Blank, method for manufacturing structural member, and structural member

The hot stamping blank with varying aluminum plating amounts on steel plates of different thicknesses addresses non-uniform hardenability and dimensional issues in hot stamping, enhancing the performance and accuracy of annular structural members by ensuring rapid temperature increase and extended high-temperature holding.

WO2024225328A1PCT designated stage expired Publication Date: 2024-10-31NIPPON STEEL CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016111
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

In hot stamping processes for manufacturing structural members, such as automobile body components, the integration of steel plates with different thicknesses can lead to non-uniform hardenability and dimensional accuracy issues, resulting in reduced shock absorption performance and increased risk of twisting and dimensional inaccuracies, especially in large annular structural members.

Method used

A hot stamping blank is designed with a plurality of steel plates arranged to form an annular shape, where the first steel plate has the smallest thickness and a second steel plate has a greater thickness, both with aluminum-based plating layers. The amount of aluminum plating on the first steel plate is less than on the second, allowing for rapid temperature increase and extended high-temperature holding, which delays ferrite transformation and improves hardenability, ensuring uniform hardness and reduced stress non-uniformity.

Benefits of technology

This configuration enhances the hardenability and uniformity of the structural member, improving shock absorption performance, reducing twisting, and maintaining dimensional accuracy, even in large annular structural members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016111_31102024_PF_FP_ABST
    Figure JP2024016111_31102024_PF_FP_ABST
Patent Text Reader

Abstract

This blank (20, 20A, 20B, 20C) for hot stamping is provided with a plurality of steel sheets. The plurality of steel sheets are arranged so as to have an annular shape in a plan view of the blank (20, 20A, 20B, 20C), and are bonded to each other. The plurality of steel sheets include steel sheets (21, 22). The first steel sheet (21) has a minimum sheet thickness (tmin). The sheet thickness of the second steel sheet (22) is larger than the sheet thickness (tmin) of the first steel sheet (21). The steel sheets (21, 22) are plated steel sheets that have base steel sheets (21a, 22a) and aluminum-based plating layers (21b, 22b). The adhesion amount (W1) of the plating layer (21b) in the first steel sheet (21) is less than the adhesion amount (W2) of the plating layer (22b) in the second steel sheet (22).
Need to check novelty before this filing date? Find Prior Art

Description

Blank, manufacturing method of structural member, and structural member

[0001] The present disclosure relates to a blank for hot stamping, a method for manufacturing a structural member using the blank, and the structural member.

[0002] Structures such as automobile bodies are formed from multiple structural members. Structural members are manufactured, for example, by press-forming a blank. To ensure high strength and good dimensional accuracy, structural members are sometimes manufactured by a press-forming method called hot stamping. Hot stamping is a technique in which a blank, which is a steel plate, is heated to a temperature in the austenite range, and then press-formed using a die. The blank is then held in the die and quenched by removing heat (rapid cooling).

[0003] Patent Document 1 discloses an overlapping blank for hot stamping. The overlapping blank in Patent Document 1 includes a first steel sheet and a second steel sheet having an area smaller than that of the first steel sheet. The second steel sheet is overlapped on the surface of the first steel sheet and welded to the first steel sheet. Both the first steel sheet and the second steel sheet are aluminum-plated steel sheets, and the coating weight of the plating layer on both surfaces is 20 g / m. 2 120g / m or more 2 When the average coating weight of the aluminum-based plating layer on both surfaces of the first steel sheet is W1, the coating weight of the aluminum-based plating layer on the surface of the second steel sheet not in contact with the first steel sheet is W2, the sheet thickness of the first steel sheet is t1, and the sheet thickness of the second steel sheet is t2, the overlapping blank of Patent Document 1 satisfies the following conditions: 30≦(W1−W2)≦100, and (W1 / W2) 2 × (t1 / t2) ≥ 1.5 is satisfied. According to Patent Document 1, by satisfying these relationships, it is possible to quickly progress the alloying reaction of the coating layer, which increases the emissivity during heating in hot stamping, to the surface in the overlapping portion between the first steel sheet and the second steel sheet.

[0004] Patent Document 2 discloses a method for manufacturing an automobile body side structural frame from a plurality of blanks. In Patent Document 2, the plurality of blanks are joined to form a composite blank, and the composite blank is press-formed to manufacture the body side structural frame. Patent Document 2 also describes hot forming (hot stamping) the composite blank.

[0005] Patent No. 6642777 Publication Special Publication No. 2021-528248

[0006] In recent years, integrating two or more components from the blank stage has been considered to simplify the manufacturing process of structures. Patent Document 2, for example, discloses a method of hot stamping a composite blank having an annular shape in a plan view to form an annular body side structural frame integrated with pillars, rockers, and the like. However, if the composite blank contains steel sheets of different thicknesses, the performance of the resulting structural component may be degraded. Specifically, during hot stamping, the blank is heated, for example, in a heating furnace until its microstructure is austenitized, and then formed using a die. However, because thinner steel sheets are more easily cooled than thicker steel sheets, the portions of the blank where the thinner steel sheets are located may begin to transform to ferrite before the blank is removed from the heating furnace and forming begins, potentially resulting in poor hardenability. Partially degraded hardenability of the blank may result in non-uniform hardness in the structural component formed from the blank, potentially reducing its impact absorption performance. Furthermore, partial degraded hardenability may result in non-uniform stress in the structural component. This can lead to twisting, particularly in the case of annular structural members, and can lead to a deterioration in dimensional accuracy. The deterioration in impact absorption performance (crash resistance performance) due to deterioration in hardenability or dimensional accuracy becomes more pronounced as the annular structural member becomes larger.

[0007] An object of the present disclosure is to provide a hot stamping blank that can improve the performance of an annular structural component, particularly a large annular structural component, when the component is formed from a steel plate having a thickness smaller than that of other steel plates.

[0008] A hot stamping blank according to the present disclosure includes a plurality of steel sheets. The plurality of steel sheets are arranged and joined to form an annular shape in a plan view of the blank. The plurality of steel sheets include a first steel sheet and a second steel sheet. The first steel sheet has the smallest sheet thickness among the plurality of steel sheets. The second steel sheet has a sheet thickness greater than that of the first steel sheet. The first steel sheet and the second steel sheet are each plated steel sheets. The plated steel sheet has a base steel sheet and an aluminum-based plating layer. The aluminum-based plating layer covers both surfaces of the base steel sheet. The coating weight (g / m) of the aluminum-based plating layer on the first steel sheet relative to both surfaces of the base steel sheet is 2 ) is the coating weight (g / m) of the aluminum-based plating layer on both surfaces of the base steel sheet in the second steel sheet. 2 ) less than

[0009] According to the hot stamping blank of the present disclosure, when an annular structural component, particularly a large annular structural component, is formed using a steel plate having a smaller plate thickness than other steel plates, the performance of the component can be improved.

[0010] FIG. 1 is a plan view of a structural member according to the first embodiment. FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1. FIG. 3A is a schematic view illustrating a method for manufacturing a structural member according to the first embodiment, showing a blank according to the first embodiment. FIG. 3B is a schematic view illustrating a method for manufacturing a structural member according to the first embodiment, showing a blank according to the first embodiment. FIG. 3C is a schematic view illustrating a method for manufacturing a structural member according to the first embodiment, showing a blank according to the first embodiment. FIG. 3D is a schematic view illustrating a method for manufacturing a structural member according to the first embodiment, showing a blank according to the first embodiment. FIG. 3E is a schematic view illustrating a method for manufacturing a structural member according to the first embodiment. FIG. 3F is a schematic view illustrating a method for manufacturing a structural member according to the first embodiment. FIG. 3G is a schematic view illustrating a method for manufacturing a structural member according to the first embodiment. FIG. 4A is a cross-sectional view of a structural member manufactured by the manufacturing method according to the first embodiment. FIG. 4B is another cross-sectional view of a structural member manufactured by the manufacturing method according to the first embodiment. FIG. 4C is yet another cross-sectional view of a structural member manufactured by the manufacturing method according to the first embodiment. FIG. 5 is a plan view of a blank according to a second embodiment. FIG. 6 is a cross-sectional view taken along line VI-VI of FIG. 5 . FIG. 7 is a plan view of a structural member according to a second embodiment. FIG. 8 is a cross-sectional view of a blank according to a third embodiment. FIG. 9 is a cross-sectional view of a blank according to a fourth embodiment. FIG. 10 is a plan view of a structural member according to a modified example of each embodiment. FIG. 11A is a diagram showing a division pattern of a structural member in the first example. FIG. 11B is a diagram showing another division pattern of a structural member in the first example. FIG. 11C is a diagram showing yet another division pattern of a structural member in the first example. FIG. 11D is a diagram showing yet another division pattern of a structural member in the first example. FIG. 11E is a diagram showing yet another division pattern of a structural member in the first example. FIG. 11F is a diagram showing yet another division pattern of a structural member in the first example. FIG. 11G is a diagram showing yet another division pattern of a structural member in the first example. FIG. 12A is a diagram showing a division pattern of a structural member in the second example. FIG. 12B is a diagram showing another division pattern of a structural member in the second example.Figure 12C is a diagram showing yet another division pattern of the structural member in the second embodiment. Figure 12D is a diagram showing yet another division pattern of the structural member in the second embodiment.

[0011] A hot stamping blank according to an embodiment includes a plurality of steel sheets. The plurality of steel sheets are arranged and joined to form an annular shape in a plan view of the blank. The plurality of steel sheets include a first steel sheet and a second steel sheet. The first steel sheet has the smallest thickness among the plurality of steel sheets. The second steel sheet has a thickness greater than that of the first steel sheet. The first steel sheet and the second steel sheet are each plated steel sheets. The plated steel sheet has a base steel sheet and an aluminum-based plating layer. The aluminum-based plating layer covers both surfaces of the base steel sheet. The coating weight (g / m) of the aluminum-based plating layer on the first steel sheet relative to both surfaces of the base steel sheet is 2 ) is the coating weight (g / m) of the aluminum-based plating layer on both surfaces of the base steel sheet in the second steel sheet. 2 ) (first configuration).

[0012] The blank according to the first configuration includes a first steel sheet having a minimum thickness and a second steel sheet having a thickness greater than that of the first steel sheet. Both the first steel sheet and the second steel sheet are plated steel sheets having an aluminum-based plating layer. However, the amount of the aluminum-based plating layer deposited on both surfaces of the base steel sheet is smaller on the first steel sheet than on the second steel sheet. As a result, when the blank is heated during hot stamping, alloying of the aluminum-based plating layer and iron progresses to the surface of the thin first steel sheet before that of the relatively thick second steel sheet, causing both surfaces of the first steel sheet to change from silvery white to black or a color close to silvery white. As a result, the emissivity of both surfaces of the first steel sheet is higher than that of the second steel sheet. Therefore, the first steel sheet can be heated to a temperature in the austenite range more quickly, and the first steel sheet can be held at that temperature for a longer period of time. This allows the austenite grains in the first steel sheet to become coarse. As a result, the ferrite transformation region (ferrite nose) in the CCT diagram shifts to the long-time side, so that the start of the ferrite transformation in the first steel sheet can be delayed after the heating of the blank is completed, and blank forming can be started while the microstructure of the first steel sheet is maintained in the austenite phase. In other words, the hardenability of the thin first steel sheet can be improved.

[0013] In the blank according to the first configuration, the hardenability of the first steel plate having a smaller thickness is improved, and therefore the first steel plate can be well hardened when a structural component is formed from the blank by hot stamping. This facilitates uniform hardness in the structural component, thereby preventing partial reductions in the structural component's strength. Furthermore, because uneven stress is less likely to occur in the structural component, twisting is less likely to occur even when the formed structural component is annular, ensuring good dimensional accuracy in the structural component. Therefore, when an annular structural component, particularly a large annular structural component, including a first steel plate having a smaller thickness than the second steel plate is formed from the blank, poor strength and dimensional accuracy of the structural component can be reduced, and the impact absorption performance (crash resistance) of the structural component can be improved.

[0014] In the blank according to the first configuration, the coating weight of the aluminum-based plating layer on the first steel sheet having the minimum thickness is smaller than the coating weight of the aluminum-based plating layer on the second steel sheet having a relatively large thickness. In this case, the first steel sheet heats up faster than the second steel sheet, and the high-temperature holding time of the first steel sheet, i.e., the time from when the first steel sheet reaches the austenite temperature range until the second steel sheet and the entire blank reach the austenite temperature range, is longer than when the coating weights of the aluminum-based plating layers on the first and second steel sheets are the same. This reduces non-uniformity in phase transformation due to differences in cooling rates between the steel sheets after the blank is heated. Specifically, the initiation of the austenite-to-ferrite phase transformation in the first steel sheet having the minimum thickness can be delayed, thereby reducing the difference in the phase transformation initiation time between the first steel sheet having the minimum thickness and the other steel sheets. As a result, the hardenability can be made uniform between the first steel sheet having the minimum thickness and the other steel sheets.

[0015] In the blank according to the first configuration, the thickness of the first steel plate is t min The thickness of the steel plate having the largest thickness among the plurality of steel plates is t max When 1.0<t max / t min Preferably, it is ≦3.2 (second configuration).

[0016] Among the multiple steel plates included in the blank, the smallest plate thickness t min The first steel plate having a maximum plate thickness t max When the difference in thickness between the steel plate and other steel plates having the minimum thickness t is large, it becomes difficult to ensure the process window in the manufacture of structural members. min and maximum plate thickness t max If the difference is large, when the blank is heated during hot stamping, the maximum plate thickness t max While waiting for the steel sheet having the minimum sheet thickness t min Maximum plate thickness t maxThe ratio is set to 3.2 or less. max The temperature rise rate and minimum plate thickness t of the steel plate min Since the heating rate of the first steel sheet does not deviate too much from that of the other steel sheet, heating of the other steel sheet can be completed before alloying of the aluminum-based plating layer of the first steel sheet progresses excessively. Therefore, a structural member can be manufactured while maintaining the corrosion resistance or weldability of the first steel sheet, and a process window can be secured in the manufacture of the structural member.

[0017] The blank according to the first or second configuration may further include an overlap portion. The overlap portion is formed by overlapping the ends of two adjacent steel sheets among the plurality of steel sheets. The overlap portion has a total sheet thickness of, for example, 4.0 mm or less. The two steel sheets may each be a plated steel sheet having a base steel sheet and an aluminum-based plating layer covering both surfaces of the base steel sheet. In this case, the coating amount (g / m) of the aluminum-based plating layer on both surfaces of the base steel sheet in each of the two steel sheets is 2 ) is the coating weight (g / m) of the aluminum-based plating layer on both surfaces of the base steel sheet in the second steel sheet. 2 ) (third configuration).

[0018] When a blank has an overlap portion formed by overlapping the ends of two steel sheets, it may be impossible to ensure a process window for manufacturing a structural component. Specifically, when the blank is heated during hot stamping, alloying of the aluminum-based plating layer of the first steel sheet having the smallest thickness progresses while waiting for the overlap portion to reach the austenite temperature range, resulting in a thick diffusion layer, making it impossible to ensure the corrosion resistance or weldability of the first steel sheet. Therefore, in the third configuration, for each steel sheet forming the overlap portion, the deposition amount of the aluminum-based plating layer on both surfaces of the base steel sheet is smaller than that of the second steel sheet. This accelerates the temperature rise of the overlap portion, allowing heating of the overlap portion to be completed before excessive alloying of the plating layer of the first steel sheet progresses, thereby enabling the manufacturing of a structural component while maintaining the corrosion resistance or weldability of the first steel sheet. In other words, the process window for manufacturing a structural component is easily ensured. In addition, in the third configuration, the total plate thickness of the overlap portion is limited to 4.0 mm or less, so that the temperature rise in the overlap portion does not become too slow relative to the first steel plate, and the process window is easily secured.

[0019] In the blank according to the third configuration, the surface of at least one of the two steel plates located outside the overlap portion may be coated with a black coating (fourth configuration).

[0020] In the fourth configuration, a black coating is applied to the surface of at least one of the two steel plates forming the overlap portion that is positioned outside the overlap portion. This increases the emissivity of the overlap portion, allowing for faster temperature rise. This makes it easier to ensure a process window in the manufacture of structural components.

[0021] In the blank according to any one of the first to fourth configurations, at least one surface of the first steel plate may be coated with a black coating (fifth configuration).

[0022] In the fifth configuration, a black coating is applied to at least one surface of the first steel plate having the minimum plate thickness. This allows the emissivity of the surface of the first steel plate to be increased in advance, so that the temperature of the first steel plate rises more quickly when the blank is heated during hot stamping. This allows the first steel plate to be held at high temperatures for a longer period of time, further promoting the coarsening of austenite grains in the first steel plate. As a result, the hardenability of the first steel plate having a small plate thickness can be further improved.

[0023] A method for manufacturing a structural component according to an embodiment includes the steps of preparing a blank according to any one of the first to fifth configurations, heating a plurality of steel plates included in the blank to a temperature equal to or higher than the austenite transformation completion temperature, and using a mold to form the heated blank into a structural component that is annular in plan view and quenching it (sixth configuration).

[0024] A structural member according to an embodiment includes a member body. The member body is formed by joining a plurality of steel plates together and has an annular shape in plan view. The plurality of steel plates include a first steel plate having a minimum plate thickness and a second steel plate having a plate thickness greater than that of the first steel plate. The first steel plate and the second steel plate are each plated steel plates having an aluminum-based plating layer on both surfaces of a base steel plate. The thickness of the aluminum-based plating layer on the first steel plate is smaller than the thickness of the aluminum-based plating layer on the second steel plate (seventh configuration).

[0025] The structural member according to the seventh configuration may be a door ring part for an automobile. The member body may include a front pillar, a center pillar, and a rocker connecting the front pillar and the center pillar (eighth configuration).

[0026] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or equivalent components are designated by the same reference numerals, and the same description will not be repeated.

[0027] <First embodiment> [Structural member] Fig. 1 is a diagram (plan view) of a structural member 10 according to this embodiment, viewed from above in a state where it is placed on a horizontal surface. The structural member 10 is used, for example, in the body of an automobile. The structural member 10 is typically a door ring component of the automobile. In this embodiment, an example in which the structural member 10 is a door ring component will be described.

[0028] The structural member 10 is a hot-stamped member. That is, the structural member 10 is formed by hot stamping (hot press processing) a blank made of multiple steel plates. The structural member 10 includes a member main body 11. The member main body 11 has an annular shape in a plan view of the structural member 10. The member main body 11 includes a front pillar 111, a center pillar 112, and a rocker 113. When the structural member 10 is assembled to the body of an automobile, the center pillar 112 is disposed rearward of the front pillar 111. The center pillar 112 extends generally in the vertical direction of the vehicle body. The front pillar 111 extends toward the center pillar 112. When the structural member 10 is assembled to the body of an automobile, the rocker 113 is disposed below the front pillar 111 and the center pillar 112. The rocker 113 connects the front pillar 111 and the center pillar 112.

[0029] In this embodiment, the member body 11 is formed of a plurality of steel plates 21, 22, and 23 joined together. In the example of FIG. 1 , the front pillar 111 is mainly formed of the steel plates 21 and 22. The center pillar 112 is mainly formed of the steel plate 23. The rocker 113 is also formed of the steel plates 21 and 23.

[0030] FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1 . FIG. 2 shows a cross-section of the structural member 10 cut in the thickness direction at the position of the steel plate 21. As shown in FIG. 2 , the steel plate 21 has an open cross-section. In a cross-sectional view of the structural member 10, the steel plate 21 has, for example, a generally hat-shaped shape. More specifically, the steel plate 21 includes a top plate 211, vertical walls 212 and 213, and flanges 214 and 215. The vertical wall 212 is disposed on the opposite side of the vertical wall 213 with respect to the top plate 211. In a cross-sectional view of the structural member 10, one end of the vertical walls 212 and 213 is connected by the top plate 211. In a cross-sectional view of the structural member 10, the other end of the vertical walls 212 and 213 is connected to flanges 214 and 215, respectively. The flanges 214 and 215 protrude from the vertical walls 212 and 213, respectively, to the outside of the structural member 10.

[0031] In the structural member 10, the width W of the steel plate 21 may be 30 mm or more and 750 mm or less. The height H of the steel plate 21 may be 25 mm or more and 150 mm or less. The width W is the distance from the end of the R on the vertical wall 212 side of the corner portion between the top plate 211 and the vertical wall 212 to the end of the R on the vertical wall 213 side of the corner portion between the top plate 211 and the vertical wall 213 in the cross section of the structural member 10. The height H is the distance from the top plate 211 to the flanges 214, 215 in the plate thickness direction of the top plate 211.

[0032] Although not shown, the other steel plates 22, 23 also have an open cross section similar to the steel plate 21. The steel plates 22, 23 may also have, for example, a generally hat shape in a cross section of the structural member 10. The width of the steel plates 22, 23 may be 15 mm or more and 300 mm or less. The height of the steel plates 22, 23 may be 10 mm or more and 150 mm or less.

[0033] The size of the annular structural member 10 in a plan view is, for example, 1.0 m or more. The size of the structural member 10 may be, for example, 4.0 m or less. The size of the structural member 10 is the length of a line segment connecting any two points on the outer periphery of the structural member 10 that are farthest apart when the structural member 10 is placed on a horizontal surface and viewed vertically.

[0034] 3A to 3G, a method for manufacturing the structural member 10 will be described. The method for manufacturing the structural member 10 according to this embodiment includes the steps of preparing a blank 20, heating the blank 20, and forming the heated blank 20 into the structural member 10.

[0035] 3A , in the preparation step, a blank 20 having a shape obtained by unfolding the structural member 10 is prepared. The blank 20 includes a plurality of steel plates 21, 22, and 23. The steel plates 21, 22, and 23 are arranged and joined together so as to have an annular shape when the blank 20 is viewed from above.

[0036] 3B, 3C, and 3D are cross-sectional views of the blank 20 showing the joints between the steel plates 21, 22, and 23. FIGS. 3B, 3C, and 3D are cross-sectional views taken along lines IIIB-IIIB, IIIC-IIIC, and IIID-IIID in FIG. 3A, respectively. Referring to FIGS. 3B and 3C, the steel plate 21 is butt-joined to each of the steel plates 22 and 23. That is, the end face of the steel plate 21 is joined to the end face of the steel plate 22 while abutting against the end face of the steel plate 22, and the other end face of the steel plate 21 is joined to the end face of the steel plate 23 while abutting against the end face of the steel plate 23. Referring to FIG. 3D, the steel plate 22 is butt-joined to the steel plate 21 as well as the steel plate 23. The end face of the steel plate 22 is joined to the end face of the steel plate 23 while abutting against the end face. The steel plates 21, 22, and 23 are joined by, for example, laser welding. In this embodiment, the blank 20 is a so-called tailor weld blank.

[0037] 3B and 3C, among the steel plates 21, 22, and 23, the steel plate 21 has a minimum plate thickness t min The steel plate 22 has a thickness t min The steel plate 23 has a thickness t min In the present embodiment, the thickness of each of the steel plates 22 and 23 is equal to or greater than the thickness t min In this embodiment, the steel plate 23 has the largest plate thickness t max The steel plate 22 has a thickness t minis larger than the thickness t of the steel plate 23 max Plate thickness t smaller than mid However, the steel plate 22 may have a thickness equal to or greater than that of the steel plate 23. That is, among the steel plates 21, 22, and 23, the steel plate 22 has the maximum plate thickness t max It can also have:

[0038] Plate thickness t of steel plate 21 min is typically less than 1.4 mm. min The thickness t of the steel plate 21 may be, for example, 0.8 mm or more. min and the thickness t of the steel plate 23 max is 1.0<t max / t min ≦3.2, and 1.3≦t max / t min It is more preferable that the ratio ≦3.2 is satisfied.

[0039] The steel sheets 21, 22, and 23 are each plated steel sheets, more specifically, aluminum-plated steel sheets. The steel sheet 21 has a base steel sheet 21a and an aluminum-based plating layer 21b. The steel sheet 22 has a base steel sheet 22a and an aluminum-based plating layer 22b. The steel sheet 23 has a base steel sheet 23a and an aluminum-based plating layer 23b. The sheet thickness t of the steel sheet 21 min is the combined thickness of the base steel sheet 21a and the aluminum-based plating layer 21b, and is the average thickness of the steel sheet 21. mid is the combined thickness of the base steel sheet 22a and the aluminum-based plating layer 22b, and is the average thickness of the steel sheet 22. max is the combined thickness of the base steel sheet 23 a and the aluminum-based plating layer 23 b, and is the average thickness of the steel sheet 23 .

[0040] The types of the base steel plates 21a, 22a, and 23a are not particularly limited, and each of the base steel plates 21a, 22a, and 23a may be the same as or different from the other base steel plates.

[0041] In the steel sheet 21, an aluminum-based plating layer 21b covers both surfaces of the base steel sheet 21a. The aluminum-based plating layer 21b is provided over the entire or almost the entire surfaces of both surfaces of the base steel sheet 21a. Similarly, in the steel sheet 22, an aluminum-based plating layer 22b covers both surfaces of the base steel sheet 22a. The aluminum-based plating layer 22b is provided over the entire or almost the entire surfaces of both surfaces of the base steel sheet 22a. Furthermore, in the steel sheet 23, an aluminum-based plating layer 23b covers both surfaces of the base steel sheet 23a. The aluminum-based plating layer 23b is provided over the entire or almost the entire surfaces of both surfaces of the base steel sheet 23a.

[0042] The chemical composition of the aluminum-based plating layers 21b, 22b, 23b is not particularly limited. Known aluminum-based plating layers (plating layers containing aluminum as a main component) can be used as the aluminum-based plating layers 21b, 22b, 23b. Although not particularly limited, the aluminum-based plating layers 21b, 22b, 23b are, for example, Al-Si-based plating layers. The aluminum-based plating layers 21b, 22b, 23b may be the same as or different from the aluminum-based plating layers of the other steel sheets 21, 22, 23, respectively.

[0043] Referring to FIG. 3B, the minimum plate thickness t min The coating weight of the aluminum-based plating layer 21b on both surfaces of the base steel sheet 21a in the steel sheet 21 having the above structure is W1 (g / m 2 ), larger plate thickness t mid The coating weight of the aluminum-based plating layer 22b on both surfaces of the base steel sheet 22a in the steel sheet 22 having the above-mentioned thickness is W2 (g / m 2 ), the coating weight W1 of the aluminum-based plating layer 21b on the steel sheet 21 is smaller than the coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22. The coating weight W1 of the aluminum-based plating layer 21b on the steel sheet 21 is the average coating weight on both surfaces of the base steel sheet 21a. Usually, the coating weight (g / m) of the aluminum-based plating layer 21b on one surface of the base steel sheet 21a is 2 ) is the coating weight (g / m) of the aluminum-based plating layer 21b on the other surface of the base steel sheet 21a. 2) is substantially equal to the coating weight (g / m) of the aluminum-based plating layer 21b on one surface of the base steel sheet 21a. However, depending on various conditions during manufacturing, for example, the coating weight of the aluminum-based plating layer 21b may vary between the front and back surfaces of the base steel sheet 21a. The coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22 is the average coating weight on both surfaces of the base steel sheet 22a. The coating weight (g / m) of the aluminum-based plating layer 22b on one surface of the base steel sheet 22a is 2 ) is usually the coating weight (g / m) of the aluminum-based plating layer 22b on the other surface of the base steel sheet 22a. 2 ) However, depending on various conditions during manufacturing, for example, the coating weight of the aluminum-based plating layer 22b may vary between the front and back surfaces of the base steel sheet 22a. The coating weight of the aluminum-based plating layer 22b may be different between one surface and the other surface.

[0044] The coating weight W1 of the aluminum-based plating layer 21b on the steel sheet 21 and the coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22 are each 20 g / m 2 120g / m or more 2 The deposition amounts W1 and W2 are preferably 30 g / m or less. 2 More preferably, 35 g / m 2 The deposition amounts W1 and W2 are preferably 115 g / m 2 More preferably, it is 100 g / m or less. 2 The difference between the adhesion amounts W1 and W2 (W2-W1) is, for example, 10 (g / m 2 ) or more. W2-W1 is preferably 20 (g / m 2 ) or more, more preferably 30 (g / m 2 ) or more. W2-W1 is 80 (g / m 2 ) or less. W2-W1 is preferably 70 (g / m 2 ) or less, more preferably 60 (g / m 2 ) or less. The adhesion amounts W1 and W2 satisfy the relationship W2 / W1>1.0. The adhesion amounts W1 and W2 preferably satisfy the relationship W2 / W1≧1.2, and more preferably W2 / W1≧1.5.

[0045] Referring to FIG. 3D, the maximum plate thickness t max The coating weight of the aluminum-based plating layer 23b on both surfaces of the base steel sheet 23a in the steel sheet 23 having the above structure is W3 (g / m 2 ), the coating weight W3 of the aluminum-based plating layer 23b on the steel sheet 23 may be smaller than the coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22. The coating weight W3 of the aluminum-based plating layer 23b is the average coating weight on both surfaces of the base steel sheet 23a. Usually, the coating weight (g / m) of the aluminum-based plating layer 23b on one surface of the base steel sheet 23a is 2 ) is the coating weight (g / m) of the aluminum-based plating layer 23b on the other surface of the base steel sheet 23a. 2 ) However, depending on various conditions during manufacturing, for example, the adhesion weight of the aluminum-based plating layer 23b may vary between the front and back surfaces of the base steel sheet 23a. The adhesion weight of the aluminum-based plating layer 23b may be different between one surface and the other surface of the base steel sheet 23a.

[0046] The coating weight W3 of the aluminum-based plating layer 23b on the steel sheet 23 is also, like the steel sheets 21 and 22, 20 g / m 2 120g / m or more 2 The deposition amount W3 is preferably 30 g / m 2 More preferably, 35 g / m 2 The adhesion amount W3 is 115 g / m 2 It is preferable that the weight is 100 g / m or less. 2 When W2>W3, the difference between the adhesion amounts W2 and W3 (W2-W3) is, for example, 10 (g / m 2 ) or more. W2-W3 is preferably 20 (g / m 2 ) or more, more preferably 30 (g / m 2 ) or more. W2-W3 is 80 (g / m 2 ) or less. W2-W3 is preferably 70 (g / m 2 ) or less, more preferably 60 (g / m 2 The coating weight W3 of the aluminum-based plating layer 23b on the steel sheet 23 is equal to or less than the minimum sheet thickness tmin The thickness W may be equal to or greater than the coating weight W1 of the aluminum-based plating layer 21b of the steel plate 21 having the thickness W1.

[0047] The method for forming the aluminum-based plating layers 21b, 22b, and 23b on the base steel sheet 21a, 22a, and 23a, respectively, is not particularly limited, but may be, for example, a general hot-dip plating method. That is, by immersing the base steel sheet 21a in a molten aluminum plating bath and gas wiping with nitrogen, air, or the like, an aluminum-plated steel sheet 21 having an adjusted coating weight W1 of the aluminum-based plating layer 21b can be obtained. Similarly, by immersing the base steel sheet 22a in a molten aluminum plating bath and gas wiping with nitrogen, air, or the like, an aluminum-plated steel sheet 22 having an adjusted coating weight W2 of the aluminum-based plating layer 22b can be obtained. Furthermore, by immersing the base steel sheet 23a in a molten aluminum plating bath and gas wiping with nitrogen, air, or the like, an aluminum-plated steel sheet 23 having an adjusted coating weight W3 of the aluminum-based plating layer 23b can be obtained. When an aluminum-based plating layer is formed by hot-dip plating, an Al—Fe-based alloy layer is formed at the interface between the base steel sheet and the aluminum-based plating layer due to the elution of Fe during the hot-dip plating process.

[0048] The coating weights W1, W2, and W3 of the aluminum-based plating layers 21b, 22b, and 23b can be measured, for example, by the sodium hydroxide-hexamethylenetetramine-hydrochloric acid stripping weight method described in JIS G 3314:2019. Specifically, in accordance with JIS G 3314:2019, a predetermined surface area S (mm 2) (for example, 50 mm × 50 mm) and measure the weight w1 (g) of each test piece. Then, each test piece is immersed in an aqueous sodium hydroxide solution, and after confirming that foaming caused by dissolution of the plating has subsided, each test piece is removed from the aqueous sodium hydroxide solution and rinsed with water. Next, each test piece that is still wet after rinsing with water is immersed in an aqueous hydrochloric acid solution containing added hexamethylenetetramine until foaming caused by dissolution of the plating has subsided. The test piece is removed from the hexamethylenetetramine-hydrochloric acid solution, immediately rinsed with water, dried, and the weight w2 (g) of the test piece is measured again. The coating weight W (g / m) of the aluminum-based plating layer of each test piece is measured. 2 ) is {(w1-w2) / S}×10 6 The average value of the coating weight W of five or more test pieces taken from each steel sheet is taken as the coating weight of the aluminum-based plating layer on that steel sheet.

[0049] However, when the size of the test specimens taken from each of the steel sheets 21, 22, and 22 is small, the cross section of each of the aluminum-based plating layers 21b, 22b, and 23b is observed with an optical microscope (area: 100 μm × 100 μm), and the thickness (μm) of the plating layer is measured in three fields of view in the same manner. The average value of the thicknesses measured in the three fields of view is tripled to convert it into the coating weight. In this case, the coating weight is calculated for each side of the base steel sheet for each of the steel sheets 21, 22, and 22, and the average of the obtained coating weights (average value for both sides) is taken as the coating weight of the aluminum-based plating layer. If an Al-Fe-based alloy layer is present at the interface between the base steel sheet and the aluminum-based plating layer, the thickness of the aluminum-based plating layer includes the thickness of the Al-Fe-based alloy layer. The thickness of the aluminum-based plating layer 21b of the thinnest steel sheet 21 is smaller than the thickness of the aluminum-based plating layer 22b of the other steel sheets 22. In this embodiment, the thickness of the aluminum-based plating layer 23b of the thickest steel plate 23 is also smaller than the thickness of the aluminum-based plating layer 22b of the steel plate 22. The thicknesses of the aluminum-based plating layers 21b, 23b may be different from each other or may be the same.

[0050] (Heating Step) The prepared blank 20 is formed into the structural member 10 (FIGS. 1 and 2) by hot stamping (hot press working). During the hot stamping, the blank 20 is subjected to a heating step. Referring to FIG. 3E, in the heating step, the blank 20 is heated, for example, by a heating furnace 30. The plurality of steel plates 21, 22, and 23 included in the blank 20 are heated to an austenite transformation completion temperature (A c3 The steel plates 21, 22, and 23 are heated to, for example, 900° C. or higher, so that the microstructures of the steel plates 21, 22, and 23 are transformed, for example, entirely or almost entirely into an austenite phase.

[0051] (Forming Process) Referring to Fig. 3F, in the forming process, a die 40 is used to form the heated blank 20 into a structural member 10 (Figs. 1 and 2) that is annular in plan view and quench it. The blank 20 heated in the heating process is removed from the heating furnace 30 (Fig. 3E) and transported to the die 40. The die 40 is attached to a known press device. The die 40 includes, for example, a punch 41 and a die 42. The blank 20 is placed between the punch 41 and the die 42.

[0052] 3G , after the blank 20 is placed between the punch 41 and the die 42, the die 42 moves relatively close to the punch 41. The blank 20 is clamped (pressed) between the punch 41 and the die 42 and formed into a shape that conforms to the forming surfaces of the punch 41 and the die 42. The blank 20 remains clamped between the punch 41 and the die 42. The blank 20 is cooled (quenched) by the die 40, and its microstructure is transformed into martensite. This allows the structural member 10 to be manufactured from the blank 20.

[0053] 4A to 4C are cross-sectional views of the structural member 10 after hot stamping. min 4B shows a cross section of the structural member 10 at the position of the steel plate 21 having a plate thickness t mid 4C shows a cross section of the structural member 10 at the location of the steel plate 22 having the maximum plate thickness t max 2 shows a cross section of the structural member 10 at the location of the steel plate 23 having the

[0054] Referring to Fig. 4A, even in the structural member 10 after hot stamping, the steel sheet 21 is a plated steel sheet having aluminum-based plating layers 21b on both surfaces of a base steel sheet 21a. Referring to Fig. 4B, the steel sheet 22 is a plated steel sheet having aluminum-based plating layers 22b on both surfaces of a base steel sheet 22a. Referring to Fig. 4C, the steel sheet 23 is a plated steel sheet having aluminum-based plating layers 23b on both surfaces of a base steel sheet 23a. However, compared to the state of the blank 20 (Figs. 3B to 3D), the aluminum-based plating layers 21b, 22b, 23b in the structural member 10 have been alloyed with iron more effectively by the heating process.

[0055] 4A and 4B , when the average thickness (plating thickness) of the aluminum-based plating layer 21b on both surfaces of the steel sheet 21 is K1 (μm), and the average thickness (plating thickness) of the aluminum-based plating layer 22b on both surfaces of the steel sheet 22 is K2 (μm), the plating thickness K1 of the steel sheet 21 is smaller than the plating thickness K2 of the steel sheet 22. The difference between the plating thicknesses K1 and K2, K2 - K1, is, for example, 7 μm or more. K2 - K1 may be 33 μm or less. Furthermore, the plating thicknesses K1 and K2 may satisfy the relationship K2 / K1 > 1.0. K2 / K1 is preferably 1.2 or more, more preferably 1.5 or more.

[0056] 4B and 4C , in this embodiment, when the average thickness (plating thickness) of the aluminum-based plating layer 23b on both surfaces of the steel sheet 23 is K3 (μm), the plating thickness K3 of the steel sheet 23 is smaller than the plating thickness K2 of the steel sheet 22. The difference between the plating thicknesses K2 and K3, K2 - K3, is, for example, 7 (μm) or more. K2 - K3 may be 33 (μm) or less.

[0057] The plating thicknesses K1, K2, and K3 of the aluminum-based plating layers 21b, 22b, and 23b on the structural member 10 can be measured as follows. Specifically, a vehicle body part is disassembled to obtain the annular structural member 10, and an analysis sample is obtained from the structural member 10, for example, by laser cutting. For example, an analysis sample is obtained from each of the multiple steel plates included in the structural member 10. The analysis sample is obtained from the center or its vicinity of the top plate of each steel plate having an open cross section. For test pieces obtained from each of the multiple steel plates, the cross section of the aluminum-based plating layer is subjected to nital etching and then observed with an optical microscope (area: 100 μm × 100 μm), and the plating layer thickness is measured in three fields of view. The average of the plating layer thicknesses measured in the three fields of view can be used as the plating thickness. In many cases, the outermost surface of the structural member 10 contains, for example, an electrodeposition coating film. In such cases, the plating layer below the electrodeposition coating film and above the base steel sheet is observed.

[0058] Minimum plate thickness t min In the cross section of the structural member 10 at the position of the steel plate 21 having the minimum martensite fraction (%), the martensite fraction variation is, for example, 20% or less, when the difference is the maximum martensite fraction (%) minus the minimum martensite fraction (%). The martensite fraction variation is preferably 15% or less, and more preferably 10% or less. The martensite fraction variation can be measured as follows. That is, min Ten or more analysis samples (for example, a length of about 10 mm) are cut out from positions at least 20 mm away from the end of the cross section of the structural member 10 at the position of the steel plate 21 having the above structure, and each sample is at least 10 mm away from the end. Then, each sample is mirror-polished so that the thickness direction of the steel plate serves as the observation surface, and etched with LePeller's reagent. Then, an optical microscope is used to observe the area from the surface of the steel plate to a depth of 1 / 4 of the plate thickness (a region from the surface of the steel plate to a depth of 1 / 8 of the plate thickness to a depth of 3 / 8 of the plate thickness) at a magnification of 1000x, with one field of view of 2,400 μm. 2 The above structural photographs are taken from 30 fields of view, and the obtained structural photographs are subjected to image analysis.

[0059] The image analysis method involves obtaining the maximum brightness value Lmax and minimum brightness value Lmin from the image, designating the area with pixels whose brightness ranges from Lmax-0.3 (Lmax-Lmin) to Lmax as a white area, and calculating the ratio of the number of pixels in the white area to the total number of pixels to measure the martensite fraction. This type of image analysis is performed on a total of 30 observation fields of each analysis sample to determine the martensite fraction, and the average value is used as the martensite fraction for each analysis sample. Furthermore, the difference between the maximum and minimum martensite fractions in 10 or more analysis samples is calculated based on the minimum plate thickness t min The variation in martensite fraction in the cross section of the structural member 10 at the position of the steel plate 21 having the minimum plate thickness t min If there are multiple steel plates having the above structure, such analysis is performed on each steel plate to determine the martensite fraction, and the maximum variation in martensite fraction among these steel plates is taken as the variation in martensite fraction in the structural member 10.

[0060] In some steel sheets, the area fraction of martensite obtained by image analysis, i.e., the area fraction of the white region, may contain a few percent of the area fraction of retained austenite. However, since the variation in the martensite fraction is calculated as a difference, the impact is minor.

[0061] After the forming process (hot stamping), the steel sheets 21, 22, and 23 can have a tensile strength of, for example, 0.5 GPa or more, and preferably 1.0 GPa or more. At least one of the steel sheets 21, 22, and 23 may have a tensile strength of 1.5 GPa or more after the forming process. The tensile strength of each of the steel sheets 21, 22, and 23 may be the same as or different from the tensile strength of the other steel sheets.

[0062] [Effect] In the blank 20 according to this embodiment, the minimum plate thickness t minThe coating weight W1 of the aluminum-based plating layer 21b of the steel sheet 21 having a thickness of 1 / 2 mm is smaller than the coating weight W2 of the aluminum-based plating layer 22b of the steel sheet 22 having a greater thickness. As a result, when the blank 20 is heated during hot stamping, the temperature rise rate of the steel sheet 21 is significantly higher than that of the steel sheet 22. Specifically, because the aluminum-based plating layer 21b on the surface of the steel sheet 21 is relatively thin, when the blank 20 is heated, alloying of the aluminum-based plating layer 21b with the iron contained in the base steel sheet 21a progresses rapidly to the surface of the steel sheet 21, and both surfaces of the steel sheet 21 turn black or a color similar to black. That is, the emissivity of both surfaces of the steel sheet 21 increases during the heating process. Therefore, the steel sheet 21 can be heated to a temperature in the austenite range more quickly, ensuring a long high-temperature holding time for the steel sheet 21. As a result, austenite grains in the microstructure of the steel sheet 21 coarsen, and the ferrite transformation region (ferrite nose) in the CCT diagram shifts to the longer time side. Therefore, it is possible to prevent austenite from transforming into ferrite in the steel sheet 21 after it is removed from the heating furnace 30 and before the start of forming by the die 40. Therefore, it is possible to start forming the blank 20 by the die 40 while maintaining the microstructure of the steel sheet 21 in the austenite phase, and it is possible to prevent the steel sheet 21 from being formed to the minimum plate thickness t min The hardenability of the steel plate 21 having this can be improved.

[0063] In this embodiment, the hardenability of the relatively thin steel plate 21 is improved, so that the hardness of the structural member 10 formed from the blank 20 can be made uniform. More specifically, the minimum plate thickness t min Since the steel plate 21 having a thickness of 1000 .0 mm or less can be quenched well, the variation in the martensite fraction in the steel plate 21 can be kept to 20% or less. This makes it less likely for deformation concentration to occur when a collision load is input to the structural member 10, making it easier for the structural member 10 to exhibit high impact absorption performance. Therefore, even when an annular structural member 10 including a thin steel plate 21, particularly a large annular structural member 10, is formed from the blank 20, it is possible to reduce strength defects in the structural member 10 and improve the impact absorption performance of the structural member 10.

[0064] The smaller the variation in the martensite fraction, the less non-uniformity there is in the mechanical properties within the structural member 10, which is preferable from the viewpoint of the functionality of the structural member 10. On the other hand, a large variation in the martensite fraction indicates that parts with insufficient hardenability, i.e., parts with insufficient hardness, are unevenly distributed within the structural member 10, and when the structural member 10 is deformed by a collision, deformation tends to concentrate in the parts with insufficient hardness, thereby reducing the functionality of the structural member 10.

[0065] In this embodiment, the hardenability of the relatively thin steel plate 21 is improved, which makes it less likely that uneven stress will occur in the structural member 10. Therefore, even when the annular structural member 10 is formed from an annular blank 20, twisting is less likely to occur in the structural member 10. Therefore, even when an annular structural member 10 including a thin steel plate 21, particularly a large annular structural member 10, is formed from the blank 20, it is possible to reduce poor dimensional accuracy of the structural member 10 and improve the impact absorption performance of the structural member 10.

[0066] In the blank 20 according to this embodiment, the minimum plate thickness t min The coating weight W1 of the aluminum-based plating layer 21b on the steel sheet 21 is smaller than the coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22 having a thickness greater than that of the steel sheet 21. This allows the steel sheet 21 to be heated more quickly than the steel sheet 22, and therefore the high-temperature holding time of the steel sheet 21 is longer than when the coating weight W1 of the aluminum-based plating layer 21b on the steel sheet 21 is the same as or greater than the coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22. Therefore, after heating of the blank 20 is completed, non-uniformity in phase transformation caused by differences in cooling rates among the steel sheets 21, 22, and 23 can be reduced. Specifically, min Since the start of the phase transformation from austenite to ferrite can be delayed for the steel plate 21, the difference in the phase transformation start time between the steel plate 21 and the other steel plates 22 and 23 is reduced. As a result, the hardenability of the steel plates 21, 22, and 23 included in the blank 20 can be made uniform.

[0067] In this embodiment, in the heating process, first, the minimum plate thickness t minThe steel plate 21 having the intermediate thickness t mid and a steel plate 22 having a maximum plate thickness t max The steel plate 23 having the minimum plate thickness t min and maximum plate thickness t max Ratio to: t max / t min It is preferable that the thickness t min The plate thickness t max Therefore, the steel plate 23 having the above-mentioned structure can be heated sufficiently until the phase transformation to austenite is completed. Therefore, the process window can be secured in the manufacturing of the structural member 10.

[0068] <Second embodiment> Fig. 5 is a plan view of a blank 20A according to a second embodiment. The blank 20 according to the first embodiment is a tailored blank in which steel plates 21, 22, and 23 are butt-joined to one another. The blank 20A according to this embodiment differs from the first embodiment mainly in the form of the joint between the steel plates.

[0069] 5, the blank 20A includes a plurality of steel plates 21, 22, 23, 24, and 25. The steel plates 21, 22, 23, 24, and 25 are arranged and joined to form an annular shape in a plan view of the blank 20. As in the first embodiment, the steel plate 21 has a minimum plate thickness t min and the coating amount of the aluminum-based plating layer is smaller than that of the other steel plates 22. Therefore, the blank 20A according to this embodiment can also achieve the same effects as those of the first embodiment.

[0070] The blank 20A has an overlap portion 26. Fig. 6 is a cross-sectional view taken along line VI-VI in Fig. 5, showing a cross section of the overlap portion 26. In this embodiment, the overlap portion 26 is formed by overlapping the ends of two adjacent steel plates 23, 24. The end of the steel plate 23 is joined to the end of the steel plate 24 in an overlapping state. The steel plates 23, 24 are joined to each other by, for example, spot welding or laser welding.

[0071] In this embodiment, the steel sheets 23, 24 are plated steel sheets. That is, the steel sheet 23 has a base steel sheet 23a and an aluminum-based plating layer 23b, as in the first embodiment. Similarly, the steel sheet 24 has a base steel sheet 24a and an aluminum-based plating layer 24b. The base steel sheets 23a, 24a may be the same type of steel sheet or different types of steel sheets. Similarly, the aluminum-based plating layers 23b, 24b may be the same type of plating layer or different types of plating layers.

[0072] The overlap portion 26 has a total thickness t. The total thickness t is the sum of the thickness t3 of the steel plate 23 and the thickness t4 of the steel plate 24. The total thickness t also includes the thickness of the aluminum-based plating layers 23b, 24b of the steel plates 23, 24. The total thickness t of the overlap portion 26 is, for example, greater than 2.5 mm. The total thickness t of the overlap portion 26 is preferably 4.0 mm or less. In this case, the coating amount of the aluminum-based plating layer 23b on both surfaces of the base steel plate 23a of the steel plate 23 is set to W3 (g / m 2 ), the coating weight of the aluminum-based plating layer 24b on both surfaces of the base steel sheet 24a of the steel sheet 24 is W4 (g / m 2 ), the coating weights W3 and W4 are smaller than the coating weight W2 (FIGS. 3B and 3D) of the aluminum-based plating layer 22b on both surfaces of the base steel sheet 22a of the steel sheet 22.

[0073] The coating weight W3 of the aluminum-based plating layer 23b on the steel sheet 23 is the average coating weight on both surfaces of the base steel sheet 23a. 2) is the coating weight (g / m) of the aluminum-based plating layer 23b on the other surface of the base steel sheet 23a. 2 ) is substantially equal to the coating weight (g / m) of the aluminum-based plating layer 24b on one surface of the base steel sheet 24a. However, depending on various conditions during manufacturing, for example, the coating weight of the aluminum-based plating layer 23b may vary between the front and back surfaces of the base steel sheet 23a. The coating weight W4 of the aluminum-based plating layer 24b on the steel sheet 24 is the average coating weight on both surfaces of the base steel sheet 24a. Usually, the coating weight (g / m) of the aluminum-based plating layer 24b on one surface of the base steel sheet 24a is 2 ) is the coating weight (g / m) of the aluminum-based plating layer 24b on the other surface of the base steel sheet 24a. 2 ) However, depending on various conditions during manufacturing, for example, the coating weight of the aluminum-based plating layer 24b may vary between the front and back of the base steel sheet 24a. The coating weight of the aluminum-based plating layer 24b may be different between one surface and the other surface of the base steel sheet 24a. The coating weights W3 and W4 are each 20 g / m 2 120g / m or more 2 The deposition amounts W3 and W4 are preferably 30 g / m or less. 2 More preferably, 35 g / m 2 The deposition amounts W3 and W4 are preferably 115 g / m 2 More preferably, it is 100 g / m or less. 2 The difference between the adhesion amounts W2 and W3 between the steel plates 22 and 23 (W2-W3) is, for example, 20 (g / m 2 ) or more. W2-W3 is 80 (g / m 2 Similarly, the difference between the adhesion amounts W2 and W4 between the steel plates 22 and 24 (W2-W4) may be, for example, 20 (g / m 2 ) or more. W2-W4 is 80 (g / m 2) or less. The coating weight W3 of the aluminum-based plating layer 23b of the steel sheet 23 and the coating weight W4 of the aluminum-based plating layer 24b of the steel sheet 24 may be the same or different. Furthermore, the sheet thickness t3 of the steel sheet 23 and the sheet thickness t4 of the steel sheet 24 may be the same or different. The sheet thickness t3 of the steel sheet 23 and the sheet thickness t4 of the steel sheet 24 are the average sheet thicknesses of the steel sheets 23 and 24, respectively, and are sheet thicknesses including the aluminum-based plating layers 23b and 24b.

[0074] The coating weight W3 of the aluminum-based plating layer 23b on the steel sheet 23 and the coating weight W4 of the aluminum-based plating layer 24b on the steel sheet 24 can be measured by the method described in the first embodiment.

[0075] If the total thickness t of the overlap portion 26 exceeds, for example, 2.5 mm, the overlap portion 26 is difficult to heat up. Therefore, when the blank 20A is heated during hot stamping, the overlap portion 26 may reach the minimum thickness t by the time it reaches the temperature in the austenite region. min In some cases, alloying of the aluminum-based plating layer 21b (FIGS. 3B and 3C) of the steel sheet 21 having the above-mentioned thickness progresses, resulting in a thick diffusion layer and making it impossible to ensure the corrosion resistance or weldability of the steel sheet 21. However, in the present embodiment, the emissivity of the overlap portion 26 is increased to promote temperature rise. Therefore, even if the total sheet thickness t of the overlap portion 26 is greater than, for example, 2.5 mm, the overlap portion 26 can be sufficiently heated until the phase transformation to austenite is completed before alloying of the aluminum-based plating layer 21b of the steel sheet 21 progresses, causing the diffusion layer to grow excessively and resulting in a loss of corrosion resistance or weldability. This makes it possible to ensure a process window in the manufacture of structural members.

[0076] In the blank 20A according to this embodiment, the steel plate 21 may be butt-joined to the steel plates 22 and 23, or may form an overlap portion 26 with one or both of the steel plates 22 and 23. The steel plate 25 may be butt-joined to the steel plates 22 and 24, or may form an overlap portion 26 with one or both of the steel plates 22 and 24.

[0077] 7 is a plan view of a structural member 10A manufactured from a blank 20A. The structural member 10A has substantially the same configuration as the structural member 10 of the first embodiment (FIGS. 1 and 2). However, in the structural member 10A, the member body 11 is formed from five steel plates 21, 22, 23, 24, and 25. The method for manufacturing the structural member 10A from the blank 20A is the same as that of the first embodiment.

[0078] The structural member 10A can have a size similar to that of the structural member 10 according to the first embodiment. That is, the size of the structural member 10A, which is annular in plan view, is, for example, 1.0 m or more and 4.0 mm or less. In the structural member 10A, each of the steel plates 21, 22, 23, 24, and 25 has an open cross section similar to that of the first embodiment. Each of the steel plates 21, 22, 23, 24, and 25 can have, for example, a generally hat shape in a cross-sectional view of the structural member 10A.

[0079] Although not shown, in the structural member 10A, the width of the steel plate 21 arranged on the upper part of the front pillar 111 is, for example, 15 mm or more and 300 mm or less. The height of the steel plate 21 may be, for example, 10 mm or more and 150 mm or less. In the structural member 10A, the width of the steel plate 22 arranged on the lower part of the front pillar 111 is, for example, 30 mm or more and 750 mm or less. The height of the steel plate 22 may be, for example, 25 mm or more and 150 mm or less. In the structural member 10A, the width of the steel plates 23, 24 arranged at the position of the center pillar 112 is, for example, 15 mm or more and 300 mm or less. The height of the steel plates 23, 24 may be, for example, 10 mm or more and 150 mm or less. In the structural member 10A, the width of the steel plate 25 arranged at the position of the rocker 113 is, for example, 30 mm or more and 300 mm or less. The height of the steel plate 25 may be, for example, 25 mm or more and 150 mm or less.

[0080] Third Embodiment Fig. 8 is a cross-sectional view of a blank 20B according to a third embodiment. In Fig. 8, the minimum thickness t min 8 shows a joint between a steel plate 21 having a thickness t1 and a steel plate 22 having a greater thickness t2. The example shown in Fig. 8 differs from the example shown in Fig. 3B in the first embodiment only in the configuration of the steel plate 21.

[0081] In this embodiment, one surface of the steel plate 21 is covered with a substantially black coating 27. On the other hand, the steel plate 22 is not provided with a substantially black coating 27. For example, the lightness L * Value (CIE 1976 lightness index L defined in JIS Z8781-4:2013) * ) is 60 or less, the coating 27 can be determined to be black. The coating 27 is provided over the entire surface of the steel sheet 21. The coating 27 may be a carbon-based surface treatment coating (a coating containing carbon (C)). By providing such a black coating 27, the emissivity of the surface of the steel sheet 21 is higher than the emissivity of both surfaces of the steel sheet 22. For example, at a measurement temperature of 25°C and a wavelength of 8.0 μm, the emissivity of the surface of the steel sheet 21 is higher than the emissivity of both surfaces of the steel sheet 22. The difference in emissivity at a wavelength of 8.0 μm at 25°C between the steel sheets 21 and 22 is preferably greater than 5%, more preferably greater than 10%, and even more preferably greater than 20%.

[0082] The coating 27 may be, for example, a surface treatment coating described in International Publication No. 2022 / 215229. That is, the coating 27 may contain, for example, carbon black. The coating 27 may further contain a metal oxide. The metal oxide may be, for example, one or more oxides selected from the group consisting of Zr oxide, Zn oxide, and Ti oxide. The coating 27 may also contain silica.

[0083] The coating 27 may contain graphite, soot, or the like instead of or in addition to carbon black. Alternatively, the coating 27 may contain, for example, an acicular compound having a hexagonal crystal structure with an aspect ratio of 4 to 50 in order to increase the emissivity of the steel sheet 21. The compound having a hexagonal crystal structure is typically graphite (C), but may also be lanthanum silicate, magnesium diboride, beryllium oxide (beryllia), zinc oxide, β-quartz, goethite (NiS), wurtzite (ZnS), or the like.

[0084] In this embodiment, the minimum plate thickness tmin A black coating 27 is applied to one surface of the steel sheet 21. This allows the emissivity of the surface of the steel sheet 21 to be increased in advance, so that when the blank 20B is heated during hot stamping, the temperature of the steel sheet 21 rises more quickly. This therefore ensures that the steel sheet 21 can be held at high temperatures for a longer period of time. This further improves the hardenability of the thinnest steel sheet 21.

[0085] In this embodiment, only one side of the steel sheet 21 is coated with the coating 27. However, the coating 27 may coat both sides of the steel sheet 21. The thickness of the coating 27 is, for example, 0.5 μm or more and 5.0 μm or less. The thickness of the coating 27 is preferably 1.0 μm or more and 3.0 μm or less. The thickness of the coating 27 is determined based on the thickness t of the steel sheet 21. min Therefore, the thickness of the steel plate 21 measured including the coating 27 is set to the thickness t min can be treated as

[0086] <Fourth embodiment> Fig. 9 is a cross-sectional view of a blank 20C according to a fourth embodiment. Fig. 9 shows an overlap portion 26 of the blank 20C formed by steel plates 23 and 24. The example shown in Fig. 9 differs from the example shown in the second embodiment (Fig. 6) in that the coating 27 described in the third embodiment is applied to the overlap portion 26.

[0087] In this embodiment, the surface of each of the steel plates 23, 24 located outside the overlap portion 26 is coated with a substantially black coating 27. In the steel plate 23, the entire surface opposite the mating steel plate 24 is coated with the coating 27. In the steel plate 24, the entire surface opposite the mating steel plate 23 is also coated with the coating 27. In other words, the surfaces of the steel plates 23, 24 that form the front and back surfaces of the overlap portion 26 are each coated with the coating 27. This increases the emissivity of the overlap portion 26, and therefore, when the blank 20C is heated during hot stamping, the temperature rise of the overlap portion 26 can be accelerated. Therefore, the plate thickness t of the steel plate 21 minThe overlap portion 26 can be heated to a temperature in the austenite range before alloying of the aluminum-based plating layer 21b (FIGS. 3B and 3C) progresses excessively, and the structural member 10 can be manufactured while maintaining the corrosion resistance or weldability of the steel plate 21. This makes it easier to ensure a process window in the manufacture of the structural member 10.

[0088] In the example of FIG. 9 , in each of the steel plates 23 and 24, the surface located outside the overlap portion 26 is coated with a substantially black coating 27. However, in one of the steel plates 23 and 24, the surface located outside the overlap portion 26 may be coated with the coating 27, and in the other of the steel plates 23 and 24, the surface located outside the overlap portion 26 may not be coated with the coating 27. Also, in the example of FIG. 9 , in each of the steel plates 23 and 24, the surface located inside the overlap portion 26 is not substantially coated with the black coating 27. However, in each of the steel plates 23 and 24, the surface located inside the overlap portion 26 may also be coated with the coating 27. However, from the viewpoint of uniformly heating the blank 20C during hot stamping, it is preferable that in each of the steel plates 23 and 24, the surface outside the overlap portion 26 is coated with the coating 27 and the surface located inside the overlap portion 26 is not coated with the coating 27.

[0089] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure.

[0090] In the first embodiment, the minimum plate thickness t min Not only the steel plate 21 having a maximum plate thickness t max In the example described above, the coating weight W3 of the aluminum-based plating layer 23b on the steel sheet 23 having the maximum sheet thickness t maxThe coating weight W3 of the aluminum-based plating layer 23b on the steel sheet 23 can be set to be equal to or greater than the coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22. In this case, in the structural member 10 after hot stamping, the plating thickness K3 of the steel sheet 23 is also equal to or greater than the plating thickness K2 of the steel sheet 22. min It is sufficient that the coating weight W1 of the aluminum-based plating layer 21b on the steel sheet 21 having the above-mentioned structure is less than the coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22.

[0091] In the first embodiment, the blank 20 includes three steel plates 21, 22, and 23. In the second embodiment, the blank 20A includes five steel plates 21, 22, 23, 24, and 25. However, the number of steel plates included in the blanks 20 and 20A is not limited to this. The blanks 20 and 20A have at least a minimum plate thickness t min and a steel plate 21 having a plate thickness t min The steel plate 22 may have a thickness greater than the minimum plate thickness t min It is sufficient that the coating weight W1 of the aluminum-based plating layer 21b on the steel sheet 21 having the above-mentioned configuration is smaller than the coating weight W2 of the aluminum-based plating layer 22b on the steel sheet 22. The steel sheet 21 is joined directly or indirectly to the steel sheet 22. The blank 20, 20A, which is annular in plan view, may typically include three or more steel sheets. In the blank 20, 20A, the coating weight of the aluminum-based plating layer on the steel sheets other than the steel sheets 21, 22 is not particularly limited. The steel sheets other than the steel sheets 21, 22 may be aluminum-plated steel sheets, or may be other plated steel sheets, or may be steel sheets without a plating layer on their surfaces (bare materials). In the annular blank 20, 20A, the arrangement of the multiple steel sheets including the steel sheets 21, 22 is not particularly limited.

[0092] The minimum thickness t of either the blank 20 or 20A minWhen there are a plurality of steel sheets 21 having the minimum plate thickness t, it is preferable that the coating weight W1 of the aluminum-based plating layer 21b of all the steel sheets 21 is smaller than the coating weight W2 of the aluminum-based plating layer 22b of the other steel sheets 22. The coating weights W1 of the aluminum-based plating layer 21b of these steel sheets 21 may be the same or different. min When there are a plurality of steel plates 21, the difference W2-W1 between the coating weights W1, W2 of the aluminum-based plating layers 21b, 22b of the steel plates 21, 22 is calculated by referring to the steel plate 21 among the plurality of steel plates 21 that has the largest coating weight W1 of the aluminum-based plating layer 21b.

[0093] In the first embodiment, the mold 40 used for hot stamping the blank 20 includes a punch 41 and a die 42. However, the configuration of the mold 40 is not limited to the example described in the first embodiment. The mold 40 may further include, for example, a pad and a blank holder.

[0094] In the above embodiment, the main body 11 of the structural member 10, 10A includes a front pillar 111, a center pillar 112, and a rocker 113. However, the member main body 11 may further include other components. For example, as shown in FIG. 10 , the member main body 11 may further include a rear pillar 114. The structural members 10, 10A according to the above embodiment are door ring components having a single ring shape (single door ring component). On the other hand, the structural member shown in FIG. 8 is a door ring component having a double ring shape (double door ring component). When manufacturing double door ring components, the blank used as the raw material also has a double ring shape.

[0095] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to the following examples.

[0096] [First Example] In order to confirm the effects of the present disclosure, a CAE analysis was performed on a press-formed (hot stamped) structural member that is a single door ring part, using commercially available software (AUTOFORM R.10, manufactured by AUTOFORM) while changing the type (material type) and thickness of the steel plate included in the structural member, as well as the division pattern of the structural member.

[0097] The steel plates used in this analysis are shown in Table 1.

[0098]

[0099] In Table 1, the material type is listed in the order of plating type, tensile strength, and application (hot stamping). However, in cases where a black coating containing carbon (C) is provided on the plating layer, the material type is prefixed with the words "black coating (one side)" or "black coating (both sides)." "Black coating (one side)" means that one entire side of the plated steel sheet is covered with a black coating. "Black coating (both sides)" means that both entire sides of the plated steel sheet are covered with a black coating. In Table 1, the coating weight of the plating layer is shown as a value per side, but in this analysis, the coating weight of the plating layer is the same on both sides of the material.

[0100] The division patterns of the structural members are shown in Figures 11A to 11G. Figures 11A to 11G show the number of steel plates (materials) included in the structural member, which is a single door ring component, and the positions of the joints between the steel plates in the structural member. In Figures 11A to 11G, each steel plate is given a number in parentheses.

[0101] The analysis conditions and results for division patterns 1 and 2 shown in Figures 11A and 11B are shown in Table 2. In Figures 11A and 11B, the structural member is formed from three pieces of material (1) to (3).

[0102]

[0103] Referring to Table 2, in Example 1, the coating weight of the aluminum-based plating layer on both surfaces of the base steel sheet was the minimum thickness t minIn Example 2, the coating weight of the aluminum-based plating layer is small for the material (3) having a thickness of 1.2 mm, and is large for the other materials (1) and (2) having a thickness larger than that of the material (3). min In Example 3, the coating weight of the aluminum-based plating layer is small for the material (1) having a thickness of 1.2 mm, and is large for the other material (3) having a thickness larger than that of the material (1). min The coating weight of the aluminum-based plating layer is small for the material (2) having a thickness of 1.2 mm, and is large for the other materials (1) and (3) having a thickness larger than that of the material (2). On the other hand, in Comparative Examples 1 and 2, the coating weights of the aluminum-based plating layer are equal for the materials (1) to (3).

[0104] In Table 2, the "time to reach 910°C" indicates the time to reach 910°C (A) the fastest among the materials contained in the blank. c3 The "phase transformation start time" is the shortest time required for the blank to start transforming to ferrite after it is heated at a furnace temperature of 920°C for 5 minutes and 30 seconds and removed from the heating furnace. The "plating thickness difference" is the minimum time required for the blank to start transforming to ferrite after it is heated at a furnace temperature of 920°C for 5 minutes and 30 seconds and removed from the heating furnace. min The adhesion mass of the aluminum-based plating layer on a material having a thickness greater than the thickness of the aluminum-based plating layer (thickness t min In cases where there are multiple materials with a thickness greater than 100 mm and the coating weights of the aluminum-based plating layer differ between these materials, this is the difference between the coating weight and the maximum coating weight. Table 2 shows that in Examples 1 to 3, in which the coating weight of the aluminum-based plating layer on the thinnest material was made smaller than the coating weight of the aluminum-based plating layer on one or more other materials, the time to reach 910°C was 20 seconds or more shorter than in Comparative Examples 1 and 2, and the temperature rise rate of the thinnest material in the heating process was higher. Furthermore, in Examples 1 to 3, the phase transformation start time exceeded 20 seconds, which was later than in Comparative Examples 1 and 2. This makes it easier to start forming the blank before the onset of ferrite transformation, enabling the blank to be uniformly quenched in the forming process.

[0105] The analysis conditions and results for division patterns 3 and 4 shown in Figures 11C and 11D are shown in Table 3. In Figures 11C and 11D, the structural member is formed from four pieces of material (1) to (4).

[0106]

[0107] Referring to Table 3, in Examples 4 to 10, the minimum plate thickness t min The coating weight of the aluminum-based plating layer on the material having the minimum plate thickness t is smaller than the coating weight of the aluminum-based plating layer on any one or more of the other materials. min In the case where there are a plurality of materials having the same thickness, the coating weight of the aluminum-based plating layer of each of these materials is set to be less than the coating weight of the aluminum-based plating layer of the material having the smallest thickness t min In Examples 6 and 9 and Comparative Example 5, the base material (1) is a galvannealed steel sheet (GA-plated steel sheet).

[0108] From Table 3, it can be seen that in Examples 4 to 10, the time to reach 910°C was 20 seconds or more shorter than in Comparative Examples 3 to 7, and the temperature rise rate of the thinnest material in the heating process was higher. Furthermore, in Examples 4 to 10, the phase transformation start time exceeded 20 seconds, which was later than in Comparative Examples 3 to 7. This made it easier to start forming the blank before the onset of ferrite transformation, and made it possible to uniformly quench the blank in the forming process.

[0109] In Examples 4, 5, and 10, the minimum plate thickness t min In Examples 4, 5, and 10, the minimum thickness t minIn comparison with Examples 6 to 9 in which a black coating was not applied to the material having the above thickness, the time to reach 910°C was shortened by 20 seconds or more, and the temperature rise of the thinnest material in the heating process was even faster. In addition, in Examples 4, 5, and 10, the phase transformation start time was also delayed compared with Examples 6 to 9. Therefore, the minimum plate thickness t min By increasing the emissivity of the surface of the material having the above-mentioned structure by using a black coating in advance, the temperature rise of the material can be accelerated, and the start of transformation into the ferrite phase can be further delayed.

[0110] The analysis conditions and results for division patterns 5 to 7 shown in Figures 11E to 11G are shown in Table 4. In Figures 11E to 11G, the structural member is formed from five pieces of material (1) to (5).

[0111]

[0112] Referring to Table 4, in Examples 11 to 15, the minimum plate thickness t min The coating weight of the aluminum-based plating layer on the material having the minimum plate thickness t is smaller than the coating weight of the aluminum-based plating layer on any one or more of the other materials. min In the case where there are a plurality of base materials having the above-mentioned thickness, the coating weights of the aluminum-based plating layers of all of these base materials are set to be less than the coating weights of the aluminum-based plating layers of the base materials having a greater thickness. On the other hand, in Comparative Examples 8 to 11, the coating weights of the aluminum-based plating layers of the base materials (1) to (5) are equal to each other.

[0113] Table 4 shows that in Examples 11 to 15, the time to reach 910°C was 20 seconds or more shorter than in Comparative Examples 8 to 11, and the temperature rise rate of the thinnest material in the heating process was higher. Furthermore, in Examples 11 to 15, the phase transformation start time was slower than in Comparative Examples 8 to 11. This makes it easier to start forming the blank before the ferrite transformation begins, and makes it possible to uniformly harden the blank in the forming process.

[0114] In Examples 12 and 14, the minimum plate thickness t min In Example 12, the material (1) has a minimum plate thickness tmin In the material (5) having the same division pattern, material type (excluding coating weight), and plate thickness, one side is coated with a black coating. For example, when Example 12 is compared with Comparative Example 9, which has the same combination of division pattern, material type (excluding coating weight), and plate thickness, the time to reach 910°C in Example 12 is shorter by more than 40 seconds, and the temperature rise of the thinnest material in the heating process is significantly faster. In addition, in Example 12, the phase transformation start time is also clearly slower than in Comparative Example 9. Therefore, the minimum plate thickness t min By increasing the emissivity of the surface of the material having the above-mentioned structure by using a black coating in advance, the temperature rise of the material can be accelerated, and the start of transformation into the ferrite phase can be further delayed.

[0115] In each of the examples and comparative examples shown in Tables 2 to 4, the materials are butted together and then laser-joined (butt welding). On the other hand, in each of the examples shown in Table 5 below, some of the materials are joined by, for example, spot welding to form overlapping portions.

[0116]

[0117] Referring to Table 5 and Figure 11F, in Examples 16 and 18 and Comparative Example 12, material (2) and material (5), material (3) and material (4), and material (4) and material (5) form overlapping portions at their joints. Referring to Table 5 and Figure 11E, in Examples 17 and 19 and Comparative Examples 13 and 14, material (2) and material (5), and material (3) and material (4) form overlapping portions at their joints.

[0118] Referring to Table 5, in Examples 16 to 19, the minimum plate thickness t min In Examples 16 and 17, the difference in plating thickness between the thinnest material and the other materials was 40 g / m 2 In Examples 18 and 19, the difference in plating thickness between the thinnest material and the other materials was 60 g / m 2 , 20 g / m 2On the other hand, in Comparative Examples 12 and 13, the coating weights of the aluminum-based plating layers of the materials (1) to (5) are equal to each other. min The coating mass of the aluminum-based plating layer on the material (4) having the above thickness is greater than the coating mass of the aluminum-based plating layer on the other materials (1), (2), and (5) having a greater plate thickness. In Comparative Example 14, the difference in plating thickness between the thinnest material and the other materials is -20 g / m 2 is.

[0119] As shown in Table 5, in Examples 16 to 19, the time to reach 910°C was 20 seconds or more shorter than in Comparative Examples 12 to 14, and the phase transformation initiation time was also delayed. Therefore, it was confirmed that even when an overlap portion is present in the blank, the same effect as in the case of butt joining can be obtained by reducing the adhesion amount of the aluminum-based plating layer on the thinnest material. In particular, in Examples 16 and 18, in which a black coating was applied to both sides of the thinnest material, the time to reach 910°C was 40 seconds or more shorter than in Comparative Examples 12 to 14, and the phase transformation initiation time was even later.

[0120] In Example 19, the difference in plating thickness between the thinnest material and the other materials was 20 g / m 2 It was also confirmed that in Example 19, the time to reach 910°C was significantly shorter than in Comparative Examples 12 to 14, and the time to start phase transformation was also significantly delayed.

[0121] Second Example Regarding the press forming (hot stamping) of a structural member that is a double door ring part, an analysis similar to that of the first example was carried out while changing the material type and plate thickness of the structural member, as well as the division pattern of the structural member.

[0122] As with the first embodiment, the steel plates used as raw materials were selected from those shown in Table 1. The division pattern of the structural members is as shown in Figures 12A to 12D. Figures 12A to 12D show the number of steel plates (raw materials) included in the structural members that are double door ring components, and the positions of the joints between the steel plates in the structural members. In Figures 12A to 12D, each steel plate used as raw material is given a number in parentheses.

[0123] The analysis conditions and results for division patterns 8 and 9 shown in Figures 12A and 12B are shown in Table 6. In Figures 12A and 12B, the structural member is formed from six materials (1) to (6).

[0124]

[0125] Referring to Table 6, in Examples 20 to 22, the minimum plate thickness t min In Examples 20 to 22, the coating weight of the aluminum-based plating layer on the material having a thickness difference of 20 g / m 2 On the other hand, in Comparative Example 15, the coating weights of the aluminum-based plating layers of the materials (1) to (6) are equal to each other. min The coating weight of the aluminum-based plating layer on the other material is greater than that on the material having the same thickness, and the plating thickness difference is -20 g / m 2 It is as follows.

[0126] Table 6 shows that in Examples 20 to 22, the time to reach 910°C was approximately 20 seconds shorter than in Comparative Examples 15 and 16, and the temperature rise rate of the thinnest material in the heating step was higher. Furthermore, in Examples 20 to 22, the phase transformation start time was slower than in Comparative Examples 15 and 16. Therefore, it can be said that by reducing the adhesion amount of the aluminum-based plating layer on the thinnest material, it becomes easier to start forming the blank before the onset of ferrite transformation, and it becomes possible to uniformly quench the blank in the forming step.

[0127] The analysis conditions and results for division patterns 10 and 11 shown in Figures 12C and 12D are shown in Table 7. In Figures 12C and 12D, the structural member is formed from seven pieces of material (1) to (7).

[0128]

[0129] Referring to Table 7, in Examples 23 to 25, the minimum plate thickness t minOn the other hand, in Comparative Examples 17 and 18, the coating weights of the aluminum-based plating layer in the materials (1) to (7) are equal to each other.

[0130] From Table 7, it can be seen that in Examples 23 to 25, the time to reach 910°C was shorter and the temperature rise rate of the thinnest material in the heating process was higher compared to Comparative Examples 17 and 18. Furthermore, in Examples 23 to 25, the phase transformation start time was slower than in Comparative Examples 17 and 18. Therefore, it becomes easier to start forming the blank before the start of ferrite transformation, and it becomes possible to uniformly quench the blank in the forming process.

[0131] [Example 3] To confirm the influence of plate thickness on the press forming (hot stamping) of a structural member that is a single door ring part, an analysis similar to that of Example 1 was carried out while changing the combination of materials and the joining mode. The analysis conditions and results are shown in Table 8.

[0132]

[0133] The division pattern of Test Examples 1 and 5 is division pattern 7 shown in FIG. 11G. The division pattern of Test Example 4 is division pattern 5 shown in FIG. 11E. In Test Examples 1, 4, and 5, some of the materials form overlapping portions at the joints. More specifically, in Test Examples 1 and 5, material (1) and material (2), material (1) and material (3), material (2) and material (5), and material (4) and material (5) each form overlapping portions at the joints. In Test Example 4, material (1) and material (2), material (1) and material (3), material (3) and material (4), and material (2) and material (5) each form overlapping portions at the joints. In all of these test examples, the minimum plate thickness t min The coating weight of the aluminum-based plating layer on the material having the thickness is smaller than the coating weight of the aluminum-based plating layer on one or more of the materials having a larger thickness.

[0134] The division pattern of Test Examples 2, 3, and 6 is Division Pattern 7 shown in FIG. 11G. In Test Examples 2, 3, and 6, the materials are joined by butt welding. In all of these Test Examples, the minimum plate thickness t min The coating weight of the aluminum-based plating layer on the material having the thickness is smaller than the coating weight of the aluminum-based plating layer on one or more of the materials having a larger thickness.

[0135] The "process window (PW)" in Table 8 is the value obtained by subtracting the time required for the entire blank to reach 910°C after the earliest temperature reached 910°C from the heating time that can be tolerated for the material contained in the blank that reached 910°C first. If the process window is 5 seconds or less, alloying of the plating layer of the material that reached 910°C first in the heating process will progress, making it impossible to ensure the corrosion resistance of the plating layer and making it difficult to manufacture a structural component with good quality.

[0136] As shown in Table 8, the minimum plate thickness t min Maximum plate thickness t max Ratio of: t max / t min In Test Examples 5 and 6, where t exceeded 3.2, the process window was negative, and it was not possible to ensure the process window necessary for satisfactory manufacturing of structural members. max / t min In Test Examples 1 to 4 where the value was 3.2 or less, a process window of 5 seconds or more could be secured.

[0137] As shown in Table 8, in Test Example 5, where the maximum total plate thickness t of the overlap portion exceeded 4.0 mm, the process window was negative and it was not possible to ensure the process window necessary for satisfactory manufacturing of structural members. On the other hand, in Test Examples 1 and 4, where the maximum total plate thickness t of the overlap portion was 4.0 mm or less, a process window of 5 seconds or more was ensured.

[0138] Reference Example 1 is an example of division pattern 5 similar to Test Example 4, but there is no difference in the coating weight of the aluminum-based plating layer between the materials. However, in Reference Example 1, there is no difference in plate thickness between the materials, and the problem of alloying progression of the plating layer in the thinnest material does not occur, so a process window of 5 seconds or more could be ensured.

[0139] For Test Examples 1 to 4 and Comparative Examples 11 and 13A, the blanks were heated at a furnace temperature of 920°C until the entire blank reached 910°C. Then, the blanks were transferred to a press in 17 seconds, hot stamped at a forming speed of 40 mm / s, and held at bottom dead center for 20 seconds while applying a pressure of 3000 kN to obtain hot-stamped structural components. Analysis samples were taken from the thinnest portions of these structural components using the method described in the above embodiment, and the martensite fraction variation was measured. Furthermore, shape accuracy and impact absorption performance measurements were also conducted on these structural components. The evaluation results are shown in Table 9.

[0140]

[0141] In Table 9, the variation in martensite fraction is, as explained in the above embodiment, the variation in the minimum plate thickness t min The martensite fraction (%) is the maximum martensite fraction (%) minus the minimum martensite fraction (%) in the cross section of the structural member at the location of the material having the martensite fraction (%).

[0142] The shape accuracy was evaluated by measuring the distance between the structural member and the mating member at the overlapping portion when the structural member, which is approximately hat-shaped in cross section, is attached to another member. In Table 9, a value of ○ indicates that the distance from the surface of the mating member is within ±2.0 mm, a value of △ indicates that the distance is between ±2.0 mm and ±3.0 mm, and a value of × indicates that the distance is greater than ±3.0 mm.

[0143] Regarding the impact absorption performance, a small overlap (SOL) collision and a side collision were assumed with the structural member assembled to a vehicle, and an impactor simulating a vehicle was collided with the structural member to evaluate the maximum intrusion amount during the SOL collision (maximum SOL intrusion amount) and the maximum intrusion amount during a side collision (maximum side impact intrusion amount). The impact absorption performance was evaluated based on the impact absorption performance of a door ring component formed by hot stamping each material and then joining them, and compared with the impact absorption performance of the base. In Table 9, impact absorption performance equivalent to the impact absorption performance of the base is represented by "good," impact absorption performance superior to the base impact absorption performance is represented by "better," impact absorption performance slightly lower than the base impact absorption performance is represented by "marginal," and impact absorption performance even lower than the base impact absorption performance is represented by "poor."

[0144] Comparative Example 11 is a comparative example of the first embodiment, and similar to Test Example 2, the materials were butt-joined by laser welding. Comparative Example 13A is the same plate assembly as Comparative Example 13 of the first embodiment, but similar to Test Example 4, the materials were partially overlap-joined. Unlike each test example, in Comparative Examples 11 and 13A, the coating weight of the plating layer on the thinnest material was equal to the coating weight of the plating layer on the other materials. As shown in Table 9, the variation in martensite fraction was 20% or less in all of Test Examples 1 to 4, and the variation in martensite fraction was significantly reduced compared to Comparative Examples 11 and 13A. Test Examples 1 to 4 also had better shape accuracy than Comparative Examples 11 and 13A.

[0145] Test Examples 1 to 4, which had small variations in the martensite fraction, also had improved impact absorption performance compared to Comparative Examples 11 and 13A. In particular, Test Examples 1, 2, and 4, which had variations in the martensite fraction of 15% or less, were able to ensure impact absorption performance equal to or greater than that of the base. In other words, even though multiple materials were integrated at the blank stage to form an annular structural member, they were able to ensure impact absorption performance equal to or greater than that of a structural member formed by press-molding the materials individually and then joining them. Among Test Examples 1 to 4, Test Example 2 had the best impact absorption performance. Test Example 2 demonstrated high impact absorption performance, especially in side collisions.

[0146] 10, 10A: Structural member 11: Member body 20, 20A, 20B, 20C: Blank 21: Steel plate (first steel plate) 21a: Base steel plate 21b: Aluminum-based plating layer 22: Steel plate (second steel plate) 22a: Base steel plate 22b: Aluminum-based plating layer 23: Steel plate (third steel plate) 23a: Base steel plate 23b: Aluminum-based plating layer 24, : Steel plate 24a: Base steel plate 24b: Aluminum-based plating layer 25: Steel plate 26: Overlap portion 27: Coating 40: Mold 111: Front pillar 112: Center pillar 113: Rocker

Claims

1. A blank for hot stamping, comprising a plurality of steel sheets arranged and joined to have an annular shape in a plan view of the blank, the plurality of steel sheets including a first steel sheet having a minimum sheet thickness among the plurality of steel sheets, and a second steel sheet having a sheet thickness greater than that of the first steel sheet, the first steel sheet and the second steel sheet each being a plated steel sheet having a base steel sheet and an aluminum-based plating layer covering both surfaces of the base steel sheet, and a coating amount (g / m) of the aluminum-based plating layer on both surfaces of the base steel sheet in the first steel sheet 2 ) is the adhesion amount (g / m) of the aluminum-based plating layer on both surfaces of the base steel sheet in the second steel sheet. 2 ) less than blank.

2. The blank according to claim 1, wherein the thickness of the first steel plate is t min The thickness of the steel plate having the largest thickness among the plurality of steel plates is t max When 1.0<t max / t min ≦3.2, blank.

3. A blank according to claim 1, further comprising an overlap portion formed by overlapping ends of two adjacent steel sheets among the plurality of steel sheets, the overlap portion having a total sheet thickness of 4.0 mm or less, the two steel sheets being plated steel sheets each having a base steel sheet and an aluminum-based plating layer covering both surfaces of the base steel sheet, and the adhesion amount (g / m2) of the aluminum-based plating layer on both surfaces of the base steel sheet in each of the two steel sheets being 2 ) is the adhesion amount (g / m) of the aluminum-based plating layer on both surfaces of the base steel sheet in the second steel sheet. 2 ) less than blank.

4. A blank according to claim 3, wherein the surface of at least one of the two steel plates located outside the overlapping portion is coated with a black coating.

5. A blank according to claim 1, wherein at least one surface of the first steel plate is coated with a black coating.

6. A method for manufacturing a structural component, comprising the steps of: preparing a blank as described in any one of claims 1 to 5; heating the multiple steel plates contained in the blank to a temperature equal to or higher than the austenite transformation completion temperature; and using a die to form the heated blank into a structural component that is annular in plan view and quenching it.

7. A structural component comprising a component body having an annular shape in a plan view, the component body being formed by a plurality of steel plates joined together, the first steel plate having a minimum thickness and a second steel plate having a thickness greater than that of the first steel plate, the first steel plate and the second steel plate being plated steel plates each having an aluminum-based plating layer on both surfaces of a base steel plate, the thickness of the aluminum-based plating layer in the first steel plate being smaller than the thickness of the aluminum-based plating layer in the second steel plate.

8. A structural member according to claim 7, which is a door ring part of an automobile, and the member body includes a front pillar, a center pillar, and a rocker connecting the front pillar and the center pillar.

Citation Information

Patent Citations

  • Vehicle body side structural frame

    JP2021528248A

  • Overlapped blank for hot stamping, method for manufacturing overlapped hot-stamped product, and overlapped hot-stamped product

    JP6642777B1

  • Steel sheet for hot stamping and hot-stamped member

    WO2022215229A1

  • Steel sheet for radiation heating, which is suitable to produce metallic processed article having portion with different strength and which is used for hot stamping and method of producing the same

    JP2011152589A

  • Tailored blank for hot stamping

    JP2013204090A