Drug coating and medical device comprising same, system, and preparation method

By using non-degradable polymers and gradient drug-loading design in the coating of drug-eluting stent, the problem of unstable drug release is solved, long-term stable drug release in peripheral arteries is achieved, and the treatment of peripheral arterial diseases is satisfied. need.

WO2024222834A1PCT designated stage expired Publication Date: 2024-10-31BEIJING SALUBRIS MEDTECH CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/089941
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-25
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

It is difficult for existing drug-eluting stents to achieve stable and sustained drug release during long-term use, especially in large-diameter blood vessels such as peripheral arteries, resulting in too rapid initial drug release or insufficient late-stage drug release, making it ineffective in treating peripheral arterial diseases such as peripheral arterial disease.

Method used

Non-degradable polymers are used as the drug coating matrix, and inner and outer layers with different drug loading concentrations are formed in the coating. The drug loading concentration of the inner layer is greater than that of the outer layer, and the thickness of the outer layer is controlled to not exceed 20 μm to ensure that the drug is Stable release during treatment cycle.

Benefits of technology

It achieves long-term stable drug release for more than 30 days, avoids early excessive drug release, ensures therapeutic effect, and is suitable for long-term treatment in large-diameter blood vessels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024089941_31102024_PF_FP_ABST
    Figure CN2024089941_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a drug coating and a medical device comprising the drug coating, a system, and a preparation method. The drug coating comprises a non-degradable fluorinated polymer matrix and a drug dispersed therein. An inner layer and an outer layer which have different drug-loading concentrations are formed along the thickness direction of the drug coating, the inner layer has a drug-loading concentration not less than 10 wt%, the outer layer has a drug-loading concentration less than 10 wt%, and the thickness of the outer layer is not greater than 20 μm. The drug coating of the present invention can allow for the release of a long-term stable amount of a drug into a tissue wall in contact with the drug coating, so as to achieve a long-term therapeutic or preventive effect on diseases such as luminal stenosis.
Need to check novelty before this filing date? Find Prior Art

Description

Drug coating and medical device, system and preparation method containing the same Technical Field

[0001] The present invention relates to the technical field of medical devices, in particular to drug-carrying devices and coatings for achieving long-term drug release, and particularly to implantable medical devices for intracavitary delivery, such as drug-eluting stents, and related preparation methods. Background Art

[0002] A drug-eluting stent (DES) consists of three components: a metal skeleton, a polymer coating, and the anti-restenosis drug carried on it. Since its introduction, the polymer coating has been a crucial component of DES, acting as a drug carrier, controlling drug release, and preventing intra-stent thrombosis and restenosis.

[0003] DES are currently classified into two main categories: permanent polymers or biodegradable polymers.

[0004] Biodegradable polymers mainly use materials such as polylactic acid. After DES implantation, they degrade into carbon dioxide and water in human tissue and blood environment. The coating degrades and gradually becomes thinner and eventually disappears as the drug is released. The release kinetics curve of the drug in the body is generally considered to be affected by the degradation characteristics of the biodegradable polymer and the drug loading concentration.

[0005] Permanent polymers, primarily fluorinated polymers, are non-degradable in the human body and exhibit excellent biocompatibility. Drug release is generally considered to be primarily determined by the coating's drug concentration. Fluorinated polymer coatings are widely used for applications requiring short-term drug release (typically less than 30 days), such as coronary DES. However, their application in permanent polymer DES with long-term drug release requirements (e.g., greater than 30 days) is less studied and reported. Compared to biodegradable polymer coatings, which can extend effective drug release by tailoring the biodegradable polymer's degradation properties and drug loading, designing fluorinated polymer coatings for long-term effective drug release is more challenging. Directly increasing the coating's drug loading to extend drug release is generally not considered feasible because it results in excessively high and rapid initial drug release, leading to drug waste or significant drug toxicity. Furthermore, during the middle and later stages of drug release, the amount of drug retained in the coating decreases, or the drug loading concentration decreases, resulting in lower drug release and a lower release rate. This is insufficient to achieve the required effective dose within the desired therapeutic period, preventing effective long-term drug release.

[0006] A prime example of the demand for long-term release DES is the treatment of peripheral arterial disease (PAD). PAD is a chronic systemic disease primarily caused by conditions such as atherosclerosis and Takayasu arteritis. PAD often manifests as stenosis and reduced blood flow in the lower and / or upper extremity arteries, posing a significant threat to human health. DES, due to its excellent biocompatibility and ability to carry drugs, is expected to have broad application prospects in the treatment of peripheral arterial occlusive disease.

[0007] However, what is more challenging is that compared with other blood vessels such as coronary arteries, the peripheral arteries of the lower limbs are longer, have larger diameters, and have stronger blood flow impact. For example, the diameter of the subepicardial coronary artery is generally 0.5-5 mm, and the blood flow velocity is 10-30 cm / s, while the diameter of the femoral artery is generally 6-9 mm, and the blood flow velocity is 70-90 cm / s. In order to achieve long-term and stable treatment effects on lower limb PAD, DES needs to carry a larger amount of drug, which exacerbates the initial large-scale release of drugs in a short period of time (burst release), and in the medium- and long-term release cycle of more than 30 days, more stringent requirements are placed on the uniformity of the drug coating and a larger drug release rate. Otherwise, it may be difficult to achieve long-term effective therapeutic drug release.

[0008] Summary of the Invention

[0009] One of the objectives of the present invention is to provide a medical device containing a drug coating, which utilizes the drug coating to release drugs to the tissue wall in contact with the device to achieve a therapeutic or preventive effect.

[0010] The drug coating includes a non-degradable polymer as a coating matrix and a drug carrier. The drug can be dispersed in the coating matrix and released outside the coating during the treatment cycle, while the coating matrix is ​​basically retained.

[0011] The present invention particularly provides a drug coating or a medical device having such a drug coating. The drug coating comprises a non-degradable polymer matrix and a drug dispersed therein. The coating comprises an outer layer and an inner layer having different drug loading concentrations along the thickness of the coating, wherein the inner layer has a higher drug loading concentration than the outer layer. The outer layer has a relatively small thickness, for example, no greater than 20 microns. In a preferred embodiment, the inner layer is thicker than the outer layer. The drug coating can be applied to the surface of the body of the medical device.

[0012] One of the purposes of the present invention is to provide a method for preparing the aforementioned medical device containing a drug coating, comprising: first coating the main body of the medical device with a first coating composition to form an inner layer of the drug coating, and then coating the inner layer with a second coating composition to form an outer layer of the drug coating, wherein the drug loading concentration of the inner layer is greater than the drug loading concentration of the outer layer.

[0013] It should be understood that the inner layer and outer layer referred to in the present invention are continuous along the thickness direction of the coating, without any visible separation, gap or interlayer between the two, and the inner layer is closer to the body than the outer layer. Typically, the inner layer and the outer layer are composed of the same non-degradable polymer matrix.

[0014] As previously mentioned, during the coating preparation process, the inner layer may be prepared first, and the outer layer may be prepared on the surface of the inner layer. In certain embodiments, the inner layer is formed by coating a first coating composition in liquid form and then drying it, and then coating the outer surface of the inner layer with a second coating composition in liquid form and then drying it to form the outer layer. Furthermore, the weight of the drug in the first coating composition is greater than the weight of the drug in the second coating composition.

[0015] The coating method can be any method known in the art, including but not limited to spray coating and dipping.

[0016] During the coating preparation process, a base coat can be applied to the device body surface before the inner coat is applied. Specifically, a base coat solution is prepared by mixing and dissolving a base coat film-forming substance and a solvent. This base coat solution is then applied to the body surface to form the base coat of the drug coating. This improves adhesion between the drug coating and the body, or prevents the drug in the drug coating from migrating to the device body surface. In one embodiment, the base coat film-forming substance can be poly(n-butyl acrylate), and the solvent can be tetrahydrofuran.

[0017] On another level, the present invention also provides a drug-eluting stent with a diameter greater than 5 mm, particularly a drug-eluting stent suitable for peripheral arteries, which can provide uses such as preventing or treating stenosis and restenosis in large-diameter blood vessels, treating inflammation, etc., and in particular, providing long-term and stable drug release for more than 30 days.

[0018] As mentioned above, after a blood vessel with a large diameter lumen, such as a peripheral artery, is expanded by a drug-eluting stent at a narrowed site to expand the blood flow channel, the drug-eluting stent will be in a long-term impact environment of a large flow of blood. The present invention provides the aforementioned drug-eluting stent, which can withstand the long-term impact of a large flow of blood, avoid the early excessive release of drugs from the drug coating, and has the ability to release drugs continuously and stably in multiple smaller cycles within a longer treatment cycle (e.g., more than 30 days, or even about 1 year), so as to achieve long-term treatment or prevention effects.

[0019] In certain embodiments, the drug coating of the drug eluting stent has a drug loading capacity of not less than 100 μg / cm 2 , for example 110 μg / cm 2 , 120μg / cm 2 , or 130 μg / cm 2 , or 140 μg / cm 2 In certain embodiments, the drug coating of the drug eluting stent has a drug loading amount of not less than 150 μg / cm 2 , for example 160 μg / cm 2 , or 180 μg / cm 2 , or 200 μg / cm 2 In certain embodiments, the drug coating of the drug eluting stent has a drug loading amount of not less than 200 μg / cm 2 , for example 210 μg / cm 2 , or 230 μg / cm 2 , or 250 μg / cm 2 , or 260 μg / cm 2 , or 280 μg / cm 2 In certain embodiments, the drug coating of the drug eluting stent has a drug loading amount of not less than 300 μg / cm 2 , for example 310 μg / cm 2 , or 330 μg / cm 2 , or 350 μg / cm 2 , or 380 μg / cm 2 or 400 μg / cm 2 In certain embodiments, the drug coating of the drug eluting stent has a drug loading amount of not less than 400 μg / cm 2 , for example 410 μg / cm 2 , or 450 μg / cm 2 , or 480 μg / cm 2 , or 500 μg / cm 2 .

[0020] In certain embodiments, the drug coating thickness of the drug eluting stent does not exceed 50 μm, and preferably, the drug coating thickness does not exceed 30 μm, for example, 30 μm, 25 μm, 20 μm, 15 μm or 12 μm.

[0021] Although those skilled in the art understand that regulating the drug concentration, coating thickness, and / or drug loading of a drug-loaded coating is a common practice for controlling drug release, they have not clearly anticipated that this common practice could yield a drug coating that could be clinically used for long-term drug release. The inventors surprisingly discovered that, by controlling the thickness and / or drug loading concentration of the inner and outer layers of the drug coating of the present invention under specific conditions, it is possible to achieve long-term, controlled drug release from a non-degradable polymer drug-loaded coating, particularly safe and therapeutically effective drug release for clinically longer than or far exceeding 30 days, such as for the treatment of periarthritis (PAD).

[0022] With respect to the drug coating of the present invention, the drug loading concentration of the inner layer is greater than that of the outer layer. At the same time, the thickness of the outer layer should not be too large, for example, not more than 20 μm, but generally not more than 10 μm. Particularly preferably, the thickness of the outer layer is not more than 8 μm, for example, 6 μm, 5 μm, 4 μm, 3 μm, 2 μm, 1 μm.

[0023] Preferably, the thickness of the outer layer is 1 μm to 8 μm, particularly 1 μm to 3 μm, or 2 μm to 4 μm.

[0024] Based on the aforementioned drug coating, it is possible to achieve a significant reduction in the initial drug release under high drug loading conditions or avoid large-scale and concentrated drug release within a short period of time (e.g., 24 hours, 48 ​​hours, or 7 days). This avoids the potential waste of drugs or dose toxicity to tissues caused by excessive initial drug release, and maintains a basically stable drug release over a longer release period, in order to achieve long-term therapeutic effects.

[0025] The present invention also provides a drug coating, in certain embodiments of which the drug coating is configured to release no more than 30% of the drug in the first 24 hours, 48 ​​hours, or 7 days after implantation into a mammalian blood vessel, and to release no less than 15% of the drug in the first 30 days.

[0026] The mammals may be humans, pigs, sheep, rabbits, etc.

[0027] The drug coating with the aforementioned drug release characteristics may be configured with any of the aforementioned selected settings of drug loading concentration and thickness of the inner and outer layers.

[0028] The inventors believe that the low drug loading and thin thickness of the outer layer may be the main reason for the aforementioned effects. The inventors speculate that during the initial release phase of the drug coating, on the one hand, the low drug loading concentration of the outer layer directly affects the drug release rate of the drug coating during the initial release phase. On the other hand, the non-degradable polymer matrix of the outer layer acts as a shield or barrier, delaying the release of the drug from the higher drug loading concentration inner layer out of the coating. However, after the initial release phase of the drug coating, the outer layer, which may have already released most of the original drug, unexpectedly does not behave like the unloaded non-degradable polymer matrix layer, which almost completely blocks the release of the drug from the inner layer out of the drug coating. At this time, the outer layer of the present invention acts like a control valve, allowing the drug from the inner layer to migrate or diffuse out of the drug coating through the outer layer at a steady rate, achieving a steady release of the drug from the drug coating to the external environment (e.g., tissue wall) over a long period of time. In certain embodiments, the drug release curve over this long period can be substantially linear.

[0029] Despite this speculation, those skilled in the art will appreciate that the controlled release mechanism of a coating is often complex, affected by multiple factors such as the swelling and dissolution of the coating matrix material in the tissue or blood environment, and the solubility, lipophilicity, or hydrophilicity of the drug.

[0030] In a preferred embodiment of the present invention, the thickness of the inner layer should be greater than that of the outer layer, and the thickness of the inner layer is generally not less than 10 μm. For example, the thickness can be selected from 10 μm to 22 μm. In certain embodiments, the thickness of the inner layer is selected from the range of 12 μm to 16 μm.

[0031] For example, the thickness of the outer layer can be selected to be 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, while the thickness of the inner layer can be selected to be 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm.

[0032] The thickness of the inner layer is selected to be greater than that of the outer layer, which is conducive to obtaining a drug loading concentration in the inner layer greater than that in the outer layer.

[0033] The drug loading concentration referred to in the present invention is expressed as a percentage by weight, and the drug loading concentration can be calculated as follows:

[0034] Drug loading concentration of the inner layer = the mass of the drug contained in the inner layer / (the sum of the mass of the non-degradable polymer in the inner layer and the mass of the drug contained in the inner layer) × 100%;

[0035] Drug loading concentration of the outer layer = mass of the drug contained in the outer layer / (sum of the mass of the non-degradable polymer in the outer layer and the mass of the drug contained in the outer layer)×100%.

[0036] In the embodiment of the present invention, the inner layer and the outer layer of the drug coating are generally loaded with a total drug load of no less than the total therapeutic amount required by the medical device. For treatment lumens with large diameters and lengths, the total drug loading of the drug coating can be greater than 100 μg / cm 2 For example, the total drug loading can be 110 μg / cm 2 ~400 μg / cm 2 The drug loading of the inner layer and the outer layer is usually different. Since the drug loading concentration of the inner layer is greater than that of the outer layer, or the thickness of the inner layer is greater than that of the outer layer, the drug loading of the inner layer is usually significantly greater than that of the outer layer. For example, the drug loading of the inner layer is 100 μg / cm 2 ~400 μg / cm 2 The drug loading of the outer layer is 2 μg / cm 2 ~60μg / cm 2 Alternatively, the drug loading of the inner layer is 150 μg / cm 2 ~350μg / cm 2 The drug loading of the outer layer is 2 μg / cm 2 ~30 μg / cm 2 .

[0037] In some preferred embodiments of the present invention, the inner layer has a drug loading concentration of not less than 10 wt % by weight, and the outer layer has a drug loading concentration of less than 10 wt % by weight. The outer layer may be selected to have a thickness of not more than 10 μm.

[0038] For example, in certain embodiments, the drug loading concentration of the inner layer may be 10 wt % to 45 wt %, and the drug loading concentration of the outer layer may be 1 wt % to 8 wt %.

[0039] In certain embodiments, the drug loading concentration of the inner layer is 10 wt % to 30 wt %, and the drug loading concentration of the outer layer is 3 wt % to 5 wt %.

[0040] In certain embodiments, the drug loading concentration of the inner layer is 10 wt % to 20 wt %, and the drug loading concentration of the outer layer is 3 wt % to 5 wt %.

[0041] In certain embodiments, the drug loading concentration of the inner layer is 10 wt% to 20 wt%, and the drug loading concentration of the outer layer is 3 wt% to 4 wt%;

[0042] In certain embodiments, the drug loading concentration of the inner layer is 20 wt% to 30 wt%, and the drug loading concentration of the outer layer is 4 wt% to 5 wt%;

[0043] In certain embodiments, the drug loading concentration of the inner layer is 15 wt % to 25 wt %, and the drug loading concentration of the outer layer is 3 wt % to 5 wt %.

[0044] In certain embodiments, the drug loading concentration of the inner layer is 10 wt%, 13 wt%, 15 wt%, 18 wt% or 20 wt%, and the drug loading concentration of the outer layer is 3 wt%, 4 wt% or 5 wt%.

[0045] Another object of the present invention is to provide a drug coating having a specific drug release profile or a medical device containing the drug coating and a treatment method, wherein the release profile of the drug coating satisfies the requirement that the drug release rate within the first 24 hours after implantation into a mammalian blood vessel is no greater than 40%, and the drug release rate within the first 30 days is no less than 15%.

[0046] In certain embodiments, the drug release rate of the drug coating in the first 30 days after implantation into a mammalian blood vessel is no less than 15%, and no more than 60%, or no more than 50%, or no more than 40%. Preferably, the drug release rate is no more than 40%.

[0047] In certain embodiments, the drug release rate of the drug coating in the first 14 days after implantation into a mammalian blood vessel is no less than 15%, and no more than 30%, or no more than 40%, or no more than 50%. Preferably, the drug release rate is no more than 30%.

[0048] In certain embodiments, the weekly drug release rate of the drug coating from the second week to the seventeenth week after implantation into a blood vessel of a mammal is about 6% to 2%.

[0049] In certain embodiments, the drug coating releases no less than 30%, or no less than 40%, or no less than 50% of the drug within the 31st to 360th day after implantation into a mammalian blood vessel. Preferably, the drug release rate is no less than 50%.

[0050] In certain embodiments, the drug release rate of the drug coating in the first 24 hours after implantation in a mammalian blood vessel is no greater than 15%, or no greater than 20%, or no greater than 30%. Preferably, the drug release rate in the first 24 hours is no greater than 15%.

[0051] The non-degradable polymers referred to in the present invention are biocompatible and chemically and physically stable, and suitable for contact with human or animal tissue walls, such as blood vessels. Preferred non-degradable polymers are fluorinated polymers. Those skilled in the art will understand that fluorinated polymers are polymers with a C—C chain as the backbone, and one or more fluorine atoms, or even all fluorine atoms, attached to the side chains or branches.

[0052] Fluorinated polymers can be selected from fluorinated copolymers, and the comonomers can be, for example, tetrafluoroethylene (TFE), hexafluoropropylene, chlorotrifluoroethylene and perfluoroalkyl vinyl ether (PFVE), among which PFVE includes perfluoromethyl vinyl ether (methyl ether), perfluoropropyl vinyl ether (propyl ether) and perfluorodioxole.

[0053] Fluorinated polymers may also preferably be fluorinated acrylic polymers, for example, comonomers may be perfluoroalkyl (meth)acrylates, heteroatom-containing perfluoroalkyl (meth)acrylates, perfluoroamide (meth)acrylates, and perfluorosulfonamide (meth)acrylates.

[0054] The fluorinated copolymer used in the present invention as a film-forming polymer should have a molecular weight high enough to provide sufficient toughness so that the film containing such polymer will not be rubbed off during the stent processing or installation process, or the coating will not show obvious cracking when the stent or other medical devices such as occluders and vena cava filters expand.

[0055] In a preferred embodiment, the fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene (PVDF-HFP), comprising 50%-92% vinylidene fluoride and 50%-8% hexafluoropropylene by weight. This polymer has been reported and used, for example, in Chinese invention patent publication number CN1225292C, the entire text of which is incorporated herein by reference. This Chinese invention patent discloses the preparation method and performance testing of the aforementioned fluoropolymer coating.

[0056] In certain embodiments, the non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer comprises 55%-65% of vinylidene fluoride and 45%-35% of hexafluoropropylene by weight.

[0057] In certain embodiments, the non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer comprises 70%-90% of vinylidene fluoride and 30%-10% of hexafluoropropylene by weight.

[0058] In certain embodiments, the drug coating further includes a non-drug-carrying bottom layer, which is located below the inner layer and covers the medical device body, and is used to allow the drug coating to adhere to the medical device body. In this case, the inner layer is not directly attached to the surface of the medical device body.

[0059] The bottom layer can be made of one or more of polymethacrylonitrile, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polyhydroxyethyl methacrylate, and polyhydroxypropyl methacrylate. The bottom layer also has good toughness so that the coating will not crack.

[0060] Another object of the present invention is to provide an implantable medical system for interventional procedures, comprising the aforementioned medical device and a delivery device detachable from the medical device, wherein the body of the medical device, or at least a portion thereof, is expandable and adapted to be compressed to a smaller diameter for delivery via a catheter. The aforementioned drug coating may be disposed on the surface of the expandable portion of the medical device. Thus, the drug coating preferably has excellent elongation, and satisfies the requirement that the drug coating remains substantially intact and free of rupture when the medical device deforms from a compressed state to an unconstrained state.

[0061] In certain embodiments, the medical device may be a drug eluting stent, and the stent may be crushed to 50% of its unconstrained diameter without substantial disruption of the drug coating.

[0062] In certain embodiments, the medical device may be a drug eluting stent that can be crushed to 30% of its unconstrained diameter without substantial disruption of the drug coating.

[0063] In certain embodiments, the medical device may be a drug eluting stent that can be crushed to 20% of its unconstrained diameter without substantial disruption of the drug coating.

[0064] Drug-eluting stents typically have a body made of a metal material, such as stainless steel, nickel-titanium alloy, or cobalt-chromium alloy, with a drug coating disposed on the alloy surface of the body.

[0065] Based on some embodiments of the present invention, it can be expected that the provided drug coating has the function of meeting the requirements of long-term stable drug release. In particular, some embodiments provide long-term and stable drug release for more than 30 days, 60 days, 180 days or 360 days. The drug release amount during the release period can be always controlled above the minimum effective dose to ensure or improve the medical effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] FIG1 is a schematic structural diagram of a drug-eluting stent according to an embodiment of the present invention;

[0067] FIG2 is a schematic cross-sectional view of a slender rod portion of a drug-eluting stent according to an embodiment of the present invention;

[0068] FIG3 shows the drug release rate results of the drug-eluting stent according to an embodiment of the present invention in animal experiments;

[0069] FIG4 shows the drug release rate results of the drug-eluting stent according to an embodiment of the present invention in animal experiments;

[0070] FIG5 shows the drug release rate results of the drug-eluting stent according to an embodiment of the present invention in an in vitro test;

[0071] FIG6 is a schematic structural diagram of an implantable medical device system for interventional procedures according to an embodiment of the present invention;

[0072] FIG. 7 is a partial enlarged view of FIG. 6 , showing the assembled position of the drug eluting stent in the delivery device. DETAILED DESCRIPTION

[0073] The present invention will be further illustrated by the following examples. However, these examples are merely illustrative and intended to facilitate understanding of the present invention by those skilled in the art, and are not intended to limit the scope of the present invention. Other variations beyond the examples are possible, and it is not necessary to enumerate all embodiments here. It should be understood that any equivalent variations or modifications made in accordance with the spirit and substance of the present invention are encompassed within the scope of the present invention.

[0074] The present invention provides one or more embodiments of drug-eluting stents having a drug coating attached to the surface of the stent. The drug coating may be any of the following or those described above in the specification.

[0075] Drug-eluting stents are primarily used to treat diseases within vascular cavities, such as stenosis, restenosis, and inflammation in peripheral arteries, peripheral veins, cerebral nerve vessels, and arteriovenous fistulas. However, those skilled in the art will appreciate that drug-eluting stents can also be used to treat diseases within body cavities such as the esophagus and intestines.

[0076] Without limitation, the drug coating can also be applied to other medical devices, such as various occluders and filters that can be permanently or temporarily placed in the body through interventional procedures, or medical devices that require long-term contact with tissue walls without interventional procedures. The drug coating is attached to the surface of the device body in order to enable the drug coating to deliver drugs outward.

[0077] The present invention provides some embodiments of drug coatings having long-term controlled-release functional properties, such as a drug release profile that delivers drugs to the tissue wall for 30 days or more, or 60 days or more, or 120 days or more, or 240 days or more, or 360 days or more, while satisfying that the average daily release amount or the average weekly release amount of the drug within the preset release period at least reaches or exceeds the required minimum therapeutic dose.

[0078] In certain embodiments, the minimum therapeutic dose required is 1% to 10% of the total amount of drug loaded in the drug coating. In certain embodiments, the drug release profile satisfies a weekly average release of at least 1% to 10% of the total amount of drug loaded in the drug coating, such as 8%, 6%, or at least 1% to 5%, such as 1%, 2%, 3%, or 4%.

[0079] In certain embodiments, in contrast to the aforementioned average weekly release, the drug release profile satisfies a predetermined release period (e.g., 4 to 52 weeks) in which the designed weekly release of the drug at least reaches or exceeds the required minimum therapeutic dose, which is 1% to 10% of the total drug load of the drug coating. In certain embodiments, the drug release profile satisfies a predetermined release period in which the designed weekly release of the drug at least reaches or exceeds 1% to 6%, e.g., 1%, 2%, 3%, 4%, 5%, or 6%, of the total drug load of the drug coating.

[0080] Compared to the average weekly release, the designed weekly release rate more accurately reflects the characteristics of long-term drug release control, especially when meeting the minimum therapeutic dose requirement. Because the average weekly release rate may not fully reflect or accurately reflect the actual weekly drug release control, the designed weekly release rate refers to the amount of drug required for controlled release each week, from the first to the last week of the predetermined drug release cycle. To ensure long-term therapeutic effects, the designed weekly release rate must at least reach or exceed the minimum therapeutic dose.

[0081] The present invention further provides another embodiment of a drug coating having the functional property of suppressing the short-term burst release of a high-drug-loaded drug coating. For example, the high-drug-loaded coating has a drug release rate of no more than 40% within the first 24 hours of drug delivery to the tissue wall, and a drug release rate of no less than 15% within the first 30 days. Unless otherwise specified, the drug release rate referred to herein, herein, and hereinafter refers to the ratio of the amount of drug released by the drug coating to the total amount of drug loaded in the drug coating.

[0082] In certain embodiments, the high drug loading coating has a drug release rate of no more than 30%, or no more than 20%, or no more than 10% in the first 24 hours of drug delivery to the tissue wall, and at the same time, the drug release rate in the first 30 days is no less than 15%, or no less than 20%, or no less than 30%, or no less than 40%.

[0083] It has been proven that applying a barrier layer to the drug coating is particularly helpful in suppressing the short-term burst release of drugs from the drug coating. The barrier layer can be an additional coating layer that is the same as or different from the drug coating matrix and is usually unloaded with drugs. It can be called a blank barrier layer. However, a blank barrier layer of a non-degradable polymer matrix makes it difficult for the underlying drug coating to release drugs outside the coating, and it may not be possible to maintain the minimum therapeutic dose of drug release over a long period of time during the release cycle. Therefore, one direction for improvement is to select a matrix material that can be rapidly broken and dissolved as a sacrificial barrier layer to block drug release before drug release or in the early stages of the release cycle, and to achieve the removal of the barrier layer during the release cycle, for example, by dissolution, degradation, fluid flushing, etc.

[0084] Different from this, the drug coating of the embodiment of the present invention mainly realizes short-term and long-term drug release control through a double-layer drug-loading layer with gradient concentration, especially for drug coatings with high drug loading.

[0085] Compared with small diameter vessels, the drug-eluting stents used in coronary arteries usually have a drug loading of 10 μg / cm 2 The drug loading amount of the high drug loading drug coating referred to in the present invention is usually not less than 50 μg / cm 2 , especially not less than 100 μg / cm 2 .

[0086] In certain preferred embodiments of the present invention, the aforementioned long-acting controlled release functional characteristics and the functional characteristics of suppressing short-term burst release of high drug loading drug coatings are simultaneously satisfied.

[0087] In certain embodiments, the drug release rate of the drug coating in the first 30 days after implantation into a mammalian blood vessel is no less than 15%, and no more than 60%, or no more than 50%, or no more than 40%.

[0088] In certain embodiments, the drug release rate of the drug coating in the first 14 days after implantation into a blood vessel of a mammal is no less than 15%, and no more than 30%, or no more than 40%, or no more than 50%.

[0089] In certain embodiments, the weekly drug release rate of the drug coating from the second week to the seventeenth week after implantation into a blood vessel of a mammal is about 6% to 2%.

[0090] In certain embodiments, the drug coating releases no less than 30%, or no less than 40%, or no less than 50% of the drug within the 31st to 360th day after implantation into a blood vessel of a mammal.

[0091] In certain embodiments, the drug coating releases no more than 15%, or no more than 20%, or no more than 30% of the drug within the first 24 hours after implantation into a blood vessel of a mammal.

[0092] A notable feature of the drug coating of the present invention is that it provides a relatively thin outer layer and a relatively thick inner layer. Typically, the outer layer has a lower drug loading and / or drug loading concentration, while the inner layer has a higher drug loading and / or drug loading concentration.

[0093] In one embodiment, the thickness of the outer layer is selected from the range of 1 μm to 6 μm, while the thickness of the inner layer having a significant thickness is selected from the range of 10 μm to 18 μm.

[0094] The present invention further provides an embodiment of a drug-eluting stent having the aforementioned drug coating, which is particularly suitable for implantation into a peripheral artery.

[0095] Certain embodiments of drug-eluting stents suitable for peripheral arterial implantation may have a length of 15 mm to 200 mm and a diameter of 3 mm to 12 mm. Certain embodiments of drug-eluting stents may have a length L of 20 mm to 150 mm and a diameter of 5 mm to 10 mm.

[0096] In one embodiment, the drug eluting stent has a length of 20 mm and a diameter of 5 mm. In another embodiment, the drug eluting stent has a length of 150 mm and a diameter of 8 mm. Both can be delivered through a sheath with an outer diameter of 7 French.

[0097] The drug coating may be applied to the entire surface of the stent body, but is not limited thereto. Those skilled in the art may also choose to apply the drug coating to portions of the stent body. For example, certain portions of the stent body may have exposed surfaces that are not coated with the drug coating. The stent body is typically made of metal and has excellent elastic deformation properties to provide good support and grip.

[0098] A significant advantage of the drug-eluting stent implanted in a peripheral artery of the present invention is that it provides a less damaging and more effective treatment effect during the peripheral artery treatment process.

[0099] The drug-eluting stent can be delivered to the diseased site in the blood vessel by a delivery device when it is compressed and gripped to a smaller diameter. The delivery device is operated to release the drug-eluting stent into the blood vessel lumen. The drug-eluting stent can self-expand or be expanded by a balloon, and contact the blood vessel wall and use its radial force to support the expansion of the narrowed blood vessel wall. The drug coating, such as anti-proliferative drugs, can be released to the diseased site to prevent and reduce restenosis of the blood vessel lumen.

[0100] In one embodiment, as shown in Figures 6 and 7, a drug-eluting stent 3 can be assembled into a delivery device. Referring to Figure 7, the drug-eluting stent 3 is sheathed on an inner sheath 4 of the delivery device. An outer sheath 5 is slidably sheathed outside the inner sheath 4 to constrain the drug-eluting stent 3 to the inner sheath 4. The distal end 1 of the inner sheath 4 is a tapered head, and a developing ring 2 is provided near the distal end 1. The proximal end of the inner sheath 4 is connected to a front handle 7. A stress diffusion tube 6 is provided at the distal end of the front handle 7 to enhance the strength of the tube. During operation, the delivery device injects saline through a proximal connector 12 to flush the tube body. The stent is then delivered into the human body through the introduction channel established by the guidewire. When the distal end of the inner sheath 4 reaches the designated lesion location, the operator removes the stopper 10 from the knob 8, grasps the front handle 7, releases the lock between the button 9 and the screw 11, and operates the knob 8 to retract (proximally move) along the screw 11, driving the outer sheath 5 to retract and release the drug-eluting stent 3. Figure 7 shows that the outer sheath 5 slides toward the proximal end to expose the drug-eluting stent 3, freeing the drug-eluting stent 3 from the outer sheath 5. During the release process, the self-expandable stent is no longer constrained by the radial direction of the outer sheath 5 from the distal end to the proximal end, and thus gradually expands, tending to restore its preset shape and supporting the dilation of the narrowed blood vessel lumen within the blood vessel.

[0101] Some drug-eluting stent embodiments have the capability of suppressing the burst release of drugs that occurs in the early stages of stent implantation, which is very advantageous in most cases.

[0102] For example, for drug coatings loaded with rapamycin or its analogs, in the early post-angioplasty period, stent expansion damages endothelial cells, tears and exposure of the vascular lining, a decrease in the endothelial barrier and protective function, vascular stretch, and blood flow impact, leading to platelet adhesion, aggregation, and secretion. At this time, released drugs like rapamycin may have no significant effect. Therefore, excessive drug release is not recommended. For drug coatings loaded with paclitaxel, for the same reasons mentioned above, a large amount of paclitaxel released in a short period of time in the early post-angioplasty period may exhibit severe cytotoxicity, causing additional damage to the vascular wall and other tissues in the systemic circulation.

[0103] Although studies have shown that the incidence of restenosis in peripheral arteries such as the superficial femoral artery is high within one year after dilation, see Osamu et al., "Timing of the restenosis following nitinol stenting in the superficial femoral artery and the factors associated with early and late restenoses," published in the journal Catheterization & Cardiovascular Interventions Official Journal of the Society for Cardiac Angiography & Interventions in 2011, no suitable peripheral arterial drug-eluting stent has been proposed to address this clinical problem.

[0104] Therefore, an object of the present invention is to provide a method for preventing or treating restenosis and a drug-eluting stent used in the method.

[0105] The drug-eluting stent may be any of the examples described above or below, and satisfies the requirement that, in one embodiment, the drug-eluting arterial stent implanted in a stenotic peripheral artery has a drug release period of more than 3 months.

[0106] In another embodiment, a drug-eluting arterial stent implanted in a stenotic peripheral artery has a drug release period exceeding 6 months.

[0107] In a preferred embodiment, a drug-eluting stent implanted in a peripheral arterial stenosis has a drug release cycle of approximately 12 months. This is because, considering that previously reported studies have shown a steep peak in restenosis at approximately 12 months, designing the drug-eluting stent's total drug release cycle to one year effectively reduces the restenosis rate. This allows for a long-term, effective release of the drug that inhibits stenosis, thereby more effectively improving the 12-month patency rate of the lumen. In particular, maintaining the effective release of the drug during the period prior to the 12th month after stent implantation, when the probability of restenosis is higher, may further enhance the prevention or reduction of restenosis. In certain embodiments, the drug released by the drug-eluting stent in the first 7-12 months after implantation is 10% to 40%, for example, approximately 30%, of the total drug coating load.

[0108] The following describes an example of a drug coating using polyvinylidene fluoride copolymer (PVDF-HFP) as the fluorinated polymer matrix, but is not limited thereto, and those skilled in the art may also select other suitable fluorinated polymer matrices.

[0109] Please refer to FIG. 1 , which shows an embodiment of a drug eluting stent 100 having a cylindrical structure formed by a mesh body, and can provide radial support to the lumen of a blood vessel.

[0110] Referring again to FIG. 2 , a drug coating 32 is shown covering the body 1 of a drug-eluting stent 100 or other similar device. The drug coating 32 may substantially circumferentially surround the body 1. The cross-section of the elongated stem portion of the stent body 1 is shown as a quadrilateral. However, in certain embodiments, the cross-section may alternatively be circular, elliptical, or arcuate.

[0111] This is not intended to be limiting, and the drug coating does not necessarily circumferentially surround the stent body 1. In certain embodiments, the drug coating may cover only the outer circumference of the stent body 1, i.e., the surface of the stent body 1 that contacts the tissue wall. In certain embodiments, the outer circumference of the stent body 1 may be provided with grooves, and the drug coating may selectively cover only the grooves or the entire outer circumference of the stent body 1.

[0112] In some embodiments, the outer and inner surfaces of the stent body 1 may be covered with drug coatings of the same or different thicknesses. In some embodiments, the thickness of the drug coating on the outer surface of the stent body 1 is greater than the thickness of the drug coating on the inner surface.

[0113] The stent body 1 can be made of a non-biodegradable material, particularly a metal, such as 316L stainless steel, cobalt-chromium alloy, magnesium alloy, iron alloy, zinc alloy, nickel-titanium alloy, nickel-iron alloy, or other biocompatible metals with good memory properties and support. However, without limitation, the stent body 1 can also be made of a polymer, such as polyamide, polyolefin, or non-absorbable polyester. Without limitation, the stent body 1 can also be made of a biodegradable or bioabsorbable material that is substantially or largely undegraded or absorbed during the drug release cycle, although this option may not be preferred.

[0114] The drug coating matrix of the embodiment of FIG1 selects polyvinylidene fluoride copolymer (PVDF-HFP), which is formed by copolymerization of vinylidene fluoride and hexafluoropropylene. The polymer has excellent biocompatibility, and its stable chemical properties ensure that the drug can be stably released without the risk of producing acidic degradation substances and increasing inflammatory reactions. The drug loaded by the drug coating can be antiproliferative drugs such as rapamycin and its derivatives, paclitaxel, and heparin. In the embodiment of FIG1 , the loaded drug is selected as rapamycin, which has the effect of inhibiting cell proliferation and migration. At the same time, it also has the effect of reducing the production of local vascular wall cytokines and the activation of inflammatory cells, inhibiting cell apoptosis, and promoting the re-endothelialization of vascular injury sites. Restenosis is mainly caused by excessive proliferation of the vascular endothelium after stent implantation. Rapamycin inhibits cell proliferation and migration, thereby inhibiting the occurrence of restenosis.

[0115] The drug coating 32 of the embodiment of FIG2 includes an inner layer 321 formed of a polyvinylidene fluoride copolymer and an outer layer 322 also formed of a polyvinylidene fluoride copolymer. The inner layer 321 and the outer layer 322 are loaded with rapamycin at different concentrations, wherein the drug concentration of the inner layer 321 is greater than that of the outer layer 322. Referring to FIG2 , the thickness of the inner layer 321 is shown to be greater than that of the outer layer 322. The thickness of the outer layer 322 should not be too large, for example, no greater than 20 μm, but generally no greater than 10 μm. In this embodiment, the thickness of the outer layer 322 is between 1 μm and 8 μm. The combined thickness of the inner layer 321 and the outer layer 322 is generally no greater than 50 μm, and preferably no greater than 30 μm.

[0116] In some embodiments, the overall thickness of the inner layer 321 and the outer layer 322 may be selected to be 11 μm to 27 μm.

[0117] For example, the thickness of the inner layer 321 is 10 μm to 22 μm, and the thickness of the outer layer 322 is 1 μm to 5 μm. The thickness of the inner layer 321 may be twice or more the thickness of the outer layer 322. For example, the coating thickness ratio of the inner layer 321 to the outer layer 322 is between approximately 22:1 and 10:1. For another example, the thickness of the inner layer 321 is 12 μm to 16 μm, and the thickness of the outer layer 322 is 1 μm to 3 μm, and the coating thickness ratio of the inner layer 321 to the outer layer 322 is between approximately 16:1 and 12:1. Alternatively, the thickness of the inner layer 321 is 12 μm to 16 μm, and the thickness of the outer layer 322 is 2 μm to 4 μm, and the coating thickness ratio of the inner layer 321 to the outer layer 322 is between approximately 16:2 and 12:2.

[0118] The drug coating 32 of the embodiment of FIG1 also includes a non-drug-loaded bottom layer 33. Although it is not necessary, in some cases, it is preferred to include the bottom layer 33. The inner layer 321 of the drug coating 32 is attached to the surface of the bottom layer 33, and the bottom layer 33 is directly attached to the surface of the stent body 31. Selecting a suitable bottom layer 33 can enhance the adhesion of the drug coating 32 on the stent. The material of the bottom layer 33 can be, for example, a non-biodegradable polymer such as polymethacrylonitrile, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polyhydroxyethyl methacrylate, and polyhydroxypropyl methacrylate, which basically does not produce tissue rejection and tissue inflammation caused by degradation. In this embodiment, polybutyl methacrylate (PBMA) is used as the bottom layer 33. Polybutyl methacrylate has strong adhesion to the metal material of the stent body 31 and has good compatibility with the drug-loaded fluorinated copolymer, so that the contact interface between the inner layer 321 and the bottom layer 33 is mixed, and each can play a "locking" role to form a stable and high-strength coating system on the stent.

[0119] The thickness of the bottom layer 33 should not be too large, and those skilled in the art can select the thickness according to their needs. In this embodiment, the thickness of the bottom layer 33 is 0.5 μm to 1.5 μm, for example, 0.5 μm, 1 μm, or 1.5 μm.

[0120] It can be understood that the drug molecules carried in the inner layer 321 close to the surface of the stent body 31 must migrate a longer distance to be released outside the coating. At the same time, as the drug is released, the drug concentration difference between the drug eluting stent and the blood or tissue gradually decreases, and the release gradually becomes slower.

[0121] Thus, in this embodiment, along the coating thickness direction, the drug concentration in at least a portion of the inner layer 321 is greater than the drug concentration in at least a portion of the outer layer 322, forming a gradient concentration dual-layer drug coating 32. Obviously, in a preferred embodiment, the inner layer 321 and the outer layer 322 each have a relatively uniform drug concentration, while the drug concentration in all regions of the inner layer 321 is greater than the drug concentration in all regions of the outer layer 322. This is particularly beneficial for controlling the release of the entire drug coating 32.

[0122] In this embodiment, the drug loading concentration of the inner layer 321 may be 10wt% to 45wt%, and the drug loading concentration of the outer layer 322 may be 1wt% to 8wt%. Preferably, the drug loading concentration of the inner layer 321 may be 10wt% to 30wt%, and the drug loading concentration of the outer layer 322 may be 3wt% to 5wt%. Alternatively, the drug loading concentration of the inner layer 321 may be 10wt% to 20wt%, and the drug loading concentration of the outer layer 322 may be 3wt% to 5wt%. Alternatively, the drug loading concentration of the inner layer 321 may be 10wt% to 20wt%, and the drug loading concentration of the outer layer 322 may be 3wt% to 4wt%. More preferably, the drug loading concentration of the inner layer 321 may be 10wt%, 13wt%, 15wt%, 18wt%, or 20wt%, and the drug loading concentration of the outer layer 322 may be 3wt%, 4wt%, or 5wt%.

[0123] In one embodiment of the present invention, the drug release rate of the drug-eluting stent 12 months after implantation is greater than or equal to 98%, with little burst release in the initial release and long-term release maintained in the middle and late stages.

[0124] The drug coating 32 of this embodiment is loaded with a sufficient amount of drug, for example, 110 μg / cm 2 ~500μg / cm 2 .

[0125] Obviously, the above-mentioned drug-eluting stent embodiments are not limited to peripheral arteries, but can also be applied to other arteries or veins with fast blood flow or thick blood vessels that require long-term release.

[0126] The following provides an example of preparing the aforementioned drug-eluting stent.

[0127] Example 1

[0128] A method for preparing a drug-eluting stent comprises the following steps:

[0129] 1) Providing a mesh tube-shaped stent body, ultrasonically cleaning and drying it;

[0130] 2) Prepare a non-drug-loaded primer, including:

[0131] The bottom film-forming material and the solvent are mixed and dissolved to obtain a bottom solution. Specifically, the bottom solution is prepared by weighing 0.40 g of polybutyl acrylate, adding it to a 250 ml volumetric flask, adding 60 ml of tetrahydrofuran to the flask, and stirring until it is completely dissolved.

[0132] 3) forming a bottom layer on the stent body, including:

[0133] The base layer solution was loaded into the ultrasonic spraying equipment (ultrasonic atomization spraying system TLS-2000). After the stent body was cleaned and dried, the stent body was placed under ultrasonic spraying until the liquid flowed out of the nozzle. The base layer with a thickness of 0.5 to 1.5 μm was sprayed. After the spraying was completed, it was dried in an oven at 50°C for 2 hours.

[0134] 4) Preparing a drug-loaded coating, specifically including:

[0135] Weigh 4 g of PVDF-HFP (75%-25%) solid, put it into a 50 ml volumetric flask, add methyl ethyl ketone to the volume, stir until completely dissolved to obtain the carrier stock solution, and store it below room temperature.

[0136] Take 5 ml of each of the above carrier stock solutions and put them into a 100 ml volumetric flask, add 16.5 mg and 100 mg of rapamycin solid respectively, make up to volume with methyl ethyl ketone, and stir until completely dissolved. These are used as the coating solutions for preparing the outer and inner layers of the drug coating.

[0137] 5) forming a drug-loaded coating on the bottom layer of the stent, comprising:

[0138] After the base layer is formed, the drug-loaded coating is sprayed onto it to form the inner and outer layers. First, the inner layer is sprayed: 1 mg / mL of the inner layer coating solution is loaded into an ultrasonic spraying device (ULTRASONIC ATOMIZING SPRAY SYSTEM TLS-2000). After the liquid flows from the nozzle, the stent is placed under ultrasonic spraying and sprayed to form an inner layer with a thickness of 12 to 16 μm. After spraying, the stent is dried in a vacuum oven at 40°C for 12 hours.

[0139] Then spray the outer layer: load 0.165 mg / mL of outer layer coating solution into the aforementioned ultrasonic spray equipment until the liquid flows out of the nozzle, place the stent under ultrasonic spraying, spray the stent to form an outer layer with a thickness of 2 to 4 μm. After spraying, dry it in a vacuum oven at 40°C for 12 hours.

[0140] Through the above steps, the drug eluting stent of this embodiment is obtained, wherein the drug loading concentration of the inner layer is 20wt%, the drug loading concentration of the outer layer is 4wt%, and the drug loading capacity of the inner layer is 200μg / cm 2 ~268μg / cm 2 The drug loading of the outer layer is 7 μg / cm 2 ~14 μg / cm 2 The thickness of the inner layer is 12μm~16μm, and the thickness of the outer layer is 2μm~4μm.

[0141] In other embodiments, the drug-eluting stent may not include a bottom layer. After the stent body is cleaned and dried, the inner layer and outer layer solutions are sprayed sequentially to form corresponding inner and outer layers, so that the drug-loaded coating can directly adhere to the surface of the stent body through the inner layer.

[0142] Obviously, the steps of this embodiment are not limited to the above-described exemplary sequence. For example, a bottom layer solution, an inner layer solution, or an outer layer solution may be prepared simultaneously, and then the corresponding solution may be selected and sprayed on the stent body as needed.

[0143] Example 2

[0144] Referring to the preparation method of Example 1, this example prepares a drug-eluting stent with a different drug loading concentration compared to Example 1. The bottom layer in this example is the same as that in Example 1 and will not be described again.

[0145] The coating solution preparation method for the inner layer and outer layer of the drug coating is as follows:

[0146] Weigh 9 g of PVDF-HFP (50%-50%) solid, put it into a 50 ml volumetric flask, add methyl ethyl ketone to make up the volume, stir until completely dissolved to obtain the carrier stock solution, and store it below room temperature.

[0147] Take 1 ml of each of the above-mentioned carrier stock solutions and put them into a 100 ml volumetric flask, add 6 mg and 20 mg of rapamycin solid respectively, make up to volume with methyl ethyl ketone, and stir until completely dissolved. These are used as the coating solutions for preparing the outer and inner layers of the drug coating.

[0148] First, the inner layer was sprayed. A 20 mg / mL inner layer coating solution was loaded into an ultrasonic spraying device (ultrasonic atomization spraying system TLS-2000). After the liquid flowed out of the nozzle, the stent was placed under the ultrasonic spraying. The inner layer with a thickness of 14 to 18 μm was sprayed on the bottom layer. After spraying, the stent was dried in a vacuum oven at 40°C for 12 hours.

[0149] Then spray the outer layer: load 6 mg / mL of outer layer coating solution into the aforementioned ultrasonic spray equipment until the liquid flows out of the nozzle, and place the stent under ultrasonic spraying to form an outer layer with a thickness of 1 to 3 μm. After spraying, dry it in a vacuum oven at 40°C for 12 hours.

[0150] Through the above steps, the drug eluting stent of this embodiment is obtained, wherein the drug loading concentration of the inner layer is 10wt%, the drug loading concentration of the outer layer is 3wt%, and the drug loading capacity of the inner layer is 126μg / cm 2 ~162 μg / cm 2 The drug loading of the outer layer is 3μg / cm 2 ~9μg / cm 2 The inner layer thickness is 14μm~18μm, and the outer layer thickness is 1μm~3μm.

[0151] Example 3

[0152] Referring to the preparation method of Example 1, this example prepares another drug eluting stent having a different drug loading concentration compared with Examples 1 and 2. The bottom layer in this example is the same as that in Example 1 and will not be described again.

[0153] The coating solution preparation method for the inner layer and outer layer of the drug coating is as follows:

[0154] Weigh 5 g of PVDF-HFP (60%-40%) solid, put it into a 50 ml volumetric flask, add methyl ethyl ketone to the volume, stir until completely dissolved to obtain the carrier stock solution, and store it below room temperature.

[0155] Take 1 ml of each of the above-mentioned carrier stock solutions and put them into a 100 ml volumetric flask. Add 5.3 mg and 44 mg of rapamycin solid respectively, make up to volume with methyl ethyl ketone, and stir until dissolution is complete. This is used to prepare the outer layer coating solution with a concentration of 5.3 μg / ml and the inner layer coating solution with a concentration of 440 μg / mL.

[0156] First, the inner layer was sprayed. A 400 μg / mL inner layer coating solution was loaded into an ultrasonic spraying device (ultrasonic atomization spraying system TLS-2000). After the liquid flowed out of the nozzle, the stent was placed under the ultrasonic spraying. The inner layer with a thickness of 10 to 12 μm was sprayed on the bottom layer. After spraying, the stent was dried in a vacuum oven at 40°C for 12 hours.

[0157] Then spray the outer layer: load 21.5μg / mL of outer layer coating solution into the aforementioned ultrasonic spray equipment until the liquid flows out of the nozzle and the stent is placed under ultrasonic spraying to form an outer layer with a thickness of 3 to 5μm. After spraying, dry it in a vacuum oven at 40℃ for 12h.

[0158] Through the above steps, the drug eluting stent of this embodiment is obtained, wherein the drug loading concentration of the inner layer is 30wt%, the drug loading concentration of the outer layer is 5wt%, and the drug loading capacity of the inner layer is 264μg / cm 2 ~316μg / cm 2 The outer layer drug loading is 13μg / cm 2 ~22 μg / cm 2 The thickness of the inner layer is 10μm~12μm, and the thickness of the outer layer is 3μm~5μm.

[0159] Animal test examples

[0160] Using miniature Bama pigs as an animal model, 66 sets of drug-eluting stents from Example 1 were randomly assigned and implanted into 33 miniature pigs, with one drug-eluting stent implanted in each pig's left and right iliac (femoral) arteries. Two stents implanted in three pigs were removed at each of 11 time points after implantation, and the drug residue in the stent drug coating was analyzed by liquid chromatography. The average drug residue in the drug coating at each time point was measured and calculated, and the drug release rate data of the drug-eluting stent from Example 1 at each time point were obtained, as shown in Table 1 below. Based on this, drug release rate curves and release rate curves were plotted, as shown in Figures 3 and 4.

[0161] Using the miniature Bama pig as the animal model, the six drug-eluting stents from Example 2 were randomly implanted in three miniature pigs, with one stent implanted in each pig's left and right iliac (femoral) arteries. Two stents implanted in each pig were removed at three time points after implantation, and the drug residue in the stent drug coating was analyzed by liquid chromatography. The average drug residue in the drug coating at each time point was measured and calculated, yielding the drug release rate data for the drug-eluting stent from Example 2 at each time point, as shown in Table 1 below.

[0162] Similarly, six sets of drug-eluting stents from Example 3 were randomly assigned and implanted in three minipigs, with one set implanted in each pig's left and right iliac (femoral) arteries. Two sets of stents implanted in one pig were removed at three time points after implantation, and the drug residue in the stent drug coating was analyzed by liquid chromatography. The average drug residue in the drug coating at each time point was measured and calculated, yielding the drug release rate data for the drug-eluting stent from Example 3 at each time point, as shown in Table 1 below.

[0163] Table 1: Drug release rate in miniature Bama pigs

[0164] According to the above data and accompanying drawings, it can be seen that the drug release of the drug coating of Example 1 covers the entire restenosis cycle (369 days) and the release rate is as high as over 90%. In the first 1 to 2 months when smooth muscle proliferation is relatively rapid, the drug is released at a relatively fast rate. After about 50 days, the drug release rate enters a relatively plateau region and maintains a stable release rate until the drug is completely released.

[0165] Based on the above data, the drug coatings of these embodiments have the following effects on the development of restenosis:

[0166] (1) Within 1 to 12 hours after angioplasty, platelets adhere, aggregate and secrete due to damage to endothelial cells caused by angioplasty, tearing and exposure of the vascular endothelium, reduction of endothelial barrier and protective function, vascular stretching and blood flow impact. At this time, rapamycin has no significant effect. Therefore, the release amount should not be too large. The drug-eluting stent of the above embodiment controls the release rate to about 10% in the early stage, avoiding sudden release of drugs and ensuring that sufficient drugs are retained for release in the later stage.

[0167] (2) Immediately after surgery, which can last for about 7 days, is also caused by endothelial cell damage. At this stage, rapamycin mainly inhibits inflammation and has not yet exerted an anti-proliferative effect. Therefore, rapamycin has no significant effect at this stage. The drug-eluting stent of the above embodiment controls the release rate to less than 20% at this stage, avoiding premature waste and loss of drugs.

[0168] (3) The peak of smooth muscle proliferation is reached after 7 to 14 days and can last for 1 to 2 months. Within two months, the peak of smooth muscle proliferation causes intimal thickening, leading to restenosis in the later stage. During this stage, the above embodiment releases about 50% of the drug, that is, it reaches the peak stage to release enough drugs to meet the treatment needs while ensuring smooth and stable release during this stage.

[0169] (4) Finally, the blood vessels adapt to the changes in the external environment by self-adjusting to adapt to the changes in hemodynamics and vascular wall structure under different physiological and pathological conditions. In the middle and late stages, for example, at 270 days, the drug can still be continuously released, reaching a release rate of more than 80%, until the maximum release is completed at the time point of the entire release cycle.

[0170] In vitro test examples

[0171] Despite the aforementioned animal studies, accelerated in vitro testing is often used to assess the release characteristics of drug-eluting stent coatings. For accelerated in vitro release testing, the release medium can be a solvent or combination thereof that releases the drug more readily than blood, allowing for a quicker evaluation of different drug coatings.

[0172] Thus, the present invention also provides a method for in vitro drug release testing of a drug-eluting stent, comprising using a buffer solution system containing a trace amount of a water-soluble nonionic surfactant mixed with acetonitrile as a release medium. For example, a buffer solution system containing approximately 0.1% to 1% of a water-soluble nonionic surfactant mixed with approximately 10% of acetonitrile is used as the release medium. The pH of the release medium can be adjusted to approximately 7.4.

[0173] Taking the drug-eluting stent of Example 1 as an example, the steps of performing an in vitro drug release test are as follows:

[0174] 1) Preparation of release medium: Place 20 mL of acetonitrile and 1.8 mL of 70% Triton X-405 in a 200 mL volumetric flask. Dose to volume with PBS solution (38.0 g of sodium dihydrogen phosphate and 5.04 g of sodium dihydrogen phosphate, add water to make up to 1000 mL). Shake well and adjust the pH to 7.4 ± 0.1 with hydrochloric acid or sodium hydroxide to obtain a release medium composed of 0.9% Triton X-405 mixed with 10% acetonitrile.

[0175] 2) Release test: Place the drug-eluting stent to be tested in a release medium maintained in a water bath at 37°C ± 2°C at an oscillation frequency of 60 r / min to simulate drug release. Remove the drug-eluting stent at 5 min, 10 min, 30 min, 60 min, 90 min, 180 min, 240 min, 480 min, 1200 min, and 1440 min, and place it in a dissolution bottle containing acetonitrile. Ultrasonicate in an ice bath for 30 min to completely dissolve the residual rapamycin in the drug-eluting stent in the acetonitrile in the dissolution bottle. After quantification, sample the dissolved drug in the dissolution bottle for detection by chromatography.

[0176] The measured release curve is shown in Figure 5. It can be seen that the release rate has reached more than 90% at the late stage of 1440 minutes and approaches 100% at 1800 minutes.

[0177] Wherein, multiple stents of Example 1 were prepared, and one stent was taken out at each time point for drug dissolution testing.

[0178] Using the same preparation method as above, several other examples of drug-eluting stents with different drug coatings as shown in the following table were prepared.

[0179] Comparative Example

[0180] A comparative drug-eluting stent was prepared using the method of Example 1. The stent included a base layer covering the stent body, a drug-loading layer covering the base layer, and a blank barrier layer covering the drug-loading layer. The base layer was the same as that in Example 1, and the drug-loading layer and the blank barrier layer were made of the same fluorinated polymer as in Example 1.

[0181] In the comparative example, the drug-loaded layer is a coating containing a single concentration of drug, the drug loading concentration is 10wt% to 20wt%, the drug-loaded layer thickness is 12μm to 15μm, the barrier layer is 2μm to 4μm, and the blank barrier layer is a fluorinated polymer coating without drug loading.

[0182] By studying its in vivo or in vitro drug release curve, the results showed that the control group reduced the burst release phenomenon in the early stage of release, but the drug release in the middle and late stages was obviously insufficient, and the release rate over 30 days was far below 15%, making it difficult to achieve a therapeutic effect.

[0183] A comparative drug-eluting stent without a barrier layer was also prepared using the same or similar preparation method. The stent comprises a base layer covering the stent body and a drug-loading layer covering the base layer. No barrier layer or other drug-loading layer is provided on the drug-loading layer. The base layer is the same as in Example 1, and the drug-loading layer comprises the same fluorinated polymer as in Example 1.

[0184] The drug-loading layer parameters were set as shown in the following table to prepare comparative examples 1-4.

[0185] In vitro release comparison experiment

[0186] Taking the drug-eluting stents of Examples 4-8 and Comparative Examples 1-4 as examples, in vitro drug release tests were performed.

[0187] To observe the release of drug-eluting stents over a longer release time, the release medium used in the in vitro drug release test was prepared using the following method: 8 mL of acetonitrile and 0.6 mL of Tween-20 were placed in a 200 mL volumetric flask, made up to volume with PBS solution (38.0 g of sodium dihydrogen phosphate and 5.04 g of sodium dihydrogen phosphate, and water were added to make up to 1000 mL), shaken well, and the pH was adjusted to 7.4 ± 0.1 with hydrochloric acid or sodium hydroxide to obtain a release medium of 0.3% Tween-20 mixed with 4% acetonitrile.

[0188] The drug-eluting stent to be tested was placed in the release medium, maintained in a water bath at 37°C ± 2°C, and oscillated at a frequency of 60 r / min to simulate drug release. The stent was removed at multiple corresponding time points and placed in a dissolution bottle containing acetonitrile. Ice-bath ultrasonication was performed for 30 minutes to completely dissolve the residual rapamycin in the drug-eluting stent in the acetonitrile in the dissolution bottle. After quantification, the amount of dissolved drug in the dissolution bottle was sampled and tested by chromatography. The corresponding drug release results are shown in the following table.

[0189] In each embodiment and comparative example, multiple stents were prepared. In the aforementioned examples, one stent was taken out at each time point to perform drug dissolution testing.

[0190] At intermediate time points, such as 10 hours, the release rate of the present invention can reach 40%, and even Example 4 can reach more than 50%, which is significantly different from Comparative Examples 1 and 2, which can only reach a release rate of about 26% to 29%; and it is significantly different from Comparative Examples 3 and 4, which show a trend of burst release.

[0191] As can be seen from the above table, the drug-carrying layers of Examples 4-8 can release the drug evenly and slowly, achieving long-term sustained release. Compared with Comparative Examples 2 and 3 without a barrier layer, there is no burst release in the initial stage. Compared with Comparative Example 1 with a blank barrier layer, the drug can be released in a stable amount for a long time, and the release rate in the later stage is significantly higher.

[0192] Although the present invention has been disclosed above in terms of preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications to the technical solutions of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solutions of the present invention shall fall within the scope of protection of the technical solutions of the present invention.

Claims

1. A drug coating, characterized in that The drug coating is used to be arranged on a medical device, and the drug coating includes a non-degradable fluorinated polymer matrix and a drug dispersed therein, and an outer layer and an inner layer with different drug loading concentrations are formed along the thickness direction of the drug coating, the drug loading concentration of the inner layer is greater than that of the outer layer, and the thickness of the outer layer is not more than 20 μm.

2. The drug coating according to claim 1, characterized in that: The drug coating is configured to have a drug release rate of no more than 40% in the first 24 hours after implantation in a blood vessel of a mammal, and a drug release rate of no less than 15% in the first 30 days.

3. The drug coating according to claim 1 or 2, characterized in that: The mammal is a human or a pig.

4. The drug coating according to any one of claims 1 to 3, characterized in that The inner layer has a drug loading concentration of not less than 10 wt % by weight, and the outer layer has a drug loading concentration of less than 10 wt % by weight; Alternatively, the drug loading concentration of the inner layer is 10wt% to 45wt%, and the drug loading concentration of the outer layer is 1wt% to 8wt%; Alternatively, the drug loading concentration of the inner layer is 10wt% to 30wt%, and the drug loading concentration of the outer layer is 3wt% to 5wt%; Alternatively, the drug loading concentration of the inner layer is 10wt% to 20wt%, and the drug loading concentration of the outer layer is 3wt% to 5wt%; Alternatively, the drug loading concentration of the inner layer is 10wt% to 20wt%, and the drug loading concentration of the outer layer is 3wt% to 4wt%; Alternatively, the drug loading concentration of the inner layer is 20wt% to 30wt%, and the drug loading concentration of the outer layer is 4wt% to 5wt%; Alternatively, the drug loading concentration of the inner layer is 10wt%, 13wt%, 15wt%, 18wt% or 20wt%, and the drug loading concentration of the outer layer is 3wt%, 4wt% or 5wt%.

5. The drug coating according to any one of claims 1 to 4, characterized in that: The thickness of the outer layer is not less than 1 μm and not more than 10 μm, or the thickness of the outer layer is 1 μm to 8 μm.

6. The drug coating according to any one of claims 1 to 5, characterized in that: The thickness of the inner layer is greater than that of the outer layer, or the thickness of the inner layer is 10 μm to 22 μm.

7. The drug coating according to any one of claims 1 to 6, characterized in that: The thickness of the inner layer is 12 μm to 16 μm, and the thickness of the outer layer is 2 μm to 4 μm.

8. The drug coating according to any one of claims 1 to 7, characterized in that: The total drug loading of the drug coating is 110 μg / cm 2 ~500μg / cm 2 .

9. The drug coating according to any one of claims 1 to 8, characterized in that The drug loading amount of the inner layer is greater than that of the outer layer.

10. The drug coating according to any one of claims 1 to 9, characterized in that: The drug loading of the inner layer is 100 μg / cm 2 ~400 μg / cm 2 The drug loading of the outer layer is 2 μg / cm 2 ~60 μg / cm 2 Alternatively, the drug loading of the inner layer is 150 μg / cm 2 ~350 μg / cm 2 The drug loading of the outer layer is 2 μg / cm 2 ~30 μg / cm 2 .

11. The drug coating according to any one of claims 1 to 10, characterized in that: The drug is selected from paclitaxel, rapamycin, heparin, probucol, dexamethasone, or analogs of the aforementioned drugs.

12. The drug coating according to any one of claims 1 to 11, characterized in that: The drug is selected from lipophilic drugs.

13. The drug coating according to any one of claims 1 to 12, characterized in that: The drug coating is configured to have a drug release rate of not less than 15%, and not more than 60%, or not more than 50%, or not more than 40% in the first 30 days after implantation in a blood vessel of a mammal.

14. The drug coating according to any one of claims 1 to 13, characterized in that: The drug coating is configured to have a drug release rate of not less than 10%, and not more than 30%, or not more than 40%, or not more than 50% in the first 14 days after implantation in a blood vessel of a mammal.

15. The drug coating according to any one of claims 1 to 14, characterized in that The drug coating is configured to have a weekly drug release rate of 6% to 2% from the second week to the seventeenth week after implantation in a mammalian blood vessel; Alternatively, within the 31st day to the 360th day after implantation, the drug release rate is not less than 30%, or not less than 40%, or not less than 50%.

16. The drug coating according to any one of claims 1 to 15, characterized in that The drug coating is configured to release the drug at a rate of no greater than 15%, or no greater than 20%, or no greater than 30% in the first 24 hours after implantation into a blood vessel of a mammal.

17. The drug coating according to any one of claims 1 to 16, characterized in that: The non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer contains 50%-92% of vinylidene fluoride and 50%-8% of hexafluoropropylene by weight.

18. The drug coating according to any one of claims 1 to 17, characterized in that: The non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer contains 55%-65% of vinylidene fluoride and 45%-35% of hexafluoropropylene by weight.

19. The drug coating according to any one of claims 1 to 18, characterized in that: The non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer contains 70%-90% of vinylidene fluoride and 30%-10% of hexafluoropropylene by weight.

20. The drug coating according to any one of claims 1 to 19, characterized in that Also included is a bottom layer that is not loaded with drugs, and the inner layer is attached to the bottom layer.

21. The drug coating according to any one of claims 1 to 20, characterized in that The bottom layer is made of one or more of polymethacrylonitrile, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polyhydroxyethyl methacrylate and polyhydroxypropyl methacrylate.

22. A medical device containing a drug coating, characterized in that: include: The body of the medical device and the drug coating according to any one of claims 1 to 21, wherein the drug coating is disposed on the surface of the body.

23. The medical device according to claim 22, characterized in that The body of the medical device has an expandable portion, and the drug coating is disposed on the surface of the expandable portion.

24. The medical device according to claim 22 or 23, characterized in that The medical device is a drug eluting stent, an occluder or a filter, and the medical device has a body made of metal.

25. The medical device according to any one of claims 22 to 24, characterized in that The drug coating is disposed on the surface of a portion of the body having a diameter greater than or equal to 5 mm.

26. The medical device according to any one of claims 22 to 25, characterized in that The medical device is a drug eluting stent for treating peripheral arterial stenosis. The length of the drug eluting stent is between 15 mm and 200 mm, and the diameter is between 3 mm and 12 mm.

27. An implantable medical device system, characterized in that: It comprises a medical device as described in any one of claims 22 to 26 and a conveying device detachable from the medical device, wherein the medical device is installed in the conveying device in a compressed state during delivery, and when the lesion position is reached, the conveying device is detached from the medical device, so that the medical device contacts the tissue wall in an expanded state.

28. A method for preparing a medical device containing a drug coating, characterized in that: The preparation method is used to prepare the medical device according to any one of claims 22 to 26, and the preparation method comprises: Providing a body of the medical device; A first solution and a second solution are configured to form drug coatings with different drug loading concentrations; Firstly, the first solution is applied to the body to form the inner layer of the drug coating; Then coating the inner layer with the second solution to form the outer layer of the drug coating; The drug loading concentration of the first solution is greater than that of the second solution, and the thickness of the inner layer is greater than that of the outer layer.

29. The preparation method according to claim 28, characterized in that: The method further comprises: preparing a bottom layer solution, wherein the bottom layer membrane-forming material and a solvent are mixed and dissolved to obtain the bottom layer solution; The bottom layer solution is applied to the surface of the main body to form the bottom layer, and then the first solution is applied to the main body on the bottom layer to form the inner layer of the drug coating.

Citation Information

Patent Citations

  • Coatings for medical devices

    CN1225292C

  • Organism indwelling support

    CN101052362A

  • Local vascular delivery system of probucol alone or in combination with sirolimus

    CN101543659A

  • Intracoronary stent with asymmetric drug releasing controlled coating

    CN101641059A

  • Medicament coated thrombus filter

    CN101843531A