ex-situ XRD pattern of a high-nickel layered cathode material at different temperatures in the S3 process provided in an embodiment of the present application;
[0043] FIG2 is a comparison chart of the specific capacity of uncoated and coated Example 1 as a function of the number of cycles provided in the examples of the present application;
[0044] FIG3 is a comparison diagram of differential scanning calorimetry curves of Example 1 before and after coating provided in the examples of the present application. DETAILED DESCRIPTION
[0045] The present invention will be further described in detail below with reference to specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, the purpose of providing these embodiments is to provide a more thorough and comprehensive understanding of the present invention.
[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are intended only to describe specific embodiments and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0047] The determination of surface residual alkali in this patent is carried out in accordance with GB / T 41704-2022.
[0048] Based on the above technical problems, some embodiments of the present application provide a positive electrode composite material, including: a main body material and a coating layer; the main body material includes a general formula Li w Ni a Co b Mn c X 1-a-b-c O2 material, wherein X includes one or more of Al, Ti, Zr, Mg and W, and 0.95≤w≤1.1, 0.6≤a≤1, b≥0, c≥0; the material formula of the coating layer is Li α Ni β Co γ Mn δ O2, wherein 0<α≤1, 0≤β≤0.6, 0≤γ≤1, 0≤δ≤1, and β, γ and δ are not 0 at the same time; the interface between the bulk material and the coating layer is a coherent phase boundary.
[0049] Among them, the above-mentioned main material is a high-nickel layered positive electrode material, and the material of the coating layer is a low-nickel material. At the same time, since the material of the coating layer contains elements with good electrochemical activity such as Ni, Co and / or Mn, the material of the coating layer has higher electrochemical activity.
[0050] Most crystalline materials are composed of many grains. The interface between grains that belong to the same solid phase but are in different phases is called a grain boundary. In a crystal structure, if the structures between two grains are different, we call it: the two grains with different structures have different crystal phases, and the interface between two phases with different structures is called a phase boundary. A coherent phase boundary means that the atoms on the interface are simultaneously located at the nodes of the two phase lattices, that is, the lattices of the two phases are connected to each other, and the atoms on the interface are shared by both. Here, the interface between the bulk material and the coating is a coherent phase boundary, which means that the crystal structures of the bulk material and the coating are different, and the atoms on the interface of the two different crystal structures are shared by the bulk material and the coating.
[0051] In the positive electrode composite material provided in the embodiment of the present application, a coating layer is formed on the surface of the high-nickel layered positive electrode material (i.e., the main material). Since the coating layer has good electrochemical activity, the battery capacity loss caused by the use of an inert coating layer in the related art can be effectively reduced. At the same time, since the interface between the main material and the coating layer is a coherent phase boundary, on the one hand, the coating layer and the main material are chemically bonded, and therefore, the bonding stability between the coating layer and the main material can be effectively improved; on the other hand, the interface between the two is a coherent phase boundary, which can effectively improve the interface stability and structural stability between the coating layer and the main material. Therefore, the coating layer can relieve the stress accumulation of the high-nickel layered positive electrode material during the battery cycle, avoid direct contact between the high-nickel layered positive electrode material and the electrolyte, thereby effectively inhibiting the Ni on the surface of the high-nickel layered positive electrode material. 4+ The side reactions between the coating and the electrolyte can effectively improve the battery cycle performance. On the other hand, the formation of the coating can consume the residual lithium compounds on the surface of the high-nickel layered positive electrode material, thereby reducing the residual lithium compounds on the surface of the high-nickel layered positive electrode material and effectively reducing battery gas production. This solves the problem of poor interface stability and structural stability between the coating layer and the main material in related technologies.
[0052] In some embodiments, in the crystal structures of the bulk material and the coating layer, the oxygen ions are closely packed; and / or, the space group of the coating layer is one or more of Fd-3m, Fm-3m, R-3m or C2 / m.
[0053] The space group of the coating layer is one or more of Fd-3m, Fm-3m, R-3m or C2 / m, so that the interface between the coating layer and the bulk material can be a coherent phase boundary.
[0054] In some embodiments, the thickness of the coating layer is ≤ 200 nm.
[0055] In these embodiments, by controlling the thickness of the coating layer to ≤200 nm, the coating layer can be coated on the surface of the base material in a thin and uniform manner, which can not only protect the high-nickel layered positive electrode material from electrolyte invasion and inhibit side reactions, but also reduce the hindrance to the diffusion of lithium during the insertion and extraction process.
[0056] Some embodiments of the present application provide a method for preparing the positive electrode composite material as described above, comprising:
[0057] Prepare or provide bulk materials;
[0058] The bulk material is mixed with a coating additive, and a positive electrode composite material is prepared through a topological conversion reaction.
[0059] A topological chemical reaction refers to a chemical reaction in which the structure of the product is related to the structure of the reactant, and the reaction can proceed while maintaining a certain crystal structure of the reactant.
[0060] In the preparation method of the positive electrode composite material provided in the embodiment of the present application, on the one hand, the residual lithium compounds on the surface of the high-nickel layered positive electrode material can be used to in situ generate a coherent coating layer with a good stable structure, thereby effectively reducing the residual lithium compounds on the surface of the bulk material and reducing battery gas production; in addition, by using coating additives containing elements with high electrochemical activity such as Ni, Co, and Mn, the higher reaction activity can more effectively consume the residual lithium compounds on the surface of the bulk material; on the other hand, in the multi-step topological chemical reaction, with the help of the synergistic effect of the first precursor and the reaction aid, the secondary calcination mode is regulated, and the topological transformation of the continuous dense packing structure of oxygen ions is realized. The eutectic lattice growth of the coating layer on the surface of the primary calcination product A is achieved, reducing the diffusion effect of metal ions to the bulk phase, and the coherent coating layer finally obtained can effectively improve the interface stability and structural stability between the coating layer and the bulk material, thereby alleviating the stress accumulation of the high-nickel layered positive electrode material during the battery cycle, avoiding direct contact between the high-nickel layered positive electrode material and the electrolyte, thereby effectively inhibiting the Ni on the surface of the high-nickel layered positive electrode material. 4+ The side reaction between the electrolyte and the electrolyte can effectively improve the battery cycle performance.
[0061] In some embodiments, the bulk material is mixed with the coating additive, and the cathode composite material is prepared by a topoconversion reaction, comprising:
[0062] Mixing the bulk material and the coating additive;
[0063] The mixed two materials are calcined step by step to prepare the positive electrode composite material.
[0064] Among them, there is no specific limitation on the specific spatial structure and calcination conditions of the above-mentioned coating additives in the calcination step, as long as the residual lithium compounds of the coating additives and the main material can undergo a multi-step topological transformation based on the oxygen dense packing structure during the entire calcination process to generate a coherent coating layer coated with the high-nickel layered positive electrode material.
[0065] The stepwise calcination includes two steps, wherein the first step calcination temperature is 400-600°C and the time is 1-5 hours; the second step calcination temperature is 600-800°C and the time is 3-10 hours, and the atmosphere of the stepwise calcination is an oxygen-containing atmosphere.
[0066] In these embodiments, by controlling the first precursor to have an oxygen close-packed structure during the step-by-step calcination, with space groups including one or more of Fd-3m, Fm-3m, R-3m, and C2 / m, the coating layer can form a coherent phase boundary with the bulk material in the form of a shared oxygen lattice, thereby forming a coherent coating layer. By limiting the temperature and time of the step-by-step calcination to within the aforementioned ranges, the residual lithium compound on the surface of the coating additive and the bulk material can undergo a multi-step topological transformation based on the oxygen close-packed structure, resulting in a coherent coating layer with excellent performance.
[0067] The oxygen-containing atmosphere may include one or more of oxygen and dry air.
[0068] In some embodiments, the coating additive includes a first precursor and a reaction aid, wherein the first precursor includes: Ni x Co y Mn z (OH)2、Ni x Co y Mn z OOH、Ni x Co y Mn z O, wherein 0≤x≤0.6, 0≤y≤1, 0≤z≤1, and x, y and z are not 0 at the same time, and the reaction auxiliary agent includes one or more of lithium oxide, lithium carbonate and lithium hydroxide.
[0069] In some embodiments, the first precursor satisfies one of the following conditions:
[0070] (1) The specific surface area of the first precursor is ≥ 20m 2 / g;
[0071] (2) the molar ratio of the first precursor to the bulk material is 0.5 mol% to 10 mol%;
[0072] (3) The total number of metal atoms in the first precursor is M, and the total number of residual lithium atoms in the reaction assistant and the bulk material is L, where M and L satisfy 0.8 < L / M < 1.2.
[0073] In these embodiments, the particle size of the above first precursor can be in the micron range. Thus, the integrity of the coating layer preparation can be effectively improved. By controlling the molar ratio of the first precursor to the bulk material to be 0.5:100 to 10:100, the components and content of the coating layer can be optimized; by controlling the total number of lithium atoms in the reaction assistant and the residual lithium atoms in the bulk material to be L, and the total number of metal atoms of the first precursor to be M, such that 0.8 < L / M < 1.2, the topochemical reaction can be made complete and controllable, thereby ensuring the smooth progress of the multi-step topochemical reaction and the generation of coherent phase boundaries.
[0074] In some embodiments, preparing the bulk material includes:
[0075] Mixing a high-nickel material precursor and a lithium salt in an oxygen-containing atmosphere, heating to calcine and then cooling with the furnace, and performing crushing and sieving treatments;
[0076] Optionally, preparing the bulk material satisfies one of the following conditions:
[0077] (1) The high-nickel material precursor includes one or more of oxides and hydroxides;
[0078] (2) The lithium salt includes one or more of lithium carbonate and lithium hydroxide;
[0079] (3) The molar ratio of lithium atoms in the high-nickel material precursor to those in the reaction assistant is 1.0:(0.9 - 1.1);
[0080] (4) The heating rate is 2 - 8 °C / min, the calcination temperature is 700 - 1100 °C, and the time is 12 h - 24 h.
[0081] Some embodiments of the present application provide a positive electrode sheet, which includes a positive electrode current collector and a positive electrode material layer formed on the positive electrode current collector. The positive electrode material layer includes the positive electrode composite material as described above or the positive electrode composite material prepared by the preparation method as described above.
[0082] The beneficial technical effects of the positive electrode sheet provided by the embodiments of the present application are the same as those of the positive electrode composite material provided by the embodiments of the present application, and will not be elaborated here.
[0083] Some embodiments of the present application provide a battery, including the positive electrode sheet as described above.
[0084] Among them, the battery exemplified can be a lithium-ion battery.
[0085] The beneficial technical effects of the battery provided in the embodiment of the present application are the same as the beneficial technical effects of the high-nickel positive electrode composite material modified based on the topological transformation reaction provided in the embodiment of the present application, and will not be repeated here.
[0086] In order to objectively evaluate the technical effects of the embodiments of the present application, the present application will be described in detail and exemplarily through embodiments and comparative examples below.
[0087] In the following examples and comparative examples, all raw materials can be purchased commercially, and in order to maintain the reliability of the experiments, the raw materials used in the following examples and comparative examples have the same physical and chemical parameters or have undergone the same treatment.
[0088] Example 1
[0089] S1, 1000g of Ni 0.92 Co 0.04 Mn 0.03 Al 0.01 (OH)2(D50 is 3.5μm, specific surface area is 20m 2 / g) and 470g LiOH·H2O were mixed uniformly in a high-speed mixer. The mixture was placed in an oxygen atmosphere furnace and heated to 810°C at a heating rate of 3°C / min. After holding for 15 hours, the mixture was cooled in the furnace and crushed and sieved to obtain an uncoated and modified primary calcined product (i.e., the above-mentioned bulk material). The residual lithium compound content on the surface of the primary calcined product was tested, and the content of LiOH in the residual lithium compound in the primary calcined product was 5200ppm, and the content of Li2CO3 in the primary calcined product was 2700ppm. Both tests were performed in accordance with national standards.
[0090] S2, 500g of the primary calcined product, 1.675g of Li2O, 23.390g of the first precursor Co 0.5 Mn 0.5 (OH)2(specific surface area 25m 2 / g) were mixed evenly to obtain the second mixed material, wherein Co 0.5 Mn 0.5 The amount of (OH)2 meets the following requirements: Co 0.5 Mn 0.5 The molar ratio of (OH)2 to the primary calcined product is 5:100. The first precursor Co 0.5 Mn 0.5 The number of metal atoms in (OH)2 is M, the total number of lithium atoms in the reaction aid Li2O and the residual lithium in the primary calcination product is L, and L / M is 1.0.
[0091] S3, the above two mixed materials were calcined again in oxygen in steps, wherein the first step calcination temperature I was 450 ° C, the time was 2 h; the second step calcination temperature II was 720 ° C, the time was 8 h, and the calcination was completed and the furnace was cooled to obtain the coated modified LiNi 0.92 Co 0.04 Mn 0.03 Al 0.01 O2 material, expressed in chemical formula as 0.05LiCo 0.5 Mn 0.5 O2@LiNi 0.92 Co 0.04 Mn 0.03 Al 0.01 O2.
[0092] Example 2
[0093] S1, 1000g of Ni 0.90 Co 0.06 Mn 0.03 Al 0.01 (OH)2(D50 is 13.0μm, specific surface area is 6m 2 / g) and 455g of LiOH·H2O were mixed uniformly in a high-speed mixer. The mixture was placed in an oxygen atmosphere furnace and heated to 775°C at a rate of 4°C / min. After holding for 16 hours, the mixture was cooled in the furnace and crushed and sieved to obtain an uncoated and modified primary calcined product. The residual lithium compound content on the surface of the primary calcined product was measured, and the content of LiOH·H2O in the residual lithium compound in the primary calcined product was 4800ppm, and the content of Li2CO3 in the primary calcined product was 3700ppm.
[0094] S2, 500g of the primary calcined product was mixed with 0.170g of LiOH·H2O, 11.820g of the first precursor CoOOH (specific surface area of 55m 2 / g) were uniformly mixed to obtain a second mixture, wherein the amount of CoOOH satisfied: the molar ratio of CoOOH to the primary calcined product was 2.5:100, the number of metal atoms of the first precursor CoOOH was M, the total number of lithium atoms of the reaction aid LiOH·H2O and the residual lithium in the primary calcined product was L, and L / M was 1.1.
[0095] S3, the above two mixed materials are calcined again in oxygen in steps, wherein the first step calcination temperature I is 450 ° C, the time is 3 h; the second step calcination temperature II is 750 ° C, the time is 6 h, and after the calcination is completed, the furnace is cooled to obtain the coated modified LiNi 0.90 Co 0.06 Mn 0.03 Al 0.01 O2 material, expressed as 0.025Li by chemical formula0.9 CoO2@Li 1.005 Ni 0.90 Co 0.06 Mn 0.03 Al 0.01 O2.
[0096] Example 3
[0097] S1, 1000g of Ni 0.92 Co 0.05 Mn 0.02 Zr 0.01 (OH)2(D50 is 3.3μm, and the specific surface area is 18m 2 / g) and 450g of LiOH·H2O were mixed uniformly in a high-speed mixer. The mixture was placed in an oxygen atmosphere furnace and heated to 700°C at a rate of 2°C / min. After holding for 12 hours, the mixture was cooled in the furnace and crushed and sieved to obtain an uncoated and modified primary calcined product. The residual lithium compound content on the surface of the primary calcined product was measured, and the content of LiOH·H2O in the residual lithium compound in the primary calcined product was 5300ppm, and the content of Li2CO3 in the primary calcined product was 3700ppm.
[0098] S2, 500g of the primary calcined product and 11.614g of the first precursor Co 0.33 Ni 0.33 Mn 0.33 (OH)2(specific surface area is 30m 2 / g) were mixed evenly to obtain the second mixture, without adding reaction aids, wherein Co 0.33 Ni 0.33 Mn 0.33 The amount of (OH)2 meets the following requirements: Co 0.33 Ni 0.33 Mn 0.33 The molar ratio of (OH)2 to the primary calcined product is 2.5:100. The first precursor Co 0.33 Ni 0.33 Mn 0.33 The number of metal atoms in (OH)2 is M, the number of lithium atoms in the residual lithium in the primary calcination product is L, and L / M is 1.1.
[0099] S3, the above two mixed materials are calcined again in oxygen in steps, wherein the first step calcination temperature I is 400 ° C, the time is 4h; the second step calcination temperature II is 800 ° C, the time is 10h, and after the calcination is completed, the furnace is cooled to obtain the coated modified LiNi 0.92 Co 0.05 Mn 0.02 Zr 0.01 O2 material, expressed as 0.025Li by chemical formula 0.7Co 0.33 Ni 0.33 Mn 0.33 O2@Li 0.95 Ni 0.92 Co 0.05 Mn 0.02 Zr 0.01 O2.
[0100] Example 4
[0101] S1, 1000g of Ni 0.83 Co 0.11 Mn 0.05 W 0.01 (OH)2(D50 is 10.5μm, specific surface area is 8m 2 / g) and 480g of LiOH·H2O were mixed uniformly in a high-speed mixer. The mixture was placed in an oxygen atmosphere furnace and heated to 1100°C at a rate of 8°C / min. After holding for 24 hours, the mixture was cooled in the furnace and crushed and sieved to obtain an uncoated and modified primary calcined product. The residual lithium compound content on the surface of the primary calcined product was measured, and the content of LiOH·H2O in the residual lithium compound in the primary calcined product was 5400ppm, and the content of Li2CO3 in the primary calcined product was 5200ppm.
[0102] S2, 500g of the primary calcined product, 0.292g of Li2O, 23.002g of the first precursor Co 0.5 Mn 0.5 (OH)2(specific surface area 25m 2 / g) were mixed evenly to obtain the second mixed material, wherein Co 0.5 Mn 0.5 The amount of (OH)2 meets the following requirements: Co 0.5 Mn 0.5 The molar ratio of (OH)2 to the primary calcined product is 5:100. The first precursor Co 0.5 Mn 0.5 The number of metal atoms in (OH)2 is M, the total number of lithium atoms in the reaction aid Li2O and the residual lithium in the primary calcination product is L, and L / M is 0.85.
[0103] S3, the above two mixed materials were calcined again in oxygen in steps, wherein the first step calcination temperature I was 600 ° C, the time was 5h; the second step calcination temperature II was 600 ° C, the time was 3h, and after the calcination was completed, the modified LiNi was obtained by cooling in the furnace. 0.83 Co 0.11 Mn 0.05 W 0.01 O2 material, expressed as 0.05Li by chemical formula 0.85 Co 0.5Mn 0.5 O2@LiNi 0.83 Co 0.11 Mn 0.05 W 0.01 O2.
[0104] Example 5
[0105] S1, 1000g of Ni 0.68 Co 0.12 Mn 0.195 Al 0.005 (OH)2(D50 is 3.8μm, and the specific surface area is 22m 2 / g) and 495g of LiOH·H2O were mixed uniformly in a high-speed mixer. The mixture was then placed in a dry air atmosphere furnace and heated to 920°C at a rate of 4°C / min. After holding for 18 hours, the mixture was cooled in the furnace and crushed and sieved to obtain an uncoated and modified primary calcined product. The residual lithium compound content on the surface of the primary calcined product was measured, and the content of LiOH in the residual lithium compound in the primary calcined product was 3700ppm, and the content of Li2CO3 in the primary calcined product was 2900ppm.
[0106] S2, 500g of the primary calcined product was mixed with 7.523g of Li2O, 48.026g of the first precursor Co(OH)2 (specific surface area of 35m 2 / g) are mixed uniformly to obtain a second mixture, wherein the amount of Co(OH)2 satisfies: the molar ratio of Co(OH)2 to the primary calcined product is 10:100, the number of metal atoms of the first precursor Co(OH)2 is M, the total number of lithium atoms of the reaction aid Li2O and the residual lithium in the primary calcined product is L, and L / M is 1.1.
[0107] S3, the above two mixed materials were calcined again in dry air in steps, wherein the first step calcination temperature I was 500 ° C, the time was 1 h; the second step calcination temperature II was 600 ° C, the time was 3 h, and after the calcination was completed, the furnace was cooled to obtain the coated modified LiNi 0.68 Co 0.12 Mn 0.195 Al 0.005 O2 material, expressed as 0.1Li by chemical formula 0.3 CoO2@Li 1.08 Ni 0.68 Co 0.12 Mn 0.195 Al 0.005 O2.
[0108] Example 6
[0109] S1, 1000g of Ni 0.90 Co0.05 Mn 0.04 Mg 0.01 (OH)2(D50 is 3.0μm, specific surface area is 25m 2 / g) and 455g of LiOH·H2O were mixed uniformly in a high-speed mixer. The mixture was then placed in a dry air atmosphere furnace and heated to 800°C at a rate of 5°C / min. The mixture was held at this temperature for 15 hours, then cooled in the furnace, crushed, and sieved to obtain an uncoated and modified primary calcined product. The residual lithium compound content on the surface of the primary calcined product was measured, and the content of LiOH·H2O in the residual lithium compound in the primary calcined product was 6200ppm, and the content of Li2CO3 in the primary calcined product was 4200ppm.
[0110] S2, 500g of the primary calcined product was mixed with 4.493g of LiOH·H2O, 27.765g of the first precursor Co 0.5 Mn 0.5 OOH (specific surface area 30m 2 / g) were mixed evenly to obtain the second mixed material, wherein Co 0.5 Mn 0.5 The amount of OOH meets the following requirements: 0.5 Mn 0.5 The molar ratio of OOH to the primary calcined product is 6:100. The first precursor Co 0.5 Mn 0.5 The number of metal atoms in OOH is M, the total number of lithium atoms in the reaction aid LiOH·H2O and the residual lithium in the primary calcined product is L, and L / M is 0.95.
[0111] S3, the above two mixed materials were calcined again in dry air in steps, wherein the first step calcination temperature I was 450 ° C, the time was 5 h; the second step calcination temperature II was 750 ° C, the time was 8 h, and after the calcination was completed, the modified LiNi was obtained by cooling the furnace. 0.90 Co 0.05 Mn 0.04 Mg 0.01 O2 material, expressed as 0.06Li by chemical formula 0.45 Co 0.5 Mn 0.5 O2@Li 1.03 Ni 0.90 Co 0.05 Mn 0.04 Mg 0.01 O2.
[0112] Example 7
[0113] S1, 1000g of Ni 0.88 Co 0.06 Mn 0.05Zr 0.01 (OH)2(D50 is 8.5μm, specific surface area is 22m 2 / g) and 480g of LiOH·H2O were mixed uniformly in a high-speed mixer. The mixture was placed in a dry air atmosphere furnace and heated to 815°C at a rate of 5°C / min. After holding for 15 hours, the mixture was cooled in the furnace and crushed and sieved to obtain an uncoated and modified primary calcined product. The residual lithium compound content on the surface of the primary calcined product was measured, and the content of LiOH·H2O in the residual lithium compound in the primary calcined product was 6400ppm, and the content of Li2CO3 in the primary calcined product was 5500ppm.
[0114] S2, 500g of the primary calcined product was mixed with 5.755g of LiOH·H2O, 27.974g of the first precursor Co 0.33 Ni 0.33 Mn 0.33 O(specific surface area is 35m 2 / g) were mixed evenly to obtain the second mixed material, wherein Co 0.33 Ni 0.33 Mn 0.33 The amount of O meets the following requirements: 0.33 Ni 0.33 Mn 0.33 The molar ratio of O to the primary calcined product is 7.5:100. The first precursor Co 0.33 Ni 0.33 Mn 0.33 The number of metal atoms of O is M, the total number of lithium atoms of the reaction aid LiOH·H2O and the residual lithium in the primary calcination product is L, and L / M is 0.9.
[0115] S3, the above two mixed materials were calcined again in dry air in steps, wherein the first step calcination temperature I was 400 ° C, the time was 4h; the second step calcination temperature II was 700 ° C, the time was 8h, and after the calcination was completed, the modified LiNi was obtained by cooling in the furnace. 0.88 Co 0.06 Mn 0.05 Zr 0.01 O2 material, expressed as 0.075Li by chemical formula 0.9 Co 0.33 Ni 0.33 Mn 0.33 O2@LiNi 0.88 Co 0.06 Mn 0.05 Zr 0.01 O2.
[0116] Comparative Example 1
[0117] In comparative example 1, steps S1 and S3 are the same as those in example 1. In S2, 500 g of the primary calcined product is mixed with 1.675 g of Li2O, 23.390 g of the first precursor Co 0.5 Mn 0.5 (OH)2(specific surface area is 15m 2 / g) were mixed evenly to obtain the second mixed material, wherein Co 0.5 Mn 0.5 The amount of (OH)2 meets the following requirements: Co 0.5 Mn 0.5 The molar ratio of (OH)2 to the primary calcined product is 5:100. The first precursor Co 0.5 Mn 0.5 The number of metal atoms in (OH)2 is M, the total number of lithium atoms in the reaction aid Li2O and the residual lithium in the primary calcination product is L, and L / M is 1.0.
[0118] Comparative Example 2
[0119] In comparative example 2, steps S1 and S3 are the same as those in example 1. In S2, 500 g of the primary calcined product is mixed with 23.390 g of the first precursor Co 0.5 Mn 0.5 (OH)2(specific surface area 25m 2 / g) were mixed evenly to obtain the second mixture, without adding reaction aids, wherein Co 0.5 Mn 0.5 The amount of (OH)2 meets the following requirements: Co 0.5 Mn 0.5 The molar ratio of (OH)2 to the primary calcined product is 5:100. The first precursor Co 0.33 Ni 0.33 Mn 0.33 The number of metal atoms in (OH)2 is M, the number of lithium atoms in the residual lithium in the primary calcination product is L, and L / M is about 0.5.
[0120] Comparative Example 3
[0121] In comparative example 3, steps S1 and S3 are the same as those in example 1. In S2, 500 g of the primary calcined product is mixed with 3.596 g of Li2O, 23.390 g of the first precursor Co 0.5 Mn 0.5 (OH)2(specific surface area 25m 2 / g) were mixed evenly to obtain the second mixed material, wherein Co 0.5 Mn 0.5 The amount of (OH)2 meets the following requirements: Co 0.5 Mn 0.5 The molar ratio of (OH)2 to the primary calcined product is 5:100. The first precursor Co 0.5 Mn 0.5The number of metal atoms in (OH)2 is M, the total number of lithium atoms in the reaction aid Li2O and the residual lithium in the primary calcination product is L, and L / M is 1.5.
[0122] Comparative Example 4
[0123] In Comparative Example 4, steps S1 and S2 are the same as those in Example 1. In S3, the two mixtures are calcined again in oxygen at a temperature of 720° C. for 12 h.
[0124] The difference between Comparative Example 1 and Example 1 is that the first precursor selected in Comparative Example 1 has a smaller specific surface area and poorer reaction activity, so the modified material obtained does not form a complete coating layer, and the residual lithium compounds on the surface of the bulk material are not significantly improved.
[0125] The difference between Comparative Example 2 and Example 1 is that in Comparative Example 2, only the residual lithium compound on the surface of the bulk material is used as a reaction aid, and no additional reaction aid is added, which results in a low amount of lithium salt in the coating additive, resulting in incomplete topological transformation reaction. The coating layer in the modified material obtained is not an oxygen-tight docking structure, and no coherent phase boundary is generated.
[0126] The difference between Comparative Example 3 and Example 1 is that the amount of lithium salt in the coating additive selected in Comparative Example 3 is relatively high, which leads to the runaway topological transformation reaction. The coating layer in the modified material obtained is not an oxygen close-packed structure, and no coherent interface is generated. In addition, the residual lithium content on the surface of the once-calcined product is too high, which easily causes gas production in the battery.
[0127] The difference between Comparative Example 4 and Example 1 is that the calcination of the two mixtures in Comparative Example 4 was changed to a one-step calcination, resulting in incomplete topological transformation reaction, and excessively long high-temperature calcination aggravated the metal ion diffusion effect. The modified material obtained thereby had no obvious surface coating layer, and therefore no coherent interface was generated in the modified material.
[0128] Test Case
[0129] 1. The high-nickel layered positive electrode material (i.e., the bulk material) under different temperature conditions in the S3 process of Example 1 was subjected to non-in situ XRD testing, and the non-in situ XRD pattern of the high-nickel layered positive electrode material was obtained as shown in Figure 1. In Figure 1, at 450°C, the XRD peak was mainly the R-3m structure of the bulk material, of which some miscellaneous peaks corresponded to the Fd-3m phase of the spinel structure; at 720°C, the XRD peak was still mainly the R-3m structure of the bulk material, of which some miscellaneous peaks corresponded to the Fd-3m phase of the spinel structure and the Fm-3m phase of the rock salt structure; after cooling to room temperature RT with the furnace, the material was completely transformed into the R-3m structure.
[0130] 2. Electrochemical performance test:
[0131] (1) Preparation of positive electrode sheet and lithium-ion battery:
[0132] The modified materials prepared in Examples 1 to 7 and Comparative Examples 1 to 4 were mixed with acetylene black and polyvinylidene fluoride in a mass ratio of 90:5:5, and an appropriate amount of N-methylpyrrolidone was added as a dispersant, and the mixture was ground into a slurry. The slurry was then evenly coated on an aluminum foil and vacuum dried at 120° C. for 12 h. The dried electrode was rolled with a roller mill, and the aluminum foil was cut with a slicer into circular electrode pieces with a diameter of 10 mm. The loading amount of the active material was controlled at 12 mg.cm -2 about.
[0133] Then, the half-cell was assembled in an argon atmosphere glove box, controlling the water partial pressure ≤0.1ppm and the oxygen partial pressure ≤0.1ppm; metallic lithium was used as the counter electrode, 1M LiPF6 (EC / DMC, volume ratio of 1:1) solution was used as the electrolyte, and the assembly specification was CR2032 button cell.
[0134] (2) Charge and discharge cycle test:
[0135] The battery was charged and discharged at room temperature using constant current charge and discharge mode, with a voltage range of 2.5-4.3V and a current density of 100mA / g (0.5C rate) for 100 cycles. During this process, the battery's first-cycle charge capacity, first-cycle discharge capacity, first-cycle coulombic efficiency, and capacity retention after 100 cycles were tested.
[0136] The specific test results can be found in Table 1 and Figure 2. Figure 2 is a comparison of the specific capacity of Example 1 before and after coating as a function of the number of cycles.
[0137] Table 1
[0138] As shown in Table 1 and Figure 2, the modified high-nickel layered cathode materials all exhibited excellent charge-discharge capacity and cycling performance, and the coated materials exhibited higher first coulombic efficiencies (>90%). Therefore, it can be seen that the coating layer obtained through the topoconversion reaction can significantly improve the interface stability.
[0139] (3) Differential Scanning Calorimetry (DSC) test:
[0140] The positive electrode sheets charged to 4.3V were disassembled to obtain positive electrode powder, which was then placed in a high-pressure crucible. 50 μL of electrolyte was added dropwise, and the temperature was raised from room temperature to the specified temperature at a rate of 2°C / min. The differential scanning calorimetry data for Comparative Examples 1-4 and Examples 1-7 were obtained, as shown in Table 2 below. This data was used to evaluate the safety and thermal stability of the batteries of Comparative Examples 1-4 and Examples 1-7. Additionally, Figure 3 shows a comparison of the differential scanning calorimetry curves for Example 1, uncoated and coated.
[0141] Table 2
[0142] It can be seen from Table 2 and Figure 3 that the high-nickel layered cathode material modified based on the topochemical transformation reaction has lower surface residual lithium compounds. The DSC test shows that the modified high-nickel layered cathode material has a higher exothermic peak temperature and less heat generation, which effectively inhibits the precipitation of highly active oxygen from the bulk material and improves the safety of the high-nickel material.
[0143] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of the present application.
[0144] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and these modifications and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.
Claims
1. A positive electrode composite material, characterized in that: Including body material and cladding layer; The bulk material includes the general formula Li w Ni a Co b Mn c X 1-a-b-c O2 material, wherein X includes one or more of Al, Ti, Zr, Mg and W, and 0.95≤w≤1.1, 0.6≤a≤1, b≥0, c≥0; The coating layer comprises the general formula Li α Ni β Co γ Mn δ O2 materials, wherein 0<α≤1, 0≤β≤0.6, 0≤γ≤1, 0≤δ≤1, and β, γ and δ are not 0 at the same time; The interface between the bulk material and the cladding layer is a coherent phase boundary.
2. The positive electrode composite material according to claim 1, characterized in that: In the crystal structures of the bulk material and the coating layer, oxygen ions are all in a densely packed structure; and / or, The space group to which the coating layer belongs includes one or more of Fd-3m, Fm-3m, R-3m and C2 / m.
3. The positive electrode composite material according to claim 1, characterized in that: The thickness of the coating layer is ≤200nm.
4. A method for preparing a positive electrode composite material according to any one of claims 1 to 3, characterized in that: include: preparing or providing the bulk material; The bulk material is mixed with a coating additive, and the positive electrode composite material is prepared through a topological conversion reaction.
5. The preparation method according to claim 4, characterized in that: The bulk material is mixed with the coating additive, and the positive electrode composite material is prepared by a topological conversion reaction, comprising: Mixing the bulk material and the coating additive; calcining the mixed two materials step by step to prepare the positive electrode composite material; The stepwise calcination includes two steps of calcination, wherein the temperature of the first step of calcination is 400-600°C and the time is 1-5 hours; the temperature of the second step of calcination is 600-800°C and the time is 3-10 hours, and the atmosphere of the stepwise calcination is an oxygen-containing atmosphere.
6. The preparation method according to claim 4 or 5, characterized in that: The coating additive includes a first precursor and a reaction aid, wherein the first precursor includes: Ni x Co y Mn z (OH)2、Ni x Co y Mn z OOH、Ni x Co y Mn z One of O, wherein 0≤x≤0.6, 0≤y≤1, 0≤z≤1, and x, y, and z are not 0 at the same time; The reaction aid includes one or more of lithium oxide, lithium carbonate and lithium hydroxide; Optionally, in the step-by-step calcination, the first precursor is an oxygen close-packed structure, and the space group includes one or more of Fd-3m, Fm-3m, R-3m and C2 / m.
7. The preparation method according to claim 6, characterized in that: The first precursor satisfies at least one of the following conditions: (1) The specific surface area of the first precursor is ≥ 20m 2 / g; (2) The molar ratio of the first precursor to the bulk material is 0.5 mol% to 10 mol%; (3) The total number of metal atoms in the first precursor is M, the total number of residual lithium atoms in the reaction aid and the main material is L, and M and L satisfy 0.8 <L / M<1.2。 8. The preparation method according to claim 6, characterized in that: The preparation of the bulk material comprises: In an oxygen-containing atmosphere, a high-nickel material precursor and a lithium salt are mixed, calcined at a high temperature, cooled with the furnace, and crushed and sieved; Optionally, the preparation of the bulk material satisfies at least one of the following conditions: (1) The high nickel material precursor includes: one or more of oxides and hydroxides; (2) The lithium salt includes one or more of lithium carbonate and lithium hydroxide; (3) The molar ratio of lithium atoms in the high nickel material precursor and the reaction aid is 1.0:(0.9-1.1); (4) The heating rate is 2-8°C / min, the calcination temperature is 700-1100°C, and the calcination time is 12h-24h.
9. A positive electrode sheet, characterized in that: include: A positive electrode current collector, and a positive electrode material layer formed on at least one surface of the positive electrode current collector; The positive electrode material layer comprises the positive electrode composite material according to any one of claims 1 to 3 or the positive electrode composite material prepared by the preparation method according to any one of claims 4 to 8.
10. A battery, characterized in that: include: The positive electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Positive electrode material, and preparation method thereof and lithium ion battery
CN112820861A
Ultrahigh-nickel low-cobalt single-crystal positive electrode material and preparation method thereof
CN114975923A
Composite in-situ coated high-nickel single-crystal positive electrode material and preparation method thereof
CN115571927A
Core-shell structure ternary positive electrode material for all-solid-state battery, preparation method of core-shell structure ternary positive electrode material and all-solid-state battery
CN115954451A
Positive electrode composite material and preparation method thereof, positive plate and battery
CN116525784A