Curable liquid silicone composition and cured product thereof
The curable liquid silicone composition, featuring diorganopolysiloxane, organohydrogenpolysiloxane, and a platinum catalyst mixture, addresses storage stability and curing efficiency issues by using atmospheric moisture for room temperature curing, enhancing applicability and energy efficiency.
Patent Information
- Application Number
- PCT/JP2024/010738
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing one-component silicone compositions face challenges with storage stability at room temperature and curing efficiency, particularly in dark areas without UV irradiation, and require high-temperature heating processes, which are energy-intensive and limit their applications.
A curable liquid silicone composition comprising a linear or branched diorganopolysiloxane, organohydrogenpolysiloxane, a platinum catalyst mixture with a phosphite compound, and a hydrolysis reaction catalyst, which cures at room temperature due to atmospheric moisture, ensuring stability and efficient curing without heating, and can be further enhanced with a platinum catalyst activated by UV light for improved curing rates.
The composition exhibits long-term storage stability at room temperature, enables curing in dark areas, and reduces energy consumption by avoiding high-temperature processes, while improving workability and curing speed through UV activation, making it suitable for various applications like sealants and adhesives.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Curable liquid silicone composition and cured product thereof
[0001] The present invention relates to a curable liquid silicone composition that exhibits one-component storage stability in a sealed container at room temperature (23°C±15°C, the same applies hereinafter) and that can be cured by exposure to atmospheric moisture at room temperature to give a cured silicone rubber (elastic silicone elastomer) or a cured silicone gel, as well as to a cured product of the composition.
[0002] In order to achieve carbon neutrality by 2050, various companies are promoting the use of environmentally friendly materials. In particular, improvements are being sought for heat-curing compositions, which involve high-temperature heating processes that require a huge amount of energy, time, and equipment. In addition, one-component materials are becoming more popular for their ease of use and to prevent errors during use.
[0003] Among the one-component crosslinking reactions that can be cured without heating, there are condensation reactions, UV radical reactions, and addition reactions that have significantly shorter shelf lives, and some that can be activated by UV light. However, all of these have poor deep curing properties or curing properties in dark areas exposed to UV light, limiting the applications in which they can be used.
[0004] Among these, among the technologies that cure silicone compositions into rubber or gel by crosslinking using an addition reaction with a platinum catalyst, the following technologies aim to improve the shelf life and usable life of the unreacted one-part composition and to cure at lower temperatures.
[0005] Japanese Patent No. 2722304 (Patent Document 1) proposes a method of adding an amine compound with an ethylenediamine skeleton to a silicone composition that cures by crosslinking using a platinum-catalyzed addition reaction. Japanese Patent No. 4530147 (Patent Document 2) proposes a method of using a catalyst in which a specific phosphite ester compound is heated and aged with a platinum catalyst.
[0006] However, silicone compositions obtained using the above techniques tend to thicken and gel when exposed to temperatures above 50°C for extended periods of time, and therefore require low-temperature conditions during storage and transportation to maintain performance stability.
[0007] To solve these problems, WO 2022 / 050103 (Patent Document 3) proposes a one-component silicone composition that exhibits stable properties and characteristics even when exposed to temperatures exceeding 50° C. for extended periods by adding a specific phosphite triester compound to a branched organopolysiloxane and organohydrogenpolysiloxane having a specific structure and a platinum catalyst. However, heating to approximately 100 to 160° C. is necessary to cure the composition in a short period of time.
[0008] Japanese Patent No. 2722304 Japanese Patent No. 4530147 International Publication No. 2022 / 050103 U.S. Patent No. 3,220,972 U.S. Patent No. 3,159,601 U.S. Patent No. 3,159,662 U.S. Patent No. 3,775,452 U.S. Patent No. 4,510,094 U.S. Patent No. 4,530,879
[0009] The present invention has been made in view of the above circumstances, and has as its object to provide a curable liquid silicone composition that can be stored in a sealed container as a single component at room temperature and that can be cured to form a cured silicone rubber or cured silicone gel when used in the presence of moisture at room temperature without heating, as well as a cured product thereof.
[0010] As a result of extensive research conducted by the present inventors in order to achieve the above-mentioned object, they discovered that a curable liquid silicone composition containing a linear or branched diorganopolysiloxane having at least one alkenyl group per molecule, a linear or branched organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule, a platinum catalyst mixture containing a platinum catalyst and a specific amount of a phosphite ester compound, and a hydrolysis reaction catalyst in a specific ratio, exhibits one-part storage stability at room temperature in a sealed container, and cures at room temperature due to atmospheric moisture during use without heating, leading to the completion of the present invention.
[0011] The curable liquid silicone composition of the present invention cures at room temperature without heating due to atmospheric moisture during use, and therefore can be cured even in areas where curing is difficult, such as dark areas that are not irradiated with ultraviolet light, which is a problem with ultraviolet-curable liquid silicone compositions.
[0012] Accordingly, the present invention provides a curable liquid silicone composition that can be cured to give a cured silicone rubber (elastic silicone elastomer) or a cured silicone gel, as well as the cured product thereof, as shown below. [1] A curable liquid silicone composition comprising: (A) a linear or branched diorganopolysiloxane having at least one alkenyl group per molecule, (B) a linear or branched organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms per molecule, in an amount such that there are 0.5 to 4 moles of silicon-bonded hydrogen atoms in component (B) per mole of alkenyl groups in component (A), (C) a platinum catalyst mixture containing a platinum catalyst and a phosphite ester compound in an amount of 0.5 to 3 moles per mole of platinum atoms, in an amount such that the platinum atoms in component (C) are 0.1 to 1,000 ppm by mass relative to the combined mass of components (A) and (B), and (D) a hydrolysis reaction catalyst in an amount of 0.01 to 3 mass% of the combined mass of components (A) and (B). [2] The curable liquid silicone composition according to [1], which is a one-component composition. [3] The curable liquid silicone composition according to [1] or [2], further comprising: (E) a dehydrating agent in an amount of 0.01 to 5% by mass of the total mass of components (A) and (B). [4] The curable liquid silicone composition according to any one of [1] to [3], further comprising: (F) a platinum catalyst compound activated by ultraviolet light in an amount such that the platinum atoms in component (F) are 0.1 to 1,000 ppm by mass relative to the total mass of components (A) and (B). [5] The curable liquid silicone composition according to any one of [1] to [4], further comprising: (G) a photoinitiator in an amount of 0.01 to 3% by mass of the total mass of components (A) and (B). [6] A cured product of the curable liquid silicone composition according to any one of [1] to [5].
[0013] The curable liquid silicone composition of the present invention exhibits one-part shelf life at room temperature in a sealed container and cures during use with atmospheric moisture at room temperature without heating. During use, the phosphite ester compound, which functions as a platinum catalyst inhibitor, is hydrolyzed upon contact with atmospheric moisture (humidity) in the presence of a hydrolysis catalyst to form a phosphonic acid, which no longer functions as an inhibitor. The platinum catalyst is activated and acts as a hydrosilylation addition reaction catalyst, resulting in curing. The curable liquid silicone composition of the present invention exhibits "long-term one-part shelf life at room temperature in a sealed container," sufficient for storage and transportation at refrigerated to room temperature, and cures during use without heating at room temperature in the atmosphere, contributing to energy conservation and the production of parts and products in line with the SDGs. Furthermore, the addition of a platinum catalyst that is activated by ultraviolet light and the application of ultraviolet light during curing can also improve the curing reaction rate and enhance workability.
[0014] 1 is a schematic diagram showing an ultraviolet irradiation method in measuring shadow curing property in an example of the present invention. FIG. 2 is a schematic diagram showing evaluation sites in measuring shadow curing property in an example of the present invention.
[0015] The present invention will be described in detail below.
[0016] [Curable Liquid Silicone Composition] The curable liquid silicone composition of the present invention (curable liquid silicone rubber composition or curable liquid silicone gel composition) is a blend of components (A) to (D) described below, and, if necessary, other components.
[0017] [(A) Alkenyl Group-Containing Diorganopolysiloxane] The alkenyl group-containing diorganopolysiloxane of component (A) is a linear or branched diorganopolysiloxane having at least one alkenyl group per molecule, and serves as the main component (base polymer) of the curable liquid silicone composition of the present invention (hereinafter also referred to as the composition of the present invention). Typically, it is a linear diorganopolysiloxane whose main chain is basically composed of repeating diorganosiloxane units and whose molecular chain is terminated at both ends with triorganosiloxy groups, and it may also be a branched diorganopolysiloxane containing a branched structure in part of the siloxane structure that makes up the molecular chain.
[0018] The alkenyl-containing diorganopolysiloxane of component (A) contains at least one alkenyl group (usually 1 to 50), preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 or 2 alkenyl groups per molecule. Examples of alkenyl groups include vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, and cyclohexenyl, which typically have about 2 to 8 carbon atoms. The alkenyl group may be bonded to a silicon atom at a molecular chain terminal or to a silicon atom at a non-terminal end (in the middle of the molecular chain). Preferably, the alkenyl group contains alkenyl groups bonded to silicon atoms at at least (both) molecular chain terminals. In this case, the alkenyl groups may be present only at (both) molecular chain terminals, or may be present at (both) molecular chain terminals and non-terminal end (in the middle of the molecular chain).
[0019] Examples of such alkenyl group-containing diorganopolysiloxanes include linear diorganopolysiloxanes represented by the following general formula (1). (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups that do not contain aliphatic unsaturated bonds. X is an alkenyl group, and at least one is contained in one molecule. n is an integer of 0 or greater, m is an integer of 0 or greater, and a is an integer of 0 to 3 for each silicon atom to which it is bonded, with at least one of a and m at both ends being an integer of 1 or greater.
[0020] In the above formula (1), R 1 Examples of the unsubstituted or substituted monovalent hydrocarbon group not containing an aliphatic unsaturated bond include those having 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 6 carbon atoms. Specific examples include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenylyl; aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl; and carbon atoms of these groups. Examples of such groups include groups in which some or all of the hydrogen atoms bonded to an atom have been substituted with halogen atoms such as fluorine, chlorine or bromine, or with a cyano group, such as a chloromethyl group, a 2-bromoethyl group, a 3-chloropropyl group, a 3,3,3-trifluoropropyl group, a chlorophenyl group, a fluorophenyl group, a cyanoethyl group or a 3,3,4,4,5,5,6,6,6-nonafluorohexyl group, and the like. Preferred are unsubstituted or substituted alkyl groups having 1 to 3 carbon atoms such as a methyl group, an ethyl group, a propyl group, a chloromethyl group, a bromoethyl group, a 3,3,3-trifluoropropyl group or a cyanoethyl group, and unsubstituted or substituted phenyl groups such as a phenyl group, a chlorophenyl group or a fluorophenyl group, and more preferred are a methyl group and a phenyl group.
[0021] In the above formula (1), examples of the alkenyl group for X include those having about 2 to 8 carbon atoms, such as a vinyl group, an allyl group, a propenyl group, an isopropenyl group, a butenyl group, a hexenyl group, and a cyclohexenyl group. Of these, lower alkenyl groups such as a vinyl group and an allyl group are preferred.
[0022] In the above formula (1), n is an integer of 0 or greater, preferably an integer of 10 to 2,000, more preferably an integer of 50 to 1,200, and m is an integer of 0 or greater, preferably an integer of 0 to 40, more preferably an integer of 0 to 20. Furthermore, n and m are preferably integers that satisfy 10≦n+m≦2,000, more preferably 50≦n+m≦1,200, and are integers that satisfy 0≦m / (n+m)≦0.2. In this case, the units in parentheses enclosed by n and m may be arranged randomly. In the above formula (1), a is an integer of 0 to 3, preferably 0 or 1, for each silicon atom to be bonded.
[0023] The alkenyl group-containing diorganopolysiloxane may be, for example, a diorganopolysiloxane having a monofunctional siloxy unit (X a R 1 (3-a) SiO 1 / 2 unit) and difunctional siloxane units ((X)(R 1 ) SiO 2 / 2 Units, (R 1 ) SiO 2 / 2 In addition to the trifunctional siloxane unit (i.e., (R 1 ) SiO 3 / 2 or (X) SiO 3 / 2 Examples of suitable branched diorganopolysiloxanes include those having a small amount of silsesquioxane units represented by the following formula (II) in the molecule.
[0024] Furthermore, it is preferable that such alkenyl-containing diorganopolysiloxanes have a viscosity at 23°C of about 10 to 1,000,000 mPa·s, and particularly about 100 to 500,000 mPa·s.
[0025] In the present invention, the number of repeating diorganosiloxane units (or degree of polymerization) per molecule can be determined as the polystyrene-equivalent number average molecular weight (or number average degree of polymerization) by gel permeation chromatography (GPC) analysis using toluene or the like as a developing solvent. Viscosity can be measured using a rotational viscometer (e.g., BL type, BH type, BS type, cone-plate type, rheometer, etc.) at 23°C.
[0026] The alkenyl group-containing diorganopolysiloxane of component (A) may be used alone or in combination of two or more types. Furthermore, in order to prevent variations in storage stability due to differences in the water content in the composition, it is advisable to reduce the water content in the alkenyl group-containing diorganopolysiloxane of component (A) before blending it into the composition, and this is desirably done by, for example, heating, reducing pressure, or a combination of these methods.
[0027] [(B) Organohydrogenpolysiloxane] The organohydrogenpolysiloxane of component (B) is a linear or branched (branched or three-dimensional network structure (resin structure)) organohydrogenpolysiloxane having at least two (typically 2 to 200), and preferably about 2 to 100, hydrogen atoms bonded to silicon atoms (SiH groups) per molecule, and functions as a curing agent (crosslinking agent) for the curable liquid silicone composition of the present invention.
[0028] Examples of such organohydrogenpolysiloxanes include linear or branched organohydrogenpolysiloxanes represented by the following average composition formula (2). (In the formula, R 2 are independently an unsubstituted or substituted monovalent hydrocarbon group containing no aliphatic unsaturated bonds, and b and c are numbers that satisfy 0.001≦b≦1.2, 0.8≦c≦2, and 0.8<b+c≦3, and preferably 0.05≦b≦1, 1.2≦c≦2, and 1.5≦b+c≦2.7.
[0029] In the above formula (2), R 2 The unsubstituted or substituted monovalent hydrocarbon group not containing an aliphatic unsaturated bond includes R 1 Examples include those having 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 7 carbon atoms, and particularly preferred are lower alkyl groups having 1 to 3 carbon atoms such as a methyl group, a phenyl group, and a 3,3,3-trifluoropropyl group.
[0030] Component (B) is preferably a compound that is liquid at room temperature (23°C ± 15°C, hereinafter the same) and has 2 to 300 silicon atoms per molecule, particularly 3 to 150, and especially about 3 to 100. The hydrogen atoms bonded to the silicon atoms may be located at either the terminals of the molecular chain, midway along the molecular chain (non-terminal), or both.
[0031] Examples of such organohydrogenpolysiloxanes include 1,1,3,3-tetramethyldisiloxane, 1,1,3,3,5,5-hexamethyltrisiloxane, tris(dimethylhydrogensiloxy)methylsilane, tris(dimethylhydrogensiloxy)phenylsilane, methylhydrogenpolysiloxanes terminally blocked with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymers terminally blocked with trimethylsiloxy groups, diphenylsiloxane-methylhydrogensiloxane copolymers terminally blocked with trimethylsiloxy groups, methylphenylsiloxane-methylhydrogensiloxane copolymers terminally blocked with trimethylsiloxy groups, and dimethylsiloxane-diphenylsiloxane copolymers terminally blocked with trimethylsiloxy groups. and methylhydrogensiloxane copolymer, dimethylpolysiloxane terminally blocked with dimethylhydrogensiloxy groups, methylhydrogenpolysiloxane terminally blocked with dimethylhydrogensiloxy groups, dimethylsiloxane and methylhydrogensiloxane copolymer terminally blocked with dimethylhydrogensiloxy groups, diphenylsiloxane and methylhydrogensiloxane copolymer terminally blocked with dimethylhydrogensiloxy groups, methylphenylsiloxane and methylhydrogensiloxane copolymer terminally blocked with dimethylhydrogensiloxy groups, dimethylsiloxane, diphenylsiloxane and methylhydrogensiloxane copolymer terminally blocked with dimethylhydrogensiloxy groups, and dimethylhydrogensiloxy units and SiO 4 / 2Examples of such silicone resins include silicone resins having a three-dimensional network structure consisting of units and which may optionally contain trimethylsiloxy units, dimethylsiloxane units, methylhydrogensiloxane units, hydrogensilsesquioxane units, and / or methylsilsesquioxane units, and compounds in which some or all of the methyl groups in the above-mentioned exemplary compounds have been substituted with other alkyl groups or phenyl groups.
[0032] The linear or branched organohydrogenpolysiloxane used in the composition of the present invention can be obtained by known methods, for example, a compound represented by the following general formula: 2 SiHCl2 and R 2 2SiHCl (wherein R 2 is the same as above.) or by (co)hydrolytic condensation of the chlorosilane with a compound represented by the following general formula: R 2 3SiCl and R 2 2SiCl2 (wherein, R 2 are the same as above.) and at least one chlorosilane selected from the group consisting of chlorosilanes ...
[0033] From the viewpoint of providing a good silicone rubber and gel upon curing, the amount of organohydrogenpolysiloxane of component (B) blended is an amount such that the number of hydrogen atoms bonded to silicon atoms (i.e., SiH groups) in the organohydrogenpolysiloxane of component (B) is 0.5 to 4 moles, and preferably 0.8 to 2.5 moles, per mole of alkenyl groups in the alkenyl group-containing diorganopolysiloxane of component (A).
[0034] The organohydrogenpolysiloxane of component (B) may be used alone or in combination of two or more. Furthermore, in order to prevent variations in storage stability due to differences in the water content in the composition, it is advisable to reduce the water content in the organohydrogenpolysiloxane of component (B) before blending it into the composition. This can be done, for example, by heating, reducing pressure, or a combination of these methods.
[0035] [(C) Platinum catalyst mixture containing a platinum catalyst and a phosphite ester compound] The platinum catalyst mixture of component (C) contains a platinum catalyst and a phosphite ester compound in an amount of 0.5 to 3 moles per mole of platinum atom, with the phosphite ester compound inhibiting activation of the platinum catalyst. When the composition is in use, the phosphite ester compound undergoes hydrolysis with moisture in the air to form phosphonic acid, which prevents it from functioning as a regulator, thereby activating the platinum catalyst and allowing it to act as a hydrosilylation addition reaction catalyst.
[0036] The platinum catalyst used in component (C) is a catalyst containing platinum or a platinum compound that has conventionally been used to promote hydrosilylation addition reactions. Specific examples include, for example, platinum (including platinum black) alone; platinum chlorides such as HPtCl.xH0, HPtCl.xH0, NaHPtCl.xH0, KHPtCl.xH0, NaPtCl.xH0, KPtCl.xH0, PtCl.xH0, PtCl, and NaHPtCl.xH0 (wherein x is an integer of 0 to 6, preferably 0 or 6); Examples of such a complex include platinic acid and chloroplatinic acid salts; alcohol-modified chloroplatinic acid (see U.S. Pat. No. 3,220,972 (Patent Document 4)); complexes of chloroplatinic acid with olefins (see U.S. Pat. Nos. 3,159,601 (Patent Document 5), 3,159,662 (Patent Document 6), and 3,775,452 (Patent Document 7)); complexes of platinum chloride, chloroplatinic acid, or chloroplatinic acid salts with vinyl group-containing siloxanes, particularly vinyl group-containing cyclic siloxanes; and complexes of platinum with alcohols or vinyl group-containing siloxanes.
[0037] The platinum catalyst is preferably used by dissolving it in a solvent such as toluene, a lower alcohol, a higher alcohol, a silicone-based solvent, etc. In this case, the platinum atom content (concentration) in the solution is preferably 0.1 to 2 mass %.
[0038] Examples of the phosphite ester compound used in component (C) include those represented by the following general formula (3). (In the formula, R3 are independently a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, and Y is independently a hydrogen atom or a methyl group.
[0039] In the above formula (3), R 3 is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclohexyl, octyl, and decyl, and alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and isobutenyl. A monovalent hydrocarbon group having no aliphatic unsaturated bond is desirable, and among these, alkyl groups are preferred, with methyl, ethyl, and propyl being particularly preferred. 3 In the formula (3), Y is a hydrogen atom or a methyl group, and a hydrogen atom is preferred.
[0040] Specific examples of the phosphite ester compound having the structure represented by formula (3) above include triisopropyl phosphite, tri(tert-butyl phosphite), tri(sec-butyl phosphite), tris(1-ethylpropyl phosphite), tris(1-ethylbutyl phosphite), and tris(1-propylbutyl) phosphite.
[0041] The amount of the phosphite ester compound added is 0.5 to 3 moles per mole of platinum atoms in the platinum catalyst. If the amount of the phosphite ester compound is less than 0.5 moles per mole of platinum atoms, the control ability of the platinum catalyst decreases, and the one-component storage stability at room temperature decreases. Furthermore, if the amount of the phosphite ester compound exceeds 3 moles per mole of platinum atoms, there will be a large amount of phosphite ester compound capable of coordinating with the platinum atoms, which will require time for the platinum catalyst to activate and act as a hydrosilylation addition reaction catalyst, resulting in decreased moisture (aerobic) curability. A preferred amount of the phosphite ester compound added is 0.8 to 2 moles, more preferably 1.0 to 1.3 moles, per mole of platinum atoms in the platinum catalyst.
[0042] A platinum catalyst mixture containing a platinum catalyst and a phosphite ester compound can be obtained, for example, by uniformly mixing the platinum catalyst and the phosphite ester compound under a nitrogen atmosphere at room temperature (23° C.) and allowing the mixture to stand for 24 hours or more for aging. When preparing the platinum catalyst mixture, it is desirable to dissolve the platinum catalyst and the phosphite ester compound in a solvent as needed.
[0043] The amount of the platinum catalyst mixture containing the platinum catalyst and phosphite compound of component (C) is, in terms of the mass of platinum atoms, 0.1 to 1,000 ppm, preferably 1 to 300 ppm, relative to the total mass of components (A) and (B). If component (C) is too little, the curable liquid silicone composition will not cure, whereas if it is too much, the probability of the platinum catalyst being activated increases, significantly reducing the one-part storage stability of the composition.
[0044] [(D) Hydrolysis Reaction Catalyst] The hydrolysis reaction catalyst of component (D) is a catalyst that accelerates the hydrolysis reaction of the phosphite ester compound in component (C). During use, in the presence of the hydrolysis reaction catalyst of component (D), the curable liquid silicone composition of the present invention cures by hydrolyzing the phosphite ester compound, which functioned as an inhibitor for the platinum catalyst in component (C), with moisture (humidity) in the air to form phosphonic acid, which no longer functions as an inhibitor, activating the platinum catalyst and acting as a hydrosilylation addition reaction catalyst.
[0045] Examples of the hydrolysis reaction catalyst for component (D) include metal compounds such as titanate esters (tetra(isopropyl)titanate (TPT), tetrabutyl titanate (TBT), tetra(2-ethylhexyl)titanate (TOT), etc.), titanium chelate compounds (titanium diisopropoxybis(ethylacetoacetate), titanium tetraacetylacetonate, etc.), and tin compounds (dibutyldimethoxytin, dibutyltin dilaurate, etc.).
[0046] The amount of component (D) added is preferably 0.01 to 3 mass%, particularly preferably 0.01 to 1 mass%, of the total mass of components (A) and (B). If the amount added is less than 0.01 mass%, the effect as a hydrolysis reaction catalyst will be insufficient, and if it exceeds 3 mass%, the one-component storage stability at room temperature will decrease.
[0047] [Other Components] In addition to the components (A) through (D) described above, the curable liquid silicone composition of the present invention can contain various optional components, as described below, as needed, provided that the object of the present invention is not impaired.
[0048] [(E) Dehydrating Agent] The curable liquid silicone composition of the present invention can further contain, as an optional component, a dehydrating agent (component (E)) to remove water from the composition, if necessary. By incorporating a dehydrating agent (component (E)), it becomes possible to obtain even better storage stability.
[0049] As described above, the curable liquid silicone composition of the present invention exhibits one-component storage stability at room temperature in a sealed container, and can be cured at room temperature by atmospheric moisture when in use without heating. For this reason, it has been confirmed that the one-component storage stability of the curable liquid silicone composition can be improved by reducing the amount of water in each component and in the mixed composition, and it is useful in ensuring one-component storage stability to introduce a mechanism (dehydration using a dehydrating agent (E)) that consumes the water derived from each component in the composition and the trace amounts of water that enter from outside the container within the composition when stored in a sealed container.
[0050] The dehydrating agent for component (E) may be either an inorganic or organic compound, so long as it does not impair the functions of components (A), (B), (C), and (D). However, depending on the dehydrating agent, compounds produced as by-products in the dehydration reaction may cause foaming, and many dehydrating agents also cause decomposition of the organohydrogenpolysiloxane for component (B) or a decrease in the catalytic activity of the platinum catalyst in component (C).
[0051] Therefore, silyl ketenes (including silyl ketene acetals), silyl enol esters, and α-silyl esters are suitable as dehydrating agents for component (E), as they enable efficient in-system dehydration. These compounds have a structure such that the by-products produced during dehydration do not impair the functions of components (A), (B), (C), and (D), and they dissolve in the curable liquid silicone composition, allowing for the formation of a stable curable liquid silicone composition. Among these, silyl ketenes (including silyl ketene acetals) and α-silyl esters undergo dehydration reactions under non-basic conditions, and therefore do not decompose the organohydrogenpolysiloxane of component (B) or reduce the catalytic activity of the platinum catalyst in component (C).
[0052] Examples of silyl ketenes (containing silyl ketene acetals) include 1-methoxy-2-methyl-1-(trimethylsiloxy)propene, dimethyl ketene trimethylsilyl acetal, and tert-butoxy-1-(trimethylsiloxy)propene.
[0053] Examples of α-silyl esters include ethyl 2-(trimethoxysilyl)propionate (ECMS) and octyl 2-(methyldimethoxysilyl)propionate (OCMS-2).
[0054] When a dehydrating agent (E) is added, it may be added to each component beforehand, during the preparation of the composition, or after the composition has been prepared. When the component (E) is added, the amount added is preferably 0.01 to 5 mass%, particularly 0.1 to 2 mass%, of the total mass of the components (A) and (B). Adding too much component (E) may adversely affect the changes in the physical properties of the cured product during heat resistance.
[0055] The hydrolysis reaction catalyst for component (D) also promotes the reaction between the dehydrating agent for component (E) and water. Therefore, when component (E) is added, it not only promotes the hydrolysis reaction of the phosphite ester compound, but also has the effect of promoting dehydration within the system.
[0056] [(F) Platinum catalyst compound activated by ultraviolet light] If necessary, the curable liquid silicone composition of the present invention may further contain, as an optional component, a platinum catalyst compound activated by ultraviolet light (component (F))) for the purpose of improving the curing reaction rate.
[0057] As mentioned above, the curable liquid silicone composition of the present invention exhibits one-component storage stability at room temperature in a sealed container, and when used, it cures at room temperature due to atmospheric moisture without heating, but it takes about a week to fully cure. Therefore, in order to improve the curing reaction speed, it is useful to add a platinum catalyst compound that is activated by ultraviolet light, component (F). This improves the curing reaction speed in the areas directly irradiated with ultraviolet light, improving workability, while allowing areas that are difficult to cure, such as dark areas not irradiated with ultraviolet light, to cure later.
[0058] Component (F) in the curable liquid silicone composition of the present invention is a platinum catalyst that is activated by light with a wavelength of 200 to 500 nm, preferably ultraviolet light with a wavelength of 200 to 400 nm. In other words, it is a catalyst that is inactive when shielded from light, and that is converted into a platinum catalyst (hydrosilylation addition reaction catalyst) that is active at room temperature when irradiated with light with a wavelength of 200 to 500 nm, preferably ultraviolet light with a wavelength of 200 to 400 nm, thereby promoting the hydrosilylation addition reaction between alkenyl groups in component (A) and silicon-bonded hydrogen atoms in component (B).
[0059] As the platinum catalyst compound activated by ultraviolet light, which is the component (F), there are used platinum acetylacetonate complexes and platinum cyclopentadienyl complexes, etc., as disclosed in U.S. Pat. No. 4,510,094 (Patent Document 8) and U.S. Pat. No. 4,530,879 (Patent Document 9). Specific examples of such component (F) include (η 5 and complexes of bis(β-diketonato)platinum compounds. Among these, cyclopentadienyltrimethylplatinum complex and methylcyclopentadienyltrimethylplatinum complex are preferred. Also included are complexes of bis(β-diketonato)platinum compounds. Among these, bis(acetylacetonato)platinum complex is preferred.
[0060] When a platinum catalyst compound of component (F) is blended, the blending amount is preferably an amount equivalent to 0.1 to 1,000 ppm, more preferably 0.1 to 500 ppm, and even more preferably 0.1 to 50 ppm, of platinum atoms contained in component (F) relative to the total mass of components (A) and (B). If the blending amount of component (F) is less than the above range, the curing reaction rate may be insufficient or the composition may not cure due to the influence of surrounding curing inhibitors, while if the blending amount is more than the above range, sufficient storage stability may not be obtained.
[0061] Component (F) may be used alone or in combination of two or more. When using component (F), if it is a solid catalyst, it can be used in solid form. However, to obtain a more uniform cured product, it is preferable to use the catalyst dissolved in an appropriate solvent, such as toluene, xylene, ethyl acetate, or 2-(2-butoxyethoxy)ethyl acetate. In this case, the platinum atom content (concentration) in the solution is preferably 0.1 to 2 mass%.
[0062] [(G) Photoinitiator] It is also useful to incorporate a photoinitiator (G) as an optional component into the curable liquid silicone composition of the present invention, for the purpose of reducing the control ability of the phosphite ester compound against the platinum catalyst in the platinum catalyst mixture (C). As described above, in the curable liquid silicone composition of the present invention, the phosphite ester compound is hydrolyzed by moisture in the atmosphere to form phosphonic acid, reducing its control ability against the platinum catalyst and allowing curing to proceed. However, by adding a photoinitiator (G) and irradiating with ultraviolet light, the phosphite ester compound can be oxidized by peroxy radicals formed by the combination of oxygen with radicals generated from the photoinitiator, thereby reducing its control ability against the platinum catalyst.
[0063] The photoinitiator of component (G) can be any of those that have been used in conventional UV-curable liquid silicone compositions. Specific examples include acetophenone, propiophenone, benzophenone, fluorene, benzaldehyde, anthraquinone, triphenylamine, carbazole, 3-methylacetophenone, 4-methylacetophenone, 3-pentylacetophenone, 4-methoxyacetophenone, 3-bromoacetophenone, 4-allylacetophenone, p-diacetylbenzene, 3-methoxybenzophenone, 4-methylbenzophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, 2,2'-diethoxyacetophenone, 4-chloro-4'-benzylbenzophenone, 3-chloroxanthone, 3,9-dichloroxanthone, 3-chloro-8-nonylxanthone, benzoin, and benzoin. Methyl ether, benzoin butyl ether, bis(4-dimethylaminophenyl) ketone, benzyl methoxy ketal, 2-chlorothioxanthone, diethylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1[4-(methylthio)phenyl]-2-morpholino-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone, 1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propan-1-one, 2,2-dimethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, cyclohexyl phenyl ketone, 2-hydroxy-2-methylpropiophenone, and the like.
[0064] When a photoinitiator as component (G) is added, the amount added is preferably 0.01 to 3 mass %, more preferably 0.01 to 1 mass %, and even more preferably 0.01 to 0.1 mass %, of the total mass of components (A) and (B). If component (G) is added in an amount less than the above range, its addition effect may be lost, whereas if it is added in an amount greater than the above range, sufficient storage stability may not be obtained.
[0065] In addition to the optional components such as (E) the dehydrating agent, (F) the platinum catalyst compound activated by ultraviolet light, and (G) the photoinitiator, the curable liquid silicone composition of the present invention may also contain, as necessary, other optional components such as inorganic fillers, adhesion promoters, pigment pastes, and reinforcing silicone resins, provided that the object of the present invention is not impaired.
[0066] The curable liquid silicone composition of the present invention can be prepared by mixing the above-mentioned components (A) to (D) and, if necessary, other components in a conventional manner, but it is preferable to add (A) the alkenyl group-containing diorganopolysiloxane, (B) the organohydrogenpolysiloxane, (D) the hydrolysis reaction catalyst, and (C) the platinum catalyst mixture in this order while mixing. When adding the dehydrating agent (E), it is preferable to add it after adding the organohydrogenpolysiloxane (B), and then adding the hydrolysis reaction catalyst (D), after which the container is sealed and allowed to age under a nitrogen atmosphere overnight or longer before adding the platinum catalyst mixture (C). When adding the platinum catalyst compound (F) activated by ultraviolet light and / or the photoinitiator (G), it is preferable to use a shielded container and add it after adding the platinum catalyst mixture (C).
[0067] The curable liquid silicone composition of the present invention can achieve better one-component shelf life by using and storing the composition in a highly airtight container that can block or reduce the intrusion of moisture, particularly atmospheric moisture (humidity) (however, when component (F) is added, it can block ultraviolet light and block or reduce the intrusion of moisture, particularly atmospheric moisture (humidity), and when component (G) is added, it can block ultraviolet light and block or reduce the intrusion of oxygen and moisture, particularly atmospheric moisture (humidity) and oxygen).This allows the composition to be distributed and sold as a one-component curable liquid silicone composition.
[0068] Furthermore, when in use, the curable liquid silicone composition of the present invention will cure at room temperature due to moisture in the atmosphere (however, if component (F) is contained, the ultraviolet-irradiated areas will cure upon irradiation, and then exposure to the atmosphere and contact with atmospheric moisture (humidity) at room temperature will cure even dark areas that are not reached by the ultraviolet light; if component (G) is contained, the composition will cure upon irradiation with ultraviolet light, then exposure to the atmosphere and contact with atmospheric moisture (humidity) and oxygen at room temperature), thereby giving a cured silicone rubber or cured silicone gel.
[0069] When the composition contains a platinum catalyst compound (component (F)) activated by ultraviolet light and / or a photoinitiator (component (G)), the ultraviolet irradiation method involves irradiating the curable liquid silicone composition of the present invention with ultraviolet light at room temperature (23°C ± 15°C), preferably with light of 200 to 500 nm at room temperature. When the composition contains component (F), ultraviolet irradiation activates the platinum catalyst compound (component (F)) in the ultraviolet-irradiated section, causing it to act as a hydrosilylation addition reaction catalyst, accelerating the hydrosilylation addition reaction and resulting in curing. When the composition contains component (G), ultraviolet irradiation generates radicals from the photoinitiator (component (G)), which combine with oxygen in the air to form peroxy radicals, which oxidize the phosphite ester compound, activating the platinum catalyst in component (C) and causing it to act as a hydrosilylation addition reaction catalyst, accelerating the hydrosilylation addition reaction and resulting in curing.
[0070] The lamp for irradiating ultraviolet light is not particularly limited as long as it can supply light with a wavelength of 200 to 500 nm, and examples thereof include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, xenon lamps, metal halide lamps, ultraviolet LED lamps, etc. The ultraviolet light irradiation dose varies depending on the type and amount of the platinum catalyst compound (component (F)) and the photoinitiator (component (G)) used, but is generally 10 to 1,000 mW / cm. 2 , especially 20 to 400 mW / cm 2 It is preferable to irradiate the ultraviolet light having the above intensity for 0.1 seconds to 5 minutes, and particularly for 0.5 seconds to 1 minute.
[0071] The curable liquid silicone composition of the present invention has good curing properties even in dark areas where ultraviolet light does not reach, and therefore can be suitably used as a sealant or coating agent for components that have complex structures and many dark areas when the curable composition is cured by ultraviolet light irradiation, as well as a liquid optically clear adhesive (LOCA), etc.
[0072] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following examples, the viscosity is measured using a rotational viscometer at 23°C, and parts indicate parts by mass. "Room temperature" means 23°C.
[0073] Comparative Example 1, Examples 1 to 4 Curable liquid silicone compositions were prepared as follows. <Preparation of Curable Liquid Silicone Composition> Each composition was prepared by uniformly mixing the components in the amounts shown in Table 1 in a brown glass bottle under a nitrogen atmosphere at room temperature (23°C), and then sealing the bottle in a light-shielded condition. The molar ratio of SiH groups in component (B) to vinyl groups in component (A) was 1.1. The following components were added in this order while mixing: (A) alkenyl group-containing diorganopolysiloxane, (B) organohydrogenpolysiloxane, (E) dehydrating agent, (D) hydrolysis reaction catalyst, and (C) platinum catalyst mixture containing a platinum catalyst and a phosphite compound. When the dehydrating agent (E) was added, the brown glass bottle was sealed after adding the hydrolysis reaction catalyst (D) and the mixture was aged under a nitrogen atmosphere overnight or longer before adding (C) platinum catalyst mixture containing a platinum catalyst and a phosphite compound. Furthermore, when not only the dehydrating agent (E) but also the platinum catalyst compound (F) activated by ultraviolet light and / or the photoinitiator (G) were added, they were added after the platinum catalyst mixture containing the platinum catalyst and the phosphite ester compound (C) was added.
[0074] The components are as follows: (A) Alkenyl group-containing diorganopolysiloxane: A vinyl group-containing branched dimethylpolysiloxane having a viscosity of 1,000 mPa·s at 23° C. and represented by the following average formula (4):
[0075] (B) Organohydrogenpolysiloxane: A linear methylhydrogenpolysiloxane represented by the following average formula (5) (dimethylpolysiloxane blocked at both molecular chain terminals with dimethylhydrogensiloxy groups)
[0076] (C) Platinum catalyst mixture containing a platinum catalyst and a phosphite ester compound: A platinum catalyst mixture prepared by adding 1.05 moles of triisopropyl phosphite per mole of platinum atom to a platinum-divinyltetramethyldisiloxane complex / toluene solution (platinum atom content: 0.5% by mass) under a nitrogen atmosphere.
[0077] (D) Hydrolysis reaction catalyst: tetra(isopropyl)titanate (TPT)
[0078] (E) Dehydrating agent: ethyl 2-(trimethoxysilyl)propionate (ECMS) (α-silyl esters)
[0079] (F) Platinum catalyst compound activated by ultraviolet light: toluene solution of methylcyclopentadienyltrimethylplatinum complex (platinum atom content 0.5% by mass)
[0080] (G) Photoinitiator: Darocur 1173 (2-hydroxy-2-methylpropiophenone) manufactured by BASF Japan Ltd.
[0081] The curable liquid silicone compositions thus prepared were evaluated for cured product appearance, one-component storage stability in a light-shielded, sealed container at room temperature, moisture (aerobic) curing in a light-shielded, atmospheric, room temperature container, and shadow curing ability under ultraviolet light irradiation, as described below.
[0082] The appearance of the cured product was evaluated visually and was colorless and transparent to brownish and transparent in each of the Examples and Comparative Examples. The evaluation results are shown in Table 1.
[0083] [One-component storage stability (protected from light, sealed, at room temperature)] To determine one-component storage stability, fill a brown glass bottle with curable liquid silicone composition under nitrogen atmosphere, seal it, then leave the brown glass bottle in the air / room temperature, and observe the thickening and gelling behavior of the curable liquid silicone composition.At this time, when tilting the brown glass bottle, observe the degree to which the composition in the brown glass bottle flows along with it (fluidity), and when the fluidity becomes worse than that immediately after sealing, judge that the curable liquid silicone composition has thickened or gelled.Check every week, and the week when thickening and gelling are confirmed is listed in Table 1.
[0084] [Moisture (aerobic) curability (protected from light, in the atmosphere, at room temperature)] Moisture curability was measured by filling a brown glass bottle with the curable liquid silicone composition in a nitrogen atmosphere, sealing it, and then, after 3 hours, pouring 9 g of the curable liquid silicone composition from the brown glass bottle into a glass petri dish with an inner diameter of 10 mm. The dish was then covered with aluminum foil in the atmosphere at room temperature to protect it from light, and the condition was observed after 1 week. The results are shown in Table 1.
[0085] [Shadow Curability Upon UV Irradiation] 9 g of each composition prepared above (approximately 3.2 mm thick) was filled into a circular aluminum Petri dish with an inner diameter of 60 mm, and a light-shielding plate with a 20 mm diameter hole (void) was placed on top of the dish. Using an ultraviolet irradiation device (manufactured by CCS Inc.) with a UV-LED lamp as the light source, the exposure dose of ultraviolet light with a wavelength of 365 nm was 8,000 mJ / cm in an atmospheric atmosphere at room temperature (23°C). 2The composition was cured by irradiating with ultraviolet light so that the cured gel was cured. A schematic diagram is shown in Figure 1. Here, 1 is an aluminum petri dish, 2 is the curable liquid silicone composition, 3 is a light-shielding plate, 4 is a hole (void) in the light-shielding plate, and 5 is the direction of ultraviolet light irradiation. For each composition, the liquid portion was removed 10 minutes, 24 hours, and 72 hours after ultraviolet light irradiation, and the distance from the outer edge of the light-receiving portion to the edge of the cured gel was evaluated as the shadow cured size. A schematic diagram is shown in Figure 2. Here, 6 is the cured portion of the ultraviolet-receiving portion (20 mm diameter) that was directly irradiated with ultraviolet light, 7 is the cured portion of the shadow portion covered by the shielding plate and not irradiated with ultraviolet light, 8 is the uncured portion of the shadow portion covered by the shielding plate and not irradiated with ultraviolet light, and 9 is the shadow cured size measured and evaluated as described above. The maximum shadow cured size in this evaluation was 20 mm. The results are shown in Table 1.
[0086]
[0087] The above results confirm that the curable liquid silicone composition of the present invention exhibits one-component storage stability at room temperature in a sealed container, and that it cures at room temperature without heating due to atmospheric moisture during use.
[0088] REFERENCE SIGNS LIST 1 Aluminum Petri dish 2 Curable liquid silicone composition 3 Light shielding plate 4 Hole (gap) in light shielding plate (diameter 20 mm) 5 Direction of ultraviolet light irradiation 6 UV light receiving part (diameter 20 mm) 7 Cured part in shadow 8 Uncured part in shadow 9 Size of cured part in shadow
Claims
1. A curable liquid silicone composition comprising: (A) a linear or branched diorganopolysiloxane having at least one alkenyl group per molecule; (B) a linear or branched organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms per molecule: in an amount such that there are 0.5 to 4 moles of hydrogen atoms bonded to silicon atoms in component (B) per mole of alkenyl groups in component (A); (C) a platinum catalyst mixture containing a platinum catalyst and a phosphite compound in an amount of 0.5 to 3 moles per mole of platinum atoms: in an amount such that the platinum atoms in component (C) are 0.1 to 1,000 ppm by mass relative to the combined mass of components (A) and (B); and (D) a hydrolysis reaction catalyst: 0.01 to 3 mass% of the combined mass of components (A) and (B).
2. The curable liquid silicone composition according to claim 1, which is a one-component composition.
3. The curable liquid silicone composition according to claim 1, further comprising: (E) a dehydrating agent: 0.01 to 5 mass % of the combined mass of components (A) and (B).
4. The curable liquid silicone composition according to claim 1, further comprising (F) a platinum catalyst compound activated by ultraviolet light: in an amount such that the mass of platinum atoms in component (F) is 0.1 to 1,000 ppm relative to the combined mass of components (A) and (B).
5. The curable liquid silicone composition according to claim 1, further comprising: (G) a photoinitiator: 0.01 to 3 mass % of the combined mass of components (A) and (B).
6. A cured product of the curable liquid silicone composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
One-liquid type organopolysiloxane composition
JP2722304B2
One-component organopolysiloxane gel composition
JP4530147B2
Platinum-olefin complex catalyzed addition of hydrogen- and alkenyl-substituted siloxanes
US3159601A
Addition reaction
US3159662A
Organosilicon process using a chloroplatinic acid reaction product as the catalyst
US3220972A