Non-aqueous electrolyte battery

The non-aqueous electrolyte battery design with a high-absorption-rate second separator protruding from the first separator addresses electrolyte depletion and uneven distribution, improving discharge capacity and reliability by ensuring even electrolyte distribution and reducing short circuit risks.

WO2024225069A1PCT designated stage expired Publication Date: 2024-10-31FDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014761
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-12
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Non-aqueous electrolyte batteries face reduced discharge capacity due to electrolyte depletion around the positive electrode at the end of discharge, leading to uneven electrolyte distribution and potential short circuits.

Method used

A non-aqueous electrolyte battery design featuring a wound body with a first separator and a second separator having a higher liquid absorption speed, where the second separator protrudes outward from the first separator, is used to mitigate electrolyte depletion and ensure even electrolyte distribution, with the second separator positioned closer to the positive electrode and made of nonwoven fabric, while the first separator is a microporous film.

Benefits of technology

This configuration enhances the discharge capacity and reliability of the battery by reducing electrolyte depletion and uneven distribution, minimizing the risk of short circuits, especially during high-current discharge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014761_31102024_PF_FP_ABST
    Figure JP2024014761_31102024_PF_FP_ABST
Patent Text Reader

Abstract

This non-aqueous electrolyte battery includes: a wound body wound in a state in which a negative electrode and a positive electrode are laminated with a separator therebetween; and an outer can for housing the wound body. The separator includes a first separator and a second separator having a liquid absorption speed higher than that of the first separator, wherein the second separator protrudes to the outside of the first separator at least at one end in the axial direction of the wound body.
Need to check novelty before this filing date? Find Prior Art

Description

non-aqueous electrolyte battery

[0001] The present invention relates to a non-aqueous electrolyte battery.

[0002] Non-aqueous electrolyte batteries such as lithium primary batteries and lithium ion secondary batteries have high energy densities and are therefore used in many electronic devices. For example, lithium primary batteries have an extremely long shelf life and can be stored for a long period of 10 years or more at room temperature, so they are widely used as the main power source and memory backup power source for various meters.

[0003] Known examples of such non-aqueous electrolyte batteries include batteries having a structure (spiral structure) in which a negative electrode and a positive electrode are stacked and wound with a separator interposed therebetween. Because the opposing surface area of ​​the positive and negative electrodes in such batteries is large, they are often used in applications where output characteristics are important, i.e., applications requiring large currents.

[0004] On the other hand, such batteries are also required to have improved reliability. For example, in lithium primary batteries, a microporous film made of polyethylene or polypropylene is generally used as the separator. Here, if the battery is subjected to, for example, excessive impact, the microporous film may move, causing a short circuit. Also, a short circuit may occur when dendrites or active material break through the separator. There is a demand for suppressing battery fires and explosions caused by these and improving reliability.

[0005] In contrast, Patent Document 1 discloses a cylindrical nonaqueous electrolyte battery including a wound body in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound together, in which the separator includes a microporous film and a nonwoven fabric, and the nonwoven fabric is arranged so as to be in contact with the negative electrode.

[0006] Japanese Patent Application Laid-Open No. 2006-139918

[0007] In the battery described above, the inclusion of a microporous film and a nonwoven fabric makes it less susceptible to short circuits than a battery containing only a microporous film, thereby improving reliability to a certain extent. However, when the battery is discharged at a large current, the electrolyte may be depleted around the positive electrode at the end of the discharge. This may result in uneven distribution of the electrolyte around the positive electrode, resulting in a decrease in discharge capacity.

[0008] The present invention has been made in view of the above circumstances, and has as its object to provide a nonaqueous electrolyte battery in which the decrease in discharge capacity due to the depletion of electrolyte around the positive electrode at the end of discharge is small.

[0009] [1] A nonaqueous electrolyte battery including: a wound body in which a positive electrode and a negative electrode are wound in a stacked state with a separator interposed therebetween; and an outer can housing the wound body, wherein the separator includes a first separator and a second separator stacked on the first separator and having a higher electrolyte absorption rate than the first separator, wherein the second separator protrudes outward from the first separator at at least one axial end of the wound body. [2] The nonaqueous electrolyte battery according to [1], wherein the width of the second separator in a direction perpendicular to the winding direction is greater than the width of the first separator in the direction perpendicular to the winding direction. [3] The nonaqueous electrolyte battery according to [1] or [2], wherein the second separator is disposed closer to the positive electrode than the first separator. [4] The nonaqueous electrolyte battery according to any one of [1] to [3], wherein the first separator and the second separator are resin separators, and the melting point of the second separator is higher than the melting point of the first separator. [5] The nonaqueous electrolyte battery according to any one of [1] to [4], wherein the second separator is a nonwoven fabric, and the first separator is a microporous film. [6] The nonaqueous electrolyte battery according to any one of [1] to [5], wherein the negative electrode contains lithium metal or a lithium alloy.

[0010] According to the present invention, it is possible to provide a nonaqueous electrolyte battery in which the decrease in discharge capacity due to the depletion of electrolyte around the positive electrode at the end of discharge is small.

[0011] Fig. 1 is a schematic cross-sectional view showing a nonaqueous electrolyte battery according to one embodiment of the present invention. Fig. 2 is an enlarged view of the wound body and its surrounding essential parts shown in Fig. 1. Figs. 3A to 3C are schematic partial cross-sectional views showing how the end of the separator is folded and formed. Fig. 4 is an enlarged view of the wound body and its surrounding essential parts according to a modified example.

[0012] As described above, depletion of the electrolyte around the positive electrode at the end of discharge, specifically depletion of the electrolyte in the separator around the positive electrode, is likely to occur when the expanded positive electrode absorbs the electrolyte in the separator during high-current discharge. When this depletion of the electrolyte in the separator occurs, the distribution of the electrolyte in the separator is likely to become uneven, and the discharge capacity is likely to decrease.

[0013] In response to this, two or more separators with different liquid absorption rates are placed between the positive electrode and the negative electrode, and the second separator with a higher liquid absorption rate protrudes beyond the first separator with a lower liquid absorption rate at at least one axial end of the wound body. This allows the second separator to more easily absorb the electrolyte in the outer can, thereby reducing depletion of the electrolyte in the separators and reducing uneven distribution of the electrolyte even at the end of discharge. The configuration of the nonaqueous electrolyte battery is described in detail below.

[0014] 1. Nonaqueous Electrolyte Battery Hereinafter, a lithium primary battery will be described as an example of the nonaqueous electrolyte battery according to this embodiment.

[0015] Fig. 1 is a schematic cross-sectional view showing a nonaqueous electrolyte battery 1 according to one embodiment of the present invention. Fig. 2 is an enlarged view of the wound body 3 shown in Fig. 1 and the main parts around it.

[0016] As shown in FIG. 1 , the nonaqueous electrolyte battery 1 according to this embodiment includes an outer can 2 , an electrode group (wound body) 3 housed in the outer can 2 , an electrolyte 4 , and a sealing body 5 .

[0017] The outer can 2 is a metal battery case that houses the wound body 3. In this embodiment, the outer can 2 is a cylindrical battery case with an opening and a bottom. The material of the outer can 2 can be iron, stainless steel, or the like.

[0018] The sealing body 5 seals the opening of the outer can 2 and also serves as a positive electrode terminal. The sealing body 5 includes a sealing plate 6, a positive electrode terminal 7, a metal washer 8, and a resin sealing gasket 9.

[0019] In this embodiment, the sealing plate 6 is disk-shaped and has an opening in the center. A metal positive electrode terminal 7 and a metal washer 8 are crimped into the opening of the sealing plate 6 via a resin sealing gasket 9. The edge of the sealing plate 6 and the upper edge of the outer can 2 are laser welded.

[0020] The wound body 3 is an electrode group including a positive electrode 10, a negative electrode 11, and a separator 12, and is housed in the outer can 2. In this embodiment, the wound body 3 is formed by, for example, winding a strip-shaped laminate sheet, in which a separator 12, a positive electrode 10, a separator 12, a negative electrode 11, and a separator 12 are laminated, in the length direction with the negative electrode 11 facing outward. As will be described later, the separator 12 includes a first separator 13 and a second separator 14 (see FIG. 2 ).

[0021] The positive electrode 10 of the wound body 3 is connected to the positive electrode terminal 7 via a positive electrode lead 15. On the other hand, the negative electrode 11 arranged on the outermost surface of the wound body 3 is connected to the inner surface of the outer can 2 via a negative electrode lead 16. As a result, the negative electrode 11 and the outer can 2, which is the negative electrode terminal, are electrically connected to each other.

[0022] The nonaqueous electrolyte battery 1 further includes an upper insulating plate 17 and a lower insulating plate 18. The upper insulating plate 17 is disposed between the wound body 3 and the sealing body 5. The lower insulating plate 18 is disposed between the wound body 3 and the bottom of the outer can 2. This prevents an internal short circuit between the positive electrode 10 and the negative electrode 11.

[0023] The electrolyte solution 4 is sealed in the outer can 2. The electrolyte solution 4 is a solution in which an electrolyte is dissolved in an organic solvent.

[0024] The type of organic solvent is not particularly limited, and examples thereof include cyclic carbonates such as propylene carbonate (PC) and ethylene carbonate (EC), chain carbonates such as dimethyl carbonate (DMC) and diethyl carbonate (DEC), ethers such as 1,2-dimethoxyethane (DME), and lactones such as γ-butyrolactone. These may be used alone or in combination of two or more. For example, from the viewpoint of achieving a better balance between dielectric constant and viscosity, a cyclic carbonate and a chain carbonate may be used in combination.

[0025] The electrolyte is a lithium salt, examples of which include lithium hexafluorophosphate (LiPF 6 ), lithium perchlorate (LiClO 4 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 Among them, from the viewpoint of further improving the safety of the battery, LiCF 3 SO 3 The concentration of the electrolyte in the electrolytic solution 4 is not particularly limited, but may be, for example, 0.1 to 5 mol %, and preferably 0.25 to 3.5 mol %.

[0026] Next, each member constituting the wound body 3 will be described.

[0027] The wound body 3 includes a positive electrode 10 , a negative electrode 11 , and a separator 12 .

[0028] (Positive Electrode 10) The positive electrode 10 includes a positive electrode current collector and a positive electrode mixture layer.

[0029] The material of the positive electrode current collector may be any material that is corrosion-resistant at the positive electrode potential, such as stainless steel or aluminum. Among these, stainless steel (SUS316, SUS444, etc.) is preferred. The shape of the positive electrode current collector is not particularly limited, and may be any of plain woven wire mesh, expanded metal, punched metal, metal foil, etc.

[0030] The positive electrode mixture layer is supported on the positive electrode current collector and contains a positive electrode active material and a conductive agent. The positive electrode active material contains manganese dioxide and may further contain other active materials as needed. Examples of the other active materials include graphite-based active materials such as graphite fluoride, MoO 3 , V 2 O 5 , Mn 2 O 4 Metal oxides such as TiS 2 , and metal sulfides such as MoS.

[0031] Examples of the conductive agent include natural graphite, artificial graphite, carbon black, carbon fiber, etc. The amount of the conductive agent contained in the positive electrode mixture can be, for example, 1 to 10 parts by mass per 100 parts by mass of the positive electrode active material.

[0032] The positive electrode mixture may further contain a binder as needed. Examples of binders include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), and styrene butadiene rubber (SBR). The amount of binder contained in the positive electrode mixture can be, for example, 1 to 10 parts by mass per 100 parts by mass of the positive electrode active material.

[0033] The thickness of the positive electrode 10 when the positive electrode mixture layers are disposed on both sides of the positive electrode current collector may be, for example, 100 to 800 μm, depending on the desired capacity. When the thickness of the positive electrode 10 is 100 μm or more, the discharge capacity is more likely to be increased, and when it is 800 μm or less, the diffusion distance of Li ions in the positive electrode mixture can be more shortened, making it easier to suppress the internal resistance value of the battery.

[0034] (Negative electrode 11) The negative electrode 11 includes a negative electrode active material layer. The negative electrode active material layer may be a sheet (foil) of metallic lithium or a lithium alloy. Examples of lithium alloys include lithium aluminum alloys (Li—Al), lithium magnesium alloys (Li—Mg), lithium tin alloys (Li—Sn), lithium zinc alloys (Li—Zn), lithium antimony alloys (Li—Sn), and lithium silicon alloys (Li—Si, Li—Ni—Si).

[0035] A portion of the sheet-like metallic lithium or lithium alloy may be pulverized. For example, the negative electrode active material layer may include a layer formed by laminating a metal foil (e.g., aluminum foil) that alloys with lithium on a lithium foil and alloying the metal through an electrochemical reaction. The alloying metal is not particularly limited as long as it is an element that alloys with lithium, and examples thereof include magnesium, tin, zinc, silicon, etc.

[0036] The negative electrode 11 may further include a negative electrode current collector supporting a negative electrode active material layer. The material of the negative electrode current collector may be any material that is corrosion-resistant at the negative electrode potential, such as copper, nickel, or stainless steel. The shape of the negative electrode current collector may be the same as that of the positive electrode current collector.

[0037] (Separator 12) The separator 12 is disposed between the positive electrode 10 and the negative electrode 11 to electrically insulate them. The separator 12 includes a first separator 13 and a second separator 14 (see FIG. 2).

[0038] The second separator 14 has a higher liquid absorption rate than the first separator 13. That is, the second separator 14 absorbs the electrolyte faster than the first separator 13. The second separator 14 may be disposed closer to the positive electrode 10 or the negative electrode 11 than the first separator 13. In particular, depletion of the electrolyte in the separator at the end of discharge is likely to occur when the expanded positive electrode 10 absorbs the electrolyte in the separator due to high-current discharge. Therefore, as in this embodiment, it is preferable that the second separator 14, which has a higher liquid absorption rate, be disposed closer to the positive electrode 10 (see FIG. 2 ). The liquid absorption rate of the separator can be measured according to JIS L 1907 / Byreck method using a mixed solvent of PC / EC / DME = 10 / 10 / 80 (mass ratio) instead of water.

[0039] The liquid absorption rate of the separator can be adjusted by the microstructure, average pore size, material, etc. For example, separators with a microstructure that is prone to capillary action, such as nonwoven fabrics, and separators made of materials that have affinity for the electrolyte solution tend to have a high liquid absorption rate.

[0040] The difference in the liquid absorption rate between the second separator 14 and the first separator 13 is not particularly limited, but may be, for example, 0.5 cm / 10 min or more. The larger the difference in the liquid absorption rate, the easier it is for the second separator 14 to absorb the electrolyte solution in the outer can 2 by protruding.

[0041] At at least one end in the axial direction of the wound body 3 (X direction in FIG. 1 ), the second separator 14 protrudes outward from the first separator 13 (see FIG. 2 ). That is, at least one end in the axial direction of the wound body 3, the end of the second separator 14 is located outward in the axial direction from the end of the first separator 13. In this embodiment, at one end in the axial direction of the wound body 3 (the can bottom side in FIG. 1 ), the second separator 14 protrudes outward from the first separator 13.

[0042] The amount L of protrusion of the second separator 14 from the first separator 13 in the axial direction of the wound body 3 may be any amount, from the viewpoint of further suppressing poor electrolyte supply caused by compartmentalizing the electrode (positive electrode 10 in this embodiment) by the first separator 13 when folding and forming the separator end. The upper limit of the amount L of protrusion of the second separator 14 is not particularly limited, but from the viewpoint of minimizing a decrease in the electrode packing efficiency, it is preferably 10 times the thickness of the electrode, more preferably 5.0 mm or less. The amount L of protrusion depends on the battery size, but can be, for example, 0.1 mm or more and 5.0 mm or less, more preferably 0.5 mm or more and 4.0 mm or less.

[0043] The widths of the first separator 13 and the second separator 14 may be the same or different. The width of the separator refers to the length in a direction perpendicular to the winding direction (lengthwise direction) of the separator, and refers to the length between one end and the other end of the separator in the axial direction. For example, the first separator 13 and the second separator 14 of the same width may be stacked with a mutual offset, or the first separator 13 may be stacked with the second separator 14 having a larger width. From the viewpoint of improving reliability and liquid absorption, it is preferable that the width of the second separator 14 be larger than the width of the first separator 13, as in this embodiment.

[0044] The first separator 13 and the second separator 14 are each made of resin, and may have the same or different melting points. As will be described later, from the viewpoint of preventing isolation of the electrode (positive electrode 10 in this embodiment) due to welding of the second separator 14 on the inner side of the winding to the second separator 14 on the outer side of the winding when the axial ends of the first separator 13 and the second separator 14 are thermoformed, and further suppressing uneven distribution of the electrolyte, it is preferable that the melting point of the second separator 14 be higher than the melting point of the first separator 13.

[0045] The difference in melting point between the second separator 14 and the first separator 13 is preferably, for example, 20° C. or more. The greater the difference in melting point, the less likely the second separator 14 on the inner side of the winding and the second separator 14 on the outer side of the winding will be welded together when the axial ends of the first separator 13 and the second separator 14 are thermoformed, making it easier to ensure a gap for taking in the electrolyte.

[0046] The melting point of the separator can be measured by differential scanning calorimetry (DSC) as the minimum temperature of the endothermic peak when the temperature is raised from room temperature to 200° C. at a rate of 10° C. / min.

[0047] (First separator 13) The first separator 13 may be a microporous film or a nonwoven fabric. In this embodiment, the first separator 13 is preferably a microporous film. The material of the microporous film is not particularly limited, but examples include olefin resins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, and thermoplastic resins such as polyphenylene sulfide and cellulose. The microporous film may contain inorganic particles as needed.

[0048] The liquid absorption rate of the first separator 13 is not particularly limited, but may be, for example, 0.05 cm / 10 minutes or more and less than 0.2 cm / 10 minutes.

[0049] The melting point of the first separator 13 is preferably lower than the melting point of the second separator 14, and more preferably within the range of 120±25°C (95 to 145°C). This makes it easier to shut down at around 120°C, thereby further improving reliability.

[0050] The thickness of the first separator 13 is not particularly limited, but may be, for example, 10 μm or more and 40 μm or less. When the thickness of the first separator 13 is 10 μm or more, the electrolyte retention can be further improved, and when the thickness is 40 μm or less, the internal resistance of the battery can be further reduced.

[0051] (Second separator 14) The second separator 14 is laminated on the first separator 13. The second separator 14 may be any separator that has a higher liquid absorption rate than the first separator 13, and may be a microporous film or a nonwoven fabric. In particular, the second separator 14 is preferably a nonwoven fabric from the viewpoint of exhibiting high liquid absorption due to capillary action. The material of the nonwoven fabric is not particularly limited, and the same materials as those listed as materials for the microporous film can be used.

[0052] The liquid absorption rate of the second separator 14 is not particularly limited, but is preferably 0.2 cm / 10 min or more, and more preferably 0.5 cm / 10 min or more. The upper limit of the liquid absorption rate of the second separator 14 is not particularly limited, but can be, for example, 5.0 cm / 10 min or less.

[0053] The melting point of the second separator 14 is preferably higher than the melting point of the first separator 13. For example, preferred examples of materials for the second separator 14 include polypropylene. Polypropylene (PP) has a melting point of 125 to 160°C for random copolymers of ethylene and the like (random copolymers) and 160 to 170°C for homopolymers (homopolymers). However, the melting point of the second separator 14 is not limited to polypropylene (PP) and can be within the range of 165±20°C (145 to 185°C).

[0054] The thickness of the second separator 14 is not particularly limited, but from the same viewpoint as the thickness of the first separator 13, it may be, for example, 10 μm or more and 40 μm or less.

[0055] 2. Method for Manufacturing the Non-Aqueous Electrolyte Battery The non-aqueous electrolyte battery can be manufactured by any method. For example, the non-aqueous electrolyte battery can be manufactured through the steps of 1) preparing a wound body 3 and 2) encapsulating the wound body 3 and the electrolyte 4 in an outer can 2 and sealing the opening of the outer can 2.

[0056] Regarding step 1), first, the positive electrode 10 and the negative electrode 11 are prepared.

[0057] The positive electrode 10 can be produced, for example, by the following procedure. First, a positive electrode active material and optional additives (conductive agent and binder) are mixed to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry is applied to or filled on a positive electrode current collector, dried, rolled as necessary, and cut to a predetermined size to obtain the positive electrode 10. A positive electrode lead 15 is welded to one end in the longitudinal direction of the obtained strip-shaped positive electrode 10.

[0058] The negative electrode 11 can be obtained, for example, by cutting a sheet of lithium metal or lithium alloy to a predetermined size. A negative electrode lead 16 is welded to one end of the resulting strip-shaped negative electrode 11 in the longitudinal direction.

[0059] Next, the obtained positive electrode 10 and negative electrode 11 are stacked with a separator 12 interposed therebetween and wound together to prepare a wound body 3 .

[0060] Specifically, first, the separator 12, the positive electrode 10, the separator 12, and the negative electrode 11 are laminated in this order. In this embodiment, the separator 12 is laminated such that the first separator 13 is on the negative electrode 11 side and the second separator 14 is on the positive electrode 10 side. This strip-shaped laminate sheet is then wound in the length direction with the negative electrode 11 on the outside to form the wound body 3. In this embodiment, the width of the second separator 14 is greater than the width of the first separator 13, so that the second separator 14 protrudes outward from the first separator 13 at one axial end of the wound body 3.

[0061] The first separator 13 and the second separator 14 may be pre-welded at a portion of their overlapping portions. This makes it difficult for the first separator 13 and the second separator 14 to shift positions relative to each other even if pressure is applied to the battery due to dropping or crushing when the battery is assembled, thereby further improving the reliability of the battery. The welding method is not particularly limited, and may be either ultrasonic welding or heat welding.

[0062] In addition, from the viewpoint of adjusting the storage height of the wound body 3 when stored in the outer can 2, the separator 12 at at least one end of the wound body 3 in the axial direction may be folded.

[0063] 3A to 3C are schematic partial cross-sectional views showing how the end of the separator 12 is folded and formed. For convenience of explanation, the drawings show only one end of the wound body 3.

[0064] In this embodiment, the ends of the first separator 13 and the second separator 14 in the wound state are heated by applying hot air from the outside (see FIGS. 3A and 3B), thereby folding the ends of the first separator 13 and the second separator 14 inward (see FIG. 3C).

[0065] As described above, the melting point of the second separator 14 is preferably higher than the melting point of the first separator 13. Furthermore, the heating temperature using hot air is preferably lower than the melting point of the second separator 14, for example, a temperature equal to or higher than the melting point of the first separator 13 (e.g., 120°C) and lower than the melting point of the second separator 14. This allows the first separator 13 to be thermoformed while the second separator 14 on the inner side of the winding and the second separator 14 on the outer side of the winding are not welded together, ensuring a gap. This prevents isolation of the electrode (positive electrode 10 in this embodiment) due to welding between the second separator 14 on the inner side of the winding and the second separator 14 on the outer side of the winding, and further prevents uneven distribution of the electrolyte.

[0066] Regarding step 2), the obtained wound body 3 is housed in an outer can 2, and after the electrolyte is poured into it, the opening of the outer can 2 is sealed with a sealing member 5. In this way, the nonaqueous electrolyte battery 1 can be obtained.

[0067] 3. Modifications In the above embodiment, the second separator 14 protrudes outward beyond the first separator 13 at one end of the wound body 3 in the axial direction (the end on the can bottom side), but the present invention is not limited to this.

[0068] 4 is an enlarged view of a wound body and its surroundings according to a modified example. As shown in FIG. 4, the second separator 14 may protrude beyond the first separator 13 at both ends of the wound body 3 in the axial direction. In this case, the amount L of the second separator 14 protruding from the first separator 13 may be the same or different between the ends. For example, the amount L of protrusion on the can bottom side may be greater than the amount L of protrusion on the sealing body 5 side.

[0069] In the above embodiment, the separator 12 is composed of two separators, the first separator 13 and the second separator 14, but the number of separators is not limited to this and may be three or more. In this case, it is preferable that the separator with the highest liquid absorption rate among the three or more separators protrudes outward from the other separators at least one axial end of the wound body 3. The protrusion amount L of the separator with the highest liquid absorption rate relative to the other separators may be the same as above.

[0070] In the above embodiment, the outer can 2 has a cylindrical shape, but the shape is not limited to this and may be rectangular.

[0071] Furthermore, in the above embodiment, a lithium primary battery is shown as an example of a nonaqueous electrolyte battery, but the present invention is not limited to this and may be, for example, a lithium ion secondary battery.

[0072] The present invention will be further described below with reference to examples and comparative examples, but the technical scope of the present invention is not limited thereto.

[0073] 1. Measurement of separator properties Separators shown in Table 1 were prepared.

[0074] The liquid absorption rate and melting point of the separator were measured by the following method.

[0075] [Liquid Absorption Rate] The liquid absorption rate of the separator was measured by the same test as JIS L 1907 / Byreck method, except that a mixed solvent of PC / EC / DME=10 / 10 / 80 (mass ratio) was used instead of water.

[0076] [Melting Point] The melting point of the separator was determined as the temperature of the minimum point of the endothermic peak when the temperature was raised from room temperature to 200°C at a rate of 10°C / min by differential scanning calorimetry (DSC).

[0077] 2. Preparation and Evaluation of Battery Example 1 (1) Preparation of Positive Electrode Electrolytic manganese dioxide as a positive electrode active material, a carbon material (graphite) as a conductive agent, and a fluorine-based binder (PTFE) as a binder were mixed in a mass ratio of 90:5:5 to prepare a positive electrode mixture.

[0078] Next, the prepared positive electrode mixture was filled into a stainless steel wire mesh as a positive electrode current collector, dried, rolled to a thickness of 0.4 mm using a roll press, and cut to the specified dimensions (width 38 mm, length 230 mm) to obtain a positive electrode. The positive electrode mixture was peeled off from a part of the positive electrode to expose the positive electrode current collector, and a positive electrode lead was welded to the exposed part.

[0079] (2) Preparation of negative electrode A lithium aluminum alloy sheet having a thickness of 0.2 mm was cut to a predetermined size (width 36 mm, length 230 mm) and used as a negative electrode. A negative electrode lead was connected to the negative electrode.

[0080] (3) Preparation of Wound Body The prepared positive electrode and negative electrode were wound with a microporous film 1 (first separator, width 40 mm) shown in Table 1 and a nonwoven fabric 2 (second separator, width 42 mm) shown in Table 1 interposed therebetween. Specifically, the microporous film 1 was on the negative electrode side and the nonwoven fabric 2 was on the positive electrode side, and the resulting laminate was wound in the order of microporous film 1 / nonwoven fabric 2 / positive electrode / nonwoven fabric 2 / microporous film 1 / negative electrode. This resulted in a wound body in which the positive electrode and negative electrode were stacked with the separator interposed between them, with the negative electrode disposed on the outermost surface. At one end of the obtained wound body in the axial direction, the nonwoven fabric 2 protruded 2 mm outward from the microporous film 1.

[0081] One end of the roll in the axial direction was heated to 120° C. by externally applying hot air, and the end of the microporous film 1 and the end of the nonwoven fabric 2 were folded inward of the roll.

[0082] (4) Preparation of Electrolyte Solution Propylene carbonate (PC), ethylene carbonate (EC), and 1,2-dimethoxyethane (DME) were mixed in a mass ratio of 10:10:80, and a predetermined amount of additive was further added to obtain a base solution. LiCF4 was added as a non-aqueous electrolyte to this base solution. 3 SO 3 was added to give a concentration of 0.5 mol / L to obtain an electrolyte solution.

[0083] (5) Assembly of Battery Next, a ring-shaped lower insulating plate was placed at the bottom of a bottomed cylindrical outer can, and then the prepared wound body was housed in the outer can so that the one end (the side from which the nonwoven fabric 2 protruded) faced the can bottom. Then, the positive electrode lead was welded to the underside of the positive electrode terminal, and the negative electrode lead of the negative electrode was welded to the inner surface of the outer can.

[0084] The electrolyte solution prepared above was poured into the outer can, an upper insulating plate was placed on the wound body, and the opening of the outer can was sealed with a sealing plate, thereby obtaining a cylindrical lithium primary battery of 17450 size as shown in FIG.

[0085] Example 2 A cylindrical lithium primary battery was obtained in the same manner as in Example 1, except that in the preparation of the wound body (3) above, before winding, a microporous film 1 (first separator, width 40 mm) and a nonwoven fabric 2 (second separator, width 42 mm) were overlapped and both widthwise ends of the overlapping portion were ultrasonically welded.

[0086] Example 3 A cylindrical lithium primary battery was obtained in the same manner as in Example 1, except that in the preparation of the wound body (3), the microporous film 1 (first separator, width 40 mm) was placed on the positive electrode side and the nonwoven fabric 2 (second separator, width 42 mm) was placed on the negative electrode side.

[0087] Comparative Example 1 A cylindrical lithium primary battery was obtained in the same manner as in Example 1, except that in the preparation of the above (3) wound body, only nonwoven fabric 2 (second separator, width 42 mm) was used and microporous film 1 (first separator, width 40 mm) was not used.

[0088] Comparative Example 2 A cylindrical lithium primary battery was obtained in the same manner as in Example 1, except that in the preparation of the above (3) wound body, only microporous film 1 (first separator, width 40 mm) was used, and nonwoven fabric 2 (second separator, width 42 mm) was not used.

[0089] Comparative Example 3 A cylindrical lithium primary battery was obtained in the same manner as in Example 1, except that in the preparation of the wound body (3) above, the layers were laminated in the order of nonwoven fabric 1 / microporous film 2 / positive electrode / microporous film 2 / nonwoven fabric 1 / negative electrode, and the laminate was wound so that microporous film 2 (first separator, width 42 mm) was on the positive electrode side and nonwoven fabric 1 (second separator, width 40 mm) was on the negative electrode side. In the wound body of the obtained battery, the microporous film 2 protruded outward by 2 mm from the nonwoven fabric 1 at one axial end.

[0090] [Evaluation] (1) Discharge Test (Pre-Discharge, Aging) The sealed battery was pre-discharged at a constant current for a specified time, and then aged at 70° C. for 6 hours.

[0091] (Discharge) A load of 560 Ω was applied to the obtained battery, and the discharge capacity was measured until the battery voltage reached 2.0 V. Note that the number of batteries was 5, and the average value was taken as the discharge capacity.

[0092] (2) Impact Test (Free Fall Test) In accordance with IEC 60086: Test J, the obtained cylindrical battery was dropped so that its height direction was perpendicular to the ground, and the number of times until the battery voltage decreased was counted.

[0093] (3) Absorption When a predetermined amount of electrolyte was injected during the production of the battery, the time required for the injection (the time until the injected electrolyte was absorbed by the wound body and the electrolyte surface became invisible) was measured.

[0094] The evaluation results of the batteries of Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Table 2.

[0095]

[0096] As shown in Table 2, the batteries of Comparative Examples 1 and 2, which used only one of the microporous film (first separator) and the nonwoven fabric (second separator), not only had low discharge capacity but also were prone to short circuits due to free fall, indicating low reliability. Furthermore, the battery of Comparative Example 3, which used both the microporous film (first separator) and the nonwoven fabric (second separator) and had the microporous film extend beyond the nonwoven fabric at one axial end of the wound body (the end on the can bottom side), showed few short circuits due to free fall but a discharge capacity lower than 2400 mAh.

[0097] In contrast, the batteries of Examples 1 to 3, which used a combination of a microporous film (first separator) and a nonwoven fabric (second separator) and had the nonwoven fabric protrude beyond the microporous film at one axial end of the wound body (the end on the can bottom side), showed fewer short circuits due to free fall and a large discharge capacity of 2400 mAh or more.

[0098] From these findings, it can be seen that by configuring the second separator to extend outward beyond the first separator at at least one axial end of the wound body, it is possible to increase reliability while minimizing the decrease in discharge capacity.

[0099] In particular, it is clear that disposing the nonwoven fabric on the positive electrode side increases the discharge capacity more than disposing it on the negative electrode side (comparison between Examples 2 and 3).

[0100] It is also clear that welding the separator beforehand makes it more difficult for a short circuit to occur due to free fall (comparison between Examples 1 and 2).

[0101] This application claims priority from Japanese Patent Application No. 2023-074601, filed April 28, 2023. The contents of the specification and drawings of that application are incorporated herein by reference in their entirety.

[0102] According to the present invention, it is possible to provide a nonaqueous electrolyte battery in which the decrease in discharge capacity due to the depletion of electrolyte around the positive electrode at the end of discharge is small.

[0103] REFERENCE SIGNS LIST 1 nonaqueous electrolyte battery 2 outer can 3 electrode group (wound body) 4 electrolyte 5 sealing body 6 sealing plate 7 positive electrode terminal 8 metal washer 9 sealing gasket 10 positive electrode 11 negative electrode 12 separator 13 first separator 14 second separator 15 positive electrode lead 16 negative electrode lead 17 upper insulating plate 18 lower insulating plate

Claims

1. A nonaqueous electrolyte battery comprising: a wound body in which a positive electrode and a negative electrode are wound in a stacked state with a separator interposed between them; and an outer can for housing the wound body, wherein the separators include a first separator and a second separator stacked on the first separator and having a faster electrolyte absorption rate than the first separator, wherein the second separator protrudes outward beyond the first separator at least on one axial end of the wound body.

2. The nonaqueous electrolyte battery according to claim 1, wherein the width of the second separator in the direction perpendicular to the winding direction is greater than the width of the first separator in the direction perpendicular to the winding direction.

3. The nonaqueous electrolyte battery according to claim 1, wherein the second separator is disposed closer to the positive electrode than the first separator.

4. The nonaqueous electrolyte battery according to claim 1, wherein the first separator and the second separator are resin separators, and the melting point of the second separator is higher than the melting point of the first separator.

5. The nonaqueous electrolyte battery according to claim 1, wherein the second separator is a nonwoven fabric, and the first separator is a microporous film.

6. The nonaqueous electrolyte battery according to claim 1, wherein the negative electrode comprises lithium metal or a lithium alloy.

Citation Information

Patent Citations

  • The spiral-type cell

    JP1984178862U

  • Cylindrical lithium battery

    JP1992012255U

  • Lithium battery

    JP1995037594A

  • Cylindrical nonaqueous electrolyte solution battery

    JP2007250414A

  • Battery separator

    JP2015032379A