Back contact solar cell and method for preparing same
By using cylindrical hole structures and doped back field layers in back-contact solar cells, combined with electrode design, the problem of low carrier collection efficiency is solved and more efficient cell performance is achieved.
Patent Information
- Application Number
- PCT/CN2023/123977
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-10-11
- Publication Date
- 2024-10-31
AI Technical Summary
Existing back-contact solar cells have deficiencies in carrier collection efficiency, resulting in low cell efficiency. In particular, the shunt problem caused by the surface charge of the dielectric layer is difficult to effectively solve.
A columnar hole structure is used to arrange the doped back field layer, and first and second electrodes are provided on the back side of the silicon substrate. The first electrode is in electrical contact with the doped back field layer, the second electrode is in electrical contact with the doped polysilicon layer, and the two electrodes are extremely They are opposite in nature and insulated from each other. This structure increases the back field collection area and emitter area and improves the carrier collection efficiency.
Through the design of the cylindrical hole structure, the thickness of the silicon substrate is fully utilized to form a deep back field area, which shortens the carrier transmission distance, enhances the carrier collection effect, and improves the overall efficiency of the solar cell.
Smart Images

Figure CN2023123977_31102024_PF_FP_ABST
Abstract
Description
Back-contact solar cell and preparation method thereof
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 28, 2023, with application number 202310501272.9 and invention name “A back-contact solar cell and its preparation method”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention belongs to the technical field of solar cells, and in particular relates to a back-contact solar cell and a preparation method thereof. Background Art
[0003] As fossil fuels gradually deplete, solar cells are becoming increasingly popular as a new energy alternative. Solar cells convert sunlight into electricity by utilizing the photovoltaic principle to generate charge carriers, which are then extracted using electrodes, facilitating efficient utilization of the electrical energy.
[0004] Back-contact cells are also called back contact cells, among which p-type back-contact solar cells are also called IBC cells. IBC stands for Interdigitated Back-Contacted. The most significant feature of IBC cells is that the emitter and metal contact are both on the back of the cell, leaving the front unobstructed by metal electrodes. Therefore, they have a higher short-circuit current Jsc. At the same time, the back can accommodate wider metal grid lines to reduce the series resistance Rs, thereby increasing the fill factor FF. Furthermore, this unobstructed front-side cell not only has high conversion efficiency but also looks more aesthetically pleasing. Furthermore, full back-electrode components are easier to assemble. IBC cells are currently one of the technical directions for achieving high-efficiency crystalline silicon cells.
[0005] Currently, conventional p-type interdigitated back-contact solar cells have a p-type base or a diffused n-type emitter on their rear region, but choosing a dielectric layer that can passivate both regions equally well is a challenge, and most dielectric layers have surface charges that can cause shunting, resulting in extremely poor cell effects. For example, well-known passivation dielectric layers are aluminum oxide (aluminum oxide, Al2O3) with a negative surface charge and hydrogenated amorphous silicon nitride (α-SiNx:H) with a positive surface charge. In addition, the carriers of the back-junction back-contact cell need to diffuse from the front to the back field on the back to be collected, resulting in poor collection efficiency, which in turn leads to reduced cell efficiency.
[0006] Chinese patent publication number CN111108609A discloses an interdigitated back-contact solar cell with p-type conductivity. The interdigitated back-contact solar cell has a front surface for receiving radiation and a rear surface. The rear surface comprises a tunnel oxide layer and an n-type doped polysilicon layer. The tunnel oxide layer and the n-type doped polysilicon layer form a patterned layer stack with gaps therein. An Al-Si alloyed contact is disposed within each of the gaps, electrically contacting the base layer of the substrate, and one or more Ag contacts or transition metal contacts are disposed on and electrically contacting the patterned doped polysilicon layer. While this structure can reduce shunting and improve cell efficiency, it is complex and the fabrication method is difficult.
[0007] Summary of the Invention
[0008] In view of this, the technical problem to be solved by the present invention is to provide a back-contact solar cell and a preparation method thereof, wherein the back-contact solar cell can enhance the carrier collection effect and improve the battery efficiency.
[0009] The present invention provides a back-contact solar cell, comprising:
[0010] Silicon substrate;
[0011] The back side of the silicon substrate is provided with columnar holes and non-columnar hole areas;
[0012] The columnar hole is provided with a doped back surface field layer;
[0013] A first electrode is provided on the back side of the silicon substrate; the first electrode is in electrical contact with the doped back field layer;
[0014] The non-columnar hole region is provided with a doped emitter layer; the doped emitter layer includes a doped polysilicon layer;
[0015] A second electrode is provided on the back of the silicon substrate; the second electrode is in electrical contact with the doped polysilicon layer;
[0016] The first electrode and the second electrode have opposite polarities and are insulated from each other.
[0017] Preferably, the doped back field layer is disposed on the sidewalls and bottom surface of the columnar hole.
[0018] Preferably, the diameter of the columnar holes is 50-300 μm; the number of the columnar holes is multiple; the interval between adjacent columnar holes is 500-3000 μm; the depth of the columnar holes is 30%-80% of the thickness of the silicon substrate.
[0019] Preferably, there are multiple cylindrical holes, each of which is provided with a first electrode; the multiple first electrodes are connected by a first conductive paste line;
[0020] There are multiple second electrodes; the multiple second electrodes are connected by second conductive paste lines;
[0021] Furthermore, the first conductive paste line does not contact the second conductive paste line.
[0022] Preferably, the first conductive paste line is connected to the first electrode in a serpentine shape;
[0023] The second conductive paste line is connected to the second electrode in a serpentine shape.
[0024] Preferably, the doped emitter layer further includes a tunneling oxide layer; the tunneling oxide layer is disposed between the silicon substrate in the non-columnar hole region and the doped polysilicon layer.
[0025] Preferably, the thickness of the tunnel oxide layer is 0.1-5 nm; the thickness of the doped polysilicon layer is 30-300 nm; the diameter of the first electrode is 200-100 μm; and the diameter of the second electrode is 10-30 μm.
[0026] Preferably, the silicon substrate is a P-type silicon substrate; the doped back field layer is a back field layer doped with group III elements; and the doped polysilicon layer is a polysilicon layer doped with group V elements.
[0027] Preferably, the silicon substrate is an N-type silicon substrate; the doped back field layer is a back field layer doped with group V elements; and the doped polysilicon layer is a polysilicon layer doped with group III elements.
[0028] The present invention also provides a method for preparing the above-mentioned back-contact solar cell, comprising the following steps:
[0029] S1) depositing an intrinsic amorphous silicon layer on the back side of the silicon substrate;
[0030] S2) performing a first doping treatment on the silicon substrate on which the intrinsic amorphous silicon layer is deposited to form a doped polysilicon layer;
[0031] S3) printing an acidic etching material on the back side of the silicon substrate on which the doped polysilicon layer is formed, and performing a polishing process to form columnar holes;
[0032] S4) performing a second doping treatment on the silicon substrate with the columnar holes formed therein to form a doped back surface field layer;
[0033] S5) acid-washing the silicon substrate on which the doped back field layer is formed;
[0034] S6) preparing a first electrode electrically contacting the doped back field layer and a second electrode electrically contacting the doped polysilicon layer on the back side of the acid-washed silicon substrate to obtain a back-contact solar cell; the first electrode and the second electrode have opposite polarities and are insulated from each other.
[0035] The present invention provides a back-contact solar cell, comprising: a silicon substrate; a columnar hole and a non-columnar hole region are provided on the back side of the silicon substrate; a doped back field layer is provided in the columnar hole; a first electrode is provided on the back side of the silicon substrate; the first electrode is in electrical contact with the doped back field layer; a doped emitter layer is provided in the non-columnar hole region; the doped emitter layer includes a doped polysilicon layer; a second electrode is provided on the back side of the silicon substrate; the second electrode is in electrical contact with the doped polysilicon layer. Compared with the existing technology, the present invention uses a columnar hole structure to arrange the back field area, which can make full use of the thickness of the silicon substrate. The bottom area and the column wall formed form the back field area, which increases the back field collection area without occupying the back surface area, and also maximizes the back emission area. For a solar cell, within a certain proportion range, the larger the proportion of the emitter area, the higher the capture and transmission performance of minority carriers, and the efficiency of the cell is relatively high. At the same time, the back field area penetrates deep into the silicon wafer, so that the majority carriers can be collected inside the silicon wafer, shortening the transmission and collection distance and enhancing the collection effect, so that the structure has an enhanced collection effect on both minority carriers and majority carriers, thereby improving the efficiency of the cell as a whole. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] FIG1 is a schematic structural diagram of a back-contact solar cell provided by the present invention;
[0037] FIG2 is a schematic diagram of the distribution of columnar holes in a back-contact solar cell provided by the present invention;
[0038] FIG3 is a schematic diagram of the electrode arrangement of a back-contact solar cell provided by the present invention;
[0039] FIG4 is a schematic structural diagram of a P-type silicon substrate provided by the present invention after etching and polishing to form cylindrical holes;
[0040] FIG5 is a schematic structural diagram of a P-type silicon substrate provided by the present invention after a second doping treatment to form a doped back field layer;
[0041] FIG6 is a schematic structural diagram of a silicon substrate after pickling provided by the present invention. DETAILED DESCRIPTION
[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0043] The present invention provides a back-contact solar cell, comprising:
[0044] Silicon substrate;
[0045] The back side of the silicon substrate is provided with columnar holes and non-columnar hole areas;
[0046] The columnar hole is provided with a doped back surface field layer;
[0047] A first electrode is provided on the back side of the silicon substrate; the first electrode is in electrical contact with the doped back field layer;
[0048] The non-columnar hole region is provided with a doped emitter layer; the doped emitter layer includes a doped polysilicon layer;
[0049] A second electrode is provided on the back side of the silicon substrate; the second electrode is in electrical contact with the doped polysilicon layer.
[0050] Referring to FIG1 , FIG1 is a schematic structural diagram of a back-contact solar cell provided by the present invention.
[0051] The silicon substrate in the back-contact solar cell provided by the present invention can be any substrate well known to those skilled in the art without any particular limitation, and can be either a P-type silicon substrate or an N-type silicon substrate.
[0052] The back side of the silicon substrate is provided with cylindrical holes and / or conical holes; the cylindrical holes can be cylindrical holes and / or prismatic holes, and there is no special limitation; in a specific embodiment provided by the present invention, the silicon substrate is preferably provided with cylindrical holes, see Figure 2, Figure 2 is a schematic diagram of the distribution of cylindrical holes of the back-contact solar cell provided by the present invention; the diameter of the cylindrical holes is preferably 50 to 300 μm, more preferably 80 to 200 μm, and more preferably 100 to 150 μm; the number of the cylindrical holes is preferably multiple; the interval between adjacent cylindrical holes is preferably 500 to 3000 μm, more preferably 800 to 2000 μm, more preferably 800 to 1500 μm, and most preferably 1000 μm; the depth of the cylindrical holes is preferably 30% to 80% of the thickness of the silicon substrate. In a specific embodiment provided by the present invention, the bottom and / or side walls of the columnar holes and / or conical holes are provided with a concave-convex texture structure; the number of the concave-convex texture structures can be one or more, and there is no special restriction; the concave-convex texture structure is provided at the bottom and / or side walls of the columnar holes and / or conical holes to further expand the area of the back field region.
[0053] The columnar hole is provided with a doped back field layer; the thickness of the doped back field layer is preferably 0.3 to 1 μm; in the present invention, the doped back field layer is preferably provided on the sidewall and bottom surface of the columnar hole; the doping elements in the doped back field layer can be selected according to the type of silicon substrate; when the silicon substrate is a P-type silicon substrate, the doped back field layer is a back field layer doped with group III elements, preferably a boron-doped back field layer and / or a gallium-doped back field layer, as a P+ back field region for selectively transmitting hole carriers; when the silicon substrate is an N-type silicon substrate; the doped back field layer is preferably a P+ back field region for selectively transmitting hole carriers; The layer is a back field layer doped with group V elements, preferably a phosphorus-doped back field layer, which serves as an N+ back field region for selectively transmitting electron carriers; in the present invention, preferably, a back passivation layer is further provided on the surface of the doped back field layer; the thickness of the back passivation layer is preferably 62 to 220 nm; the back passivation layer can be a back passivation layer well known to those skilled in the art, and there is no special limitation. In the present invention, it is preferred that the back passivation layer include an aluminum oxide layer and a silicon nitride layer stacked; the thickness of the aluminum oxide layer is preferably 2 to 20 nm; the thickness of the silicon nitride layer is preferably 60 to 200 nm.
[0054] A first electrode is provided on the back side of the silicon substrate, that is, a first electrode is provided in the cylindrical hole; the first electrode is electrically contacted with the doped back field layer; the shape of the first electrode can be cylindrical or conical, and there is no special restriction. In the present invention, it is preferably a cylinder; the diameter of the first electrode is preferably 200 to 100 μm; the height of the first electrode preferably extends to the vicinity of the flat area surface of the silicon substrate, that is, the height of the first electrode is less than or equal to the depth of the cylindrical hole and / or the conical hole, and more specifically, the height of the first electrode is less than or equal to the depth of the cylindrical hole; the first electrode is preferably an aluminum electrode; the first electrode serves to electrically contact the doped back field layer.
[0055] In the present invention, since there are multiple cylindrical holes and / or conical holes, a first electrode is arranged in each cylindrical hole and / or conical hole, and the number of first electrodes is also multiple, it is preferably also included a first conductive grid line, which can also be called a first conductive paste line, and multiple first electrodes are connected by the first conductive grid line or the first conductive paste line; more preferably, the first conductive grid line or the first conductive wire paste line is arranged on the surface of the back passivation layer to connect the multiple first electrodes; further preferably, the first conductive grid line or the first conductive paste line connects the first electrode in a serpentine shape; the width of the first conductive grid line or the first conductive paste line is preferably 20 to 300 μm; the type of the first conductive grid line or the first conductive paste line can be a grid line or paste line familiar to those skilled in the art, and there is no special limitation. In the present invention, it is preferably aluminum paste (sintered according to a method familiar to those skilled in the art).
[0056] The back side of the silicon substrate is a non-columnar hole area except for the columnar holes and / or the conical holes; a doped emitter layer is provided on the surface of the silicon substrate in the non-columnar hole area; the doped emitter layer includes a doped polysilicon layer; the thickness of the doped polysilicon layer is preferably 30 to 300 nm; the type of doping element in the doped polysilicon layer is selected according to the type of the silicon substrate. When the silicon substrate is a P-type silicon substrate, the doped polysilicon layer is a polysilicon layer of group V elements, preferably a phosphorus-doped polysilicon layer; when the silicon substrate is an N-type silicon substrate, the doped polysilicon layer is a polysilicon layer doped with group III elements, preferably a boron-doped polysilicon layer and / or a gallium-doped polysilicon layer; in the present invention, preferably, the doped emitter layer also includes a tunneling oxide layer; the tunneling oxide layer is provided between the silicon substrate in the non-columnar hole area and the doped polysilicon layer; the thickness of the tunneling oxide layer is preferably 0.1 to 5 nm, more preferably 0.5 to 4 nm, and even more preferably 1 to 3 nm; the tunneling oxide layer can be a silicon oxide layer, a silicon oxynitride layer or a silicon nitride layer; in the present invention, preferably, a back passivation layer is provided on the surface of the doped emitter layer, and more preferably, the back passivation layer in the non-columnar hole area is integrated with the back passivation layer in the columnar hole and / or the conical hole; that is, in the present invention, the back passivation layer is arranged on the back side of the silicon substrate and covers the doped back field layer and the doped polysilicon layer; the back passivation layer is provided with an opening, and the first electrode is electrically in contact with the doped back field layer through the opening; the second electrode is electrically in contact with the doped polysilicon layer through the opening; the thickness of the back passivation layer in the non-columnar hole area is preferably 62 to 220 nm; the back passivation layer can be a back passivation layer well known to those skilled in the art, and there is no special limitation. In the present invention, it preferably includes an aluminum oxide layer, and more preferably includes a stacked aluminum oxide layer and a silicon nitride layer; the thickness of the aluminum oxide layer is preferably 2 to 20 nm; the thickness of the silicon nitride layer is preferably 60 to 200 nm.
[0057] The back side of the silicon substrate is provided with a second electrode, that is, the non-columnar hole area of the silicon substrate is provided with a second electrode; the polarity of the second electrode is opposite to that of the first electrode, and they are insulated from each other; the shape of the second electrode is preferably cylindrical; the diameter of the second electrode is preferably 10 to 30 μm; the type of the second electrode is preferably a silver electrode; the number of the second electrodes is preferably multiple; the multiple second electrodes are preferably connected by a second conductive grid line, which can also be called a second conductive paste line, and the first conductive grid line or the first conductive paste does not contact the second conductive grid line or the second conductive wire paste line; further preferably, the second conductive grid line or the second conductive paste is provided on the surface of the back passivation layer to connect the multiple second Electrode; further preferably, the second conductive grid line or the second conductive paste line is connected to the second electrode in a serpentine shape, see Figure 3, Figure 3 is a schematic diagram of the electrode arrangement of the back-contact solar cell provided by the present invention, wherein the black dot is the first electrode, the black line is the first conductive grid line or the first conductive paste line, the red dot is the second electrode, and the red line is the second conductive grid line or the second conductive paste line; the width of the second conductive grid line or the second conductive paste line is preferably 100 to 2000 μm; the type of the second conductive grid line or the second conductive paste can be any type familiar to those skilled in the art, and there is no special limitation. In the present invention, aluminum paste is preferably used (sintered and formed according to a method familiar to those skilled in the art).
[0058] The front side of the silicon substrate is a pyramid velvet surface; a front side passivation layer is provided on the front side of the silicon substrate; the front side passivation layer is provided on the surface of the light-receiving side of the silicon substrate; the thickness of the front side passivation layer is preferably 57 to 120 nm; the front side passivation layer can be a front side passivation layer well known to those skilled in the art, and there is no special limitation. In the present invention, it is preferably an aluminum oxide layer, and more preferably includes a stacked aluminum oxide layer, a silicon nitride layer and a silicon oxide layer; the aluminum oxide layer has a high-density fixed negative charge and is suitable for surface passivation of p-type silicon wafers; the thickness of the aluminum oxide layer is preferably 2 to 20 nm; the thickness of the silicon nitride layer is preferably 50 to 80 nm; the thickness of the silicon oxide layer is preferably 5 to 20 nm.
[0059] The present invention utilizes columnar holes and / or conical hole structures to arrange the back field area, which can make full use of the thickness of the silicon substrate. The bottom area and the sidewalls of the holes formed form the back field area, thereby increasing the back field collection area without occupying the back surface area, and maximizing the back emission area. For a solar cell, within a certain proportion range, the larger the proportion of the emitter area, the higher the capture and transmission performance of minority carriers, and the higher the efficiency of the cell. At the same time, the back field area penetrates deep into the silicon wafer, so that the majority carriers can be collected inside the silicon wafer, shortening the transmission and collection distance and enhancing the collection effect, so that the structure has an enhanced collection effect on both minority carriers and majority carriers, thereby improving the efficiency of the cell as a whole.
[0060] The present invention also provides a method for preparing the above-mentioned back-contact solar cell, comprising the following steps: S1) depositing an intrinsic amorphous silicon layer on the back side of a silicon substrate; S2) performing a first doping treatment on the silicon substrate on which the intrinsic amorphous silicon layer is deposited to form a doped polycrystalline silicon layer; S3) printing an acidic etching material on the back side of the silicon substrate on which the doped polycrystalline silicon layer is formed, and performing a polishing treatment to form columnar holes and / or conical holes; S4) performing a second doping treatment on the silicon substrate on which the columnar holes and / or conical holes are formed to form a doped back field layer; S5) acid-washing the silicon substrate on which the doped back field layer is formed; S6) preparing a first electrode electrically in contact with the doped back field layer and a second electrode electrically in contact with the doped polycrystalline silicon layer on the back side of the acid-washed silicon substrate, respectively, to obtain a back-contact solar cell; the first electrode and the second electrode have opposite polarities and are insulated from each other.
[0061] The present invention has no particular limitation on the sources of all raw materials, and any commercially available raw materials may be used.
[0062] In the present invention, it is preferred to first perform double-sided polishing on the silicon substrate; the double-sided polishing method is a method well known to those skilled in the art and is not particularly limited. In the present invention, alkali polishing is preferably used; the alkali in the alkaline polishing liquid used for the alkali polishing is preferably one or more of potassium hydroxide, sodium hydroxide and tetramethylammonium hydroxide (TMAH); the mass concentration of the alkali in the alkaline polishing liquid is preferably 5% to 20%; in addition to the alkali, the alkaline polishing liquid may also be added with polishing additives, which is conducive to a smoother surface; the temperature of the polishing treatment is preferably 60°C to 90°C; the polishing treatment can remove surface cutting damage, smooth the surface, and reduce surface defects.
[0063] Then, an intrinsic amorphous silicon layer is deposited on the back side of the silicon substrate, and more preferably, a tunneling oxide layer is first deposited on the back side of the silicon substrate and then the intrinsic amorphous silicon layer is deposited; in the present invention, the tunneling oxide layer can be a silicon oxide layer, a silicon oxynitride layer or a silicon nitride layer; the method for depositing the tunneling oxide layer can be a method well known to those skilled in the art, and there is no special limitation. In the present invention, one or more of LPCVD (low-pressure chemical vapor deposition), PECVD (plasma chemical vapor deposition) and PEALD (plasma enhanced atomic layer deposition) are preferably used; the thickness of the tunneling oxide layer is preferably 0.1 to 5 nm; the method for depositing the intrinsic amorphous silicon layer can be a method well known to those skilled in the art, and in the present invention, one or more of LPCVD, PEALD and PVD (physical deposition) are used; the thickness of the intrinsic amorphous silicon layer is preferably 30 to 300 nm.
[0064] The silicon substrate on which the intrinsic amorphous silicon layer is deposited is subjected to a first doping treatment to form a doped polysilicon layer; the doping treatment method is selected according to the type of the silicon substrate and the doping element in the doped polysilicon layer; when the silicon substrate is a P-type silicon substrate, this step is preferably a diffusion of a V group element or an ion implantation of a V group element, more preferably a phosphorus diffusion or an ion implantation of phosphorus; the phosphorus diffusion is preferably a high-temperature tubular phosphorus diffusion; the phosphorus source of the phosphorus diffusion is preferably phosphorus oxychloride; the temperature of the phosphorus diffusion is preferably 930° C. to 980° C.; the time of the phosphorus diffusion is preferably 60 to 80 minutes; the energy of the phosphorus ion implantation is preferably 5 to 200 keV; the dose of the phosphorus ion implantation is preferably 1*10 19 / cm 3 ~10*10 19 / cm 3 ; After the ion implantation of phosphorus, an oxidation annealing treatment is preferably performed; the temperature of the oxidation annealing treatment is preferably 900℃~980℃; the time of the oxidation annealing treatment is preferably 30~50min; the oxidation annealing treatment is preferably performed in an air atmosphere; the square resistance of the silicon substrate after phosphorus diffusion or ion implantation of phosphorus is preferably 20~80Ω / □, more preferably 20~50Ω / □. In this process, a silicon oxide layer containing phosphorus elements is formed on the surface, commonly known as PSG layer, with a thickness of preferably 40~60nm; when this step is phosphorus diffusion for doping, a conventional phosphorus-doped emitter will also be formed on the front side, which plays the role of absorbing impurities. In the subsequent texturing step, the emitter and the absorbed impurities will be removed together. And in this step, the intrinsic amorphous silicon will be transformed into the corresponding doped polysilicon. When the silicon substrate is an N-type silicon substrate, the first doping treatment is preferably doping with group III elements, more preferably boron diffusion; the boron diffusion is preferably a high-temperature tubular boron diffusion treatment; the boron source for the boron diffusion is preferably boron trichloride and / or boron tribromide; the temperature of the boron diffusion is preferably 930°C to 980°C; the time of the boron diffusion is preferably 60 to 80 minutes; the square resistance of the silicon substrate after the boron diffusion treatment is preferably 20 to 80Ω / □, more preferably 40 to 50Ω / □; during this process, a silicon oxide layer containing boron elements is formed on the surface, commonly known as a BSG layer, with a thickness of preferably 40 to 60nm.
[0065] An acidic etching material is printed on the back of the silicon substrate on which the doped polysilicon layer is formed; in the present invention, the acidic etching material is printed according to the distribution of columnar holes and / or conical holes by screen printing, and the acidic etching material can remove the PSG or BSG formed during the first doping process, exposing the underlying silicon substrate; the acidic etching material preferably includes oxalic acid, a surfactant, a thickener, modified silicon dioxide, deionized water and sodium fluoride, which can corrode the PSG layer or BSG layer at room temperature or under heating conditions; the mass concentration of oxalic acid in the acidic etching material is preferably 5% to 20%; the acidic etching material The surfactant concentration in the material is preferably 5% to 10% by mass; the surfactant is preferably sodium citrate; the thickener concentration in the acidic etching material is preferably 10% to 20% by mass; the thickener is preferably a resin; the modified silica concentration in the acidic etching material is preferably 20% to 40% by mass; the modified silica is preferably surface-smoothed silica particles with a diameter of 10 to 20 μm; the deionized water concentration in the acidic etching material is preferably 5% to 20% by mass; and the sodium fluoride concentration in the acidic etching material is preferably 1% to 10% by mass. After printing the acidic etching material, the residual etching material is washed away, and the PSG or BSG layer on the back side, where the acidic etching material is not printed, remains. This layer can serve as an alkali barrier to protect the underlying doped polysilicon layer during the polishing process. As a byproduct of the initial doping process, the PSG or BSG layer acts as a barrier to alkali etching, eliminating the need to deposit a separate silicon oxide or silicon nitride layer as an alkali etching barrier, reducing process steps and costs.
[0066] The silicon substrate from which the acidic corrosive material has been cleaned is polished to form cylindrical holes and / or conical holes. The polishing method is any method well known to those skilled in the art and is not particularly limited. In the present invention, alkali polishing is preferably used. The alkali in the alkaline polishing solution used for the alkali polishing is preferably one or more of potassium hydroxide, sodium hydroxide and tetramethylammonium hydroxide (TMAH). The mass concentration of the alkali in the alkaline polishing solution is preferably 5% to 20%. In addition to the alkali, the alkaline polishing solution may also contain a polishing additive to protect the oxide layer and ensure that the PS The PSG or BSG layer is not back-etched, and preferably, 30 to 50 nm of the PSG or BSG layer remains. The polishing temperature is preferably 60°C to 90°C. The area not protected by the PSG or BSG layer forms a polished flat structure, i.e., the patterned area on the back side has a polished structure with a certain depth, forming cylindrical holes and / or tapered holes. The depth of the cylindrical holes and / or tapered holes is preferably 30% to 80% of the thickness of the silicon wafer. In this step, the front surface of the silicon substrate is protected by the PSG or BSG layer and is not polished. See Figure 4, which shows the structure of the P-type silicon substrate after etching and polishing to form cylindrical holes.
[0067] The silicon substrate with the columnar holes and / or the conical holes formed therein is subjected to a second doping treatment to form a doped back surface field layer. The method of the second doping treatment can be selected according to the type of silicon substrate and the doping element in the doped polysilicon layer. When the silicon substrate is a P-type silicon substrate, this step is preferably doping with a Group III element, more preferably boron diffusion. The method of the boron diffusion is the same as described above and will not be repeated here. When the silicon substrate is an N-type silicon substrate, this step is preferably group V element diffusion or ion implantation of a Group V element, more preferably phosphorus diffusion or phosphorus ion implantation. The methods of phosphorus diffusion and phosphorus ion implantation are the same as described above and will not be repeated here. See Figure 5, which is a schematic diagram of the structure of the P-type silicon substrate after the second doping treatment to form a doped back surface field layer.
[0068] Since a PSG layer or a BSG layer will be formed on the front side of the silicon substrate during the first doping treatment, it is preferred to remove the PSG layer or the BSG layer on the front side of the silicon substrate forming the doped back field layer, then perform a texturing treatment, and then perform pickling to remove the PSG layer and the BSG layer on the back side; the PSG layer or the BSG layer on the front side is preferably removed by chain removal, and the solution for the chain removal is preferably a hydrofluoric acid solution, more preferably a 1% to 10% hydrofluoric acid solution; the texturing treatment solution is preferably an alkaline solution; the alkali in the texturing treatment solution is preferably one or more of potassium hydroxide, sodium hydroxide and tetramethylammonium hydroxide (TMAH); the mass concentration of the alkali in the texturing treatment solution is preferably 5% to 20%; during the texturing treatment, a texturing additive is preferably added; the additive is preferably an additive with the function of protecting the oxide layer; the texturing treatment makes the front side of the silicon substrate a pyramid velvet surface, which plays a sinking role. The back side is protected by the oxide layer and does not experience texturing. After texturing the front surface, the BGS layer and PSG layer on the back surface are removed by pickling; the pickling solution is preferably a hydrofluoric acid solution, more preferably a hydrofluoric acid solution with a concentration of 1% to 10%. See Figure 6, which is a schematic diagram of the structure of the silicon substrate after pickling.
[0069] According to the present invention, a back passivation layer is preferably deposited on the back side of the silicon substrate after pickling, and more preferably a front passivation layer is also deposited on the front side of the silicon substrate after pickling; the present invention has no special restrictions on the order of deposition of the front passivation layer and the back passivation layer, and the front passivation layer can be deposited first or the back passivation layer can be deposited first without special restrictions; in the present invention, in order to save preparation steps, the front passivation layer and the back passivation layer are preferably prepared at the same time, and more preferably prepared in the same reaction chamber; the types of the front passivation layer and the back passivation layer are the same as described above and will not be repeated here; in the present invention, it is further preferred that the front passivation layer and the back passivation layer are preferably formed by double-sided aluminum oxide coating on the silicon substrate after pickling; the method for depositing the front passivation layer and the back passivation layer can be a method well known to those skilled in the art, and there are no special restrictions. In the present invention, PECVD, ALD or PEALD is preferred.
[0070] A first electrode electrically contacting the doped back field layer and a second electrode electrically contacting the doped polysilicon layer are respectively prepared on the back side of the silicon substrate on which the back passivation layer is deposited, that is, a first electrode is prepared in the columnar holes and / or conical holes on the back side of the silicon substrate on which the back passivation layer is deposited, and a second electrode is prepared in the non-columnar hole area to obtain a back-contact solar cell; the first electrode is preferably prepared according to the following method: openings are made in the columnar holes and / or conical holes using a laser or acid etching material, the back passivation layer in the opening area is removed, and the first electrode is printed. In the present invention, a first conductive paste is preferably printed at the same time to form a first conductive paste line connecting the first electrode; the diameter of the opening is preferably 10 to 50 μm; the first electrode is preferably a low-corrosion aluminum paste or a non- Corrosive aluminum; the first conductive paste is preferably a low-corrosive aluminum paste or a non-corrosive aluminum paste; the preparation method of the second electrode is preferably specifically as follows: printing a corrosive paste in the non-columnar hole area to form a second electrode, and then printing a second conductive paste to form a second conductive paste line to connect the second electrode; the corrosive paste is preferably a corrosive silver paste; the glass body in the corrosive paste can open the back passivation layer, so that the paste contacts the doped polysilicon layer; the second conductive paste is preferably a low-corrosive aluminum paste or a non-corrosive aluminum paste; finally, electrical contact is preferably formed by sintering to obtain a back-contact solar cell; the sintering temperature is preferably 600°C to 800°C; the sintering time is preferably 2 to 5 minutes.
[0071] In order to further illustrate the present invention, a back-contact solar cell and a preparation method thereof provided by the present invention are described in detail below with reference to examples.
[0072] The reagents used in the following examples are all commercially available; the polishing additive used in the examples is: Tuobang New Energy Co., Ltd., model PI10V02 polishing additive; the resin thickener used in the examples is: Xiamen Haoer New Materials Co., Ltd., model HR575; the silica particles with smoothed surface are: Xiamen Haoer New Materials Co., Ltd., model HR575; the texturing additive is: Tuobang New Energy Co., Ltd., model EP32.
[0073] Example 1
[0074] 1.1: Double-sided polishing of P-type silicon wafer
[0075] Conventional alkaline polishing, 10% potassium hydroxide solution, 1% polishing additive, chemical reaction at 80℃ for 300s, the purpose is to remove surface cutting damage, smooth the surface and reduce surface defects.
[0076] 1.2: Backside deposition of tunneling layer and intrinsic amorphous silicon layer
[0077] A tunneling layer silicon oxide layer is deposited on the back using LPCVD (low pressure chemical vapor deposition) with a thickness of 1.5 nm, and then intrinsic amorphous silicon is deposited using LPCVD with a thickness of 150 nm.
[0078] 1.3: Double-sided phosphorus diffusion
[0079] The silicon wafer obtained in 1.2 was subjected to double-sided phosphorus diffusion using a high-temperature tubular diffusion process. The phosphorus source was phosphorus oxychloride (POCl3). The diffusion temperature was 950°C for 60 minutes, followed by an oxidation annealing process at 900°C in air for 30 minutes. The sheet resistance of the silicon wafer after phosphorus diffusion was 50Ω / □. This process formed a phosphorus-containing silicon oxide layer, commonly known as the PSG layer, with a thickness of 40nm.
[0080] Phosphorus diffusion is performed on both sides at this time, forming a phosphorus-doped conventional emitter on the front side, which acts as an impurity absorber. In the subsequent texturing step, this emitter and the absorbed impurities will be removed together. In this step, the intrinsic amorphous silicon will be converted into the corresponding N-type doped polysilicon.
[0081] 1.4: Printing acidic corrosive materials
[0082] After double-sided phosphorus diffusion, a PSG layer (phosphorus-containing silicon dioxide) forms on the front and back surfaces of the silicon wafer. An acidic etching material is then screen-printed in the pattern of cylindrical holes in the back surface field area. The diameter of these cylindrical holes is 100μm, and the spacing between the cylinders is 1000μm. This etching material removes the PSG in these areas, exposing the underlying P-type silicon substrate.
[0083] This etching material, composed of oxalic acid, a surfactant, a thickener, modified silica, deionized water, and sodium fluoride, corrodes the PSG layer at room temperature or under heating. The ingredients are: 10wt% oxalic acid, 8wt% sodium citrate, a surfactant, 10wt% resin thickener, 30wt% surface-smoothed silica particles, 5wt% sodium fluoride, and the balance deionized water. After printing the etching material, it is cleaned to remove any remaining etching material. The PSG layer on the back, unprinted with the acidic etching material, remains and serves as an alkali barrier during the S5 polishing process, protecting the underlying N-type doped polysilicon. (As a byproduct of the phosphorus diffusion process, the PSG layer acts as an alkali etch barrier, eliminating the need for separately depositing a silicon oxide or silicon nitride layer as an alkali etch barrier, reducing process steps and costs.)
[0084] 1.5: The cylindrical hole area on the back is polished to form a hole
[0085] After cleaning the acidic corrosive material, the silicon wafer is polished using 10% potassium hydroxide and 1% polishing additive, which protects the oxide layer. The polishing process lasts 300 seconds at 80°C. Excessive PSG etching is ensured, leaving a 30nm residual PSG layer. A polished, flat structure forms in areas not protected by the PSG layer. This means that a polished structure appears on the backside patterned area, with a depth of 50% of the wafer thickness. The front side of the wafer, protected by the PSG layer, remains unpolished.
[0086] 1.6: Backside Boron Diffusion
[0087] The silicon wafer obtained in 1.5 was subjected to backside boron diffusion using a high-temperature, tubular boron diffusion process. The boron source was boron trichloride (BCl3), the temperature was 950°C, and the diffusion time was 60 minutes. The sheet resistance of the wafer after boron diffusion was 40Ω / □. This process formed a 50nm thick silicon oxide layer containing boron, commonly known as BSG, on the surface.
[0088] 1.7: Remove the front PSG layer and the front texturing
[0089] The silicon wafer obtained in 1.6 undergoes chain removal of the PSG layer on the front side using a 5% HF solution. A texturing process is then performed in a 10% potassium hydroxide solution with a 1.5% texturing additive, which protects the oxide layer. The texturing process is performed for 400 seconds at 80°C. This results in a pyramidal velvet finish on the entire front side, providing a tack-resistant surface. The back side, protected by the oxide layer, exhibits no texturing. After texturing the front side, the BGS and PSG layers on the back side are removed by pickling using a 50% HF solution for 300 seconds.
[0090] 1.8: Front and back stack passivation
[0091] A hydrogen-containing dielectric layer is deposited on both the front and back surfaces to chemically passivate the back surface. Specifically, the back surface is passivated using a stack of aluminum oxide and silicon nitride. The aluminum oxide is produced by PECVD to a thickness of 10nm. The silicon nitride is produced by PECVD to a thickness of 100nm. The front surface is a stack of aluminum oxide, silicon nitride, and silicon oxide, all produced by PECVD, with thicknesses of 10nm, 50nm, and 5nm, respectively.
[0092] 1.9: Back metallization (distribution structure shown in Figure 3)
[0093] Laser or acid etching is used to create an opening in the cylindrical deep hole of the P zone. The diameter of the opening is 50μm. Only the dielectric layer is removed in the opening area. A low-corrosion aluminum paste (black dots) is printed above the opening area of the P zone. The shape is cylindrical, with a diameter of 50μm and a height extending to near the back surface of the silicon wafer, which acts as an electrical contact to the P zone. At the same time, a black low-corrosion aluminum paste is printed with a width of 20μm to connect the black contact points of the P zone.
[0094] Corrosive silver paste is printed locally on N-type polysilicon (the red dot is the emitter's burn-through paste contact point, with a diameter of 20μm). The glass in the corrosive silver paste can open the dielectric layer, allowing the silver to contact the N-type polysilicon. Non-corrosive connecting lines (red line segments) are then printed to connect the red contact points, with a width of 100μm. Finally, the electrodes are co-sintered at 800℃ for 3 minutes to form electrodes.
[0095] Example 2
[0096] 2.1: Double-sided polishing of P-type silicon wafer
[0097] Conventional alkaline polishing, 20% potassium hydroxide solution, 1.5% polishing additive, chemical reaction at 80 ° C for 300 seconds, the purpose is to remove surface cutting damage, smooth the surface, and reduce surface defects.
[0098] 2.2: Backside deposition of tunneling layer and intrinsic amorphous silicon layer
[0099] A tunneling layer silicon oxide layer is deposited on the back using LPCVD (low pressure chemical vapor deposition) with a thickness of 2nm, and then intrinsic amorphous silicon is deposited using LPCVD with a thickness of 250nm.
[0100] 2.3: Double-sided phosphorus diffusion
[0101] The silicon wafer obtained in 2.2 was subjected to double-sided phosphorus diffusion using a high-temperature tubular diffusion process. The phosphorus source was phosphorus oxychloride (POCl3). The diffusion temperature was 935°C for 60 minutes, followed by an oxidation annealing process at 900°C in air for 30 minutes. The sheet resistance of the silicon wafer after phosphorus diffusion was 20Ω / □. During this process, a phosphorus-containing silicon oxide layer, commonly known as PSG, was formed on the surface, with a thickness of 40nm.
[0102] Phosphorus diffusion is performed on both sides at this time, forming a phosphorus-doped conventional emitter on the front side, which acts as an impurity absorber. In the subsequent texturing step, this emitter and the absorbed impurities will be removed together. In this step, the intrinsic amorphous silicon will be converted into the corresponding N-type doped polysilicon.
[0103] 2.4: Printing acidic corrosive materials
[0104] After double-sided phosphorus diffusion, a PSG layer (phosphorus-containing silicon dioxide) forms on the front and back surfaces of the silicon wafer. An acidic etching material is then screen-printed in the pattern of cylindrical holes in the back surface field area. The diameter of these cylindrical holes is 100μm, and the spacing between the cylinders is 1000μm. This etching material removes the PSG in these areas, exposing the underlying P-type silicon substrate.
[0105] This etching material, composed of oxalic acid, a surfactant, a thickener, modified silica, deionized water, and sodium fluoride, corrodes the PSG layer at room temperature or under heating. The ingredients are: 10wt% oxalic acid, 8wt% sodium citrate, a surfactant, 10wt% resin thickener, 30wt% surface-smoothed silica particles, 5wt% sodium fluoride, and the balance deionized water. After printing the etching material, it is washed to remove any remaining etching material. The PSG layer on the back, unprinted with the acidic etching material, remains and serves as an alkali barrier during the polishing process in step 2.5, protecting the underlying N-type doped polysilicon. (As a byproduct of the phosphorus diffusion process, the PSG layer acts as an alkali etch barrier, eliminating the need for a separate silicon oxide or silicon nitride layer to serve as an alkali etch barrier, reducing process steps and costs.)
[0106] 2.5: The cylindrical hole area on the back is polished to form a hole
[0107] After cleaning the acidic corrosive material, the silicon wafer was polished using 15% potassium hydroxide and 1.2% polishing additive, which protects the oxide layer. The polishing time was 300 seconds at 80°C. Excessive PSG etching was prevented, leaving a 30nm residual PSG layer. A polished, flat structure formed in areas not protected by the PSG layer. This polished structure appeared on the backside patterned area, with a depth of 40% of the wafer thickness. The front side of the wafer, protected by the PSG layer, was not polished.
[0108] 2.6: Backside Boron Diffusion
[0109] The silicon wafer obtained in 2.5 was subjected to backside boron diffusion using a high-temperature, tubular boron diffusion process. The boron source was boron trichloride (BCl3), the temperature was 950°C, and the diffusion time was 60 minutes. After the boron diffusion, the sheet resistance of the silicon wafer was 40Ω / □. During this process, a boron-containing silicon oxide layer, commonly known as BSG, was formed on the surface, with a thickness of 40-50nm.
[0110] 2.7: Remove the front PSG layer and the front texturing
[0111] The silicon wafer obtained in 2.6 undergoes chain removal of the PSG layer on the front side using a 5% HF solution. A texturing process is then performed in a 10% potassium hydroxide solution with a 1.5% texturing additive, which protects the oxide layer. The texturing process is performed for 400 seconds at a temperature of 80°C. This results in a pyramidal velvet finish on the entire front side, providing a sunken feel. The back side, protected by the oxide layer, exhibits no texturing. After texturing the front side, the BGS and PSG layers on the back side are removed by pickling using a 50% HF solution for 300 seconds.
[0112] 2.8: Front and back stack passivation
[0113] A hydrogen-containing dielectric layer is deposited on both the front and back surfaces to chemically passivate the back surface. Specifically, the back surface is passivated using a stack of aluminum oxide and silicon nitride. The aluminum oxide is produced by PECVD to a thickness of 10nm. The silicon nitride is produced by PECVD to a thickness of 100nm. The front surface is a stack of aluminum oxide, silicon nitride, and silicon oxide, all produced by PECVD, with thicknesses of 10nm, 50nm, and 5nm, respectively.
[0114] 2.9: Back metallization (distribution structure shown in Figure 3)
[0115] Laser or acid etching is used to create an opening in the cylindrical deep hole of the P zone. The opening has a diameter of 50μm. Only the dielectric layer is removed in the opening area. A low-corrosion aluminum paste (black dots) is printed above the opening area of the P zone. The shape of the cylinder is 50μm in diameter and the height extends to near the back surface of the silicon wafer, which acts as an electrical contact to the P zone. At the same time, a black low-corrosion aluminum paste is printed with a width of 50μm to connect the black contact points of the P zone.
[0116] Corrosive silver paste is printed locally on N-type polysilicon (the red dots are the emitter burn-through paste contact points, with a diameter of 20 μm). The glass in the corrosive silver paste can open the dielectric layer, allowing the silver to contact the N-type polysilicon. Non-corrosive connecting lines (red line segments) are then printed to connect the red contact points, with a width of 100 μm. Finally, they are co-sintered at 780°C for 3 minutes to form electrodes.
[0117] The back-contact solar cells obtained in Example 1 and Example 2 were tested for performance. The testing method was as follows: 2 The battery electrical performance test was conducted using an AM1.5G light source, and the results are shown in Table 1. The conventional IBC battery in Table 1 is a "Zebra" structure IBC battery produced by State Power Investment Xining Solar Power Co., Ltd., with a size of 166*166mm and a specific model of the "Andromeda" series.
[0118] Table 1 Solar cell performance test results
[0119] The specific embodiments described herein are merely illustrative of the spirit of the present invention. Persons skilled in the art may make various modifications, additions, or substitutions to the described specific embodiments without departing from the spirit of the present invention or exceeding the scope of the appended claims.
Claims
1. A back-contact solar cell, characterized in that: include: Silicon substrate; The back side of the silicon substrate is provided with columnar holes and non-columnar hole areas; The columnar hole is provided with a doped back field layer; A first electrode is provided on the back side of the silicon substrate, and the first electrode is in electrical contact with the doped back field layer; The non-columnar hole region is provided with a doped emitter layer; the doped emitter layer comprises a doped polysilicon layer; A second electrode is provided on the back side of the silicon substrate, and the second electrode is in electrical contact with the doped polysilicon layer; The first electrode and the second electrode have opposite polarities and are insulated from each other.
2. A back-contact solar cell, characterized in that: include: a silicon substrate having a first doping type; The back side of the silicon substrate is provided with columnar holes and / or conical holes and non-columnar hole areas; The columnar hole is provided with a doped back field layer, and the back field layer has a first doping type; A first electrode is provided on the back side of the silicon substrate, and the first electrode is in electrical contact with the doped back field layer; The non-columnar hole region is provided with a doped emitter layer; the doped emitter layer comprises a doped polysilicon layer; the doped polysilicon layer has a second doping type; A second electrode is provided on the back side of the silicon substrate, and the second electrode is in electrical contact with the doped polysilicon layer; The first electrode and the second electrode have opposite polarities and are insulated from each other.
3. The back-contact solar cell according to claim 1 or 2, characterized in that: The doped back field layer is arranged on the sidewall and bottom surface of the columnar hole and / or the conical hole.
4. The back-contact solar cell according to claim 1 or 2, characterized in that: The diameter of the cylindrical holes and / or conical holes is 50 to 300 μm; the number of the cylindrical holes and / or conical holes is multiple; the interval between adjacent cylindrical holes and / or conical holes is 500 to 3000 μm; the depth of the cylindrical holes and / or conical holes is 30% to 80% of the thickness of the silicon substrate.
5. The back-contact solar cell according to claim 1 or 2, characterized in that: There are multiple cylindrical holes and / or conical holes, each of which is provided with a first electrode; the multiple first electrodes are connected by a first conductive grid line; There are multiple second electrodes; the multiple second electrodes are connected by second conductive grid lines; Furthermore, the first conductive grid line does not contact the second conductive grid line.
6. The back-contact solar cell according to claim 5, characterized in that: The first conductive line is connected to the first electrode in a serpentine shape; The second conductive gate line is connected to the second electrode in a serpentine shape.
7. The back-contact solar cell according to claim 1 or 2, characterized in that: The doped emitter layer also includes a tunneling oxide layer; the tunneling oxide layer is arranged between the silicon substrate in the non-columnar hole area and the doped polysilicon layer.
8. The back-contact solar cell according to claim 7, characterized in that: The thickness of the tunneling oxide layer is 0.1-5 nm; the thickness of the doped polysilicon layer is 30-300 nm; the diameter of the first electrode is 200-100 μm; and the diameter of the second electrode is 10-30 μm.
9. The back-contact solar cell according to claim 1 or 2, characterized in that: The silicon substrate is a P-type silicon substrate; the doped back field layer is a back field layer doped with group III elements; and the doped polysilicon layer is a polysilicon layer doped with group V elements.
10. The back-contact solar cell according to claim 8, characterized in that: It also includes a front passivation layer and a back passivation layer; the front passivation layer is arranged on the surface of the light-receiving surface of the silicon substrate; the back passivation layer is arranged on the back of the silicon substrate and covers the doped back field layer and the doped polysilicon layer; the front passivation layer and the back passivation layer include aluminum oxide; the back passivation layer is provided with an opening, and the first electrode is electrically in contact with the doped back field layer through the opening; The second electrode is in electrical contact with the doped polysilicon layer through the opening.
11. The back-contact solar cell according to claim 1 or 2, characterized in that: The bottom and / or sidewall of the columnar hole and / or the conical hole is provided with a concave-convex texture structure.
12. A method for preparing a back-contact solar cell, characterized in that: The following steps are involved: S1) depositing an intrinsic amorphous silicon layer on the back side of a silicon substrate; S2) performing a first doping treatment on the silicon substrate on which the intrinsic amorphous silicon layer is deposited to form a doped polysilicon layer; S3) printing an acidic etching material on the back side of the silicon substrate on which the doped polysilicon layer is formed, and performing a polishing process to form columnar holes and / or conical holes; S4) performing a second doping treatment on the silicon substrate with the columnar holes and / or the conical holes formed therein to form a doped back field layer; S5) acid washing the silicon substrate on which the doped back field layer is formed; S6) preparing a first electrode electrically contacting the doped back field layer and a second electrode electrically contacting the doped polysilicon layer on the back side of the acid-washed silicon substrate to obtain a back-contact solar cell; the first electrode and the second electrode have opposite polarities and are insulated from each other.
13. The preparation method according to claim 12, characterized in that: The first doping treatment in step S2) is double-sided diffusion doping, and after step S4), it also includes a front surface texturing treatment to remove the doping layer formed on the front surface during the first doping treatment.
14. The preparation method according to claim 12, characterized in that: In the step S3), the acidic corrosion material includes oxalic acid, a surfactant, a thickener, modified silicon dioxide, deionized water and sodium fluoride; the mass concentration of oxalic acid in the acidic corrosion material is 5% to 20%; the mass concentration of the surfactant in the acidic corrosion material is 5% to 10%; the mass concentration of the thickener in the acidic corrosion material is 10% to 20%; the mass concentration of the modified silicon dioxide in the acidic corrosion material is 20% to 40%; the mass concentration of the deionized water in the acidic corrosion material is 5% to 20%; the mass concentration of the sodium fluoride in the acidic corrosion material is 1% to 10%.
15. The preparation method according to claim 12, characterized in that: After step S5), the method further includes depositing a back passivation layer on the back side of the pickled silicon substrate and depositing a front passivation layer on the front side of the pickled silicon substrate; the back passivation layer and the front passivation layer are prepared in the same reaction chamber.
16. The preparation method according to claim 15, characterized in that: The back passivation layer and the front passivation layer are prepared by double-sided aluminum oxide coating on a pickled silicon substrate.
17. The preparation method according to claim 12, characterized in that: In the step S6), the first electrode is prepared according to the following method: openings are made in the columnar holes and / or conical holes by using laser or acid etching materials, the back passivation layer in the opening area is removed, and the first electrode is printed.
18. The preparation method according to claim 17, characterized in that: When printing the first electrode, a first conductive paste is printed to form a first conductive paste line to connect the first electrode; the first electrode is low-corrosive aluminum paste or non-corrosive aluminum; the first conductive paste is low-corrosive aluminum paste or non-corrosive aluminum paste.
19. The preparation method according to claim 12, characterized in that: The preparation method of the second electrode is specifically as follows: printing a corrosive paste in the non-columnar hole area to form the second electrode, and then printing a second conductive paste to form a second conductive paste line to connect the second electrode; the corrosive paste is a corrosive silver paste; the second conductive paste is a low-corrosive aluminum paste or a non-corrosive aluminum paste.
20. The preparation method according to claim 12, characterized in that: The process of preparing a first electrode electrically contacting a doped back field layer and a second electrode electrically contacting a doped polysilicon layer on the back of a pickled silicon substrate includes sintering to form electrical contact; the sintering temperature is 600°C to 800°C; and the sintering time is 2 to 5 minutes.
Citation Information
Patent Citations
Interdigitated back-contacted solar cell with p-type conductivity
CN111108609A
Crystalline silicon back junction solar cell preparation method
CN103618025A
Full back side contact crystalline silicon cell and preparation method thereof
CN103904138A
Back contact type solar cell and preparation method thereof
CN116525697A
Solar cell and method of manufacture
US7339110B1
Cited By
Heterojunction solar cell and manufacturing method therefor, and device
WO2026113067A1