Electrode, battery, and method for manufacturing electrode
The electrode design with a high-particle, binder-rich end insulating layer addresses the peeling issue, ensuring strong adhesion and improved battery performance by bonding the insulating layer to the current collecting and active material layers.
Patent Information
- Application Number
- PCT/JP2024/014852
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional electrode manufacturing techniques face challenges in preventing the peeling of the end insulating layer from the current collecting layer, which affects the reliability and performance of batteries.
The electrode design incorporates an end insulating layer with a high proportion of particles and a binder, applied as a slurry and dried to a specific thickness, which is bonded to both sides of the current collecting layer and active material layer, ensuring strong adhesion and preventing peeling.
This configuration effectively suppresses peeling of the end insulating layer, enhancing the stability and performance of the electrode and the battery it is used in.
Smart Images

Figure JP2024014852_31102024_PF_FP_ABST
Abstract
Description
Electrode, battery, and method for manufacturing electrode
[0001] The present invention relates to an electrode, a battery, and a method for manufacturing an electrode.
[0002] BACKGROUND ART Conventionally, there has been known a technique relating to an electrode in which an active material layer and an insulating layer are joined at the end of a current collecting layer (see, for example, Patent Document 1).
[0003] Patent No. 3613400
[0004] It is required to prevent the end insulating layer bonded to the active material layer from peeling off from the current collecting layer.
[0005] The electrode of the present invention has a current collecting layer, an active material layer, and an edge insulating layer. The active material layer is laminated and bonded to the current collecting layer and contains an active material. The edge insulating layer is laminated and bonded from the edge side of the current collecting layer to the side of the active material layer and contains particles and a binder. The proportion of the particles in the edge insulating layer is 55% or more and 99.5% or less. The proportion of the particles and the binder in the edge insulating layer is 55.5% or more and 99% or less. The thickness of the edge insulating layer in the stacking direction is 1 / 20 or more and 1 / 2 or less of the thickness of the active material layer in the stacking direction.
[0006] The battery of the present invention includes a positive electrode, a negative electrode, and an insulator provided between the positive electrode and the negative electrode. At least one of the positive electrode and the negative electrode is the electrode.
[0007] The electrode manufacturing method of the present invention is a method for manufacturing the electrode. The electrode manufacturing method uses an end insulating layer slurry that contains the particles, the binder, and a volatilizable solvent, and that forms the end insulating layer after being applied to the current collecting layer and the active material layer. The electrode manufacturing method includes a coating step of coating the end insulating layer slurry on the current collecting layer and the active material layer. The shrinkage rate of the end insulating layer slurry due to drying is 1% or more and 40% or less.
[0008] It is possible to obtain an electrode in which the end insulating layer is prevented from peeling off from the current collecting layer, and a battery including such an electrode.
[0009] 7 is a perspective view showing a battery 1 of a first embodiment. A perspective view showing a charging / discharging body 10 of the battery 1. A cross-sectional view showing the charging / discharging body 10 at 3A-3B in FIG. 2. A cross-sectional view showing the charging / discharging body 10 in region 4 in FIG. 3. A side view schematically showing a method for manufacturing a positive electrode 100. A top view schematically showing a state in which a slurry is applied to the positive electrode current collecting layer 110 of FIG. 5. A cross-sectional view showing a charging / discharging body 20 of a battery of a second embodiment. A side view schematically showing a method for manufacturing a positive electrode 400 included in the charging / discharging body 20 of FIG. 7. A top view schematically showing a state in which a slurry is applied to the positive electrode current collecting layer 110 of FIG. 8. A cross-sectional view showing a charging / discharging body 30 of a battery of a third embodiment.
[0010] Embodiments for carrying out the present invention will be described with reference to the drawings. To facilitate understanding of each embodiment, the size and proportions of components may be exaggerated in each drawing. In cross-sectional views of active material layers, etc., adjacent active materials are shown not in contact with each other to illustrate the binders and additives surrounding the active materials. In each drawing, identical components are assigned the same reference numerals. The arrows indicate the short-side direction X of the stacked positive electrode 100, negative electrode 200, and separator 300. The arrows indicate the long-side direction Y of the stacked positive electrode 100, negative electrode 200, and separator 300. The arrows indicate the stacking direction Z of the stacked positive electrode 100, negative electrode 200, and separator 300.
[0011] The electrode in the embodiment corresponding to the present invention will be described as a positive electrode. The electrode in the embodiment corresponding to the present invention also includes a negative electrode. The battery 1 in the embodiment corresponding to the present invention will be described as a rectangular parallelepiped battery. The battery 1 in the embodiment corresponding to the present invention also includes a cylindrical battery.
[0012] (Configuration of Battery 1 Including Positive Electrode 100 of First Embodiment) The configuration of a battery 1 including a positive electrode 100 of the first embodiment will be described with reference to FIGS. 1 to 4. FIG.
[0013] Fig. 1 is a perspective view showing a battery 1 of the first embodiment. Fig. 2 is a perspective view showing a charging / discharging body 10 of the battery 1. Fig. 3 is a cross-sectional view showing the charging / discharging body 10 at 3A-3B in Fig. 2. Fig. 4 is a cross-sectional view showing the charging / discharging body 10 in region 4 in Fig. 3.
[0014] The battery 1 is, for example, a lithium ion secondary battery. As shown in Figures 1 to 4, the battery 1 includes a charge / discharge unit 10, an exterior body 50, and external terminals 60. The main components included in the battery 1 will be described below.
[0015] The charge / discharge unit 10 is charged and discharged. The charge / discharge unit 10 shown in FIGS. 2 and 3 includes a positive electrode 100, a negative electrode 200, a separator 300, and an electrolyte (so-called electrolytic solution). The charge / discharge unit 10 is formed, for example, by stacking the positive electrode 100, the negative electrode 200, and two separators 300 in this order, and then winding them into a rectangular parallelepiped shape. In the charge / discharge unit 10, the electrolyte is permeated, particularly into the separator 300. The charge / discharge unit 10 is covered with an insulating sheet in a state where the positive electrode current collector and the negative electrode current collector are joined together.
[0016] As shown in FIG. 3 , the positive electrode 100 (electrode) includes a positive electrode current collecting layer 110 , a positive electrode active material layer 120 , and an end insulating layer 130 .
[0017] The positive electrode current collecting layer 110 (current collecting layer) is configured, for example, in a long shape. That is, the positive electrode current collecting layer 110 is formed in a foil shape. A positive electrode current collecting portion 110a is provided along the longitudinal direction Y at one end of the positive electrode current collecting layer 110 in the short direction X. The positive electrode current collecting layer 110 is formed, for example, from aluminum or an aluminum alloy. For example, JIS standard A3003 is used for the positive electrode current collecting layer 110. A3003 is a non-heat-treated type Al-Mn-based alloy. The thickness of the positive electrode current collecting layer 110 along the stacking direction Z is, for example, 10 μm. The thickness of the positive electrode current collecting layer 110 is selected, for example, from the range of 5 μm to 30 μm.
[0018] The positive electrode active material layer 120 (active material layer) is provided on the positive electrode current collecting layer 110. The positive electrode active material layers 120 are laminated and bonded to both sides of the positive electrode current collecting layer 110, facing each other along the lamination direction Z. The thickness of the positive electrode active material layer 120 along the lamination direction Z is, for example, 30 μm or 40 μm. The thickness of the positive electrode active material layer 120 is selected, for example, within the range of 10 μm to 200 μm.
[0019] The positive electrode active material layer 120 contains a positive electrode active material 121 , a positive electrode binder 122 , and a positive electrode conductive additive 123 .
[0020] The positive electrode active material 121 (active material) is, for example, a lithium-containing composite oxide. The lithium-containing composite oxide is, for example, a metal element such as nickel (Ni), cobalt (Co), or manganese (Mn), and lithium (Li). The positive electrode active material 121 is formed in a particulate form. The average particle diameter (D50) of the positive electrode active material 121 is, for example, 25 μm. The average particle diameter (D50) of the positive electrode active material 121 is selected, for example, within the range of 1 μm to 50 μm.
[0021] The positive electrode binder 122 bonds the positive electrode active material 121 together. For example, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyethylene (PE), polystyrene, polybutadiene, polyacrylonitrile, polyvinyl fluoride, polypropylene fluoride, polychloroprene fluoride, butyl rubber, nitrile rubber, styrene butadiene rubber (SBR), polysulfide rubber, nitrocellulose, cyanoethyl cellulose, various latexes, acrylic resins, or mixtures thereof are used for the positive electrode binder 122.
[0022] The positive electrode conductive additive 123 improves the characteristics of the positive electrode 100. The positive electrode conductive additive 123 is mixed with the positive electrode active material 121 and increases the electrical conductivity between the positive electrode current collecting layer 110 and the positive electrode active material 121. That is, the positive electrode conductive additive 123 ensures a conductive path between the positive electrode current collecting layer 110 and the positive electrode active material 121 in the positive electrode 100. The positive electrode conductive additive 123 is, for example, a carbon-based material. The carbon-based material is, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon is, for example, artificial graphite, natural graphite, or a mixture thereof. The natural graphite is, for example, flake graphite, lump graphite, or amorphous graphite. The amorphous carbon is, for example, carbon black. The carbon black is, for example, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, or a mixture thereof.
[0023] As shown in FIG. 4 , the end insulating layer 130 is laminated and joined from the end 110 b side of the positive electrode current collecting layer 110 to the side portion 120 a of the positive electrode active material layer 120 .
[0024] The thickness t1 of the end insulating layer 130 along the stacking direction Z is 1 / 20 or more and 1 / 2 or less of the thickness t2 of the positive electrode active material layer 120 along the stacking direction Z. The thickness t1 of the end insulating layer 130 along the stacking direction Z may be 1 / 10 or more and 1 / 5 or less of the thickness t2 of the positive electrode active material layer 120 along the stacking direction Z. The thickness t1 of the end insulating layer 130 along the stacking direction Z is 1 μm or more and 15 μm or less at a portion joined to the positive electrode current collecting layer 110 or a portion joined to the positive electrode active material layer 120. The thickness t1 of the end insulating layer 130 along the stacking direction Z may be 2 μm or more and 5 μm or less.
[0025] As shown in FIG. 4, the end insulating layer 130 contains particles 131, a binder 132, and an additive 133.
[0026] The particles 131 are inorganic or organic. The particles 131 are, for example, organic particles or inorganic particles. The organic particles are, for example, acrylic particles. Organic particles are easier to disperse in a solvent than inorganic particles. In particular, acrylic particles are relatively easier to disperse in a solvent. The particles 131 have an average particle diameter (D50) of 0.5 μm or more and 5.0 μm or less. The particles 131 are insulating. It is preferable that the particles 131 are heat resistant. The proportion of the particles 131 in the end insulating layer 130 is 55% or more and 99.5% or less.
[0027] The binder 132 bonds the particles 131 together. The binder 132 has insulating properties. The proportion of the particles 131 and the binder 132 in the end insulating layer 130 is 55.5% or more and 99% or less. In other words, the proportion of the binder 132 in the end insulating layer 130 is 0.5% or more and 45% or less.
[0028] The additive material 133, for example, uniformly disperses the particles 131 and the binder 132. The additive material 133 is not essential for the edge insulating layer 130.
[0029] The positive electrode 100 may include an insulating layer that covers the positive electrode active material layer 120. The insulating layer has heat resistance. The insulating layer contains, for example, an inorganic material or an organic material and a binder. The inorganic material is, for example, alumina particles.
[0030] As shown in FIG. 3 , the negative electrode 200 includes a negative electrode current collecting layer 210 and a negative electrode active material layer 220 .
[0031] The negative electrode current collecting layer 210 is configured, for example, in an elongated shape. That is, the negative electrode current collecting layer 210 is formed in a foil shape. A negative electrode current collecting portion 210a is provided along the longitudinal direction Y at one end of the negative electrode current collecting layer 210 in the short side direction X. The negative electrode current collecting portion 210a of the negative electrode current collecting layer 210 faces the positive electrode current collecting portion 110a of the positive electrode current collecting layer 110 in the short side direction X. The negative electrode current collecting layer 210 is formed, for example, from copper or a copper alloy. The thickness of the negative electrode current collecting layer 210 along the stacking direction Z is, for example, 10 μm. The thickness of the negative electrode current collecting layer 210 is selected, for example, within a range of 5 μm to 30 μm.
[0032] The negative electrode active material layer 220 is provided on the negative electrode current collecting layer 210. The negative electrode active material layers 220 are bonded to both sides of the negative electrode current collecting layer 210 and face each other along the stacking direction Z. The negative electrode active material layer 220 has a greater width along the short-side direction X than the positive electrode active material layer 120. When the negative electrode 200 faces the positive electrode 100 via the separator 300, both ends of the negative electrode active material layer 220 in the short-side direction X are located further outward in the short-side direction X than both ends of the positive electrode active material layer 120 in the short-side direction X. The thickness of the negative electrode active material layer 220 along the stacking direction Z is, for example, 30 μm or 40 μm. The thickness of the negative electrode active material layer 220 is selected, for example, within a range of 10 μm to 200 μm.
[0033] The negative electrode active material layer 220 contains a negative electrode active material 221 and a negative electrode binder 222. The negative electrode active material layer 220 may also contain a negative electrode conductive additive 223.
[0034] The negative electrode active material 221 is made of, for example, carbon. The carbon is, for example, graphite, non-graphitizable carbon (hard carbon), or easily graphitizable carbon (soft carbon). The graphite is, for example, natural graphite or artificial graphite. The natural graphite is, for example, flake graphite, lump graphite, or amorphous graphite. The negative electrode active material 221 is formed in a particulate form. The average particle size (D50) of the negative electrode active material 221 is, for example, 25 μm. The average particle size (D50) of the negative electrode active material 221 is selected, for example, within the range of 1 μm to 50 μm.
[0035] The negative electrode binder 222 bonds the negative electrode active material 221 together. For the negative electrode binder 222, for example, the same material as the positive electrode binder 122 is used.
[0036] The negative electrode conductive additive 223 improves the characteristics of the negative electrode 200. The negative electrode conductive additive 223 is mixed with the negative electrode active material 221 and disposed therein to increase the electrical conductivity between the negative electrode current collecting layer 210 and the negative electrode active material 221. That is, the negative electrode conductive additive 223 ensures a conductive path between the negative electrode current collecting layer 210 and the negative electrode active material 221 in the negative electrode 200.
[0037] The negative electrode 200 may include an insulating layer that covers the negative electrode active material layer 220. The insulating layer has heat resistance. The insulating layer contains, for example, an inorganic material or an organic material and a binder. The inorganic material is, for example, alumina particles.
[0038] As shown in FIG. 3 , the separator 300 insulates the positive electrode 100 from the negative electrode 200. The separator 300 also holds an electrolyte (so-called electrolytic solution). The separator 300 is formed in an elongated shape. The separator 300 has a width along the short-side direction X that is greater than that of the negative electrode active material layer 220. When the positive electrode 100 and the negative electrode 200 face each other via the separator 300, both ends of the positive electrode active material layer 120 along the short-side direction X and both ends of the negative electrode active material layer 220 along the short-side direction X are located within the range of the separator 300 along the short-side direction X. The thickness of the separator 300 along the stacking direction Z is, for example, 20 μm. The thickness of the separator 300 is selected, for example, within a range of 5 μm to 60 μm.
[0039] The separator 300 is made of a porous material, such as polyethylene, polypropylene, polyester, cellulose, or polyamide. The separator 300 may be made of a laminate of multiple different porous materials.
[0040] The separator 300 may include an insulating layer. The insulating layer has heat resistance. The insulating layer contains, for example, an inorganic material or an organic material and a binder. The inorganic material is, for example, alumina particles.
[0041] The electrolyte allows lithium ions to flow between the positive electrode 100 and the negative electrode 200. The electrolyte is also called an electrolytic solution.
[0042] The electrolyte contains an organic solvent and a lithium salt, and may contain an additive.
[0043] The organic solvent may be, for example, a carbonate ester such as ethylene carbonate. The lithium salt may be, for example, lithium hexafluorophosphate (LiPF 6 ) is used as the additive. For example, lithium hexafluorophosphate (LiPF6 ) is used.
[0044] The exterior body 50 houses the charging / discharging unit 10. As shown in FIG. 1 , the exterior body 50 includes a container 51, a lid 52, a filling tap 53, and a split valve 54. The container 51 is formed in a rectangular parallelepiped shape. The container 51 houses the charging / discharging unit 10. The lid 52 is welded to the container 51. The lid 52 has a filling hole. The filling hole is a hole for injecting an electrolyte (so-called electrolytic solution) into the interior of the battery 1. The filling tap 53 is attached to the filling hole of the lid 52. After the electrolyte is injected into the interior of the battery 1 through the filling hole, the filling tap 53 is inserted into the filling hole and welded. The lid 52 has a split valve 54. The split valve 54 is formed integrally with the lid 52. The split valve 54 splits outward from the battery 1 when the internal pressure of the battery 1 exceeds a predetermined value.
[0045] The external terminals 60 relay the input and output of power between the current collectors provided inside the battery 1 and electrical equipment provided outside the battery 1. The electrical equipment is, for example, a relay or inverter provided in the vehicle. Furthermore, the external terminals 60 provided on one battery 1 are electrically connected to the external terminals 60 provided on other batteries 1 via bus bars or the like, relaying the input and output of power between the one battery 1 and the other batteries 1. As shown in FIG. 1 , the external terminals 60 include a positive terminal 61 and a negative terminal 62. The positive terminal 61 is electrically connected to the positive current collecting portion 110a of the positive current collecting layer 110 via a positive current collecting plate. The positive terminal 61 is attached to the lid 52 via a positive electrode insulating member. The negative terminal 62 is electrically connected to the negative current collecting portion 210a of the negative current collecting layer 210 via a negative current collecting plate. The negative terminal 62 is attached to the lid 52 via a negative electrode insulating member.
[0046] (Method for manufacturing the positive electrode 100 of the first embodiment) A method for manufacturing the positive electrode 100 will be described with reference to Fig. 5 and Fig. 6. Fig. 5 is a side view that schematically shows the method for manufacturing the positive electrode 100. Fig. 6 is a top view that schematically shows the state in which the slurry is applied to the positive electrode current collecting layer 110 of Fig. 5.
[0047] In the method for manufacturing the positive electrode 100 , in the coating step, the positive electrode current collecting layer 110 is coated with the positive electrode active material layer slurry 1100 and the end insulating layer slurry 1200 .
[0048] The positive electrode active material layer slurry 1100 used in the coating step contains a solvent in addition to the components that make up the positive electrode active material layer 120. The components that make up the positive electrode active material layer 120 include a positive electrode active material 121, a positive electrode binder 122, and a positive electrode conductive additive 123. The solvent disperses the components contained in the positive electrode active material layer 120. For example, a solvent that is vaporizable at a temperature equal to or higher than room temperature is used. For example, the solvent is N-methyl-2-pyrrolidone (NMP).
[0049] The end insulating layer slurry 1200 used in the application process contains a solvent in addition to the components that make up the end insulating layer 130. The particles 131, binder 132, etc. contained in the end insulating layer 130 are dispersed in the solvent. The solvent used is, for example, one that evaporates at a temperature equal to or higher than room temperature. The solvent is, for example, N-methyl-2-pyrrolidone (NMP). The shrinkage rate of the end insulating layer slurry 1200 due to drying is 1% or more and 40% or less.
[0050] As shown in FIG. 5, the manufacturing apparatus 1000 for the positive electrode 100 includes a conveying section 1010, a coating section 1020, a drying section 1030, and a rolling section 1040.
[0051] 5, the conveying unit 1010 conveys the members that constitute the positive electrode 100. The conveying unit 1010 includes a conveying roller 1011.
[0052] The conveying unit 1010 conveys the positive electrode current collecting layer 110 wound around a first roller (not shown) to the coating unit 1020, the drying unit 1030, and the rolling unit 1040 via conveying rollers 1011 and the like. The conveying unit 1010 winds the positive electrode current collecting layer 110, to which the positive electrode active material layer 120 and the end insulating layer 130 are bonded, around a second roller (not shown). When the second roller to which the positive electrode current collecting layer 110 is attached rotates, the conveying roller 1011 and the first roller in contact with the positive electrode current collecting layer 110 also rotate, conveying the positive electrode current collecting layer 110. The conveying direction H of the positive electrode current collecting layer 110 corresponds to the longitudinal direction Y of the positive electrode current collecting layer 110.
[0053] 5, the coating unit 1020 coats the positive electrode current collecting layer 110 with slurry. The coating unit 1020 includes a first coating head 1021, a first liquid feed pipe 1022, a second coating head 1023, and a second liquid feed pipe 1024.
[0054] As shown in FIGS. 5 and 6 , two first coating heads 1021 are provided along the conveying direction H of the positive electrode current collecting layer 110, i.e., the short direction X perpendicular to the longitudinal direction Y of the positive electrode current collecting layer 110. The two first coating heads 1021 face each other along the short direction X of the positive electrode current collecting layer 110. An opening is formed in each first coating head 1021. The opening is connected to a first liquid feed pipe 1022. The end insulating layer slurry 1200 is supplied to each first coating head 1021 from a tank (not shown) via a pump (not shown) and the first liquid feed pipe 1022. Each first coating head 1021 faces the conveying roller 1011 with the positive electrode current collecting layer 110 interposed therebetween. While the positive electrode current collecting layer 110 is being transported, each of the first coating heads 1021 coats the positive electrode current collecting layer 110 with the end insulating layer slurry 1200. The end insulating layer slurry 1200 is coated on the positive electrode current collecting layer 110 so as to face each other in the short direction of the positive electrode current collecting layer 110 and to extend along the long direction of the positive electrode current collecting layer 110.
[0055] As shown in FIGS. 5 and 6 , the second coating head 1023 is provided along the short-side direction X of the positive electrode current collecting layer 110. The second coating head 1023 is aligned with the two first coating heads 1021 along the conveyance direction H of the positive electrode current collecting layer 110. The second coating head 1023 is located downstream of each of the first coating heads 1021 in the conveyance direction H of the positive electrode current collecting layer 110. An elongated opening is formed in the second coating head 1023. The elongated opening is connected to a second liquid supply pipe 1024. The positive electrode active material layer slurry 1100 is supplied to the second coating head 1023 from a tank (not shown) via a pump (not shown) and the second liquid supply pipe 1024. The second coating head 1023 faces the conveyance roller 1011 with the positive electrode current collecting layer 110 interposed therebetween. The second coating head 1023 coats the positive electrode active material layer slurry 1100 onto the positive electrode current collecting layer 110 and the end insulating layer slurry 1200 while the positive electrode current collecting layer 110 is being transported.
[0056] 5 , the drying unit 1030 dries the slurry. The drying unit 1030 is provided downstream of the coating unit 1020 in the conveying direction H of the positive electrode current collecting layer 110. The drying unit 1030 includes a dryer 1031.
[0057] As shown in Fig. 5 , the dryer 1031 is provided along the transport direction H of the positive electrode current collecting layer 110, i.e., the longitudinal direction Y of the positive electrode current collecting layer 110. The dryer 1031 dries the positive electrode active material layer slurry 1100 and the end insulating layer slurry 1200 while the positive electrode current collecting layer 110 is being transported. The dryer 1031 is equipped with a plurality of heat sources along the transport direction H of the positive electrode current collecting layer 110. The dryer 1031 uses the multiple heat sources to dry the positive electrode active material layer slurry 1100 and the end insulating layer slurry 1200 under a plurality of conditions.
[0058] In the drying section 1030, the solvent in the positive electrode active material layer slurry 1100 evaporates, thereby forming the positive electrode active material layer 120. The NMP contained in the positive electrode active material layer slurry 1100 evaporates, thereby drying the positive electrode active material layer slurry 1100. As the positive electrode active material layer slurry 1100 dries, its thickness along the stacking direction Z decreases. The positive electrode active material layer 120 is bonded to the positive electrode current collecting layer 110. The solvent in the end insulating layer slurry 1200 evaporates, thereby forming the end insulating layer 130. The NMP contained in the end insulating layer slurry 1200 evaporates, thereby drying the end insulating layer slurry 1200. As the end insulating layer slurry 1200 dries, its thickness along the stacking direction Z decreases. The end insulating layer 130 is bonded to the side portion 120a of the positive electrode active material layer 120.
[0059] 5 , the rolling unit 1040 rolls the positive electrode current collecting layer 110, the positive electrode active material layer 120, and the end insulating layer 130, which are bonded together. The rolling unit 1040 is provided downstream of the drying unit 1030 in the conveying direction H of the positive electrode current collecting layer 110. The rolling unit 1040 includes a rolling roller 1041 and a driven roller 1042.
[0060] As shown in FIG. 5 , the rolling roller 1041 is provided along the short-side direction X of the positive electrode current collecting layer 110. The rolling roller 1041 faces the positive electrode active material layer 120 and the end insulating layer 130 of the positive electrode 100. As shown in FIG. 5 , the driven roller 1042 is provided along the short-side direction X of the positive electrode current collecting layer 110. The driven roller 1042 faces the rolling roller 1041 across the positive electrode 100. The driven roller 1042 faces the positive electrode current collecting layer 110 of the positive electrode 100. The rolling unit 1040 determines the thickness of the positive electrode active material layer 120 by the distance between the rolling roller 1041 and the driven roller 1042.
[0061] In the method for manufacturing the positive electrode 100, the configuration described with reference to FIGS. 5 and 6 is a configuration in which the positive electrode active material layer 120 and the end insulating layer 130 are bonded to one surface of the positive electrode current collecting layer 110. That is, the method for manufacturing the positive electrode 100 shown in FIGS. 5 and 6 is a so-called single-sided coating method for manufacturing the positive electrode 100. On the other hand, as shown in FIG. 3, for example, the positive electrode 100 has the positive electrode active material layer 120 and the end insulating layer 130 bonded to both surfaces of the positive electrode current collecting layer 110. That is, the positive electrode 100 shown in FIG. 3 is configured by so-called double-sided coating. Therefore, in the method for manufacturing the positive electrode 100, after the configuration described with reference to FIGS. 5 and 6, the positive electrode active material layer 120 and the end insulating layer 130 are bonded to the other surface of the positive electrode active material layer 120.
[0062] (Comparative Experimental Results of Positive Electrode 100 of First Embodiment and Comparative Positive Electrode) The comparative experimental results of positive electrode 100 of the first embodiment and comparative positive electrodes will be described with reference to Table 1. Table 1 shows the results of an experiment to peel off the end insulating layer from the positive electrode current collecting layer.
[0063]
[0064] The end insulating layer under condition 1 corresponds to the end insulating layer 130 of the positive electrode 100 of the embodiment (first embodiment). On the other hand, the end insulating layers under conditions 2, 3, and 4 correspond to the end insulating layers of the positive electrodes of the comparative examples.
[0065] In condition 1, the proportion of the particles 131 was set to 69% and the proportion of the binder 132 was set to 31% in the end insulating layer 130. Also, in condition 1, the thickness of the end insulating layer 130 in the stacking direction Z was set to 10 μm.
[0066] In condition 2, the proportion of insulator in the edge insulating layer was set to 69% and the proportion of binder was set to 31%, similar to condition 1. Also, in condition 2, unlike condition 1, the thickness of the edge insulating layer in the stacking direction Z was set to 18 μm.
[0067] In condition 3, the conditions were reversed from condition 1, with the proportion of insulator in the edge insulating layer set to 31% and the proportion of binder set to 69%. Also, in condition 3, as in condition 1, the thickness of the edge insulating layer in the stacking direction Z was set to 10 μm.
[0068] In condition 4, the proportion of insulator in the edge insulating layer was set to 31% and the proportion of binder was set to 69%, similar to condition 1. In condition 3, the thickness of the edge insulating layer in the stacking direction Z was set to 18 μm, similar to condition 2.
[0069] The end insulating layer 130 under condition 1 was sufficiently suppressed from warping relative to the positive electrode current collecting layer 110. That is, the end insulating layer 130 under condition 1 was sufficiently suppressed from peeling from the positive electrode current collecting layer 110. Therefore, the end insulating layer 130 under condition 1 was evaluated as ○ (sufficiently capable of suppressing peeling) for the suppression of peeling.
[0070] The end insulating layer under condition 2 was prevented from warping relative to the positive electrode current collecting layer to a certain extent. That is, the end insulating layer under condition 2 was prevented from peeling from the positive electrode current collecting layer to a certain extent. Therefore, the end insulating layer under condition 2 was evaluated as △ (peel-off can be prevented to a certain extent) in terms of peel-off prevention.
[0071] The end insulating layer under condition 3 showed significant warpage relative to the positive electrode current collecting layer. That is, the end insulating layer under condition 3 peeled off from the positive electrode current collecting layer. Therefore, the end insulating layer under condition 3 was evaluated as × (peel-off could not be suppressed) for the prevention of peeling.
[0072] The end insulating layer under condition 4 warped more against the positive electrode current collecting layer than the end insulating layer under condition 3. That is, the end insulating layer under condition 4 peeled off from the positive electrode current collecting layer, similar to the end insulating layer under condition 3. Therefore, the end insulating layer under condition 4 was evaluated as × (peel-off could not be suppressed) for the prevention of peeling.
[0073] Under condition 1, the end insulating layer slurry 1200 containing a relatively small amount of binder 132 is relatively prevented from shrinking when the solvent dries to form the end insulating layer 130. As a result, the end insulating layer 130 is prevented from peeling off from the positive electrode current collecting layer 110. The end insulating layer slurry 1200 having a relatively thin layer thickness is relatively prevented from shrinking when the solvent dries to form the end insulating layer 130. As a result, the end insulating layer 130 is prevented from peeling off from the positive electrode current collecting layer 110.
[0074] (Effects of the Battery 1 Including the Positive Electrode 100 of the First Embodiment) The effects of the battery 1 including the positive electrode 100 of the first embodiment will be described.
[0075] (1), (7), and (8) The positive electrode 100 (electrode) has an end insulating layer 130. The end insulating layer 130 is laminated and joined from the end 110b of the positive electrode current collecting layer 110 (current collecting layer) to the side 120a of the positive electrode active material layer 120 (active material layer). The end insulating layer 130 contains particles 131 and a binder 132. The proportion of the particles 131 in the end insulating layer 130 is 55% or more and 99.5% or less. The proportion of the particles 131 and the binder 132 in the end insulating layer 130 is 55.5% or more and 99% or less. In this case, the binder 132 is 0.5% or more and 45% or less. The thickness of the end insulating layer 130 in the stacking direction Z is 1 / 20 or more and 1 / 2 or less of the thickness of the positive electrode active material layer 120 in the stacking direction Z. With this configuration, the end insulating layer 130 can be prevented from warping relative to the positive electrode current collecting layer 110. That is, with this configuration, the end insulating layer 130 can be prevented from peeling off from the positive electrode current collecting layer 110. As a result, a positive electrode 100 can be obtained in which the end insulating layer 130 is prevented from peeling off from the positive electrode current collecting layer 110. Furthermore, with this configuration, a battery 1 can be obtained that includes a positive electrode 100 in which the end insulating layer 130 is prevented from peeling off from the positive electrode current collecting layer 110.
[0076] (2) The thickness of the end insulating layer 130 in the stacking direction Z is 1 / 10 to 1 / 5 of the thickness of the positive electrode active material layer 120 in the stacking direction Z. With this configuration, the end insulating layer 130 is also sufficiently bonded to the positive electrode active material layer 120, and therefore peeling off from the positive electrode current collecting layer 110 can be sufficiently suppressed.
[0077] (3) The thickness of the end insulating layer 130 along the stacking direction Z is 1 μm or more and 15 μm or less at the portion bonded to the positive electrode current collecting layer 110 or at the portion bonded to the positive electrode active material layer 120. With this configuration, the end insulating layer 130 is also sufficiently bonded to the positive electrode active material layer 120, and therefore peeling off from the positive electrode current collecting layer 110 can be sufficiently suppressed.
[0078] (4) The thickness of the end insulating layer 130 along the stacking direction Z is 2 μm or more and 5 μm or less. With this configuration, the end insulating layer 130 is also sufficiently bonded to the positive electrode active material layer 120, and therefore peeling off from the positive electrode current collecting layer 110 can be sufficiently suppressed.
[0079] (9) In the method for manufacturing the positive electrode 100, in the coating step, the shrinkage rate of the end insulating layer slurry 1200 due to drying is 1% or more and 40% or less. With this configuration, the end insulating layer 130 can be sufficiently prevented from warping relative to the positive electrode current collecting layer 110 due to shrinkage during drying. In other words, with this configuration, the end insulating layer 130 can be sufficiently prevented from peeling off from the positive electrode current collecting layer 110.
[0080] (Configuration of Positive Electrode 400 of Second Embodiment) The configuration of the positive electrode 400 of the second embodiment will be described with reference to Fig. 7. Fig. 7 is a cross-sectional view showing the charge / discharge body 20 of the battery of the second embodiment.
[0081] The positive electrode 400 differs from the positive electrode 100 of the first embodiment in that an end insulating layer 430 is also provided at the end 120b of the positive electrode active material layer 120. In the second embodiment, the same components as those in the first embodiment are denoted by the same reference numerals and descriptions thereof are omitted.
[0082] The end insulating layer 430 is laminated and joined from the end 110b side of the positive electrode current collecting layer 110, through the side portion 120a of the positive electrode active material layer 120, to the end 120b of the positive electrode active material layer 120. The end insulating layer 430 is joined to both the positive electrode current collecting layer 110 and the positive electrode active material layer 120 along the short-side direction X, with the side portion 120a of the positive electrode active material layer 120 as the boundary. In other words, the end insulating layer 430 partially overlaps with the positive electrode active material layer 120 along the lamination direction Z.
[0083] (Method of Manufacturing Positive Electrode 400 of Second Embodiment) Regarding the method of manufacturing the positive electrode 400, only the configurations different from the method of manufacturing the positive electrode 100 will be described with reference to Fig. 8 and Fig. 9. Fig. 8 is a side view schematically showing a method of manufacturing the positive electrode 400 included in the charge / discharge body 20 of Fig. 7. Fig. 9 is a top view schematically showing a state in which the slurry is applied to the positive electrode current collecting layer 110 of Fig. 8.
[0084] As shown in FIG. 8 , the manufacturing apparatus 2000 for the positive electrode 400 includes a conveying section 1010 , a coating section 2020 , a drying section 1030 , and a rolling section 1040 .
[0085] 8 , the coating unit 2020 applies slurry to the positive electrode current collecting layer 110 and the like. The coating unit 2020 includes a first coating head 2021, a first liquid feed pipe 1022, a second coating head 2023, and a second liquid feed pipe 1024.
[0086] As shown in FIGS. 8 and 9 , the first coating head 2021 is provided along the conveying direction H of the positive electrode current collecting layer 110, i.e., along the short direction X perpendicular to the longitudinal direction Y of the positive electrode current collecting layer 110. An elongated opening is formed in the first coating head 2021. The elongated opening is connected to a first liquid supply pipe 1022. The positive electrode active material layer slurry 1100 is supplied to the first coating head 2021 from a tank (not shown) via a pump (not shown) and the first liquid supply pipe 1022. The first coating head 2021 faces the conveying roller 1011 across the positive electrode current collecting layer 110. The first coating head 2021 applies the positive electrode active material layer slurry 1100 to the positive electrode current collecting layer 110 while the positive electrode current collecting layer 110 is being conveyed.
[0087] As shown in FIGS. 8 and 9 , two second coating heads 2023 are provided along the short-side direction X of the positive electrode current collecting layer 110. The two second coating heads 2023 face each other along the short-side direction X of the positive electrode current collecting layer 110. The second coating heads 2023 are aligned with the first coating head 2021 along the conveyance direction H of the positive electrode current collecting layer 110. The second coating head 2023 is located downstream of the first coating head 2021 in the conveyance direction H of the positive electrode current collecting layer 110. An opening is formed in the second coating head 2023. The opening is connected to a second liquid supply pipe 1024. The end insulating layer slurry 1200 is supplied to each second coating head 2023 from a tank (not shown) via a pump (not shown) and the second liquid supply pipe 1024. Each second coating head 2023 faces the conveying roller 1011 with the positive electrode current collecting layer 110 interposed therebetween. While the positive electrode current collecting layer 110 is being conveyed, each second coating head 2023 applies the end insulating layer slurry 1200 to the ends of the positive electrode current collecting layer 110 and the positive electrode active material layer slurry 1100. The end insulating layer slurry 1200 is applied to the positive electrode current collecting layer 110 so as to face each other in the short-side direction of the positive electrode current collecting layer 110 and to extend along the long-side direction of the positive electrode current collecting layer 110. The end insulating layer slurry 1200 is applied so as to cover both ends of the positive electrode active material layer slurry 1100 in the short-side direction.
[0088] (Effects of the Battery Including the Positive Electrode 400 of the Second Embodiment) The effects of the battery including the positive electrode 400 of the second embodiment will be described.
[0089] (5) The end insulating layer 430 is laminated and bonded from the end 110b side of the positive electrode current collecting layer 110, through the side portion 120a of the positive electrode active material layer 120, to the end 120b of the positive electrode active material layer 120. With this configuration, the positive electrode active material layer 120 is sufficiently bonded to the end insulating layer 130, which can sufficiently prevent peeling from the positive electrode current collecting layer 110. Furthermore, with this configuration, the end insulating layer 130 is sufficiently bonded to the positive electrode active material layer 120, which can sufficiently prevent peeling from the positive electrode current collecting layer 110.
[0090] (Configuration of Positive Electrode 500 of Third Embodiment) The configuration of the positive electrode 500 of the third embodiment will be described with reference to Fig. 10. Fig. 10 is a cross-sectional view showing the charge / discharge body 30 of the battery of the third embodiment.
[0091] The positive electrode 500 differs from the positive electrode 100 of the first embodiment in that an end insulating layer 530 is also provided between the positive electrode current collecting layer 110 and the positive electrode active material layer 120 along the stacking direction Z. In the third embodiment, the same components as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted.
[0092] The end insulating layer 530 is laminated and bonded from the end 110b side of the positive electrode current collecting layer 110 to between the positive electrode active material layer 120 and the positive electrode current collecting layer 110. The end insulating layer 530 is bonded to both the positive electrode current collecting layer 110 and the positive electrode active material layer 120 along the short direction X, with the side portion 120a of the positive electrode active material layer 120 as the boundary. The end insulating layer 530 is also provided between the positive electrode current collecting layer 110 and the positive electrode active material layer 120. In other words, the end insulating layer 530 partially overlaps with the positive electrode active material layer 120 along the stacking direction Z.
[0093] (Effects of the Battery Including the Positive Electrode 500 of the Third Embodiment) The effects of the battery including the positive electrode 500 of the third embodiment will be described.
[0094] (6) The end insulating layer 530 is laminated and bonded from the end 110b side of the positive electrode current collecting layer 110 to between the positive electrode active material layer 120 and the positive electrode current collecting layer 110. That is, the positive electrode active material layer 120 is sufficiently bonded to the positive electrode current collecting layer 110 along the stacking direction Z via the end insulating layer 130, which has a higher affinity than the positive electrode current collecting layer 110. With this configuration, the positive electrode active material layer 120 is sufficiently bonded to the end insulating layer 130, which can sufficiently prevent the positive electrode active material layer 120 from peeling off from the positive electrode current collecting layer 110. Furthermore, with this configuration, the end insulating layer 130 is sandwiched between the positive electrode active material layer 120 and the positive electrode current collecting layer 110 and sufficiently bonded to the positive electrode current collecting layer 110, which can sufficiently prevent the end insulating layer 130 from peeling off from the positive electrode current collecting layer 110.
[0095] (Battery of Other Embodiments) The battery of the present invention is not limited to the configuration of the battery described in the embodiments, and can be configured appropriately based on the content described in the claims.
[0096] The embodiments are described in detail or simply to make the present invention easier to understand, and do not necessarily include all of the components described, or may include components not shown. Also, some of the components of the embodiments may be deleted, replaced with components of other embodiments, or combined with components of other embodiments.
[0097] In the electrode (positive electrode) of the present invention, the positive electrode active material is not limited to nickel (Ni), cobalt (Co), and manganese (Mn)-based materials. The positive electrode active material of the present invention may be, for example, iron (olivine)-based.
[0098] In the electrode (negative electrode) of the present invention, the negative electrode active material is not limited to a carbon-based material, but may be, for example, a silicon-based material.
[0099] The battery of the present invention is not limited to a configuration in which the charge / discharge body is sealed by a container and a lid, but can be applied to a configuration in which the charge / discharge body is sealed by a laminate film.
[0100] The battery of the present invention is not limited to a lithium-ion battery, but can be applied to, for example, a nickel-metal hydride battery.
[0101] The battery of the present invention is not limited to a secondary battery, but can be applied to a primary battery.
[0102] In the battery of the present invention, the charge / discharge body is not limited to a wound type in which a positive electrode, a separator, and a negative electrode each formed in a long shape are bundled and wound up. A stacked type in which a positive electrode, a separator, and a negative electrode each formed in a rectangular shape are alternately stacked can be used as the charge / discharge body of the battery of the present invention.
[0103] In the battery of the present invention, the charge / discharge body may be a stacked type in which a plurality of relatively short positive electrodes and a plurality of short negative electrodes are alternately arranged facing each other with the separator interposed therebetween, with the separator being folded and stacked.
[0104] In the battery of the present invention, the charging / discharging body is not limited to a rectangular parallelepiped type, and a cylindrical or columnar type may also be used as the charging / discharging body of the battery of the present invention.
[0105] In the battery of the present invention, the charge / discharge body is not limited to a configuration in which an insulating separator is provided between the positive electrode and the negative electrode. The battery of the present invention can also be applied to a configuration in which an insulating layer is provided on at least one of the positive electrode and the negative electrode without providing a separator. Such a configuration corresponds to a so-called separatorless configuration.
[0106] In the battery of the present invention, the charge / discharge body can be applied to a configuration in which an insulating separator 300 is provided between the positive electrode 100 and the negative electrode 200, as well as a configuration in which an insulating layer is provided on the positive electrode 100 or an insulating layer is provided on the negative electrode 200.
[0107] The battery of the present invention is not limited to a configuration in which only one charging / discharging element is provided, but can be applied to a configuration in which two or more charging / discharging elements are provided.
[0108] The electrodes (positive and negative electrodes) of the present invention are not limited to a configuration in which the ends of the current collecting layer are joined to the current collecting plate. The electrodes of the battery of the present invention can be applied to a type in which electrode tabs protruding outward from the edges of the current collecting layer are joined to the current collecting plate.
[0109] The electrodes (positive electrode, negative electrode) of the present invention are not limited to a configuration in which active material layers are bonded to both sides of a current collecting layer, and may be configured to have an active material layer bonded to only one side of a current collecting layer.
[0110] The method for manufacturing an electrode (positive electrode, negative electrode) of the present invention is not limited to a configuration in which an active material layer and an end insulating layer are formed by simultaneously coating and drying an active material layer slurry and an end insulating layer slurry. The method for manufacturing an electrode (positive electrode, negative electrode) of the present invention can be applied to a configuration in which an active material layer is first formed by coating and drying the active material layer slurry on a current collecting layer. In such a configuration, the end insulating layer is then formed by coating and drying the end insulating layer slurry on the current collecting layer. Furthermore, the method for manufacturing an electrode (positive electrode, negative electrode) of the present invention can be applied to a configuration in which an end insulating layer is first formed by coating and drying the end insulating layer slurry on a current collecting layer. In such a configuration, the active material layer is then formed by coating and drying the active material layer slurry on the current collecting layer.
[0111] The method for manufacturing electrodes (positive electrode, negative electrode) of the present invention is not limited to a configuration in which the first coating head and the second coating head are provided independently, but can be applied to a configuration in which the first coating head and the second coating head are integrated.
[0112] DESCRIPTION OF SYMBOLS 1 Battery, 10, 20, 30 Charger / discharger, 50 Exterior body, 51 Container, 52 Lid, 53 Injection plug, 54 Cleavage valve, 60 External terminal, 61 Positive electrode terminal, 62 Negative electrode terminal, 100, 400, 500 Positive electrode (electrode), 110 Positive electrode current collecting layer (current collecting layer), 110a Positive electrode current collecting portion, 110b End, 120 Positive electrode active material layer (active material layer), 120a Side, 120b End, 121 Positive electrode active material (active material), 122 Positive electrode binder, 123 Positive electrode conductive additive, 130, 430, 530 End insulating layer, 131 Particle, 132 Binder, 133 Additive, 200 Negative electrode, 210 negative electrode current collecting layer, 210a negative electrode current collecting portion, 220 negative electrode active material layer, 221 negative electrode active material, 222 negative electrode binder, 223 negative electrode conductive additive, 300 separator (insulator), 1000, 2000 manufacturing apparatus, 1010 conveying portion, 1011 conveying roller, 1020, 2020 coating portion, 1021, 2021 first coating head, 1022 first liquid supply pipe, 1023, 2023 second coating head, 1024 second liquid supply pipe, 1030 drying portion, 1031 dryer, 1040 rolling portion, 1041 rolling roller, 1042 driven roller, 1100 positive electrode active material layer slurry, 1200 Insulating layer slurry, t1: thickness of end insulating layer 130 along stacking direction Z, t2: thickness of positive electrode active material layer 120 along stacking direction Z, X: short side direction (of positive electrode 100, negative electrode 200, separator 300), Y: long side direction (of positive electrode 100, negative electrode 200, separator 300), Z: stacking direction (of positive electrode 100, negative electrode 200, separator 300), H: transport direction (longitudinal direction Y) (of positive electrode 100, negative electrode 200, separator 300).
Claims
1. An electrode comprising: a current collecting layer; an active material layer laminated and joined to the current collecting layer, the active material layer containing an active material; and an end insulating layer laminated and joined from an end side of the current collecting layer to a side side of the active material layer, the end insulating layer containing particles and a binder, wherein the proportion of the particles in the end insulating layer is 55% or more and 99.5% or less, the proportion of the particles and the binder in the end insulating layer is 55.5% or more and 99% or less, and the thickness of the end insulating layer in the stacking direction is 1 / 20 or more and 1 / 2 or less of the thickness of the active material layer in the stacking direction.
2. The electrode according to claim 1, wherein the thickness of the end insulating layer in the stacking direction is 1 / 10 or more and 1 / 5 or less of the thickness of the active material layer in the stacking direction.
3. The electrode according to claim 1, wherein the thickness of the end insulating layer along the stacking direction is 1 μm or more and 15 μm or less at the portion joined to the current collecting layer or the portion joined to the active material layer.
4. The electrode according to claim 3, wherein the thickness of the end insulating layer in the stacking direction is 2 μm or more and 5 μm or less.
5. The electrode according to claim 1, wherein the end insulating layer is laminated and joined from the end side of the current collecting layer through the side portion of the active material layer to the end of the active material layer.
6. The electrode according to claim 1, wherein the end insulating layer is laminated and joined from the end side of the current collecting layer to between the active material layer and the current collecting layer.
7. The electrode according to claim 1, wherein the current collecting layer is a positive electrode current collecting layer, and the active material layer is a positive electrode active material layer containing a positive electrode active material.
8. A battery comprising: a positive electrode; a negative electrode; and an insulator insulating the positive electrode from the negative electrode, wherein at least one of the positive electrode and the negative electrode comprises: a current collecting layer; an active material layer joined to the current collecting layer and containing an active material; and an end insulating layer joined from an end side of the current collecting layer to a side part of the active material layer and containing particles and a binder.
9. A method for producing an electrode comprising: a current collecting layer; an active material layer laminated and joined to the current collecting layer, the active material layer including an active material; and an end insulating layer laminated and joined from an end side of the current collecting layer to a side part of the active material layer, the end insulating layer including particles and a binder, wherein a ratio of the particles in the end insulating layer is 55% or more and 99.5% or less, a ratio of the particles and the binder in the end insulating layer is 55.5% or more and 99% or less, and a thickness of the end insulating layer along the lamination direction is 1 / 20 or more and 1 / 2 or less of a thickness of the active material layer along the lamination direction, the method comprising: using an end insulating layer slurry including the particles, the binder, and a volatile solvent, the end insulating layer being formed after being coated on the current collecting layer and the active material layer, the method comprising a coating step of coating the current collecting layer and the active material layer with the end insulating layer slurry, and a shrinkage rate due to drying of the end insulating layer slurry being 1% or more and 40% or less. A method for manufacturing an electrode.
Citation Information
Patent Citations
Non-aqueous secondary battery and method for manufacturing the same
JP3613400B2
Electrode and cell having electrode
WO2015064586A1
Winding-type battery
WO2017010042A1
Lithium ion secondary battery, electrode and method for producing same
WO2017163846A1
Cited By
Electrode and secondary battery
WO2026191390A1