Phosphogypsum-based construction material and preparation and application thereof
By mixing phosphogypsum premix with high-temperature ceramsite for combustion and mixing and calcination, the problem of improving the performance of phosphogypsum-based building materials is solved, the harmless treatment and performance improvement of phosphogypsum are achieved, and a high-strength phosphogypsum material suitable for use as a building material is formed. Remaining materials.
Patent Information
- Application Number
- PCT/CN2023/115003
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2023-08-25
- Publication Date
- 2024-10-31
AI Technical Summary
In the existing technology, when phosphogypsum is used to prepare gypsum-based building materials, comprehensive resource utilization and product performance synergy are difficult to achieve simultaneously, and the obtained phosphogypsum powder has a large space for performance improvement during application.
By mixing the phosphogypsum premix with a temperature above 60°C and ceramsite above 800°C, using the waste heat of the ceramsite to burn and continue mixing and calcining, the remaining material with a ceramic powder content of ≤30wt% is separated to achieve phosphogypsum. Harmless and efficient processing and performance improvement.
It achieves efficient and harmless treatment of phosphogypsum, improves the strength and performance of the remaining materials, making it more suitable for use as phosphogypsum-based building materials, and completes the combustion and mixing and calcination processes in a zero-emission system, further improving the material's Strength and application value.
Smart Images

Figure PCTCN2023115003-FTAPPB-I100001 
Figure PCTCN2023115003-FTAPPB-I100002
Abstract
Description
A phosphogypsum-based building material and its preparation and application
[0001] Cross-references
[0002] This application claims priority to Chinese patent application No. 202310470428.1 filed on April 27, 2023, entitled “A phosphogypsum-based building material, its preparation and application,” and all disclosures of which are incorporated herein by reference in their entirety. Technical Field
[0003] The present invention relates to the technical field of harmless treatment of phosphogypsum and building materials, and in particular to a phosphogypsum-based building material and a preparation and application thereof. Background Art
[0004] The primary step in producing gypsum building materials from phosphogypsum is calcining and dehydrating it to produce gypsum powder. Patent CN 112624642 B discloses an apparatus and method for calcining and regenerating phosphogypsum using high-temperature ceramsite. This technical solution integrates the drying and crushing of wet phosphogypsum slag, the preheating and dehydration of dry phosphogypsum powder, and the cooling of calcined gypsum powder. This solution utilizes the high temperature of the ceramsite to achieve high-temperature dehydration of the phosphogypsum. Furthermore, it utilizes the porous adsorption properties of the ceramsite to absorb some harmful substances and evaporated water from the phosphogypsum, thereby purifying the phosphogypsum. While this method achieves zero-pollution treatment of phosphogypsum and produces gypsum powder, in practice, it has been found that the performance of the fully dehydrated phosphogypsum powder suspended in a rotary kiln, when used as gypsum building materials, still leaves much room for improvement.
[0005] In view of this, the present invention is proposed.
[0006] Summary of the Invention
[0007] Through further study of the technical solution in CN 112624642 B, the present invention finds that the performance of the phosphogypsum powder obtained by this method is not significantly different from that of the phosphogypsum obtained by drying phosphogypsum slag by other methods. Therefore, the present invention provides a phosphogypsum-based building material and its preparation and application. Based on the structural characteristics of ceramsite and phosphogypsum, the process of dehydration and drying of phosphogypsum is redesigned to solve the technical problem in the prior art of using phosphogypsum to prepare gypsum-based building materials, which is the difficulty in simultaneously achieving comprehensive resource utilization and synergistic improvement of product performance.
[0008] Specifically, the present invention provides a method for preparing a phosphogypsum-based building material, comprising: mixing a phosphogypsum premix having a temperature of 60°C or above, a free water content of 10% or less, and an organic matter content of 5 to 20% by weight with ceramsite having a temperature of 800°C or above, burning the ceramsite using waste heat, and then continuing to mix and calcine, then separating ceramsite coarse aggregate to obtain a residue having a ceramsite powder content of 30% or less by weight, and post-processing the residue to obtain the product.
[0009] Through further research on the technical solution in CN 112624642 B, the present invention observed that secondary combustion occurs at the moment when ceramsite with a temperature above 800°C and phosphogypsum obtained under specific conditions come into contact at the feed port of a rotary kiln. Furthermore, through a large number of experiments, it was verified that the phosphogypsum premix of the present invention is combustible. When it is added to ceramsite with a temperature above 800°C, it can be burned using the waste heat of the ceramsite. Moreover, the combustion process is conducive to achieving efficient harmless treatment of phosphogypsum, especially significantly improving the degree of solidification or passivation of harmful substances. Moreover, compared with conventional mixed calcination, the residual material obtained by continuing mixed calcination after combustion in the present invention has higher strength and is more suitable for use as a phosphogypsum-based building material.
[0010] The above-mentioned post-treatment can be: cooling, grinding, and aging the residual material to obtain the phosphogypsum-based building material; or, grinding, cooling, and aging the residual material to obtain the phosphogypsum-based building material.
[0011] The above-mentioned mixing can be carried out by adding the phosphogypsum premix into ceramsite at a temperature above 800°C.
[0012] According to the method for preparing phosphogypsum-based building materials provided by the present invention, the combustion and the subsequent mixing and calcining processes are both carried out in a zero-emission system.
[0013] In order to achieve zero emissions, the present invention completes the combustion and the continued mixed calcination processes in a zero-emission system (such as the combustion occurs in the feed inlet section of the kiln, and the mixed calcination occurs in the middle and tail ends of the kiln). However, it was unexpectedly discovered from a large number of experiments that completing the process in a zero-emission system will further improve the strength of the residual material when used as a phosphogypsum-based building material.
[0014] According to the preparation method of the phosphogypsum-based building material provided by the present invention, the density of the ceramsite is ≤1200kg / m 3 , average particle size <31.5mm, porosity >30%;
[0015] According to the test of the present invention, the porous adsorption of ceramsite can achieve the regulation of water in the system. In the process of mixing and calcining after the combustion, the structural parameters such as the particle size and pore size of the ceramsite will affect the degree of mutual conversion between dihydrate calcium sulfate, hemihydrate calcium sulfate and anhydrous calcium sulfate in the phosphogypsum. Moreover, in the zero-emission system, this regulation effect is more significant. When the density is selected to be ≤1200kg / m 3 When the ceramsite has an average particle size of less than 31.5 mm and a porosity of more than 30%, more β-type gypsum can be obtained.
[0016] According to the method for preparing phosphogypsum-based building materials provided by the present invention, the content of SiO2 in the ceramsite is 53-70%;
[0017] Preferably, the ceramsite is obtained by mixing, aging, granulating and calcining the following materials according to the following ratios (all in mass percentage):
[0018] Waste soil 40-70%, sludge 20-50%, phosphogypsum 5-8% and mineral balance;
[0019] Among them, minerals mainly include: SiO2 53-70%, Al2O3 12-26% and CaO 3-5%;
[0020] The remaining components of the above-mentioned mineral components are mainly one or more of NaO2, FeO, MgO and Fe2O3, accounting for 8 to 24%.
[0021] The main raw materials for preparing ceramsite, such as waste soil and sludge, can provide a large amount of SiO2 after calcination. At the same time, the specific structure and SiO2 content of ceramsite can be adjusted by selecting minerals to achieve the purpose of the present invention.
[0022] Experiments have also shown that the combustion and mixed calcination of siliceous ceramsite in the present invention can produce siliceous phosphogypsum-based building materials. High-temperature calcination followed by ball milling further stimulates the activity of the siliceous phosphogypsum-based building materials. The addition of the siliceous material reduces the water requirement of the siliceous phosphogypsum-based building materials from 60% to below 40%, resulting in a more homogeneous material and significantly improved strength.
[0023] According to the preparation method of phosphogypsum-based building materials provided by the present invention, the ceramsite is obtained by mixing waste soil, sludge, phosphogypsum and minerals, aging, granulating and calcining at a temperature greater than 1100°C.
[0024] In order to rationally utilize energy, the present invention directly uses the residual heat of the material obtained by calcining at a temperature greater than 1100°C during its cooling process to treat specific phosphogypsum. It was unexpectedly found that this method not only fully utilizes the thermal energy of the system, but also found that the uncooled material after calcination has the characteristics of an open flame, and can instantly mix with the specific phosphogypsum premix of the present invention to play a combustion-supporting role, thereby accelerating the solidification and passivation of harmful substances in the phosphogypsum premix and improving the mechanical properties of the residual material.
[0025] According to the method for preparing phosphogypsum-based building materials provided by the present invention, the content of ceramic powder in the residual material is within 10%.
[0026] The present invention has found that the strength of the obtained residue is also significantly related to the content of ceramic powder in the residue. In practical applications, by reasonably controlling the mass ratio of the phosphogypsum premix and the ceramsite, and combining the process of continuing mixing and calcining after the combustion, the residue can have a better component ratio. According to tests, it was found that when the content of ceramic powder in the residue is controlled within 10%, the performance of the obtained phosphogypsum-based building material is better.
[0027] According to the method for preparing phosphogypsum-based building materials provided by the present invention, the mass content of calcium sulfate dihydrate in the phosphogypsum premix is ≥60%, preferably 60% to 75%.
[0028] The key component of the phosphogypsum premix is organic matter, and the main component is calcium sulfate dihydrate. Experiments have found that the content of calcium sulfate dihydrate will affect the performance of the final phosphogypsum-based building materials. When the mass content of calcium sulfate dihydrate in the phosphogypsum premix is greater than 60%, the combustion and mixed calcination systems are more stable.
[0029] According to the method for preparing phosphogypsum-based building materials provided by the present invention, the phosphogypsum premix is obtained by heating phosphogypsum slag, a by-product of a wet-process phosphoric acid process, in a zero-emission system at above 160°C.
[0030] The present invention has been found in experiments that by treating the by-product phosphogypsum slag of the wet-process phosphoric acid process in a zero-emission system, a phosphogypsum premix with a certain free water and organic matter content can be obtained. More importantly, at a higher temperature, the free water in the phosphogypsum premix can be made more active and the organic matter can be more easily burned, thereby allowing the ceramsite to play a more effective role in the combustion and mixed calcination stages.
[0031] The zero-emission system in the present invention means that no gas or impurities are emitted to the outside during the reaction of materials in the system.
[0032] For example, during the process of continuing to mix and calcine the phosphogypsum premix and ceramsite after the combustion, the moisture and impurities in the phosphogypsum premix are always retained in the entire system, and the ceramic powder generated by friction is also retained in the entire system. After the process of continuing to mix and calcine after the combustion is completed, only two parts, namely, separated ceramsite coarse aggregate and siliceous phosphogypsum-based building material residue, are produced. For example, this process can occur in the middle and tail end devices of the mixing and calcining rotary kiln.
[0033] For another example, in the process of preparing the phosphogypsum premix from the phosphogypsum slag, the free water and impurities generated by the heating of the phosphogypsum slag are not discharged to the outside, but are fully mixed with the phosphogypsum to form the phosphogypsum premix, and are added to the expanded clay together. For example, this process can occur in the initial feed port section device of the mixing and calcining rotary kiln.
[0034] In the present invention, the entire intermediate process can be placed in a zero-emission system by controlling the feeding portion of the phosphogypsum slag and the ceramsite, and controlling the discharging portion of the ceramsite coarse aggregate and the residual material. This not only achieves full recycling of the phosphogypsum slag, but also rationally utilizes the energy of the system and the mutual influence between materials in the system. More importantly, the performance of the obtained phosphogypsum-based building material is significantly better than the industry standard, and has great application value and technical contribution.
[0035] Preferably, the phosphogypsum premix is obtained by heating the phosphogypsum slag, a by-product of the wet phosphoric acid process, under the action of the waste heat of the combustion and the mixed calcination.
[0036] In order to be low-carbon and environmentally friendly and to fully utilize energy, the waste heat from the combustion and the mixed calcination can be used to preheat the phosphogypsum slag, a by-product of the wet-process phosphoric acid process. In practical applications, the waste heat utilization device can be reasonably designed to maximize the energy conversion rate.
[0037] According to the method for preparing phosphogypsum-based building materials provided by the present invention, the combustion time is 3 to 15 seconds, and the mixing and calcining time is greater than 5 minutes;
[0038] Preferably, the temperature of the mixed calcination is above 400°C.
[0039] In order to better passivate harmful substances such as soluble phosphorus, soluble fluorine, soluble sodium, soluble magnesium and various heavy metals contained in phosphogypsum, experiments have shown that when mixed calcination is above 400°C, the harmful substances in the phosphogypsum slag used in the preparation of building materials are treated and disposed of to the greatest extent, thereby improving the quality and scope of use of phosphogypsum-based building materials.
[0040] In addition, during the mixed calcination process, high-quality zero-carbon emission calcination is achieved based on the thermal energy conversion efficiency, and the input amount of phosphogypsum slag is pre-controlled to ensure the pre-treated moisture content and flash quality.
[0041] The present invention also provides phosphogypsum-based building materials prepared by the method for preparing the phosphogypsum-based building materials.
[0042] Preferably, the phosphogypsum-based building material contains more than 80% of β-gypsum;
[0043] More preferably, the phosphogypsum-based building material further contains 5-10% silicate.
[0044] The phosphogypsum-based building material prepared by the present invention has excellent performance and a wide range of applications. It can be used for gypsum-based thermal insulation mortar and is more suitable for gypsum-based stabilized base materials in road engineering.
[0045] In the preparation method of the phosphogypsum-based building material of the present invention, the separated ceramsite coarse aggregate has the characteristic of residual gypsum-based cementitious material and can be used for self-insulating wall materials, building blocks, lightweight concrete dry mixes, etc. in green building projects.
[0046] The present invention provides a phosphogypsum-based building material and its preparation and application. The phosphogypsum premix having a temperature of above 60°C, a free water content of ≤10%, and an organic matter content of 5 to 20 wt% is mixed with ceramsite having a temperature of above 800°C, and then the ceramsite is burned using the waste heat of the ceramsite and then mixed and calcined. This achieves efficient harmless treatment of the phosphogypsum, especially significantly improving the degree of solidification or passivation of harmful substances. Moreover, compared with conventional mixed calcination, the residue obtained by the combustion and subsequent mixed calcination in the present invention has higher strength and is more suitable for use as a phosphogypsum-based building material. DETAILED DESCRIPTION
[0047] To make the objectives, technical solutions, and advantages of the present invention more clear, the technical solutions of the present invention are described clearly and completely below. Obviously, the embodiments described are only some of the embodiments of the present invention, not all of them. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0048] If no specific techniques or conditions are specified in the examples, the experiments were carried out according to the techniques or conditions described in the literature in the field or according to the product instructions. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0049] The minerals in the present invention are derived from industrial tailings, waste slag, etc., and their main mineral components include: SiO2 53-70%, Al2O3 12-26% and CaO 3-5%; the remaining components are mainly NaO2, FeO, MgO and Fe2O3, accounting for 8-24%.
[0050] Example 1
[0051] A method for preparing phosphogypsum-based building materials, the process is as follows:
[0052] (1) Pre-treating phosphogypsum by heating to obtain a phosphogypsum premix having a temperature of 70° C., a free water content of 10%, and an organic matter content of 15%, wherein the mass content of calcium sulfate dihydrate in the phosphogypsum premix is 60%.
[0053] 60% of waste soil, 30% of sludge, 5% of phosphogypsum and the rest of the minerals are mixed according to the proportion, aged, granulated and calcined at high temperature (calcination temperature is 1100°C).
[0054] (2) adding the phosphogypsum premix in step (1) to the ceramsite obtained after high-temperature calcination in step (1), at this time, ensuring that the temperature of the ceramsite is above 800° C. when adding, utilizing the residual heat of the ceramsite to burn, and then continuing to mix and calcine, and then separating ceramsite coarse aggregate with an average particle size of 2.36 mm or more, so that the ceramic powder content in the obtained residue is 5%, and further grinding, cooling, and aging the obtained residue to obtain the phosphogypsum-based building material;
[0055] The SiO2 content in the ceramsite is 65%, and the density of the ceramsite is 450kg / m 3 The average particle size is 30 mm, the porosity is 45%, and the mass ratio of the phosphogypsum premix and the expanded clay is 1:1. Without external heating, the two continue to burn for 10 seconds, the time for controlling the mixed calcination is 10 minutes, and the material temperature gradually reaches 400-600°C after a brief rise.
[0056] The prepared phosphogypsum-based building material was tested, and the test results showed that the phosphogypsum-based building material contained 82% of beta-gypsum and 5% of silicate; and the strength of the phosphogypsum-based building material reached grade 3.0.
[0057] The present invention also analyzed the above-mentioned phosphogypsum premix and the prepared phosphogypsum-based building materials and found that the contents of some elements therein changed significantly, as follows:
[0058] The present invention also tests the acidity and alkalinity of the above-mentioned phosphogypsum premix and the prepared phosphogypsum-based building materials, and finds that the pH value of the phosphogypsum-based building materials is significantly higher than that of the phosphogypsum premix, and is increased to above 7.
[0059] Example 2
[0060] A method for preparing a phosphogypsum-based building material, the process of which is substantially the same as that of Example 1, except that: ceramsite coarse aggregate with an average particle size of 5 mm or more is separated, so that the ceramic powder content in the remaining material is 10%.
[0061] Example 3
[0062] A method for preparing a phosphogypsum-based building material, the process of which is substantially the same as that of Example 1, except that: ceramsite coarse aggregate with an average particle size of 8 mm or more is separated, so that the ceramic powder content in the remaining material is 20%.
[0063] Example 4
[0064] A method for preparing a phosphogypsum-based building material, the process of which is substantially the same as that of Example 1, except that: ceramsite coarse aggregate with an average particle size of more than 10 mm is separated, so that the ceramic powder content in the remaining material is 30%.
[0065] The strength of the phosphogypsum-based building materials obtained in Examples 1 to 4 was tested, and the test results are as follows:
[0066] Example 5
[0067] A method for preparing a phosphogypsum-based building material, the process of which is basically the same as that of Example 1, except that: the phosphogypsum premix is obtained by heating phosphogypsum slag, a by-product of a wet-process phosphoric acid process, in a zero-emission system at 160°C, wherein the phosphogypsum slag is derived from a phosphogypsum storage yard, and the mass content of calcium sulfate dihydrate in the obtained phosphogypsum premix is 50%.
[0068] The results showed that the strength of the prepared phosphogypsum-based building material was significantly lower than that of Example 1, specifically, the 2-hour flexural strength was 1.6 MPa, and the 2-hour compressive strength was 4.3 MPa.
[0069] Example 6
[0070] A method for preparing a phosphogypsum-based building material, the process of which is basically the same as that of Example 1, except that the SiO2 content in the mineral is adjusted so that the SiO2 content in the ceramsite is 70%.
[0071] The results showed that the prepared phosphogypsum-based building material contained 5-7% silicate; and the 2-hour strength of the phosphogypsum-based building material was 8.75 MPa in compressive strength and 3.85 MPa in flexural strength.
[0072] Example 7
[0073] A method for preparing a phosphogypsum-based building material, the process of which is substantially the same as that of Example 1, except that the processing technology of ceramsite is adjusted so that the porosity of the prepared ceramsite is about 20%.
[0074] The results showed that the prepared phosphogypsum-based building materials contained 65% of β-gypsum.
[0075] Example 8
[0076] A method for preparing phosphogypsum-based building materials, the process of which is basically the same as that of Example 1, except that the process of continuing mixing and calcining after combustion is carried out in a zero-emission system.
[0077] The results showed that the prepared phosphogypsum-based building materials contained 86% of β-gypsum.
[0078] Example 9
[0079] A method for preparing a phosphogypsum-based building material, the process of which is basically the same as that of Example 5, except that the phosphogypsum premix is obtained by heating the phosphogypsum slag, a by-product of the wet phosphoric acid process, under the action of the waste heat of the combustion and the mixed calcination.
[0080] Comparative Example 1
[0081] A method for preparing a phosphogypsum-based building material is described. The process is substantially the same as in Example 1, except that the phosphogypsum premix in step (1) is cooled to 50° C. and then added to the ceramsite obtained after high-temperature calcination in step (1). The strength of the resulting phosphogypsum-based building material was found to be reduced. Analysis of the remaining material revealed that the content of ceramic powder in the remaining material was too high and the content of β-gypsum was too low.
[0082] Comparative Example 2
[0083] A method for preparing a phosphogypsum-based building material, the process being substantially the same as in Example 1, differing only in that the free water content of the phosphogypsum premix was 50%. It was found that upon contact with ceramsite, combustion failed to occur, resulting in reduced strength and excessively high levels of harmful components and impurities in the resulting phosphogypsum-based building material.
[0084] Comparative Example 3
[0085] A method for preparing a phosphogypsum-based building material, the process of which is basically the same as that of Example 1, except that: the phosphogypsum premix in step (1) is added to the ceramsite obtained after high-temperature calcination in step (1) at a temperature of 750°C. The results show that no combustion phenomenon occurs at the feeding inlet, and there is no secondary temperature rise phenomenon during the combustion of organic matter. When the proportion of β-gypsum reaches more than 80%, the time of mixed calcination needs to be extended to 30 minutes or more, and the feeding ratio of the phosphogypsum premix is changed from 1:1 to 0.8:1 or less, the conversion rate of β-gypsum is greatly reduced, the mixed calcination temperature is in a linear attenuation state, and the efficiency is significantly reduced.
[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the various embodiments of the present invention.
Claims
1. A method for preparing phosphogypsum-based building materials, characterized in that: include: A phosphogypsum premix with a temperature of more than 60°C, a free water content of ≤10% and an organic matter content of 5-20wt% is mixed with ceramsite at a temperature of more than 800°C, and the ceramsite is burned using the waste heat, followed by continued mixing and calcination, and then the ceramsite coarse aggregate is removed to obtain a residue with a ceramsite powder content of ≤30wt%, and the residue is post-treated to obtain the product.
2. The method for preparing phosphogypsum-based building materials according to claim 1, characterized in that: The combustion and the subsequent mixed calcination process are both carried out in a zero emission system.
3. The method for preparing the phosphogypsum-based building material according to claim 1 or 2, characterized in that: The density of the ceramsite is ≤1200kg / m 3 , average particle size <31.5mm, porosity >30%.
4. The method for preparing phosphogypsum-based building materials according to any one of claims 1 to 3, characterized in that: The content of SiO2 in the ceramsite is 53-70%; Preferably, the ceramsite is obtained by mixing, aging, granulating and calcining the following materials according to a ratio: Waste soil 40-70%, sludge 20-50%, phosphogypsum 5-8% and mineral remainder.
5. The method for preparing phosphogypsum-based building materials according to any one of claims 1 to 4, characterized in that: The ceramsite is obtained by mixing, aging, granulating and calcining waste soil, sludge, phosphogypsum and minerals at a temperature greater than 1100°C.
6. The method for preparing phosphogypsum-based building materials according to any one of claims 1 to 5, characterized in that: The content of the ceramic powder in the residual material is 5-10%.
7. The method for preparing phosphogypsum-based building materials according to any one of claims 1 to 6, characterized in that: The mass content of calcium sulfate dihydrate in the phosphogypsum premix is greater than 60%; Preferably, the phosphogypsum premix is obtained by heating the by-product phosphogypsum slag of the wet phosphoric acid process in a zero-emission system at a temperature above 160°C; Further preferably, the phosphogypsum premix is obtained by heating the phosphogypsum slag as a by-product of the wet phosphoric acid process under the effect of the waste heat of the combustion and the mixed calcination.
8. The method for preparing phosphogypsum-based building materials according to any one of claims 1 to 7, characterized in that: The combustion time is 3 to 15 seconds, and the mixed calcination time is greater than 5 minutes; Preferably, the temperature of the mixed calcination is above 400°C.
9. A phosphogypsum-based building material, characterized in that: The phosphogypsum-based building material is prepared by the preparation method of the phosphogypsum-based building material according to any one of claims 1 to 8.
10. An application of phosphogypsum-based building materials, characterized in that: The phosphogypsum-based building material as claimed in claim 9 is used.
Citation Information
Patent Citations
Production method of high-temperature gypsum powder
CN112341021A
Device for exercising and regenerating ardealite by utilizing high-temperature ceramsite and using method thereof
CN112624642A
Calcination of gypsum
GB392780A