Secondary battery

The secondary battery design with regionally varying positive electrode core strength and a non-aqueous electrolyte system addresses deformation and elongation issues during charging and discharging, enhancing performance and safety by managing stress and elongation effectively.

WO2024224996A1PCT designated stage expired Publication Date: 2024-10-31PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD

Patent Information

Application Number
PCT/JP2024/014107
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-05
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Secondary batteries with wound-type electrode bodies experience deformation and elongation during charging and discharging, leading to reduced performance and increased risk of short circuits due to local stress and expansion.

Method used

A secondary battery design featuring a positive electrode core with distinct regions of varying yield strength, where the 0.2% proof stress is 50 N/mm² in the first region and 100 N/mm² in the second region, to manage stress and elongation, using a strip-shaped positive electrode core and composite layer, and a negative electrode wound with a separator, along with a non-aqueous electrolyte and specific materials for the electrodes and separator.

Benefits of technology

This design effectively suppresses electrode plate deformation and elongation during charging and discharging, maintaining battery performance and reducing the risk of short circuits by distributing stress and controlling elongation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014107_31102024_PF_FP_ABST
    Figure JP2024014107_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a secondary battery capable of suppressing electrode plate deformation and electrode plate elongation caused by charging and discharging. This secondary battery has an electrode body in which a negative electrode and a positive electrode, which has a belt-like positive electrode core body (30) and a positive electrode mixture layer provided on the positive electrode core body (30), are wound with a separator therebetween. The secondary battery is characterized in that: the positive electrode core body (30) has a first region (32) which is a winding start end part and a second region (34) which is a region other than the first region (32); the 0.2% yield strength of the positive electrode core body in the first region (32) is 50 N / mm2 or less; and the 0.2% yield strength of the positive electrode core body in the second region (34) is greater than 50 N / mm2.
Need to check novelty before this filing date? Find Prior Art

Description

secondary battery

[0001] The present disclosure relates to secondary batteries.

[0002] Secondary batteries such as lithium-ion secondary batteries are used as power sources for a wide range of devices, including electric vehicles, and there is a demand for ever higher capacity. A secondary battery has a configuration in which, for example, a wound electrode assembly in which a positive electrode and a negative electrode are wound with a separator interposed therebetween is enclosed in an outer can together with an electrolyte solution and the like (for example, Patent Document 1).

[0003] International Publication No. 2020 / 045375

[0004] In secondary batteries equipped with a wound electrode assembly in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, local stress is applied to the center (winding core) of the electrode assembly when the electrode assembly expands during charging and discharging, which can cause plate deformation at the electrode's winding start end. Plate deformation can lead to a decrease in battery performance. While this plate deformation can be improved by using a soft positive electrode core, this can sometimes result in plate elongation, in which the positive electrode core stretches in the width direction (the direction of the electrode assembly's winding axis). Furthermore, if the plate elongation becomes significant during charging and discharging, the distance from one end of the positive electrode to one end of the negative electrode in the direction of the electrode assembly's winding axis becomes shorter, increasing the risk of short circuiting.

[0005] Therefore, an object of the present disclosure is to provide a secondary battery capable of suppressing deformation and elongation of electrode plates that occur during charging and discharging.

[0006] The present disclosure relates to a secondary battery having an electrode assembly in which a positive electrode having a strip-shaped positive electrode core and a positive electrode composite layer provided on the positive electrode core, and a negative electrode are wound together with a separator interposed therebetween, the positive electrode core having a first region at a winding start end and a second region other than the first region, and the 0.2% yield strength of the positive electrode core in the first region is 50 N / mm 2 The 0.2% yield strength of the positive electrode substrate in the second region is 50 N / mm 2 It is characterized by being super.

[0007] According to the present disclosure, a secondary battery can be provided that can suppress electrode plate deformation and electrode plate elongation that occur during charging and discharging.

[0008] 1 is a schematic cross-sectional view of a secondary battery according to an embodiment of the present invention;

[0009] An example of an embodiment of a secondary battery according to the present disclosure will be described in detail below.

[0010] Fig. 1 is a schematic cross-sectional view of a secondary battery according to an embodiment. The secondary battery 10 shown in Fig. 1 includes a wound electrode assembly 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, a non-aqueous electrolyte, insulating plates 18 and 19 disposed above and below the electrode assembly 14, and a battery case 15 serving as an exterior body. The battery case 15 is composed of a case body 16 that houses the electrode assembly 14, the non-aqueous electrolyte, and the like, and a sealing body 17 that closes the opening of the case body 16. The battery case 15 is not limited to a cylindrical or rectangular metal case, and may be, for example, a resin case formed by laminating a resin sheet (a so-called laminate type).

[0011] The non-aqueous electrolyte is, for example, an electrolyte having lithium ion conductivity, and may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.

[0012] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. Examples of the non-aqueous solvent include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents of these. The non-aqueous solvent may contain a halogen-substituted compound (e.g., fluoroethylene carbonate) in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. Examples of the electrolyte salt include LiPF 6 Lithium salts such as

[0013] Furthermore, examples of the solid electrolyte that can be used include solid or gel polymer electrolytes, inorganic solid electrolytes, etc. Examples of the inorganic solid electrolyte that can be used include materials known in all-solid-state lithium ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halogen-based solid electrolytes, etc.) Examples of the polymer electrolyte include a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. Examples of the matrix polymer include a polymer material that absorbs a non-aqueous solvent and gels. Examples of the polymer material include fluororesins, acrylic resins, and polyether resins. The non-aqueous electrolyte is just one example, and aqueous electrolytes may also be used if applicable.

[0014] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 22, which is a portion of the side surface that protrudes inward and supports the sealing body 17. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.

[0015] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and all components except for the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. If the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 may deform and rupture, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure further increases, the upper valve body 26 may rupture, and gas may be discharged from the opening of the cap 27.

[0016] In the secondary battery 10 shown in Fig. 1, a positive electrode lead 20 attached to the positive electrode 11 passes through a through-hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom side of the case body 16. The positive electrode lead 20 is connected by welding or the like to the underside of a filter 23, which is the bottom plate of the sealing body 17, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected by welding or the like to the inner bottom surface of the case body 16, and the case body 16 serves as the negative electrode terminal.

[0017] The positive electrode 11, the negative electrode 12, and the separator 13 will be described in detail below.

[0018] The positive electrode 11 has a strip-shaped positive electrode core and a positive electrode composite layer provided on the positive electrode core. The positive electrode composite layer may be formed on both sides of the positive electrode core or on one side of the positive electrode core. The positive electrode core may be made of a foil of a metal such as aluminum that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface layer. The positive electrode composite layer includes, for example, a positive electrode active material, a binder, a conductive material, etc. The positive electrode composite layer can be produced, for example, by applying a positive electrode composite slurry containing a positive electrode active material, a binder, a conductive material, etc. to the positive electrode core, drying the coating, and then rolling it.

[0019] Fig. 2 is a schematic plan view showing an example of a positive electrode core. In Fig. 2, the positive electrode core 30 is shown in a straightly extended state. The longitudinal direction (direction of arrow X) of the positive electrode core 30 shown in Fig. 2 is the winding direction of the positive electrode 11. In Fig. 2, the right side of the paper surface is the winding start side of the positive electrode 11, and the left side of the paper surface is the winding end side of the positive electrode 11.

[0020] 2, the positive electrode substrate 30 has a first region 32 at the winding start end, which is the winding start side of the positive electrode 11, and a second region 34, which is the region other than the first region 32. The 0.2% yield strength of the positive electrode substrate 30 in the first region 32 is 50 N / mm 2 The 0.2% yield strength of the positive electrode substrate 30 in the second region 34 is 50 N / mm 2 The 0.2% yield strength of the positive electrode substrate 30 in the first region 32 is 50 N / mm 2By softening the positive electrode substrate 30 in the first region 32 as described below, it is possible to disperse stress that is locally applied to the center of the electrode body 14 due to charge and discharge, making it possible to suppress plate deformation at the winding start end of the electrode. Furthermore, in the second region 34, which is located on the outer side in the winding direction than the first region 32 at the winding start end, plate elongation, in which the positive electrode substrate 30 stretches in the width direction due to charge and discharge, is more likely to occur. However, in this embodiment, the 0.2% yield strength of the positive electrode substrate 30 in the second region 34 is 50 N / mm 2 By making the positive electrode substrate 30 in the second region 34 harder than the positive electrode substrate 30 in the first region 32, it is possible to suppress electrode plate elongation due to charge and discharge. The 0.2% yield strength of the positive electrode substrate 30 in the second region 34 is, for example, 100 N / mm 2 It is preferable that this is equal to or greater than this.

[0021] The method for measuring the 0.2% yield strength will be described. For example, a 12.5 mm x 63 mm positive electrode substrate (test piece) is cut out from each of the first region 32 and the second region 34. A tensile test is performed on the test piece on the first region 32 side and the test piece on the second region 34 side, and the 0.2% yield strength is determined from the stress-strain curve (hereinafter referred to as the SS curve) obtained by the tensile test. Specifically, the 0.2% strain point on the SS curve is used as a reference point, and a straight line parallel to the rising slope of the SS curve is drawn from that reference point. The intersection of this line and the SS curve is the value of the 0.2% yield strength. The value of the 0.2% yield strength is the average of the test results for 10 test pieces. The SS curve is measured in accordance with JIS C5016-1994.

[0022] The positive electrode substrate 30 has a resistance of, for example, 50 N / mm 2 More than 100 N / mm 2 The above-described core body was prepared, and the first region 32 of the core body was heat-treated to reduce the 0.2% yield strength of the first region 32 to 50 N / mm 2The positive electrode core 30 is fabricated by the following method. While the heat treatment method is not particularly limited, a method in which a heating roller is brought into contact with the first region 32 is preferred because it is easy to heat only the first region 32. Other heat treatment methods include, for example, infrared heating. The heat treatment temperature is preferably, for example, 180°C or higher and 250°C or lower. The thickness of the positive electrode core 30 is preferably, for example, 10 μm or higher and 50 μm or lower, so that the 0.2% proof stress of the second region can be maintained high. Note that the 0.2% proof stress is also affected by the thickness of the positive electrode core 30. Therefore, even without the above-described heat treatment, by reducing the thickness of the first region 32 and increasing the thickness of the second region, a positive electrode core 30 can be obtained in which the 0.2% proof stress of the first region 32 and the second region 34 satisfies the above-mentioned value.

[0023] In order to further suppress deformation and elongation of the electrode plate due to charging and discharging, it is preferable that the length W1 of the first region 32 in the winding direction of the positive electrode 11 (the direction of arrow X) be 1 / 10 or less of the total length W of the positive electrode core 30 in the winding direction of the positive electrode 11, and it is preferable that the length W2 of the second region 34 in the winding direction of the positive electrode 11 be 9 / 10 or more of the total length W of the positive electrode core 30 in the winding direction of the positive electrode 11.

[0024] The positive electrode active material contained in the positive electrode mixture layer can be, for example, a lithium transition metal oxide containing a transition metal element such as Co, Mn, or Ni. x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co y Ni 1-y O 2 , Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn 2 O 4 , Li x Mn 2-y M y O4 , LiMPO 4 , Li 2 MPO 4 F (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, 0<x≦1.2, 0<y≦0.9, 2.0≦z≦2.3). These may be used alone or in combination. The thickness of the positive electrode composite layer is, for example, in the range of 10 μm or more and 100 μm or less.

[0025] Examples of the binder contained in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), and polyethylene oxide (PEO).

[0026] Examples of the conductive material contained in the positive electrode mixture layer include carbon materials such as carbon black (CB), acetylene black (AB), ketjen black, carbon nanotubes (CNT), graphene, and graphite.

[0027] The negative electrode 12 has, for example, a strip-shaped negative electrode core and a negative electrode composite layer disposed on the negative electrode core. The negative electrode composite layer may be formed on both sides of the negative electrode core or on one side of the negative electrode core. The negative electrode core may be a foil of a metal such as copper that is stable within the potential range of the negative electrode 12, or a film with such a metal disposed on the surface layer. The thickness of the negative electrode core is, for example, in the range of 5 μm to 50 μm. The negative electrode composite layer includes, for example, a negative electrode active material and a binder. The thickness of the negative electrode composite layer 50 is, for example, in the range of 10 μm to 100 μm. The negative electrode 12 can be produced, for example, by applying a negative electrode paste containing a negative electrode active material and a binder to the surface of the negative electrode core, drying the coating, and then rolling it.

[0028] Examples of the negative electrode active material include materials that can reversibly absorb and release lithium ions, such as carbon materials such as natural graphite and artificial graphite, metals such as Si and Sn, alloys, or oxides. Examples of the binder include those similar to those in the case of the positive electrode 11. The negative electrode mixture layer may contain a conductive material. Examples of the conductive material include those similar to those in the case of the positive electrode 11.

[0029] The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of porous sheets include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator include olefin-based resins such as polyethylene and polypropylene, and cellulose. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin-based resin. Alternatively, the separator 13 may be a multilayer separator including a polyethylene layer and a polypropylene layer, and the surface of the separator 13 may be coated with a material such as an aramid-based resin or ceramic.

[0030] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0031] <Example> [Preparation of Positive Electrode] 100 parts by mass of LiNi 0.88 Co 0.09 Al 0.03 O 2 1 part by mass of acetylene black (AB) and 0.9 parts by mass of polyvinylidene fluoride (PVDF) were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode composite slurry. Next, the positive electrode composite slurry was applied to both sides of an aluminum foil serving as a positive electrode core, and the coating was dried. Then, the coating was rolled using a roller and then cut to a predetermined electrode size, and a positive electrode having a positive electrode composite layer formed on both sides of the positive electrode core was produced.

[0032] The specifications of the aluminum foil used were as follows: Total length W of aluminum foil: 861 mm (width: 63 mm, thickness: 15 μm) Ratio of length W1 of first region to length W2 of second region: 1:9 0.2% yield strength of first region: 41 N / mm 2 0.2% yield strength of the second region: 152 N / mm 2

[0033] [Preparation of Negative Electrode] 100 parts by mass of graphite powder, 1 part by mass of carboxymethyl cellulose sodium (CMC-Na), and 1 part by mass of a dispersion of styrene butadiene rubber (SBR) were mixed, and an appropriate amount of water was added to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied to both sides of a copper foil with a thickness of 8 μm, and the coating was dried. Then, a negative electrode was prepared by rolling the coating using a roller.

[0034] [Preparation of non-aqueous electrolyte] 5 parts by mass of vinylene carbonate (VC) was added to 100 parts by mass of a mixed solvent in which ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 3:7, and lithium hexafluorophosphate (LiPF 6 A non-aqueous electrolyte was prepared by dissolving 1.5 mol / L of ammonium hydroxide in water.

[0035] [Fabrication of Secondary Battery] A positive electrode lead was attached to the positive electrode, and a negative electrode lead was attached to the negative electrode. The positive and negative electrodes were then wound with a separator interposed therebetween to fabricate a wound electrode assembly. Insulating plates were placed above and below the electrode assembly, and the electrode assembly was housed in a case body. The negative electrode lead was welded to the bottom of the case body, and the positive electrode lead was welded to a sealing member. After injecting a nonaqueous electrolyte into the case body, the opening of the case body was sealed with a sealing member via a gasket to fabricate a secondary battery.

[0036] <Comparative Example 1> In the production of the positive electrode, the 0.2% proof stress of the first region and the second region was 41 N / mm 2 A secondary battery was fabricated in the same manner as in Example 1, except that an aluminum foil of the same material was used.

[0037] <Comparative Example 2> In the production of the positive electrode, the 0.2% yield strength of the first region and the second region was 152 N / mm 2 A secondary battery was fabricated in the same manner as in Example 1, except that an aluminum foil of the same material was used.

[0038] [Charge / Discharge Test] The secondary batteries of the example and comparative examples were charged at a constant current of 0.3 C in a temperature environment of 25° C., and then charged at a constant voltage until the charging current became 0.01 mA or less when the battery voltage reached 4.2 V. Next, a constant current discharge of 0.5 C was performed until the battery voltage reached 2.5 V. This charge / discharge cycle was repeated 500 times.

[0039] Using an X-ray CT device (Shimadzu Corporation, SMX-225CT FPD HR), the center of the electrode body of the secondary batteries of the Examples and each Comparative Example after the charge-discharge test was observed, and the presence or absence of plate deformation was evaluated. The results are summarized in Table 1. Regarding the evaluation of plate deformation, if the electrode at the center of the electrode body was not bent, it was deemed that no plate deformation had occurred and was given a rating of A, and if the electrode at the center of the electrode body was bent, it was deemed that plate deformation had occurred and was given a rating of B. Furthermore, using an X-ray CT device (Shimadzu Corporation, SMX-225CT FPD HR), the end of the electrode body in the winding axis direction of the secondary batteries of the Examples and each Comparative Example was observed, and plate elongation was evaluated. The results are summarized in Table 1. The evaluation of electrode plate elongation was performed using the distance from one end of the positive electrode to one end of the adjacent negative electrode in the direction of the winding axis of the electrode body before the charge / discharge test as the reference (1.0). If the above distance in the electrode body after the charge / discharge test was 0.5 or more, the electrode plate elongation was suppressed and the evaluation was given an A rating, and if the above distance in the electrode body after the charge / discharge test was less than 0.5, the electrode plate elongation was generated and the evaluation was given a B rating.

[0040]

[0041] In the examples, plate deformation and elongation due to charge and discharge were suppressed. On the other hand, plate elongation due to charge and discharge occurred in Comparative Example 1, and plate deformation due to charge and discharge occurred in Comparative Example 2. From these results, it was found that the 0.2% yield strength of the positive electrode substrate in the first region at the winding start end was 50 N / mm 2 and the 0.2% yield strength of the positive electrode substrate in the second region other than the first region is 50 N / mm 2 It can be said that by using a thick positive electrode substrate, it is possible to suppress deformation and elongation of the electrode plate that accompanies charge and discharge.

[0042] 10 Secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 15 Battery case, 16 Case body, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Protruding portion, 23 Filter, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket, 30 Positive electrode core body, 32 First region, 34 Second region.

Claims

1. A secondary battery having an electrode assembly in which a positive electrode having a strip-shaped positive electrode core and a positive electrode composite layer provided on the positive electrode core, and a negative electrode are wound with a separator interposed therebetween, the positive electrode core having a first region at a winding start end and a second region other than the first region, and the 0.2% yield strength of the positive electrode core in the first region is 50 N / mm 2 The 0.2% yield strength of the positive electrode core body in the second region is 50 N / mm 2 A super secondary battery.

2. The 0.2% yield strength of the positive electrode substrate in the second region is 100 N / mm 2 The secondary battery according to claim 1 .

3. A secondary battery as described in claim 1 or 2, wherein the length of the first region in the winding direction of the positive electrode is 1 / 10 or less of the total length of the positive electrode core in the winding direction of the positive electrode, and the length of the second region in the winding direction of the positive electrode is 9 / 10 or more of the total length of the positive electrode core in the winding direction of the positive electrode.

Citation Information

Patent Citations

  • Electrochemical device

    WO2020045375A1

  • Conductive core for electrode plate of battery and battery using the same

    JP2002110171A

  • Alkaline storage battery

    JP2004247221A

  • Nonaqueous electrolyte secondary battery

    WO2022168852A1

Cited By

  • Cylindrical battery

    WO2026205015A1