Lithium secondary battery
The lithium secondary battery design addresses output and productivity issues by using a metal sheet to reduce resistance and enhance bonding quality, ensuring stable electrical connections and improved performance through a unique bonding mark configuration.
Patent Information
- Application Number
- PCT/JP2023/016526
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Existing lithium secondary battery technologies face challenges in maintaining output characteristics and productivity due to increased resistance and mechanical bonding issues, particularly when folding current collectors to connect metal layers, which complicates the lamination process and can lead to decreased battery performance.
The lithium secondary battery design incorporates a metal sheet between current collector ends, acting as an additional conductive layer to reduce resistance and improve bonding quality, with a unique bonding mark configuration that prevents overlap and ensures efficient electrical connection, thereby enhancing output characteristics and productivity.
This design effectively suppresses resistance increases at bonding marks, improving the output characteristics and productivity of lithium secondary batteries by ensuring stable electrical connections and reducing the risk of conductive layer damage during the lamination process.
Smart Images

Figure JP2023016526_31102024_PF_FP_ABST
Abstract
Description
Lithium secondary battery
[0001] Exemplary embodiments of the present disclosure relate to lithium secondary batteries.
[0002] Patent Document 1 discloses that the safety of a battery cell is improved by using a current collector in which metal layers are formed on both sides of a resin film. The front and back of the resin film are separated by an insulating resin layer, preventing electrical continuity. Therefore, when connecting an electrode tab for drawing wiring to the electrode film, continuity between the front and back of the electrode, and also between multiple electrodes and the electrode tab, is not achieved. In this regard, Patent Document 2 discloses that multiple current collectors are folded and laminated on each metal layer in order to connect each metal layer separated by a resin layer to the electrode tab for drawing wiring.
[0003] JP 11-102711 A JP 2013-016321 A
[0004] The present disclosure provides a technique for suppressing a decrease in output characteristics and productivity of lithium secondary batteries.
[0005] In one exemplary embodiment of the present disclosure, there is provided a lithium secondary battery, the lithium secondary battery including: (a) a first laminate including a first current collector having a first insulating layer sandwiched between a pair of first conductive layers; and a first electrode disposed on the first current collector, the first current collector having a first end where the first electrode is not disposed; (b) an intermediate laminate including an electrode having a polarity different from that of the first electrode and a separator; and (c) a second laminate disposed in a stacking direction apart from the first laminate via the intermediate laminate, the second current collector having a second insulating layer sandwiched between a pair of second conductive layers; and a second current collector disposed on the second current collector, the first electrode being disposed on the first current collector. (d) a metal sheet arranged in parallel with the first end and the second end in the stacking direction, the metal sheet having a first bonding mark due to bonding to either the first end or the second end; and (e) an electrode tab electrically connected to the first stack and the second stack, the electrode tab having a second bonding mark due to bonding to the first end, the metal sheet, and the second end, the second bonding mark being in a position different from the first bonding mark when viewed from the stacking direction.
[0006] According to one exemplary embodiment of the present disclosure, a technique can be provided that suppresses a decrease in output characteristics and productivity of a lithium secondary battery.
[0007] 7. FIG. 8 is an exploded perspective view illustrating an example of the configuration of a secondary battery 1. FIG. 9 is a perspective view illustrating an example of a negative electrode 10. FIG. 10 is a perspective view illustrating another example of a negative electrode 10. FIG. 11 is a perspective view illustrating an example of a positive electrode laminate 30 and a metal sheet MS. FIG. 12 is a view illustrating an example of a joining mark. FIG. 13 is a view illustrating another example of a joining mark. FIG. 14 is a view illustrating another example of a joining mark. FIG. 15 is a view illustrating a joining state of a positive electrode tab 40, an end P, and a metal sheet MS. FIG. 16 is a view illustrating a second joining mark WR2. FIG. 17 is a flowchart illustrating an example of the present manufacturing method. FIG. 18 is a view illustrating step ST1 of FIG. 19. FIG. 19 is a view illustrating step ST2 of FIG. 20. FIG. 19 is a view illustrating step ST2 of FIG. 21. FIG. 19 is a view illustrating step ST3 of FIG. 22. FIG. 19 is a perspective view illustrating another example of a negative electrode 10. FIG. 19 is a perspective view illustrating another example of a negative electrode 10. FIG. 19 is a cross-sectional view of a main portion illustrating another example of the configuration of a lithium secondary battery. FIG. 19 is a cross-sectional view of a main portion illustrating another example of the configuration of a lithium secondary battery. Fig. 1 is a perspective view for explaining another example of the configuration of a positive electrode laminate. Fig. 2 is a perspective view for explaining another example of the configuration of a positive electrode laminate. Fig. 3 is a diagram showing the configurations and results of an example and a comparative example. Fig. 4 is a diagram showing the stacking patterns of metal sheets in an example and a comparative example.
[0008] Hereinafter, each embodiment of the present disclosure will be described.
[0009] In one exemplary embodiment, a lithium secondary battery includes: (a) a first stack including a first current collector having a first insulating layer sandwiched between a pair of first conductive layers, and a first electrode disposed on the first current collector, the first current collector having a first end where the first electrode is not disposed; (b) an intermediate stack including an electrode having a polarity opposite to that of the first electrode and a separator; and (c) a second stack disposed apart from the first stack in the stacking direction via the intermediate stack, the second current collector having a second insulating layer sandwiched between a pair of second conductive layers, and a second current collector disposed on the second current collector, the first electrode. and a second electrode of the same polarity as the first end and the second end, and the second current collector has a second end where the second electrode is not located; (d) a metal sheet arranged alongside the first end and the second end in the stacking direction, the metal sheet having a first bonding mark due to bonding to either the first end or the second end; and (e) an electrode tab electrically connected to the first stack and the second stack, the electrode tab having a second bonding mark due to bonding to the first end, the metal sheet, and the second end, the second bonding mark being located at a different position from the first bonding mark when viewed from the stacking direction.
[0010] In one exemplary embodiment, the first bond mark is a weld mark.
[0011] In one exemplary embodiment, the first bonding mark is in the form of one or more lines.
[0012] In one exemplary embodiment, the first bonding marks are in the form of one or more dots.
[0013] In one exemplary embodiment, the second bond mark is a weld mark.
[0014] In one exemplary embodiment, the second bonding marks are in the form of one or more lines.
[0015] In one exemplary embodiment, the second bonding marks are in the form of one or more dots.
[0016] In one exemplary embodiment, the second bonding marks include, in a cross section in the stacking direction, a region where the pair of first conductive layers, the metal sheet, and the pair of second conductive layers are integrated.
[0017] In one exemplary embodiment, the first bonding mark and the second bonding mark do not overlap each other when viewed in the stacking direction.
[0018] In one exemplary embodiment, a plurality of first stacks and second stacks are arranged alternately in the stacking direction with an intermediate stack sandwiched between them.
[0019] In one exemplary embodiment, the first laminate is formed from a flat sheet, and the second laminate is formed from a flat sheet separate from the first laminate.
[0020] In one exemplary embodiment, the first and second laminates are constructed by folding or rolling a single sheet.
[0021] In one exemplary embodiment, a total of 10 or more layers of the first laminate and the second laminate are arranged.
[0022] In one exemplary embodiment, the metal sheet is provided on at least one of the plurality of first ends and the plurality of second ends.
[0023] In one exemplary embodiment, the metal sheet is provided on one side of at least one edge.
[0024] In one exemplary embodiment, the metal sheets are provided one on each side of at least one edge.
[0025] In one exemplary embodiment, the number of metal sheets is no more than three times the total number of first ends and second ends.
[0026] In one exemplary embodiment, the metal sheet is constructed of the same material as the first and second conductive layers.
[0027] In one exemplary embodiment, the first electrode and the second electrode are positive electrodes.
[0028] In one exemplary embodiment, the first electrode and the second electrode are negative electrodes.
[0029] Hereinafter, each embodiment of the present disclosure will be described in detail with reference to the drawings. In each drawing, the same or similar elements are designated by the same reference numerals, and redundant explanations will be omitted. Unless otherwise specified, the positional relationships, such as up, down, left, and right, will be described based on the positional relationships shown in the drawings. The dimensional ratios in the drawings do not represent actual ratios, and the actual ratios are not limited to the ratios shown in the drawings.
[0030] As mentioned above, Patent Document 2 proposes folding a current collector multiple times and stacking it on each metal layer to connect each metal layer separated by a resin layer to an electrode tab for wiring. However, this method requires a new device mechanism for stacking the current collector while folding back the end of the current collector for each metal layer. Furthermore, the end of the current collector must be folded back in conjunction with the stacking, significantly reducing productivity. Furthermore, even if this method can mechanically join the electrode tab, the current collector, and each metal layer, the resistance of the joint increases, resulting in reduced output characteristics. A lithium secondary battery 1 (hereinafter also referred to as "secondary battery 1") according to one embodiment can solve these problems.
[0031] <Configuration Example of Secondary Battery> Fig. 1 is an exploded perspective view illustrating a configuration example of a secondary battery 1. As shown in Fig. 1, the secondary battery 1 includes a negative electrode 10, a separator 20, a first positive electrode laminate 30A, a second positive electrode laminate 30B, a metal sheet MS, a positive electrode tab 40, and a negative electrode tab 42. Each component will be described in detail below.
[0032] 2A is a perspective view showing an example of the negative electrode 10. In one embodiment, the negative electrode 10 includes a negative electrode current collector 12 and a negative electrode active material 14 disposed on the negative electrode current collector 12.
[0033] 2A , the negative electrode active material 14 is disposed on each of both sides of the negative electrode current collector 12. In another embodiment, the negative electrode active material 14 may be disposed on only one side of the negative electrode current collector 12.
[0034] In one embodiment, the negative electrode current collector 12 is formed from at least one selected from the group consisting of metals that do not react with Cu, Ni, Ti, Fe, and Li, alloys thereof, and stainless steel.
[0035] The negative electrode active material 14 is a material that causes an electrode reaction, i.e., an oxidation reaction and a reduction reaction, at the negative electrode. The negative electrode active material 14 may be, for example, lithium metal, an alloy containing lithium metal, a carbon-based material, a metal oxide, a metal that alloys with lithium, or an alloy containing such a metal. The carbon-based material may be, for example, graphene, graphite, hard carbon, carbon nanotubes, or the like. The metal oxide may be, for example, a titanium oxide-based compound, a cobalt oxide-based compound, or the like. The metal that alloys with lithium may be, for example, silicon, silicon oxide, germanium, tin, lead, aluminum, gallium, or any of these pre-doped with lithium.
[0036] 2B is a perspective view showing another example of the negative electrode 10. As shown in FIG. 2B, the negative electrode 10 may be configured to include a negative electrode current collector 16 and a negative electrode active material 14 disposed on each of both surfaces of the negative electrode current collector 16. The material of the negative electrode active material 14 may be the same as that described in FIG. 2A. The negative electrode current collector 16 may be configured to include a negative electrode insulating layer 160 and a pair of negative electrode conductive layers 162 disposed so as to sandwich the negative electrode insulating layer 160 therebetween.
[0037] In one embodiment, the negative electrode insulating layer 160 may be composed of a sheet-like (film-like) or fibrous resin. The negative electrode conductive layer 162 is formed of at least one selected from the group consisting of a metal that does not react with Cu, Ni, Ti, Fe, or Li, an alloy thereof, and stainless steel. In one example, the negative electrode conductive layer 162 is Cu. By including the negative electrode insulating layer 160, the negative electrode current collector 16 can be made lighter than when the negative electrode current collector 16 is composed of only a conductive layer, while ensuring the thickness (rigidity) required for the negative electrode current collector 16.
[0038] As shown in Figures 2A and 2B, the negative electrode current collector (12, 16) has a negative electrode end Q. In one embodiment, the negative electrode end Q is configured as a part of the negative electrode current collector, extending outward (in the x direction) from the side surface of the negative electrode current collector. No negative electrode active material 14 is formed on the negative electrode end Q. A bonding mark WL2 with the negative electrode tab 42 is formed on the negative electrode end Q.
[0039] (Negative Electrode Tab 42) As shown in Fig. 1 , the negative electrode tab 42 is arranged to be aligned with each negative electrode end Q in the stacking direction (z direction). In one embodiment, the negative electrode tab 42 may be arranged above or below each negative electrode end Q. In one embodiment, the negative electrode tab 42 may be arranged between a certain negative electrode end Q and an adjacent negative electrode end Q.
[0040] The negative electrode tab 42 is joined to each negative electrode end Q. The negative electrode end 42 is electrically connected to each negative electrode 10 via each negative electrode end Q. A joining mark WL2 is formed on the negative electrode tab 42 due to joining with each negative electrode end Q. The joining mark WL2 may be one or more points (spots), or may be a continuous line or surface. In one embodiment, the negative electrode tab 42 and each negative electrode end Q may be joined by welding. In this case, the joining mark WL2 is a weld mark. The welding may be, for example, ultrasonic welding, laser welding, resistance welding, or spot welding.
[0041] (Separator 20) The separator 20 is disposed on the negative electrode 10. In the example shown in FIG. 1 , the separator 20 is disposed on both sides of the negative electrode 10. The separator 20 physically and / or electrically isolates the negative electrode 10 from the positive electrode laminate 30 and ensures ionic conductivity of lithium ions. In one embodiment, the separator 20 may be at least one selected from the group consisting of an insulating porous material, a polymer electrolyte, a gel electrolyte, and an inorganic solid electrolyte. The separator 20 may be formed of one type of material alone or a combination of two or more types of materials.
[0042] When the separator 20 includes an insulating porous member, the pores of the porous member are filled with an ion-conductive substance (such as an electrolytic solution, a polymer electrolyte, and / or a gel electrolyte). This allows the separator 20 to exhibit ion conductivity. The material constituting the insulating porous member is not particularly limited, and examples thereof include insulating polymer materials, specifically polyethylene (PE) and polypropylene (PP). That is, the separator 20 may be a porous polyethylene (PE) film, a porous polypropylene (PP) film, or a laminate structure thereof.
[0043] In one embodiment, one or both surfaces of the separator 20 may be coated with a separator coating layer. This may improve the cycle characteristics of the secondary battery 1. In one embodiment, the separator coating layer may be a continuous film with a uniform thickness over 50% or more of the surface area of the separator 20. In one embodiment, the separator coating layer may include a binder such as polyvinylidene fluoride (PVDF), a mixture of styrene butadiene rubber and carboxymethyl cellulose (SBR-CMC), and polyacrylic acid (PAA). In one embodiment, the separator coating layer may be formed by adding inorganic particles such as silica, alumina, titania, zirconia, or magnesium hydroxide to the binder.
[0044] In one embodiment, the thickness of the separator 20 (including the coating layer if the separator 20 includes the coating layer) may be 3.0 μm or more and 40 μm or less. This can reduce the volume occupied by the separator 20 while isolating the negative electrode 10 and the positive electrode stack 30. In one embodiment, the thickness of the separator 20 may be 5.0 μm or more, 7.0 μm or more, or 10 μm or more. In one embodiment, the thickness of the separator 20 may be 30 μm or less, 20 μm or less, or 10 μm or less.
[0045] (Intermediate laminate LM) As shown in FIG. 1 , in one embodiment, the negative electrode 10 and the separator 20 constitute an intermediate laminate LM. The intermediate laminate LM may have a structure in which the separator 20, the negative electrode 10, and the separator 20 are stacked in this order in the stacking direction (z direction). The secondary battery 1 includes a plurality of intermediate laminates LM. In one embodiment, the plurality of intermediate laminates LM may each be configured as a single flat sheet, as shown in FIG. 1 . In one embodiment, the plurality of intermediate laminates LM may be configured as a single sheet (an example of this embodiment will be described later using FIGS. 13 and 14 ).
[0046] (Positive Electrode Stack 30 and Metal Sheet MS) As shown in FIG. 1 , the first positive electrode stack 30A includes a current collector 32A and a positive electrode 34A. The first positive electrode stack 30A is an example of a first stack. In one embodiment, the first positive electrode stack may have a structure in which a positive electrode 34A, a current collector 32A, and a positive electrode 34A are stacked in this order in the stacking direction. The current collector 32A has a first end P1 exposed from the positive electrode 34A. In other words, the positive electrode 34A is not formed on the first end P1. The first end P1 extends outward (in the x direction) from the side surface of the current collector 32A as part of the current collector 32A.
[0047] The second positive electrode laminate 30B includes a current collector 32B and a positive electrode 34B. The second positive electrode laminate 30B is an example of a second laminate. In one embodiment, the second positive electrode laminate 30B may have a structure in which a positive electrode 34B, a current collector 32B, and a positive electrode 34B are stacked in this order in the stacking direction. The current collector 32B has a second end P2 exposed from the positive electrode 34B. In other words, the positive electrode 34B is not formed on the second end P2. The second end P2 extends outward (in the x direction) from the side surface of the current collector 32B as part of the current collector 32B.
[0048] The first positive electrode laminate 30A and the second positive electrode laminate 30B are alternately stacked in the stacking direction with intermediate laminates LM interposed therebetween (hereinafter, when there is no need to distinguish between the first positive electrode laminate 30A and the second positive electrode laminate 30B, they are collectively referred to as "positive electrode laminate 30"). In one embodiment, the multiple positive electrode laminates 30 may each be configured as a single flat sheet, as shown in FIG. 1. In one embodiment, the multiple positive electrode laminates 30 may be configured as a single sheet (an example of this embodiment will be described later using FIGS. 15 and 16).
[0049] In one embodiment, the total number of positive electrode laminates 30 included in the secondary battery 1 may be 5 or more, 10 or more, or 20 or more. In one embodiment, the total number of positive electrode laminates 30 included in the secondary battery 1 may be 50 or less, 40 or less, or 30 or less. In one embodiment, the energy density of the secondary battery 1 may be 300 Wh / kg or more. In one embodiment, the rated capacity of the secondary battery 1 may be 1.5 Ah or more, or may be 5 Ah or more.
[0050] As shown in FIG. 1 , metal sheets MS are arranged on a first end P1 and a second end P2 (hereinafter, when there is no need to distinguish between the two, they will be collectively referred to as "ends P"). In one embodiment, metal sheets MS may be arranged on all of the ends P. In another embodiment, metal sheets MS may be arranged on some of the ends P, and no metal sheets MS may be arranged on the remaining ends P. For example, metal sheets MS may be arranged every few ends P.
[0051] In one embodiment, the number and thickness of metal sheets to be placed on an end P may be set based on the position of the end P in the stacking direction. For example, two or more metal sheets MS may be placed on the end P in the center of the stacking direction of the secondary battery 1, and one metal sheet MS may be placed on each of the end Ps at the top and bottom in the stacking direction. Also, for example, the thickness of the metal sheet MS placed on the end P in the center of the stacking direction of the secondary battery 1 may be made larger than the thickness of the metal sheets placed on the end Ps at the top and bottom in the stacking direction. This can suppress variations in resistance between the end Ps at the center.
[0052] In one embodiment, the number of metal sheets MS may be three times or less, or may be two times or less, the total number of end parts P. In one embodiment, the number of metal sheets MS may be the same as the total number of end parts P, or may be less than the total number of end parts P, for example, half or less of the total number of end parts P.
[0053] 3 is a perspective view showing an example of a positive electrode laminate 30 and a metal sheet MS. In one embodiment, the positive electrode laminate 30 may have a current collector 32 and positive electrodes 34 disposed on both sides of the current collector 32. The current collector 32 has an insulating layer 320 and conductive layers 322 formed so as to sandwich the insulating layer 320.
[0054] The insulating layer 320 of the current collector 32 may be made of, for example, a sheet-like (film-like) or fibrous resin. The resin may be, for example, at least one of polyolefin resins such as polyethylene terephthalate (PET), polyethylene, and polypropylene, and thermoplastic resins such as polystyrene, polyvinyl chloride, and polyamide. The insulating layer 320 may be made by laminating multiple layers of at least one of the resins. In one embodiment, the insulating layer 320 is made of a material having a melting point of 150°C or higher and 300°C or lower. In one embodiment, the thickness of the insulating layer 320 may be 3 μm or higher and 10 μm or lower, or 4 μm or higher and 8 μm or lower.
[0055] The insulating layer 320 melts in the event of abnormal heat generation due to overcharge or high temperature conditions, damaging the positive electrode laminate 30 and functioning to interrupt short-circuit current within the battery. This can suppress a sudden temperature rise within the secondary battery 1 and prevent the battery from catching fire. In other words, the insulating layer 320 can contribute to improving the safety of the secondary battery 1.
[0056] The conductive layers 322 of the current collector 32 are formed on both sides of the insulating layer 320 so as to sandwich the insulating layer 320. The conductive layers 322 are in physical and / or electrical contact with the positive electrode 34 and function to donate and receive electrons to and from the positive electrode 34. The conductive layers 322 are made of a conductor that does not react with lithium ions in the battery. In one embodiment, the conductive layers 322 are made of at least one material selected from the group consisting of aluminum, titanium, stainless steel, nickel, and alloys thereof. In one example, the conductive layers 322 are aluminum or aluminum alloys. In one embodiment, the conductive layers 322 are formed by vapor deposition, sputtering, electroplating, or lamination of the above materials on both surfaces of the insulating layer 320. In one embodiment, the thickness of each conductive layer 322 may be 0.5 μm to 5 μm, 0.7 μm to 3 μm, or 0.8 μm to 2.0 μm.
[0057] The positive electrodes 34 are formed on both sides of the current collector 32. A known material may be appropriately selected for the positive electrodes 34 depending on the application. The thickness of the positive electrodes 34 may be appropriately adjusted depending on the desired capacity and rate characteristics of the battery. In one embodiment, the thickness of each positive electrode 34 is, for example, 20 μm or more and 150 μm or less.
[0058] In one embodiment, the positive electrode 34 includes a positive electrode active material. The positive electrode active material is a material for holding a carrier metal in the positive electrode 34 and can also be referred to as a host material for the carrier metal. The positive electrode active material may be a material for holding lithium ions in the positive electrode 34. In this case, lithium ions are loaded into and deloaded from the positive electrode active material as the battery is charged and discharged. This can improve the stability and output voltage of the battery.
[0059] In one embodiment, the positive electrode active material is a metal oxide or a metal phosphate. The metal oxide may be, for example, a cobalt oxide-based compound, a manganese oxide-based compound, or a nickel oxide-based compound. The metal phosphate may be, for example, an iron phosphate-based compound or a cobalt phosphate-based compound. In one embodiment, the positive electrode active material is LiCoO 2 , LiNi x Co y Mn z O(x+y+z=1), LiNi x Co y Al z O(x+y+z=1), LiNi x Mn y O(x+y=1), LiNiO 2 , LiMn 2 O 4 , LiFePO 4 , LiCoPO 4 , LiFeOF, LiNiOF, and LiTiS 2 The positive electrode active material may be at least one selected from the group consisting of: (a) and (b) above. The positive electrode active material may be used singly or in combination of two or more. In one embodiment, the content of the positive electrode active material in the positive electrode 34 may be 50% by mass or more and 100% by mass or less with respect to the entire positive electrode 34.
[0060] In one embodiment, the positive electrode 34 may include one or more components other than the positive electrode active material.
[0061] In one embodiment, the positive electrode 34 may include a sacrificial positive electrode material, which is a lithium-containing compound that undergoes an oxidation reaction and does not substantially undergo a reduction reaction in the charge / discharge potential range of the positive electrode active material.
[0062] In one embodiment, the positive electrode 34 may include a gel electrolyte. The gel electrolyte may improve adhesion between the positive electrode 34 and the current collector 32. In one example, the gel electrolyte includes a polymer, an organic solvent, and a lithium salt. The polymer in the gel electrolyte may be, for example, a copolymer of polyethylene and / or polyethylene oxide, polyvinylidene fluoride, or a copolymer of polyvinylidene fluoride and hexafluoropropylene.
[0063] In one embodiment, the positive electrode 34 may include a conductive additive and / or a binder. In one example, the conductive additive is carbon black, single-walled carbon nanotubes (SWCNT), multi-walled carbon nanotubes (MWCNT), carbon nanofibers (CF), or the like. In one example, the binder is polyvinylidene fluoride, polytetrafluoroethylene, styrene butadiene rubber, acrylic resin, polyimide resin, or the like. In one embodiment, the content of the conductive additive is 0.5% by mass to 30% by mass or less with respect to the entire positive electrode 34. In one embodiment, the content of the binder may be 0.5% by mass to 30% by mass or less with respect to the entire positive electrode 34.
[0064] In one embodiment, the positive electrode 34 may include a polymer electrolyte. In one example, the polymer electrolyte is a solid polymer electrolyte primarily containing a polymer and an electrolyte, or a semi-solid polymer electrolyte primarily containing a polymer, an electrolyte, and a plasticizer. In one embodiment, the total content of the polymer electrolyte may be 0.5% by mass to 30% by mass or less with respect to the entire positive electrode 34.
[0065] 3 , the metal sheet MS may be bonded to one surface of the end P of the current collector 32 (one surface of the pair of conductive layers 322). In another embodiment, the metal sheet MS may be bonded to the other surface of the end P of the current collector 32 (the other surface of the pair of conductive layers 322). In another embodiment, one or more metal sheets MS may be provided at the end P. For example, one metal sheet MS may be bonded to one surface and one metal sheet MS to the other surface of the end P of the current collector 32.
[0066] As shown in FIG. 3 , a first joining mark WR1 is formed between the metal sheet MS and the end P by joining the metal sheet MS and the end P. In one embodiment, the first joining mark WR1 may be a joining mark formed by welding, i.e., a welding mark. The welding may be, for example, ultrasonic welding, laser welding, resistance welding, or spot welding. In one example, the welding is ultrasonic welding. In one embodiment, the metal sheet MS and the conductive layer 322 of the end P may be partially or completely fused together at the first joining mark WR1 by heat or the like. A second joining mark WR2 is also formed on the metal sheet MS and the end P. As will be described in detail later, the second joining mark WR2 is a joining mark between the end P and the metal sheet MS and the positive electrode tab 40.
[0067] In one embodiment, as shown in FIG. 3 , the metal sheet MS may be configured to cover only a portion of the end P of the current collector 32, rather than the entire end P. For example, the metal sheet MS may be positioned a predetermined distance away from the positive electrode 34. In this case, an insulating layer may be provided on the conductive layer 322 at the end P in an area where the metal sheet MS is not disposed. In this case, if the separator 20 is damaged, a short circuit between the negative electrode 10 and the positive electrode 34 via the conductive layer 322 at the end P and / or the metal sheet MS is suppressed, thereby improving the safety of the secondary battery 1. The insulating layer may be, for example, a sheet-shaped (film-shaped) or fibrous resin. The resin may be, for example, at least one of a polyolefin resin such as polyethylene terephthalate (PET), polyethylene, or polypropylene, or a thermoplastic resin such as polystyrene, polyvinyl chloride, or polyamide. Note that in one embodiment, the metal sheet MS may be configured to cover the entire end P of the current collector.
[0068] In one embodiment, the metal sheet MS is made of at least one material selected from the group consisting of aluminum, titanium, stainless steel, nickel, and alloys thereof. In one example, the metal sheet MS is a hard aluminum foil. In one example, the metal sheet MS is a soft aluminum foil. The soft aluminum foil may be formed by subjecting the hard aluminum foil to a high-temperature heat treatment (around 400°C). In one embodiment, the metal sheet MS may be made of the same material as the conductive layer 322.
[0069] In one embodiment, the thickness of the metal sheet MS may be set based on the thickness of the insulating layer 320 and the thickness of the conductive layer 322. For example, where X (= A + B) is the sum of the total thickness of each metal sheet MS (A) and the total thickness of each conductive layer 322 (B), and Y is the total thickness of each insulating layer 320, the thickness of the metal sheet MS may be set so that the relationship 0.85<X / Y<2.3 holds. In one embodiment, 1.0<X / Y<2.0 may be true. In one embodiment, the thickness of the metal sheet MS may be thicker than the thickness of the insulating layer 320. In one embodiment, all of the metal sheets MS may have the same thickness, or some may have different thicknesses. In one embodiment, the thickness of the metal sheet MS may be 3 μm or more, 5 μm or more, or 7 μm or more. In one embodiment, the thickness of the metal sheet MS may be 15 μm or less, 12 μm or less, or 10 μm or less.
[0070] 4A is a diagram illustrating an example of a bonding mark. FIG. 4A is a plan view of the vicinity of end P of the positive electrode laminate 30 shown in FIG. 3. As shown in FIG. 3, the first bonding marks WR1 may be formed in multiple lines (for example, two lines) along the width direction (y direction) of the end P. As shown in FIG. 4A, the first bonding marks WR1 are formed at a different position from the second bonding marks WR2 when viewed from the stacking direction. In other words, the first bonding marks WR1 and the second bonding marks WR2 do not overlap in a plan view.
[0071] 4B to 4D are diagrams illustrating other examples of bonding marks. In one embodiment, the first bonding marks WR1 may be formed in a line along the width direction (y direction) of the end P, as shown in FIG. 4B. In one embodiment, the first bonding marks WR1 may be formed in a dot shape, as shown in FIGS. 4C and 4D, and may be formed in a line (FIG. 4C) or multiple lines (FIG. 4D) along the width direction (y direction) of the end P. In all of FIGS. 4B to 4D, the first bonding marks WR1 are positioned at different positions from the second bonding marks WR2 when viewed from the stacking direction. That is, in all of FIGS. 4B to 4D, the first bonding marks WR1 and the second bonding marks WR2 do not overlap in a plan view.
[0072] (Positive Electrode Tab 40) As shown in Fig. 1 , the positive electrode tab 40 is arranged to be aligned in the stacking direction (z direction) with each end P (P1, P2) of the current collector 32 (32A, 32B) and each metal sheet MS. In one embodiment, the positive electrode tab 40 may be arranged above or below the end P of each current collector 32 and each metal sheet MS. In one embodiment, the positive electrode tab 40 may be arranged between an end P and an adjacent end P.
[0073] The positive electrode tab 40 is made of a conductive material. For example, the positive electrode tab 40 may be made of aluminum or an aluminum alloy. In one example, the positive electrode tab 40 may be made of hard aluminum. In one embodiment, the thickness of the positive electrode tab 40 may be 0.05 mm or more and 1 mm or less, or 0.1 mm or more and 0.5 mm or less.
[0074] The positive electrode tab 40 is joined to each end P of each current collector 32 and each metal sheet MS. As a result, the positive electrode tab 40 is electrically connected to each positive electrode 34 via each end P. A second joining mark WR2 is formed on the positive electrode tab 40 by joining to each end P. The second joining mark WR2 may be one or more points (spots) in a plan view, or may be a continuous line or surface.
[0075] In one embodiment, the positive electrode tab 40 may be joined to each end P and each metal sheet MS by welding. The welding may be, for example, ultrasonic welding, laser welding, resistance welding, or spot welding. In one example, the welding is ultrasonic welding.
[0076] 5 is a diagram for explaining the bonding state of the positive electrode tab 40, the end P, and the metal sheet MS. Fig. 5 is a schematic cross-section of the end P, taken along the xz plane, at a location including the first bonding mark WR1 and the second bonding mark WR2.
[0077] As shown in Figure 5, the first bonding mark WR1 and the second bonding mark WR2 are provided at different positions from each other when viewed from the stacking direction. The first bonding mark WR1 is formed for each end P. In other words, one first bonding mark WR1 is not formed across multiple end Ps. In contrast, the second bonding mark WR2 is formed over the positive electrode tab 40, each end P, and each metal sheet MS. In other words, the second bonding mark WR2 is formed continuously in the stacking direction from the positive electrode tab 40 to the end P of the lowest layer.
[0078] 6 is a diagram illustrating the second bonding mark WR2. FIG. 6 schematically shows a cross section of the second bonding mark WR2 taken along the zy plane (cross section A-A in FIG. 5). As shown in FIG. 6, the cross section of the second bonding mark WR2 includes a first region R1 and a second region R2. In one embodiment, the cross section of the second bonding mark WR2 may have a recess recessed on one side in the stacking direction.
[0079] In the first region R1, the conductive layer 322 and the metal sheet MS are integrally stacked and joined to the positive electrode tab 40. Here, being integrally stacked includes a state in which the conductive layers 322 and the metal sheet MS are partially or entirely fused together by heat or the like (a state in which the layers are indistinguishable).
[0080] In one embodiment, the first region R1 may be substantially free of the insulating layer 320 along the stacking direction, and provides a physical path for electrical connection between the electrode tab 40 and each conductive layer 322 and the metal sheet MS.
[0081] In one embodiment, the first region R1 may be configured between two second regions R2. In one embodiment, the maximum thickness of the first region R1 may be half or less of the maximum thickness of the second region R2.
[0082] In the second region R2, a pair of conductive layers 322 and the metal sheet MS are stacked, sandwiching the insulating layer 320. That is, the second region R2 is a region that includes the insulating layer 320 along the stacking direction.
[0083] In one embodiment, the second joining mark WR2 may be formed by welding. In this case, the second joining mark WR2 is a welding mark. During welding, the positive electrode tab 40, the end P, and the metal sheet MS may be pressed along the stacking direction. This softens the insulating layer 320 at the welded location and pushes it outward in the width direction (left-right direction in FIG. 6 ) from the welded location. Furthermore, at the welded location, each conductive layer 322 and the metal sheet MS are thermally fused and integrated. This allows the first region R1 and the second region R2 to be formed.
[0084] As described above, the insulating layer 320 can suppress a rapid temperature rise inside the secondary battery 1 and prevent the battery from catching fire in the event of abnormal heat generation due to overcharge or high temperature conditions. In a current collector sandwiching an insulating layer between conductive layers, as the number of current collectors increases or the thickness of the insulating layers increases, it becomes more difficult to bond the current collector end to the electrode tab and ensure stable bonding quality (controlling variations) at each layer. For example, if a strong pressure is applied to weld all of the electrode tabs to the end, there is a risk that the conductive layer at the end will be damaged or broken, especially if the conductive layer is thin. On the other hand, if the electrode tab is welded to the current collector with a force that does not damage the conductive layer, the bond may be insufficient, resulting in increased resistance between the current collector end and the electrode tab.
[0085] In this regard, in the secondary battery 1 according to one embodiment, a metal sheet MS is disposed between at least one end P. The metal sheet MS functions as an additional conductive layer for the conductive layer 322 at the second bonding mark WR2, increasing the ratio of the conductive layer to the insulating layer 320. This can suppress an increase in resistance at the second bonding mark WR2. This can improve the output characteristics of the secondary battery 1. The metal sheet MS can also function as a protective layer for the conductive layer 322 at the end P when bonding the positive electrode tab 40 to the end P. This can suppress damage or breakage of the conductive layer 322, even when the total number (number of stacked layers) of the secondary battery 1 is large and the positive electrode tab 40 is bonded to each end P by pressing with a strong force. This can improve the production yield of the secondary battery 1. In one embodiment, the resistance of the second bonding mark WR2 may be 5.0 mΩ or less, 3.0 mΩ or less, 1.0 mΩ or less, or 0.5 mΩ or less.
[0086] (Electrolyte) In one embodiment, the secondary battery 1 may contain an electrolyte. The electrolyte is a liquid containing a solvent and an electrolyte, and has ion conductivity. The electrolyte may also be referred to as a liquid electrolyte, and acts as a conductive path for lithium ions. Therefore, when the secondary battery 1 contains an electrolyte, the internal resistance can be reduced, and the energy density, capacity, and cycle characteristics can be improved.
[0087] The electrolytic solution may be, for example, a solution that fills the housing (pouch) of the secondary battery 1. Furthermore, for example, the electrolytic solution may be impregnated into the separator 20, or may be held in a polymer to form a polymer electrolyte or a gel electrolyte.
[0088] The electrolyte contained in the electrolytic solution may be, for example, a lithium salt. Examples of the lithium salt include LiI, LiCl, LiBr, LiF, and LiBF. 4 , LiPF 6 , LiAsF 6 , LiSO 3 CF 3 , LiN(SO 2 F) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO2 CF 3 CF 3 ) 2 , LiB(O 2 C 2 H 4 ) 2 , LiB(C 2 O 4 ) 2 , LiB(O 2 C 2 H 4 ) F 2 , LiB(OCOCF 3 ) 4 , LiNO 3 , and Li 2 SO 4 It may be one or a combination of two or more selected from the group consisting of:
[0089] As the solvent contained in the electrolytic solution, for example, a non-aqueous solvent containing fluorine atoms (hereinafter referred to as a "fluorinated solvent") and a non-aqueous solvent containing no fluorine atoms (hereinafter referred to as a "non-fluorinated solvent") may be added.
[0090] The fluorinated solvent may be, for example, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether.
[0091] The fluorine-free solvent may be, for example, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, 1,2-dimethoxyethane, dimethoxyethane, dimethoxypropane, dimethoxybutane, diethylene glycol dimethyl ether, acetonitrile, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, chloroethylene carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, trimethyl phosphate, triethyl phosphate, and 12-crown-4.
[0092] The above fluorinated solvents and / or non-fluorinated solvents may be used alone or in any combination of two or more in any ratio. The contents of the fluorinated solvent and non-fluorinated solvent are not particularly limited, and the ratio of the fluorinated solvent to the total solvent may be 0 to 100% by volume, or the ratio of the non-fluorinated solvent to the total solvent may be 0 to 100% by volume.
[0093] <Method of Manufacturing Secondary Battery> Next, an example of a method of manufacturing the secondary battery 1 (hereinafter also referred to as "this manufacturing method") will be described with reference to FIGS. 7 to 10. FIG. 7 is a flowchart showing an example of this manufacturing method. FIGS. 8A and 8B are diagrams for explaining step ST1 in FIG. 7. FIGS. 9A to 9D are diagrams for explaining step ST2 in FIG. 7. FIG. 10 is a diagram for explaining step ST3 in FIG. 7.
[0094] As shown in FIG. 7 , this manufacturing method includes step ST1 of preparing a positive electrode laminate sheet, step ST2 of joining metal sheets of the positive electrode laminate sheet, step ST3 of cutting out a positive electrode laminate from the positive electrode laminate sheet, step ST4 of assembling a molded body, step ST5 of joining electrode tabs and current collectors, and step ST6 of sealing the molded body in a sealed container.
[0095] First, in step ST1, a positive electrode laminate sheet S1 is prepared as shown in FIGS. 8A and 8B . FIG. 8A is a plan view of the positive electrode laminate sheet S1. FIG. 8B is a cross-sectional view taken along the line B-B of FIG. 8A . As shown in FIG. 8A , the positive electrode laminate sheet S1 may be a strip-shaped sheet having a longitudinal direction (y direction) and a transverse direction (x direction). In one embodiment, as shown in FIGS. 8A and 8B , the positive electrode laminate sheet S1 may be composed of a current collector 32 and a positive electrode 34 applied to both sides of the current collector 32. The current collector 32 may have an insulating layer 320 and conductive layers 322 formed to sandwich the insulating layer 320. At one end of the positive electrode laminate sheet in the transverse direction (x direction), the positive electrode 34 is not formed, and the conductive layer 322 of the current collector 32 is exposed.
[0096] Next, in step ST2, a metal sheet MS is joined to one short-side end of the positive electrode laminate sheet S1, as shown in Figures 9A to 9D. Figure 9A is a plan view of the positive electrode laminate sheet S1 joined to the metal sheet MS. Figures 9B to 9D are examples of cross sections taken along the line CC of Figure 9A.
[0097] As a result of the joining in step ST2, a first joining mark WR1 is formed in the longitudinal direction, for example, in a line shape, as shown in FIG. 9A . The metal sheet MS may be joined to the positive electrode laminate sheet S1 by welding. The welding may be, for example, ultrasonic welding, laser welding, resistance welding, or spot welding. One example of the welding is ultrasonic welding.
[0098] In one embodiment, the bonding in step ST2 may be performed by pressing the metal sheet MS against the current collector 32. For example, as shown in FIGS. 9B and 9C , the first bonding mark WR1 may be formed so that the metal sheet MS is recessed toward the current collector 32. In one embodiment, the first bonding mark WR1 may be provided between the metal sheet MS and one conductive layer 322 (with which the metal sheet MS is in contact) as shown in FIG. 9B . In this case, the metal sheet MS is not electrically connected to the other conductive layer 322 at the first bonding mark WR1. In one embodiment, the first bonding mark WR1 may be provided between the metal sheet MS and both conductive layers 322 as shown in FIG. 9C . In this case, the metal sheet MS is electrically connected to both conductive layers 322 at the first bonding mark WR1.
[0099] In one embodiment, the bonding in step ST2 may be performed by pressing the current collector 32 against the metal sheet MS. For example, as shown in Fig. 9D, the first bonding mark WR1 may be formed so that the current collector 32 is recessed toward the metal sheet MS. In this case, the metal sheet MS is electrically connected to both conductive layers 322 at the first bonding mark WR1.
[0100] Next, in step ST3, the positive electrode laminate 30 is cut out. Specifically, using a cutting blade, a laser, or the like, a plurality of positive electrode laminates 30 having a given shape are cut out from the positive electrode laminate sheet S1 in a state in which the metal sheet MS is joined to the positive electrode laminate sheet S1, as shown in Fig. 10. In this way, a plurality of positive electrode laminates 30 are obtained.
[0101] Next, in step ST4, a molded body is assembled in which positive electrode laminates 30 and intermediate laminates LM are alternately stacked. Specifically, the multiple positive electrode laminates 30 prepared in step ST3 are arranged so as to be spaced apart from one another in the stacking direction, with the intermediate laminates LM interposed therebetween, as shown in Fig. 1. Note that, as will be described later, when the negative electrode 10 and the separator 20 are configured in a sheet-like shape, the positive electrode laminates 30 may be arranged between separators 20 formed by folding the sheet in a zigzag shape (see Fig. 9) or between separators 20 formed by rolling the sheet (see Fig. 10).
[0102] Next, in step ST5, the electrode tabs and the current collectors are joined. Specifically, the end P of each current collector 32 and the metal sheet MS are joined to the electrode tab 40 so as to form the second joining mark WR2 described above. The second joining mark WR2 is joined so as not to overlap the first joining mark WR1 in the stacking direction. Furthermore, the negative electrode end Q is joined to the negative electrode tab 42 so as to form a joining mark WL2. The joining may be performed by ultrasonic welding, laser welding, resistance welding, or spot welding.
[0103] Next, in step ST6, the molded body prepared in step ST5 is sealed in a sealed container. In one embodiment, an electrolyte may be sealed in the sealed container. The sealed container may be, for example, a laminate film. In this way, the secondary battery 1 is manufactured.
[0104] In this manufacturing method, in step ST2, a metal sheet MS is bonded to a positive electrode laminate sheet MS in advance. Therefore, in step ST3, the metal sheet MS can be simultaneously cut out to match the shape of the end P of the positive electrode laminate sheet S1. That is, a separate step of cutting out the metal sheet MS to match the shape of the end P is not required. Furthermore, in step ST5, alignment of the metal sheet MS with the end P of the current collector 32 is not required, facilitating bonding of the positive electrode tab 40 to the end P. Furthermore, in principle, in step ST5, the second bonding mark WR2 can be provided so as not to overlap with the first bonding mark WR1 in the stacking direction. By providing the second bonding mark WR2 so as not to overlap with the first bonding mark WR1 in the stacking direction, the bonding state of the second bonding mark WR2 is improved compared to when the two are provided overlapping, and an increase in the resistance of the second bonding mark WR2 can be suppressed.
[0105] <Method of Using the Secondary Battery> The secondary battery 1 is charged and discharged by connecting the positive electrode tab 40 to one end of an external circuit and the negative electrode tab 42 to the other end of the external circuit. The external circuit may be, for example, a resistor, a power source, an apparatus, a device, another battery, or a potentiostat. The ends P of the multiple positive electrode laminates 30 may be connected to the external circuit at the same potential. The negative electrode ends Q of the multiple negative electrodes 10 may be connected to the external circuit at the same potential.
[0106] When a voltage is applied between the positive electrode tab 40 and the negative electrode tab 42 such that a current flows from the negative electrode tab 42 to the positive electrode tab 40 through an external circuit, the secondary battery 1 is charged, and lithium metal is deposited on the negative electrode 10. When the positive electrode tab 40 and the negative electrode tab 42 of the charged secondary battery 1 are connected via a desired external circuit, the secondary battery 1 is discharged, and lithium metal in the negative electrode 10 is electrolytically dissolved.
[0107] In one embodiment, a solid electrolyte interface layer (SEI layer) may be formed on the surface of the negative electrode 10 or the surface of the separator 20 (i.e., the interface between the negative electrode 10 and the separator 20) during the first charge (initial charge) after assembly of the secondary battery 1. The SEI layer may contain, for example, an inorganic compound containing lithium or an organic compound containing lithium. In one embodiment, the thickness of the SEI layer is 1.0 nm or more and 10 μm or less. When an SEI layer is formed in the secondary battery 1, lithium metal is precipitated or dissolved at the interface between the negative electrode 10 and / or the separator 20 and the SEI layer during charge and discharge.
[0108] According to the secondary battery 1 described above, the output characteristics and productivity of the battery can be improved.
[0109] <Modifications> The secondary battery 1 can be modified in various ways without departing from the scope and spirit of the present disclosure.
[0110] (Negative electrode 10) FIG. 11 is a perspective view showing another example of the negative electrode 10. In one embodiment, a metal sheet may be provided at the negative electrode end Q of the negative electrode 10. The example shown in FIG. 11 is an example in which a negative electrode metal sheet MS2 is provided on one surface of the negative electrode end Q of the negative electrode 10 shown in FIG. 2B. In one embodiment, the negative electrode metal sheet MS2 may be made of the same material as the negative electrode conductive layer 162. In one example, the negative electrode metal sheet MS2 is made of Cu.
[0111] 11 , a first bonding mark WL1 may be formed between the negative electrode metal sheet MS2 and the negative electrode end Q by joining them. Furthermore, a second bonding mark WL2 may be formed by joining the negative electrode end Q and the negative electrode metal sheet MS2 to the negative electrode tab 42. The bonding form and positional relationship of the first bonding mark WL1 and the second bonding mark WL2 at the negative electrode end Q may be similar to the first bonding mark WR1 and the second bonding mark WR2 at the end P, and therefore a description thereof will be omitted.
[0112] FIG. 12 is a perspective view showing another example of the negative electrode 10. In one embodiment, the negative electrode 10 may be substantially free of a negative electrode active material. In the example shown in FIG. 12, the negative electrode 10 is made of at least one metal selected from the group consisting of Cu, Ni, Ti, Fe, and other metals that do not react with Li, alloys thereof, and stainless steel (SUS). The "metal that does not react with Li" may be a metal that does not react with lithium ions or lithium metal to form an alloy when the secondary battery 1 is in operation. The negative electrode 10 also functions as a current collector.
[0113] Note that the negative electrode 10 being "substantially free of negative electrode active material" includes, for example, that the thickness of the layer of negative electrode active material deposited on the negative electrode 10 at the end of discharge (e.g., a state in which the open circuit voltage of the battery is 2.5 V or more and 3.6 V or less) is 25 μm or less. In one embodiment, the thickness of the layer of negative electrode active material at the end of discharge may be 20 μm or less, 15 μm or less, 10 μm or less, or 5 μm or less, or may even be 0 μm. When the negative electrode 10 is substantially free of negative electrode active material, the energy density per volume can be improved in addition to the energy density per weight. Note that in this case, the secondary battery 1 can also be referred to as an "anode-free lithium battery," a "zero anode lithium battery," or an "anodeless lithium battery."
[0114] In one embodiment, the negative electrode 10 does not have a negative electrode active material before the initial charge of the battery (the state from the assembly of the battery to the first charge). That is, after the initial charge, the secondary battery 1 may be charged and discharged by depositing lithium metal on the negative electrode and electrolytically dissolving the deposited lithium metal. In this case, the volume and mass occupied by the negative electrode active material are reduced, the volume and mass of the entire battery are reduced, and the energy density is, in principle, increased. Note that "lithium metal deposited on the negative electrode" not only refers to lithium metal being deposited on the surface of the negative electrode, but also includes lithium metal being deposited on the surface of a solid electrolyte interface (SEI) layer or on or inside a buffer functional layer, which will be described later.
[0115] In one embodiment, the mass of lithium metal deposited on the negative electrode when the voltage is 4.2 V is M 4.2 The same mass at a voltage of 3.0 V is M3.0 In this case, M 3.0 / M 4.2 may be 40% or less, or 35% or less. 3.0 / M 4.2 may be 1.0% or more, 2.0% or more, 3.0% or more, or 4.0% or more.
[0116] In one embodiment, the thickness of the negative electrode 10 may be 1.0 μm or more and 30 μm or less, which can reduce the volume occupied by the negative electrode 10 in the secondary battery 1 and improve the energy density. The thickness of the negative electrode 10 may be 2.0 μm or more and 20 μm or less, 2.0 μm or more and 18 μm or less, or 3.0 μm or more and 15 μm or less.
[0117] In one embodiment, the negative electrode 10 may be coated on at least a portion of the surface facing the positive electrode laminate 30 with a compound (hereinafter also referred to as "negative electrode coating agent") containing an aromatic ring to which two or more elements selected from the group consisting of N, S, and O are independently bonded. The negative electrode coating agent can be held on the negative electrode 10 by the above elements being coordinately bonded to metal atoms constituting the negative electrode 10. According to this aspect, a non-uniform deposition reaction of lithium metal on the surface of the negative electrode 10 can be suppressed, and the lithium metal deposited on the negative electrode 10 can be suppressed from growing in a dendritic form.
[0118] In one embodiment, the anode coating agent is coated on at least a portion of the surface of the anode 10. In one embodiment, the anode coating agent may be present on 10% or more of the surface area, or may be present on 20% or more, 40% or more, 60% or more, or 80% or more of the surface area.
[0119] In one embodiment, the aromatic ring contained in the negative electrode coating agent may be an aromatic hydrocarbon such as benzene, naphthalene, azulene, anthracene, and pyrene, or a heteroaromatic compound such as furan, thiophene, pyrrole, imidazole, pyrazole, pyridine, pyridazine, pyrimidine, and pyrazine. In one example, the aromatic ring is an aromatic hydrocarbon. In one example, the aromatic ring is benzene or naphthalene. In one example, the aromatic ring is benzene.
[0120] In one embodiment, the negative electrode coating agent may be configured by one or more nitrogen atoms bonded to an aromatic ring. In one embodiment, the negative electrode coating agent may be a compound having a structure in which a nitrogen atom is bonded to an aromatic ring and, in addition to the nitrogen atom, one or more elements selected from the group consisting of N, S, and O are each independently bonded. Using a compound in which a nitrogen atom is bonded to an aromatic ring as the negative electrode coating agent can improve the cycle characteristics of the battery.
[0121] The negative electrode coating agent may be, for example, at least one selected from the group consisting of benzotriazole, benzimidazole, benzimidazole thiol, benzoxazole, benzoxazole thiol, benzothiazole, and mercaptobenzothiazole, and derivatives thereof. In one example, the negative electrode coating agent is at least one selected from the group consisting of benzotriazole, benzimidazole, benzoxazole, and mercaptobenzothiazole, and derivatives thereof.
[0122] (Buffer Functional Layer) In one embodiment, a porous or fibrous buffer functional layer may be provided between the negative electrode 10 and the separator 20. The buffer functional layer has a solid portion (including a gel-like portion) that has ionic conductivity and electrical conductivity, and a pore portion formed by gaps in this solid portion. In this case, lithium metal may precipitate on the surface of the negative electrode 10 (the interface between the negative electrode 10 and the buffer functional layer) and / or inside the buffer functional layer (the surface of the solid portion of the buffer functional layer).
[0123] 13 and 14 are cross-sectional views of a main part for explaining another example of the configuration of a lithium secondary battery. In one embodiment, the negative electrode 10 and the separators 20 arranged on both sides of the negative electrode 10 may be configured as a single sheet SH.
[0124] In one embodiment, as shown in FIG. 13 , the sheet SH may be folded multiple times at acute angles to form an intermediate laminate, and each positive electrode laminate 30 (30A, 30B) may be disposed between the separators 20 facing each other in the intermediate laminate.
[0125] In one embodiment, as shown in Fig. 14 , the sheet SH may be wound multiple times to form an intermediate laminate, and each positive electrode laminate 30 (30A, 30B) may be disposed between the opposing separators 20 of the intermediate laminate. Note that in the example shown in Fig. 14 , each positive electrode laminate 30 may also be formed by winding a single sheet, as described below (see Fig. 15 ).
[0126] 13 and 14, even if the negative electrode 10 and separator 20 are very thin, they can be handled as a single sheet SH, which can improve the productivity of the battery. Furthermore, in the sheet SH, physical pressure is applied from both sides to the negative electrode 10 sandwiched between the separators 20, so wrinkles are less likely to occur in the negative electrode 10 when the sheets SH are stacked, which can improve the cycle characteristics of the battery.
[0127] (Positive Electrode Stack) FIGS. 15 and 16 are perspective views illustrating other configuration examples of the positive electrode stack. In one embodiment, each positive electrode stack 30 may be configured by winding a single sheet SH2 multiple times, as shown in FIG. 15 . In one embodiment, each positive electrode stack 30 may be configured by alternately folding a single sheet SH2 multiple times at acute angles, as shown in FIG. 16 . The sheet SH2 may include, for example, a current collector 32 and positive electrodes 34 disposed on both sides of the current collector 32. In the examples shown in FIGS. 15 and 16 , even if the current collector 32 and the positive electrodes 34 are very thin, they can be handled as a single sheet SH2, which can improve battery productivity.
[0128] Examples and Comparative Examples Next, examples and comparative examples will be described. The present disclosure is not limited in any way by the following examples and comparative examples.
[0129] Fig. 17 is a diagram showing the configurations and results of the examples and comparative examples. Fig. 18 is a diagram showing the lamination patterns of the metal sheets in the examples and comparative examples. "Pattern 1" to "Pattern 4" in Fig. 18 correspond to "Pattern 1" to "Pattern 4" shown in "Lamination Pattern" in Fig. 17.
[0130] Example 1 In Example 1, a lithium secondary battery having the structure shown in FIG. 1 was fabricated. First, a negative electrode 10 having the structure shown in FIG. 2B was prepared. A 6 μm-thick polyethylene terephthalate (PET) was used as the negative electrode insulating layer 160 of the negative electrode current collector 16, and 1.0 μm of Cu was vapor-deposited as the negative electrode conductive layer 162. The negative electrode active material 14 was a mixture of 97 parts by mass of graphite, 0.5 parts by mass of carbon black as a conductive additive, and 1.5 parts by mass of carboxymethyl cellulose (CMC) and 1.0 part by mass of styrene-butadiene rubber (SBR) as binders, mixed with water as a solvent. Thus, 21 negative electrodes 10 were prepared. Then, a negative electrode metal sheet MS2 (4 μm-thick copper foil) was attached to the negative electrode end Q of each negative electrode 10 by ultrasonic welding, resulting in the structure shown in FIG. 11 . Next, as the separator 20, polyvinylidene fluoride (PVDF) and Al 2 O 3 A sheet (thickness: 15 μm) whose surface was coated with the mixture was prepared. Then, both sides of the negative electrode 10 were sandwiched between separators 20 and pressed together to obtain an intermediate laminate LM.
[0131] The current collector 32 of the positive electrode laminate 30 was a 6 μm thick polyethylene terephthalate (PET) film with an insulating layer 320 and a 1.0 μm thick conductive layer 322 of Al vapor-deposited on both sides. The positive electrode 34 was made of N-methyl-pyrrolidone (NMP) as a solvent and LiNi as a positive electrode active material. 0.8 Co 0.15 Al 0.05 O 2 The positive electrode 34 was applied to both sides of the current collector 32 so as to have a basis weight of 23 mg / cm. 2A positive electrode laminate 30 was obtained by applying the solution of 0.2 mm nickel to the cathode laminate 30. Twenty positive electrode laminates 30 were prepared. A metal sheet MS (12 μm hard aluminum) having the configuration shown in "Example 1" of FIG. 17 was attached to the end P of the current collector 32 of each of the ten positive electrode laminates 30 by ultrasonic welding. A positive electrode tab 40 (0.2 mm thick) made of the material (hard aluminum) shown in "Example 1" of FIG. 17 was also prepared. Nickel-plated copper having a thickness of 0.2 mm was used as the negative electrode tab 42.
[0132] Next, intermediate laminates LM and positive electrode laminates 30 were alternately stacked. At this time, positive electrode laminates 30 with metal sheets MS attached to their end portions P and positive electrode laminates 30 without metal sheets MS attached were appropriately selected to form the stacking pattern (pattern 1) shown in FIG. 18 . Then, each end portion P of the current collector 32 was overlapped with the metal sheet MS and joined to the positive electrode tab 40 by ultrasonic welding. Furthermore, the negative electrode end portion Q was overlapped with the negative electrode metal sheet MS2 and joined to the negative electrode tab 42 by ultrasonic welding. This structure was inserted into a laminate outer casing and sealed together with an electrolyte to obtain a lithium secondary battery. The electrolyte was prepared by dissolving lithium hexafluorophosphate (LiPF ) in a solvent containing a 30:35:35 mass part mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) to a concentration of 1 M. 6 The electrolyte used was prepared by dissolving 2 parts by weight of vinylene carbonate (VC) in the electrolyte.
[0133] (Examples 2 to 8) In Examples 2 to 8, as shown in Figures 17 and 18, lithium secondary batteries were produced in the same manner as in Example 1, except that the material and thickness of the metal sheet MS, the material of the positive electrode tab 40, and the lamination pattern of the metal sheet MS were different.
[0134] Comparative Example 1 In Comparative Example 1, a lithium secondary battery was produced in the same manner as in Example 1, except that the metal sheet MS was not used.
[0135] 17, "X / Y" is the value obtained by dividing X by Y, where X (=A+B) is the sum of the total thickness (A) of each metal sheet MS and the total thickness (B) of each conductive layer 322, and Y is the total thickness of each insulating layer 320, for Examples 1 to 8. In Comparative Example 1, no metal sheet MS was used, so X is the total thickness of each conductive layer.
[0136] In FIG. 17 , “resistance [mΩ]” is the resistance at the second bonding mark WR2. The lithium secondary batteries according to the examples and comparative examples were disassembled and measured using a four-terminal method. Specifically, the positive terminal of a clip-type lead of a HIOKI BT3561 resistance meter was connected to the positive electrode tab 40, and the negative terminal of one of the 20 positive electrode laminates 30 was clipped with a clip at a location on the positive electrode laminate where the positive electrode active material was not applied, and the impedance at 1 kHz was measured using the four-terminal lead. Next, the negative terminal was connected to another positive electrode laminate, and measurements were conducted, and the average value of the 20 values was calculated. This average value is the “resistance (mΩ)” shown in FIG. 17 . As shown in FIG. 17 , the resistance at the second bonding mark WR2 in Examples 1 to 8 was significantly lower than that in Comparative Example 1.
[0137] A nail penetration test was conducted on the lithium secondary batteries according to Examples 1 to 8 and Comparative Example 1, and no fire or explosion occurred in any of them. The nail penetration test is a test in which a nail is penetrated into each battery to simulate an internal short circuit and check whether the battery will fire or explode.
[0138] Comparative Example 2 In Comparative Example 2, a lithium secondary battery was fabricated in the same manner as in Example 1, except that the metal sheet MS2 for the negative electrode was not used.
[0139] In Example 1 and Comparative Example 2, the resistance at the joint region between the negative electrode tab 42 and the negative electrode end Q was measured in the same manner as described above. In Comparative Example 2, the resistance was 19.4 mΩ. In contrast, in Example 1, the resistance was 0.88 mΩ, which was significantly lower than that of Comparative Example 2.
[0140] Embodiments of the present disclosure further include the following aspects.
[0141] (Supplementary Note 1) A lithium secondary battery comprising: (a) a first laminate including a first current collector formed by sandwiching a first insulating layer between a pair of first conductive layers, and a first electrode disposed on the first current collector, the first current collector having a first end where the first electrode is not disposed; (b) an intermediate laminate including an electrode having a polarity different from that of the first electrode and a separator; (c) a second laminate disposed in a stacking direction apart from the first laminate via the intermediate laminate, the second laminate including a second current collector formed by sandwiching a second insulating layer between a pair of second conductive layers, and a second electrode disposed on the second current collector and having the same polarity as the first electrode, the second current collector having a second end where the second electrode is not disposed; and (d) a metal sheet disposed alongside the first end and the second end in the stacking direction, the metal sheet having a first joining mark resulting from joining to either the first end or the second end. (e) an electrode tab electrically connected to the first stack and the second stack, the electrode tab having a second bonding mark formed by bonding the first end, the metal sheet, and the second end, the second bonding mark being located at a different position from the first bonding mark when viewed from the stacking direction.
[0142] (Supplementary Note 2) The lithium secondary battery according to Supplementary Note 1, wherein the first joining mark is a welding mark.
[0143] (Supplementary Note 3) The lithium secondary battery according to Supplementary Note 1 or Supplementary Note 2, wherein the first bonding mark has one or more line shapes.
[0144] (Supplementary Note 4) The lithium secondary battery according to Supplementary Note 1 or Supplementary Note 2, wherein the first bonding marks are in the form of one or more dots.
[0145] (Supplementary Note 5) The lithium secondary battery according to any one of Supplementary Note 1 to Supplementary Note 4, wherein the second joining mark is a welding mark.
[0146] (Supplementary Note 6) The lithium secondary battery according to any one of Supplementary Notes 1 to 5, wherein the second bonding marks are in the form of one or more lines.
[0147] (Supplementary Note 7) The lithium secondary battery according to any one of Supplementary Notes 1 to 5, wherein the second bonding marks are in the form of one or more dots.
[0148] (Supplementary Note 8) The lithium secondary battery according to any one of Supplementary Note 1 to Supplementary Note 7, wherein the second joining marks include, in a cross section in the stacking direction, a region where the pair of first conductive layers, the metal sheet, and the pair of second conductive layers are integrated.
[0149] (Supplementary Note 9) The lithium secondary battery according to any one of Supplementary Note 1 to Supplementary Note 8, wherein the first bonding mark and the second bonding mark do not overlap each other when viewed from the stacking direction.
[0150] (Supplementary Note 10) The lithium secondary battery according to any one of Supplementary Note 1 to Supplementary Note 9, wherein a plurality of the first stacked bodies and the second stacked bodies are arranged alternately in the stacking direction with the intermediate stacked body sandwiched therebetween.
[0151] (Appendix 11) The lithium secondary battery according to appendix 10, wherein the first laminate is formed of a flat sheet, and the second laminate is formed of a flat sheet separate from the first laminate.
[0152] (Appendix 12) The lithium secondary battery according to appendix 10, wherein the first laminate and the second laminate are formed by folding or rolling a single sheet.
[0153] (Supplementary Note 13) The lithium secondary battery according to any one of Supplementary Note 10 to Supplementary Note 12, wherein the first stacked body and the second stacked body are arranged in a total of 10 or more layers.
[0154] (Supplementary Note 14) The lithium secondary battery according to any one of Supplementary Note 10 to Supplementary Note 13, wherein the metal sheet is provided on at least one end of the plurality of first ends and the plurality of second ends.
[0155] (Supplementary Note 15) The lithium secondary battery according to Supplementary Note 14, wherein the metal sheet is provided on one side of the at least one end portion.
[0156] (Supplementary Note 16) The lithium secondary battery according to Supplementary Note 14, wherein the metal sheets are provided one on each side of the at least one end portion.
[0157] (Supplementary Note 17) The lithium secondary battery according to any one of Supplementary Note 10 to Supplementary Note 16, wherein the number of the metal sheets is three times or less the total number of the first end portions and the second end portions.
[0158] (Supplementary Note 18) The lithium secondary battery according to any one of Supplementary Note 1 to Supplementary Note 17, wherein the metal sheet is made of the same material as the first conductive layer and the second conductive layer.
[0159] (Supplementary Note 19) The lithium secondary battery according to any one of Supplementary Note 1 to Supplementary Note 18, wherein the first electrode and the second electrode are positive electrodes.
[0160] (Supplementary Note 20) The lithium secondary battery according to any one of Supplementary Note 1 to Supplementary Note 18, wherein the first electrode and the second electrode are negative electrodes.
[0161] 1... Lithium secondary battery, 10... Negative electrode, 20... Separator, 30... Positive electrode laminate, 32... Current collector, 320... Insulating layer, 322... Conductive layer, 34... Positive electrode, 40... Positive electrode tab, 42... Negative electrode tab, MS... Metal sheet, LM... Intermediate laminate, WR1... First bonding mark, WR2... Second bonding mark
Claims
1. A lithium secondary battery comprising: (a) a first stack, the first stack including a first current collector having a first insulating layer sandwiched between a pair of first conductive layers, and a first electrode disposed on the first current collector, the first current collector having a first end where the first electrode is not disposed; (b) an intermediate stack including an electrode having a polarity different from that of the first electrode and a separator; (c) a second stack disposed in a stacking direction spaced apart from the first stack via the intermediate stack, the second stack including a second current collector having a second insulating layer sandwiched between a pair of second conductive layers, and a second electrode disposed on the second current collector and having the same polarity as the first electrode, the second current collector having a second end where the second electrode is not disposed; and (d) a metal sheet disposed in line with the first end and the second end in the stacking direction, the metal sheet having a first bonding mark resulting from bonding to either the first end or the second end. (e) an electrode tab electrically connected to the first stack and the second stack, the electrode tab having a second joint mark formed by joining the first end, the metal sheet, and the second end, the second joint mark being located in a different position from the first joint mark when viewed from the stacking direction.
2. The lithium secondary battery according to claim 1, wherein the first joining mark is a welding mark.
3. The lithium secondary battery according to claim 2, wherein the first bonding mark is in the form of one or more lines.
4. The lithium secondary battery according to claim 2, wherein the first bonding mark is in the form of one or more dots.
5. The lithium secondary battery according to claim 1, wherein the second joining mark is a welding mark.
6. The lithium secondary battery according to claim 5, wherein the second bonding mark is in the form of one or more lines.
7. The lithium secondary battery according to claim 5, wherein the second bonding mark is in the form of one or more dots.
8. A lithium secondary battery as described in claim 1, wherein the second bonding marks include, in a cross section in the stacking direction, an area where the pair of first conductive layers, the metal sheet, and the pair of second conductive layers are integrated.
9. The lithium secondary battery according to claim 1, wherein the first bonding mark and the second bonding mark do not overlap each other when viewed from the stacking direction.
10. A lithium secondary battery according to any one of claims 1 to 9, wherein a plurality of the first laminates and the second laminates are arranged alternately in the stacking direction with the intermediate laminate sandwiched between them.
11. The lithium secondary battery according to claim 10, wherein the first laminate is formed of a flat sheet, and the second laminate is formed of a flat sheet separate from the first laminate.
12. The lithium secondary battery according to claim 10, wherein the first laminate and the second laminate are formed by folding or rolling a single sheet.
13. The lithium secondary battery according to claim 10, wherein a total of 10 or more layers of the first laminate and the second laminate are arranged.
14. The lithium secondary battery according to claim 10, wherein the metal sheet is provided on at least one of the plurality of first ends and the plurality of second ends.
15. The lithium secondary battery according to claim 14, wherein the metal sheet is provided on one side of the at least one end portion.
16. The lithium secondary battery according to claim 14, wherein the metal sheets are provided one on each side of the at least one end portion.
17. The lithium secondary battery according to claim 10, wherein the number of said metal sheets is three times or less the total number of said first ends and said second ends.
18. A lithium secondary battery according to any one of claims 1 to 9, wherein the metal sheet is made of the same material as the first conductive layer and the second conductive layer.
19. A lithium secondary battery according to any one of claims 1 to 9, wherein the first electrode and the second electrode are positive electrodes.
20. A lithium secondary battery according to any one of claims 1 to 9, wherein the first electrode and the second electrode are negative electrodes.
Citation Information
Patent Citations
Thin film magnetic head
JP1989102711A
Collector and nonaqueous secondary battery
JP2013016321A
Nonaqueous secondary battery
JP2012129114A
Nonaqueous secondary battery
JP2012185938A