Composition, negative electrode active material, method for manufacturing negative electrode active material, and secondary battery
The use of bonded polysiloxane and phenol resin with silicon nanoparticles in the negative electrode active material addresses the capacity limitations of graphite and silicon-based materials, enhancing the discharge capacity retention of lithium-ion batteries.
Patent Information
- Application Number
- PCT/JP2024/013972
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-04
- Publication Date
- 2024-10-31
AI Technical Summary
Lithium-ion secondary batteries face limitations in capacity improvement due to the low theoretical capacity density of graphite negative electrode active materials, and existing silicon-based active materials do not adequately maintain discharge capacity over time.
A negative electrode active material is produced using silicon nanoparticles and a composite resin where polysiloxane and phenol resin are bonded, which is then fired to enhance discharge capacity retention in secondary batteries.
The approach significantly improves the discharge capacity maintenance rate of secondary batteries compared to traditional materials, achieving better performance and longevity.
Smart Images

Figure JP2024013972_31102024_PF_FP_ABST
Abstract
Description
Composition, negative electrode active material, method for producing negative electrode active material, and secondary battery
[0001] The present invention relates to a composition, a negative electrode active material, a method for producing a negative electrode active material, and a secondary battery.
[0002] In recent years, the widespread use of mobile electronic devices such as smartphones has led to an increasing demand for small, high-capacity secondary batteries. Among these, lithium-ion secondary batteries (sometimes abbreviated as LIBs) have been rapidly deployed in electric vehicles (EVs), and their industrial applications are continuing to expand. Graphite, a carbonaceous negative electrode active material (natural or artificial), is widely used as the negative electrode active material for lithium-ion secondary batteries. However, the theoretical capacity density of graphite is low (372 mAh / g), and advances in lithium-ion secondary batteries are reaching their limits in improving battery capacity.
[0003] Silicon (Si) can form an alloy (intermetallic compound) with metallic lithium, so it can electrochemically absorb and release lithium ions. 22 Si 5 The theoretical capacity when the negative electrode active material is formed is 4200 mAh / g, and the silicon negative electrode active material can have a higher capacity than the graphite negative electrode active material.
[0004] For example, Patent Document 1 discloses a silicon active material produced by baking a composition obtained by mixing silicon nanoparticles, polysiloxane, and a phenolic resin.
[0005] Patent No. 7088438
[0006] According to the investigations of the present inventors, there is room for further improvement in the negative electrode active material described in Patent Document 1 in terms of the retention rate of the discharge capacity of the secondary battery.
[0007] Therefore, an object of one aspect of the present invention is to provide a negative electrode active material that can improve the retention rate of the discharge capacity of a secondary battery, a composition for producing the negative electrode active material, and a method for producing the negative electrode active material.
[0008] The present inventors have discovered that by firing a composition containing silicon nanoparticles and a composite resin in which polysiloxane and phenolic resin are pre-bonded, a negative electrode active material can be obtained that can improve the retention rate of the discharge capacity of a secondary battery, compared to firing a composition obtained by mixing silicon nanoparticles, polysiloxane, and phenolic resin.
[0009] The present invention includes the following aspects. [1] A composition containing silicon nanoparticles and a composite resin in which polysiloxane and phenolic resin are bonded to each other. [2] The composition according to [1], which is used for producing a secondary battery material. [3] The composition according to [1], which is used for producing a negative electrode active material. [4] A method for producing a negative electrode active material, comprising a step of firing a composition containing silicon nanoparticles and a composite resin in which polysiloxane and phenolic resin are bonded to each other. [5] A negative electrode active material containing a fired product of a composition containing silicon nanoparticles and a composite resin in which polysiloxane and phenolic resin are bonded to each other. [6] A secondary battery, comprising a negative electrode containing the negative electrode active material according to [5].
[0010] According to one aspect of the present invention, it is possible to provide a negative electrode active material capable of improving the retention rate of the discharge capacity of a secondary battery, a composition for producing the negative electrode active material, and a method for producing the negative electrode active material.
[0011] 1 shows elemental mapping by SEM-EDX of the dried precursor mixture prepared in Example 1. FIG. 2 shows elemental mapping by SEM-EDX of the dried precursor mixture prepared in Example 2. FIG. 3 shows elemental mapping by SEM-EDX of the dried precursor mixture prepared in Example 3. FIG. 4 shows elemental mapping by SEM-EDX of the dried precursor mixture prepared in Example 4. FIG. 5 shows elemental mapping by SEM-EDX of the dried precursor mixture prepared in Comparative Example 1.
[0012] One embodiment of the present invention is a composition containing silicon nanoparticles and a composite resin in which a polysiloxane and a phenolic resin are bonded to each other. This composition is suitable for use in producing a secondary battery material, and is particularly suitable for use in producing a negative electrode active material.
[0013] [Silicon Nanoparticles] Silicon nanoparticles are particles made of silicon (Si, 0 valence). Silicon nanoparticles can be obtained, for example, by pulverizing silicon particles having a particle size of about several hundred μm to nano-size particles.
[0014] The silicon particles can be pulverized using a pulverizer such as a ball mill, a bead mill, or a jet mill. The pulverization may be wet pulverization. The organic solvent used for wet pulverization is not particularly limited as long as it is an organic solvent that can suitably pulverize the silicon particles. For example, the organic solvent may be an alcohol, a ketone, or an aromatic hydrocarbon such as toluene, xylene, naphthalene, or methylnaphthalene.
[0015] The average particle diameter (D50) of the silicon nanoparticles is preferably 10 nm or more, more preferably 20 nm or more, even more preferably 30 nm or more, and preferably 300 nm or less, more preferably 250 nm or less, and even more preferably 200 nm or less. When the average particle diameter is 10 nm or more, aggregation of the silicon nanoparticles is suppressed, making it easier to uniformly disperse the silicon nanoparticles in the negative electrode active material, and it is possible to suppress the increase of by-products on the surface when the silicon nanoparticles are baked. When the average particle diameter is 300 nm or less, it is possible to suppress the deterioration of the charge / discharge performance of the negative electrode active material due to the pulverization phenomenon during charge / discharge.
[0016] The average particle diameter (D50) is the particle diameter at which the cumulative volume distribution curve of the silicon nanoparticles reaches 50% of the cumulative volume when the cumulative volume distribution curve is plotted from the smallest diameter side in the particle diameter distribution of the silicon nanoparticles. The average particle diameter (D50) is measured using a laser diffraction particle size distribution analyzer.
[0017] [Composite resin and its manufacturing method] A composite resin is a resin in which a polysiloxane and a phenolic resin are bonded (chemically bonded) to each other. A composite resin is different from a mixture in which a polysiloxane and a phenolic resin are simply mixed. The types of polysiloxane and phenolic resin are not particularly limited. Below, an example of a method for combining a polysiloxane and a phenolic resin (a manufacturing method for a composite resin) will be described, and then an example of the structure of the composite resin obtained thereby will be described.
[0018] In one embodiment, a method for producing a composite resin uses a silane compound having an epoxy group and a hydrolyzable silyl group (hereinafter also referred to as an "epoxysilane compound") as a raw material for polysiloxane, as described in detail below. Examples of such a production method include a production method (hereinafter also referred to as "production method A") in which a silane compound containing an epoxysilane compound is polycondensed in the presence of a phenolic resin to produce a polysiloxane and obtain a composite resin, a production method (hereinafter also referred to as "production method B") in which a phenolic resin is produced by polycondensing a phenolic compound and an aldehyde in the presence of a polysiloxane that is a polycondensate of a silane compound containing an epoxysilane compound, and obtain a composite resin in which the polysiloxane and the phenolic resin are bonded to each other, and a production method (hereinafter also referred to as "production method C") in which a phenolic compound, an aldehyde, and a silane compound containing an epoxysilane compound are polycondensed all at once to obtain a composite resin in which the polysiloxane and the phenolic resin are bonded to each other.
[0019] In any of Production Methods A to C for obtaining the composite resin, it is preferable to use a silane compound in which an aromatic hydrocarbon group is bonded to a silicon atom as the silane compound for producing polysiloxane, from the viewpoint of making it easier to further improve the retention rate.
[0020] (Production Method A) A method for producing a composite resin according to one embodiment of the present invention (production method A) includes a step (step (A-1)) of reacting a phenolic resin with a silane compound represented by the following formula (11) to obtain an intermediate. In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, and m1 and m2 represent either (m1, m2)=(0, 3) or (1, 2).
[0021] The phenolic resin used in step (A-1) is not particularly limited. The phenolic resin can be obtained by reacting a phenol with an aldehyde by a known method. Alternatively, a commercially available phenolic resin may be used as the phenolic resin. In this specification, the term "phenol" refers to a phenolic compound as a monomer constituting a phenolic resin, and does not include phenolic resins.
[0022] Examples of phenolic resins include novolac-type phenolic resins (e.g., obtained by reacting phenols with aldehydes in the presence of an acid catalyst) and resol-type phenolic resins (e.g., obtained by reacting phenols with aldehydes in the presence of an alkali catalyst).
[0023] Examples of phenols include monohydric phenols such as phenol, cresols such as o-cresol, m-cresol, and p-cresol; xylenols such as 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol; ethylphenols such as o-ethylphenol, m-ethylphenol, and p-ethylphenol; butylphenols such as isopropylphenol, butylphenol, and p-tert-butylphenol; alkylphenols such as p-tert-amylphenol, p-octylphenol, p-nonylphenol, and p-cumylphenol; halogenated phenols such as fluorophenol, chlorophenol, bromophenol, and iodophenol; substituted monohydric phenols such as p-phenylphenol, aminophenol, nitrophenol, dinitrophenol, and trinitrophenol; and naphthols such as 1-naphthol and 2-naphthol. Further, examples of phenols include divalent or higher phenols such as resorcinol, alkylresorcinol, pyrogallol, catechol, alkylcatechol, hydroquinone, alkylhydroquinone, phloroglucinol, and dihydroxynaphthalene. Further, examples of phenols include bisphenols such as bisphenol F and bisphenol A, and phenol derivatives derived from natural products such as cashew oil. These phenols may be used alone or in combination of two or more.
[0024] Examples of effective aldehydes include formaldehydes such as formaldehyde, paraformaldehyde, and trioxane; acetaldehyde, furfural, and urotropine (hexamethylenetetramine). These aldehydes may be used alone or in combination of two or more.
[0025] The amount of aldehydes may be 10 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more, and may be 50 parts by mass or less, 45 parts by mass or less, or 40 parts by mass or less, relative to 100 parts by mass of phenols. The molar ratio of the amount of aldehydes to the amount of phenols (aldehydes / phenols) may be 0.3 or more, preferably 0.5 or more, and may be 3.0 or less, preferably 2.0 or less.
[0026] The phenolic resin may be modified with a modifying agent such as a compound containing a triazine ring, such as melamine, acetoguanamine, benzoguanamine, cyanuric acid, methyl cyanurate, ethyl cyanurate, acetyl cyanurate, or cyanuric chloride; a urea-based compound, such as urea, ethylene urea, or thiourea; dicyandiamide; or guanidine.
[0027] The polysiloxane, phenols, and aldehydes can be reacted by adding a catalyst such as an organic acid catalyst, an inorganic acid catalyst, or an alkaline catalyst as a reaction catalyst. Examples of organic acid catalysts include formic acid, acetic acid, propionic acid, paratoluenesulfonic acid, methanesulfonic acid, lactic acid, mandelic acid, tartaric acid, citric acid, 2-hydroxybutyric acid, quinic acid, malic acid, paratoluenesulfonic acid, and phenolsulfonic acid. Examples of inorganic acid catalysts include boric acid, phosphoric acid, hydrochloric acid, and sulfuric acid. Examples of alkaline catalysts include ammonia, organic amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, choline, sodium hydroxide, potassium hydroxide, and calcium hydroxide.
[0028] R in formula (11) 11 In one embodiment, may be a monovalent group having a glycidyl group, is preferably a monovalent group having a glycidoxy group, and is more preferably a group represented by the following formula (11a): In the formula, R a represents an alkylene group, and * represents a bond bonded to the Si atom in formula (11).
[0029] R aThe alkylene group represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkylene group may be 1 or more, 2 or more, or 3 or more, and may be 10 or less, 9 or less, or 8 or less.
[0030] R in formula (11) 11 In one embodiment, may be a monovalent group having an alicyclic epoxy group, and is preferably a group represented by the following formula (11b): In the formula, R b represents a single bond or an alkylene group, and * represents a bond bonded to the Si atom in formula (11).
[0031] R b The alkylene group represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkylene group may be 1 or more, 2 or more, or 3 or more, and may be 10 or less, 9 or less, or 8 or less.
[0032] R 12 and R 13 The alkyl groups represented by the formula (I) may each independently be linear or branched. The number of carbon atoms in the alkyl groups may each independently be 1 or more, 5 or less, 4 or less, 3 or less, or 2 or less, or may be 1 or 2. 13 may be the same as each other or may be different from each other.
[0033] Specific examples of the silane compound represented by formula (11) include glycidoxypropyltrimethoxysilane, epoxycyclohexyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 8-glycidoxyoctyltrimethoxysilane.
[0034] The amount of the silane compound represented by formula (11) may be 1 part by mass or more or 3 parts by mass or more, and may be 1,500 parts by mass or less or 1,000 parts by mass or less, relative to 100 parts by mass of the phenolic resin.
[0035] The amount of the silane compound represented by formula (11) may be 7 mol% or more and 62 mol% or less, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12) described below. The amount of the silane compound represented by formula (11) is preferably 10 to 60 mol% based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12) described below. The lower limit of the amount of the silane compound represented by formula (11) may be 12 mol%, 14 mol%, or 16 mol%. The upper limit of the amount of the silane compound represented by formula (11) may be 58 mol%, 56 mol%, or 54 mol%.
[0036] In step (A-1), a catalyst may be used when reacting the phenolic resin with the silane compound represented by formula (11). Specific examples of the catalyst include imidazoles, organic phosphines, and tertiary amines. Examples of imidazoles include 2-methylimidazole, 2-phenylimidazole, 2-phenyl-2-methylimidazole, and 2-heptadecylimidazole. Examples of organic phosphines include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine. Examples of tertiary amines include triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethyl, and tris(dimethylaminomethyl)phenol.
[0037] In step (A-1), in addition to the phenolic resin and the silane compound represented by formula (11), a silane compound other than the silane compound represented by formula (11) may be further reacted. As such a silane compound, a silane compound represented by formula (12) described in step (A-2) below can be used.
[0038] When a silane compound other than the silane compound represented by formula (11) is used, the amount of the silane compound may be 1 part by mass or more or 3 parts by mass or more, and may be 1,500 parts by mass or less or 1,000 parts by mass or less, relative to 100 parts by mass of the phenolic resin.
[0039] The reaction temperature and reaction time in step (A-1) can be appropriately set. The reaction temperature may be, for example, 70° C. or higher and 160° C. or lower. The reaction time may be, for example, 1 hour or higher and 5 hours or lower.
[0040] By the above step (A-1), an intermediate is obtained, which is a reaction product of the phenolic resin and the silane compound represented by formula (11) (and further, a silane compound other than the silane compound represented by formula (11) that is used as needed). More specifically, a hydroxyl group in the phenolic resin and an epoxy group or an alkoxysilyl group in the silane compound represented by formula (11) (Si—OR 13 The hydroxyl group in the phenolic resin may be a phenolic hydroxyl group (a hydroxyl group bonded to an aromatic ring in the phenolic resin), or, when the phenolic resin has a methylol group, may be a hydroxyl group constituting the methylol group.
[0041] Following the step (A-1), the production method A includes a step (A-2) of polycondensing the intermediate obtained in the step (A-1) with a silane compound represented by the following formula (12): In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, and n1 and n2 represent either (n1, n2)=(1, 3) or (2, 2).
[0042] R 21 The alkyl group represented by the formula (I) may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group may be 1 or more, 6 or less, 5 or less, 4 or less, 3 or less, or 2 or less, or may be 1.
[0043] R 21The aromatic hydrocarbon group represented by the formula (I) is a monovalent hydrocarbon group having an aromatic ring. Examples of the aromatic hydrocarbon group include an aryl group and an aralkyl group. Examples of the aryl group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group. Examples of the aralkyl group include a benzyl group and a phenethyl group. When n1 is 2, two R groups present in one molecule are 21 may be the same as or different from each other. From the viewpoint of further improving the maintenance rate, when (n1, n2)=(1, 3), R 21 is preferably an aromatic hydrocarbon group, and when (n1, n2)=(2, 2), R 21 At least one of these is preferably an aromatic hydrocarbon group.
[0044] R 21 The alkyl portion of the (meth)acryloyloxyalkyl group represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkyl portion may be 1 or more, and may be 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, or 3 or less.
[0045] R 22 The alkyl group represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkyl group may be 1 or more, 4 or less, 3 or less, or 2 or less, or may be 1. 22 may be the same as each other or may be different from each other.
[0046] In step (A-2), one or more, preferably two or more, silane compounds represented by formula (12) are used. When two or more silane compounds represented by formula (12) are used, R 21 is an alkyl group, or a silane compound 21 It is preferable to use a combination of two or more silane compounds in which R is an aryl group.
[0047] Specific examples of the silane compound represented by formula (12) include silane compounds having an aromatic hydrocarbon group (R 21 wherein R is an aromatic hydrocarbon group), silane compounds such as methyltrimethoxysilane, methyltriethoxysilane, methyltri-n-butoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldi-n-butoxysilane, diethyldimethoxysilane, and methylcyclohexyldimethoxysilane. 21 silane compounds in which all of R 21 a silane compound having a (meth)acryloyloxyalkyl group (R 21 and silane compounds in which the alkyl group is a (meth)acryloyloxyalkyl group.
[0048] The amount of the silane compound represented by formula (12) may be 1 part by mass or more or 3 parts by mass or more, and may be 1,500 parts by mass or less or 1,000 parts by mass or less, relative to 100 parts by mass of the phenolic resin.
[0049] The amount of the silane compound represented by formula (12) may be 38 mol% or more and 93 mol% or less, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12). The amount of the silane compound represented by formula (12) is preferably 40 to 90 mol%, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12). The lower limit of the amount of the silane compound represented by formula (12) may be 52 mol%, 54 mol%, or 56 mol%. The upper limit of the amount of the silane compound represented by formula (12) may be 88 mol%, 86 mol%, or 84 mol%.
[0050] In step (A-2), a catalyst such as an organic acid catalyst, an inorganic acid catalyst, or an alkaline catalyst may be used to promote the reaction (hydrolysis condensation reaction) between the intermediate and the silane compound represented by formula (12). Examples of organic acid catalysts include formic acid, acetic acid, propionic acid, paratoluenesulfonic acid, methanesulfonic acid, lactic acid, mandelic acid, tartaric acid, citric acid, 2-hydroxybutyric acid, quinic acid, and malic acid. Examples of inorganic acid catalysts include boric acid and phosphoric acid. Examples of alkaline catalysts include ammonia, organic amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, choline, sodium hydroxide, potassium hydroxide, and calcium hydroxide.
[0051] In step (A-2), the intermediate and the silane compound represented by formula (12) may be reacted in one step or in multiple steps (for example, two steps). For example, in the case of a two-step reaction, first, the intermediate and the silane compound represented by formula (12) R 21 is an aryl group, and then reacting with a silane compound represented by the formula (12) 21 can be further reacted with a silane compound in which is an alkyl group.
[0052] The reaction temperature and reaction time in step (A-2) can be appropriately set. The reaction temperature may be, for example, 70° C. or higher and 120° C. or lower. The reaction time may be, for example, 1 hour or higher and 5 hours or lower.
[0053] Production method A may further include, after step (A-2), a step (A-3) of distilling the reaction product obtained in step (A-2) under reduced pressure. By step (A-3), for example, methanol and water produced in step (A-2) can be removed.
[0054] A composite resin in which polysiloxane and phenolic resin are bonded to each other can be obtained by the above-described manufacturing method A. The composite resin will be described in detail later.
[0055] (Production Method B) A method for producing a composite resin according to another embodiment of the present invention (Production Method B) includes a step (step (B-1)) of polycondensing a phenol and an aldehyde in the presence of a polysiloxane having a structural unit represented by the following formula (21) and a structural unit represented by the following formula (22). In the formula, R 11 represents a monovalent group having an epoxy group, R 12 and R 13 each independently represents an alkyl group, p1 and p2 represent either (p1, p2)=(0, 1) or (1, 0), and * represents a bond. In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group; R 22 represents an alkyl group, q1 and q2 represent either (q1, q2)=(1, 1) or (2, 0), and * represents a bond. 21 is preferably an aromatic hydrocarbon group, and when (q1, q2)=(2, 0), R 21 At least one of these is preferably an aromatic hydrocarbon group.
[0056] R in formula (21) 11 , R 12 and R 13 The details of R in formula (11) explained in the above-mentioned production method A are 11 , R 12 and R 13 are the same as the above. R in formula (22) 21 and R 22 The details of R in formula (21) explained in the above-mentioned production method A are 21 and R 22 are the same as
[0057] A polysiloxane having a structural unit represented by formula (21) and a structural unit represented by formula (22) can be obtained by polycondensing a silane compound represented by formula (11) and a silane compound represented by formula (12), which are described in the above-mentioned production method A, by a known method.
[0058] The polysiloxane has one or more, preferably two or more, structural units represented by formula (22). When the polysiloxane has two or more structural units represented by formula (22), the polysiloxane preferably has one or more structural units represented by formula (22) in which R 21 is an alkyl group or a structural unit in formula (22) 21 is an aryl group.
[0059] The amount of the structural unit represented by formula (21) may be 7 mol% or more and 62 mol% or less, based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22). The amount of the structural unit represented by formula (21) is preferably 10 to 60 mol% based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22). The lower limit of the amount of the structural unit represented by formula (21) may be 12 mol%, 14 mol%, or 16 mol%. The upper limit of the amount of the structural unit represented by formula (21) may be 58 mol%, 56 mol%, or 54 mol%.
[0060] The amount of the structural unit represented by formula (22) may be 38 mol% or more and 93 mol% or less, based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22). The amount of the structural unit represented by formula (22) is preferably 60 to 90 mol%, based on the total amount of the structural unit represented by formula (21) and the structural unit represented by formula (22). The lower limit of the amount of the structural unit represented by formula (22) may be 52 mol%, 54 mol%, or 56 mol%. The upper limit of the amount of the structural unit represented by formula (22) may be 88 mol%, 86 mol%, or 84 mol%.
[0061] In step (B-1), the polysiloxane is reacted with a phenol and an aldehyde to polycondense the phenol and the aldehyde. As the phenol and the aldehyde, one or more of the phenols and the aldehydes described in the above-mentioned production method A can be used.
[0062] The amount of polysiloxane may be 3 parts by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 4,500 parts by mass or less, 4,000 parts by mass or less, or 3,500 parts by mass or less, per 100 parts by mass of the phenols.
[0063] The amount of aldehydes may be 10 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more, and may be 50 parts by mass or less, 45 parts by mass or less, or 40 parts by mass or less, relative to 100 parts by mass of phenols. When the phenolic resin is a resol-type phenolic resin, the molar ratio of the amount of aldehydes to the amount of phenols (aldehydes / phenols) may be 0.3 or more, preferably 0.5 or more, and may be 3.0 or less, preferably 2.0 or less.
[0064] In the step (B-1), the following may be used as the modifying agent: a compound containing a triazine ring, such as melamine, acetoguanamine, benzoguanamine, cyanuric acid, methyl cyanurate, ethyl cyanurate, acetyl cyanurate, or cyanuric chloride; a urea-based compound, such as urea, ethylene urea, or thiourea; dicyandiamide; or guanidine.
[0065] In step (B-1), the polysiloxane, phenols, and aldehydes can be reacted by adding a catalyst such as an organic acid catalyst, an inorganic acid catalyst, or an alkaline catalyst as a reaction catalyst. Examples of organic acid catalysts include formic acid, acetic acid, propionic acid, paratoluenesulfonic acid, methanesulfonic acid, lactic acid, mandelic acid, tartaric acid, citric acid, 2-hydroxybutyric acid, quinic acid, malic acid, paratoluenesulfonic acid, and phenolsulfonic acid. Examples of inorganic acid catalysts include boric acid, phosphoric acid, hydrochloric acid, and sulfuric acid. Examples of alkaline catalysts include ammonia, organic amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, choline, sodium hydroxide, potassium hydroxide, and calcium hydroxide.
[0066] The reaction temperature and reaction time in step (B-1) can be appropriately set. The reaction temperature may be, for example, 60° C. or higher and 180° C. or lower. The reaction time may be, for example, 1 hour or higher and 24 hours or lower.
[0067] Production method B may further include, after step (B-1), a step (B-2) of dehydrating the reaction product obtained in step (B-1) under reduced pressure. By step (B-2), for example, water generated in step (B-1) can be removed.
[0068] A composite resin in which polysiloxane and phenolic resin are bonded to each other can be obtained by the above-described manufacturing method B. The composite resin will be described in detail later.
[0069] (Production Method C) A method for producing a composite resin according to another embodiment of the present invention (production method C) includes a step (step (C-1)) of simultaneously polycondensing a phenol, an aldehyde, a silane compound represented by the above formula (11), and a silane compound represented by the above formula (12).
[0070] Details of the phenols, the silane compound represented by formula (11), and the silane compound represented by formula (12) used in step (C-1) are the same as the details of the phenols, the silane compound represented by formula (11), and the silane compound represented by formula (12) described in production method A.
[0071] Details of the aldehydes are the same as those of the aldehydes described in Production Method A. In this step (C-1), the phenols and the aldehydes are polycondensed to form a phenolic resin, the silane compound represented by Formula (11) and the silane compound represented by Formula (12) are polycondensed to form a polysiloxane, and further, the phenolic resin and the polysiloxane are bonded to each other to form a composite resin.
[0072] The amount of the silane compound represented by formula (11) may be 3 parts by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 3,500 parts by mass or less, 3,300 parts by mass or less, or 3,100 parts by mass or less, relative to 100 parts by mass of the phenols.
[0073] The amount of the silane compound represented by formula (12) may be 3 parts by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 4,500 parts by mass or less, 4,000 parts by mass or less, or 3,500 parts by mass or less, relative to 100 parts by mass of the phenols.
[0074] The molar ratio of the amount of aldehydes to the amount of phenols (aldehydes / phenols) may be 0.3 or more, preferably 0.5 or more, and may be 3.0 or less, preferably 2.0 or less.
[0075] The amount of the silane compound represented by formula (11) may be 7 mol% or more and 62 mol% or less, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12) described below. The amount of the silane compound represented by formula (11) is preferably 10 to 60 mol% based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12) described below. The lower limit of the amount of the silane compound represented by formula (11) may be 12 mol%, 14 mol%, or 16 mol%. The upper limit of the amount of the silane compound represented by formula (11) may be 58 mol%, 56 mol%, or 54 mol%.
[0076] The amount of the silane compound represented by formula (12) may be 38 mol% or more and 93 mol% or less, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12). The amount of the silane compound represented by formula (12) is preferably 40 to 90 mol%, based on the total amount of the silane compound represented by formula (11) and the silane compound represented by formula (12). The lower limit of the amount of the silane compound represented by formula (12) may be 52 mol%, 54 mol%, or 56 mol%. The upper limit of the amount of the silane compound represented by formula (12) may be 88 mol%, 86 mol%, or 84 mol%.
[0077] In the step (C-1), a catalyst (organic acid catalyst, inorganic acid catalyst, alkali catalyst, etc.) described in the production method A may be used to promote the reaction (hydrolysis condensation reaction).
[0078] The reaction temperature and reaction time in step (C-1) can be appropriately set. The reaction temperature may be, for example, 60° C. or higher and 180° C. or lower. The reaction time may be, for example, 1 hour or higher and 24 hours or lower.
[0079] Production method C may further include, after step (C-1), a step (C-2) of distilling the reaction product obtained in step (C-1) under reduced pressure. By step (C-2), for example, methanol and water produced in step (C-1) can be removed.
[0080] A composite resin in which polysiloxane and phenolic resin are bonded to each other can be obtained by the above-described production method C. The composite resin will be described in detail later.
[0081] (Composite Resin) In the composite resin obtained by each of the above-described production methods, the polysiloxane and the phenolic resin are bonded to each other. In this composite resin, the polysiloxane has a structural unit represented by the following formula (1A) or (1B) and a structural unit represented by the following formula (2). In the formula, R 11 represents a monovalent group having an epoxy group, R 12 represents an alkyl group, and R 14 represents a linking group, R 15 represents a hydrogen atom or a hydrocarbon group, R 14 and R 15 may be bonded to each other to form a ring, p1 and p2 represent either (p1, p2)=(0, 1) or (1, 0), and * represents a bond. In the formula, R 21 represents an alkyl group, an aromatic hydrocarbon group, a vinyl group, or a (meth)acryloyloxyalkyl group, q1 and q2 represent either (q1, q2)=(1, 1) or (2, 0), and * represents a bond.
[0082] R in formula (1A) 11 and R 12 The details of R in formula (11) explained in the above-mentioned production method A are 11 and R 12 R in formula (1B) is the same as 12The details of R in formula (11) explained in the above-mentioned production method A are 12 R in formula (2) is the same as 21 The details of R in formula (12) explained in the above-mentioned production method A are 21 is the same as
[0083] The phenolic resin is bonded to the polysiloxane via a hydroxyl group contained in the phenolic resin. The hydroxyl group in the phenolic resin may be a phenolic hydroxyl group (a hydroxyl group bonded to an aromatic ring in the phenolic resin), or, if the phenolic resin has a methylol group, may be a hydroxyl group constituting the methylol group.
[0084] In one embodiment, the phenolic resin may be bonded to the structural unit represented by formula (1A) or (1B) via a hydroxyl group, and -(O-*) in the structural unit represented by formula (1A) p2 and -(O-*) in the structural unit represented by formula (1B) may be bonded to a bond of a group represented by formula (1B). p2 and in the structural unit represented by formula (1B), 14 -CH(OH)-CH(R 15 In another embodiment, the phenol resin may be bonded to the structural unit represented by formula (2) via a hydroxyl group, and the —(O-*) in the structural unit represented by formula (2) may be bonded to the bond of the group represented by formula (2). q2 It may be bonded to a bond of a group represented by the following formula:
[0085] The structural unit represented by formula (1B) is a structural unit produced by the reaction of an epoxy group in the silane compound represented by formula (11) or the structural unit represented by formula (21) with a hydroxyl group in the phenol resin. 14 and R 15 is R in formula (11) and formula (21). 11 is a group having a structure corresponding to the structure of
[0086] For example, R in formula (11) and formula (21) 11is a group represented by the above formula (11a), the structural unit represented by formula (1B) becomes a structural unit represented by the following formula (1C) (R 15 is a hydrogen atom). In the formula, R 12 , p1 and p2 are R in formula (1B) 12 , p1 and p2, and R a is R in formula (11a) a and * represents a bond.
[0087] For example, R in formula (11) and formula (21) 11 is a group represented by the above formula (11b), the structural unit represented by formula (1B) becomes a structural unit represented by the following formula (1D) (R 14 and R 15 are bonded to each other to form a ring). In the formula, R 12 , p1 and p2 are R in formula (1B) 12 , p1 and p2, and R b is R in formula (11b). b and * represents a bond.
[0088] In another embodiment, when the phenolic resin has an amino group, the phenolic resin may be bonded to the structural unit represented by formula (1B) via the amino group, and -R 14 -CH(OH)-CH(R 15 )-- may be bonded to a bond of the group represented by *.
[0089] In another embodiment, the polysiloxane has a vinyl group or a (meth)acryloyloxyalkyl group (R 21 is a vinyl group or a (meth)acryloyloxyalkyl group), the phenolic resin may be bonded to the polysiloxane via the vinyl group or the (meth)acryloyloxyalkyl group.
[0090] The polysiloxane has one or more, preferably two or more, structural units represented by formula (2). When the polysiloxane has two or more structural units represented by formula (2), the polysiloxane preferably has one or more structural units represented by formula (2) in which R 21 is an alkyl group or a structural unit in formula (22) 21 is an aryl group.
[0091] The amount of the structural units represented by formula (1A) or (1B) may be 7 mol% or more and 62 mol% or less, based on the total amount of the structural units represented by formula (1A) or (1B) and the structural units represented by formula (2). The amount of the structural units represented by formula (1A) or (1B) is preferably 10 to 60 mol% based on the total amount of the structural units represented by formula (1A) or (1B) and the structural units represented by formula (2). The lower limit of the amount of the structural units represented by formula (1A) or (1B) may be 12 mol%, 14 mol%, or 16 mol%. The upper limit of the amount of the structural units represented by formula (1A) or (1B) may be 58 mol%, 56 mol%, or 54 mol%.
[0092] The amount of the structural unit represented by formula (2) may be 38 mol% or more and 93 mol% or less, based on the total amount of the structural unit represented by formula (1A) or (1B) and the structural unit represented by formula (2). The amount of the structural unit represented by formula (2) is preferably 40 to 90 mol%, based on the total amount of the structural unit represented by formula (1A) or (1B) and the structural unit represented by formula (2). The lower limit of the amount of the structural unit represented by formula (2) may be 52 mol%, 54 mol%, or 56 mol%. The upper limit of the amount of the structural unit represented by formula (2) may be 88 mol%, 86 mol%, or 84 mol%.
[0093] In the composite resin, the mass ratio (polysiloxane segment / phenolic resin segment) of the content of the structure derived from polysiloxane (polysiloxane segment) to the content of the structure derived from phenolic resin (phenolic resin segment) may be 5 / 95 or more, 10 / 90 or more, or 15 / 85 or more, and may be 95 / 5 or less, 90 / 10 or less, 80 / 20 or less, or 70 / 30 or less.
[0094] The content of the composite resin in the composition is preferably 50 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 150 parts by mass or more, per 100 parts by mass of silicon nanoparticles, from the viewpoint of further improving the discharge capacity retention rate of the secondary battery, and is preferably 500 parts by mass or less, more preferably 400 parts by mass or less, and even more preferably 350 parts by mass or less, from the viewpoint of further improving the initial efficiency of the secondary battery. When the composition further contains a dispersant, the content of the composite resin in the composition may be the above content per 100 parts by mass of the total amount of the silicon nanoparticles and the dispersant.
[0095] The composition may contain only silicon nanoparticles and a composite resin, or may further contain other components in addition to the silicon nanoparticles and the composite resin.
[0096] Other components include, for example, a dispersion medium and a dispersant. The dispersion medium may be, for example, an organic solvent such as methyl ethyl ketone. The dispersant may be a known dispersant that can improve the dispersibility of silicon nanoparticles in the dispersion medium. Examples of dispersants include non-aqueous dispersants. Examples of non-aqueous dispersants include polymer types (polyethers, polyalkylene polyamines, polycarboxylic acid partial alkyl esters, etc.), low molecular weight types (polyhydric alcohol esters, alkyl polyamines, etc.), and inorganic polyphosphates.
[0097] The content of the dispersion medium may be, for example, 200 parts by mass or more and 600 parts by mass or less relative to 100 parts by mass of silicon nanoparticles. From the viewpoint of suitably dispersing the silicon nanoparticles in the dispersion medium, the content of the dispersant is preferably 7 parts by mass or more, more preferably 12 parts by mass or more, and preferably 75 parts by mass or less, more preferably 50 parts by mass or less relative to 100 parts by mass of silicon nanoparticles.
[0098] [Negative Electrode Active Material and Manufacturing Method Thereof] Next, a method for manufacturing a negative electrode active material using the above-mentioned composition will be described. One embodiment of the present invention includes a step of baking a composition containing silicon nanoparticles and a composite resin in which polysiloxane and a phenolic resin are bonded to each other (baking step).
[0099] The composition used in the baking step may be, for example, a negative electrode active material precursor in which silicon nanoparticles and a composite resin are uniformly mixed. The negative electrode active material precursor is produced, for example, by mixing a dispersion of silicon nanoparticles with a composite resin, removing the solvent, and drying the mixture to homogenize (homogenization step). That is, the method for producing a negative electrode active material according to one embodiment may further include a homogenization step before the baking step. The dispersion of silicon nanoparticles may contain the above-mentioned dispersion medium and dispersant in addition to silicon nanoparticles.
[0100] The mixing ratio of the silicon nanoparticle dispersion and the composite resin in the homogenization step may be, for example, 100 to 400 parts by mass, 150 to 380 parts by mass, or 170 to 360 parts by mass of the composite resin per 100 parts by mass of silicon nanoparticles (solid content).
[0101] The solvent removal in the homogenization step can be carried out, for example, at 80 to 150° C. under a flow of an inert gas (e.g., nitrogen gas). The drying in the homogenization step can be, for example, drying under reduced pressure at 25 to 200° C. The drying time can be, for example, 1 minute to 24 hours.
[0102] The negative electrode active material precursor obtained in the homogenization step may contain C, N, O, and Si as constituent elements. The ratio of C in the negative electrode active material precursor may be 35 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more, and may be 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less, relative to 100 parts by mass of the total of C, N, O, and Si. The ratio of N in the negative electrode active material precursor may be 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more, and may be 7 parts by mass or less, 6 parts by mass or less, or 5 parts by mass or less, relative to 100 parts by mass of the total of C, N, O, and Si. The ratio of O in the negative electrode active material precursor may be 5 parts by mass or more, 7 parts by mass or more, or 9 parts by mass or more, and may be 30 parts by mass or less, 25 parts by mass or less, or 20 parts by mass or less, relative to 100 parts by mass of the total of C, N, O, and Si. The ratio of Si in the negative electrode active material precursor may be 10 parts by mass or more, 13 parts by mass or more, or 15 parts by mass or more, and may be 50 parts by mass or less, 45 parts by mass or less, or 40 parts by mass or less, relative to 100 parts by mass of the total of C, N, O, and Si.
[0103] In the calcination step, the composition (negative electrode active material precursor) is calcined in an inert atmosphere (e.g., a nitrogen atmosphere) at a maximum temperature within a range of 1000°C to 1180°C for 1 to 48 hours. The calcination method is not particularly limited, and may be a continuous method, a batch method, or the like, using a device having a heating function in an inert atmosphere. The device may be selected appropriately depending on the purpose from among a fluidized bed reactor, a rotary furnace, a vertical moving bed reactor, a tunnel furnace, a batch furnace, a rotary kiln, and the like.
[0104] The method for producing a negative electrode active material according to one embodiment may further include a step of pulverizing the fired product obtained in the firing step (pulverization step). The pulverization may be performed in one step until the fired product has a desired particle size, or may be performed in multiple steps. The pulverization method may be appropriately selected depending on the size of the fired product, and may be pulverization using a jaw crusher, roll crusher, glow mill, ball mill, bead mill, jet mill, or the like.
[0105] The negative electrode active material can be obtained by the manufacturing method described above. That is, one embodiment of the present invention is a negative electrode active material containing a fired product of a composition containing silicon nanoparticles and a composite resin in which a polysiloxane and a phenolic resin are bonded to each other.
[0106] [Negative electrode and secondary battery] The above-described negative electrode active material is suitably used for a negative electrode (negative electrode of a secondary battery). That is, one embodiment of the present invention is a negative electrode containing the above-described negative electrode active material. Another embodiment of the present invention is a secondary battery including a negative electrode containing the above-described negative electrode active material.
[0107] The negative electrode includes, for example, a current collector and a negative electrode material layer provided on the current collector. The current collector may be, for example, a metal foil such as copper, nickel, titanium, or stainless steel. The negative electrode material layer includes, for example, the above-described negative electrode active material and an organic binder.
[0108] The organic binder is not particularly limited, but examples thereof include styrene-butadiene rubber copolymer (SBR); ethylenically unsaturated carboxylic acid esters (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, (meth)acrylonitrile, and hydroxyethyl (meth)acrylonitrile); and polymer compounds such as polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamideimide, and carboxymethyl cellulose (CMC).
[0109] The content of the negative electrode active material in the negative electrode layer may be 70% by mass or more, 80% by mass or more, or 85% by mass or more, and may be 99% by mass or less, 98% by mass or less, or 97% by mass or less. The content of the organic binder in the negative electrode layer may be 1% by mass or more, 2% by mass or more, or 3% by mass or more, and may be 30% by mass or less, 20% by mass or less, or 15% by mass or less.
[0110] The negative electrode layer may further contain a conductive additive. Examples of the conductive additive include carbon black, graphite, acetylene black, and conductive oxides and nitrides. The content of the conductive additive may be 1 part by mass or more and 15 parts by mass or less per 100 parts by mass of the negative electrode active material.
[0111] The secondary battery including the negative electrode may be a non-aqueous electrolyte secondary battery or a solid electrolyte secondary battery, and is preferably a non-aqueous electrolyte secondary battery. The non-aqueous electrolyte secondary battery includes, for example, the negative electrode, a positive electrode, a separator, and an electrolytic solution.
[0112] The negative electrode includes, for example, a current collector and a positive electrode material layer provided on the current collector. The current collector may be, for example, a metal foil such as copper, nickel, titanium, or stainless steel.
[0113] The positive electrode material contained in the positive electrode layer may be, for example, a metal compound, a metal oxide, a metal sulfide, or a conductive polymer material capable of doping or intercalating lithium ions. Specific examples include lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMnO 2 ), and their composite oxides (LiCo x Ni y Mn z O 2 , x + y + z = 1), lithium manganese spinel (LiMn 2 O 4 ), lithium vanadium compounds, V 2 O 5 , V 6 O 13 , V.O. 2 , MnO 2 , TiO 2 , MoV 2 O 8 , TiS 2 , V 2 S 5 , V.S. 2 , MoS 2 , MoS 3 , Cr 3 O 8 , Cr 2 O 5 , olivine-type LiMPO 4 (M: Co, Ni, Mn, Fe), conductive polymers such as polyacetylene, polyaniline, polypyrrole, polythiophene, and polyacene, porous carbon, and the like can be used alone or in combination.
[0114] The separator may be, for example, a nonwoven fabric, cloth, or microporous film mainly composed of a polyolefin such as polyethylene or polypropylene, or a combination thereof. Note that if the positive electrode and negative electrode of the nonaqueous electrolyte secondary battery to be fabricated are not in direct contact with each other, there is no need to use a separator.
[0115] The electrolyte may be, for example, LiClO 4 , LiPF 6 , LiAsF 6 , LiBF 4 , LiSO 3 CF 3 A so-called organic electrolyte solution can be used in which a lithium salt such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, ethyl acetate, or the like is dissolved in a non-aqueous solvent of a single component or a mixture of two or more components.
[0116] The structure of a non-aqueous electrolyte secondary battery is not particularly limited, but typically, a positive electrode, a negative electrode, and an optional separator are wound into a flat spiral to form a wound electrode assembly, or these are stacked as flat plates to form a stacked electrode assembly, and the electrode assembly is sealed in an outer casing. Non-aqueous electrolyte secondary batteries are used as paper batteries, button batteries, coin batteries, stacked batteries, cylindrical batteries, prismatic batteries, etc.
[0117] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0118] Synthesis Example 1: Preparation of silicon nanoparticle dispersion A1 (silicon nanoparticle dispersion process) In a 150 ml small bead mill device container, zirconia beads with a particle size of 0.1 mm to 0.2 mm at a filling rate of 60% and 165 parts by mass of methyl ethyl ketone solvent (MEK) were added. Then, 40 parts by mass of silicon powder (manufactured by Kojundo Chemical Co., Ltd. "SIE23PB") with an average particle size of 5 μm and 8 parts by mass of cationic dispersant liquid (BYK Japan Co., Ltd. "BYK102") were added, and bead mill wet pulverization was performed to obtain a dark brown liquid silicon nanoparticle dispersion A1 with a solid concentration of 23% by mass. The average particle size (D50) of the silicon nanoparticles was 85 nm.
[0119] Synthesis Example 2: Preparation of silicon nanoparticle dispersion A2 (silicon nanoparticle dispersion process) In a 150 ml small bead mill device container, zirconia beads with a particle size of 0.1 mm to 0.2 mm at a filling rate of 60% and 193 parts by mass of methyl ethyl ketone solvent (MEK) were added. Then, 40 parts by mass of silicon powder (manufactured by Kojundo Chemical Co., Ltd. "SIE23PB") with an average particle size of 5 μm and 16 parts by mass of cationic dispersant liquid (BYK Japan Co., Ltd. "BYK102") were added, and bead mill wet pulverization was performed to obtain a dark brown liquid silicon nanoparticle dispersion A2 with a solid concentration of 23% by mass. The average particle diameter (D50) of the silicon nanoparticles was 83 nm.
[0120] Synthesis Example 3: Preparation of Composite Resin B1 A reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet was charged with 100 parts by weight of MEK, 469 parts by weight of glycidoxypropyltrimethoxysilane (GPTMS), and 275 parts by weight of dimethyldimethoxysilane (DMDMS). The temperature was raised to 75 ° C. with stirring, and a mixture of 1 part by weight of butyl acid phosphate and 160 parts by weight of deionized water was added dropwise over 1 hour. Then, 163 parts by weight of methyltrimethoxysilane (MTMS) was added, and the mixture was stirred at the same temperature for 4 hours to undergo a hydrolysis-condensation reaction, resulting in a reaction product. Next, the reaction product was distilled under conditions of a reduced pressure of 10 to 300 kPa and a temperature of 60 to 80°C for 10 hours to remove the produced methanol and water, and then 430 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of polysiloxane b1 having a nonvolatile content of 60.0% by mass.
[0121] Subsequently, a reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser and nitrogen gas inlet was charged with 350 parts by mass of the polysiloxane b1, 234 parts by mass of phenol, 234 parts by mass of 2-naphthol, 16 parts by mass of melamine, 344 parts by mass of 50% formalin, and 15.4 parts by mass of 25% aqueous ammonia, and the temperature was raised to 80 ° C. with stirring, and the reaction was carried out for 2 hours at 80 ° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 380 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B1 having a non-volatile content of 60.0% by mass.
[0122] In the obtained composite resin B1, the content of epoxy silane compounds in the total amount of silane compounds (hereinafter referred to as "epoxy silane content") was 37.5 mol%, and the mass ratio of the content of polysiloxane segments to the content of phenolic resin segments (hereinafter referred to as "PSi / Ph") was 30 / 70. In addition, the decomposition onset temperature of composite resin B1 measured by the method described below was 248°C.
[0123] Synthesis Example 4: Preparation of Composite Resin B2 The same synthesis procedure as for Composite Resin B1 was carried out, except that the amount of polysiloxane b1 added after obtaining the polysiloxane b1 was changed to 535 parts by mass, to obtain 1,000 parts by mass of a solution of Composite Resin B2. In the obtained Composite Resin B2, the epoxysilane content was 37.5 mol%, and the PSi / Ph ratio was 40 / 60. The decomposition onset temperature of Composite Resin B2, measured by the method described below, was 238 ° C.
[0124] Synthesis Example 5: Preparation of Composite Resin B3 After obtaining the polysiloxane b1, 213 parts by mass of the polysiloxane b1 was added, 496 parts by mass of 3,5-xylenol, 16 parts by mass of melamine, 292 parts by mass of 50% formalin, and 9.9 parts by mass of 25% aqueous ammonia. The mixture was heated to 80 ° C with stirring and reacted at 80 ° C for 2 hours. Next, dehydration was performed under reduced pressure of 10 to 300 kPa, and 410 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B3 with a non-volatile content of 60.0% by mass. In the obtained composite resin B3, the epoxysilane content was 37.5 mol%, and the PSi / Ph ratio was 20 / 80. The decomposition onset temperature of composite resin B3, measured using the method described below, was 310 ° C.
[0125] Synthesis Example 6: Preparation of Composite Resin B4 A reaction vessel equipped with a stirrer, thermometer, dropping funnel, cooling tube, and nitrogen gas inlet was charged with 180 parts by weight of MEK, 290 parts by weight of GPTMS, 374 parts by weight of DMDMS, and 277 parts by weight of MTMS. Then, the temperature in the system was raised to 70 ° C. with stirring, and a mixture of 5 parts by weight of triethylamine (TEA) and 200 parts by weight of deionized water was added dropwise over 2 hours. The mixture was then stirred at the same temperature for 6 hours to undergo a hydrolysis and condensation reaction, resulting in a reaction product. Next, the reaction product was distilled under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. for 10 hours to remove the produced methanol and water, and then 350 parts by weight of MEK was added to obtain 1,000 parts by weight of a solution of polysiloxane b2 having a non-volatile content of 60.0% by weight.
[0126] Subsequently, 213 parts by mass of the polysiloxane b2, 496 parts by mass of 3,5-xylenol, 16 parts by mass of melamine, 292 parts by mass of 50% formalin, and 9.9 parts by mass of 25% aqueous ammonia were charged into a reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser, and nitrogen gas inlet, and the mixture was heated to 80° C. with stirring and reacted for 2 hours at 80° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 410 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B4 having a nonvolatile content of 60.0% by mass.
[0127] In the obtained composite resin B4, the content of epoxysilane was 20 mol %, and PSi / Ph was 20 / 80. The decomposition starting temperature of composite resin B4 measured by the method described below was 301°C.
[0128] Synthesis Example 7: Preparation of Polysiloxane C A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet was charged with 1,421 parts by mass of MTMS, and the temperature was raised to 60° C. Next, a mixture of 0.17 parts by mass of butyl acid phosphate and 207 parts by mass of deionized water was added dropwise to the reaction vessel over 5 minutes, and the mixture was stirred at 80° C. for 4 hours to carry out a hydrolysis and condensation reaction of MTMS.
[0129] The condensate obtained by the hydrolysis-condensation reaction was distilled at a temperature of 40°C to 60°C under a reduced pressure of 40 kPa to 1.3 kPa. "Under a reduced pressure of 40 kPa to 1.3 kPa" means that the reduced pressure was 40 kPa at the start of methanol distillation and was ultimately reduced to 1.3 kPa. By removing the methanol and water produced during the reaction, 1,000 parts by mass of a liquid containing a MTMS condensate (c1) having a number-average molecular weight of 1,000 to 5,000 was obtained. The active ingredient content of the obtained liquid was 70% by mass.
[0130] The above-mentioned effective component is calculated by dividing the theoretical yield (parts by mass) when all methoxy groups of a silane monomer such as MTMS undergo a condensation reaction by the actual yield (parts by mass) after the condensation reaction, i.e., [theoretical yield (parts by mass) when all methoxy groups of a silane monomer undergo a condensation reaction / actual yield (parts by mass)].
[0131] Next, 150 parts by mass of MEK, 105 parts by mass of MTMS, and 277 parts by mass of DMDMS were placed in a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a condenser, and a nitrogen gas inlet, and the mixture was heated to 80°C.
[0132] Next, at the same temperature, a mixture containing 21 parts by mass of methyl methacrylate, 4 parts by mass of butyl methacrylate, 3 parts by mass of butyric acid, 2 parts by mass of methacryloyloxypropyltrimethoxysilane, 3 parts by mass of MEK, and 0.6 parts by mass of butylperoxy-2-ethylhexanoate was added dropwise to the reaction vessel over 6 hours. After completion of the addition, the mixture was allowed to react at the same temperature for an additional 20 hours to obtain an organic solvent solution of a vinyl polymer (c2) having a number average molecular weight of 10,000 and having hydrolyzable silyl groups.
[0133] Next, a mixture of 0.04 parts by mass of butyl acid phosphate and 112 parts by mass of deionized water was added dropwise over 5 minutes, and the mixture was stirred at the same temperature for a further 10 hours to cause a hydrolysis and condensation reaction, thereby obtaining a liquid containing a resin in which the hydrolyzable silyl group of the vinyl polymer (c2) and the hydrolyzable silyl group and silanol group of the polysiloxane derived from MTMS and DMDMS were bonded.
[0134] Next, 472 parts by mass of the MTMS condensate (c1) and 80 parts by mass of deionized water were added to this liquid, and the mixture was stirred at the same temperature for 10 hours to cause a hydrolysis and condensation reaction, and the produced methanol and water were removed by distillation under the same conditions as in Synthesis Example 2. Next, 250 parts by mass of MEK was added, yielding 1,000 parts by mass of a solution of polysiloxane C with a nonvolatile content of 60.1% by mass. The decomposition onset temperature of polysiloxane C, measured by the method described below, was 421°C.
[0135] Synthesis Example 8: Preparation of Composite Resin B5 A reaction vessel equipped with a stirrer, thermometer, dropping funnel, cooling tube, and nitrogen gas inlet was charged with 100 parts by weight of MEK, 665 parts by weight of GPTMS, 80 parts by weight of DMDMS, and 90 parts by weight of phenyltrimethoxysilane (PTMS). Then, the temperature in the system was raised to 70 ° C. with stirring, and a mixture of 1 part by weight of butyl acid phosphate and 160 parts by weight of deionized water was added dropwise over 1 hour. Then, 65 parts by weight of MTMS was added and stirred at the same temperature for 4 hours to cause a hydrolysis-condensation reaction, resulting in a reaction product. Next, the reaction product was distilled for 10 hours under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. to remove the produced methanol and water, and then 430 parts by weight of MEK was added to obtain 1,000 parts by weight of a solution of polysiloxane b3 having a non-volatile content of 60.0% by weight.
[0136] Subsequently, a reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser and nitrogen gas inlet was charged with 350 parts by mass of the polysiloxane b3, 234 parts by mass of phenol, 234 parts by mass of 2-naphthol, 16 parts by mass of melamine, 344 parts by mass of 50% formalin, and 15.4 parts by mass of 25% aqueous ammonia, and the temperature was raised to 80 ° C. with stirring, and the reaction was carried out for 2 hours at 80 ° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 380 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B5 having a non-volatile content of 60.0% by mass.
[0137] In the obtained composite resin B5, the content of epoxysilane was 65 mol %, the content of phenyltrimethoxysilane was 10 mol %, and PSi / Ph was 30 / 70.
[0138] Synthesis Example 9: Preparation of Composite Resin B6 A reaction vessel equipped with a stirrer, thermometer, dropping funnel, cooling tube, and nitrogen gas inlet was charged with 100 parts by weight of MEK, 341 parts by weight of GPTMS, 116 parts by weight of DMDMS, and 301 parts by weight of PTMS. Then, the temperature in the system was raised to 70 ° C. with stirring, and a mixture of 1 part by weight of butyl acid phosphate and 160 parts by weight of deionized water was added dropwise over 1 hour. Then, 145 parts by weight of MTMS was added and stirred at the same temperature for 4 hours to cause a hydrolysis and condensation reaction, resulting in a reaction product. Next, the reaction product was distilled for 10 hours under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. to remove the produced methanol and water, and then 430 parts by weight of MEK was added. 1,000 parts by weight of a solution of polysiloxane b4 with a non-volatile content of 60.0% by weight was obtained.
[0139] Subsequently, a reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser and nitrogen gas inlet was charged with 350 parts by mass of the polysiloxane b4, 234 parts by mass of phenol, 234 parts by mass of 2-naphthol, 344 parts by mass of 50% formalin, and 15.4 parts by mass of 25% aqueous ammonia, and the temperature was raised to 80 ° C. with stirring, and the reaction was carried out for 2 hours at 80 ° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 380 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B6 having a non-volatile content of 60.0% by mass.
[0140] In the obtained composite resin B6, the content of epoxysilane was 30 mol %, the content of phenyltrimethoxysilane was 30 mol %, and PSi / Ph was 30 / 70.
[0141] Synthesis Example 10: Preparation of Composite Resin B7 A reaction vessel equipped with a stirrer, thermometer, dropping funnel, cooling tube, and nitrogen gas inlet was charged with 100 parts by weight of MEK, 140 parts by weight of GPTMS, 100 parts by weight of DMDMS, and 515 parts by weight of PTMS. Then, the temperature in the system was raised to 70 ° C. with stirring, and a mixture of 1 part by weight of butyl acid phosphate and 160 parts by weight of deionized water was added dropwise over 1 hour. Then, 155 parts by weight of MTMS was added and stirred at the same temperature for 4 hours to cause a hydrolysis and condensation reaction, resulting in a reaction product. Next, the reaction product was distilled for 10 hours under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. to remove the produced methanol and water, and then 430 parts by weight of MEK was added. 1,000 parts by weight of a solution of polysiloxane b5 having a non-volatile content of 60.0% by weight was obtained.
[0142] Subsequently, a reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser and nitrogen gas inlet was charged with 350 parts by mass of the polysiloxane b5, 234 parts by mass of phenol, 234 parts by mass of 2-naphthol, 16 parts by mass of melamine, 344 parts by mass of 50% formalin, and 15.4 parts by mass of 25% aqueous ammonia, and the temperature was raised to 80 ° C. with stirring, and the reaction was carried out for 2 hours at 80 ° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 380 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B7 having a non-volatile content of 60.0% by mass.
[0143] In the obtained composite resin B7, the content of epoxysilane was 12 mol %, the content of phenyltrimethoxysilane was 50 mol %, and PSi / Ph was 30 / 70.
[0144] Synthesis Example 11: Preparation of Composite Resin B8 A reaction vessel equipped with a stirrer, thermometer, dropping funnel, cooling tube, and nitrogen gas inlet was charged with 100 parts by weight of MEK, 105 parts by weight of GPTMS, 39 parts by weight of DMDMS, and 740 parts by weight of PTMS. Then, the temperature in the system was raised to 70 ° C. with stirring, and a mixture of 1 part by weight of butyl acid phosphate and 160 parts by weight of deionized water was added dropwise over 1 hour. Then, 19 parts by weight of MTMS was added, and the mixture was stirred at the same temperature for 4 hours to cause a hydrolysis-condensation reaction, resulting in a reaction product. Next, the reaction product was distilled for 10 hours under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. to remove the produced methanol and water, and then 430 parts by weight of MEK was added. 1,000 parts by weight of a solution of polysiloxane b6 having a non-volatile content of 60.0% by weight was obtained.
[0145] Subsequently, a reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser and nitrogen gas inlet was charged with 350 parts by mass of the polysiloxane b6, 234 parts by mass of phenol, 234 parts by mass of 2-naphthol, 16 parts by mass of melamine, 344 parts by mass of 50% formalin, and 15.4 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80 ° C. with stirring and reacted for 2 hours at 80 ° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 380 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B8 having a non-volatile content of 60.0% by mass.
[0146] In the obtained composite resin B8, the content of epoxysilane was 10 mol %, the content of phenyltrimethoxysilane was 80 mol %, and PSi / Ph was 30 / 70.
[0147] Synthesis Example 12: Preparation of Composite Resin B9 A reaction vessel equipped with a stirrer, thermometer, dropping funnel, cooling tube, and nitrogen gas inlet was charged with 100 parts by weight of MEK, 52 parts by weight of GPTMS, 16 parts by weight of DMDMS, and 825 parts by weight of PTMS. Then, the temperature in the system was raised to 70 ° C. with stirring, and a mixture of 1 part by weight of butyl acid phosphate and 160 parts by weight of deionized water was added dropwise over 1 hour. Then, 13 parts by weight of MTMS was added, and the mixture was stirred at the same temperature for 4 hours to undergo a hydrolysis-condensation reaction, resulting in a reaction product. Next, the reaction product was distilled for 10 hours under a reduced pressure of 10 to 300 kPa at 60 to 80 ° C. to remove the produced methanol and water, and then 430 parts by weight of MEK was added. 1,000 parts by weight of a solution of polysiloxane b7 with a non-volatile content of 60.0% by weight was obtained.
[0148] Subsequently, a reaction vessel equipped with a stirrer, thermometer, dropping funnel, condenser and nitrogen gas inlet was charged with 350 parts by mass of the polysiloxane b7, 234 parts by mass of phenol, 234 parts by mass of 2-naphthol, 16 parts by mass of melamine, 344 parts by mass of 50% formalin, and 15.4 parts by mass of 25% aqueous ammonia, and the mixture was heated to 80 ° C. with stirring and reacted for 2 hours at 80 ° C. Next, dehydration was carried out under reduced pressure of 10 to 300 kPa, and 380 parts by mass of MEK was added to obtain 1,000 parts by mass of a solution of composite resin B9 having a non-volatile content of 60.0% by mass.
[0149] In the obtained composite resin B9, the content of epoxysilane was 5 mol %, the content of phenyltrimethoxysilane was 90 mol %, and PSi / Ph was 30 / 70.
[0150] [Example 1] (Homogenization Step) 640 parts by mass of the silicon nanoparticle dispersion A1 obtained in Synthesis Example 1 and 360 parts by mass of the composite resin B1 produced in Synthesis Example 3 were thoroughly mixed in a stirrer. As a result, a suspension of a negative electrode precursor mixture with a solid concentration of 36.3 mass% was obtained. Subsequently, the solvent was removed in a 120°C oil bath under nitrogen flow conditions, and then the mixture was dried under reduced pressure at 110°C for 10 hours using a vacuum dryer to obtain a dried product of the precursor mixture as a negative electrode active material precursor.
[0151] (Firing Step) The dried product obtained in the homogenization step was fired in a nitrogen atmosphere at 1100° C. for 4 hours to obtain a black solid product.
[0152] (Pulverization Step) The black solid obtained in the firing step was pulverized in a planetary ball mill to prepare a negative electrode active material.
[0153] Example 2 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 644 parts by mass of the silicon nanoparticle dispersion A1 and 356 parts by mass of the composite resin B2 prepared in Synthesis Example 4 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 36.2% by mass.
[0154] Example 3 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 587 parts by mass of the silicon nanoparticle dispersion A1 and 413 parts by mass of the composite resin B3 prepared in Synthesis Example 5 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 38.3% by mass.
[0155] Example 4 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 564 parts by mass of the silicon nanoparticle dispersion A1 and 436 parts by mass of the composite resin B4 prepared in Synthesis Example 6 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 39.1% by mass.
[0156] Example 5 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 604 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 396 parts by mass of the composite resin B1 produced in Synthesis Example 3 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 37.7% by mass.
[0157] Example 6 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 608 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 392 parts by mass of the composite resin B2 produced in Synthesis Example 4 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 37.5% by mass.
[0158] Example 7 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 550 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 450 parts by mass of the composite resin B3 produced in Synthesis Example 5 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 39.7% by mass.
[0159] Example 8 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 526 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 474 parts by mass of the composite resin B4 produced in Synthesis Example 6 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 40.5% by mass.
[0160] Example 9 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 649 parts by mass of the silicon nanoparticle dispersion A1 obtained in Synthesis Example 1 and 351 parts by mass of the composite resin B5 produced in Synthesis Example 8 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 36.0% by mass.
[0161] Example 10 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 667 parts by mass of the silicon nanoparticle dispersion A1 obtained in Synthesis Example 1 and 333 parts by mass of the composite resin B6 produced in Synthesis Example 9 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 35.3 mass%.
[0162] Example 11 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 682 parts by mass of the silicon nanoparticle dispersion A1 obtained in Synthesis Example 1 and 318 parts by mass of the composite resin B7 produced in Synthesis Example 10 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 34.8% by mass.
[0163] Example 12 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 703 parts by mass of the silicon nanoparticle dispersion A1 obtained in Synthesis Example 1 and 297 parts by mass of the composite resin B8 produced in Synthesis Example 11 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 34.0% by mass.
[0164] Example 13 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 709 parts by mass of the silicon nanoparticle dispersion A1 obtained in Synthesis Example 1 and 291 parts by mass of the composite resin 9 produced in Synthesis Example 12 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 33.8% by mass.
[0165] Example 14 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 614 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 386 parts by mass of the composite resin 5 produced in Synthesis Example 8 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 37.3 mass%.
[0166] Example 15 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 631 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 369 parts by mass of the composite resin 6 produced in Synthesis Example 9 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 36.6 mass%.
[0167] Example 16 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 648 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 352 parts by mass of the composite resin 7 produced in Synthesis Example 10 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 36.0 mass%.
[0168] Example 17 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 670 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 330 parts by mass of the composite resin 8 produced in Synthesis Example 11 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 35.2 mass%.
[0169] Example 18 A negative electrode active material was prepared in the same manner as in Example 1, except that in the homogenization step, 676 parts by mass of the silicon nanoparticle dispersion A2 obtained in Synthesis Example 2 and 324 parts by mass of the composite resin 9 produced in Synthesis Example 12 were used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 35.0 mass%.
[0170] Comparative Example 1 A negative electrode active material was produced in the same manner as in Example 1, except that in the homogenization step, 665.8 parts by mass of the silicon nanoparticle dispersion A1 obtained in Synthesis Example 1, 49.6 parts by mass of polysiloxane C produced in Synthesis Example 7, and 284.6 parts by mass of a phenolic resin ("HE100C-30" manufactured by Air Water Performance Chemicals Inc.) to which methyl ethyl ketone had been added as an organic solvent was used to obtain a suspension of a negative electrode precursor mixture having a solid concentration of 21.9% by mass.
[0171] The average particle size (D50) of the silicon nanoparticles was measured using a Mastersizer 3000 (Laser Micron Sizer LMS-3000, manufactured by Malvern Instruments).
[0172] (Measurement of Resin Decomposition Onset Temperature) First, the resin to be measured was dried under reduced pressure at 110°C for 10 hours using a vacuum dryer. To measure the resin decomposition onset temperature, approximately 10 mg of the dried resin was weighed into a Pt pan, the weight was accurately recorded, and the TG-DTA device was placed in a nitrogen flow at a temperature increase rate of 10° / min and a maximum temperature of 1000°C. The measurement device used was a Rigaku Thermo PIUS EV02. The obtained results were analyzed using the software provided with the Rigaku Thermo PIUS EV02, and the decomposition onset temperature was recorded.
[0173] (Evaluation of Uniformity of Dried Product) For the dried product of the precursor mixture, carbon, nitrogen, oxygen, and silicon were quantified using SEM-EDX (JSM-7800F, manufactured by JEL), and the element ratio (mass ratio) of these elements, C / N / O / Si, was determined. Furthermore, for each of Examples 1 to 4 and Comparative Example 1, the results of element mapping of the dried product are shown in Figures 1 to 5, respectively. In Figures 1 to 5, the white mapped areas correspond to silicon (Si), and the black mapped areas correspond to carbon (C).
[0174] (Evaluation of Battery Characteristics) Each negative electrode active material (8 parts by mass) obtained above, acetylene black (1 part by mass) as a conductive additive, and an organic binder (1 part by mass, breakdown: SBR (0.75 parts by mass) + CMC (0.25 parts by mass)) were mixed and stirred for 10 minutes using a rotation-revolution type foaming blender to prepare a slurry. The slurry was applied to a copper foil having a thickness of 20 μm using an applicator, and then dried at 110 ° C under reduced pressure to obtain a thin electrode film. Subsequently, a circular electrode having a diameter of 14 mm was punched out and pressed using a tablet press to a thickness of approximately 40 μm. The thickness was measured by calculating the average value of five points on the thin electrode film using a thickness meter. In a dry room with an extremely low moisture content (dew point -40 ° C or less), a Li foil was placed opposite the thin electrode film via a 25 μm thick polypropylene separator. Thereafter, an electrolyte (Kishida Chemical Co., Ltd., 1 mol / L LiPF 6 A half battery (CR2032 type) for evaluation was fabricated by adsorbing a 1:1 (volume ratio) diethyl carbonate:ethylene carbonate. The battery characteristics of the resulting half battery were measured using a secondary battery charge / discharge tester (Hokuto Denko Corporation). The battery was kept at room temperature of 25°C, with a cutoff voltage range of 0.005 to 1.5 V, and a charge / discharge rate of 0.1 C (1 to 3 cycles) and 0.2 C (after 4 cycles). The battery was then subjected to a constant-current / constant-voltage charge / constant-current discharge test. The battery was left open-circuited for 30 minutes between each charge / discharge cycle. The initial efficiency and cycle characteristics (referring to the retention rate of discharge capacity after 10 cycles) were determined as follows. The results are shown in Tables 1 to 4. Initial efficiency (%) = initial discharge capacity (mAh / g) / initial charge capacity (mAh / g) Retention rate (%) = initial discharge capacity (mAh / g) / discharge capacity after 10 cycles (mAh / g)
[0175]
[0176]
[0177]
[0178]
[0179] As can be seen from Tables 1 to 4, the use of a composite resin of polysiloxane and phenolic resin significantly improved the discharge capacity retention rate compared to when a mixture of polysiloxane and phenolic resin was used. When a composite resin of polysiloxane and phenolic resin was used, as can be seen from a comparison of Figures 1 to 4 with Figure 5, the homogeneity of the components in the precursor was higher than when a mixture of polysiloxane and phenolic resin was used, and it is presumed that this improvement in the discharge capacity retention rate was achieved.
Claims
1. A composition containing silicon nanoparticles and a composite resin in which a polysiloxane and a phenolic resin are bonded to each other.
2. The composition according to claim 1, which is used to manufacture a secondary battery material.
3. The composition according to claim 1, which is used to manufacture a negative electrode active material.
4. A method for producing a negative electrode active material, comprising a step of firing a composition containing silicon nanoparticles and a composite resin in which polysiloxane and a phenolic resin are bonded to each other.
5. A negative electrode active material comprising a fired product of a composition containing silicon nanoparticles and a composite resin in which polysiloxane and a phenolic resin are bonded to each other.
6. A secondary battery comprising a negative electrode containing the negative electrode active material according to claim 5.
Citation Information
Patent Citations
Silicon-based composite negative electrode material for lithium ion battery
CN104241621A
Silicon nanoparticles, non-aqueous secondary battery negative electrode active material using said silicon nanoparticles, and secondary battery
WO2020129467A1
Secondary battery material, negative electrode active material, and secondary battery
WO2023017694A1
Cited By
Preparation method and application of organic matter modified vanadium oxide composite material