Composite electrode material, and preparation method therefor and use thereof

By introducing organic sulfonic acids into lithium-ion battery electrode materials to form a nitrogen-sulfur-doped carbon coating, the problem of insufficient rate performance and cycle performance of lithium-ion batteries is solved, and the performance improvement and cost reduction of electrode materials are achieved. .

WO2024221949A1PCT designated stage expired Publication Date: 2024-10-31EVE POWER CO LTD

Patent Information

Application Number
PCT/CN2023/137261
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-12-07
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The rate performance and cycle performance of existing lithium-ion batteries are insufficient, which results in increased internal resistance and reduced service life of the battery during high-rate charge and discharge. Moreover, the cost of electrode materials is high, making it difficult to effectively improve performance.

Method used

Organic sulfonic acids containing carbon, nitrogen, and sulfur are mixed with the main electrode material, and composite electrode materials are prepared through ball milling and step-by-step calcination to form a nitrogen-sulfur-doped carbon coating layer to improve the conductivity and structure of the electrode material. stability.

Benefits of technology

It significantly improves the rate performance and cycle performance of the electrode material, increases the high-rate charge and discharge capacity, and reduces the preparation cost, which has good development potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023137261_31102024_PF_FP_ABST
    Figure CN2023137261_31102024_PF_FP_ABST
Patent Text Reader

Abstract

A composite electrode material, and a preparation method therefor and the use thereof. The preparation method comprises the following steps: mixing an electrode main material and an organic sulfonic acid substance, and calcining the mixture to obtain a composite electrode material, wherein elements in the organic sulfonic acid substance comprise carbon, nitrogen and sulfur. By introducing a carbon coating layer doped with nitrogen and sulfur, the rate capability and cycling performance of the electrode material are improved, and the high-rate charge-discharge capacity of the electrode material is also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Composite electrode material and its preparation method and application

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 28, 2023, with application number 202310480663.7. The entire contents of the above application are incorporated by reference into this application. Technical Field

[0002] The present invention relates to the field of lithium-ion battery materials, and specifically relates to a composite electrode material and its preparation method and application. Background Art

[0003] In practical applications, the rate performance and cycle performance of lithium batteries affect the charging speed and service life of the battery. The main reasons why electrode materials affect the rate performance and cycle performance of batteries are: (1) The migration ability of lithium ions between the positive and negative electrodes, the electrolyte, and their interfaces is limited. High-rate charging and discharging requires accelerated lithium ion transmission, which will increase the internal resistance of the battery cell and reduce performance; (2) The negative electrode capacity is insufficient. After hundreds of cycles, the negative electrode structure is severely damaged and cannot fully receive the lithium ions provided by the positive electrode, resulting in lithium plating, causing premature capacity loss and shortened service life.

[0004] At present, the rate performance and cycle performance of the battery are improved by adding citric acid and glucose to the positive and negative electrode materials to form a coated carbon layer or doping nitrogen or sulfur, and certain effects have been achieved.

[0005] In the related art, for example, in a carbon-coated lithium vanadium phosphate positive electrode material and a preparation method thereof, the method includes the following steps: mixing a lithium source, a vanadium source, a phosphorus source and a carbon source, adding anhydrous ethanol, placing the mixture in a ball mill, and then drying and sintering the mixture in a three-temperature zone rotary kiln. The carbon-coated lithium vanadium phosphate positive electrode material can be obtained by cooling the temperature to room temperature; wherein the carbon source is a mixed carbon source of sucrose and citric acid.

[0006] For example, in a preparation method of a carbon-coated sodium vanadium phosphate positive electrode material, the method includes the following steps: using glucose as a reducing agent and carbon source and water as a dispersant, ball-milling NH4VO3, NaH2PO4·2H2O and glucose in water, spray drying, and calcining to obtain a carbon-coated sodium vanadium phosphate positive electrode material.

[0007] For example, in a preparation method of a biomass nitrogen-doped carbon-coated lithium-rich lithium iron phosphate positive electrode material, the method includes the following steps: adding deionized water to lithium hydroxide and stirring to dissolve it; placing silk in the lithium hydroxide solution, heating and stirring to dissolve it, adding the carbon-coated lithium iron phosphate positive electrode material, and drying and sintering the mixed slurry to obtain the biomass nitrogen-doped carbon-coated lithium iron phosphate positive electrode material. SUMMARY OF THE INVENTION

[0008] The high cost of related technologies and the limited improvement in rate performance and cycle performance of electrode materials have been difficult to solve.

[0009] In a first aspect, the present application provides a method for preparing a composite electrode material, the preparation method comprising the following steps: mixing an electrode main material and an organic sulfonic acid substance, and calcining to obtain the composite electrode material; wherein the elements in the organic sulfonic acid substance include carbon, nitrogen and sulfur.

[0010] In some embodiments, the organic sulfonic acid substance includes taurine and / or aminosulfonic acid.

[0011] In some embodiments, the mass ratio of the electrode main material to the organic sulfonic acid substance is (120-150):(1-18).

[0012] In some embodiments, the mixing method comprises ball milling.

[0013] In some embodiments, the ball milling mixing comprises dry ball milling or wet ball milling.

[0014] In some embodiments, the wet ball milling step includes: dispersing the electrode main material and the organic sulfonic acid substance in a solvent to obtain a mixed slurry; and ball milling the mixed slurry.

[0015] In some embodiments, the solvent includes at least one of methanol, ethanol, or N-methylpyrrolidone, or a combination of at least two thereof.

[0016] In some embodiments, the ball milling speed is 200-300 rpm.

[0017] In some embodiments, the mixing temperature is 40-80°C.

[0018] In some embodiments, the mixing time is 5-7 hours.

[0019] In some embodiments, the calcination is performed under a protective atmosphere.

[0020] In some embodiments, the gas in the protective atmosphere includes at least one of nitrogen, argon, or helium, or a combination of at least two of them.

[0021] In some embodiments, the calcination step is a stepwise calcination; the stepwise calcination includes a first-stage calcination and a second-stage calcination.

[0022] In some embodiments, the temperature of the first-stage calcination is 200-300°C.

[0023] In some embodiments, the first-stage calcination time is 2-4 hours.

[0024] In some embodiments, the temperature of the second-stage calcination is 450-600°C.

[0025] In some embodiments, the second-stage calcination time is 2-5 hours.

[0026] In some embodiments, the preparation method includes the following steps: mixing the electrode main material with an organic sulfonic acid substance in a mass ratio of (120-150): (1-18) in a solvent at 200-300 rpm and ball milling for 5-7 hours at a mixing temperature of 40-80°C to obtain a mixture; calcining the mixture in a protective atmosphere at 200-300°C for 2-4 hours, and then calcining the mixture in a protective atmosphere at 450-600°C for 2-5 hours to obtain the composite electrode material.

[0027] In a second aspect, the present application provides a composite electrode material prepared by the above-mentioned preparation method, wherein the composite electrode material comprises an electrode material core and a sulfur-nitrogen-doped carbon coating layer located on the surface of the core.

[0028] In a third aspect, the present application provides an electrode plate, which includes the above-mentioned composite electrode material. Beneficial effects

[0029] The beneficial effects of the present application are as follows: by introducing organic sulfonic acid substances containing carbon, nitrogen, and sulfur into the electrode material, a nitrogen-sulfur-doped carbon coating layer is formed on the surface of the electrode material particles, which increases the active sites on the electrode surface, thereby improving the conductivity of the material and making the structure more stable, thereby improving the rate performance and cycle performance of the electrode material and increasing the high-rate charge and discharge capacity of the electrode material;

[0030] The preparation method of the composite electrode material of the present application has simple process, low cost and good development potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] FIG1 is a simplified diagram of the preparation process of the composite electrode material provided in Example 1 of this application. Modes for Carrying Out the Invention

[0032] This application combines an organic sulfonic acid containing carbon, nitrogen, and sulfur with a primary electrode material and calcines it to produce a nitrogen- and sulfur-doped carbon-coated electrode material. The introduction of a nitrogen- and sulfur-doped carbon coating not only improves the rate performance and cycle performance of the electrode material, but also increases its high-rate charge-discharge capacity. This preparation method is simple, low-cost, and has great potential for development.

[0033] The present application provides a method for preparing a composite electrode material, which comprises the following steps: mixing an electrode main material and an organic sulfonic acid substance, and calcining to obtain the composite electrode material.

[0034] The elements in the organic sulfonic acid substance include carbon, nitrogen and sulfur.

[0035] This application introduces organic sulfonic acid substances containing carbon, nitrogen, and sulfur into the electrode material, forming a nitrogen- and sulfur-doped carbon coating on the surface of the electrode material particles. This increases the active sites on the electrode surface, enhances the material's conductivity, and makes the structure more stable, thereby improving the electrode material's rate performance and cycle performance, and increasing the high-rate charge and discharge capacity of the electrode material. This preparation method is simple, low-cost, and has great development potential.

[0036] This application uses organic sulfonic acid substances, which can effectively reduce the temperature rise caused by the increase in ohmic polarization under high-rate charge and discharge of the battery, and the doping of sulfur and nitrogen atoms can expand the interlayer spacing of the electrode material and slow down the irreversible collapse of the interlayer structure of the electrode material.

[0037] It should be noted that this application does not limit the main electrode material. For example, the main electrode material can be a positive electrode material such as lithium iron phosphate, lithium cobalt oxide, or lithium manganese oxide, or a negative electrode material such as artificial graphite or natural graphite.

[0038] In some embodiments, the organic sulfonic acid substance includes taurine and / or aminosulfonic acid.

[0039] In this application, taurine is a simple sulfur-containing amino acid in animals, and aminosulfonic acid is an inorganic solid acid formed by replacing the hydroxyl group of sulfuric acid with an amino group. When used in electrode materials, the nitrogen element in the amino group can accelerate the charge transfer process of the electrode reaction on the electrode surface, and the sulfur element in the sulfonic acid group can stabilize the interlayer structure of the electrode.

[0040] In some embodiments, the mass ratio of the electrode main material and the organic sulfonic acid substance is (120-150): (1-18), wherein the selection range of the electrode main material "120-150" can be, for example, 120, 125, 130, 135, 140, 145 or 150, etc., and the selection range of the organic sulfonic acid substance "1-18" can be, for example, 1, 3, 5, 7, 9, 12, 14, 16 or 18, etc.

[0041] In this application, if the mass ratio of the electrode main material and the organic sulfonic acid substance is too small, that is, the amount of organic sulfonic acid substance used is too much, the lithium ion insertion or removal channel will be lengthened and the difficulty of lithium ion migration will increase; if the mass ratio of the electrode main material and the organic sulfonic acid substance is too large, that is, the amount of organic sulfonic acid substance used is too little, the electrode main material structure cannot be completely covered and the improvement effect is not obvious.

[0042] In some embodiments, the mixing method comprises ball milling.

[0043] In some embodiments, the ball milling mixing includes dry ball milling or wet ball milling, preferably wet ball milling. In the present application, wet ball milling is used to fully mix the electrode main material and the organic sulfonic acid substance.

[0044] In some embodiments, the specific steps of the wet ball milling include:

[0045] The electrode main material and the organic sulfonic acid substance are dispersed in a solvent to obtain a mixed slurry; and the mixed slurry is ball-milled.

[0046] In some embodiments, the solvent includes any one of methanol, ethanol, or N-methylpyrrolidone, or a combination of at least two thereof.

[0047] In some embodiments, the ball milling speed is 200-300 rpm, for example, 200 rpm, 225 rpm, 250 rpm, 275 rpm, or 300 rpm.

[0048] In some embodiments, the mixing temperature is 40-80°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.

[0049] In some embodiments, the mixing time is 5-7 hours, for example, 5 hours, 5.5 hours, 6 hours, 6.5 hours or 7 hours, etc. In some embodiments, the calcination is performed under a protective atmosphere.

[0050] In some embodiments, the gas in the protective atmosphere includes any one of nitrogen, argon, or helium, or a combination of at least two of them.

[0051] In some embodiments, the calcination method is stepwise calcination.

[0052] In some embodiments, the stepwise calcination includes a first-stage calcination and a second-stage calcination.

[0053] In some embodiments, the temperature of the first-stage calcination is 200-300°C, for example, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C or 300°C.

[0054] In the present application, if the temperature of the first-stage calcination is too low, the coating will agglomerate and cannot form a layered structure; if the temperature of the first-stage calcination is too high, the coating will crack and the structure will be destroyed.

[0055] In some embodiments, the first-stage calcination time is 2-4 hours, for example, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, 3 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours or 4 hours.

[0056] In some embodiments, the temperature of the second-stage calcination is 450-600°C, for example, 450°C, 470°C, 490°C, 500°C, 520°C, 540°C, 560°C, 580°C or 600°C.

[0057] In the present application, if the temperature of the second-stage calcination is too low, the coating layer will be unevenly carbonized, reducing the improvement effect; if the temperature of the second-stage calcination is too high, the pore size of the coating layer will shrink, hindering ion transfer.

[0058] In some embodiments, the second-stage calcination time is 2-5 h, for example, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.6 h, 3.8 h, 4 h, 4.2 h, 4.4 h, 4.6 h, 4.8 h or 5 h.

[0059] In some embodiments, the protective atmosphere of the first-stage calcination is the same as the protective atmosphere of the second-stage calcination. As a preferred technical solution, the preparation method includes the following steps:

[0060] (1) The electrode main material and the organic sulfonic acid substance in a mass ratio of (120-150):(1-18) are ball-milled in a solvent at 200-300 rpm for 5-7 hours at a mixing temperature of 40-80°C to obtain a mixture;

[0061] (2) The mixed material of step (1) is calcined in a protective atmosphere at 200-300° C. for 2-4 hours in a first stage, and then calcined in a protective atmosphere at 450-600° C. for 2-5 hours in a second stage to obtain the composite electrode material.

[0062] The present application provides a composite electrode material prepared by the above-mentioned preparation method, wherein the composite electrode material comprises an electrode material core and a sulfur-nitrogen-doped carbon coating layer located on the surface of the core.

[0063] In the present application, the electrode material may be a positive electrode material, such as lithium iron phosphate or lithium manganese oxide, or a negative electrode material, such as graphite negative electrode material.

[0064] The present application provides an electrode plate, which includes the composite electrode material as described above.

[0065] The present application provides a lithium-ion battery, which includes the above-mentioned electrode plate.

[0066] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, this application no longer exhaustively lists the specific point values ​​included in the range.

[0067] The technical solutions and technical effects of the present application are described in detail below through specific embodiments, comparative examples and application examples. The following embodiments are only some embodiments of the present application and do not specifically limit the present application.

[0068] Example 1

[0069] This embodiment provides a method for preparing a composite positive electrode material, as shown in FIG1 . The preparation method comprises the following steps:

[0070] (1) The electrode main material and the organic sulfonic acid substance were mixed in a solvent at a mass ratio of 135:10 to obtain a mixed slurry, and the mixed slurry was ball-milled at 200 rpm for 7 h at a mixing temperature of 60°C to obtain a mixed material;

[0071] The main electrode material is lithium iron phosphate, the organic sulfonic acid substance is taurine, and the solvent is methanol.

[0072] (2) The mixture of step (1) is calcined in a protective atmosphere (i.e., nitrogen) at 300°C for 4 hours, and then calcined in a second step at 550°C for 3 hours under a protective atmosphere (i.e., nitrogen) to obtain a composite electrode material, i.e., a lithium iron phosphate positive electrode material with a sulfur-nitrogen doped carbon coating layer.

[0073] Example 2

[0074] This embodiment provides a method for preparing a composite positive electrode material, the preparation method comprising the following steps:

[0075] (1) Lithium manganate and aminosulfonic acid in a mass ratio of 120:18 were mixed in ethanol to obtain a mixed slurry, and the mixed slurry was ball-milled at 250 rpm for 6 h at a mixing temperature of 40° C. to obtain a mixture;

[0076] (2) The mixture of step (1) was calcined in an argon atmosphere at 300° C. for 2 h in a first stage, and then calcined in an argon atmosphere at 450° C. for 5 h in a second stage to obtain a lithium manganate positive electrode material having a sulfur-nitrogen doped carbon coating layer.

[0077] Example 3

[0078] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:

[0079] (1) Artificial graphite and taurine in a mass ratio of 142:5 were mixed in N-methylpyrrolidone to obtain a mixed slurry, and the mixed slurry was ball-milled at 275 rpm for 5.5 h at a mixing temperature of 50°C to obtain a mixture;

[0080] (2) The mixed material of step (1) is calcined in a helium atmosphere at 250° C. for 3 h in a first stage, and then calcined in a helium atmosphere at 500° C. for 4 h in a second stage to obtain the graphite negative electrode material having a sulfur-nitrogen doped carbon coating layer.

[0081] Example 4

[0082] This embodiment provides a method for preparing a composite negative electrode material, the preparation method comprising the following steps:

[0083] (1) Natural graphite and aminosulfonic acid at a mass ratio of 150:1 were mixed in ethanol to obtain a mixed slurry, and the mixed slurry was ball-milled at 300 rpm for 5 h at a mixing temperature of 80°C to obtain a mixture;

[0084] (2) The mixture of step (1) was calcined in a nitrogen atmosphere at 200° C. for 4 h in a first stage, and then calcined in a nitrogen atmosphere at 600° C. for 2 h in a second stage to obtain a graphite negative electrode material having a sulfur-nitrogen doped carbon coating layer.

[0085] Example 5

[0086] The difference between this embodiment and embodiment 1 is that the mass ratio of lithium iron phosphate to taurine in step (1) is 110:18.

[0087] The rest of the preparation methods and parameters remained the same as in Example 1.

[0088] Example 6

[0089] The difference between this embodiment and embodiment 1 is that the mass ratio of lithium iron phosphate to taurine in step (1) is 160:1.

[0090] The rest of the preparation methods and parameters remained the same as in Example 1.

[0091] Example 7

[0092] The difference between this embodiment and embodiment 1 is that the temperature of the first-stage calcination in step (2) is 150° C. The rest of the preparation methods and parameters are the same as those in embodiment 1.

[0093] Example 8

[0094] The difference between this embodiment and embodiment 1 is that the temperature of the first-stage calcination in step (2) is 350° C. The rest of the preparation methods and parameters are the same as those in embodiment 1.

[0095] Example 9

[0096] The difference between this embodiment and embodiment 1 is that the temperature of the second-stage calcination in step (2) is 400° C. The rest of the preparation method and parameters are the same as those in embodiment 1.

[0097] Example 10

[0098] The difference between this embodiment and embodiment 1 is that the temperature of the second-stage calcination in step (2) is 650° C. The rest of the preparation method and parameters are the same as those in embodiment 1.

[0099] Comparative Example 1

[0100] The difference between this comparative example and Example 1 is that the taurine in step (1) is replaced by benzenesulfonic acid.

[0101] The rest of the preparation methods and parameters remained the same as in Example 1.

[0102] Comparative Example 2

[0103] The difference between this comparative example and Example 1 is that the taurine in step (1) is replaced by benzenesulfonamide.

[0104] The rest of the preparation methods and parameters remained the same as in Example 1.

[0105] Comparative Example 3

[0106] This comparative example provides the same lithium iron phosphate positive electrode material as that of Example 1, except that taurine is not used for coating.

[0107] Application Example 1

[0108] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 1, conventional artificial graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0109] Application Example 2

[0110] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 2, conventional artificial graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0111] Application Example 3

[0112] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 5, conventional artificial graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0113] Application Example 4

[0114] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 6, conventional artificial graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0115] Application Example 5

[0116] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 7, conventional artificial graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0117] Application Example 6

[0118] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 8, conventional artificial graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0119] Application Example 7

[0120] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 9, conventional natural graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0121] Application Example 8

[0122] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 10, conventional natural graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0123] Application Example 9

[0124] This application example provides a lithium-ion battery, which uses the negative electrode plate prepared from the composite negative electrode material provided in Example 3, conventional lithium manganese oxide as the positive electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0125] Application Example 10

[0126] This application example provides a lithium-ion battery, which uses the negative electrode plate prepared from the composite negative electrode material provided in Example 4, conventional lithium iron phosphate as the positive electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0127] Application Example 11

[0128] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 1, a negative electrode plate prepared from the composite negative electrode material provided in Example 3, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0129] Application Example 12

[0130] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 2, a negative electrode plate prepared from the composite negative electrode material provided in Example 4, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0131] Application Example 13

[0132] This application example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Example 1, a negative electrode plate prepared from the composite negative electrode material provided in Example 4, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0133] Comparative Application Example 1

[0134] This application comparative example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Comparative Example 1, conventional artificial graphite as a negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0135] Application Comparative Example 2

[0136] This application comparative example provides a lithium-ion battery, which uses a positive electrode plate prepared from the composite positive electrode material provided in Comparative Example 2, conventional artificial graphite as the negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0137] Application Comparative Example 3

[0138] This application comparative example provides a lithium-ion battery, which uses a positive electrode plate prepared from the positive electrode material provided in comparative example 3, conventional natural graphite as the negative electrode plate, a ceramic-coated diaphragm, and an electrolyte of lithium hexafluorophosphate organic electrolyte to assemble a lithium-ion battery.

[0139] Performance Testing

[0140] Electrochemical performance testing was performed on the lithium-ion batteries provided in Example 1-13 and Comparative Example 1-3. Test conditions included: rate testing at 1C, cycle stability at 4000 cycles, and high-rate charge / discharge capacity at 3C. The test results are shown in Table 1.

[0141] Table 1

[0142] Rate performance (%) Cycle capacity retention rate (%) High rate charge and discharge capacity (Ah) Application example 1 98.9% 86.5 55.6 Application example 2 98.5% 85.7 53.8 Application example 3 98.7% 86.0 54.6 Application example 4 98.4% 85.4 53.1 Application example 5 98.0% 84.6 52.4 Application example 6 97.8% 84.0 51.9 Application example 7 97.8% 83.8 51.8 Application example 8 97. 6%83.251.2Application Example 998.5%85.853.7Application Example 1098.3%86.052.8Application Example 1199.3%87.557.2Application Example 1298.9%87.055.9Application Example 1399.1%87.356.9Application Comparison Example 196.8%80.548.6Application Comparison Example 297.0%81.849.8Application Comparison Example 396.7%80.148.1

[0143] analyze:

[0144] From the data results of application examples 1-2, it can be seen that the effect of taurine on the coating of lithium iron phosphate materials on improving the battery rate performance and cycle performance is better than the effect of aminosulfonic acid on the coating of lithium manganese iron materials; from the data results of application examples 9-10, it can be seen that the effect of taurine on the coating of artificial graphite materials on improving the battery rate performance and cycle performance is better than the effect of aminosulfonic acid on the coating of natural graphite materials; from the data results of application examples 11-13, it can be seen that the best improvement effect is achieved by coating both the positive and negative electrode materials with taurine at the same time.

[0145] From the comparison of the data results of Application Example 1 and Application Examples 3-4, it can be seen that if the amount of taurine is too much, the lithium ion insertion or deintercalation channel will be lengthened, and the difficulty of lithium ion migration will increase, resulting in the improvement of battery rate performance and cycle performance not being obvious; if the amount of taurine is too little, the main material structure of the electrode cannot be completely covered, and the improvement of battery rate performance and cycle performance is not obvious.

[0146] From the comparison of the data results of Application Example 1 and Application Examples 5-6, it can be seen that if the temperature of the first-stage calcination is too low, the coating will agglomerate and cannot form a layered structure, resulting in a decrease in the rate performance and cycle performance of the battery; if the temperature of the first-stage calcination is too high, the coating will crack and the structure will be destroyed, resulting in a decrease in the rate performance and cycle performance of the battery.

[0147] From the comparison of the data results of Application Example 1 and Application Examples 7-8, it can be seen that if the temperature of the second-stage calcination is too low, the carbonization of the coating layer will be uneven, reducing the improvement effect; if the temperature of the second-stage calcination is too high, the pore size of the coating layer will shrink, hindering ion charge transfer, resulting in a decrease in the battery's rate performance and cycle performance.

[0148] From the comparison of the data results of Application Example 1 and Comparative Example 1, it can be seen that compared with benzenesulfonic acid, taurine is better in improving the battery rate performance and cycle performance when applied to the coated lithium iron phosphate material.

[0149] From the comparison of the data results of Application Example 1 and Comparative Example 2, it can be seen that compared with benzenesulfonamide, taurine is better used in coating lithium iron phosphate materials to improve battery rate performance and cycle performance.

[0150] From the comparison of the data results of Application Example 1 and Comparative Example 3, it can be seen that the application of taurine in coating lithium iron phosphate materials has a significant improvement in the battery rate performance and cycle performance.

Claims

1. A method for preparing a composite electrode material, wherein: The preparation method comprises the following steps: The electrode main material and the organic sulfonic acid substance are mixed and calcined to obtain the composite electrode material; wherein the elements in the organic sulfonic acid substance include carbon, nitrogen and sulfur.

2. The preparation method according to claim 1, wherein The organic sulfonic acid substances include taurine and / or aminosulfonic acid.

3. The preparation method according to claim 1, wherein The mass ratio of the electrode main material to the organic sulfonic acid substance is (120-150):(1-18).

4. The preparation method according to any one of claims 1 to 3, wherein: The mixing method includes ball milling.

5. The preparation method according to claim 4, wherein The ball milling mixing includes dry ball milling or wet ball milling.

6. The preparation method according to claim 5, wherein: The steps of wet ball milling include: Dispersing the electrode main material and the organic sulfonic acid substance in a solvent to obtain a mixed slurry; The mixed slurry is ball milled.

7. The preparation method according to claim 6, wherein: The solvent includes at least one of methanol, ethanol or N-methylpyrrolidone, or a combination of at least two thereof.

8. The preparation method according to any one of claims 4 to 7, wherein: The ball milling speed is 200-300 rpm.

9. The preparation method according to any one of claims 1 to 8, wherein: The mixing temperature is 40-80°C.

10. The preparation method according to any one of claims 1 to 8, wherein the mixing time is 5 to 7 hours.

11. The preparation method according to any one of claims 1 to 10, wherein: The calcination is carried out under a protective atmosphere.

12. The preparation method according to any one of claim 11, wherein: The gas in the protective atmosphere includes at least one of nitrogen, argon or helium, or a combination of at least two of them.

13. The preparation method according to any one of claims 1 to 12, wherein: The calcination step is a step-by-step calcination; The stepwise calcination includes a first-step calcination and a second-step calcination.

14. The preparation method according to claim 13, wherein: The temperature of the first-stage calcination is 200-300°C.

15. The preparation method according to claim 13, wherein: The first-stage calcination time is 2-4 hours.

16. The preparation method according to claim 13, wherein: The temperature of the second stage calcination is 450-600°C.

17. The preparation method according to claim 13, wherein: The second stage calcination time is 2-5h.

18. The preparation method according to any one of claims 1 to 17, wherein: The preparation method comprises the following steps: The electrode main material and the organic sulfonic acid substance in a mass ratio of (120-150):(1-18) are ball-milled in a solvent at 200-300 rpm for 5-7 hours at a mixing temperature of 40-80° C. to obtain a mixture; The mixed material is first calcined in a protective atmosphere at 200-300° C. for 2-4 hours, and then second calcined in a protective atmosphere at 450-600° C. for 2-5 hours to obtain the composite electrode material.

19. A composite electrode material prepared by the preparation method according to any one of claims 1 to 18, wherein: The composite electrode material comprises an electrode material core and a sulfur-nitrogen doped carbon coating layer located on the surface of the core.

20. An electrode plate, wherein: The electrode plate comprises the composite electrode material as claimed in claim 19.

Citation Information

Patent Citations

  • Lithium iron phosphate / nitrogen and sulfur codoped graphene composite material and preparation method thereof

    CN108565432A

  • Preparation method of carbon-coated lithium iron phosphate positive electrode material

    CN112599730A

  • Double-coated positive electrode material as well as preparation method and application thereof

    CN115810744A

  • Lithium iron phosphate positive electrode material and preparation method and application thereof

    CN116002654A

  • Composite electrode material and preparation method and application thereof

    CN116525827A

Cited By

  • Preparation method of biomass derived hard carbon negative electrode material and sodium ion battery

    CN119873816A