Positive electrode active material for secondary battery, and secondary battery
By controlling the particle size distribution of lithium metal composite oxides and incorporating elements like Ti and fluorine, the challenges of achieving high capacity and stability in secondary batteries are addressed, resulting in batteries with enhanced energy density and reduced cycle deterioration.
Patent Information
- Application Number
- PCT/JP2024/015360
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-31
AI Technical Summary
Lithium metal composite oxides with a rock salt structure used in secondary batteries face challenges in achieving high capacity and maintaining cycle characteristics due to particle size control issues during synthesis, leading to side reactions and capacity deterioration.
The use of lithium metal composite oxides with a rock salt type crystal structure, specifically with a D50 particle size distribution of 0.05 μm to 10 μm, achieved by pulverizing highly hard particles synthesized through firing, to enhance electrode capacity and reduce cycle deterioration, along with the inclusion of elements like Ti and fluorine to stabilize the structure and increase discharge potential.
This approach results in secondary batteries with improved high energy density and reduced cycle deterioration, allowing for higher discharge capacity and more stable rock salt-type crystal structures, even after repeated charging and discharging.
Smart Images

Figure JP2024015360_31102024_PF_FP_ABST
Abstract
Description
Positive electrode active material for secondary battery and secondary battery
[0001] The present disclosure relates to a positive electrode active material for a secondary battery and a secondary battery.
[0002] Secondary batteries, especially lithium-ion secondary batteries, have high power output and high energy density, and are expected to be used in small consumer applications, power storage devices, and electric vehicles. The cathode active material of lithium-ion secondary batteries is a composite oxide of lithium and a transition metal (e.g., cobalt). Replacing part of the cobalt with nickel can increase the battery capacity.
[0003] On the other hand, in recent years, in response to the demand for high energy density, the rock salt structure Li 1+x Mn 1-x O 2 Li-excess lithium metal composite oxides based on the above have been attracting attention.
[0004] Patent Document 1 describes a compound having a crystal structure belonging to the space group Fm-3m and having the composition formula Li 1+x Nb y Me z A p O 2 (Me is a transition metal including Fe and / or Mn, 0<x<1, 0<y<0.5, 0.25≦z<1, A is an element other than Nb and Me, 0≦p≦0.2, provided that Li 1+p Fe 1-q Nb q O 2 and excluding those in which 0.15<p≦0.3 and 0<q≦0.3), a positive electrode active material containing a lithium transition metal composite oxide represented by the formula (2) is disclosed.
[0005] Patent No. 6197029 specification
[0006] In Patent Document 1, high capacity is possible by controlling the composition (i.e., by adding Nb), but the effect of improving capacity is insufficient, and there is still room for improvement.
[0007] In view of the above, one aspect of the present disclosure relates to a positive electrode active material for a secondary battery, comprising a lithium metal composite oxide having a rock-salt crystal structure assignable to the space group Fm-3m, the lithium metal composite oxide containing at least Li and Mn, and having a D50 in a volume-based cumulative particle size distribution of the lithium metal composite oxide of 0.05 μm or more and 10 μm or less.
[0008] Another aspect of the present disclosure relates to a secondary battery including a positive electrode, a negative electrode, an electrolyte, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode includes the above-described positive electrode active material for a secondary battery.
[0009] According to the present disclosure, a secondary battery with high energy density can be realized.
[0010] The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.
[0011] 1 is a schematic perspective view of a secondary battery according to an embodiment of the present disclosure, in which a portion thereof is cut away; 2 is a graph showing the particle size distribution of the lithium metal composite oxide used in Examples 7 to 10 and Comparative Example 3;
[0012] The following describes embodiments of the present disclosure using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the term "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits for specific physical properties or conditions are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit. When multiple materials are exemplified, one of the materials may be selected and used alone, or two or more materials may be used in combination.
[0013] The present disclosure also encompasses combinations of two or more features arbitrarily selected from the appended claims, i.e., two or more features arbitrarily selected from the appended claims can be combined unless a technical contradiction arises.
[0014] In the following description, the term "comprises" encompasses "contains," "consists essentially of," and "consists of."
[0015] The secondary battery includes at least a non-aqueous electrolyte secondary battery such as a lithium ion battery or a lithium metal secondary battery, and an all-solid-state battery using a solid electrolyte.
[0016] A positive electrode active material for a secondary battery according to an embodiment of the present disclosure includes a lithium metal composite oxide (hereinafter also referred to as "lithium metal composite oxide (Fm)") having a rock salt type crystal structure that can be assigned to the space group Fm-3m. The lithium metal composite oxide (Fm) has a crystal structure based on a rock salt structure that belongs to the space group Fm-3m, and has a crystal structure similar to the rock salt structure represented by NaCl, for example. In such a crystal structure, oxygen atoms are arranged at the anion sites, and Li atoms and metal atoms other than Li can be irregularly arranged at the cation sites.
[0017] The lithium metal composite oxide (Fm) contains at least Li and Mn. 1+x Mn 1-x O 2 The lithium metal composite oxide (Fm) based on this is expected to exhibit high capacity.
[0018] Currently, several reports have been published on the synthesis of lithium metal composite oxides (Fm) at the laboratory level by applying high shear force to a raw material mixture containing a lithium compound and a manganese compound using a stirring device such as a ball mill.
[0019] On the other hand, when mass-producing lithium metal composite oxide (Fm), it is necessary to efficiently synthesize it by calcining a raw material mixture. The particles of lithium metal composite oxide (Fm) synthesized by calcination are usually very hard and lumpy.
[0020] Furthermore, the lithium metal composite oxide (Fm) synthesized by ball milling tends to have a small particle size. Therefore, the surface area contributing to the electrode reaction in the positive electrode active material is large, and side reactions also increase. Therefore, when used as a positive electrode active material for a secondary battery, the cycle characteristics tend to deteriorate. To prevent deterioration in cycle characteristics, the average particle size (meaning the median diameter D50 in the volume-based cumulative particle size distribution) of the lithium metal composite oxide (Fm) is preferably 0.05 μm or more or 0.1 μm or more. However, it is difficult to control the particle size within the above range when synthesized by ball milling.
[0021] By pulverizing the lithium metal composite oxide (Fm) synthesized by calcination, a lithium metal composite oxide (Fm) having a desired particle size distribution and an average particle diameter D50 of 0.05 μm or more can be obtained. By using this lithium metal composite oxide (Fm) as a positive electrode active material, a secondary battery with high discharge capacity and little deterioration in cycle characteristics can be realized.
[0022] In the positive electrode active material for a secondary battery according to an embodiment of the present disclosure, the lithium metal composite oxide (Fm) has a volume-based cumulative particle size distribution D50 of 0.05 μm or more and 10 μm or less. The D50 of the particle size distribution can be controlled within the above range by pulverizing the high-hardness lithium metal composite oxide (Fm) obtained by calcining the raw material mixture under appropriate conditions. Increasing the D50 facilitates increasing the electrode capacity. The D50 is 0.05 μm or more, preferably 0.1 μm or more, and more preferably 0.15 μm or more. The D50 may be 0.2 μm or more. The D50 is 10 μm or less, preferably 1 μm or less, and more preferably 0.8 μm or less, 0.6 μm or less, or 0.5 μm or less. The upper and lower limits of the D50 can be arbitrarily combined.
[0023] Furthermore, the D90 (particle size at which the cumulative volume, calculated from the smallest particle size, accounts for 90% of the total) in the volume-based cumulative particle size distribution of the lithium metal composite oxide (Fm) is preferably 1 μm or more and 10 μm or less, since this facilitates increasing the electrode capacity. The particle size D90 is preferably 1 μm or more, and more preferably 2 μm or more. The particle size D90 is preferably 10 μm or less, and more preferably 8 μm or less. The upper and lower limits of D90 can be combined as desired.
[0024] A laser diffraction particle size measuring device (e.g., "Mastersizer 3000" manufactured by Malvern Panalytical) is used to measure the particle size distribution of the positive electrode active material for secondary batteries. A sample of the positive electrode active material is dispersed in 4 mL of an aqueous solution of sodium hexametaphosphate. Dispersion treatment is performed by ultrasonic treatment for 1 minute. The entire amount of the sample is placed in the device and measured. The concentration of the aqueous solution of sodium hexametaphosphate is 0.02 to 1 mass %.
[0025] When the lithium metal composite oxide (Fm) synthesized by calcination is subjected to a pulverization treatment using a ball mill or the like, the peak in the volumetric particle size distribution shifts to the smaller particle size side and the peak in the volumetric particle size distribution splits, so that two peaks can be observed. As the time required for the pulverization treatment increases, the height of the peak on the smaller particle size side increases and the height of the peak on the larger particle size side decreases.
[0026] When mounted on the positive electrode of a secondary battery, the average particle diameter (median diameter D50 in the cumulative particle size distribution on a volume basis) of the lithium metal composite oxide (Fm) can be measured using particles of the lithium metal composite oxide (Fm) observed in a scanning electron microscope (SEM) image of a cross section in the thickness direction of the positive electrode (hereinafter simply referred to as a "cross-sectional SEM image"). The particles observed in the cross-sectional SEM image of the positive electrode may be cross-sections of particles. The average particle diameter D50 (and D90) can be determined from the cumulative particle size distribution of 100 or more lithium metal composite oxide (Fm) particles (particle cross-sections) arbitrarily selected from the cross-sectional SEM image. An example of a procedure for determining the average D50 value from a cross-sectional SEM image is described below.
[0027] (1) Preparation of a Cross Section of a Positive Electrode First, a positive electrode to be measured is prepared. Typically, a positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the surface of the positive electrode current collector. The positive electrode active material layer and the positive electrode current collector are simultaneously cut along the thickness direction of the positive electrode to form a cross section. At this time, a thermosetting resin may be filled into the positive electrode active material layer and cured. For example, a cross section sample of the positive electrode active material layer may be obtained by a CP (cross section polisher) method, an FIB (focused ion beam) method, or the like.
[0028] The positive electrode to be measured is taken from a secondary battery with a depth of discharge (DOD) of 90% or more. Depth of discharge (DOD) is the ratio of the amount of discharged electricity to the amount of electricity in a fully charged battery. Note that the amount of electricity charged (i.e., the fully charged amount) when a battery in a fully discharged state (DOD = 100%) is charged to a fully charged state (SOC = 100%, DOD = 0%) corresponds to the rated capacity. The voltage of a battery in a fully charged state corresponds to the end-of-charge voltage. The voltage of a battery in a fully discharged state corresponds to the end-of-charge voltage.
[0029] (2) Taking a Cross-Sectional SEM Image Next, a cross-sectional sample of the positive electrode (positive electrode active material layer) is observed using an SEM. Observation using an SEM is performed at a magnification of, for example, 500 to 3000 times. The cross-sectional SEM image is taken so that a region having a length of 30 μm or more (preferably 40 μm or more) in the plane direction of the positive electrode active material layer is observed.
[0030] (3) Image analysis The area of each particle (particle cross section) is measured, and the measured area Sd is used to calculate the diameter Dd (Dd = 8√(Sd / π)) of an equivalent sphere having the average cross-sectional area of the sphere. 3 )) and calculate the cumulative particle size distribution of their diameters (Dd). The particle size distribution based on volume is calculated assuming that each particle is spherical with a diameter Dd. D50 (median diameter) is the diameter of the equivalent sphere when the cumulative volume reaches 50% when integrating the smallest equivalent sphere diameter values. D50 can be selected depending on the electrode design.
[0031] In the image analysis, image analysis software (e.g., ImageJ) may be used. In the image analysis, the cross-sectional SEM image may be binarized so that the lithium metal composite oxide (Fm) particles are black (or white) and the rest are white (or black).
[0032] In the image analysis, elemental analysis may be performed on the cross-sectional SEM image using EDX (energy dispersive X-ray spectroscopy) or EPMA (electron probe microanalyzer). A mapping image of the lithium metal composite oxide (Fm) may then be obtained from the analysis data. Using such a mapping image, a cumulative particle size distribution on a volume basis may be derived based on each of 100 or more arbitrarily selected particles (particle cross sections) of the lithium metal composite oxide (Fm), and D50 may be calculated.
[0033] Because the lithium metal composite oxide (Fm) is hard and sturdy, the volume-based cumulative particle size distribution determined from 100 or more lithium metal composite oxide (Fm) particles (particle cross sections) randomly selected from a cross-sectional SEM image will be similar to the volume-based cumulative particle size distribution determined for the lithium metal composite oxide (Fm) as a raw material powder for an electrode or for the lithium metal composite oxide (Fm) powder separated and recovered from the positive electrode after disassembling a completed battery. The volume-based cumulative particle size distribution of the raw material powder or the powder separated and recovered from the positive electrode can be obtained, for example, by converting the volume-based cumulative particle size distribution measured using a laser diffraction / scattering particle size distribution analyzer.
[0034] The lithium metal composite oxide (Fm) may contain an element M other than Li and Mn. Such an element M may be any electropositive element other than hydrogen, and may also be a metal element (including so-called metalloid elements). In other words, the lithium metal composite oxide (Fm) may be a lithium transition metal composite oxide containing at least three types of metals.
[0035] The element M may be, for example, at least one element selected from the group consisting of Ti, Fe, Ge, Si, Ga, Ni, Co, Sn, Cu, Nb, Mo, Bi, V, Cr, Y, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, Ta, W, La, Ce, Pr, Gd, Sm, Eu, Yb, Dy, Al, and Er. The lithium metal composite oxide (Fm) may contain, as the element M, any two or more elements selected from the above group.
[0036] Even when the lithium metal composite oxide (Fm) contains the element M, it is preferable that the main component of the metal elements other than Li is Mn. The number b of Mn atoms in the lithium metal composite oxide (Fm) may be the largest among the number of atoms of metals other than Li in the lithium metal composite oxide (Fm). The number of Mn atoms may be greater than the total number c of atoms of metal elements excluding Li and Mn. The ratio (b / c) of the number b of Mn atoms to the number c of atoms of metal elements other than Li and Mn in the lithium metal composite oxide (Fm) is, for example, 1 or more and 15 or less, preferably 1 or more and 12 or less, or may be greater than 1 and 12 or less, or may be 2 or more and 12 or less.
[0037] The lithium metal composite oxide (Fm) preferably contains at least Ti as the element M. The lithium metal composite oxide (Fm) containing Ti as the element M can exhibit particularly high capacity. Although the reason for this is not clear, one possible reason is that in the lithium metal composite oxide, Ti has an empty d orbital. 4+ This is thought to be because the crystal structure can exist in the form of a rock-salt salt. In this case, a rock-salt crystal structure with high symmetry, stability, and capacity is thought to be formed. Furthermore, such a rock-salt structure is thought to be less likely to become unstable even after repeated charge and discharge.
[0038] When the lithium metal composite oxide (Fm) contains Ti, the ratio of the number of Mn atoms to the number of Ti atoms in the lithium metal composite oxide (Mn / Ti) may be 4 or more, 5 or more, or 6 or more, and preferably 7 or more. Moreover, Mn / Ti may be 70 or less, 30 or less, and is preferably 15 or less.
[0039] The lithium metal composite oxide (Fm) may contain fluorine (F). Fluorine can substitute oxygen atoms at the anion site in the crystal structure. This stabilizes the crystal structure and provides a higher capacity even when the lithium metal composite oxide (Fm) is in a Li-excess state. Furthermore, the substitution of fluorine atoms increases the average discharge potential. The Li-excess state refers to a state in which the number of Li atoms in the lithium metal composite oxide (Fm) is greater than the total number of atoms of metal elements other than Li.
[0040] In Li-excess lithium metal composite oxides (Fm), the arrangement of Li in the cation sites is irregular, resulting in a variety of Li bonding states. Therefore, the voltage distribution associated with Li release is wide. Therefore, it can be difficult to utilize the low-potential tail of the voltage distribution as capacitance. However, by introducing fluorine atoms, the voltage distribution associated with Li release shifts to the high-potential side, making it easier to utilize the tail as capacitance. This further increases the available capacity.
[0041] Lithium metal composite oxide (Fm) has the composition formula Li a Mn b M c O d F e where 1≦a<1.4, 0.5≦b<0.9, 0≦c≦0.4, 1.33≦d≦2, 0≦e≦0.67, and 1.7≦d+e≦2.2 are satisfied.
[0042] The lithium metal composite oxide (Fm) containing Ti has the composition formula Li a Mn b Ti c1 M 2 c2 O d F e where M 2is the element M other than Ti, and 1≦a≦1.4, 0.3≦b≦0.9, 0<c1≦0.5, 0<c2≦0.25, 0≦e≦0.7, and 1.7≦d+e≦2 are satisfied. Alternatively, 1≦a≦1.4, 0.5≦b≦0.9, 0.02<c1≦0.4, 0≦e≦0.67, and 1.7≦d+e≦2.2 are satisfied. d+e is often 2 or less, and may be 1.94 or less, 1.9 or less, or 1.8 or less.
[0043] As shown in the above composition formula, some of the oxygen atoms in the anion site may be substituted with fluorine atoms. This stabilizes the Li-excess state (a > 1) and provides high capacity. Furthermore, as described above, the average discharge potential increases, further increasing the available capacity.
[0044] The fluorine-free lithium metal composite oxide (Fm) has the composition formula Li a Mn b M c O d Here, the following conditions are satisfied: 1≦a<1.4, 0.5≦b<0.75, 0≦c≦0.35, and 1.6≦d≦2.
[0045] The content of elements constituting the lithium metal composite oxide (Fm) can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0046] (Specific Surface Area) The lithium metal composite oxide (Fm) synthesized in a laboratory by applying high shear force to a raw material mixture using a stirring device such as a ball mill has a very large specific surface area. In contrast, the lithium metal composite oxide (Fm) synthesized by calcination, even if it is in the form of particles or powder obtained by crushing agglomerated particles, does not have a history of shear force high enough to cause a solid-state reaction. Therefore, the specific surface area of the lithium metal composite oxide (Fm) synthesized by calcination is, for example, 0.13 m 2 / g or more 13.2m 2 / g or less, and 2 / g to 10m 2 / g. When the specific surface area is within the above range, it is advantageous in that the loading rate of the lithium metal composite oxide (Fm) in the positive electrode can be increased and side reactions can be easily suppressed. If the specific surface area is excessively large, the surface state becomes unstable, making it difficult to suppress side reactions.
[0047] The specific surface area may be measured using the lithium metal composite oxide (Fm) as a raw material powder before it is made into a positive electrode, or may be measured using the lithium metal composite oxide (Fm) separated from the positive electrode. Either method will provide roughly similar measurement results.
[0048] Here, the specific surface area of the lithium metal composite oxide (Fm) is measured by taking 0.20 g to 0.25 g of a lithium metal composite oxide (Fm) sample, placing the sample in a measurement cell composed of a glass tube for specific surface area measurement, and then drying and degassing the measurement cell. The drying and degassing is performed for at least one hour at a pressure of 6.67 Pa and a temperature of 250°C ± 5°C. The mass of the sample in the measurement cell is then measured to the nearest 0.1 mg. The amount of nitrogen adsorption of the sample at a temperature of -196°C is then measured using a specific surface area measurement device. For example, a Shimadzu Corporation automatic specific surface area / pore distribution measurement device, "Tristar II 3020," is used as the measurement device. From the measurement results of the adsorption amount, the specific surface area of the lithium metal composite oxide (Fm) is determined using the BET multipoint method within a partial pressure (relative pressure) range of 0.001 to 0.2.
[0049] <Method for Producing Lithium Metal Composite Oxide (Fm)> The method for producing the lithium metal composite oxide (Fm) is not limited, but it is desirable to obtain it by firing a raw material mixture of elements that constitute the lithium metal composite oxide (Fm). The firing promotes the growth of crystals similar to a rock salt structure belonging to the space group Fm-3m, and a lithium metal composite oxide with a large crystallite size is obtained. The crystallite size may then be controlled to a desired range by performing a pulverization treatment.
[0050] As raw materials for the elements constituting the lithium metal composite oxide, Mn compounds, compounds of element M, lithium compounds, fluorine compounds, titanium compounds, etc. may be arbitrarily selected and used. The types and mixing ratios of the raw materials may be appropriately selected depending on the desired composition described above.
[0051] Examples of Mn compounds include MnO 2 , Mn 2 O 3 Examples of compounds of element M include M salts such as oxides, oxyfluorides, and hydroxides. Examples of lithium compounds include Li 2 Lithium oxides such as O, lithium carbonate (Li 2 CO 3 ), LiOH, lithium manganese oxide (LiMnO 2 Examples of the fluorine compounds include fluorine salts such as lithium fluoride (LiF). Examples of the titanium compounds include TiO 2 and titanium salts such as lithium titanate.
[0052] The atmosphere for firing the raw material mixture may vary depending on the composition of the lithium metal composite oxide (Fm) to be obtained and the types of raw materials, but may be, for example, an oxidizing atmosphere (e.g., in air or in the presence of oxygen).It is desirable to circulate the atmospheric gas.
[0053] The firing temperature of the raw material mixture may vary depending on the composition of the lithium metal composite oxide (Fm) to be obtained and the types of raw materials, but may be, for example, 700°C or higher, and is preferably 900°C or higher and 1300°C or lower.
[0054] When the lithium metal composite oxide (Fm) obtained by firing is in the form of aggregated particles, the aggregated particles may be pulverized to a desired aspect ratio or circularity using a stirring device capable of applying a large shear force to particles, such as a ball mill or a bead mill.
[0055] There are various methods for controlling particle shape, and they are not limited to methods that involve crushing agglomerated particles. For example, the raw material mixture may be fired while stirring the raw material mixture. For example, the raw material mixture may be fired while stirring using a firing furnace equipped with a fluidized bed. Furthermore, particles that are nearly spherical may be used as part of the raw material. For example, a manganese compound or a manganese-titanium composite compound that is nearly spherical may be used as the raw material.
[0056] Next, a secondary battery according to an embodiment of the present disclosure will be described in detail. The secondary battery includes, for example, a positive electrode, a negative electrode, an electrolyte, and a separator as described below.
[0057] [Positive Electrode] The positive electrode comprises a positive electrode current collector and a positive electrode mixture layer formed on the surface of the positive electrode current collector and containing a positive electrode active material. The above-mentioned positive electrode for a secondary battery is used as the positive electrode. The positive electrode mixture layer can be formed, for example, by applying a positive electrode slurry, in which a positive electrode mixture containing a positive electrode active material, a binder, etc. is dispersed in a dispersion medium, to the surface of the positive electrode current collector and drying it. The dried coating may be rolled as necessary. The positive electrode mixture layer may be formed on one surface or both surfaces of the positive electrode current collector.
[0058] The positive electrode mixture layer contains a positive electrode active material as an essential component, and may contain, as optional components, a binder, a thickener, a conductive agent, a positive electrode additive, etc. Known materials can be used as the binder, thickener, and conductive agent.
[0059] The positive electrode active material includes the aforementioned lithium metal composite oxide (Fm) having a crystal structure similar to a rock salt structure belonging to the space group Fm-3m. The lithium metal composite oxide (Fm) is, for example, a secondary particle formed by agglomeration of a plurality of primary particles. The particle size of the primary particles is generally 0.01 μm to 1 μm.
[0060] The lithium metal composite oxide (Fm) may be mixed with other known lithium metal oxides and used as a positive electrode active material. Examples of other known lithium metal oxides include Li a CoO2, Li a NiO2, Li a MnO2, Li a Co b Ni 1-b O2, Li a Co b M 1-b O c , Li a Ni 1-b M b O c , Li a Mn2O4, Li a Mn 2-b M bO 4、 LiMePO 4、 Examples of lithium transition metal composite oxides include Li2MePO4F. Here, M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B. Me contains at least a transition element (e.g., at least one selected from the group consisting of Mn, Fe, Co, and Ni). Here, 0≦a≦1.2, 0≦b≦0.9, and 2.0≦c≦2.3. The value a, which indicates the molar ratio of lithium, increases or decreases with charge and discharge.
[0061] The shape and thickness of the positive electrode current collector can be selected from the shape and range corresponding to those of the negative electrode current collector. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloy, and titanium.
[0062] [Negative Electrode] The negative electrode may include, for example, a negative electrode current collector and a negative electrode active material layer formed on the surface of the negative electrode current collector. The negative electrode active material layer can be formed, for example, by applying a negative electrode slurry, in which a negative electrode mixture containing a negative electrode active material, a binder, etc. is dispersed in a dispersion medium, to the surface of the negative electrode current collector and drying the slurry. The dried coating may be rolled as necessary. In other words, the negative electrode active material may be a mixture layer. Alternatively, a lithium metal foil or a lithium alloy foil may be attached to the negative electrode current collector. The negative electrode active material layer may be formed on one surface or both surfaces of the negative electrode current collector.
[0063] The negative electrode active material layer contains a negative electrode active material as an essential component, and may contain optional components such as a binder, a conductive agent, a thickener, etc. Known materials can be used as the binder, conductive agent, and thickener.
[0064] Examples of negative electrode active materials include materials that electrochemically absorb and release lithium ions, lithium metal, and lithium alloys. Examples of materials that electrochemically absorb and release lithium ions include carbon materials and alloy-based materials. Examples of carbon materials include graphite, easily graphitized carbon (soft carbon), and hardly graphitized carbon (hard carbon). Of these, graphite is preferred because of its excellent charge / discharge stability and low irreversible capacity. Examples of alloy-based materials include those containing at least one metal that can form an alloy with lithium. For example, a lithium ion conductive phase and a composite material in which a silicon phase is dispersed in the lithium ion conductive phase may be used.
[0065] The negative electrode current collector may be a non-porous conductive substrate (such as a metal foil) or a porous conductive substrate (such as a mesh, net, or punched sheet). Examples of the material for the negative electrode current collector include stainless steel, nickel, nickel alloys, copper, and copper alloys.
[0066] [Electrolyte] The electrolyte may be a liquid electrolyte (electrolytic solution), a gel electrolyte, or a solid electrolyte. The liquid electrolyte is, for example, an electrolytic solution containing a non-aqueous solvent and a salt dissolved in the non-aqueous solvent. The concentration of the salt in the electrolytic solution is, for example, 0.5 mol / L or more and 2 mol / L or less. The electrolytic solution may contain known additives.
[0067] The gel electrolyte contains a salt and a matrix polymer, or a salt, a non-aqueous solvent, and a matrix polymer. The matrix polymer is, for example, a polymer material that absorbs the non-aqueous solvent and gels. Examples of the polymer material include fluororesin, acrylic resin, polyether resin, and polyethylene oxide.
[0068] As the solid electrolyte, for example, a material known in all-solid-state lithium ion secondary batteries (for example, oxide-based solid electrolytes, sulfide-based solid electrolytes, halide-based solid electrolytes, etc.) can be used.
[0069] For example, a liquid non-aqueous electrolyte is prepared by dissolving a salt in a non-aqueous solvent. The salt is an electrolyte salt that ionizes in the electrolyte, and may include, for example, a lithium salt. The electrolyte may contain various additives. The electrolyte is usually used in its liquid state, but its fluidity may be limited by a gelling agent or the like.
[0070] Examples of non-aqueous solvents that can be used include cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, and chain carboxylic acid esters. Examples of cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC). Examples of chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL) and γ-valerolactone (GVL). Examples of chain carboxylic acid esters include methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP). One type of non-aqueous solvent may be used alone, or two or more types may be used in combination.
[0071] Examples of lithium salts include lithium salts of chlorine-containing acids (LiClO4, LiAlCl4, LiB 10 Cl 10 etc.), lithium salts of fluorine-containing acids (LiPF6, LiPF 2 O 2 , LiBF4, LiSbF6, LiAsF6, LiCF3SO3, LiCF3CO2, etc.), lithium salts of fluorine-containing acid imides (LiN(FSO2)2, LiN(CF3SO2)2, LiN(CF3SO2)(CF4F9SO2), LiN(CF5SO2)2, etc.), lithium halides (LiCl, LiBr, LiI, etc.), etc., can be used. One type of lithium salt may be used alone, or two or more types may be used in combination.
[0072] The concentration of the lithium salt in the electrolyte may be 1 mol / L or more and 2 mol / L or less, or 1 mol / L or more and 1.5 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte having excellent ionic conductivity and appropriate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.
[0073] [Separator] A separator is interposed between the positive electrode and the negative electrode. The separator has high ion permeability and adequate mechanical strength and insulating properties. The separator can be made of a microporous thin film, woven fabric, nonwoven fabric, or the like. The separator is preferably made of polyolefin such as polypropylene or polyethylene.
[0074] An example of the structure of a secondary battery is a structure in which an electrode group formed by winding a positive electrode and a negative electrode with a separator interposed therebetween and a non-aqueous electrolyte are housed in an outer casing. Alternatively, instead of a wound electrode group, other types of electrode groups may be used, such as a stacked electrode group formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween. The secondary battery may be in any shape, such as a cylindrical shape, a prismatic shape, a coin shape, a button shape, or a laminate shape.
[0075] FIG. 1 is a schematic perspective view, partially cut away, of a prismatic secondary battery according to an embodiment of the present disclosure. The battery includes a bottomed prismatic battery case 4, an electrode group 1, and a nonaqueous electrolyte (not shown) housed within the battery case 4. The electrode group 1 includes a long, strip-shaped negative electrode, a long, strip-shaped positive electrode, and a separator interposed therebetween. The negative electrode current collector is electrically connected to a negative electrode terminal 6 provided on a sealing plate 5 via a negative electrode lead 3. The negative electrode terminal 6 is insulated from the sealing plate 5 by a resin gasket 7. The positive electrode current collector is electrically connected to the back surface of the sealing plate 5 via a positive electrode lead 2. That is, the positive electrode is electrically connected to the battery case 4, which also serves as the positive electrode terminal. The periphery of the sealing plate 5 fits into the open end of the battery case 4, and the fitting is laser-welded. The sealing plate 5 has an injection hole for the nonaqueous electrolyte, which is closed with a seal plug 8 after injection.
[0076] The secondary battery may have a cylindrical, coin, or button shape with a metal battery case, or may be a laminated battery with a battery case made of a laminate sheet that is a laminate of a barrier layer and a resin sheet. In the present disclosure, the type, shape, etc. of the secondary battery are not particularly limited.
[0077] (Additional Notes) The above embodiments disclose the following technologies. (Technology 1) A positive electrode active material for a secondary battery, comprising a lithium metal composite oxide having a rock-salt crystal structure assignable to space group Fm-3m, the lithium metal composite oxide containing at least Li and Mn, and D50 in a volume-based cumulative particle size distribution of the lithium metal composite oxide being 0.05 μm or more and 10 μm or less. (Technology 2) A positive electrode active material for a secondary battery according to Technology 1, in which a ratio b / c of the number of Mn atoms b to the number of atoms c of metal elements other than Li and Mn in the lithium metal composite oxide is 1 or more and 15 or less. (Technology 3) A positive electrode active material for a secondary battery according to Technology 1 or 2, in which the lithium metal composite oxide contains fluorine. (Technology 4) The lithium metal composite oxide is a positive electrode active material for a secondary battery, comprising a lithium metal composite oxide having a composition formula Li a Mn b M c O d F eThe positive electrode active material for a secondary battery according to any one of Techniques 1 to 3, wherein M contains at least one element excluding Li and Mn, and satisfies 1≦a<1.4, 0.5≦b<0.9, 0≦c≦0.4, 1.33≦d≦2, 0≦e≦0.67, and 1.7≦d+e≦2. (Technology 5) The positive electrode active material for a secondary battery according to Technique 4, wherein the lithium metal composite oxide contains at least Ti as M. (Technology 6) The positive electrode active material for a secondary battery according to Technology 4 or 5, wherein the M comprises at least one selected from the group consisting of Ti, Fe, Ge, Si, Ga, Ni, Co, Sn, Cu, Nb, Mo, Bi, V, Cr, Y, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, Ta, W, La, Ce, Pr, Gd, Sm, Eu, Yb, Dy, Al, and Er. (Technology 7) The positive electrode active material for a secondary battery according to any one of Technology 1 to 6, wherein the lithium metal composite oxide has a volume-based cumulative particle size distribution D90 of 1 μm or more and 10 μm or less. (Technology 8) A secondary battery comprising a positive electrode, a negative electrode, an electrolyte, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode comprises the positive electrode active material for a secondary battery according to any one of Technology 1 to 7.
[0078] Hereinafter, the present disclosure will be specifically described based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0079] Examples 1 to 10 [Fabrication of Positive Electrode] Manganese oxide (Mn 2 O 3 ), lithium carbonate (Li 2 CO 3 ) and titanium oxide (TiO 2 The raw material mixture containing Li was fired at 950°C for 10 hours. a Mn b M c O d Agglomerated particles of Li-excess lithium metal composite oxide (Fm) were obtained, satisfying the following conditions: 1<a<1.4, 0.5≦b<0.75, 0.1<c≦0.4, 1.6≦d≦2. The composition of the lithium metal composite oxide (Fm) was identified by analyzing it using ICP atomic emission spectrometry.
[0080] The obtained agglomerated particles of lithium metal composite oxide (Fm) were pulverized under various conditions using a planetary ball mill to obtain lithium metal composite oxides (Fm) with different average particle diameters D50.
[0081] In Example 1, the aggregated particles of lithium metal composite oxide (Fm) were milled in a planetary ball mill (Fritsch Premium-Line P7, rotation speed: 300 rpm, container: 45 mL, ball: φ3 mm ZrO 2 The mixture was placed in a ball mill (made of stainless steel) and treated in an air atmosphere at room temperature for 1 hour. In Examples 2 to 6, the ball mill treatment time was changed from 1 hour in Example 1 to 2 hours, 3 hours, 6 hours, 12 hours, and 24 hours, respectively.
[0082] In Examples 7 to 10, the rotation speed of the planetary ball mill was changed to 150 rpm. The ball mill treatment time was 3 hours in Example 7, 6 hours in Example 8, 12 hours in Example 9, and 24 hours in Example 10.
[0083] The particle size distribution of the pulverized lithium metal composite oxide (Fm) was measured using a laser diffraction / scattering particle size measuring device, and the average particle diameter D50 and particle compaction D90 at which the cumulative volume of the particles reached 50% and 90%, respectively, were determined. An aqueous solution of sodium hexametaphosphate was used as the dispersion medium.
[0084] Furthermore, the X-ray diffraction pattern of the pulverized lithium metal composite oxide (Fm) was measured and analyzed. From the number and positions of XRD peaks, it was confirmed that the lithium metal composite oxide (Fm) had a rock salt type crystalline structure that could be assigned to the space group Fm-3m.
[0085] In addition, as a result of elemental analysis by ICP-AES, the composition of the lithium metal composite oxide (Fm) in Examples 1 to 10 was Li 1.21 Mn 0.61 Ti 0.175 O 1.78 was identified as follows.
[0086] The resulting lithium metal composite oxide (Fm), acetylene black, and polyvinylidene fluoride were mixed in a solids mass ratio of 7:2:1, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode slurry. The positive electrode slurry was then applied to a positive electrode current collector made of aluminum foil, the coating was dried and compressed, and then cut to a predetermined electrode size to obtain a positive electrode.
[0087] [Preparation of Electrolyte] A non-aqueous electrolyte was prepared by adding LiPF6 as a lithium salt to a mixed solvent prepared by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) at a predetermined volume ratio.
[0088] [Preparation of Test Cell] A test cell was prepared using the above-described positive electrode and a negative electrode counter electrode made of lithium metal foil. The above-described positive electrode and negative electrode counter electrode were arranged opposite each other with a separator interposed therebetween to form an electrode assembly, and the electrode assembly was housed in a coin-shaped outer can. After injecting an electrolyte into the outer can, the outer can was sealed to obtain a coin-shaped test secondary battery.
[0089] [Evaluation] (Discharge Capacity) The secondary battery was charged at a constant current of 0.1 C under room temperature conditions up to a battery voltage of 4.95 V, and then further charged at a constant voltage of 4.95 V until the current reached 0.01 C. After a 20-minute pause, the battery was discharged at a constant current of 0.1 C down to a battery voltage of 2.5 V, and the discharge capacity was measured. The discharge capacity C per mass of the lithium metal composite oxide (Fm) was 1 (mAh / g) was evaluated.
[0090] <Comparative Example 1> In the production of a positive electrode, a spinel structure Li 2 MnO 4 was prepared as a positive electrode active material, and acetylene black and polyvinylidene fluoride were mixed with this in a solid content mass ratio of 7:2:1, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode slurry. A positive electrode was fabricated in the same manner as in Example 1 except for this, and a secondary battery was obtained. The obtained secondary battery was evaluated in the same manner as in Example 1.
[0091] <Comparative Example 2> In the preparation of the positive electrode, the pulverization treatment using a planetary ball mill was not performed, and the agglomerated particles of the lithium metal composite oxide (Fm) were pulverized in an agate mortar and then sieved through a 75 μm sieve to obtain a powder of the lithium metal composite oxide (Fm). The average particle diameter D50 of the obtained powder of the lithium metal composite oxide (Fm) was measured in the same manner as in Example 1. Furthermore, as a result of the XRD measurement and ICP-AES analysis, the composition of the lithium metal composite oxide (Fm) was found to be Li 1.21 Mn 0.61 Ti 0.175 O 1.78 It was confirmed that the crystal structure was a rock salt type that could be assigned to the space group Fm-3m.
[0092] This lithium metal composite oxide (Fm) powder was mixed with acetylene black and polyvinylidene fluoride in a solid content mass ratio of 7:2:1, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode slurry. A positive electrode was fabricated and a secondary battery was obtained in the same manner as in Example 1 except for this. The obtained secondary battery was evaluated in the same manner as in Example 1.
[0093] Comparative Example 3 In the production of the positive electrode, titanium oxide (TiO 2 ) and lithium oxide (Li 2 O) and lithium manganese oxide (LiMnO 2 The mixed powder was charged into a planetary ball mill (Fritsch Premium-Line P7, rotation speed: 600 rpm, container: 45 mL, ball: φ5 mm Zr ball) and processed in an Ar atmosphere at room temperature for 35 hours (35 cycles of 1 hour operation followed by 10 minutes of rest) to obtain a powder of the composition formula Li 1.2 Mn 0.6 Ti 0.1 O 2 A lithium transition metal composite oxide (Fm) represented by the following formula was obtained.
[0094] The average particle sizes D50 and D90 of the obtained lithium composite oxide (Fm) powder were measured in the same manner as in Example 1. The average particle size D50 was 0.83 μm, and the D90 was 20 μm. Furthermore, measurement and analysis of the X-ray diffraction pattern confirmed that the obtained lithium composite oxide (Fm) had a rock salt-type crystal structure that could be assigned to the space group Fm-3m.
[0095] The evaluation results are shown in Table 1. Table 1 also shows the discharge capacity C 1 The values of D50 and D90 are shown together with the average particle diameters D50 and D90 of the positive electrode active material (lithium metal composite oxide (Fm)) used. In Table 1, A1 to A10 correspond to Examples 1 to 10, respectively, and B1 and B2 correspond to Comparative Examples 1 and 2, respectively.
[0096]
[0097] Figure 2 shows the volumetric particle size distribution and cumulative particle size distribution of the lithium metal composite oxides (Fm) synthesized in Examples 7 to 10 and Comparative Example 3. In Figure 2, B3 corresponds to the comparative example. As shown in Figure 2, the lithium metal composite oxide of Comparative Example 3 (B3), which was synthesized by ball milling without sintering the raw material mixture, has a particle size distribution in the range exceeding 10 μm, and the particle size distribution is broad. As a result, D90 is larger than that of the lithium metal composite oxides of Examples 1 to 10, which were synthesized by sintering.
[0098] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.
[0099] The positive electrode active material for a secondary battery according to the present disclosure can provide a secondary battery with high energy density. The secondary battery according to the present disclosure is useful as a main power source for mobile communication devices, portable electronic devices, and the like.
[0100] 1: electrode group, 2: positive electrode lead, 3: negative electrode lead, 4: battery case, 5: sealing plate, 6: negative electrode terminal, 7: gasket, 8: sealing plug
Claims
1. A positive electrode active material for a secondary battery, comprising a lithium metal composite oxide having a rock-salt type crystal structure that can be assigned to the space group Fm-3m, the lithium metal composite oxide containing at least Li and Mn, and a D50 in a volume-based cumulative particle size distribution of the lithium metal composite oxide being 0.05 μm or more and 10 μm or less.
2. The positive electrode active material for a secondary battery according to claim 1, wherein the ratio b / c of the number of Mn atoms b to the number of atoms c of metal elements other than Li and Mn in the lithium metal composite oxide is 1 or more and 15 or less.
3. The positive electrode active material for a secondary battery according to claim 1, wherein the lithium metal composite oxide contains fluorine.
4. The lithium metal composite oxide has the composition formula Li a Mn b M c O d F e 2. The positive electrode active material for a secondary battery according to claim 1 , wherein M contains at least one element excluding Li and Mn, and satisfies the following conditions: 1≦a<1.4, 0.5≦b<0.9, 0≦c≦0.4, 1.33≦d≦2, 0≦e≦0.67, and 1.7≦d+e≦2.
5. The positive electrode active material for a secondary battery according to claim 4, wherein the lithium metal composite oxide contains at least Ti as the M.
6. The positive electrode active material for a secondary battery according to claim 4, wherein M includes at least one selected from the group consisting of Ti, Fe, Ge, Si, Ga, Ni, Co, Sn, Cu, Nb, Mo, Bi, V, Cr, Y, Zr, Zn, Na, K, Ca, Mg, Pt, Au, Ag, Ru, Ta, W, La, Ce, Pr, Gd, Sm, Eu, Yb, Dy, Al, and Er.
7. The positive electrode active material for a secondary battery according to any one of claims 1 to 6, wherein the lithium metal composite oxide has a volume-based cumulative particle size distribution D90 of 1 µm or more and 10 µm or less.
8. A secondary battery comprising a positive electrode, a negative electrode, an electrolyte, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode contains the positive electrode active material for secondary batteries according to any one of claims 1 to 6.
Citation Information
Patent Citations
Active materials for non-aqueous electrolyte storage devices
JP6197029B2
High-entropy positive electrode material and preparation method and application thereof
CN115394985A
Method for producing lithium metal complex oxide powder
JP2020158335A
Positive electrode active material for lithium ion secondary battery and lithium ion secondary battery
JP2021051880A
Positive electrode active material for lithium secondary battery and method for producing same
JP2023511032A