Electrode for secondary batteries, and secondary battery

The secondary battery electrode design with a core and composite material layer arrangement, along with a rust prevention layer, addresses the issue of increased resistance by maintaining the interface state and preventing oxide film formation, thereby enhancing battery performance.

WO2024225030A1PCT designated stage expired Publication Date: 2024-10-31PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014437
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-09
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The formation of an oxide film on the surface of secondary battery electrodes due to long-term storage or heat treatment leads to increased resistance, which is typically addressed through anti-rust treatments that can alter the interface state between the core and the composite material layer, further increasing battery resistance.

Method used

A secondary battery electrode design featuring a core with an exposed portion without the composite material layer and a composite material layer arrangement part, where the lightness index of the surface is measured to ensure a specific relationship between heating times, thereby suppressing the increase in battery resistance. The core is treated with a rust prevention layer, including a chromium-containing layer, to maintain the interface state and prevent discoloration.

Benefits of technology

This design effectively suppresses the increase in battery resistance by maintaining the interface state between the core and the composite material layer, while the rust prevention layer prevents discoloration and oxide film formation, ensuring optimal battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014437_31102024_PF_FP_ABST
    Figure JP2024014437_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an electrode for secondary batteries, the electrode being capable of suppressing an increase in the battery resistance. An electrode (30) for secondary batteries comprises a core body (32) and a mixture layer (34) that is disposed on the core body (32). The electrode (30) is characterized in that: the core body (32) has an exposed part (36) in which the mixture layer (34) is not disposed, and a mixture layer disposition part (38) in which the mixture layer (34) is disposed; and if T1 is the heating time of the core body (32) until the lightness index L* of the surface of the mixture layer disposition part (38) and the lightness index ∆L* of the surface of the mixture layer disposition part (38) at the time when the surface of the core body (32) is heated at 200°C satisfy the relational expression ∆L* / L* > 1.1, and T2 is the heating time of the core body (32) until the lightness index L* of the surface of the exposed part (36) and the lightness index ∆L* of the surface of the exposed part (36) at the time when the surface of the core body (32) is heated at 200°C satisfy the relational expression ∆L* / L* > 1.1, the core body (32) satisfies the relational expression T2 > T1.
Need to check novelty before this filing date? Find Prior Art

Description

Secondary battery electrode and secondary battery

[0001] The present disclosure relates to an electrode for a secondary battery and a secondary battery.

[0002] Secondary batteries such as lithium-ion secondary batteries are used as power sources for a wide range of devices, including electric vehicles. A secondary battery is configured, for example, by encapsulating an electrode assembly including a positive electrode and a negative electrode together with an electrolyte solution in an outer can or the like. The electrodes (positive electrode and negative electrode) for secondary batteries have a core and a composite layer disposed on the core.

[0003] The surface of a core constituting a secondary battery electrode may react with ambient oxygen during long-term storage at room temperature or heat treatment during manufacturing, resulting in the formation of an oxide film and discoloration. Surface discoloration due to the formation of an oxide film may cause an increase in the resistance of the core, which may in turn lead to an increase in the resistance of the battery. Therefore, to prevent discoloration, the core is usually used with its surface subjected to an anti-rust treatment.

[0004] For example, Patent Document 1 discloses an electrode for a lithium secondary battery in which a composite layer is formed on a core body, and the core body is a metal foil whose surface has been treated for rust prevention with a chromium-containing layer.

[0005] Japanese Patent Application Laid-Open No. 2002-319407

[0006] In electrodes for secondary batteries, the composite layer is formed on a core whose surface has been treated with an anti-rust coating. For example, if the amount of anti-rust layer formed on the core surface is large, the interface condition between the core surface and the composite layer may change, which may lead to an increase in battery resistance.

[0007] Therefore, an object of the present disclosure is to provide an electrode for a secondary battery and a secondary battery that can suppress an increase in battery resistance.

[0008] The present disclosure relates to an electrode for a secondary battery comprising a core body and a composite layer disposed on the core body, wherein the core body has an exposed portion where the composite layer is not disposed and a composite layer disposed portion where the composite layer is disposed, and the core body is characterized in that, when T1 is the heating time of the core body until the lightness index L* of the surface of the composite layer disposed portion and the lightness index ΔL* of the surface of the composite layer disposed portion when the core body surface is heated at 200°C satisfy the relationship ΔL* / L* > 1.1, and T2 is the heating time of the core body until the lightness index L* of the surface of the exposed portion and the lightness index ΔL* of the surface of the exposed portion when the core body surface is heated at 200°C satisfy the relationship ΔL* / L* > 1.1,

[0009] The present disclosure also provides a secondary battery having a positive electrode and a negative electrode, wherein at least one of the positive electrode and the negative electrode is an electrode for the secondary battery.

[0010] According to the present disclosure, it is possible to provide a secondary battery electrode and a secondary battery that can suppress an increase in battery resistance.

[0011] 2 is a schematic cross-sectional view of a secondary battery according to an embodiment of the present invention, a schematic plan view showing an example of the configuration of an electrode for a secondary battery, and a schematic cross-sectional view of the electrode for a secondary battery taken along line AA in FIG.

[0012] An example of an embodiment of a secondary battery according to the present disclosure will be described in detail below.

[0013] FIG. 1 is a cross-sectional view of a secondary battery according to an embodiment. The secondary battery 10 shown in FIG. 1 includes a wound electrode assembly 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, an electrolyte, insulating plates 18 and 19 disposed above and below the electrode assembly 14, respectively, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a cylindrical case body 16 with a bottom and a sealing body 17 that closes the opening of the case body 16. Note that, instead of the wound electrode assembly 14, other electrode bodies may be used, such as a laminated electrode body formed by alternately stacking positive and negative electrodes with separators interposed therebetween. Examples of the battery case 15 include a cylindrical, rectangular, coin-shaped, or button-shaped metal case, and a resin case formed by laminating a resin sheet (a so-called laminate type).

[0014] The electrolyte has, for example, ion conductivity (for example, lithium ion conductivity). The electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.

[0015] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. Examples of the non-aqueous solvent include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents of these. The non-aqueous solvent may contain a halogen-substituted compound (e.g., fluoroethylene carbonate) in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. Examples of the electrolyte salt include LiPF 6 Lithium salts such as

[0016] Furthermore, examples of the solid electrolyte that can be used include solid or gel-like polymer electrolytes, inorganic solid electrolytes, and the like. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. For example, a polymer material that absorbs a non-aqueous solvent and gels is used as the matrix polymer. Examples of the polymer material include fluororesin, acrylic resin, and polyether resin. For example, the inorganic solid electrolyte can be a material known in all-solid-state lithium ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halogen-based solid electrolytes, and the like). While the above-exemplified electrolytes are non-aqueous electrolytes, the electrolyte is not limited to non-aqueous electrolytes and may be an aqueous electrolyte.

[0017] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 22, which is a portion of the side surface that protrudes inward and supports the sealing body 17. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.

[0018] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and all components except for the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. If the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 may deform and rupture, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure further increases, the upper valve body 26 may rupture, and gas may be discharged from the opening of the cap 27.

[0019] In the secondary battery 10 shown in Fig. 1, a positive electrode lead 20 attached to the positive electrode 11 passes through a through-hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom side of the case body 16. The positive electrode lead 20 is connected by welding or the like to the underside of a filter 23, which is the bottom plate of the sealing body 17, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected by welding or the like to the inner bottom surface of the case body 16, and the case body 16 serves as the negative electrode terminal.

[0020] The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of porous sheets include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator include olefin-based resins such as polyethylene and polypropylene, and cellulose. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin-based resin. Alternatively, the separator 13 may be a multilayer separator including a polyethylene layer and a polypropylene layer, and the surface of the separator 13 may be coated with a material such as an aramid-based resin or ceramic.

[0021] The following describes electrodes for secondary batteries that are applied to at least one of the positive electrode 11 and the negative electrode 12. The following electrodes for secondary batteries are preferably applied to the negative electrode.

[0022] Fig. 2 is a schematic plan view showing an example of the configuration of a secondary battery electrode, and Fig. 3 is a schematic cross-sectional view of the secondary battery electrode taken along line A-A in Fig. 2. The secondary battery electrode 30 shown in Fig. 2 and Fig. 3 is in a state before being wound.

[0023] The longitudinal direction (the direction of arrow X) of the secondary battery electrode 30 shown in Figure 2 is the winding direction of the electrode body 14, and the lateral direction (the direction of arrow Y, the width direction of the secondary battery electrode 30) of the secondary battery electrode 30 is the winding axis direction of the electrode body 14.

[0024] 2 and 3, the secondary battery electrode 30 includes a strip-shaped core body 32 and a composite layer 34 disposed on the strip-shaped core body 32. The composite layer 34 may be provided on both sides of the core body 32, as shown in FIG. 3, or may be provided on one side of the core body 32.

[0025] As shown in FIG. 3 , the core 32 has an exposed portion 36 where the composite layer 34 is not disposed and a composite layer disposition portion 38 where the composite layer 34 is disposed. In FIG. 2 , the exposed portion 36 is formed around the entire end of the core 32 so as to surround the periphery of the composite layer 34 (i.e., so as to surround the periphery of the composite layer disposition portion 38 of the core 32). However, the position of the exposed portion 36 on the core 32 is not limited to the above and can be appropriately set depending on the design of the electrode. For example, the exposed portion 36 may be formed at one end or both ends of the longitudinal direction of the core 32, at one end or both ends of the lateral direction of the core 32, at the center of the core 32, or at a position on the core 32 other than those illustrated above.

[0026] The core 32 satisfies the relationship T2 > T1, where T1 is the heating time of the core 32 until the lightness index L* of the surface of the composite layer placement portion 38 and the lightness index ΔL* of the surface of the composite layer placement portion 38 when the surface of the core 32 is heated at 200°C satisfy the relationship ΔL* / L* > 1.1, and T2 is the heating time of the core 32 until the lightness index L* of the surface of the exposed portion 36 and the lightness index ΔL* of the surface of the exposed portion 36 when the surface of the core 32 is heated at 200°C satisfy the relationship ΔL* / L* > 1.1. Furthermore, by using a core 32 that satisfies the relationship T2 > T1, an increase in battery resistance can be suppressed. The lightness indices L* and ΔL* are measured as follows.

[0027] (Method of measuring brightness index) From the core from which the composite layer has been peeled, the core of the exposed portion and the core of the composite layer placement portion are cut out, and each is used as a test piece. The brightness index is measured in five locations on the surface of the exposed portion of the test piece and five locations on the surface of the composite layer placement portion of the test piece using a colorimeter (CM-2500d) manufactured by Konica Minolta, Inc., according to the CIE1976 L*a*b* color space, and the respective average values ​​are calculated, and these average values ​​are used as the brightness index L* of the exposed portion surface and the brightness index L* of the composite layer placement portion surface.

[0028] The conditions for measuring the brightness index using a colorimeter are as follows: Colorimeter: CM-2500d manufactured by Konica Minolta Light source: Xenon lamp Light receiving element: Dual 40-element silicon photodiode array Measurement diameter: φ8 mm Measurement: 10° field of view Regular reflection processing mode: SCE

[0029] Next, the core of the exposed portion, which is a test piece, and the core of the composite layer placement portion, which is a test piece, are placed in a constant temperature bath heated to 200° C. The test piece that has been heated for a predetermined time is removed, and measurements are taken in the same manner as above for five locations on the surface of the exposed portion of the test piece and five locations on the surface of the composite layer placement portion of the test piece, and the respective average values ​​are calculated, and these average values ​​are used as the lightness index ΔL* of the exposed portion surface when heated for the predetermined time and the lightness index ΔL* of the composite layer placement portion surface when heated for the predetermined time.

[0030] Here, to determine the heating times T1 and T2 of the core body, for example, a plurality of test pieces are prepared by increasing the heating time in 5-second intervals, such as a test piece heated at 200°C for 5 seconds, a test piece heated for 10 seconds, a test piece heated for 15 seconds, etc., between 5 and 100 seconds, and the lightness index ΔL* of the exposed portion surface and the lightness index ΔL* of the composite layer-positioned portion surface are measured for these test pieces when heated for each time.

[0031] From the measured lightness index L* of the exposed portion surface and the lightness index ΔL* of the exposed portion surface after heating for each time, the heating time T1 of the core until the relationship ΔL* / L* > 1.1 is achieved can be calculated. The lightness index value increases as the heating time of the core increases. For example, if the lightness index ΔL* of the exposed portion surface after heating for 55 seconds at 200°C / the lightness index L* of the exposed portion surface before heating is 1.1 or less, and the lightness index ΔL* of the exposed portion surface after heating for 60 seconds at 200°C / the lightness index L* of the exposed portion surface before heating exceeds 1.1, the heating time T1 of the core until the relationship ΔL* / L* > 1.1 is 60 seconds. Similarly, from the measured lightness index L* of the composite layer-placed portion surface and the lightness index ΔL* of the composite layer-placed portion surface after heating for each time, the heating time T2 of the core until the relationship ΔL* / L* > 1.1 is achieved can be calculated.

[0032] One way to make the time T2 required for the relationship ΔL* / L* > 1.1 to be established on the surface of the exposed portion 36 longer than the time T1 required for the relationship ΔL* / L* > 1.1 to be established on the surface of the composite layer placement portion 38 is to apply a rust-proofing treatment to the surface of the core 32. Specifically, when forming a rust-proofing layer on the surface of the core 32 by rust-proofing, the relationship (T2 > T1) can be satisfied by increasing the amount of the rust-proofing layer on the exposed portion 36 of the core 32 to be greater than the amount of the rust-proofing layer on the composite layer placement portion 38 of the core 32. The amount of the rust-proofing layer refers to the mass of the rust-proofing layer per unit area of ​​the core 32. Because the amount of the rust-proofing layer is high on the exposed portion 36 of the core 32, surface discoloration due to the formation of an oxide film is suppressed. This suppresses an increase in the resistance of the core 32, and ultimately suppresses an increase in battery resistance. Furthermore, because the composite material layer 34 is disposed on the composite material layer disposition portion 38 of the core 32, discoloration of the surface due to the formation of an oxide film is unlikely to occur even if the amount of the anti-corrosion layer attached to the composite material layer disposition portion 38 is small. Furthermore, because the amount of the anti-corrosion layer attached to the composite material layer disposition portion 38 is small, the interface state between the composite material layer disposition portion 38 and the composite material layer 34 is maintained (for example, an increase in the interface resistance between the composite material layer disposition portion 38 and the composite material layer 34 is suppressed). This suppresses an increase in battery resistance.

[0033] The anticorrosive layer covering the surface of the core body 32 preferably includes a chromium-containing layer in order to improve the anticorrosive properties of the surface of the core body 32. The chromium-containing layer can be formed, for example, by chromate treatment. The chromate treatment may be performed by a conventionally known method, such as immersion or electrolytic chromate treatment using a chromate treatment agent. The chromium-containing layer may be, for example, a chromium alloy layer or a chromium oxide layer.

[0034] The anticorrosive layer may also include a zinc alloy-containing layer. It is preferable to form a zinc alloy-containing layer on the surface of the core 32 and then form a chromium-containing layer on the zinc alloy-containing layer. This can improve adhesion between the core 32 and the chromium-containing layer, for example. The zinc alloy-containing layer can be formed by electroplating, for example. The zinc alloy is preferably an alloy of zinc and at least one metal selected from nickel, cobalt, copper, and tin.

[0035] The anticorrosive layer may also include a silane coupling agent-containing layer. The silane coupling agent-containing layer is preferably formed on the chromium-containing layer in order to improve adhesion between the anticorrosive layer and the composite layer 34. The silane coupling agent may be a conventionally known material.

[0036] The heating time T2 of the core body 32 until the relationship ΔL* / L* > 1.1 is reached on the surface of the exposed portion 36 is preferably 50 seconds or more, for example, in order to further suppress an increase in battery resistance. The upper limit of the time T2 is not particularly limited, but is preferably 80 seconds or less, for example. Furthermore, the heating time T1 of the core body 32 until the relationship ΔL* is reached on the surface of the composite layer placement portion 38 is preferably 45 seconds or less, for example, in order to further suppress an increase in battery resistance. The lower limit of the time T1 is not particularly limited, but is preferably 15 seconds or more, for example.

[0037] The brightness index L* of the surface of exposed portion 36 is preferably 60 or more and 80 or less, for example, in terms of being able to further suppress an increase in battery resistance. Also, the brightness index L* of the surface of composite layer arrangement portion 38 is preferably 70 or more and 80 or less, for example, in terms of being able to further suppress an increase in battery resistance.

[0038] When the secondary battery electrode 30 is applied to the negative electrode 12, the negative electrode core corresponding to the core 32 can be, for example, a foil of a metal that is stable in the potential range of the negative electrode 12, or a film with such a metal disposed on its surface. Examples of metals that are stable in the potential range of the negative electrode 12 include copper. When the secondary battery electrode 30 is applied to the positive electrode 11, the positive electrode core corresponding to the core 32 can be, for example, a foil of a metal that is stable in the potential range of the positive electrode 11, or a film with such a metal disposed on its surface. Examples of metals that are stable in the potential range of the positive electrode 11 include aluminum.

[0039] The composite layer 34 includes, for example, an active material, a binder, a conductive material, etc. When the secondary battery electrode 30 is applied to the negative electrode 12, the negative electrode composite layer corresponding to the composite layer 34 includes, for example, a negative electrode active material. Examples of the negative electrode active material include materials that can reversibly absorb and release lithium ions, such as carbon materials such as natural graphite and artificial graphite, metals such as Si and Sn, alloys, or oxides. When the secondary battery electrode 30 is applied to the positive electrode 11, the positive electrode composite layer corresponding to the composite layer 34 includes, for example, a positive electrode active material. Examples of the positive electrode active material include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. Examples of the lithium transition metal oxides include, for example, Li x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co y Ni 1-y O 2 , Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn 2 O 4 , Li x Mn 2-y M y O 4 , LiMPO 4 , Li 2 MPO 4F (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, 0<x≦1.2, 0<y≦0.9, 2.0≦z≦2.3). These may be used alone or in combination.

[0040] Examples of binders contained in the composite layer 34 include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), and polyethylene oxide (PEO).

[0041] Examples of the conductive material contained in the composite layer 34 include carbon materials such as carbon black (CB), acetylene black (AB), ketjen black, carbon nanotubes (CNT), graphene, and graphite.

[0042] The composite layer 34 is formed by applying a composite slurry containing an active material, a binder, a conductive material, etc. onto the core 32 and compressing the applied mixture. The exposed portion 36 of the core 32 may be formed by forming the composite layer 34 on the core 32 and then removing a portion of the composite layer 34 to expose a portion of the core 32, or by intermittently applying the composite slurry onto the core 32 to expose a portion of the core 32.

[0043] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0044] <Example> [Preparation of Positive Electrode] 100 parts by mass of LiCoO 2 A positive electrode composite slurry was prepared by mixing 1 part by mass of acetylene black (AB) and 0.9 parts by mass of polyvinylidene fluoride (PVDF), and adding an appropriate amount of N-methyl-2-pyrrolidone (NMP). The positive electrode composite slurry was then applied to both sides of a strip of aluminum foil having a thickness of 15 μm. The coating was then dried and rolled using a roller to obtain a positive electrode.

[0045] [Fabrication of Negative Electrode] A first chromate treatment was performed on the surface of a strip-shaped copper foil with a thickness of 8 μm, forming a chromium-containing layer on the entire surface of the copper foil. Then, as shown in FIG. 2 , the entire periphery of the edge of the copper foil was defined as an exposed portion, and the area surrounded by this exposed portion was defined as a composite layer placement portion. This composite layer placement portion was masked, and a second chromate treatment was performed to form an additional chromium-containing layer on the surface of the exposed portion. The deposition amount of the chromium-containing layer on the composite layer placement portion was 18 μg / dm 2 The deposition amount of the chromium-containing layer on the exposed portion was 52 μg / dm 2 It was.

[0046] The lightness index of the chromate-treated copper foil was measured using the method described above. As a result, the heating time T1 of the copper foil until the relationship ΔL* / L* > 1.1 was reached on the surface of the copper foil that would become the composite layer, was 45 seconds, and the heating time T2 of the copper foil until the relationship ΔL* / L* > 1.1 was reached on the surface that would become the exposed portion of the copper foil, was 60 seconds, satisfying the relationship T2 > T1.

[0047] 100 parts by mass of graphite powder, 1 part by mass of sodium carboxymethyl cellulose (CMC-Na), and 1 part by mass of a dispersion of styrene butadiene rubber (SBR) were mixed, and an appropriate amount of water was added to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied to the composite layer placement areas on both sides of the chromate-treated copper foil, and the coating was dried. The coating was then rolled using a roller to obtain a negative electrode. The obtained negative electrode was heated at 200°C for 45 seconds. The same applies to Comparative Examples 1 and 2 below.

[0048] [Preparation of Non-Aqueous Electrolyte] 5 parts by mass of vinylene carbonate (VC) was added to 100 parts by mass of a mixed solvent in which ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:7, and lithium hexafluorophosphate (LiPF 6 ) was dissolved in a concentration of 1.5 mol / L to prepare a non-aqueous electrolyte solution.

[0049] [Preparation of Secondary Battery] A positive electrode lead was attached to the positive electrode, and a negative electrode lead was attached to the negative electrode. The positive and negative electrodes were then wound with a separator interposed therebetween to prepare a wound electrode body. Insulating plates were placed above and below the electrode body, and the electrode body was housed in a case body. The negative electrode lead was welded to the bottom of the case body, and the positive electrode lead was welded to a sealing member. After injecting a nonaqueous electrolyte into the case body, the opening of the case body was sealed with a sealing member via a gasket to prepare a secondary battery.

[0050] Comparative Example 1 The surface of a strip-shaped copper foil having a thickness of 8 μm was subjected to a chromate treatment to form a chromium-containing layer on the entire surface of the copper foil. The deposition amount of the chromium-containing layer on the exposed portion and the composite layer-disposed portion was 18 μg / dm 2 A secondary battery was fabricated in the same manner as in the Examples, except that this chromate-treated copper foil was used. As a result of measuring the lightness index of the copper foil in the same manner as in the Examples, it was found that the heating time T1 of the copper foil until the relationship ΔL* / L* > 1.1 was reached on the composite layer-disposed surface of the copper foil was 45 seconds, and the heating time T2 of the copper foil until the relationship ΔL* / L* > 1.1 was reached on the exposed portion surface of the copper foil was 45 seconds.

[0051] Comparative Example 2: The surface of a strip-shaped copper foil having a thickness of 8 μm was subjected to chromate treatment for a longer time than in Comparative Example 1, and a chromium-containing layer was formed on the entire surface of the copper foil. The deposition amount of the chromium-containing layer on the exposed portion and the composite layer-disposed portion was 52 μg / dm 2 A secondary battery was fabricated in the same manner as in the Examples, except that this chromate-treated copper foil was used. As a result of measuring the lightness index of the copper foil in the same manner as in the Examples, it was found that the heating time T1 of the copper foil until the relationship ΔL* / L* > 1.1 was reached on the composite layer-arranged surface of the copper foil was 60 seconds, and the heating time T2 of the copper foil until the relationship ΔL* / L* > 1.1 was reached on the exposed portion surface of the copper foil was 60 seconds.

[0052] [DCIR Measurement] In a temperature environment of 25°C, the secondary batteries of the example and comparative example were charged at a constant current of 0.3 It until the voltage reached 4.1 V, and then at a constant voltage of 4.1 V until the current reached 0.05 It. Subsequently, the secondary batteries were discharged at a constant current of 0.3 It for 100 minutes to bring the state of charge (i.e., SOC) to 50%. Next, voltage data was obtained when the secondary batteries with an SOC of 50% were discharged for 10 seconds at current values ​​of 0 A, 0.1 A, 0.5 A, and 1.0 A. The DC resistance (DCIR) was calculated from the absolute value of the slope when the relationship between the applied discharge current value and the voltage value after 10 seconds was approximated to a straight line using the least squares method. The results are summarized in Table 1. In Table 1, the DCIR of the example is used as the reference (100%), and the DCIR of the other comparative examples is expressed relative to it.

[0053]

[0054] The example showed a lower DCIR than comparative example 2. From these results, it can be said that, when T1 is the heating time of the core until the lightness index L* of the composite layer placement portion surface and the lightness index ΔL* of the composite layer placement portion surface when the core surface is heated at 200°C satisfy the relationship ΔL* / L* > 1.1, and T2 is the heating time of the core until the lightness index L* of the exposed portion surface and the lightness index ΔL* of the exposed portion surface when the core surface is heated at 200°C satisfy the relationship ΔL* / L* > 1.1, by using a core that satisfies the relationship T2 > T1, it can be said that an increase in battery resistance can be suppressed.

[0055] [Notes] (1) A secondary battery electrode comprising a core and a composite layer disposed on the core, wherein the core has an exposed portion where the composite layer is not disposed and a composite layer-disposed portion where the composite layer is disposed, and the core satisfies the relationship T2 > T1, where T1 is the heating time of the core until the lightness index L* of the composite layer-disposed portion surface and the lightness index ΔL* of the composite layer-disposed portion surface when the core surface is heated at 200°C satisfy the relationship ΔL* / L* > 1.1, and T2 is the heating time of the core until the lightness index L* of the exposed portion surface and the lightness index ΔL* of the exposed portion surface when the core surface is heated at 200°C satisfy the relationship ΔL* / L* > 1.1. (2) The secondary battery electrode according to (1) above, wherein the surface of the core is covered with an anticorrosive layer including a chromium-containing layer. (3) The electrode for a secondary battery according to (1) or (2) above, wherein the lightness index L* of the surface of the exposed portion is 60 or more and 80 or less. (4) The electrode for a secondary battery according to any one of (1) to (3) above, wherein the core contains copper. (5) A secondary battery having a positive electrode and a negative electrode, wherein at least one of the positive electrode and the negative electrode is the electrode for a secondary battery according to any one of (1) to (4) above.

[0056] 10 Secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 15 Battery case, 16 Case body, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Protruding portion, 23 Filter, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket, 30 Secondary battery electrode, 32 Core body, 34 Composite layer, 36 Exposed portion, 38 Composite layer placement portion.

Claims

1. An electrode for a secondary battery comprising a core body and a composite layer disposed on the core body, wherein the core body has an exposed portion on which the composite layer is not disposed and a composite layer disposed portion on which the composite layer is disposed, and the core body satisfies the relationship T2>T1, where T1 is the heating time of the core body until the lightness index L* of the composite layer disposed portion surface and the lightness index ΔL* of the composite layer disposed portion surface when the core body surface is heated at 200°C satisfy the relationship ΔL* / L*>1.1, and T2 is the heating time of the core body until the lightness index L* of the exposed portion surface and the lightness index ΔL* of the exposed portion surface when the core body surface is heated at 200°C satisfy the relationship ΔL* / L*>1.

1.

2. The secondary battery electrode according to claim 1, wherein the surface of the core body is covered with an anticorrosive layer including a chromium-containing layer.

3. The electrode for a secondary battery according to claim 1 or 2, wherein the lightness index L* of the surface of the exposed portion is 60 or more and 80 or less.

4. The secondary battery electrode according to claim 1 or 2, wherein the core body contains copper.

5. A secondary battery having a positive electrode and a negative electrode, wherein at least one of the positive electrode and the negative electrode is an electrode for a secondary battery according to claim 1 or 2.

Citation Information

Patent Citations

  • Secondary battery, and method of manufacturing the same

    JP2013246903A

  • Nonaqueous electrolyte secondary battery, and method of manufacturing the same

    JP2013251048A

  • Battery manufacturing method and battery

    JP2014035958A

  • Manufacturing method of nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

    JP2019169413A