Positive electrode material for lithium ion secondary battery, positive electrode for lithium ion secondary battery, and method for manufacturing positive electrode material for lithium ion secondary battery
The use of carbon-coated, aggregated olivine-type lithium manganese iron phosphate particles in the positive electrode material addresses the cracking issue during drying, improving film formability and battery performance by controlling particle size and carbon content, and suppressing necking in lithium ion secondary batteries.
Patent Information
- Application Number
- PCT/JP2024/010992
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-31
AI Technical Summary
Olivine-type lithium manganese iron phosphate cathode active materials tend to crack due to shrinkage during the drying process in the manufacturing of lithium ion secondary battery positive electrodes, leading to poor film formability and battery performance.
A positive electrode material with a granule structure having a carbon coating and a core of aggregated olivine-type lithium manganese iron phosphate particles, where the primary particles are 100 nm or less in diameter, and the carbon content is between 1.8% and 3.0% by mass, is used, along with a method involving a mixing, pulverizing, drying, and firing process to suppress necking and control pore volume.
The solution enhances film formability and battery performance by preventing cracks in the positive electrode active material layer and improving the capacity of lithium ion secondary batteries, while also reducing the occurrence of necking and maintaining a suitable pore volume.
Smart Images

Figure JP2024010992_31102024_PF_FP_ABST
Abstract
Description
Positive electrode material for lithium ion secondary battery, positive electrode for lithium ion secondary battery, and method for manufacturing positive electrode material for lithium ion secondary battery
[0001] The present disclosure relates to a positive electrode material for a lithium ion secondary battery, a positive electrode for a lithium ion secondary battery, and a method for producing a positive electrode material for a lithium ion secondary battery.
[0002] Patent Document 1 describes an olivine-type lithium iron phosphate (LiFePO 4 The olivine-type structured positive electrode active material, typified by olivine-type lithium iron phosphate, is a positive electrode active material with excellent thermal stability.
[0003] Japanese Patent Application Laid-Open No. 2019-185920
[0004] The positive electrode of a lithium ion secondary battery is manufactured, for example, as follows. First, a positive electrode mixture in a slurry form containing a positive electrode active material, a binder, and a solvent is applied to the surface of a positive electrode current collector. Next, the coating formed by the application is dried to form a positive electrode active material layer on the surface of the positive electrode current collector. Here, a method for increasing the capacity of a lithium ion secondary battery is to increase the basis weight of the positive electrode active material layer by applying a thick coating of the positive electrode mixture in the above manufacturing process. However, when an olivine-type structure positive electrode active material is used as the positive electrode active material, there is a problem that cracks are likely to occur in the resulting positive electrode active material layer due to shrinkage of the coating film during drying. In particular, among olivine-type structure positive electrode active materials, olivine-type lithium manganese iron phosphate (LiMnFePO 4 ) is used, the above problems are likely to occur.
[0005] In one aspect of the present disclosure, a positive electrode material for a lithium ion secondary battery is provided having the general formula LiMn x Fe y P.O. 4The present invention includes granules having a core made of olivine-type lithium manganese iron phosphate represented by the formula (x and y are numbers satisfying x+y=1, 0<x<1, 0<y<1), and a carbon coating formed on the surface of the core. The core has a structure in which primary particles of the olivine-type lithium manganese iron phosphate are aggregated. The particle diameter of the primary particles is 100 nm or less. The pore volume of the granules in the pore diameter range of 2 nm to 300 nm is 0.2 cm 3 The carbon content of the granules is 1.8% by mass or more and 3.0% by mass or less.
[0006] 1A is a photomicrograph of a cross section of a granule; 1B is a schematic diagram showing the structure of a primary particle in a cross section of a granule; 1C is a cross-sectional view of a positive electrode; 1D is a photomicrograph of a positive electrode active material layer using Example 1, and 1E is a photomicrograph of a positive electrode active material layer using Comparative Example 1.
[0007] An embodiment of the present invention will be described below with reference to the drawings. Hereinafter, a positive electrode material for a lithium ion secondary battery and a positive electrode of a lithium ion secondary battery will be abbreviated as a positive electrode material and a positive electrode, respectively.
[0008] 1 , the positive electrode material of this embodiment includes granules 10 having a core 11 made of olivine-type lithium manganese iron phosphate and a carbon coating 12 formed on the surface of the core 11. The positive electrode material may be composed only of the granules 10, or may contain components other than the granules 10 as necessary.
[0009] The olivine-type lithium manganese iron phosphate constituting the core 11 has the general formula LiMn x Fe y P.O. 4 It is a polyanionic compound having an olivine structure represented by the general formula LiMn x Fe y P.O. 4In the formula, x and y are numerical values that satisfy x+y=1, 0<x<1, and 0<y<1. Specific examples of the ranges of x and y include 0.5≦x≦0.9, 0.1≦y≦0.5, and 0.6≦x≦0.8, 0.2≦y≦0.4. The olivine-type lithium manganese iron phosphate constituting the core 11 may be one type or two or more types.
[0010] Fig. 2 is a schematic diagram showing the structure of the area indicated by the arrow A in Fig. 1. As shown in Fig. 2, the core 11 has a structure in which primary particles 11a of olivine-type lithium manganese iron phosphate are aggregated. The core 11 also has pores 11b formed between the multiple primary particles 11a.
[0011] The particle diameter of the primary particles 11a is 100 nm or less, preferably 80 nm or less. The particle diameter of the primary particles 11a is, for example, 20 nm or more. The particle diameter of the primary particles 11a is a value determined by small angle X-ray scattering (SAXS). Specifically, the particle diameter of the primary particles 11a is a value defined as the average particle diameter (D50) obtained from the particle diameter distribution of the primary particles 11a, assuming that the primary particles 11a are spherical.
[0012] In the core 11, the pore volume in the pore diameter range of 2 nm to 300 nm is 0.2 cm 3 / g or less, preferably 0.15 cm 3 / g or less. The pore volume is, for example, 0.05 cm 3 / g or more, preferably 0.1 cm 3 / g or more. The pore volume can be determined by nitrogen adsorption / desorption measurement of the granules 10 and the Barrett Joyner Hallenda (BJH) method. The pore volume described below refers to the pore volume in the pore diameter range of 2 nm or more and 300 nm or less.
[0013] The carbon content of the granules 10 is 1.8% by mass or more, preferably 1.9% by mass or more, and more preferably 2.0% by mass or more. If the carbon content is less than 1.8%, the carbon coating 12 will not be able to cover the entire surface of the core 11. In this case, portions of the surface of the core 11 will be exposed, which will deteriorate the film-forming properties when forming the active material layer described below. The carbon content is 3.0% by mass or less, and preferably 2.7% by mass or less. The carbon content can be measured using a carbon / sulfur analyzer (CS meter).
[0014] The content of the olivine-type lithium manganese iron phosphate in the granules 10 is, for example, 95% by mass or more, preferably 96% by mass or more. The content is 99% by mass or less, preferably 98% by mass or less.
[0015] The granules 10 may contain other components in addition to the olivine-type lithium manganese iron phosphate and carbon. In this case, the content of the other components is, for example, 2 mass % or less.
[0016] The average particle size (D50) of the granules 10 is, for example, 3.0 μm or more, and preferably 5.0 μm or more. The average particle size (D50) of the granules 10 is, for example, 30 μm or less, and preferably 20 μm or less. The average particle size of the granules 10 can be measured, for example, using a laser diffraction particle size analyzer.
[0017] <Method for producing a positive electrode material> Next, an example of a method for producing a positive electrode material will be described. The example method for producing a positive electrode material includes a mixing step, a pulverizing step, a drying step, and a firing step. The positive electrode material is produced by sequentially going through the mixing step, the pulverizing step, the drying step, and the firing step.
[0018] [Mixing Step] The mixing step is a step of preparing a first slurry by mixing olivine-type lithium manganese iron phosphate particles, an aqueous solvent, a carbon source, and a carboxylic acid.
[0019] The olivine-type lithium manganese iron phosphate particles have the general formula LiMn x Fe y P.O. 4The particles are polyanionic compounds having an olivine structure represented by the general formula LiMn x Fe y P.O. 4 In the formula, x and y are numerical values that satisfy x+y=1, 0<x<1, and 0<y<1. Specific examples of the ranges of x and y include 0.5≦x≦0.9, 0.1≦y≦0.5, and 0.6≦x≦0.8, 0.2≦y≦0.4. The olivine-type lithium manganese iron phosphate particles may be made of one type or two or more types of olivine-type lithium manganese iron phosphate.
[0020] The particles have an average particle size (D50) of, for example, 3.0 μm or more, preferably 5.0 μm or more, and an average particle size (D50) of, for example, 30 μm or less, preferably 20 μm or less.
[0021] The olivine-type lithium manganese iron phosphate particles can be produced, for example, as follows: First, a Li source such as lithium hydroxide, a Mn source such as a manganese compound, a Fe source such as an iron compound, and a PO source such as orthophosphoric acid are mixed together. 4 A first precursor slurry is prepared by mixing the Li source, Mn source, and Fe source contained in the first precursor slurry with water. Next, the Li source, Mn source, and Fe source contained in the first precursor slurry are pulverized using a pulverizer such as a bead mill. This results in a second precursor slurry containing pulverized Li source, Mn source, and Fe source. Next, the second precursor slurry is dried by a method such as spray drying to obtain a particulate dried precursor. The obtained dried precursor is calcined at a temperature of, for example, about 500°C to obtain the above-mentioned particles.
[0022] The aqueous solvent is water or a mixed solvent of water and a non-aqueous solvent. The water is not particularly limited, but examples thereof include ion-exchanged water, which is water treated with an ion exchange resin, and ultrapure water, which is water treated with a reverse osmosis membrane water purification system. Examples of non-aqueous solvents constituting the mixed solvent include water-miscible solvents such as lower alcohols, acetone, tetrahydrofuran, ethylene glycol, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, acetonitrile, and dimethyl sulfoxide. One type of non-aqueous solvent may be used alone, or two or more types may be used in combination. The volume ratio of water in the mixed solvent is preferably, for example, 50% by volume or more and 99.9% by volume or less, and more preferably 60% by volume or more and 99% by volume or less.
[0023] As the carbon source, for example, an organic compound can be used. Examples of the organic compound include glucose, fructose, galactose, mannose, maltose, sucrose, lactose, glycogen, pectin, alginic acid, glucomannan, chitin, hyaluronic acid, chondroitin, agarose, polyether, polyhydric alcohol, polyvinyl alcohol, polyvinylpyrrolidone, cellulose, starch, gelatin, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, polystyrene sulfonic acid, polyacrylamide, and polyvinyl acetate. Examples of the polyhydric alcohol include polyethylene glycol, polypropylene glycol, polyglycerin, and glycerin. The carbon source may be used alone or in combination of two or more.
[0024] Examples of carboxylic acids include citric acid, formic acid, acetic acid, propionic acid, butanoic acid, pentanoic acid, malic acid, fumaric acid, tartaric acid, ascorbic acid, gluconic acid, and polyacrylic acid. One type of carboxylic acid may be used alone, or two or more types may be used in combination. Among these carboxylic acids, citric acid is preferably used. Details of this point will be described later.
[0025] Next, the amounts of the olivine-type lithium manganese iron phosphate particles, aqueous solvent, carbon source, and carboxylic acid in the first slurry will be described. The amount of the aqueous solvent is, for example, 40 parts by mass or more, preferably 50 parts by mass or more, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. The amount of the aqueous solvent is, for example, 80 parts by mass or less, preferably 70 parts by mass or less, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles.
[0026] The amount of carboxylic acid is, for example, 2 parts by mass or more, preferably 3 parts by mass or more, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. The amount of carboxylic acid is, for example, 15 parts by mass or less, preferably 12 parts by mass or less, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. Within a specific blending amount, the pore volume of the core 11 of the granules 10 decreases as the blending amount of carboxylic acid increases. Furthermore, the pore size distribution of the core 11 of the granules 10 shifts toward smaller diameters as the blending amount of carboxylic acid increases. Therefore, the pore volume of the core 11 of the granules 10 can be controlled by adjusting the blending amount of carboxylic acid.
[0027] In the mixing step, the carbon source is blended with the olivine-type lithium manganese iron phosphate particles so that the total carbon content, which is the sum of the masses of carbon in the carbon source and carbon in the carboxylic acid, is a specific amount. Therefore, the blended amount of the carbon source is, for example, an amount such that the total carbon content is 1.8 parts by mass or more, and preferably 1.9 parts by mass or more, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. The blended amount of the carbon source is, for example, an amount such that the total carbon content is 5.0 parts by mass or less, and preferably 3.0 parts by mass or less, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. The carbon content of the granules 10 can be controlled by adjusting the total carbon content based on the blended amount of the carbon source.
[0028] The first slurry may contain other components in addition to the olivine-type lithium manganese iron phosphate particles, the aqueous solvent, the carbon source, and the carboxylic acid. Examples of the other components include a dispersant.
[0029] [Pulverization Step] The pulverization step is a step of pulverizing the olivine-type lithium manganese iron phosphate particles contained in the first slurry to prepare a second slurry containing the pulverized particles. The pulverization step corresponds to a step of pulverizing the olivine-type lithium manganese iron phosphate particles in the presence of an aqueous solvent, a carbon source, and a carboxylic acid to prepare the second slurry.
[0030] The average particle size (D50) of the pulverized particles is, for example, 20 nm or more, preferably 30 nm or more. The average particle size (D50) of the pulverized particles is, for example, 100 nm or less, preferably 90 nm or less. By reducing the average particle size (D50) of the pulverized particles, the particle size of the primary particles 11a of the granules 10 can be reduced.
[0031] The pulverization method used in the pulverization step is not particularly limited as long as it can pulverize the olivine-type lithium manganese iron phosphate particles in the first slurry. Examples of the pulverization method include methods using a pulverizer such as a bead mill, a hammer mill, an agitation mill, a jet mill, or a ball mill. The temperature during pulverization is, for example, 10°C or higher and 50°C or lower.
[0032] During the pulverization of the olivine-type lithium manganese iron phosphate particles, some of the metals (Li, Mn, and Fe) contained in the particles are eluted into the slurry. In the subsequent firing step, the eluted metals cause necking between the pulverized particles, i.e., between the primary particles 11a constituting the core 11 of the granules 10, with the metals acting as neck portions. If a positive electrode material containing the granules 10 in which necking is abundant is used in the positive electrode of a lithium-ion secondary battery, the battery performance of the lithium-ion secondary battery will be reduced.
[0033] In this embodiment, the occurrence of necking is suppressed by the inclusion of carboxylic acid in the first slurry. That is, the eluted metal is captured by carboxylic acid in the slurry, and the eluted metal is prevented from contacting the surface of the pulverized olivine-type lithium manganese iron phosphate particles, particularly the newly formed surface formed by pulverization. As a result, the occurrence of necking, in which the eluted metal forms a neck portion between the pulverized particles, is suppressed.
[0034] Therefore, from the viewpoint of suppressing the occurrence of necking, it is preferable that the carboxylic acid used in the first slurry has a high ability to capture the eluted metals Li, Mn, and Fe. The bond energies of various carboxylic acids with Li, Mn, and Fe are shown in Table 1 below. The bond energy values shown in Table 1 below are values obtained as the difference in energy before and after the formation of a complex between the carboxylic acid and each of the eluted metals, and the smaller the value, the higher the ability to capture the corresponding eluted metal. The bond energy values shown in Table 1 below were calculated using CAE (Computer Aided Engineering). As shown in Table 1, citric acid has the lowest bond energy with respect to all of the eluted metals Li, Mn, and Fe. Therefore, from the viewpoint of suppressing the occurrence of necking, it is preferable to use citric acid as the carboxylic acid.
[0035]
[0036] [Drying step] The drying step is a step of spray-drying the second slurry to obtain an aggregate of the pulverized material. Examples of the spraying method in spray drying include spraying methods using a disk type, a pressure nozzle, a pressure two-fluid nozzle, a pressure four-fluid nozzle, etc. The spray temperature in spray drying is, for example, 180°C or higher and 300°C or lower.
[0037] [Firing Step] The firing step is a step of firing the aggregate obtained in the drying step to carbonize the carbon source contained in the aggregate. The firing conditions in the firing step are not particularly limited as long as they are conditions that can carbonize the carbon source. The firing temperature in the firing step is, for example, 500°C or higher and 750°C or lower. The firing time in the firing step is, for example, 1 hour or higher and 12 hours or lower. The atmosphere in the firing step is, for example, a non-oxidizing atmosphere. Examples of the non-oxidizing atmosphere include nitrogen (N 2 ), an inert atmosphere such as argon (Ar), and hydrogen (H 2 ) or the like.
[0038] <Positive Electrode> Next, a positive electrode 100 including the positive electrode material of this embodiment will be described. As shown in Fig. 3 , the positive electrode 100 includes a positive electrode current collector 101 having a first surface 101a, and a positive electrode active material layer 102 formed on the first surface 101a of the positive electrode current collector 101.
[0039] [Positive Electrode Current Collector] The positive electrode current collector 101 is a chemically inactive electrical conductor that continues to pass current through the positive electrode active material layer 102 during discharge or charge of the lithium ion secondary battery. The positive electrode current collector 101 is, for example, in the form of a foil. The thickness of the foil-shaped positive electrode current collector 101 is, for example, 1 μm or more, and preferably 10 μm or more. The thickness of the foil-shaped positive electrode current collector 101 is, for example, 100 μm or less, and preferably 60 μm or less.
[0040] Examples of materials constituting the positive electrode current collector 101 include metal materials, conductive resin materials, and conductive inorganic materials. Examples of the metal materials include copper, aluminum, nickel, titanium, and stainless steel. Examples of the conductive resin materials include resins obtained by adding a conductive filler to a conductive polymer material or a non-conductive polymer material as needed. The positive electrode current collector 101 may have multiple layers including one or more layers containing the metal materials or conductive resin materials.
[0041] An example of the positive electrode current collector 101 is an aluminum current collector. The aluminum current collector may be made of aluminum alone or an aluminum alloy. Examples of the aluminum alloy include an Al—Mn alloy, an Al—Mg alloy, and an Al—Mg—Si alloy.
[0042] The first surface 101a of the positive electrode current collector 101 may be covered with a known protective layer such as a carbon coating layer. The first surface 101a of the positive electrode current collector 101 may be treated by a known method such as plating.
[0043] [Positive Electrode Active Material Layer] The positive electrode active material layer 102 is provided on the first surface 101a of the positive electrode current collector 101. The weight of the positive electrode active material layer 102 is, for example, 20 mg / cm 2 or more, preferably 30 mg / cm 2 The weight per unit area of the positive electrode active material layer 102 is, for example, 150 mg / cm 2 or less, preferably 100 mg / cm 2 The thickness of the positive electrode active material layer 102 is, for example, 80 μm or more, and preferably 100 μm or more. The thickness of the positive electrode active material layer 102 is, for example, 1000 μm or less, and preferably 800 μm or less.
[0044] The positive electrode active material layer 102 includes a positive electrode active material capable of absorbing and releasing charge carriers such as lithium ions. The positive electrode active material layer 102 includes the granules 10 described above as the positive electrode active material. The positive electrode active material layer 102 may include a positive electrode active material other than the granules 10. Examples of the other positive electrode active material include lithium composite metal oxides having a layered rock salt structure, metal oxides having a spinel structure, and polyanion compounds other than olivine-type lithium manganese iron phosphate. One type of the other positive electrode active material may be used alone, or two or more types may be used in combination. When the other positive electrode active material is included, the mass ratio of the granules 10 to the entire positive electrode active material is preferably 50% or more, and more preferably 90% or more.
[0045] There are no particular limitations on the content of the positive electrode active material in the positive electrode active material layer 102. The content of the positive electrode active material in the positive electrode active material layer 102 is, for example, 95% by mass or more, and preferably 96% by mass or more. The content of the positive electrode active material in the positive electrode active material layer 102 is, for example, 99.5% by mass or less, and preferably 99% by mass or less.
[0046] The positive electrode active material layer 102 may further contain, as necessary, a conductive aid for increasing electrical conductivity, a binder, an electrolyte (a polymer matrix, an ion-conductive polymer, a liquid electrolyte, or the like), an electrolyte supporting salt (lithium salt) for increasing ion conductivity, and the like.
[0047] The conductive additive is added to increase the conductivity of the positive electrode 100. Examples of the conductive additive include acetylene black, carbon black, graphite, and carbon nanotubes.
[0048] Examples of binders include fluorine-containing resins such as polyvinylidene fluoride, polytetrafluoroethylene, and fluororubber; thermoplastic resins such as polypropylene and polyethylene; imide resins such as polyimide and polyamideimide; alkoxysilyl group-containing resins; acrylic resins such as polyacrylic acid and polymethacrylic acid; styrene-butadiene rubber; carboxymethyl cellulose; alginates such as sodium alginate and ammonium alginate; water-soluble cellulose ester crosslinked bodies; and starch-acrylic acid graft polymers. These binders can be used alone or in combination. Examples of solvents or dispersion media include water and N-methyl-2-pyrrolidone.
[0049] <Method for manufacturing positive electrode> Next, an example of a method for manufacturing the positive electrode 100 will be described. The example of the method for manufacturing the positive electrode 100 includes a preparation step of preparing a positive electrode composite and an active material layer formation step of forming a positive electrode active material layer using the positive electrode composite. The positive electrode 100 is manufactured by sequentially undergoing the preparation step and the active material layer formation step.
[0050] [Preparation Step] The preparation step is a step of preparing a positive electrode mixture that will become the positive electrode active material layer 102 upon solidification. The positive electrode mixture is a slurry containing a positive electrode active material, an aqueous binder, and an aqueous solvent.
[0051] The positive electrode active material blended in the positive electrode composite is the same as the positive electrode active material described in the description section for the positive electrode 100. The content of the positive electrode active material in the positive electrode composite is, for example, 70 parts by mass or more and 99 parts by mass or less, and preferably 90 parts by mass or more and 98 parts by mass or less, when the total mass of the solid content contained in the positive electrode composite, i.e., the mass of the positive electrode composite excluding the aqueous solvent (hereinafter referred to as the solid content mass), is taken as 100 parts by mass.
[0052] The aqueous binder is a binder that is soluble or dispersible in an aqueous solvent and is used by mixing the aqueous binder with the positive electrode active material in a dispersed or dissolved state in the aqueous solvent. The aqueous binder is not particularly limited, and any conventionally known material can be used as the aqueous binder contained in the positive electrode active material layer of a lithium ion secondary battery.
[0053] Examples of aqueous binders include fluorine-containing resins such as polyvinylidene fluoride, polytetrafluoroethylene, and fluororubber, thermoplastic resins such as polypropylene and polyethylene, imide resins such as polyimide and polyamideimide, alkoxysilyl group-containing resins, acrylic resins such as poly(meth)acrylic acid, styrene-butadiene rubber, carboxymethyl cellulose, alginates such as sodium alginate and ammonium alginate, water-soluble cellulose ester crosslinked bodies, and starch-acrylic acid graft polymers. The aqueous binder contained in the positive electrode active material layer 102 may be one type or two or more types.
[0054] The content of the aqueous binder in the positive electrode mixture is, for example, 1 part by mass to 30 parts by mass, and preferably 1 part by mass to 5 parts by mass, when the solid content is 100 parts by mass. The aqueous solvent contained in the positive electrode mixture can be the same as the aqueous solvent used in the manufacturing method of the positive electrode material. The content of the aqueous solvent in the positive electrode mixture is not particularly limited, but is, for example, a content such that the solid content ratio of the positive electrode mixture is 30 to 60% by mass.
[0055] The positive electrode mixture may contain optional components, such as a conductive assistant for increasing electrical conductivity, an electrolyte (a polymer matrix, an ion-conductive polymer, an electrolyte solution, etc.), and an electrolyte supporting salt (lithium salt) for increasing ion conductivity, as needed.
[0056] [Active Material Layer Forming Step] The active material layer forming step is a step of forming the positive electrode active material layer 102 on the first surface 101a of the positive electrode current collector 101 using the positive electrode mixture.
[0057] In the active material layer formation process, the method for forming the positive electrode active material layer 102 on the first surface 101a of the positive electrode current collector 101 using a slurry positive electrode composite is not particularly limited, and any known method applicable to the formation of the positive electrode 100 including the positive electrode current collector 101 and the positive electrode active material layer 102 can be used.
[0058] For example, a positive electrode composite is applied to a predetermined thickness on the first surface 101a of the positive electrode current collector 101. The coating film formed by the application is then dried and solidified to form the positive electrode active material layer 102. As a method for applying the positive electrode composite, a conventionally known method such as roll coating, dip coating, doctor blade coating, spray coating, or curtain coating can be used.
[0059] <Effects> Next, the effects of this embodiment will be described. (1) The positive electrode material for a lithium ion secondary battery is a material having the general formula LiMn x Fe y P.O. 4 The present invention includes granules 10 having a core 11 made of olivine-type lithium manganese iron phosphate represented by the formula (x and y are numbers satisfying x+y=1, 0<x<1, 0<y<1), and a carbon coating 12 formed on the surface of the core 11. The core 11 has a structure in which primary particles 11a of the olivine-type lithium manganese iron phosphate are aggregated. The particle diameter of the primary particles 11a is 100 nm or less. The pore volume in the pore diameter range of 2 nm or more and 300 nm or less in the granules 10 is 0.2 cm 3 / g or less, and the carbon content is 1.8 mass % or more and 3.0 mass % or less.
[0060] The cathode material having the above configuration is used as the cathode active material contained in the cathode active material layer 102 of the cathode 100. The cathode active material layer 102 of the cathode 100 is produced by applying a slurry cathode composite containing the cathode active material to the first surface 101a of the cathode current collector 101 and drying the coating film formed by the coating. By using the cathode material having the above configuration as the cathode active material contained in the cathode composite, even when a thick coating film is formed to increase the basis weight of the cathode active material layer 102, cracks that occur in the cathode active material layer 102 due to shrinkage of the coating film during drying can be suppressed. In other words, by using the cathode material having the above configuration, it is possible to form a cathode with a large basis weight, for example, a basis weight of 30 mg / cm 2 The film-formability of the positive electrode active material layer 102 is improved when the positive electrode active material layer 102 having the above structure is manufactured. In addition, an effect of improving battery performance based on increasing the basis weight of the positive electrode active material layer 102, for example, an effect of increasing the capacity of a lithium-ion secondary battery, can be obtained. Therefore, with the positive electrode material having the above configuration, it is possible to achieve both film-formability and improved battery characteristics when the basis weight of the positive electrode active material layer containing the olivine-type lithium manganese iron phosphate is increased.
[0061] (2) A method for producing a positive electrode material for a lithium ion secondary battery is to use a compound of the general formula LiMn x Fe y P.O. 4 The method includes a step (corresponding to a grinding step) of grinding particles of olivine-type lithium manganese iron phosphate represented by the formula (x and y are numbers satisfying x+y=1, 0<x<1, 0<y<1) in the presence of an aqueous solvent, a carbon source, and a carboxylic acid to prepare a slurry (corresponding to a second slurry) containing the ground product of the olivine-type lithium manganese iron phosphate; a step (corresponding to a drying step) of spray-drying the slurry (corresponding to a first slurry) to obtain an aggregate of the ground product; and a step (corresponding to a calcining step) of calcining the aggregate to carbonize the carbon source contained in the aggregate.
[0062] According to the above configuration, the particles are pulverized in an aqueous solvent in the presence of a carboxylic acid, so that the eluted metals eluted during pulverization are captured by the carboxylic acid. The eluted metals are captured by the carboxylic acid, which prevents the eluted metals from coming into contact with the surfaces of the pulverized olivine-type lithium manganese iron phosphate particles, particularly with the newly formed surfaces formed by pulverization. As a result, the occurrence of necking, in which the eluted metals form necks between the pulverized particles, is suppressed. Furthermore, the suppression of necking can prevent a decrease in the battery performance of lithium-ion secondary batteries due to necking. Furthermore, the pore volume in the pore diameter range of 2 nm to 300 nm in the granules 10 can be reduced compared to when the olivine-type lithium manganese iron phosphate particles are pulverized and then carboxylic acid is added.
[0063] (3) The carboxylic acid is citric acid. Citric acid has a high ability to capture metals such as Li, Mn, and Fe that are eluted during grinding, thereby more significantly achieving the effect of (2).
[0064] (4) The content of the carboxylic acid in the slurry is 10 parts by mass or less per 100 parts by mass of the olivine-type lithium manganese iron phosphate. In this case, it is possible to produce granules 10 having a small pore volume in the pore diameter range of 2 nm to 300 nm.
[0065] <Modifications> This embodiment can be modified as follows: This embodiment and the following modifications can be combined and implemented within the scope of technical compatibility.
[0066] In the method for producing a positive electrode material, the timing of adding the carboxylic acid may be changed. For example, in a mixing step, a first slurry containing olivine-type lithium manganese iron phosphate particles, an aqueous solvent, and a carbon source is prepared. Then, in a pulverizing step, the olivine-type lithium manganese iron phosphate particles contained in the first slurry are pulverized while adding a carboxylic acid or a carboxylic acid solution. In this case, too, the particles are pulverized in an aqueous solvent in the presence of a carboxylic acid, thereby suppressing the occurrence of necking due to the carboxylic acid capturing eluted metals.
[0067] Examples that further embody the above-described embodiment will be described below. <Preparation of olivine-type lithium manganese iron phosphate> Pure water (12,000 ml), LiOH (245 g) as a Li source, MnCO (300 ml) as a Mn source, 3 (840 g), Fe as the Fe source 2 C 2 O 4 (401 g), and PO 4 H as a source 3 P.O. 4 A first precursor slurry was obtained by mixing the Li, Mn, and Fe sources (1,125 g). After adding beads (media particles) with a diameter of 0.3 mm to the obtained first precursor slurry, the Li source, Mn source, and Fe source contained in the first precursor slurry were pulverized using a bead mill. This resulted in a second precursor slurry containing pulverized Li, Mn, and Fe sources. The pulverization process using the bead mill was carried out so that the average particle diameter (D50) of the Li, Mn, and Fe sources was within the range of 50 nm to 1,000 nm. Next, the second precursor slurry was dried and granulated using a spray dryer (drying outlet temperature: 200°C) to obtain a dried precursor. The obtained dried precursor was then pulverized using N 2 By heating at 500°C for 6 hours under atmospheric pressure, a compound of the general formula LiMn 0.75 Fe 0.25 P.O. 4 An olivine-type lithium manganese iron phosphate represented by the formula:
[0068] <Preparation of Granules> [Example 1] The olivine-type lithium manganese iron phosphate (45 g), fructose as a carbon source, and citric acid (2 g) as a carboxylic acid were mixed in pure water (405 ml) to obtain a first slurry. The amount of fructose was such that the total carbon amount, which is the sum of the carbon in fructose and the carbon in citric acid, was 2.5 parts by mass per 100 parts by mass of the olivine-type lithium manganese iron phosphate.
[0069] Beads (medium particles) having a diameter of 0.1 mm were added to the obtained first slurry, and then the olivine-type lithium manganese iron phosphate contained in the first slurry was pulverized using a bead mill. This resulted in a second slurry containing pulverized olivine-type lithium manganese iron phosphate. The pulverization process using the bead mill was carried out so that the average particle diameter (D50) of the olivine-type lithium manganese iron phosphate was in the range of 60 nm to 100 nm.
[0070] Next, the second slurry was dried and granulated using a spray dryer (drying outlet temperature: 200°C) to obtain aggregates of the above-mentioned pulverized material. 2 The fructose and citric acid contained in the aggregates were carbonized by heating at 650°C for 6 hours in an atmosphere, thereby obtaining granules of Example 1 having a core composed of olivine-type lithium iron manganese phosphate and a carbon coating formed on the surface of the core.
[0071] Examples 2 to 10 and Comparative Examples 1 to 4 Examples 2 to 10 and Comparative Examples 1 to 4 are examples in which the amount of citric acid was changed. Granules of Examples 2 to 10 and Comparative Examples 1 to 4 were obtained by the same method as Example 1, except that the amounts of citric acid and fructose in the first slurry were changed. The amount of citric acid in each example is as shown in Table 2 below. The amount of fructose in each example was adjusted to match the amount of citric acid so that the total carbon content was 2.5 parts by mass per 100 parts by mass of the olivine-type lithium manganese iron phosphate.
[0072] Comparative Examples 5 to 7 are examples in which the pulverization treatment using a bead mill was mainly performed roughly. Granules of Comparative Example 5 were obtained in the same manner as in Example 1, except that the amount of citric acid was set to 0 and the pulverization treatment using a bead mill was performed so that the average particle size (D50) of the olivine-type lithium manganese iron phosphate was in the range of 60 nm to 150 nm.
[0073] Granules of Comparative Example 6 were obtained in the same manner as in Example 5, except that the pulverization treatment using a bead mill was carried out so that the average particle size (D50) of the olivine-type lithium manganese iron phosphate was in the range of 100 nm or more and 120 nm or less.
[0074] A granule of Comparative Example 7 was obtained in the same manner as in Example 5, except that the pulverization treatment using a bead mill was carried out so that the average particle size (D50) of the olivine-type lithium manganese iron phosphate was in the range of 140 nm or more and 160 nm or less.
[0075] Comparative Examples 8 to 9 are examples in which the amount of fructose used as the carbon source was increased. Granules of Comparative Example 8 were obtained in the same manner as in Example 5, except that the total carbon content was adjusted to 3.2 parts by mass per 100 parts by mass of the olivine-type lithium manganese iron phosphate.
[0076] Granules of Comparative Example 9 were obtained in the same manner as in Example 5, except that the total carbon amount was adjusted to 5.1 parts by mass per 100 parts by mass of olivine-type lithium manganese iron phosphate.
[0077] Comparative Example 10 is an example in which the timing of adding citric acid was changed. Granules of Comparative Example 10 were obtained in the same manner as in Example 1, except that citric acid (2 g) was not mixed into the first slurry, but was mixed into the second slurry after the pulverization treatment using a bead mill.
[0078] <Analysis of Granules> For the granules of each Example and Comparative Example, the particle size of the primary particles, the pore volume in the pore size range of 2 nm to 300 nm, and the carbon content were measured. The results are shown in Table 2.
[0079] The particle size of the primary particles was determined as follows: Using the SAXS method, the particle size distribution of the primary particles was determined assuming that the primary particles were spherical. The average particle size (D50) obtained from the determined particle size distribution was calculated, and this value was used as the particle size of the primary particles.
[0080] The pore volume was determined as follows. The pores of the positive electrode active material were measured using a specific surface area / pore distribution measurement device. From analysis by the BJH method, the cumulative pore distribution of the granules in the pore diameter range of 2 nm to 300 nm was determined. The pore diameter was plotted on the horizontal axis and the cumulative pore volume on the vertical axis, and the pore volume in the pore diameter range of 2 nm to 300 nm was calculated from the difference between the cumulative pore volumes for pore diameters of 2 nm and 300 nm.
[0081] The carbon content was measured using a carbon / sulfur analyzer. <Preparation of Positive Electrode> A positive electrode composite was coated on one surface of a 15 μm thick aluminum foil. The coated positive electrode composite was dried to prepare a positive electrode in which a positive electrode active material layer was formed on one surface of a positive electrode current collector. The positive electrode composite used was a slurry containing the granules (positive electrode active material) of each Example and Comparative Example, carbon nanotubes (conductive additive), carboxymethyl cellulose (binder), and styrene-butadiene rubber (binder) in a solid content mass ratio of 98.25:0.05:0.4:1.3, with water as the solvent. The basis weight of the positive electrode active material layer in each prepared positive electrode was measured. As a result, the measured values were all approximately 65 to 75 mg / cm. 2 It was.
[0082] <Evaluation of Film Formability> The surface condition of the positive electrode active material layer of each prepared positive electrode was evaluated visually. The results are shown in Table 2. The evaluation criteria are as follows. For reference, FIG. 4( a) shows a photograph of the positive electrode active material layer using Example 1, which was evaluated as having a film formability of "good," and FIG. 4( b) shows a photograph of the positive electrode active material layer using Comparative Example 1, which was evaluated as having a film formability of "poor."
[0083] "Good": No cracks on the surface of the positive electrode active material layer. "Positive": Cracks present on the surface of the positive electrode active material layer. <Electrochemical Test> Positive electrode half-cells were fabricated using the fabricated positive electrodes that were rated "Good" in the film-forming property evaluation. The fabricated positive electrode was cut into a 25 mm square to form a positive electrode (evaluation electrode), and a negative electrode made of 200 μm-thick lithium metal foil cut into a 27 mm square. A separator was sandwiched between the positive electrode (evaluation electrode) and a negative electrode made of 200 μm-thick lithium metal foil cut into a 27 mm square to form an electrode body battery. The electrode body battery was housed in a laminate exterior, and a nonaqueous electrolyte was injected and sealed to obtain a half-cell for electrochemical testing. A glass filter manufactured by Hoechst Celanese was used as the separator. The nonaqueous electrolyte used was a nonaqueous electrolyte prepared by dissolving lithium hexafluorophosphate to a concentration of 1 M in a mixed solvent of ethylene carbonate and diethyl carbonate in a volume ratio of 1:1.
[0084] The prepared positive electrode half cell was charged at 25° C. with a constant current of 0.05 C up to 4.3 V and then discharged down to 3.0 V. The discharge capacity at this time was measured. The results are shown in Table 2.
[0085]
[0086] As shown in Table 2, the granules of Examples 1 to 10 satisfy all of the following three conditions: Condition 1: The particle size of the primary particles is 100 nm or less.
[0087] Condition 2: Pore volume is 0.2 cm 3 / g or less. Condition 3: The carbon content is 3.0 mass% or less. No cracks were observed on the surface of the positive electrode active material layers formed using the granules of Examples 1 to 10 as the positive electrode active material. The discharge capacities when the granules of Examples 1 to 10 were used as the positive electrode active material were 147 to 149.1 mAh / g.
[0088] In contrast, the granules of Comparative Examples 1 to 4 satisfy Conditions 1 and 3, but do not satisfy Condition 2 regarding pore volume due to their large pore volume. Cracks were observed on the surface of the positive electrode active material layers formed using the granules of Comparative Examples 1 to 4 as the positive electrode active material. From these results, in order to ensure good film formability when forming a positive electrode active material layer with a large basis weight, it is necessary to keep the pore volume at 0.2 cm 3 It can be seen that it is effective to set the value to / g or less.
[0089] On the other hand, the granules of Comparative Examples 5 to 7 satisfied Conditions 2 and 3, but did not satisfy Condition 1 due to the large particle size of the primary particles. No cracks were observed on the surface of the positive electrode active material layers formed using the granules of Comparative Examples 5 to 7 as the positive electrode active material. However, the discharge capacities when the granules of Comparative Examples 5 to 7 were used as the positive electrode active material were 132 to 141 mAh / g, which were significantly lower than the discharge capacities when the granules of Examples 1 to 10 were used as the positive electrode active material.
[0090] The granules of Comparative Examples 8 to 9 satisfied Conditions 1 and 2, but did not satisfy Condition 3 due to their high carbon content. No cracks were observed on the surface of the positive electrode active material layers formed using the granules of Comparative Examples 8 to 9 as the positive electrode active material. However, the discharge capacities of the granules of Comparative Examples 8 to 9 used as the positive electrode active material were 133.5 to 139.9 mAh / g, which were significantly lower than the discharge capacities of the granules of Examples 1 to 10 used as the positive electrode active material.
[0091] The above results when the granules of Comparative Examples 5 to 9 were used indicate that the effect of increasing the capacity of a lithium ion secondary battery cannot be obtained by simply forming a positive electrode active material layer with a large basis weight. 3 / g or less, it is also necessary to make the particle size of the primary particles 100 nm or less and the carbon content 3.0 mass % or less.
[0092] Next, we consider the relationship between the amount of citric acid blended and the pore volume of the resulting granules. Referring to the results of Examples 1 to 10 and Comparative Examples 1 to 3, within the range of 10 parts by mass or less of citric acid blended per 100 parts by mass of olivine-type lithium manganese iron phosphate, the pore volume of the resulting granules decreases as the amount of citric acid blended increases. Meanwhile, the pore volume of the granules of Comparative Example 4, in which the amount of citric acid blended was 15 parts by mass, is more than twice the pore volume of the granules of Examples 8 to 10, in which the amount of citric acid blended was 10 parts by mass. These results demonstrate that the pore volume of the granules can be reduced by increasing the amount of carboxylic acid, such as citric acid, but that the pore volume of the granules increases when the amount of carboxylic acid blended exceeds a certain amount.
[0093] Next, the timing of adding citric acid will be considered. Comparative Example 10 is an example in which citric acid was not mixed into the first slurry, but was mixed into the second slurry after the pulverization treatment. The pore volume of the granules of Comparative Example 10 is 1.5 times larger than the pore volume of the granules of Example 1, which differs only in the timing of adding citric acid. This result shows that in order to reduce the pore volume, it is necessary to perform the pulverization treatment in the presence of a carboxylic acid such as citric acid.
Claims
1. General formula LiMn x Fe y P.O. 4 (x and y are numbers satisfying x+y=1, 0<x<1, 0<y<1), and a carbon coating formed on a surface of the core, wherein the core has a structure in which primary particles of the olivine-type lithium manganese iron phosphate are aggregated, the primary particles have a particle diameter of 100 nm or less, and the pore volume in the pore diameter range of 2 nm to 300 nm in the granules is 0.2 cm 3 / g or less, and the carbon content of the granules is 1.8% by mass or more and 3.0% by mass or less.
2. A positive electrode for a lithium ion secondary battery, comprising: a positive electrode current collector having a first surface; and a positive electrode active material layer formed on the first surface of the positive electrode current collector, the positive electrode active material layer containing the positive electrode material for a lithium ion secondary battery as defined in claim 1.
3. The weight of the positive electrode active material layer is 30 mg / cm 2 100mg / cm or more 2 3. The positive electrode for a lithium ion secondary battery according to claim 2, wherein:
4. General formula LiMn x Fe y P.O. 4 (x and y are numbers satisfying x+y=1, 0<x<1, 0<y<1), in the presence of an aqueous solvent, a carbon source, and a carboxylic acid to prepare a slurry containing the pulverized material of the olivine-type lithium manganese iron phosphate; spray-drying the slurry to obtain an aggregate of the pulverized material; and calcining the aggregate to carbonize the carbon source contained in the aggregate.
5. The method for producing a positive electrode material for a lithium ion secondary battery according to claim 4, wherein the carboxylic acid is citric acid.
6. A method for producing a positive electrode material for a lithium ion secondary battery as described in claim 4 or 5, wherein the content of the carboxylic acid in the slurry is 2 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the olivine-type lithium manganese iron phosphate.
Citation Information
Patent Citations
Lithium ion secondary battery
JP2019185920A
Method for producing inorganic particle
JP2009062256A
Manufacturing method of positive electrode active material of lithium secondary battery
JP2016149297A
Positive electrode material for lithium ion secondary battery, positive electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2020126783A