Separator film, preparation method therefor, battery, and electrical apparatus

By arranging an intermediate layer in the middle layer of the isolation film and using it to polymerize at a higher temperature to reduce the porosity, the problem of insufficient stability of the isolation film at high temperatures is solved, and the thermal stability and ion conductivity of the battery are improved.

WO2024221900A1PCT designated stage expired Publication Date: 2024-10-31CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/134693
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2023-11-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing isolation films have poor stability at higher temperatures, leading to the risk of thermal runaway in batteries.

Method used

An intermediate layer is provided on one side of the base material of the isolation membrane so that it has a higher porosity at a lower temperature to facilitate ion conduction, and at a higher temperature the porosity is reduced through the polymerization of the intermediate layer components to isolate ion conduction. This alleviates the problem of continuous heating caused by positive and negative ion exchange at high temperatures.

Benefits of technology

It effectively improves the thermal stability of the isolation film, reduces the probability of thermal runaway of the battery, and maintains good ion conductivity during charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023134693_31102024_PF_FP_ABST
    Figure CN2023134693_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present application are a separator film, a preparation method therefor, a battery and an electrical apparatus. The separator film comprises: a first substrate and a middle layer located on at least one side surface of the first substrate. The porosity of the separator film at a first temperature is a, and the porosity of the separator film at a second temperature is b, the first temperature being -20℃~100℃, 40%≤a≤70%, the second temperature being not lower than 120℃, and b≤2%.
Need to check novelty before this filing date? Find Prior Art

Description

Isolation film and preparation method thereof, battery and electrical device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the priority benefit of Chinese patent application No. 202310473685.0 filed on April 27, 2023, and incorporates the entirety of the application into this document. Technical Field

[0003] The present application relates to the field of battery technology, and in particular to an isolation membrane and a preparation method thereof, a battery, and an electrical device. Background Art

[0004] In a battery's structure, the separator is a key internal layer. It isolates the positive and negative electrodes, preventing them from short-circuiting. It also conducts ions during battery operation. Current separators have poor stability at elevated temperatures, leading to the risk of thermal runaway.

[0005] Therefore, the current isolation membrane and its preparation method, battery and electrical device still need to be improved.

[0006] Summary of the Invention

[0007] The present application aims to alleviate or solve at least one of the above-mentioned problems to at least some extent.

[0008] In one aspect, the present application proposes a separator. In some embodiments of the present application, the separator comprises: a first substrate, and an intermediate layer located on at least one side of the first substrate. The separator has a porosity of a at a first temperature and a porosity of b at a second temperature. The first temperature is between -20°C and 100°C, with a value of 40% ≤ a ≤ 70%, and the second temperature is no less than 120°C, with a value of b ≤ 2%. Thus, the separator has a higher porosity at lower temperatures, facilitating the passage of ions. At higher temperatures, the separator's porosity decreases significantly, blocking the separator's pores and at least partially isolating ion conduction. This mitigates the continuous temperature rise caused by the exchange of positive and negative ions at higher temperatures, thereby reducing the probability of thermal runaway in the battery.

[0009] In some embodiments of the present application, the third temperature is between -20°C and 120°C. At the third temperature, the intermediate layer includes a first monomer that satisfies at least one of the following conditions: the first monomer molecule contains a cyclic structure, the number of atoms in the cyclic structure is 7 or less, and the cyclic structure has a first functional group; the molecular weight of the first monomer is not less than 90; and the polymerization temperature of the first monomer is not less than 120°C. As a result, the first monomer is less likely to polymerize at lower temperatures, allowing the isolation membrane to maintain a high porosity, which is beneficial for ion conduction.

[0010] In some embodiments of the present application, the mass content of the first monomer is 0.1 wt% to 20 wt% based on the total mass of the isolation membrane. Thus, the isolation membrane contains an appropriate amount of the first monomer, and polymerization of the first monomer at a higher temperature can significantly reduce the porosity of the isolation membrane, thereby improving the thermal stability of the isolation membrane.

[0011] In some embodiments of the present application, the intermediate layer further includes an inorganic filler, and the inorganic filler satisfies at least one of the following conditions: the inorganic filler includes an inert inorganic filler, and the inert inorganic filler includes at least one of silicon dioxide, titanium dioxide, zinc oxide, zirconium oxide, magnesium oxide, barium oxide, aluminum oxide, barium titanate, and magnesium hydroxide; the inorganic filler includes an active inorganic filler, and the active inorganic filler includes at least one of garnet-type solid electrolyte, perovskite-type solid electrolyte, antiperovskite-type solid electrolyte, sodium superion conductor-type solid electrolyte, and lithium phosphorus nitrogen oxide-type solid electrolyte; the surface of the inorganic filler has a second functional group, and the second functional group includes at least one of amino, epoxy, carbon-carbon double bond, aldehyde, hydroxyl, furfuryl, imide, and isocyanate. Therefore, the inorganic filler can reduce the thermal shrinkage of the isolation membrane and improve the puncture resistance of the isolation membrane, thereby further improving the performance of the isolation membrane.

[0012] In some embodiments of the present application, the inorganic filler has a mass content of 1 wt% to 20 wt% based on the total mass of the separator. Thus, the above-mentioned content of inorganic filler can significantly improve the thermal shrinkage and puncture resistance of the separator without significantly adversely affecting ion conduction.

[0013] In some embodiments of the present application, the intermediate layer further includes an oligomer containing stable free radicals. The oligomer satisfies at least one of the following conditions: the oligomer is a polymer consisting of 2-20 repeating units; the molecular weight of the oligomer is 200-10,000; and the stable free radicals include at least one of trityl, nitro, and nitroxide radicals. Thus, the stable free radicals contained in the oligomer can react with the first monomer at a higher temperature, causing the first monomer to polymerize faster, thereby reducing the porosity of the isolation membrane at higher temperatures.

[0014] In some embodiments of the present application, the nitrogen oxide free radical includes at least one of 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxide monomer, poly-2,2,6,6-tetramethylpiperidine-4-methylacrylate-1-nitroxide free radical and 2,2,6,6-tetramethyl-piperidine nitroxide free radical.

[0015] In some embodiments of the present application, the oligomer includes at least one of a polythiophenephenoxy polymer, an aromatic methyl radical polymer, a nitroxide-functionalized polyacrylamine dendrimer, a conjugated radical polymer, a comb-like nitroxide radical polymer, a polyethyleneamine-loaded nitroxide radical polymer, and a polyethyleneamine-loaded nitro radical polymer.

[0016] In some embodiments of the present application, the oligomer content is 0.1 wt%-10 wt% based on the total mass of the isolation membrane. Thus, at a higher temperature, the oligomer can rapidly polymerize the first monomer and quickly reduce the porosity of the isolation membrane.

[0017] In some embodiments of the present application, the isolation film further includes a second substrate, which is located on a side of the intermediate layer away from the first substrate. Thus, the second substrate can cooperate with the first substrate to encapsulate the intermediate layer to form a structurally stable film layer.

[0018] In some embodiments of the present application, the first substrate and the second substrate each independently include at least one of polyamide, polyamide-imide, polyketone, polysulfone, polyphenylene sulfide, polyphenylene oxide, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl chloride, polyolefin, perfluoroalkoxyalkane, polyester, liquid crystal polymer, polyoxymethylene, acrylonitrile styrene acrylate, styrene acrylonitrile, acrylonitrile butadiene styrene, polybenzimidazole, polyparaphenylene copolymer, polyacrylonitrile, polyethyleneimine, ethylene tetrafluoroethylene, polychlorotrifluoroethylene, aramid, polyetherimide, polyparaphenylene benzobisoxazole, and cellulose. Thus, both the first substrate and the second substrate have good electronic insulation properties, can better isolate the positive electrode and the negative electrode, have good ion conductivity, can conduct ions during charge and discharge; and have a certain mechanical strength, can resist dendrite puncture to a certain extent.

[0019] In another aspect of the present application, a method for preparing the aforementioned isolation membrane is provided. In some embodiments of the present application, the method for preparing the aforementioned isolation membrane includes: providing a first substrate; preparing an intermediate layer precursor solution, wherein the intermediate layer precursor solution includes an electrolyte and a first monomer; coating the intermediate layer precursor solution on at least one surface of the first substrate to form an intermediate layer precursor solution coating layer; and performing a heat treatment to obtain the isolation membrane. The isolation membrane thus prepared possesses all the characteristics and advantages of the isolation membrane described above, which will not be further elaborated here. The method is simple to operate and easy to implement, and is conducive to improving product yield.

[0020] In some embodiments of the present application, prior to the heat treatment, the method for preparing the aforementioned isolation film further includes: disposing a second substrate on a side of the intermediate layer precursor coating layer away from the first substrate. Thus, the second substrate can cooperate with the first substrate to secure the intermediate layer precursor coating layer.

[0021] In some embodiments of the present application, the intermediate layer precursor solution further includes at least one of an inorganic filler, an oligomer, a second monomer, and an initiator. Thus, the inorganic filler has good thermal stability, which helps improve the thermal stability of the isolation membrane; the oligomer can react with the first monomer at a higher temperature, rapidly reducing the porosity of the isolation membrane; the second monomer can be cured at a lower temperature; and the initiator can induce micro-crosslinking and curing of some components in the intermediate layer precursor solution, allowing the intermediate layer precursor solution coating to quickly form an intermediate layer.

[0022] In some embodiments of the present application, the method for preparing the aforementioned isolation membrane satisfies at least one of the following conditions: the electrolyte comprises ethyl methyl carbonate, fluoroethylene carbonate, and lithium bis(fluorosulfonyl)imide; the second monomer comprises pentaerythritol triacrylate; the heat treatment temperature is 60°C-70°C; and the heat treatment duration is 1 hour-20 hours. This allows the electrolyte to conduct lithium ions; and setting the heat treatment temperature or duration within the aforementioned ranges allows for micro-crosslinking and curing of some components in the intermediate layer precursor solution, resulting in an isolation membrane with excellent performance.

[0023] In another aspect of the present application, a battery is provided. In some embodiments of the present application, the battery includes a positive electrode sheet, a negative electrode sheet, and a separator positioned between the positive and negative electrode sheets, wherein the separator includes the aforementioned separator. Thus, the battery possesses all the features and advantages of the separator described above, which will not be further elaborated here. Overall, the battery has good thermal stability and a low probability of thermal runaway.

[0024] In another aspect of the present application, an electrical device is provided. In some embodiments of the present application, the electrical device includes the aforementioned battery. Thus, the electrical device has all the features and advantages of the aforementioned battery, which will not be further elaborated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0026] FIG1 shows a schematic structural diagram of an isolation membrane according to an embodiment of the present application;

[0027] FIG2 shows a schematic structural diagram of an isolation membrane according to another embodiment of the present application;

[0028] FIG3 shows a schematic structural diagram of an isolation membrane according to another embodiment of the present application;

[0029] FIG4 shows a schematic structural diagram of an isolation membrane according to another embodiment of the present application;

[0030] FIG5 shows a schematic structural diagram of a battery according to an embodiment of the present application;

[0031] FIG6 shows an exploded view of the battery in FIG5 ;

[0032] FIG7 shows a schematic structural diagram of a battery module according to an embodiment of the present application;

[0033] FIG8 shows a schematic structural diagram of a battery pack according to an embodiment of the present application;

[0034] FIG9 shows an exploded view of the battery pack in FIG8 ;

[0035] FIG10 shows a schematic structural diagram of an electrical device using a battery as a power source according to an embodiment of the present application.

[0036] Explanation of reference numerals: 100: separator; 110: first substrate; 120: intermediate layer; 130: second substrate; 1: battery pack; 2: upper case; 3: lower case; 4: battery module; 5: battery; 51: housing; 52: electrode assembly; 53: cover plate. DETAILED DESCRIPTION

[0037] The following describes in detail embodiments of the present application. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application and are not to be construed as limiting the present application.

[0038] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0039] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0041] In a battery structure, the separator serves to separate the positive and negative electrodes and conduct ions. At higher temperatures, if the separator continues to conduct ions, the exchange of positive and negative ions at high temperatures may cause a continuous rise in temperature, leading to the risk of thermal runaway. By providing an intermediate layer on one side of the separator substrate, the separator has a higher porosity at lower temperatures, allowing for better ion conduction during charge and discharge. Furthermore, by lowering the separator's porosity at higher temperatures, it hinders ion conduction at high temperatures, thereby alleviating the continuous temperature rise caused by the exchange of positive and negative ions at high temperatures and reducing the risk of thermal runaway.

[0042] Typically, the separator can be applied to a liquid electrolyte battery or a semi-solid electrolyte battery. For example, the separator can be applied to a liquid electrolyte lithium-ion battery, a semi-solid electrolyte lithium-ion battery, and the like.

[0043] The battery disclosed in the embodiments of the present application can be used in electrical devices that use the battery as a power source or various energy storage systems that use the battery as an energy storage element. The electrical device can be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, and the like. Among them, the electric toy can include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and the like, and the spacecraft can include airplanes, rockets, space shuttles, and spacecraft, and the like.

[0044] In one aspect, the present application provides an isolation film. In some embodiments of the present application, referring to FIG. 1 to FIG. 4 , the isolation film 100 may include a first substrate 110 and an intermediate layer 120 located on at least one side of the first substrate 110 . Among them, the porosity of the isolation membrane 100 at the first temperature is a, and the porosity of the isolation membrane 100 at the second temperature is b. The first temperature can be -20℃~100℃, 40%≤a≤70%. For example, the first temperature can be -20℃, -10℃, -5℃, 0℃, 10℃, 30℃, 50℃, 80℃, 100℃, etc., a can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, etc., the second temperature can be not less than 120℃, b≤2%, for example, the second temperature can be 120℃, 130℃, 150℃, 170℃, etc., b can be 0.2%, 0.5%, 1%, 1.5%, 1.8%, 2%, etc.

[0045] Herein, the term "porosity" refers to the percentage of the total volume of pores in the separator to the total volume of the separator in its natural state. At lower temperatures, the separator has a higher porosity, allowing for better ion conduction during charge and discharge. At higher temperatures, some components in the intermediate layer undergo polymerization, reducing the separator's porosity and increasing the battery's internal resistance. This can at least partially isolate ion conduction, effectively alleviating or even resolving the problem of continued temperature rise caused by positive and negative ion exchange at higher temperatures, thereby reducing the probability of thermal runaway and improving the battery's thermal stability.

[0046] In some embodiments of the present application, referring to Figures 1 and 3 , in the isolation film 100, one surface of the first substrate 110 may be provided with an intermediate layer 120. In other embodiments of the present application, referring to Figures 2 and 4 , in the isolation film 100, both surfaces of the first substrate 110 may be provided with intermediate layers 120.

[0047] In some embodiments of the present application, referring to Figures 3 and 4 , the isolation film 100 may further include a second substrate 130, which is located on a side of the intermediate layer 120 away from the first substrate 110. Thus, the second substrate can cooperate with the first substrate to firmly encapsulate the intermediate layer, thereby improving the structural stability of the isolation film.

[0048] In some embodiments of the present application, referring to FIG3 , the isolation film 100 includes a first substrate 110, an intermediate layer 120, and a second substrate 130 stacked in sequence. In other embodiments of the present application, referring to FIG4 , the intermediate layer 120 is disposed on both surfaces of the first substrate 110, and the second substrate 130 is disposed on the surface of each intermediate layer 120 away from the first substrate 110.

[0049] In some embodiments of the present application, the first substrate 110 and the second substrate 130 may each independently include at least one of polyamide (PA), polyamideimide (PAI), polyketone, polysulfone (PSU), polyphenylene sulfide (PPS), polyphenylene ether (PPE), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl chloride (PVC), polyolefin, perfluoroalkoxyalkane (PFA), polyester, liquid crystal polymer (LCP), polyoxymethylene (POM), acrylonitrile styrene acrylate (ASA), styrene acrylonitrile (SAN), acrylonitrile butadiene styrene (ABS), polybenzimidazole (PBI), polyparaphenylene copolymer (PPP), polyacrylonitrile, polyethyleneimine, ethylene tetrafluoroethylene (ETFE), polychlorotrifluoroethylene (PCTFE), aramid, polyetherimide (PEI), polyparaphenylene benzobisoxazole and cellulose. In some embodiments of the present application, the first substrate 110 and the second substrate 130 can each be independently composed of one of the aforementioned materials; in some embodiments of the present application, the first substrate 110 and the second substrate 130 can each be independently composed of two or more of the aforementioned materials. As substrates, these materials possess a certain strength and can provide good support for the intermediate layer. These materials all have excellent electronic insulation and ion conductivity, serving to isolate the positive and negative electrodes and conduct ions.

[0050] It should be noted that the polyparaphenylene copolymer may include at least one of a polyparaphenylene vinylene copolymer, a polyparaphenylene ethylene copolymer, and the like.

[0051] In some embodiments of the present application, the first substrate and the second substrate may each independently include a polyketone, for example, polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneetherketoneketone (PEKEKK), etc.

[0052] In some embodiments of the present application, the first substrate and the second substrate may each independently include polyamide, for example, polyamide 46 (PA46), polyamide 66 (PA66), polyamide 12 (PA12), polyamide 11 (PA11), polyamide 6 (PA6), polyamide 6.6 (PA6.6), polyamide 6.6 / 6 (PA6.6 / 6), amorphous polyamide (PA6-3-T), polyphthalamide (PPA), etc.

[0053] In some embodiments of the present application, the first substrate and the second substrate may each independently include polysulfone, for example, polyphenylsulfone (PPSU), polyethersulfone (PES), etc.

[0054] In some embodiments of the present application, the first substrate and the second substrate may each independently include polyester, for example, polyethylene terephthalate (PET), polycarbonate (PC), polybutylene terephthalate (PBT), polymethyl methacrylate (PMMA), etc.

[0055] In some embodiments of the present application, the first substrate and the second substrate may each independently include polyolefins, for example, polypropylene (PP), polyethylene (PE), high-density polyethylene (HDPE), polymethylpentene (PMP), etc.

[0056] In some embodiments of the present application, the first substrate and the second substrate may each independently include aramid, for example, thienyl aramid, pyrrolyl aramid, furanyl aramid, etc.

[0057] In some embodiments of the present application, the first substrate and the second substrate can each independently include at least one of polyimide, polypropylene, aramid, thienyl aramid, pyrrolyl aramid, furanyl aramid, pyridine polyamide, polyamideimide, polyetherimide, polysulfone, polyketone, poly(p-phenylene benzobisoxazole) and cellulose. The above materials have good high-temperature shrinkage resistance and a smaller shrinkage rate at higher temperatures, which can reduce the risk of short circuit between the positive and negative electrodes at higher temperatures.

[0058] In some embodiments of the present application, the intermediate layer may include a first monomer.

[0059] "Monomer" refers to a small molecule that is capable of polymerizing with other molecules of the same or other species.

[0060] In some embodiments of the present application, the molecule of the first monomer may contain a cyclic structure, the number of atoms in the cyclic structure is less than or equal to 7, and the cyclic structure has a first functional group. Therefore, the first monomer has a large steric hindrance, the reaction activity of the first monomer is low, it is not easy to undergo polymerization reaction at a low temperature, and it is not easy to block the pores of the isolation membrane.

[0061] According to some embodiments of the present application, the first functional group may include but is not limited to a carbon-oxygen double bond, a hydrocarbon functional group (e.g., methyl, ethyl, propyl, isopropyl, butyl, isobutyl, vinyl, propenyl, etc.), a carboxyl group, an ether bond, a carbonyl group, etc.

[0062] According to some specific embodiments of the present application, the first monomer may include maleic anhydride, the molecule of maleic anhydride contains a cyclic structure, the number of atoms in the cyclic structure of maleic anhydride is 5, and the cyclic structure has a first functional group carbon-oxygen double bond. The monomer has a large steric hindrance, low reaction activity, and is not easy to undergo polymerization reaction at a low temperature.

[0063] It should be noted that the first functional group on the cyclic structure does not include a functional group formed only by atoms constituting the ring. For example, the carbon-carbon double bond and carbon-oxygen single bond in maleic anhydride do not belong to the first functional group on the maleic anhydride cyclic structure.

[0064] Herein, "steric hindrance" refers to the mutual repulsion caused by the spatial arrangement of groups within a molecule. The aforementioned monomer has a large steric hindrance, which significantly affects the reactivity of the monomer.

[0065] In some embodiments of the present application, the cyclic structure of the first monomer molecule may contain at least one heteroatom such as a nitrogen atom and an oxygen atom.

[0066] In some embodiments of the present application, the molecular weight of the first monomer is not less than 90. Thus, the first monomer has a relatively large molecular weight, and the first monomer mixture is relatively viscous and not easily polymerized.

[0067] In some embodiments of the present application, the polymerization temperature of the first monomer is not lower than 120° C., so that the first monomer is less likely to undergo polymerization reaction at a lower temperature, which is beneficial to ion conduction.

[0068] In some embodiments of the present application, based on the total mass of the isolation membrane, the mass content of the first monomer can be 0.1wt%-20wt%. For example, the mass content of the first monomer can be 0.1wt%, 0.5wt%, 1wt%, 5wt%, 10wt%, 15wt%, 20wt%, etc., thereby, the isolation membrane contains an appropriate amount of the first monomer, and the first monomer is not easy to block the pores of the isolation membrane at a lower temperature, and the isolation membrane has better ion conductivity at a lower temperature; at a higher temperature, the first monomer will undergo a polymerization reaction, blocking the pores, reducing the porosity of the isolation membrane, isolating ion conduction, thereby alleviating the problem of continuous temperature rise caused by the exchange of positive and negative ions at high temperature, and reducing the probability of thermal runaway of the battery.

[0069] In some embodiments of the present application, the intermediate layer may further include an inorganic filler. Inorganic fillers have good strength, which helps improve the puncture resistance of the isolation membrane; inorganic fillers have good thermal stability, which helps reduce the thermal shrinkage of the isolation membrane, thereby improving the thermal stability of the isolation membrane.

[0070] In some embodiments of the present application, the inorganic filler may include an inert inorganic filler and / or an active inorganic filler, wherein the inert inorganic filler includes at least one of silicon dioxide, titanium dioxide, zinc oxide, zirconium oxide, magnesium oxide, barium oxide, aluminum oxide, barium titanate, and magnesium hydroxide; and the active inorganic filler includes at least one of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, an antiperovskite-type solid electrolyte, a sodium superion conductor (NASICON)-type solid electrolyte, and a lithium phosphorus nitrogen oxide (LiPON)-type solid electrolyte. The above-mentioned inorganic filler can have good thermal stability and can improve the thermal stability of the isolation membrane at least to a certain extent. In addition, the above-mentioned inorganic filler has high strength and can improve the puncture resistance of the isolation membrane. The above-mentioned active inorganic filler can also promote ion conduction during the charge and discharge process.

[0071] In some embodiments of the present application, the surface of the inorganic filler has a second functional group. The second functional group on the surface of the inorganic filler can include at least one of an amino group, an epoxy group, a carbon-carbon double bond, an aldehyde group, a hydroxyl group, a furfuryl group, an imide group, and an isocyanate group. As a result, the second functional group on the surface of the inorganic filler can undergo self-polymerization or react with the first monomer at a relatively high temperature, thereby blocking the pores in the separator and reducing the porosity of the separator at relatively high temperatures, thereby reducing the conduction of positive and negative ions. This, in turn, alleviates the problem of continuous temperature rise caused by the exchange of positive and negative ions at high temperatures and reduces the probability of thermal runaway of the battery.

[0072] In some embodiments of the present application, based on the total mass of the isolation membrane, the mass content of the inorganic filler can be 1wt%-20wt%. For example, the mass content of the inorganic filler can be 1wt%, 5wt%, 10wt%, 15wt%, 20wt%, etc. The above content of inorganic filler can at least improve the thermal stability and puncture resistance of the isolation membrane to a certain extent.

[0073] In some embodiments of the present application, the intermediate layer further includes an oligomer containing stable free radicals. Thus, the stable free radicals in the oligomer can react with the first monomer at a higher temperature, causing the first monomer to polymerize faster, blocking the pores of the isolation membrane, thereby isolating ion conduction and alleviating the problem of continuous temperature rise caused by positive and negative ion exchange at higher temperatures.

[0074] In some embodiments of the present application, the oligomer is a polymer composed of 2-20 repeating units. Therefore, the oligomer is less likely to block pores at lower temperatures and has no significant adverse effect on ion conduction at lower temperatures.

[0075] In some embodiments of the present application, the molecular weight of the oligomer is 200-10,000. Thus, the molecular weight of the oligomer is relatively low, and the oligomer is less likely to block pores at relatively low temperatures.

[0076] In some embodiments of the present application, the stable free radicals may include at least one of trityl, nitro and nitrogen oxide free radicals, etc. The above stable free radicals can react with the first monomer at a higher temperature, causing the first monomer to polymerize faster, thereby quickly blocking the pores of the isolation membrane.

[0077] In some embodiments of the present application, the nitrogen oxide free radicals may include at least one of 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl monomer, poly-2,2,6,6-tetramethylpiperidine-4-methylacrylate-1-nitroxide free radical and 2,2,6,6-tetramethyl-piperidine nitroxide free radical, whereby, at higher temperatures, the above-mentioned free radicals can promote faster polymerization of the first monomer and block the pores.

[0078] In some embodiments of the present application, the oligomer may include at least one of a polythienylphenoxy polymer, an arylmethyl radical polymer, a nitroxide-functionalized polyacrylamine dendrimer, a conjugated radical polymer, a comb-like nitroxide polymer, a polyvinylamine-supported nitroxide polymer, and a polyvinylamine-supported nitro radical polymer. At elevated temperatures, any of these oligomers can react with the first monomer, promoting rapid polymerization of the first monomer, thereby rapidly reducing the porosity of the separator and preventing ion conduction.

[0079] In some embodiments of the present application, based on the total mass of the isolation membrane, the mass content of the oligomer can be 0.1wt%-10%wt. For example, the mass content of the oligomer can be 0.1wt%, 0.5wt%, 1wt%, 5wt%, 10%wt, etc. Thus, the isolation membrane contains an appropriate amount of oligomer, which can promote the polymerization of the first monomer at a higher temperature, quickly block the pores, and reduce the conduction of ions; at a lower temperature, the above-mentioned content of oligomers has no obvious adverse effect on the conduction of ions.

[0080] In another aspect of the present application, the present application provides a method for preparing the aforementioned isolation film. In some embodiments of the present application, the method for preparing the aforementioned isolation film may include the following steps:

[0081] S100: providing a first substrate.

[0082] The specific material of the first substrate has been described in detail above and will not be repeated here.

[0083] S200: preparing an intermediate layer precursor solution.

[0084] In some embodiments of the present application, an intermediate layer precursor solution is prepared, wherein the intermediate layer precursor solution may include an electrolyte and a first monomer.

[0085] In some embodiments of the present application, the electrolyte may include carbonates, such as ethyl carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), propylene carbonate (PC), ethyl methyl carbonate (EMC), etc., and the above electrolytes can assume the ion conduction function in the intermediate layer.

[0086] In some embodiments of the present application, the electrolyte may also include fluoroethylene carbonate. Adding fluoroethylene carbonate to the electrolyte can improve the performance of the SEI membrane (solid electrolyte membrane) and can prevent the electrolyte from further decomposition to at least a certain extent, thereby improving the performance of the electrolyte.

[0087] In some embodiments of the present application, the electrolyte may further include a lithium salt, such as lithium bis(fluorosulfonyl)imide salt, lithium hexafluorophosphate, and the like.

[0088] In some specific embodiments of the present application, the electrolyte may include ethyl methyl carbonate, fluoroethylene carbonate and lithium bis(fluorosulfonyl)imide salt, and the above electrolyte may perform a good ion conduction function in the intermediate layer.

[0089] The molecular structure, molecular weight, polymerization temperature and other characteristics of the first monomer have been described in detail above and will not be repeated here.

[0090] S300: coating an intermediate layer precursor liquid on at least one surface of the first substrate to form an intermediate layer precursor liquid coating layer, and performing a heat treatment to obtain an isolation film.

[0091] In some embodiments of the present application, the intermediate layer precursor solution may be coated on one surface of the first substrate. In other embodiments of the present application, the intermediate layer precursor solution may be coated on both surfaces of the first substrate.

[0092] After the intermediate layer precursor liquid is coated on the surface of the first substrate, part of the intermediate layer precursor liquid will penetrate into the pores of the first substrate. During the heating process, the intermediate layer precursor liquid will undergo partial micro-crosslinking and curing, and the electrolyte will micro-gel to form an intermediate layer.

[0093] In some embodiments of the present application, the temperature of the heating treatment can be 60℃-70℃, for example, the temperature of the heating treatment can be 60℃, 63℃, 65℃, 68℃, 70℃, etc. At the above temperature, the intermediate layer precursor liquid can undergo partial micro-cross-linking and curing, thereby obtaining an isolation film with a micro-cross-linking structure.

[0094] In some embodiments of the present application, the heating treatment time can be 1h-20h, for example, the heating treatment time can be 1h, 3h, 5h, 8h, 10h, 12h, 15h, 20h, etc. Therefore, within the above time range, the intermediate layer precursor liquid can undergo partial micro-cross-linking and curing, and excessive cross-linking reaction is not easy to occur.

[0095] In some embodiments of the present application, the method for preparing the aforementioned isolation film may further include, before the heat treatment, placing a second substrate on a surface of the intermediate layer precursor coating layer that is distal from the first substrate. This second substrate can cooperate with the first substrate to better coat and secure the intermediate layer precursor coating layer, resulting in a more securely bonded film material after the heat treatment.

[0096] In some embodiments of the present application, the intermediate layer precursor solution may further include at least one of an inorganic filler, an oligomer, a second monomer, and an initiator. The addition of the inorganic filler can improve the thermal stability of the prepared isolation membrane; the addition of the oligomer can rapidly reduce the porosity of the prepared isolation membrane at higher temperatures, thereby improving the thermal stability of the isolation membrane; the second monomer can be cured at a lower temperature and can be cured during the heat treatment process, which is conducive to the formation of a micro-crosslinked structure; the initiator can induce partial micro-crosslinking and curing of the intermediate layer precursor solution during the heat treatment process, thereby obtaining a micro-crosslinked and cured intermediate layer after the heat treatment.

[0097] The specific materials of the inorganic filler and oligomer have been described in detail above and will not be repeated here.

[0098] In some embodiments of the present application, the second monomer may include pentaerythritol triacrylate, etc. During the heating process, the second monomer may be cross-linked and cured, which is conducive to obtaining an isolation film with a micro-cross-linked structure.

[0099] The isolation membrane prepared using the above method has a higher porosity at lower temperatures, which is conducive to ion conduction; at higher temperatures, the porosity of the isolation membrane decreases significantly, the pores are blocked, and it is more difficult for ions to pass through, which can effectively alleviate the problem of continuous temperature rise caused by positive and negative ion exchange at higher temperatures, thereby reducing the probability of thermal runaway of the battery; the above method is simple to operate and easy to implement, which is conducive to improving the yield of the product and is convenient for large-scale production.

[0100] In another aspect, the present application provides a battery. In some embodiments of the present application, the battery includes a positive electrode sheet, a negative electrode sheet, and a separator positioned between the positive and negative electrode sheets, wherein the separator includes the aforementioned separator. Thus, the battery possesses all the features and advantages of the separator described above, which will not be further elaborated here. Overall, the battery has good thermal stability and a low probability of thermal runaway.

[0101] As an example, the present application has no particular restrictions on the shape of the battery, which can be cylindrical, square, or any other shape. For example, Figure 5 is a battery 5 with a square structure as an example. Specifically, referring to Figure 6, the outer packaging of the battery 5 may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and side plates connected to the bottom plate, and the bottom plate and the side plates enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity.

[0102] As an example, the positive electrode sheet, the negative electrode sheet, and the separator can be wound or laminated to form an electrode assembly 52. ​​The electrode assembly 52 is encapsulated in a housing cavity, and the electrolyte fills the interior space of the electrode assembly 52. ​​The battery 5 can contain one or more electrode assemblies 52, and those skilled in the art can select the number based on specific practical needs.

[0103] As an example, batteries can be assembled into battery modules, and the number of batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module. Figure 7 is a battery module 4 as an example. Referring to Figure 7, in the battery module 4, multiple batteries 5 can be arranged in sequence along the length direction of the battery module 4. Of course, they can also be arranged in any other manner. The multiple batteries 5 can further be fixed by fasteners. The battery module 4 can also include a shell having a storage space, and the multiple batteries 5 are accommodated in the storage space.

[0104] As an example, the above-mentioned battery modules can also be assembled into a battery pack. The number of battery modules contained in the battery pack can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery pack. Figures 8 and 9 are a battery pack 1 as an example. Referring to Figures 8 and 9, the battery pack 1 may include a battery box and a plurality of battery modules 4 arranged in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can be covered on the lower box body 3 to form a closed space for accommodating the battery module 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0105] In some embodiments of the present application, the battery may be a lithium-ion battery, and the positive electrode active material of the positive electrode plate may include one or more of lithium iron phosphate, nickel-cobalt-manganese ternary material, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium vanadate, etc.

[0106] In some embodiments of the present application, the negative electrode active material of the negative electrode plate may include one or more of graphite, silicon-based negative electrode materials, mesophase carbon microbeads, hard carbon, soft carbon, etc.

[0107] In some embodiments of the present application, the positive electrode sheet and the negative electrode sheet may include a conductive agent and a binder, wherein the conductive agent in the positive electrode sheet and the conductive agent in the negative electrode sheet may independently include one or more of carbon nanotubes, carbon black, carbon fiber, graphene, etc., and the binder in the positive electrode sheet and the binder in the negative electrode sheet may independently include one or more of polyvinyl alcohol, polyurethane, polyacrylate, polyvinylidene fluoride, nitrile rubber, epoxy resin, vinyl acetate resin, chlorinated rubber, etc.

[0108] In another aspect of the present application, an electrical device is provided. In some embodiments of the present application, the electrical device includes the aforementioned battery. Thus, the electrical device has all the features and advantages of the aforementioned battery, which will not be further elaborated here.

[0109] Batteries, battery modules, or battery packs can be used as power sources or energy storage units for electrical devices. Electrical devices may include, but are not limited to, mobile devices (e.g., mobile phones, laptops), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks), electric trains, ships, satellites, and energy storage systems. Electrical devices can select batteries, battery modules, or battery packs based on their specific needs.

[0110] As an example, Figure 10 shows an example electric device. This device is a pure electric vehicle, hybrid electric vehicle, or plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module can be used.

[0111] As an example, the power-consuming device may also be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and may use a battery as a power source.

[0112] The present application will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are merely for illustrative purposes and are not intended to limit the scope of the present application in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment employed are all commercially available. If, in the following examples, specific processing conditions and treatment methods are not clearly described, then conditions and methods well known in the art may be used to process.

[0113] Example 1

[0114] A first substrate is provided, wherein the material of the first substrate is polyimide and the thickness of the first substrate is 8 microns; maleic anhydride monomer (first monomer), second monomer pentaerythritol triacrylate and initiator azobisisobutyronitrile are added to an electrolyte (the mass ratio of ethyl methyl carbonate, fluoroethylene carbonate and lithium bis(fluorosulfonyl)imide is 3:2:1), wherein the mass ratio of the electrolyte, maleic anhydride monomer, pentaerythritol triacrylate and azobisisobutyronitrile is 70:20:10:0.2, and the mixture is stirred at room temperature for 6 hours and mixed evenly to obtain an intermediate layer precursor liquid; the intermediate layer precursor liquid is coated on one side surface of the first substrate to form an intermediate layer precursor liquid coating layer with a thickness of 3 microns, and a second substrate is adhered to the side surface of the intermediate layer precursor liquid coating layer away from the first substrate, wherein the material of the second substrate is polyimide and the thickness of the second substrate is 8 microns, and the substrate is heat-treated at a temperature of 70°C and a holding time of 10 hours to obtain an isolation film.

[0115] During the heating process, some components in the intermediate layer precursor solution are micro-crosslinked and cured (mainly the curing of pentaerythritol triacrylate), and the electrolyte is micro-gelled. The intermediate layer of the obtained isolation membrane has a micro-crosslinked structure, and the micro-gelled electrolyte can assume the ion conduction function.

[0116] In the isolation film, the mass content of the first monomer is 10 wt %.

[0117] Example 2

[0118] A first substrate is provided, wherein the material of the first substrate is polyimide and the thickness of the first substrate is 8 microns. Maleic anhydride monomer (first monomer), inorganic filler SiO2 containing carbon-carbon double bond functional groups on the surface and polythiophene-phenoxy polymer (oligomer) are added to the electrolyte (the mass ratio of ethyl methyl carbonate, fluoroethylene carbonate and lithium bis(fluorosulfonyl)imide is 3:2:1), wherein the mass ratio of the electrolyte, maleic anhydride monomer, inorganic filler SiO2 and polythiophene-phenoxy polymer is 70:15:15:1.5, and the mixture is stirred at room temperature for 6 hours and mixed evenly to obtain an intermediate layer precursor liquid; the intermediate layer precursor liquid is coated on one side surface of the first substrate to form an intermediate layer precursor liquid coating layer with a thickness of 5 microns, and a second substrate is adhered to the surface of the intermediate layer precursor liquid coating layer away from the first substrate, wherein the material of the second substrate is polyimide and the thickness of the second substrate is 8 microns, and the substrate is heat-treated at a temperature of 70°C and a holding time of 10 hours to obtain an isolation film.

[0119] In the isolation film, the mass content of the first monomer is 10 wt %, the mass content of the inorganic filler is 10 wt %, and the mass content of the oligomer is 1 wt %.

[0120] Example 3

[0121] A first substrate is provided, wherein the material of the first substrate is polyimide and the thickness of the first substrate is 8 microns; maleic anhydride monomer (first monomer), second monomer pentaerythritol triacrylate and initiator azobisisobutyronitrile are added to an electrolyte (the mass ratio of ethyl methyl carbonate, fluoroethylene carbonate and lithium bis(fluorosulfonyl)imide is 3:2:1), wherein the mass ratio of the electrolyte, maleic anhydride monomer, pentaerythritol triacrylate and azobisisobutyronitrile is 80:10:10:0.2, and the mixture is stirred at room temperature for 6 hours and mixed evenly to obtain an intermediate layer precursor liquid; the intermediate layer precursor liquid is coated on one side surface of the first substrate to form an intermediate layer precursor liquid coating layer with a thickness of 3 microns, and a second substrate is adhered to the side surface of the intermediate layer precursor liquid coating layer away from the first substrate, wherein the material of the second substrate is polyimide and the thickness of the second substrate is 8 microns, and the substrate is heat-treated at a temperature of 70°C and a holding time of 10 hours to obtain an isolation film.

[0122] During the heating process, some components in the intermediate layer precursor solution are micro-crosslinked and cured (mainly the curing of pentaerythritol triacrylate), and the electrolyte is micro-gelled. The intermediate layer of the obtained isolation membrane has a micro-crosslinked structure, and the micro-gelled electrolyte can assume the ion conduction function.

[0123] In the isolation film, the mass content of the first monomer is 5 wt %.

[0124] Example 4

[0125] A first substrate is provided, wherein the material of the first substrate is polyimide and the thickness of the first substrate is 8 microns; maleic anhydride monomer (first monomer), second monomer pentaerythritol triacrylate and initiator azobisisobutyronitrile are added to an electrolyte (the mass ratio of ethyl methyl carbonate, fluoroethylene carbonate and lithium bis(fluorosulfonyl)imide is 3:2:1), wherein the mass ratio of the electrolyte, maleic anhydride monomer, pentaerythritol triacrylate and azobisisobutyronitrile is 60:30:10:0.2, and the mixture is stirred at room temperature for 6 hours and mixed evenly to obtain an intermediate layer precursor liquid; the intermediate layer precursor liquid is coated on one side surface of the first substrate to form an intermediate layer precursor liquid coating layer with a thickness of 3 microns, and a second substrate is attached to the side surface of the intermediate layer precursor liquid coating layer away from the first substrate, wherein the material of the second substrate is polyimide and the thickness of the second substrate is 8 microns, and the substrate is heat-treated at a temperature of 70°C and a holding time of 10 hours to obtain an isolation film.

[0126] During the heating process, some components in the intermediate layer precursor solution are micro-crosslinked and cured (mainly the curing of pentaerythritol triacrylate), and the electrolyte is micro-gelled. The intermediate layer of the obtained isolation membrane has a micro-crosslinked structure, and the micro-gelled electrolyte can assume the ion conduction function.

[0127] In the isolation film, the mass content of the first monomer is 15 wt %.

[0128] Example 5

[0129] A first substrate is provided, wherein the material of the first substrate is polyimide and the thickness of the first substrate is 8 microns; maleic anhydride monomer (first monomer), second monomer pentaerythritol triacrylate and initiator azobisisobutyronitrile are added to an electrolyte (the mass ratio of ethyl methyl carbonate, fluoroethylene carbonate and lithium bis(fluorosulfonyl)imide is 3:2:1), wherein the mass ratio of the electrolyte, maleic anhydride monomer, pentaerythritol triacrylate and azobisisobutyronitrile is 50:40:10:0.2, and the mixture is stirred at room temperature for 6 hours and mixed evenly to obtain an intermediate layer precursor liquid; the intermediate layer precursor liquid is coated on one side surface of the first substrate to form an intermediate layer precursor liquid coating layer with a thickness of 3 microns, and a second substrate is attached to the side surface of the intermediate layer precursor liquid coating layer away from the first substrate, wherein the material of the second substrate is polyimide and the thickness of the second substrate is 8 microns, and the substrate is heat-treated at a temperature of 70°C and a holding time of 10 hours to obtain an isolation film.

[0130] During the heating process, some components in the intermediate layer precursor solution are micro-crosslinked and cured (mainly the curing of pentaerythritol triacrylate), and the electrolyte is micro-gelled. The intermediate layer of the obtained isolation membrane has a micro-crosslinked structure, and the micro-gelled electrolyte can assume the ion conduction function.

[0131] In the isolation film, the mass content of the first monomer is 20 wt %.

[0132] Example 6

[0133] The difference from Example 1 is that the heating temperature is 60° C. and the holding time is 20 h. The other parameters and steps are the same as those in Example 1.

[0134] Example 7

[0135] The difference from Example 1 is that the maleic anhydride monomer is replaced by 2-chloromaleic anhydride monomer. The mass content of 2-chloromaleic anhydride monomer in the isolation membrane is 10 wt%. The remaining parameters and steps are the same as those in Example 1.

[0136] Example 8

[0137] The difference from Example 2 is that the temperature of the heating treatment is 60° C. The remaining parameters and steps are the same as those in Example 2.

[0138] Example 9

[0139] Unlike Example 2, maleic anhydride monomer and SiO2, an inorganic filler with carbon-carbon double bond functional groups on its surface, were added to the electrolyte (the mass ratio of ethyl methyl carbonate, fluoroethylene carbonate, and lithium bis(fluorosulfonyl)imide was 3:2:1), without the addition of oligomers. The mass ratio of the electrolyte, maleic anhydride monomer (first monomer), and SiO2, an inorganic filler, was 62.5:15:22.5. The mass content of the first monomer in the isolation membrane was 10 wt%, and the mass content of the inorganic filler was 15 wt%. The remaining parameters and steps were the same as in Example 2.

[0140] Example 10

[0141] Unlike Example 2, maleic anhydride monomer and polythiophene-phenoxy polymer were added to the electrolyte (the mass ratio of ethyl methyl carbonate, fluoroethylene carbonate, and lithium bis(fluorosulfonyl)imide) was 3:2:1, and no inorganic filler was added. The mass ratio of the electrolyte, maleic anhydride monomer (first monomer), and polythiophene-phenoxy polymer (oligomer) was 85:15:1.5, and the thickness of the intermediate layer precursor coating was 3 microns. The mass content of the first monomer in the isolation membrane was 10 wt%, and the mass content of the oligomer was 1 wt%. The remaining parameters and steps were the same as those in Example 2.

[0142] Example 11

[0143] Unlike Example 2, the mass ratio of the electrolyte, maleic anhydride monomer (first monomer), inorganic filler SiO2, and polythiophene phenoxy polymer (oligomer) was 55:15:30:1.5, and the thickness of the intermediate layer precursor coating was 6 μm. The isolation membrane contained 10 wt% of the first monomer, 20 wt% of the inorganic filler, and 1 wt% of the oligomer. The remaining parameters and steps were the same as in Example 2.

[0144] Example 12

[0145] Unlike Example 2, the mass ratio of the electrolyte, maleic anhydride monomer (first monomer), inorganic filler SiO2, and polythiophene phenoxy polymer (oligomer) was 83.5:15:1.5:1.5, and the thickness of the intermediate layer precursor coating was 4 μm. The isolation membrane contained 10 wt% of the first monomer, 1 wt% of the inorganic filler, and 1 wt% of the oligomer. The remaining parameters and procedures were the same as in Example 2.

[0146] Example 13

[0147] Unlike Example 2, the mass ratio of the electrolyte, maleic anhydride monomer (first monomer), inorganic filler SiO2, and polythiophenephenoxy polymer (oligomer) was 70:15:15:15. The separator contained 10 wt% of the first monomer, 10 wt% of the inorganic filler, and 10 wt% of the oligomer. The remaining parameters and steps were the same as in Example 2.

[0148] Example 14

[0149] Unlike Example 2, the mass ratio of the electrolyte, maleic anhydride monomer (first monomer), inorganic filler SiO2, and polythiophene phenoxy polymer (oligomer) was 70:15:15:0.15. The separator contained 10 wt% of the first monomer, 10 wt% of the inorganic filler, and 0.1 wt% of the oligomer. The remaining parameters and steps were the same as in Example 2.

[0150] Comparative Example 1

[0151] Unlike Example 1, maleic anhydride was not added to the electrolyte. The mass ratio of electrolyte, pentaerythritol triacrylate, and azobisisobutyronitrile was 90:10:0.2. The mass content of the first monomer in the separator was 0. The remaining parameters and steps were the same as in Example 1.

[0152] Comparative Example 2

[0153] The isolation film is formed from a polyimide substrate and has a thickness of 13 microns.

[0154] Preparation of the battery:

[0155] Preparation of positive electrode sheet: Add positive electrode active material NCM811 (the molar ratio of nickel, cobalt and manganese in the positive electrode active material is 8:1:1), binder polyvinylidene fluoride (PVDF), and conductive agent (acetylene black) to a certain amount of N-methylpyrrolidone (NMP). The mass ratio of positive electrode active material: binder: conductive agent is 9:0.5:0.5. Stir in a drying room to form a uniform positive electrode slurry. Control the viscosity to be 3000mPa·S-10000mPa·S. The above positive electrode slurry is coated on aluminum foil and dried to obtain a positive electrode sheet. The positive electrode sheet is compacted and the compaction density of the positive electrode sheet is 3.4g / cm 3 .

[0156] Preparation of negative electrode sheet: Add negative electrode active materials graphite, sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), and conductive agent (carbon fiber) to a certain amount of deionized water. The mass ratio of graphite: sodium carboxymethyl cellulose: styrene-butadiene rubber: conductive agent is 9:0.3:0.2:0.5. Stir to form a uniform negative electrode slurry. Control the viscosity to be 3000mPa·S-10000mPa·S. Coat the above negative electrode slurry on copper foil and dry it to obtain the negative electrode sheet. The negative electrode sheet is compacted to a compact density of 1.5g / cm 3 .

[0157] The prepared positive electrode sheet, negative electrode sheet and isolation membrane (isolation membrane in Examples 1-14 or Comparative Examples 1-2) are made into corresponding battery cells according to a Z-shaped laminate structure, and the battery cells are vacuum-dried at 90°C for 12 hours, and then the positive and negative electrode tabs are ultrasonically welded. The positive electrode uses an aluminum tab and the negative electrode uses a nickel tab. The positive and negative electrode tabs are located on the same side of the battery cell. The battery cell after the tabs are welded is placed in an aluminum-plastic film of appropriate size for top-side sealing. The top-side sealing temperature is 145°C, and the battery is injected (the electrolyte of the battery consists of ethyl methyl carbonate, fluoroethylene carbonate and lithium bis(fluorosulfonyl)imide salt, and the mass ratio of ethyl methyl carbonate:fluoroethylene carbonate: lithium bis(fluorosulfonyl)imide salt is 3:2:1). The battery is allowed to stand, formed, aged, exhausted, sealed, and capacity tested to obtain the prepared soft-pack laminated battery.

[0158] The mass content of the first monomer, inorganic filler, and oligomer in the isolation membrane of each embodiment and comparative example, the porosity of the isolation membrane of each embodiment and comparative example at different temperatures, and the thermal runaway data of the battery were tested, and the test results are recorded in Table 1.

[0159] Test method for mass content of each component in the isolation film:

[0160] The initial total mass of the separator is recorded as A.

[0161] Test of mass content of electrolyte in isolation membrane: Using vacuum method, the isolation membrane is kept at 40°C and vacuum degree -0.1Mpa for 20 hours. The remaining mass is recorded as B, and the ratio of (AB) / A is recorded as the mass content of electrolyte.

[0162] Method for testing the mass content of inorganic filler in the isolation membrane: the mass of the isolation membrane after combustion (under air atmosphere, temperature not less than 800 degrees Celsius) is recorded as C, and the ratio of C / A is recorded as the mass content of the inorganic filler.

[0163] Method for testing the mass content of the first monomer and oligomer: Scrape off the intermediate layer from the separator, then use high-performance liquid chromatography to determine the mass of the first monomer and oligomer, denoted as D and E, respectively. The ratios of D / A and E / A are then recorded as the mass content of the first monomer and oligomer, respectively.

[0164] The intermediate layer on the separator is scraped off, and the remaining separator substrate is recorded as F.

[0165] The mass content of the second monomer: the ratio of (ABCDEF) / A is recorded as the mass content of the second monomer.

[0166] The specific test method for the porosity of the isolation membrane can refer to GB / T 21650.2-2008 "Determination of pore size distribution and porosity of solid materials by mercury intrusion and gas adsorption method Part 2: Analysis of mesopores and macropores by gas adsorption method".

[0167] Battery thermal runaway test method: Hot box test: The battery is placed in a high-temperature box. The temperature of the high-temperature box is increased at a rate of 1°C / min, starting at 120°C and maintaining the temperature for 30 minutes at 5°C increments until the battery fails (failure criteria include fire or explosion). If the battery does not fail at temperature A, it is considered to have passed the hot box test at temperature A. The battery hot box temperature is greater than temperature A.

[0168] Table 1 Mass content of each component in the separator, separator porosity and battery thermal runaway test results

[0169] Table 1 shows that in Examples 1-14, the separators contain the first monomer in their intermediate layers. At relatively low temperatures, the separators have high porosity. At higher temperatures, the first monomer polymerizes, blocking the separator pores and significantly reducing their porosity. This inhibits ion conduction at high temperatures and alleviates the persistent temperature rise caused by positive and negative ion exchange at higher temperatures. In Comparative Examples 1 and 2, since the first monomer is not added, the difference in porosity between the separators at the first and second temperatures is relatively small. At the higher second temperature, the separators have higher porosity, resulting in lower hot box temperatures for battery thermal runaway testing.

[0170] Comparing Example 1 with Examples 3-5, it can be seen that within a certain range, the higher the content of the first monomer in the isolation membrane, the lower the porosity of the isolation membrane at a higher temperature, and the higher the hot box temperature of the battery thermal runaway test.

[0171] Compared with Example 2, Example 13 and Example 14, the higher the oligomer content in the isolation membrane, the higher the porosity at the first temperature, the lower the porosity at the second temperature, and the higher the hot box temperature of the battery thermal runaway test.

[0172] Compared with Example 11 and Example 12, the higher the content of inorganic filler in the isolation membrane, the higher the porosity at the first temperature, the lower the porosity at the second temperature, and the higher the hot box temperature of the battery thermal runaway test.

[0173] Compared with Example 1 and Example 6, the heating treatment temperature in Example 6 is lower, and the porosity of the isolation membrane at the first temperature is higher. Compared with Example 2 and Example 8, the heating temperature in Example 8 is lower, and the porosity of the isolation membrane at the first temperature is higher.

[0174] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", "some embodiments", "other embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first", "second" and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0175] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A separation film, in, include: A first substrate, and an intermediate layer located on at least one side of the first substrate, the porosity of the isolation membrane at a first temperature is a, the porosity of the isolation membrane at a second temperature is b, the first temperature is -20°C to 100°C, 40%≤a≤70%, the second temperature is not less than 120°C, and b≤2%.

2. The isolation film according to claim 1, in, The third temperature is -20°C to 120°C. At the third temperature, the intermediate layer includes a first monomer, and the first monomer satisfies at least one of the following conditions: The molecule of the first monomer contains a cyclic structure, the number of atoms in the cyclic structure is less than or equal to 7, and the cyclic structure has a first functional group; The molecular weight of the first monomer is not less than 90; The polymerization temperature of the first monomer is not less than 120°C.

3. The isolation film according to claim 2, in, Based on the total mass of the isolation membrane, the mass content of the first monomer is 0.1 wt %-20 wt %.

4. The isolation film according to claim 2 or 3, in, The intermediate layer further comprises an inorganic filler, and the inorganic filler satisfies at least one of the following conditions: The inorganic filler comprises an inert inorganic filler, and the inert inorganic filler comprises at least one of silicon dioxide, titanium dioxide, zinc oxide, zirconium oxide, magnesium oxide, barium oxide, aluminum oxide, barium titanate and magnesium hydroxide; The inorganic filler includes an active inorganic filler, and the active inorganic filler includes at least one of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, an antiperovskite-type solid electrolyte, a sodium superion conductor-type solid electrolyte, and a lithium-phosphorus-nitrogen-oxygen-type solid electrolyte; The surface of the inorganic filler has a second functional group, and the second functional group includes at least one of an amino group, an epoxy group, a carbon-carbon double bond, an aldehyde group, a hydroxyl group, a furfuryl group, an imide group and an isocyanate group.

5. The isolation film according to claim 4, in, Based on the total mass of the isolation film, the mass content of the inorganic filler is 1 wt % to 20 wt %.

6. The isolation film according to any one of claims 2 to 5, in, The intermediate layer further comprises an oligomer, wherein the oligomer contains a stable free radical, and the oligomer satisfies at least one of the following conditions: The oligomer is a polymer consisting of 2-20 repeating units; The molecular weight of the oligomer is 200-10000; The stable free radical includes at least one of a trityl radical, a nitro radical and a nitrogen oxide radical.

7. The isolation film according to claim 6, in, The nitroxide free radical includes at least one of 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxide monomer, poly-2,2,6,6-tetramethylpiperidine-4-methylacrylate-1-nitroxide free radical and 2,2,6,6-tetramethyl-piperidine nitroxide free radical.

8. The isolation film according to claim 6 or 7, in, The oligomer includes at least one of a polythienylphenoxy polymer, an arylmethyl radical polymer, a nitroxide functionalized polyacrylamine dendrimer, a conjugated radical polymer, a comb-like nitroxide radical polymer, a polyvinylamine-supported nitroxide radical polymer, and a polyvinylamine-supported nitro radical polymer.

9. The isolation film according to any one of claims 6 to 8, in, Based on the total mass of the isolation membrane, the mass content of the oligomer is 0.1 wt%-10 wt%.

10. The isolation film according to any one of claims 1 to 9, in, The invention further comprises a second substrate, wherein the second substrate is located on a side of the intermediate layer away from the first substrate.

11. The isolation film according to claim 10, in, The first substrate and the second substrate each independently include at least one of polyamide, polyamideimide, polyketone, polysulfone, polyphenylene sulfide, polyphenylene ether, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl chloride, polyolefin, perfluoroalkoxyalkane, polyester, liquid crystal polymer, polyoxymethylene, acrylonitrile styrene acrylate, styrene acrylonitrile, acrylonitrile butadiene styrene, polybenzimidazole, polyparaphenylene copolymer, polyacrylonitrile, polyethyleneimine, ethylene tetrafluoroethylene, polychlorotrifluoroethylene, aramid, polyetherimide, polyparaphenylene benzobisoxazole and cellulose.

12. A method for preparing the isolation film according to any one of claims 1 to 11, in, include: providing a first substrate; preparing an intermediate layer precursor solution, wherein the intermediate layer precursor solution comprises an electrolyte and a first monomer; The intermediate layer precursor liquid is coated on at least one side of the surface of the first substrate to form an intermediate layer precursor liquid coating layer, and then heat-treated to obtain an isolation film.

13. The method according to claim 12, in, Before the heating treatment, the method further comprises: arranging a second substrate on a side of the intermediate layer precursor liquid coating layer away from the first substrate.

14. The method according to claim 12 or 13, in, The intermediate layer precursor solution further includes at least one of an inorganic filler, an oligomer, a second monomer and an initiator.

15. The method according to claim 14, in, At least one of the following conditions is met: The electrolyte comprises ethyl methyl carbonate, fluoroethylene carbonate and bis(fluorosulfonyl)imide lithium salt; The second monomer includes pentaerythritol triacrylate; The temperature of the heating treatment is 60°C-70°C; The heating treatment time is 1h-20h.

16. A battery, in, It comprises a positive electrode sheet, a negative electrode sheet, and an isolating member located between the positive electrode sheet and the negative electrode sheet, wherein the isolating member comprises the isolating film described in any one of claims 1 to 11 or the isolating film prepared by the method described in any one of claims 12 to 15.

17. An electrical device, in, Comprising the battery of claim 16.

Citation Information

Patent Citations

  • Separator for nonaqueous secondary battery

    CN102160211A

  • Preparation method of microporous polymer diaphragm with high-temperature self-enhancing mechanism

    CN103113607A

  • Lithium-ion secondary battery with thermal action protection function

    CN110311138A

  • Porous diaphragm and preparation method thereof and lithium ion battery

    CN111834591A

  • Isolating membrane and preparation method thereof, secondary battery and electric device

    CN115832623A

Cited By

  • High-wettability long-cycle lithium battery composite diaphragm as well as preparation method and application thereof

    CN120261907A

  • Highly infiltrative long-circulation lithium battery composite diaphragm, and preparation method and application thereof

    CN120261907B