Sodium iron sulfate positive electrode material, and preparation method therefor and use thereof
By using amphiphilic molecule coating technology with a moderate hydrophilic-hydrophobic balance value in the preparation of sodium iron sulfate cathode materials, the problem of material sensitivity to air is solved, and the stability and circulation of electrochemical performance when left in the air for a long time are achieved. Performance improvements.
Patent Information
- Application Number
- PCT/CN2023/142447
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-31
AI Technical Summary
Sodium iron sulfate cathode material is sensitive to air humidity and oxidizing atmosphere, which leads to the formation of surface residual alkali and oxidation of ferrous ions, increases the difficulty of pulping and coating, and deteriorates specific capacity and cycle performance.
During the preparation process, amphiphilic molecules with moderate hydrophilic-hydrophobic balance values are introduced to coat the sodium ferric sulfate particles so that the hydrophilic end points to the sodium ferric sulfate and the hydrophobic end points to the outside, thereby isolating the sodium ferric sulfate from contact with air and improving its stability.
The electrochemical performance of the sodium iron sulfate cathode material did not decline significantly after being left in the air for 12 months, which improved its air stability and cycle performance.
Smart Images

Figure CN2023142447_31102024_PF_FP_ABST
Abstract
Description
Sodium iron sulfate positive electrode material and its preparation method and application Technical Field
[0001] The present invention belongs to the technical field of new energy materials, and in particular relates to a sodium iron sulfate positive electrode material and a preparation method and application thereof. Background Art
[0002] As a supplement to lithium-ion batteries, sodium-ion batteries are expected to be used in low-speed electric vehicles, communication base stations, large-scale energy storage and other fields. Compared with lithium-ion batteries, the advantage of sodium-ion batteries is that the crustal reserves of sodium resources are abundant (2.75%), which is more than 400 times that of lithium (0.0065%), and they are evenly distributed around the world and simple to refine. In addition, sodium-ion batteries have higher internal resistance than lithium-ion batteries, generate less instantaneous heat in the case of a short circuit, have a lower temperature rise, and have a higher thermal runaway temperature than lithium batteries, which makes them safer. Sodium-ion batteries have a wider operating temperature range (-40°C to 80°C), which makes them suitable for extremely cold and hot scenes. Sodium-ion batteries have excellent fast charging capabilities, and charging time only takes about 10 minutes. Sodium-ion batteries can use aluminum foil as positive and negative current collectors, which has a lower current collector cost. Therefore, the development of high-efficiency and low-cost sodium-ion battery technology is of great significance.
[0003] As a key component of sodium-ion batteries, positive electrode materials affect the cost, energy density, cycle life, etc. of sodium-ion batteries. Positive electrode materials affect the energy density and power density of sodium-ion batteries by affecting the ability to accommodate sodium ions and the patency of the transmission channel. At the same time, the stability and impurity composition of the positive electrode materials will affect the life of the battery. The current mainstream sodium-ion positive electrode materials are divided into three categories: oxides, polyanionic compounds and Prussian blue analogues. In comparison, oxide positive electrode materials have a simple structure, high energy density, and moderate cycle performance; polyanionic positive electrode materials have a stable structure, low energy density, and the best cycle performance; Prussian blue analogues have an adjustable working voltage, good rate performance, and the cycle performance needs to be improved. Sodium ferrous sulfate (chemical formula Na 2+x Fe 2-y (SO4)3, x = 0-0.7, y = 0–0.35) is a polyanionic cathode material used in sodium ion batteries. It has the advantages of abundant crustal reserves of raw materials, low cost, high operating voltage, and good long cycle performance. It was reported in 2014. Due to the strong inductive effect of sulfate, this material shows the highest Fe 3+ / Fe 2+Redox potential, thus making up for the shortcoming of insufficient energy density to a certain extent, and the theoretical energy density reaches 540Wh / kg. Some people have reported non-stoichiometric sodium ferric sulfate, which has expanded the scope of exploration of this system. The three-dimensional skeleton structure of sodium ferric sulfate can remain stable during the migration of sodium ions, so the cycle performance is better. One of the key problems of sodium ferric sulfate is its sensitivity to air. Due to the interaction with moisture and oxygen in the air, sodium ferric sulfate will have residual alkali on the surface, and some ferrous ions will be oxidized, which increases the difficulty of pulping and coating, and deteriorates the specific capacity and cycle performance. To address this problem, the relevant technology has improved the antioxidant ability of the material by preparing a nitrogen-doped graphene-coated sodium ferric sulfate positive electrode. The Fe detected after one month of exposure to air was 3+ The ionization rate (14%) is significantly lower than that of the uncoated material (29%). Other technologies have reported sodium iron sulfate cathodes coated with reduced graphene oxide, but these have not demonstrated the material's environmental stability. However, most existing studies require the use of graphene-based materials, which are costly and involve complex processes. Furthermore, most of the resulting materials still contain trivalent iron, which is detrimental to electrochemical performance.
[0004] Therefore, it is imperative to solve the current problems of sodium iron sulfate positive electrode materials such as sensitivity to air humidity and oxidizing atmosphere.
[0005] Summary of the Invention
[0006] The present invention aims to address at least one of the technical problems existing in the prior art. To this end, the present invention proposes a sodium ferric sulfate cathode material. By introducing amphiphilic molecules with a moderate hydrophilic-hydrophobic balance (HLB) during the preparation process, the surface of the prepared sodium ferric sulfate particles is uniformly coated with a layer of amphiphilic molecules, wherein the hydrophilic ends of the amphiphilic molecules point toward the sodium ferric sulfate and the hydrophobic ends point outward, thereby isolating the sodium ferric sulfate particles from air and protecting the sodium ferric sulfate. The sodium ferric sulfate cathode material provided by the present invention can be stored in air for long periods of time, with no significant degradation in electrochemical performance after 12 months of storage.
[0007] The second aspect of the present invention provides a method for preparing the above-mentioned sodium iron sulfate positive electrode material.
[0008] A third aspect of the present invention provides an application of a positive electrode material in the preparation of a sodium ion battery.
[0009] A fourth aspect of the present invention provides an application of a sodium ion battery in the field of secondary batteries.
[0010] According to the first aspect of the present invention, a sodium ferric sulfate positive electrode material is provided. The positive electrode material comprises sodium ferric sulfate and amphiphilic molecules modifying the sodium ferric sulfate, wherein the hydrophilic ends of the amphiphilic molecules face the sodium ferric sulfate and the hydrophobic ends of the amphiphilic molecules face away from the sodium ferric sulfate; and the HLB of the amphiphilic molecules is 10 to 16.
[0011] A sodium iron sulfate positive electrode material according to an embodiment of the present invention has at least the following beneficial effects:
[0012] During the preparation process of the sodium ferric sulfate cathode material of the present invention, amphiphilic molecules with a moderate hydrophilic-hydrophobic balance (HLB) are selected, so that the surface of the sodium ferric sulfate particles is surrounded by amphiphilic molecules. The hydrophilic ends of the amphiphilic molecules point toward the sodium ferric sulfate, while the hydrophobic ends point outward, thereby isolating the sodium ferric sulfate particles from air and effectively improving the stability of the sodium ferric sulfate in air. The sodium ferric sulfate cathode material of the present invention can be stably placed in an air environment for 12 months without significant degradation of electrochemical performance.
[0013] According to some preferred embodiments of the present invention, the HLB of the amphiphilic molecule is 13-15.
[0014] According to some embodiments of the present invention, the amphiphilic molecules include polyoxypropylene (5PO) lanolin ether, polyoxyethylene (5EO) sorbitan monooleate, polyoxyethylene cetyl ether, polyoxyethylene (20EO) sorbitan tristearate, polyoxyethylene lauryl ether, polyoxyethylene (20EO) sorbitan trioleate, polyoxyethylene oxypropylene oleate, polyoxyethylene lanolin derivatives, polyoxyethylene monooleate, polyoxyethylene monooleate, polyoxyethylene monopalmitate, polyoxyethylene monostearate, polyoxyethylene (10EO) oleyl ether, polyoxyethylene monolaurate, polyoxyethylene alkylphenol, polyoxyethylene (10EO) acetylated lanolin derivatives, polyoxyethylene sorbitol lanolin derivatives, polyoxyethylene alkylaryl ether, polyoxyethylene monolaurate, polyoxyethylene At least one of lauryl ether, polyoxyethylene castor oil, polyoxyethylene vegetable oil, polyoxyethylene (4EO) sorbitan monolaurate, cholesterol ether, lanolin alcohol ether, polyoxyethylene (20EO) sorbitan monostearate, polyoxyethylene (20EO) oleyl ether, polyoxyethylene (20EO) methyl glucoside sesquioleate, polyoxyethylene (16EO) lanolin alcohol ether, polyoxyethylene (20EO) sorbitan monooleate, polyoxyethylene monostearate, polyoxyethylene monooleate, polyoxyethylene oleyl ether, polyoxyethylene octadecyl alcohol, polyoxyethylene oleyl alcohol, polyoxyethylene fatty alcohol, polyethylene glycol monopalmitate, polyoxyethylene (20EO) sorbitan monopalmitate, polyoxyethylene cetyl alcohol, polyoxyethylene oxypropylene stearate and polyoxyethylene monostearate.
[0015] According to some embodiments of the present invention, the amphiphilic molecule further comprises mixed fatty acid polyoxyethylene ester and resin acid polyoxyethylene ester.
[0016] According to some preferred embodiments of the present invention, the amphiphilic molecule includes at least one of polyoxyethylene (10EO) acetylated lanolin derivatives, polyoxyethylene sorbitol lanolin derivatives, polyoxyethylene alkyl aryl ethers, polyoxyethylene monolaurate, polyoxyethylene lauryl ether, polyoxyethylene castor oil, polyoxyethylene vegetable oil, polyoxyethylene (4EO) sorbitan monolaurate, cholesterol ether, lanolin ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene (20EO) sorbitan monostearate, polyoxyethylene (20EO) oleyl ether, polyoxyethylene (20EO) methyl glucoside sesquioleate, polyoxyethylene (16EO) lanolin ether, polyoxyethylene (20EO) sorbitan monooleate and polyoxyethylene monostearate.
[0017] According to an embodiment of the second aspect of the present invention, a method for preparing a positive electrode material includes:
[0018] The raw material for preparing sodium ferric sulfate, the amphiphilic molecule, the non-polar organic solvent and the polar solvent are mixed and heated, and then impurities are removed;
[0019] The mixed heating includes a first heating and a second heating performed sequentially;
[0020] The temperature of the first heating is 50 to 100° C.; the time of the first heating is 1 to 12 hours;
[0021] The temperature of the second heating is 120 to 250° C.; and the time of the second heating is 1 to 12 hours.
[0022] A method for preparing a positive electrode material according to an embodiment of the present invention has at least the following beneficial effects:
[0023] 1. The first low-temperature heating and heat preservation can promote the uniformity of the system, thereby providing favorable conditions for the second high-temperature coating and improving the air stability of the positive electrode material. The second heating and heat preservation promote the formation of sodium iron sulfate positive electrode material.
[0024] 2. The effective combination of polar solvents and non-polar solvents can promote the formation of a uniform protective layer of amphiphilic molecules on the surface of the sodium ferric sulfate sample, with the hydrophilic end facing the sodium ferric sulfate and the hydrophobic end facing away from the sodium ferric sulfate.
[0025] According to some embodiments of the present invention, the temperature of the first heating is 70-90° C.; and the time of the first heating is 1-3 hours.
[0026] According to some embodiments of the present invention, the temperature of the second heating is 170-190° C.; and the time of the second heating is 3-5 hours.
[0027] According to some embodiments of the present invention, the temperature of the first heating is 80° C.; and the time of the first heating is 2 hours.
[0028] According to some embodiments of the present invention, the temperature of the second heating is 180° C.; and the time of the second heating is 4 hours.
[0029] According to some embodiments of the present invention, the impurity removal step includes cooling, solid-liquid separation, washing, and drying to obtain the target product.
[0030] According to some embodiments of the present invention, a method for preparing the positive electrode material includes:
[0031] S1: mixing the raw material for preparing sodium ferric sulfate, the amphiphilic molecule, a non-polar organic solvent and a polar solvent to obtain a mixed solution;
[0032] S2: placing the mixed solution in step S1 into a stainless steel reactor lined with polytetrafluoroethylene and heating;
[0033] S3: After heating, the mixture is cooled to room temperature, filtered (solid-liquid separation), washed with anhydrous alcohol, and dried naturally to obtain the target product.
[0034] The invention provides a preparation method with simple preparation steps, low energy consumption, good product uniformity and high yield.
[0035] According to some embodiments of the present invention, the polar solvent includes at least one of water, formamide, acetone, trifluoroacetic acid, ethanol, chloroform, ether, acetic acid, acetonitrile, isopropanol, methanol, dimethyl sulfoxide, acetonitrile, N,N-dimethylformamide, hexamethylphosphoramide, pyridine, tetramethylethylenediamine, triethylamine, n-butanol, dioxane, tetrahydrofuran and methyl formate.
[0036] According to some embodiments of the present invention, the non-polar solvent includes at least one of benzene, carbon tetrachloride, hexane, isooctane, dichloromethane, cyclohexane, petroleum ether and pentane.
[0037] According to some embodiments of the present invention, the raw materials for preparing the sodium ferric sulfate include sodium sulfate and ferrous sulfate hydrate.
[0038] According to some embodiments of the present invention, the ferrous sulfate hydrate includes at least one of ferrous sulfate monohydrate, ferrous sulfate pentahydrate, and ferrous sulfate heptahydrate.
[0039] According to some embodiments of the present invention, the ratio of the polar solvent, the non-polar solvent, the amphiphilic molecule, the sodium sulfate and the ferrous sulfate hydrate is 1-20:1-20:10-500:5-6.75:10-13.5, wherein the polar solvent and the non-polar solvent are calculated by volume liters, the amphiphilic molecule is calculated by mass grams, and the sodium sulfate and the ferrous sulfate hydrate are calculated by amount of substance mole.
[0040] According to some preferred embodiments of the present invention, the ratio of the polar solvent, the non-polar solvent, the amphiphilic molecule, the sodium sulfate and the ferrous sulfate hydrate is 10-20:10-20:100-500:5-6.75:10-13.5, wherein the polar solvent and the non-polar solvent are calculated by volume liters, the amphiphilic molecule is calculated by mass grams, and the sodium sulfate and the ferrous sulfate hydrate are calculated by amount of substance mole.
[0041] According to some preferred embodiments of the present invention, the ratio of the polar solvent, the non-polar solvent, the amphiphilic molecule, the sodium sulfate and the ferrous sulfate hydrate is 10:10:100:6:12, wherein the polar solvent and the non-polar solvent are calculated by volume liters, the amphiphilic molecule is calculated by mass grams, and the sodium sulfate and the ferrous sulfate hydrate are calculated by amount of substance mole.
[0042] According to the third aspect of the present invention, a positive electrode material is used in a sodium ion battery.
[0043] According to some embodiments of the present invention, the method for preparing a sodium ion battery includes:
[0044] A1: Mix the sodium ferric sulfate positive electrode material, conductive agent, and binder in a mass ratio of 8:1:1. After thorough grinding, add an appropriate amount of N-methylpyrrolidone to form a uniform slurry. Use a scraper to apply the slurry to the surface of aluminum foil with a thickness of 200μm. After vacuum drying, cut into discs with a diameter of 10mm, compact them, and set aside as positive electrode sheets.
[0045] A2: In an inert gas-protected glove box, press the sodium metal into thin sheets, cut them into 12 mm diameter discs, and reserve them for use as the battery negative electrode.
[0046] A3: Cut the commercial fiberglass film into 16 mm diameter discs and set aside for use as the diaphragm.
[0047] A4: In an inert gas-protected glove box, the prepared positive electrode, separator, and negative electrode were stacked tightly in sequence, and commercial electrolyte (1.0M NaClO4 in EC:PC = 1:1 Vol%) was added dropwise to completely soak the separator. The stacked portion was then encapsulated into a button-type battery casing to complete the battery assembly.
[0048] According to some embodiments of the present invention, the conductive agent includes at least one of conductive carbon black, Ketjen black, super P, conductive carbon balls, conductive graphite, carbon nanotubes, carbon fibers, and graphene.
[0049] According to some embodiments of the present invention, the binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, carboxymethyl cellulose, SBR rubber, and polyolefin.
[0050] When the sodium ferric sulfate cathode material prepared in this invention is assembled into a battery, the hydrophobic ends of the amphiphilic molecules effectively connect the cathode and the organic solvent in the electrolyte, thereby increasing the wettability between the cathode and the electrolyte and providing an effective path for the rapid conduction of sodium ions. Compared with other methods, the solution provided by this invention has a simple process and low energy consumption. The prepared sodium ferric sulfate cathode has good air stability and excellent rate performance.
[0051] According to a fourth aspect of the present invention, an embodiment of a sodium ion battery is used in the field of secondary batteries.
[0052] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the following description of the embodiments with reference to the accompanying drawings, in which:
[0054] FIG1 is a schematic structural diagram of a sodium iron sulfate positive electrode material according to Example 1 of the present invention;
[0055] FIG2 is an XRD pattern of the sodium ferric sulfate cathode material prepared in Example 1 (fresh sample), the sodium ferric sulfate cathode material prepared in Example 1 after being stored in air for 12 months (sample after being stored for 12 months), and standard ferrous sulfate;
[0056] 3 is an SEM image of the sodium ferric sulfate cathode material prepared in Example 1 (fresh sample) and the sodium ferric sulfate cathode material prepared in Example 1 after being placed in air for 12 months (sample after being placed for 12 months);
[0057] FIG4 is a graph showing the cycle capacity of batteries prepared using the fresh sample and the sample after 12 months of storage in Example 1 as raw materials;
[0058] FIG5 shows the charge-discharge curves of the 500th and 900th cycles of the battery prepared using the sample of Example 1 after being set aside for 12 months as raw material. DETAILED DESCRIPTION
[0059] The following describes embodiments of the present invention in detail. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended only to explain the present invention and are not to be construed as limiting the present invention.
[0060] Example 1
[0061] This embodiment discloses a sodium iron sulfate positive electrode material and a preparation method thereof, the specific steps are:
[0062] S1: 10 L of distilled water, 10 L of benzene, 100 g of polyoxyethylene castor oil, 6 mol of sodium sulfate, and 12 mol of ferrous sulfate heptahydrate were mixed to obtain a mixed solution;
[0063] S2: The mixed solution was placed in a 40-liter polytetrafluoroethylene-lined stainless steel reactor, heated to 80°C, kept warm for 2 hours, and then heated to 180°C and kept warm for 4 hours;
[0064] S3: Cooling to room temperature, filtering (solid-liquid separation), washing with anhydrous alcohol, and air-drying to obtain the target product.
[0065] Figure 2 shows the XRD patterns of the fresh sample obtained in Example 1, the sample after 12 months in air, and standard ferrous sulfate. As can be seen from the figure, the diffraction spectrum of the sample obtained in Example 1 matches the standard diffraction spectrum very well, and the XRD pattern of the sample after 12 months in air still matches the standard diffraction spectrum very well.
[0066] Figure 3 shows SEM images of the sample obtained in Example 1 and the sample after being stored in air for 12 months. As can be seen from the figure, the sample still has good morphology after storage, with no deformation, surface roughness, or precipitation of small particles.
[0067] Figure 4 shows the cycling capacity of batteries prepared using the fresh sample and the sample after 12 months of storage from Example 1. As can be seen from the figure, both batteries exhibit good cycling stability, and the long-term cycling performance of the sample after storage remains essentially unchanged.
[0068] FIG5 shows the charge-discharge curves of the 500th and 900th cycles of the battery prepared using the sample of Example 1 after being shelved for 12 months as raw material. As can be seen from the figure, the electrochemical reversibility and stability of the sample after shelving are good.
[0069] Compared with Example 1, Examples 2 to 8 only changed the type of non-polar solvent. The specific experimental conditions are shown in Table 1.
[0070] Compared with Example 1, Examples 9 to 10 only changed the volume of the non-polar solvent. The specific experimental conditions are shown in Table 1.
[0071] Compared with Example 1, Examples 11 to 18 only changed the type of polar solvent. The specific experimental conditions are shown in Table 1.
[0072] Compared with Example 1, Examples 19 to 20 only changed the volume of the polar solvent. The specific experimental conditions are shown in Table 1.
[0073] Compared with Example 1, Examples 21 to 40 only changed the type of amphiphilic molecules. The specific experimental conditions are shown in Table 1.
[0074] Compared with Example 1, Examples 41 to 45 only changed the mass of the amphiphilic molecules. The specific experimental conditions are shown in Table 1.
[0075] Compared with Example 1, Examples 46 to 48 only changed the amount of sodium sulfate. The specific experimental conditions are shown in Table 1.
[0076] Compared with Example 1, Examples 49 to 50 only changed the type of ferrous sulfate hydrate. The specific experimental conditions are shown in Table 1.
[0077] Compared with Example 1, Examples 51 to 53 only changed the amount of ferrous sulfate heptahydrate. The specific experimental conditions are shown in Table 1.
[0078] Compared with Example 1, Examples 54 to 55 only changed T1. The specific experimental conditions are shown in Table 1.
[0079] Compared with Example 1, Examples 56 to 57 only changed t1. The specific experimental conditions are shown in Table 1.
[0080] Compared with Example 1, Examples 58 to 59 only changed T2. The specific experimental conditions are shown in Table 1.
[0081] Compared with Example 1, Examples 60 to 61 only changed t2. The specific experimental conditions are shown in Table 1.
[0082] Compared with Example 1, Examples 62 to 65 respectively adopted a mixed polar solvent, a mixed non-polar solvent, a mixed amphiphilic molecule and a mixed ferrous sulfate hydrate.
[0083] Compared with Example 1, Examples 66 to 67 comprehensively changed T1, t1, T2, and t2. The specific experimental conditions are shown in Table 1.
[0084] Table 1 Experimental conditions of Examples 2 to 67
[0085] Comparative Example 1
[0086] This comparative example discloses a sodium iron sulfate positive electrode material and a preparation method thereof. The difference between this comparative example and Example 1 is that the polyoxyethylene castor oil in Example 1 is not included, and other conditions are the same as those in Example 1.
[0087] Comparative Example 2
[0088] This comparative example discloses a sodium iron sulfate positive electrode material and a preparation method thereof. The difference between this comparative example and Example 1 is that the distilled water in Example 1 is not included, and other conditions are the same as those in Example 1.
[0089] Comparative Example 3
[0090] This comparative example discloses a sodium iron sulfate positive electrode material and a preparation method thereof. The difference between this comparative example and Example 1 is that the benzene in Example 1 is not included, and other conditions are the same as those in Example 1.
[0091] Comparative Example 4
[0092] This comparative example discloses a sodium iron sulfate positive electrode material and a preparation method thereof. The difference between this comparative example and Example 1 is that the temperature is directly raised to 180°C without performing a 2-hour heat preservation operation at 80°C. Other conditions are the same as those in Example 1.
[0093] Comparative Example 5
[0094] This comparative example discloses a sodium iron sulfate positive electrode material and a preparation method thereof. The difference between this comparative example and Example 1 is that only a 2-hour heat preservation operation at 80°C is performed and the temperature is no longer raised to 180°C. Other conditions are the same as those in Example 1.
[0095] Comparative Example 6
[0096] This comparative example discloses a sodium iron sulfate positive electrode material and a preparation method thereof. The difference between this comparative example and Example 1 is that tetraethylene glycol oleic acid (HLB value is 7.7) with an HLB of less than 10 is introduced as an amphiphilic molecule, and other conditions are the same as those in Example 1.
[0097] Comparative Example 7
[0098] This comparative example discloses a sodium iron sulfate cathode material and a preparation method thereof. The difference between this comparative example and Example 1 is that potassium oleate (HLB value is 20) with an amphiphilic molecule having an HLB greater than 16 is introduced. Other conditions are the same as those in Example 1.
[0099] Test Example 1
[0100] Test Example 1 is a sodium ion battery prepared using the sodium iron sulfate positive electrode materials of Comparative Examples 1 to 7 and Examples 1 to 67. The preparation method includes the following steps:
[0101] A1: Preparation of positive electrode: The positive electrode active materials of Examples 1 to 67 and Comparative Examples 1 to 7, conductive carbon (SuperP), and binder (polyvinylidene fluoride) were mixed in a mass ratio of 7.5:1.5:1, and after thorough grinding, an appropriate amount of nitrogen-methyl pyrrolidone was added to form a uniform slurry; the slurry was coated on the surface of aluminum foil with a scraper to a thickness of 2 μm, and after vacuum drying, it was cut into discs with a diameter of 10 mm, compacted, and reserved as positive electrode sheets.
[0102] A2: Preparation of negative electrode: In an inert gas-protected glove box, press metallic sodium into thin sheets, cut into 12 mm diameter discs, and reserve them for use as the battery negative electrode.
[0103] A3: Preparation of diaphragm: Cut commercial glass fiber film into discs with a diameter of 16 mm and set aside as diaphragm.
[0104] A4: Assemble the battery: In an inert gas-protected glove box, stack the prepared battery positive electrode, separator, and battery negative electrode tightly in sequence, add commercial electrolyte (1.0M NaClO4 in EC:PC=1:1Vol%) to completely soak the separator, and then encapsulate the above stacked part into a button battery shell to complete the battery assembly.
[0105] Performance test: Sodium ion batteries prepared from the sodium iron sulfate positive electrode materials of comparative examples 1 to 7 and embodiments 1 to 67 were tested. The constant current charge and discharge test adopted the BTSDA test system of Shenzhen Xinwei Electronics Co., Ltd., the environment was a constant temperature and humidity room (25°C, 35%), and the test voltage range was 2.0 to 4.5V. The rate was 0.1C for the first ten cycles, and the rate was changed to 1C (1C = 120mAh / g) starting from the eleventh cycle. The test results are shown in Table 2; wherein, the median voltage refers to the median voltage of the 100th cycle, and the capacity retention rate refers to the capacity retention rate of the 1000th cycle relative to the 11th cycle. The test results are shown in Table 2.
[0106] Table 2: Electrochemical test results of sodium ion batteries
[0107] From Table 2 we can see that:
[0108] Compared with the sodium ion batteries prepared by using the sodium iron sulfate positive electrode material in Examples 2 to 67 and Example 1, the influence of different preparation conditions on the product performance is summarized as follows:
[0109] From the sodium ion batteries prepared from the sodium iron sulfate positive electrode materials of Examples 2 to 8 and Example 1, it can be seen that the type of non-polar solvent has little effect on the electrochemical performance and air stability of the battery;
[0110] It can be seen from the sodium ion batteries prepared from the sodium iron sulfate positive electrode materials of Examples 9, 10 and Example 1 that when the volume proportion of the non-polar solvent used is too small, the specific capacity of the positive electrode material and the positive electrode material after being shelved for 12 months are both reduced, and the specific capacity decreases more seriously after shelving, indicating that a small volume of the non-polar solvent is not conducive to the formation of the positive electrode material, and is not conducive to the stability of the positive electrode material in the air; when the volume proportion of the non-polar solvent reaches a certain value, it has little effect on the electrochemical properties and air stability of the positive electrode material.
[0111] From the sodium ion batteries prepared from the sodium iron sulfate positive electrode materials of Examples 11 to 18 and Example 1, it can be seen that the type of polar solvent has little effect on the electrochemical performance and air stability of the product.
[0112] It can be seen from the sodium ion batteries prepared from the sodium iron sulfate positive electrode materials of Examples 19 and 20 and Example 1 that when the volume proportion of the polar solvent used is too small, the specific capacity of the positive electrode material and the positive electrode material after being shelved for 12 months are both reduced, and the specific capacity decreases more seriously after shelving, indicating that a too small volume of the polar solvent is not conducive to the air stability of the positive electrode material; after the volume proportion reaches a certain value, it has little effect on the electrochemical performance and air stability.
[0113] The sodium-ion batteries prepared from the sodium iron sulfate cathode materials of Examples 21-40 and Example 1 demonstrate that amphiphiles with different HLB values have little effect on the electrochemical performance of the cathode materials, but a more significant impact on their air stability. When amphiphiles with HLB values between 13 and 15 were used (corresponding to Examples 21-29), the cathode materials exhibited higher first-cycle specific capacity, median voltage, and capacity retention after 12 hours of storage, indicating superior air stability.
[0114] The sodium-ion batteries prepared using the sodium iron sulfate cathode materials of Examples 41-45 and Example 1 demonstrate that the amount of amphiphilic molecules used affects the product's air stability. When the amount of amphiphilic molecules is too low (Examples 41 and 42), the electrochemical performance of the cathode materials deteriorates after 12 months of storage, indicating insufficient air stability. When the amount of amphiphilic molecules is sufficient (Examples 1, 43-45), the samples exhibit excellent air stability. A preferred amount of amphiphilic molecules is 100 / 6 grams per mole of sodium sulfate.
[0115] From the sodium ferric sulfate positive electrode materials of Examples 46 to 53 and Example 1, it can be seen that the amount of sodium sulfate, ferrous sulfate hydrate, and ferrous sulfate hydrate has little effect on the electrochemical performance and air stability of the product.
[0116] It can be seen from the sodium ion batteries prepared from the sodium iron sulfate positive electrode materials of Examples 54 to 57 and Example 1 that when the heating temperature and holding time in the first stage are insufficient, the electrochemical performance and air stability of the samples are poor; preferably, the first stage heating temperature is 80°C and the holding time is 2 hours.
[0117] It can be seen from the sodium ion batteries prepared from the sodium iron sulfate positive electrode materials of Examples 58 to 61 and Example 1 that when the second-stage heating temperature and holding time are insufficient, the electrochemical performance and air stability of the samples are poor; preferably, the second-stage heating temperature is 180°C and the holding time is 4 hours.
[0118] It can be seen from the sodium ion batteries prepared from the sodium ferric sulfate positive electrode materials of Examples 62 to 65 and Example 1 that the addition of mixed polar solvents, mixed non-polar solvents, mixed amphiphilic molecules and mixed ferrous sulfate hydrates has little effect on the electrochemical properties and air stability of the products.
[0119] It can be seen from the sodium ion batteries prepared from the sodium iron sulfate positive electrode materials of Examples 66 to 67 and Example 1 that the time of the first heating stage cannot be too short and the heating temperature of the second stage cannot be too low, otherwise the electrochemical performance and air stability of the sample will be poor.
[0120] Comparison of Examples 2 to 67 with Comparative Examples 1 to 7 yields the following conclusions:
[0121] The comparison results of Examples 2 to 67 with Comparative Example 1 show that when amphiphilic molecules are not used, the electrochemical performance of the initial samples is comparable, but the electrochemical performance of the samples significantly declines after 12 months of storage, indicating that amphiphilic molecules play a good protective role in the air stability of the samples.
[0122] The comparison results of Examples 2 to 67 and Comparative Examples 2 to 3 show that when no polar solvent or non-polar solvent is added, the electrochemical performance of the initial battery is equivalent, but the electrochemical performance of the samples after 12 months of storage significantly declines, and the capacity retention rate of Comparative Examples 2 to 3 is slightly better than that of Comparative Example 1; it is speculated that the possible reason is that the effective combination of polar solvents and non-polar solvents can promote the formation of a uniform protective layer of amphiphilic molecules on the surface of the sodium ferric sulfate sample with the hydrophilic end of the amphiphilic molecules facing the sodium ferric sulfate and the hydrophobic end of the amphiphilic molecules facing away from the sodium ferric sulfate.
[0123] The comparison results of Examples 2 to 67 and Comparative Example 4 show that the low-temperature heating and heat preservation in the first stage can improve the air stability of the sample; it is speculated that the possible reason is that the low-temperature heating and heat preservation in the first stage can promote the uniformity of the system, thereby providing favorable conditions for high-temperature coating.
[0124] Comparison of Examples 2-67 with Comparative Example 5 shows that the high-temperature heating and insulation in the second stage significantly impacts the electrochemical performance of the initial samples. This is because the second stage is the stage for generating the sodium ferric sulfate sample. The cathode material used in Comparative Example 5 was not subjected to high-temperature heating and insulation, so no sodium ferric sulfate cathode was formed. Therefore, the specific capacity obtained in the test is largely due to physical adsorption.
[0125] The comparison results of Examples 2 to 67 with Comparative Examples 6 and 7 show that when the HLB value of the amphiphilic molecules used is outside the range of 10 to 16, the electrochemical performance of the initial samples is comparable, but the electrochemical performance of the samples significantly deteriorates after 12 months of storage, indicating that the HLB value of the amphiphilic molecules has a certain influence on the protective effect; it is speculated that the possible reason is that amphiphilic molecules with too high or too low HLB values are difficult to form an effective protective layer on the sodium ferric sulfate positive electrode.
[0126] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the scope of knowledge possessed by ordinary technicians in the relevant technical field without departing from the scope of the present invention.
Claims
1. A sodium iron sulfate positive electrode material, characterized in that: The positive electrode material comprises sodium ferric sulfate and amphiphilic molecules modifying the sodium ferric sulfate, wherein the hydrophilic ends of the amphiphilic molecules face the sodium ferric sulfate and the hydrophobic ends of the amphiphilic molecules face away from the sodium ferric sulfate; and the HLB of the amphiphilic molecules is 10-16.
2. The sodium iron sulfate positive electrode material according to claim 1, characterized in that The amphiphilic molecules include polyoxypropylene lanolin ether, polyoxyethylene sorbitan monooleate, polyoxyethylene cetyl ether, polyoxyethylene sorbitan tristearate, polyoxyethylene lauryl ether, polyoxyethylene sorbitan trioleate, polyoxyethylene oxypropylene oleate, polyoxyethylene lanolin derivatives, polyoxyethylene monooleate, polyoxyethylene monooleate, polyoxyethylene monopalmitate, polyoxyethylene monostearate, polyoxyethylene oleyl ether, polyoxyethylene monolaurate, polyoxyethylene alkylphenol, polyoxyethylene acetylated lanolin derivatives, polyoxyethylene sorbitan lanolin derivatives, polyoxyethylene alkylaryl ethers, polyoxyethylene monolaurate, polyoxyethylene laurate At least one of ether, polyoxyethylene castor oil, polyoxyethylene vegetable oil, cholesterol ether, lanolin alcohol ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monostearate, polyoxyethylene oleyl alcohol ether, polyoxyethylene methyl glucoside sesquioleate, polyoxyethylene lanolin alcohol ether, polyoxyethylene sorbitan monooleate, polyoxyethylene monostearate, polyoxyethylene monooleate, polyoxyethylene oleyl ether, polyoxyethylene octadecyl alcohol, polyoxyethylene oleyl alcohol, polyoxyethylene fatty alcohol, polyethylene glycol monopalmitate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene cetyl alcohol, polyoxyethylene oxypropylene stearate and polyoxyethylene monostearate.
3. A method for preparing the sodium iron sulfate positive electrode material as claimed in claim 1 or 2, characterized in that: include: The raw material for preparing the sodium ferric sulfate, the amphiphilic molecule, the non-polar solvent and the polar solvent are mixed, heated and then impurities are removed; The mixed heating includes a first heating and a second heating performed sequentially; The temperature of the first heating is 50 to 100° C.; the time of the first heating is 1 to 12 hours; The temperature of the second heating is 120-250° C.; the time of the second heating is 1-12 hours.
4. The preparation method according to claim 3, characterized in that: The temperature of the first heating is 70-90° C.; the time of the first heating is 1-3 hours; preferably, the temperature of the second heating is 170-190° C.; the time of the second heating is 3-5 hours.
5. The preparation method according to claim 3, characterized in that: The non-polar solvent includes at least one of benzene, carbon tetrachloride, hexane, isooctane, dichloromethane, cyclohexane, petroleum ether and pentane.
6. The preparation method according to claim 3, characterized in that: The polar solvent includes at least one of water, formamide, acetone, trifluoroacetic acid, ethanol, chloroform, ether, acetic acid, acetonitrile, isopropanol, methanol, dimethyl sulfoxide, acetonitrile, N,N-dimethylformamide, hexamethylphosphoramide, pyridine, tetramethylethylenediamine, triethylamine, n-butanol, dioxane, tetrahydrofuran and methyl formate.
7. The preparation method according to claim 3, characterized in that: The raw materials for preparing the sodium ferric sulfate include sodium sulfate and ferrous sulfate hydrate.
8. The preparation method according to claim 7, characterized in that: The ratio of the polar solvent, the non-polar solvent, the amphiphilic molecule, the sodium sulfate and the ferrous sulfate hydrate is 1-20: 1-20: 10-500: 5-6.75: 10-13.5, wherein the polar solvent and the non-polar solvent are calculated by volume liter, the amphiphilic molecule is calculated by mass gram, and the sodium sulfate and the ferrous sulfate hydrate are calculated by molar amount of substance.
9. Use of the positive electrode material as claimed in claim 1 or 2 in the preparation of sodium ion batteries.
10. Use of the sodium ion battery according to claim 9 in the field of secondary batteries.
Citation Information
Patent Citations
High-density sodium ion battery positive electrode material and preparation method thereof
CN110224136A
Hydrophobic and oleophylic Na2Fe2 (SO4) 3 / C positive electrode material and preparation method thereof
CN115050934A
Method, preparation method and application of fatty acid modified sodium battery positive electrode material
CN115832304A
Hydrophobic polymer coated modified sodium battery positive electrode material, preparation method and battery
CN115954447A
Sodium ferric sulfate positive electrode material and preparation method and application thereof
CN116344824A
Cited By
Method for preparing multi-element uniformly-doped sodium ferric sulfate porous sodium battery positive electrode material by using mixed alcohol precipitation method
CN119503889A
High-performance sodium ferric sulfate polyanion positive electrode material and preparation method thereof
CN119864415A