Positive electrode active material for non-aqueous electrolyte secondary battery, positive electrode for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for manufacturing positive electrode active material for non-aqueous electrolyte secondary battery
The use of a lithium-containing transition metal composite oxide with a sulfonic acid compound and additional elements on the surface of secondary particles addresses the limitations of existing non-aqueous electrolyte secondary batteries, enhancing output and cycle characteristics during high-rate charging by reducing reaction resistance and protecting against hydrogen fluoride.
Patent Information
- Application Number
- PCT/JP2024/013926
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-04
- Publication Date
- 2024-10-31
AI Technical Summary
Existing non-aqueous electrolyte secondary batteries face challenges in improving output characteristics and cycle characteristics during high-rate charging while maintaining high capacity, as techniques in Patent Documents 1 and 2 are insufficient.
A positive electrode active material comprising a lithium-containing transition metal composite oxide with a layered structure, where the surface of secondary particles is coated with a sulfonic acid compound and additional elements like P, Ca, Sr, B, Zr, or Al, which reduces reaction resistance and protects against hydrogen fluoride, enhancing the battery's performance.
The proposed solution significantly improves output characteristics and cycle characteristics during high-rate charging by reducing reaction resistance and protecting the lithium-containing transition metal composite oxide from hydrogen fluoride, resulting in a non-aqueous electrolyte secondary battery with enhanced performance.
Smart Images

Figure JP2024013926_31102024_PF_FP_ABST
Abstract
Description
Positive electrode active material for non-aqueous electrolyte secondary battery, positive electrode for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for manufacturing positive electrode active material for non-aqueous electrolyte secondary battery
[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery, a positive electrode for a non-aqueous electrolyte secondary battery, a non-aqueous electrolyte secondary battery, and a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery.
[0002] In recent years, the applications of non-aqueous electrolyte secondary batteries have expanded to include power sources for electric vehicles and power storage devices for utilizing natural energy. The characteristics required of the positive electrode active material used in non-aqueous electrolyte secondary batteries also vary depending on the application. For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery that uses a lithium-containing transition metal composite oxide to which niobium, tungsten, or molybdenum is added as a positive electrode active material in order to improve charge / discharge capacity, charge / discharge efficiency, and cycle characteristics. Patent Document 2 also discloses a non-aqueous electrolyte secondary battery that uses a lithium-containing transition metal composite oxide with a low-solubility Li salt scattered on the surface as a positive electrode active material in order to reduce reaction resistance during storage at high temperatures.
[0003] International Publication No. 2023 / 013494 Japanese Patent Application Laid-Open No. 2019-169286
[0004] In non-aqueous electrolyte secondary batteries, it is important to improve output characteristics and cycle characteristics during high-rate charging while maintaining high capacity. The techniques described in Patent Documents 1 and 2 cannot adequately address these challenges, and there is still much room for improvement.
[0005] A positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a lithium-containing transition metal composite oxide having a layered structure, and the lithium-containing transition metal composite oxide is represented by the general formula Li x Ni a Co b Mn c M d O 2-y(wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and are secondary particles formed by aggregation of primary particles, characterized in that the surfaces of the secondary particles are provided with a sulfonic acid compound represented by formula (I) and a compound X containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al, and the sulfonic acid compound is present on the surfaces of the secondary particles via compound X. (wherein A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
[0006] A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure includes: a synthesis step of obtaining a lithium-containing transition metal composite oxide; a washing step of washing the lithium-containing transition metal composite oxide with water and dehydrating it to obtain a cake-like composition; an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition; and a drying step of drying the cake-like composition to obtain a powder-like composition. The method is characterized in that, in the washing step or the addition step, a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al is added to the cake-like composition before adding at least one of the sulfonic acid compound and the sulfonic acid solution.
[0007] A positive electrode for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure is characterized by including the above positive electrode active material.
[0008] A non-aqueous electrolyte secondary battery according to one aspect of the present disclosure is characterized by including a positive electrode containing the above-described positive electrode active material, a negative electrode, and a non-aqueous electrolyte.
[0009] According to the positive electrode active material for a nonaqueous electrolyte secondary battery of one aspect of the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery that ensures high capacity while improving output characteristics and cycle characteristics during high-rate charging.
[0010] 1 is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention;
[0011] The layered rock salt structure of a lithium-containing transition metal composite oxide has a transition metal layer such as Ni, a Li layer, and an oxygen layer, and the charge / discharge reaction of the battery progresses as Li ions present in the Li layer reversibly enter and exit. Generally, lithium nickel oxide-based lithium-containing transition metal composite oxides containing Ni as a main component are known as high-capacity positive electrode active materials. From the viewpoint of increasing the capacity of the battery, the Ni content in the lithium-containing transition metal composite oxide is preferably 75 mol % or more relative to the total number of moles of metal elements excluding Li.
[0012] As a result of investigations by the present inventors, it has become clear that a nonaqueous electrolyte secondary battery with improved output characteristics can be realized by having the sulfonic acid compound represented by the above formula (I) present on the surface of secondary particles of a lithium-containing transition metal composite oxide used as a positive electrode active material. This is thought to be because the reaction resistance in the positive electrode is reduced by the function of the sulfonic acid compound.
[0013] On the other hand, during high-rate charging, hydrogen fluoride may be generated due to decomposition of the non-aqueous electrolyte. When a lithium-containing transition metal composite oxide with a Ni content of 75% or more is used as the positive electrode active material, the generated hydrogen fluoride may react with the positive electrode, resulting in a deterioration in the cycle characteristics of the non-aqueous electrolyte secondary battery. This is presumably due to the reaction of hydrogen fluoride with the lithium-containing transition metal composite oxide, which causes reaction products to deposit on the surface of the lithium-containing transition metal composite oxide or causes transition metals to leach out of the lithium-containing transition metal composite oxide.
[0014] Therefore, the present inventors conducted extensive research to solve the above problems and found that by having a compound (hereinafter, compound X) containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al, in addition to a sulfonic acid compound, present on the surface of secondary particles of a lithium-containing transition metal composite oxide, and by having the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide via compound X, the output characteristics and cycle characteristics during high-rate charging can be improved. This is presumably because the sulfonic acid compound reduces the reaction resistance at the positive electrode, while the generated hydrogen fluoride is allowed to react preferentially with compound X, thereby protecting the lithium-containing transition metal composite oxide from hydrogen fluoride.
[0015] Hereinafter, an example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail with reference to the drawings. Note that configurations obtained by selectively combining the components of the multiple embodiments and variations described below are included within the scope of the present disclosure. Furthermore, in this specification, "to" refers to a range that includes the upper and lower limits before and after "to."
[0016] In the following, a cylindrical battery in which a wound electrode assembly 14 is housed in a cylindrical, bottomed exterior body 16 is exemplified as a nonaqueous electrolyte secondary battery; however, the exterior body of the battery is not limited to a cylindrical exterior body. The nonaqueous electrolyte secondary battery according to the present disclosure may be, for example, a prismatic battery with a prismatic exterior body, a coin-type battery with a coin-shaped exterior body, or a pouch-type battery with an exterior body composed of a laminate sheet including a metal layer and a resin layer. Furthermore, the electrode assembly is not limited to a wound type, but may also be a stacked type electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately stacked with separators interposed therebetween. Furthermore, the design of the nonaqueous electrolyte secondary battery according to the present disclosure is not limited to the design of the exemplified nonaqueous electrolyte secondary battery, and known nonaqueous electrolyte secondary battery designs may also be applied.
[0017] FIG. 1 is an axial cross-sectional view of a cylindrical nonaqueous electrolyte secondary battery 10 according to an embodiment. As shown in FIG. 1 , the nonaqueous electrolyte secondary battery 10 includes a wound electrode assembly 14, a nonaqueous electrolyte, and an exterior body 16 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The exterior body 16 is a cylindrical metal container with a bottom that is open on one axial side, and the opening of the exterior body 16 is closed by a sealing body 17. Hereinafter, for convenience of explanation, the sealing body 17 side of the battery will be referred to as the top, and the bottom side of the exterior body 16 will be referred to as the bottom.
[0018] The positive electrode 11, negative electrode 12, and separator 13 that make up the electrode assembly 14 are all rectangular, elongated bodies that are spirally wound in the longitudinal direction and stacked alternately in the radial direction of the electrode assembly 14. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other. Two separators 13 are arranged, for example, to sandwich the positive electrode 11. The electrode assembly 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like. In the electrode assembly 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the lateral direction of the positive electrode 11 and the negative electrode 12 is the axial direction. That is, the lateral end faces of the positive electrode 11 and the negative electrode 12 form the axial end faces of the electrode assembly 14.
[0019] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the exterior body 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the exterior body 16 by welding or the like, and the exterior body 16 serves as the negative electrode terminal.
[0020] A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior body 16 has a grooved portion 22 formed on its side surface that protrudes inward and supports the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the exterior body 16 by the grooved portion 22 and the open end of the exterior body 16 that is crimped to the sealing body 17.
[0021] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0022] The positive electrode 11, negative electrode 12, separator 13, and nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10, particularly the positive electrode active material that constitutes the positive electrode 11, will be described in detail below.
[0023] [Positive Electrode] The positive electrode 11 has, for example, a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core. The positive electrode mixture layer is preferably formed on both sides of the positive electrode core. The positive electrode core can be made of a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The thickness of the positive electrode core is, for example, 10 μm to 30 μm.
[0024] The positive electrode mixture layer contains, for example, a positive electrode active material, a conductive agent, and a binder. The thickness of the positive electrode mixture layer is, for example, 10 μm to 150 μm on one side of the positive electrode core. The positive electrode 11 can be produced, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a conductive agent, etc. to the surface of the positive electrode core, drying the coating, and then rolling it to form a positive electrode mixture layer on both sides of the positive electrode core.
[0025] Examples of the conductive agent contained in the positive electrode mixture layer include carbon black (CB) such as acetylene black (AB) and ketjen black, carbon nanotubes (CNT), graphene, and carbon particles such as graphite. These may be used alone or in combination of two or more.
[0026] Examples of binders contained in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyimide-based resins, acrylic-based resins, polyolefin-based resins, polyacrylonitrile (PAN), etc. These may be used alone or in combination of two or more.
[0027] The positive electrode active material contained in the positive electrode mixture layer includes a lithium-containing transition metal composite oxide. The lithium-containing transition metal composite oxide includes secondary particles formed by aggregation of primary particles. The particle size of the primary particles constituting the secondary particles of the lithium-containing transition metal composite oxide is, for example, 0.02 μm to 2 μm. The particle size of the primary particles is measured as the diameter of the circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The average particle size of the secondary particles of the lithium-containing transition metal composite oxide is, for example, 2 μm to 30 μm. Here, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also referred to as the median diameter. The particle size distribution of the secondary particles of the lithium-containing transition metal composite oxide can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.
[0028] The lithium-containing transition metal composite oxide has a layered structure. Examples of the layered structure of the lithium-containing transition metal composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and stabilizing the crystal structure, the lithium-containing transition metal composite oxide preferably has a layered structure belonging to the space group R-3m. The layered structure of the lithium-containing transition metal composite oxide may include a transition metal layer and a Li layer.
[0029] The lithium-containing transition metal composite oxide has the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr.) The content of the elements constituting the lithium-containing transition metal composite oxide can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0030] By setting the Ni content in the lithium-containing transition metal composite oxide to 75 mol % to 95 mol %, a battery with a high capacity can be obtained. The higher the Ni content, the higher the capacity of the battery.
[0031] The content of Co in the lithium-containing transition metal composite oxide is 0 mol % to 15 mol %, and Co is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Co. By containing Co, the lithium-containing transition metal composite oxide can improve the heat resistance of the battery.
[0032] The content of Mn in the lithium-containing transition metal composite oxide is 0 mol % to 25 mol %, and Mn is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain Mn. By containing Mn, the lithium-containing transition metal composite oxide can stabilize its crystal structure.
[0033] The content of M (M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr) in the lithium-containing transition metal composite oxide is 0 mol % to 10 mol %, and M is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain M.
[0034] A compound (compound X) containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. Compound X is present in the form of particles or layers on the surface of the secondary particles. Compound X is highly reactive with hydrogen fluoride, and therefore reacts preferentially with hydrogen fluoride produced by decomposition of the non-aqueous electrolyte, thereby protecting the lithium-containing transition metal composite oxide from hydrogen fluoride.
[0035] The compound X is, for example, a compound containing at least one of phosphate, sulfate, oxide, hydroxide, and chloride containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al. 3 P.O. 4 , CaO, CaCl 2 , Ca(OH) 2 , SrO, SrCl 2 , Sr(OH) 2 , B 2 O 3 , B(OH) 3 , ZrSO 4 , ZrO 2 , Er 2 (SO 4 ) 3 , Al 2 O 3 , Al(OH) 3 , NaAl(OH) 4 , AlPO 4The compound X may be used singly or in combination of two or more.
[0036] The amount of P, Ca, Sr, B, Zr, Er, and Al contained in the compound X in the positive electrode active material is preferably 0.001% by mass to 1% by mass, and more preferably 0.01% by mass to 1% by mass, relative to the mass of the lithium-containing transition metal composite oxide. In this case, the effects of the present disclosure are more pronounced. Note that when multiple types of compound X are used, it is preferable that the total amount of P, Ca, Sr, B, Zr, Er, and Al contained in all of the compounds X be within the above range.
[0037] The presence of compound X can be confirmed by synchrotron XRD measurement, X-ray photoelectron spectroscopy (XPS), time-of-flight secondary ion mass spectrometry (TOF-SIMS), etc. Compound X may be present scattered on the secondary particles so as to cover at least a portion of the surface, or may be present so as to cover the entire surface of the secondary particles. Compound X is preferably directly attached to the surface of the secondary particles. Compound X may also be present on the surface of the primary particles of the lithium-containing transition metal composite oxide.
[0038] The sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. The sulfonic acid compound is present in the form of particles or layers on the surface of the secondary particles. As described above, since compound X is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide, the sulfonic acid compound is present on the surface of the secondary particles via compound X. In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2. A is preferably a Group 1 element. Among these, Li or Na is more preferred, and Li is particularly preferred.
[0039] In formula (I), R is preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 5 or less, more preferably 3 or less. From the viewpoint of reducing reaction resistance, a suitable example of R is an alkyl group having 3 or less carbon atoms, and among these, a methyl group is preferred. In R, some of the hydrogen atoms bonded to the carbon may be substituted with fluorine. In formula (I), n is preferably 1.
[0040] Specific examples of the sulfonic acid compound include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, sodium ethanesulfonate, magnesium methanesulfonate, lithium fluoromethanesulfonate, etc. Among these, at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and sodium methanesulfonate is preferred, with lithium methanesulfonate being particularly preferred.
[0041] The sulfonic acid compound reduces the reaction resistance in the positive electrode 11, thereby improving the initial output characteristics of the battery. Even a very small amount of the sulfonic acid compound can achieve this effect, but it is preferable for the sulfonic acid compound to be present on the secondary particle surface of the composite oxide in an amount of 0.05% by mass or more relative to the mass of the lithium-containing transition metal composite oxide. The upper limit of the sulfonic acid compound content is not particularly limited, but from the viewpoint of cycle characteristics, 1.5% by mass relative to the mass of the lithium-containing transition metal composite oxide is preferred. Therefore, an example of a suitable range for the amount of the sulfonic acid compound is 0.05% by mass to 1.5% by mass relative to the mass of the lithium-containing transition metal composite oxide.
[0042] The presence of the sulfonic acid compound on the surface of the secondary particles of the lithium-containing transition metal composite oxide can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material containing lithium methanesulfonate exhibits, for example, a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm-1 , 1065 cm -1 The peak around 785 cm is due to the SO stretching vibration of lithium methanesulfonate. -1 The peak around 1000 nm is a peak due to the C-S stretching vibration derived from lithium methanesulfonate. Note that the presence of a positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate can also be confirmed from the absorption peak derived from the sulfonic acid compound in the infrared absorption spectrum.
[0043] The presence of the sulfonic acid compound can also be confirmed by X-ray photoelectron spectroscopy (XPS). In the spectrum obtained by XPS, a peak with a binding energy of approximately 165 to 170 eV and an intensity (c / s) of 200 to 1000 is observed for the positive electrode active material containing lithium methanesulfonate. The presence of the sulfonic acid compound on the secondary particle surface of the lithium-containing transition metal composite oxide can also be confirmed by ICP, atomic absorption spectroscopy, synchrotron XRD measurement, TOF-SIMS, etc.
[0044] The sulfonic acid compound may be present so as to coat at least a portion of the surface of the secondary particles of the lithium-containing transition metal composite oxide, similarly to compound X, or may be present so as to coat the entire surface of the secondary particles. When compound X is present in the form of a layer covering the entire surface of the secondary particles, substantially all of the sulfonic acid compound is fixed to the surface of compound X and is present on the surface of the secondary particles via compound X. Furthermore, a first layer made of compound X and a second layer made of the sulfonic acid compound covering the first layer may be formed on the surface of the secondary particles.
[0045] The sulfonic acid compound is preferably adhered to the surface of compound X, but may also be adhered directly to the surface of the secondary particles without via compound X. In this case, the mass of the sulfonic acid compound present on the surface of the secondary particles via compound X is preferably greater than the mass of the sulfonic acid compound directly adhered to the surface of the secondary particles. Furthermore, the sulfonic acid compound may be interposed between compound X and the secondary particles, provided that the object of the present disclosure is not impaired. Furthermore, one particle of the sulfonic acid compound may be present in contact with both the particle surface of compound X and the surface of the secondary particles. Furthermore, the sulfonic acid compound may also be present on the surface of the primary particles of the lithium-containing transition metal composite oxide.
[0046] The positive electrode active material, which is one example of the embodiment, can be produced by the following method: Note that the production method described here is only an example, and the method for producing the positive electrode active material is not limited to this method.
[0047] The manufacturing process of the positive electrode active material includes a synthesis step of obtaining a lithium-containing transition metal composite oxide, a washing step of washing the lithium-containing transition metal composite oxide obtained in the synthesis step with water and dehydrating it to obtain a cake-like composition, an adding step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition, and a drying step of drying the cake-like composition to obtain a powder-like composition.
[0048] In the synthesis step, for example, a metal oxide containing 75 mol% to 95 mol% of Ni, 0 mol% to 15 mol% of Co, 0 mol% to 25 mol% of Mn, and 0 mol% to 10 mol% of M (M is at least one element selected from W, Mg, Mo, Nb, Ti, Si, Al, and Zr) is mixed with a Li compound to obtain a mixture.
[0049] The metal oxide can be obtained, for example, by adding an alkaline solution such as sodium hydroxide dropwise to a stirred solution of a metal salt containing Ni and an arbitrary metal element (Co, Mn, M, etc.) to adjust the pH to the alkaline side (e.g., 8.5 to 12.5) to precipitate (co-precipitate) a composite hydroxide containing Ni and the arbitrary metal element, and then heat-treating the composite hydroxide. The heat-treatment temperature is not particularly limited, but is, for example, in the range of 250°C to 600°C.
[0050] Examples of Li compounds include Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of the metal oxide include O, LiH, and LiF. In order to facilitate adjustment of the above-mentioned parameters to the ranges specified above, the mixing ratio of the metal oxide and the Li compound is preferably such that the molar ratio of the total amount of metal elements in the metal oxide to Li falls within a range of 1:0.8 to 1:1.2, and more preferably falls within a range of 1:1.0 to 1:1.01.
[0051] Next, the synthesis step includes a calcination step in which the resulting mixture is calcined. The calcination step is a multi-stage calcination step that includes at least a first calcination step in which the mixture is calcined at 300°C to 680°C under an oxygen stream, and a second calcination step in which the calcined product obtained by the first calcination step is calcined at a temperature exceeding 680°C under an oxygen stream. In the first calcination step, the temperature is increased to a first set temperature of 680°C or less at a first temperature increase rate of 0.2°C / min to 4.5°C / min. In the second calcination step, the temperature is increased to a second set temperature of 900°C or less at a first temperature increase rate of 0.5°C / min to 3.5°C / min. Note that multiple first and second temperature increase rates may be set for each temperature range as long as they are within the above-specified range.
[0052] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time during which the first set temperature is maintained after reaching the first set temperature, and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 hour to 10 hours, more preferably 1 hour to 5 hours. The holding time of the second set temperature is the time during which the second set temperature is maintained after reaching the second set temperature. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / min. 3 The flow rate shall be 0.2 mL / min to 4 mL / min per kg of the mixture or 0.3 L / min or more per kg of the mixture.
[0053] The synthesis step is not limited to the above steps, and may include, for example, a known synthesis method in which a precursor obtained by co-precipitating or mixing a compound such as a hydroxide, oxide, or carbonate containing at least one element selected from Ni, Co, Mn, and M (M is at least one element selected from W, Mg, Mo, Nb, Ti, Si, Al, and Zr) is mixed with a Li source and fired to obtain a lithium-containing transition metal composite oxide. When the precursor does not contain a compound such as M, these compounds such as M may be mixed and fired when the precursor and Li source are mixed and fired. Furthermore, these compounds may be pulverized to appropriately change the particle shape or particle size, or may be used after adjusting the water content by including a hydrate.
[0054] In the washing step, the lithium-containing transition metal composite oxide is washed with water and dehydrated to obtain a cake-like composition. The particulate lithium-containing transition metal composite oxide obtained in the synthesis step can be used. By washing with water, unreacted lithium compounds added in the synthesis step and impurities other than the lithium compounds can be removed. When washing with water, for example, 300 g to 5000 g of lithium-containing transition metal composite oxide is added to 1 L of water. Note that water washing may be repeated multiple times. Dehydration after water washing can be performed, for example, using a filter press.
[0055] In the addition step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step. This allows the sulfonic acid compound to adhere to the surface of the lithium-containing transition metal composite oxide. The sulfonic acid compound may be in either powder or solution form. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when the sulfonic acid solution is added, a Li-containing sulfonic acid compound is formed. From the viewpoint of more easily achieving the effects of the present application, a Li compound or a Li compound solution may be added to the cake-like composition together with the sulfonic acid solution, or a mixed solution obtained by premixing the sulfonic acid solution with the Li compound or the Li compound solution may be added to the cake-like composition. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution obtained by dissolving LiOH in water. The amounts of the Li compound and sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The amount of sulfonic acid compound or sulfonic acid added is preferably 0.05% by mass to 1.5% by mass, and more preferably 0.1% by mass to 1.0% by mass, relative to the mass of the lithium-containing transition metal composite oxide. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass to 40% by mass.
[0056] Here, in the washing step or the adding step, a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al is added to the cake-like composition before the addition of the sulfonic acid compound. That is, when the compound is added in the adding step, at least one of the sulfonic acid compound and the sulfonic acid solution is added after the compound is added. This allows compound X to be directly fixed to the surface of the secondary particles. Compound X may be present on the surface of the secondary particles in a form different from that of the compound added in the adding step. Furthermore, a heat treatment may be performed after the addition of the compound in the adding step. The heating temperature is, for example, 100°C to 450°C. The heat treatment may be performed after the drying step described below.
[0057] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed in a vacuum atmosphere. The drying conditions are, for example, 150°C to 400°C and 0.5 hours to 15 hours.
[0058] [Negative Electrode] The negative electrode 12 may have, for example, a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core, or a metal Li foil may be used as the negative electrode 12. Alternatively, the negative electrode 12 may have a negative electrode core, and lithium metal may be deposited on the surface of the negative electrode core upon charging. When the negative electrode 12 has a negative electrode mixture layer, the negative electrode mixture layer is preferably formed on both sides of the negative electrode core. The negative electrode core may be made of a foil of a metal that is stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film with such a metal disposed on the surface layer. The thickness of the negative electrode core is, for example, 5 μm to 30 μm. The negative electrode mixture layer includes, for example, a negative electrode active material and a binder. The thickness of the negative electrode mixture layer is, for example, 10 μm to 150 μm on one side of the negative electrode core. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. to the surface of a negative electrode core, drying the coating, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode core.
[0059] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite are used. Graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides may also be used as the negative electrode active material. Furthermore, those provided with a carbon coating may also be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.
[0060] Examples of binders contained in the negative electrode mixture layer include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.
[0061] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.
[0062] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.
[0063] [Non-aqueous electrolyte] The non-aqueous electrolyte has ion conductivity (for example, lithium ion conductivity). The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0064] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).
[0065] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0066] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0067] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 to 1.8 mol per liter of the non-aqueous solvent.
[0068] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.
[0069] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.
[0070] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.
[0071] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.
[0072] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.
[0073] Hereinafter, the present disclosure will be further described with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0074] Example 1 Preparation of Positive Electrode Active Material [Ni 0.90 Mn 0.10 ](OH) 2The composite hydroxide represented by the formula (1) was calcined at 500°C for 8 hours to obtain a metal oxide containing Ni and Mn. Next, lithium hydroxide monohydrate (LiOH·H) was added to the composite hydroxide represented by the formula (1) so that the molar ratio of Li to the total amount of Ni and Mn was 1:1.03. 2 O) was mixed to obtain a mixture. Then, this mixture was placed under an oxygen flow (10 cm) with an oxygen concentration of 95%. 3 The mixture was heated from room temperature to 650°C at a temperature increase rate of 2.0°C / min under a temperature of 2 mL / min per kg of the mixture and 5 L / min per kg of the mixture, and then heated from 650°C to 740°C at a temperature increase rate of 0.5°C / min to obtain a lithium-containing transition metal composite oxide (synthesis step).
[0075] Water was added to the lithium-containing transition metal composite oxide obtained in the synthesis step so that the slurry concentration was 1500 g / L, and the mixture was stirred for 15 minutes and filtered to obtain a cake-like composition (washing step). 3 P.O. 4 was added. 3 P.O. 4 was added so that the mass of P in the positive electrode active material was 0.05% by mass with respect to the total mass of the lithium-containing transition metal composite oxide. 3 P.O. 4 Powdered lithium methanesulfonate was added to the cake-like composition to which the lithium methanesulfonate had been added (addition step). The amount of lithium methanesulfonate added was 0.3 mass% relative to the total mass of the lithium-containing transition metal composite oxide. The resulting cake-like composition was dried under vacuum at 180°C for 2 hours to obtain the positive electrode active material of Example 1 (drying step). The prepared positive electrode active material was measured by Fourier transform infrared spectroscopy (FT-IR), confirming the presence of lithium methanesulfonate on the surface of the secondary particles of the lithium-containing transition metal composite oxide. Furthermore, TOF-SIMS confirmed that a P-containing compound was present on the surface of the secondary particles as compound X, and that lithium methanesulfonate was present on the surface of the P-containing compound.
[0076] [Preparation of Positive Electrode] The positive electrode active material, acetylene black (AB), and polyvinylidene fluoride were mixed in a mass ratio of 86:10:4, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry was applied to a positive electrode core made of aluminum foil, the coating was dried and compressed, and then the positive electrode core was cut to a predetermined electrode size to obtain a positive electrode in which a positive electrode mixture layer was disposed on both sides of the positive electrode core. In addition, an exposed portion in which the surface of the positive electrode core was exposed was provided in a part of the positive electrode.
[0077] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0078] [Preparation of Test Cell] A positive electrode lead was attached to the exposed portion of the positive electrode, and a negative electrode lead was attached to the lithium metal foil serving as the negative electrode. The positive electrode and the negative electrode were spirally wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly. This electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into it. The opening of the exterior body was then sealed to obtain a test cell.
[0079] [Evaluation of Output Characteristics] The test cell was charged to 4.4 V (vs. Li) at a constant current of 0.2 C in a temperature environment of 25°C, and then constant-voltage charged at 4.4 V until the current value reached 0.01 C. After a 1-hour rest, the test cell was discharged to 2.5 V at a constant current of 0.2 C, forming an initial cycle. Next, the test cell was again charged at a constant current of 0.2 C until the battery voltage reached 4.4 V, and then constant-voltage charged at 4.4 V until the current value reached 0.01 C, after which the test cell was discharged at 1 C to 2.5 V. After a 10-minute rest, the test cell was further discharged at 0.02 C to 2.5 V, and the initial output was calculated using the following formula: Initial output = 1 C discharge capacity / (1 C discharge capacity + 0.02 C discharge capacity).
[0080] [Evaluation of cycle characteristics during high-rate charging] The test cell was charged to 4.4 V (vs. Li) at a constant current of 1 C in a temperature environment of 25°C, and then charged at a constant voltage of 4.4 V until the current value reached 0.01 C. After a 1-hour rest, the cell was discharged to 2.5 V at a constant current of 1 C, which constituted one cycle. The discharge capacity at 1 C after 30 cycles was measured. The capacity retention rate during high-rate charging was calculated using the following formula: Capacity retention rate = Discharge capacity at 1 C at 30th cycle / Discharge capacity at 1 C at 1st cycle
[0081] Example 2 In the preparation of a positive electrode active material, H 3 P.O. 4 Instead of ZrSO 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that ZrSO 4 In the case of the lithium-containing transition metal composite oxide, the mass of Zr in the positive electrode active material was added so as to be 0.06 mass % relative to the total mass of the lithium-containing transition metal composite oxide. Furthermore, it was confirmed by TOF-SIMS that a Zr-containing compound was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide as Compound X.
[0082] Example 3 In the preparation of a positive electrode active material, H 3 P.O. 4 Instead of CaCl 2 A test cell was prepared and evaluated in the same manner as in Example 1, except that CaCl was added. 2 In the case of the lithium-containing transition metal composite oxide, the amount of Ca added to the positive electrode active material was 0.01% by mass relative to the total mass of the lithium-containing transition metal composite oxide. Furthermore, it was confirmed by TOF-SIMS that a Ca-containing compound was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide as compound X.
[0083] Example 4 In the preparation of a positive electrode active material, H 3 P.O. 4 Instead of Er 2 (SO 4 ) 3 Test cells were prepared and evaluated in the same manner as in Example 1, except that Er was added. 2 (SO 4 )3 In the case of the lithium-containing transition metal composite oxide, the mass of Er in the positive electrode active material was added so as to be 0.2 mass % relative to the total mass of the lithium-containing transition metal composite oxide. Furthermore, it was confirmed by TOF-SIMS that an Er-containing compound was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide as compound X.
[0084] Example 5 In the preparation of a positive electrode active material, H 3 P.O. 4 Instead of NaAl(OH) 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that NaAl(OH) was added. 4 In the case of the lithium-containing transition metal composite oxide, the mass of Al in the positive electrode active material was added so as to be 0.02 mass % relative to the total mass of the lithium-containing transition metal composite oxide. Furthermore, it was confirmed by TOF-SIMS that an Al-containing compound was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide as Compound X.
[0085] Example 6 In the preparation of a positive electrode active material, H 3 P.O. 4 Instead of B(OH) 3 A test cell was prepared and evaluated in the same manner as in Example 1, except that B(OH) was added. 3 In Example 7, the mass of B in the positive electrode active material was 0.1 mass % relative to the total mass of the lithium-containing transition metal composite oxide. Furthermore, it was confirmed by TOF-SIMS that a B-containing compound was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide as Compound X. 0.90 Mn 0.10 ](OH) 2 and ZrSO as compound X. 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that ZrSO 4 was added so that the mass of Zr in the positive electrode active material was 0.06% by mass with respect to the total mass of the lithium-containing transition metal composite oxide.
[0086] Comparative Example 1 A test cell was prepared and evaluated in the same manner as in Example 1, except that lithium methanesulfonate and compound X were not added in the preparation of the positive electrode active material.
[0087] Comparative Example 2 A test cell was prepared and evaluated in the same manner as in Example 1, except that compound X was not added in the preparation of the positive electrode active material.
[0088] Comparative Example 3 In the preparation of a positive electrode active material, lithium methanesulfonate was not added, and ZrSO was used as the compound X. 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that ZrSO 4 was added so that the mass of Zr in the positive electrode active material was 0.06% by mass with respect to the total mass of the lithium-containing transition metal composite oxide.
[0089] Comparative Example 4 In the preparation of a positive electrode active material, lithium methanesulfonate was added to the obtained cake-like composition, and then ZrSO 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that powdered lithium methanesulfonate was added to the obtained cake-like composition in the preparation of the positive electrode active material (addition step). The amount of lithium methanesulfonate added was 0.3 mass% with respect to the total mass of the lithium-containing transition metal composite oxide. Then, ZrSO 4 was added to the cake-like composition to which lithium methanesulfonate had been added. 4 In addition, ZrSO 4 In the case of the lithium-containing transition metal composite oxide, the mass of Zr in the positive electrode active material was added so that the mass of Zr was 0.06 mass% relative to the total mass of the lithium-containing transition metal composite oxide. Furthermore, it was confirmed by TOF-SIMS that a Zr-containing compound was present on the surface of the secondary particles of the lithium-containing transition metal composite oxide via lithium methanesulfonate.
[0090] Comparative Example 5 A test cell was prepared and evaluated in the same manner as in Example 7, except that lithium methanesulfonate and compound X were not added in preparing the positive electrode active material.
[0091] Comparative Example 6 A test cell was prepared and evaluated in the same manner as in Example 7, except that compound X was not added in the addition step of preparing the positive electrode active material.
[0092] Comparative Example 7 In the preparation of a positive electrode active material, lithium methanesulfonate was not added, and ZrSO was used as the compound X. 4 A test cell was prepared and evaluated in the same manner as in Example 7, except that ZrSO 4 was added so that the mass of Zr in the positive electrode active material was 0.06% by mass with respect to the total mass of the lithium-containing transition metal composite oxide.
[0093] The initial outputs and capacity retention rates of the test cells of the examples and comparative examples are shown in Tables 1 and 2. Tables 1 and 2 also show the composition of the lithium-containing transition metal composite oxide, and the composition and added amounts of the added sulfonic acid compound and compound X. The initial outputs and capacity retention rates of the test cells of Examples 1 to 6 and Comparative Examples 1 to 4 shown in Table 1 are expressed relative to the initial output and capacity retention rate of the test cell of Comparative Example 1, which is set to 100. The initial outputs and capacity retention rates of the test cells of Example 7 and Comparative Examples 5 and 7 shown in the table are expressed relative to the initial output and capacity retention rate of the test cell of Comparative Example 5, which is set to 100. A larger initial output value indicates better output characteristics, and a larger capacity retention value indicates better cycle characteristics during high-rate charging.
[0094]
[0095]
[0096] As shown in Tables 1 and 2, the test cells of the examples have improved output characteristics and cycle characteristics during high-rate charging compared to the test cells of the comparative examples. In other words, by using a positive electrode active material in which a sulfonic acid compound is present on the surface of secondary particles and in which the sulfonic acid compound is present on the surface of secondary particles via compound X, a nonaqueous electrolyte secondary battery with improved output characteristics and cycle characteristics during high-rate charging can be provided. On the other hand, the test cells of comparative examples 2 and 6, in which only a sulfonic acid compound is present on the surface of secondary particles, have improved output characteristics compared to the test cells of comparative examples 1 and 5, but do not have improved cycle characteristics during high-rate charging. Furthermore, the test cells of comparative examples 3 and 7, in which only compound X is present on the surface of secondary particles, have worse output characteristics compared to the test cells of comparative examples 1 and 5. Furthermore, the test cell of comparative example 4, in which compound X is provided on the surface of a sulfonic acid compound, does not have improved output characteristics or cycle characteristics during high-rate charging compared to the test cell of comparative example 1.
[0097] The present disclosure is further described by the following embodiments. Configuration 1: A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium-containing transition metal composite oxide having a layered structure, the lithium-containing transition metal composite oxide having a general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and comprises secondary particles formed by aggregation of primary particles, wherein a sulfonic acid compound represented by formula (I) and a compound X containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al are present on the surfaces of the secondary particles, and the sulfonic acid compound is present on the surfaces of the secondary particles via the compound X. (wherein A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The positive electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein A is a Group 1 element. Configuration 3: The positive electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, wherein A is Li. Configuration 4: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein R is an alkyl group. Configuration 5: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein R is a methyl group. Configuration 6: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 5, wherein the amount of the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide is 0.05 mass % or more and 1.5 mass % or less, relative to the mass of the lithium-containing transition metal composite oxide. Aspect 7: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Aspects 1 to 6, wherein the amount of P, Ca, Sr, B, Zr, Er, and Al contained in Compound X is 0.001% by mass or more and 1% by mass or less, based on the mass of the lithium-containing transition metal composite oxide. Aspect 8: A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, comprising: a synthesis step of obtaining a lithium-containing transition metal composite oxide; a washing step of washing the lithium-containing transition metal composite oxide with water and dehydrating it to obtain a cake-like composition; an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition; and a drying step of drying the cake-like composition to obtain a powder-like composition, wherein in the washing step or the addition step, a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al is added to the cake-like composition before adding at least one of the sulfonic acid compound and the sulfonic acid solution. Configuration 9: A positive electrode for a non-aqueous electrolyte secondary battery, comprising the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 7. Configuration 10: A non-aqueous electrolyte secondary battery comprising the positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 9, a negative electrode, and a non-aqueous electrolyte.
[0098] REFERENCE SIGNS LIST 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 exterior body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 grooved portion, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium-containing transition metal composite oxide having a layered structure, the lithium-containing transition metal composite oxide being represented by the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and is formed by aggregation of primary particles, wherein a sulfonic acid compound represented by formula (I) and a compound X containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al are present on the surfaces of the secondary particles, and the sulfonic acid compound is present on the surfaces of the secondary particles via the compound X. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is a Group 1 element.
3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is Li.
4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is an alkyl group.
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is a methyl group.
6. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the amount of the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide is 0.05 mass % or more and 1.5 mass % or less, based on the mass of the lithium-containing transition metal composite oxide.
7. The positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, wherein the amount of P, Ca, Sr, B, Zr, Er and Al contained in compound X is 0.001 mass % or more and 1 mass % or less, based on the mass of the lithium-containing transition metal composite oxide.
8. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, comprising: a synthesis step of obtaining a lithium-containing transition metal composite oxide; a washing step of washing the lithium-containing transition metal composite oxide with water and dehydrating it to obtain a cake-like composition; an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition; and a drying step of drying the cake-like composition to obtain a powder-like composition, wherein in the washing step or the addition step, a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er and Al is added to the cake-like composition before adding at least one of the sulfonic acid compound and the sulfonic acid solution.
9. A positive electrode for a non-aqueous electrolyte secondary battery, comprising the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 7.
10. A non-aqueous electrolyte secondary battery comprising the positive electrode for a non-aqueous electrolyte secondary battery according to claim 9, a negative electrode, and a non-aqueous electrolyte.
Citation Information
Patent Citations
Positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery
WO2023013494A1
High-nickel composite positive electrode material as well as preparation method and application thereof
CN109616657A
Positive electrode active material, and positive electrode and non-aqueous electrolyte secondary battery using the same
JP2009193780A
Lithium secondary battery
JP2012084420A
Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery
JP2019169286A