Binder composition for secondary battery electrode, slurry composition for secondary battery electrode, secondary battery electrode, and secondary battery

The use of a binder composition with nitrile group-containing and ethylenically unsaturated carboxylic acid ester monomer units in secondary battery electrodes addresses crater formation issues, reducing internal resistance and improving cycle characteristics by controlling film thickness and adhesion.

WO2024225332A1PCT designated stage expired Publication Date: 2024-10-31ZEON CORP

Patent Information

Application Number
PCT/JP2024/016123
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional binder compositions for secondary battery electrodes often result in crater formation on the electrode surface, leading to increased internal resistance and deteriorated cycle characteristics in secondary batteries.

Method used

A binder composition with specific properties, including a particulate polymer containing nitrile group-containing monomer units and ethylenically unsaturated carboxylic acid ester monomer units, is used, which forms a film with controlled thickness to prevent crater formation and improve electrode performance.

Benefits of technology

The proposed binder composition effectively suppresses crater formation, reduces internal resistance, and enhances cycle characteristics of secondary batteries by controlling film formation and improving the adhesion of electrode active materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The purpose of the present invention is to provide a binder composition for a secondary battery electrode with which it is possible to form an electrode for a secondary battery in which crater formation on an electrode surface is suppressed, reduce internal resistance of the secondary battery, and realize excellent cycle characteristics. A binder composition for a secondary battery electrode according to the present invention contains a binding material, and when 10.0 g of a mixed liquid that is obtained by adjusting the binder composition for the secondary battery electrode with water so as to have a solid content concentration of 30 mass% is poured into a polytetrafluoroethylene Petri dish having a diameter of 10 cm, the amount of a coating film after standing for 2 hours at a temperature of 40°C is 1.3 g or less.
Need to check novelty before this filing date? Find Prior Art

Description

Binder composition for secondary battery electrodes, slurry composition for secondary battery electrodes, electrode for secondary battery, and secondary battery

[0001] The present invention relates to a binder composition for a secondary battery electrode, a slurry composition for a secondary battery electrode, an electrode for a secondary battery, and a secondary battery.

[0002] Secondary batteries, such as nonaqueous electrolyte secondary batteries using an organic solvent electrolyte (hereinafter sometimes abbreviated as "nonaqueous secondary batteries") and all-solid-state secondary batteries using a solid electrolyte instead of an organic solvent electrolyte, are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are therefore used in a wide range of applications. Therefore, in recent years, improvements to battery components such as electrodes have been studied in order to further improve the performance of secondary batteries.

[0003] Here, an electrode for a secondary battery typically includes a current collector and an electrode mixture layer (positive electrode mixture layer or negative electrode mixture layer) formed on the current collector. The electrode mixture layer is formed, for example, by applying a slurry composition for a secondary battery electrode (hereinafter sometimes abbreviated as "slurry composition") onto the current collector, the slurry composition being obtained by dispersing an electrode active material and a binder composition for a secondary battery electrode (hereinafter sometimes abbreviated as "binder composition") containing a binder in a dispersion medium, and then drying the applied slurry composition.

[0004] Therefore, in recent years, attempts have been made to improve the binder compositions used to form electrode mixture layers in order to achieve further performance improvements in secondary batteries. For example, Patent Document 1 discloses an electrode binder composition having a spherical volume equivalent diameter of 3 μm or more and a concentration of coarse particles and / or aggregates of 2000 ppm or less. According to Patent Document 1, the use of this binder composition makes it possible to stably manufacture batteries with high capacity retention, even when the manufacturing process is speeded up or the current collector roll length is increased.

[0005] JP 2011-76917 A

[0006] When an electrode mixture layer is formed using a slurry composition containing the conventional binder composition, minute defects (hereinafter referred to as "craters"), such as circular depressions, may occur on the electrode surface. When an electrode with such craters is used, the internal resistance of the secondary battery increases and the cycle characteristics deteriorate.

[0007] Therefore, an object of the present invention is to provide a binder composition for a secondary battery electrode and a slurry composition for a secondary battery electrode that can form a secondary battery electrode in which crater formation on the electrode surface is suppressed, and that can reduce the internal resistance of the secondary battery and exhibit excellent cycle characteristics. Another object of the present invention is to provide ... with reduced internal resistance and excellent cycle characteristics.

[0008] The present inventors have conducted extensive research to solve the above problems, and have found that by using a binder composition in which the amount of a coating formed when the binder composition is allowed to stand under predetermined conditions is equal to or less than a predetermined value, it is possible to form an electrode in which crater formation is suppressed and a secondary battery in which internal resistance is reduced and which has excellent cycle characteristics, and have completed the present invention.

[0009] That is, an object of the present invention is to advantageously solve the above-mentioned problems, and according to the present invention, there are provided the following binder compositions for secondary battery electrodes [1] to [6], the following slurry composition for secondary battery electrodes [7], the following secondary battery electrode [8], and the following secondary battery [9].

[0010] [1] A binder composition for secondary battery electrodes containing a binder, the binder composition being prepared by pouring 10.0 g of a mixture of the binder composition for secondary battery electrodes, prepared by adjusting the solids concentration with water to 30% by mass, into a 10 cm diameter polytetrafluoroethylene petri dish, and leaving the mixture at 40°C for 2 hours, after which the coating weight is 1.3 g or less. A binder composition having a coating weight of the above value or less under specified conditions can produce an electrode in which crater formation on the surface is suppressed. Furthermore, an electrode produced in this manner can exhibit excellent cycle characteristics while reducing the internal resistance of the secondary battery. In the present invention, the "coating weight" can be measured using the method described in the examples of this specification.

[0011] [2] The binder composition for secondary battery electrodes according to [1], wherein the binder comprises a particulate polymer, the particulate polymer comprising nitrile group-containing monomer units in a proportion of 1% by mass to 9% by mass and ethylenically unsaturated carboxylic acid ester monomer units in a proportion of 1% by mass to 9% by mass. When the binder composition contains a particulate polymer containing the nitrile group-containing monomer units and the ethylenically unsaturated carboxylic acid ester monomer units in the above-described proportions, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while improving the cycle characteristics. In the present invention, the "monomer unit" of a polymer refers to the "repeating unit derived from that monomer contained in a polymer obtained using that monomer." In the present invention, the content of the monomer unit in a polymer can be measured using the method described in the examples of this specification.

[0012] [3] The binder composition for a secondary battery electrode according to [2] above, wherein the particulate polymer is a random copolymer. When the particulate polymer contained in the binder composition is a random copolymer, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while the cycle characteristics can be further improved.

[0013] [4] The binder composition for secondary battery electrodes according to [2] or [3] above, wherein the ratio (Da / Db) of Da to Db (nm), where Da (nm) is the average particle diameter of the particulate polymer measured by dynamic light scattering and Db (nm) is the volume-average particle diameter of the particulate polymer measured by laser diffraction scattering, is 1.1 or more and 2.0 or less. When Da / Db is within the above-mentioned range, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics. Furthermore, the peel strength of the electrode can be improved. In the present invention, the "average particle diameter Da" of the particulate polymer means "the particle diameter (D50) at which the cumulative frequency of light scattering intensity calculated from the small diameter side in the particle size distribution measured by dynamic light scattering becomes 50% when measured from the small diameter side," and can be measured using the method described in the examples of this specification. In the present invention, the "volume average particle diameter Db" of the particulate polymer means "a particle diameter (D50) at which the cumulative volume calculated from the small diameter side in the particle size distribution (volume basis) measured by a laser diffraction scattering method becomes 50%," and can be measured using the method described in the examples of the present specification.

[0014] [5] The binder composition for secondary battery electrodes according to any one of [1] to [4] above, having a viscosity of 60 mPa·s or more and 3000 mPa·s or less at a solids concentration of 30% by mass. A binder composition having a viscosity of 60 mPa·s or more and 3000 mPa·s or less at a solids concentration of 30% by mass can further suppress crater formation on the electrode surface, further reduce the internal resistance of the secondary battery, and further improve the cycle characteristics. It can also improve the peel strength of the electrode. In the present invention, the "viscosity" of the binder composition at a solids concentration of 30% by mass can be measured using the method described in the Examples section of this specification.

[0015] [6] The binder composition for a secondary battery electrode according to any one of [1] to [5] above, further comprising water and having a pH of 6 or more and 10 or less. When the pH of the binder composition is within the above-mentioned range, it is possible to further suppress crater formation on the electrode surface, further reduce the internal resistance of the secondary battery, and further improve the cycle characteristics. It is also possible to improve the peel strength of the electrode. In the present invention, the "pH" of the binder composition means the pH measured under conditions of a temperature of 25°C.

[0016] [7] A slurry composition for a secondary battery electrode, comprising an electrode active material and the binder composition for a secondary battery electrode described in any one of [1] to [6] above. The slurry composition containing the electrode active material and any one of the binder compositions described above can produce an electrode in which crater formation on the surface is suppressed. Furthermore, the electrode produced in this manner can exhibit excellent cycle characteristics while reducing the internal resistance of the secondary battery.

[0017] [8] A secondary battery electrode comprising an electrode mixture layer formed using the slurry composition for a secondary battery electrode described in [7] above. An electrode comprising an electrode mixture layer obtained using a slurry composition containing an electrode active material and any of the binder compositions described above suppresses crater formation on the electrode surface. Furthermore, this electrode can reduce the internal resistance of the secondary battery while exhibiting excellent cycle characteristics.

[0018] [9] A secondary battery comprising the electrode for a secondary battery according to [8] above. By using the electrode for a secondary battery described above, a secondary battery having reduced internal resistance and excellent cycle characteristics can be manufactured.

[0019] According to the present invention, it is possible to provide a binder composition for a secondary battery electrode and a slurry composition for a secondary battery electrode that can form a secondary battery electrode in which crater formation on the electrode surface is suppressed, and that can reduce the internal resistance of the secondary battery and exhibit excellent cycle characteristics. Furthermore, according to the present invention, it is possible to provide a secondary battery electrode in which crater formation on the electrode surface is suppressed, and that can reduce the internal resistance of the secondary battery and exhibit excellent cycle characteristics. Furthermore, according to the present invention, it is possible to provide a secondary battery in which internal resistance is reduced and excellent cycle characteristics are exhibited.

[0020] Hereinafter, embodiments of the present invention will be described in detail. Here, the binder composition of the present invention can be used to prepare the slurry composition of the present invention. The slurry composition of the present invention can be used to form an electrode (secondary battery electrode) for a secondary battery such as a non-aqueous secondary battery or an all-solid-state secondary battery. Furthermore, the electrode of the present invention is characterized by comprising an electrode mixture layer formed from the slurry composition of the present invention. Furthermore, the secondary battery of the present invention is characterized by comprising an electrode produced using the slurry composition of the present invention.

[0021] (Binder composition for secondary battery electrodes) The binder composition of the present invention contains a binder and may optionally contain a solvent. The binder composition of the present invention may further contain components (other components) other than the binder and the solvent. Here, the binder composition of the present invention is characterized in that 10.0 g of a mixed solution prepared with water so that the solids concentration of the binder composition becomes 30 mass % is poured into a polytetrafluoroethylene petri dish having a diameter of 10 cm, and the coating weight after being left to stand under specified conditions is 1.3 g or less.

[0022] Furthermore, since the coating amount of the binder composition of the present invention is equal to or less than the above value, use of the binder composition can suppress the formation of craters on the electrode surface, reduce the internal resistance of the secondary battery, and enable the secondary battery to exhibit excellent cycle characteristics. Although the reason why the above effects are obtained by using the binder composition of the present invention is not clear, it is presumed to be as follows.

[0023] First, the pH of a binder composition may decrease during storage due to factors such as air oxidation and decay. The inventors' investigations have revealed that this decrease in pH weakens the electrostatic repulsion between solid components (e.g., binders) in the binder composition, causing the solid components to aggregate through hydrophobic interactions to form a coating. It is believed that such a coating swells and becomes flexible in the solvent of the binder composition and / or slurry composition, passing through filters used to remove foreign matter during the preparation of the slurry composition and the formation of the electrode mixture layer, causing craters on the electrode surface and adversely affecting the internal resistance and cycle characteristics of the secondary battery. In contrast, the binder composition of the present invention produces a coating amount of 1.3 g or less under specified conditions, thereby suppressing the formation of such a coating during storage. Therefore, it is believed that use of the binder composition of the present invention can suppress crater formation on the electrode surface and reduce the internal resistance of a secondary battery while exhibiting excellent cycle characteristics.

[0024] <Binder> The binder prevents components such as the electrode active material from being detached from the electrode mixture layer formed using a slurry composition containing the binder composition. The binder is not particularly limited as long as it can be used in a secondary battery. For example, the binder can be a polymer obtained by polymerizing a monomer composition containing a monomer capable of exhibiting binding properties. Note that one type of binder may be used alone, or two or more types may be used in combination at any ratio. Particulate polymers suitable for use as binders will be described in detail below.

[0025] <<Particulate Polymer>> The particulate polymer is a water-insoluble particle made of a predetermined polymer. In the present invention, the term "water-insoluble" for polymer particles means that when 0.5 g of the polymer is dissolved in 100 g of water at 25°C, the insoluble content is 90 mass % or more.

[0026] Here, the particulate polymer is not particularly limited as long as it is water-insoluble and dispersible in a solvent such as water. However, from the viewpoint of further suppressing crater formation on the electrode surface and further reducing the internal resistance of the secondary battery while further improving the cycle characteristics, the particulate polymer preferably contains at least one of a nitrile group-containing monomer unit and an ethylenically unsaturated carboxylic acid ester monomer unit, and more preferably contains both a nitrile group-containing monomer unit and an ethylenically unsaturated carboxylic acid ester monomer unit. Note that the particulate polymer may optionally further contain monomer units other than the nitrile group-containing monomer unit and the ethylenically unsaturated carboxylic acid ester monomer unit (hereinafter sometimes referred to as "other monomer units").

[0027] [Nitrile Group-Containing Monomer Unit] Examples of nitrile group-containing monomers that can form nitrile group-containing monomer units include α,β-ethylenically unsaturated nitrile monomers. Specifically, the α,β-ethylenically unsaturated nitrile monomer is not particularly limited as long as it is an α,β-ethylenically unsaturated compound having a nitrile group. Examples include acrylonitrile; α-halogenoacrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; and α-alkylacrylonitriles such as methacrylonitrile and α-ethylacrylonitrile. Among these, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred, from the viewpoints of further suppressing crater formation on the electrode surface and further reducing the internal resistance of the secondary battery while further improving the cycle characteristics. Note that one type of nitrile group-containing monomer may be used alone, or two or more types may be used in combination at any ratio.

[0028] The content of the nitrile group-containing monomer units in the particulate polymer is preferably 1% by mass or more, more preferably 1.5% by mass or more, even more preferably 2% by mass or more, and preferably 9% by mass or less, more preferably 5% by mass or less, and even more preferably 3.5% by mass or less, when the amount of all monomer units in the particulate polymer is taken as 100% by mass. When the content of the nitrile group-containing monomer units in the particulate polymer is equal to or greater than the above-mentioned lower limit, film formation due to aggregation of the particulate polymer can be suppressed. Therefore, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics. On the other hand, when the content of the nitrile group-containing monomer units in the particulate polymer is equal to or less than the above-mentioned upper limit, an excessive increase in the viscosity of the slurry composition can be suppressed, thereby suppressing film formation. Therefore, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics.

[0029] [Ethylenically unsaturated carboxylic acid ester monomer unit] As the ethylenically unsaturated carboxylic acid ester monomer capable of forming the ethylenically unsaturated carboxylic acid ester monomer unit, for example, a monomer consisting of an ester of an ethylenically unsaturated monocarboxylic acid or a monomer consisting of a diester of an ethylenically unsaturated dicarboxylic acid can be used. Here, as the monomer consisting of an ester of an ethylenically unsaturated monocarboxylic acid, for example, a (meth)acrylic acid ester monomer can be mentioned. In addition, in the present invention, "(meth)acrylic" means acrylic and / or methacrylic. Examples of the (meth)acrylic acid ester monomer include alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, t-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, and stearyl acrylate; and alkyl methacrylates such as ethyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate, and glycidyl methacrylate. Furthermore, examples of monomers comprising diesters of ethylenically unsaturated dicarboxylic acids include dialkyl maleates such as diethyl maleate and dibutyl maleate, dialkyl fumarate esters such as diethyl fumarate and dibutyl fumarate, and dialkyl itaconate esters such as diethyl itaconate and dibutyl itaconate.Among these, from the viewpoints of further suppressing crater formation on the electrode surface and further improving cycle characteristics while further reducing the internal resistance of the secondary battery, (meth)acrylic acid ester monomers are preferred, and methyl methacrylate is more preferred. Note that the ethylenically unsaturated carboxylic acid ester monomers may be used alone or in combination of two or more at any ratio.

[0030] The content of the ethylenically unsaturated carboxylic acid ester monomer units in the particulate polymer is preferably 1% by mass or more, more preferably 1.5% by mass or more, even more preferably 2% by mass or more, and preferably 9% by mass or less, more preferably 5% by mass or less, and even more preferably 3.5% by mass or less, when the amount of all monomer units in the particulate polymer is taken as 100% by mass. When the content of the ethylenically unsaturated carboxylic acid ester monomer units in the particulate polymer is equal to or greater than the above-mentioned lower limit, film formation due to aggregation of the particulate polymer can be suppressed. Therefore, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics. On the other hand, when the content of the ethylenically unsaturated carboxylic acid ester monomer units in the particulate polymer is equal to or less than the above-mentioned upper limit, an excessive increase in the viscosity of the slurry composition can be suppressed, thereby suppressing film formation. Therefore, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics.

[0031] [Other Monomer Units] The other monomer units contained in the particulate polymer are not particularly limited.Preferred examples of the other monomer units include aromatic vinyl monomer units, aliphatic conjugated diene monomer units, and acidic group-containing monomer units.Among these, the particulate polymer preferably contains an aliphatic conjugated diene monomer unit as the other monomer unit, and more preferably contains both an aromatic vinyl monomer unit and an aliphatic conjugated diene monomer unit.

[0032] —Aromatic vinyl monomer unit— Examples of aromatic vinyl monomers that can form aromatic vinyl monomer units include aromatic monovinyl compounds such as styrene, α-methylstyrene, p-t-butylstyrene, butoxystyrene, vinyltoluene, chlorostyrene, and vinylnaphthalene. Among these, styrene is preferred. These can be used alone or in combination of two or more, but it is preferable to use one type alone.

[0033] The content of the aromatic vinyl monomer unit in the particulate polymer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, and is preferably 65% ​​by mass or less, more preferably 55% by mass or less, even more preferably 47% by mass or less, and particularly preferably 23% by mass or less, when the amount of all monomer units in the particulate polymer is taken as 100% by mass. If the content of the aromatic vinyl monomer unit in the particulate polymer is not less than the above lower limit, the stability of the slurry composition can be improved. On the other hand, if the content of the aromatic vinyl monomer unit in the particulate polymer is not more than the above upper limit, the peel strength of the electrode can be improved.

[0034] -Aliphatic conjugated diene monomer unit- Examples of aliphatic conjugated diene monomers that can form aliphatic conjugated diene monomer units include conjugated diene compounds having 4 or more carbon atoms, such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene. Among these, 1,3-butadiene and isoprene are preferred, and 1,3-butadiene is more preferred. These can be used alone or in combination of two or more.

[0035] The content of the aliphatic conjugated diene monomer units in the particulate polymer is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, particularly preferably 67% by mass or more, and preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 77% by mass or less, and particularly preferably 72% by mass or less, when the amount of all monomer units in the particulate polymer is taken as 100% by mass. If the content of the aliphatic conjugated diene monomer units in the particulate polymer is not less than the above-mentioned lower limit, the peel strength of the electrode can be improved. On the other hand, if the content of the aliphatic conjugated diene monomer units in the particulate polymer is not more than the above-mentioned upper limit, the stability of the slurry composition can be increased.

[0036] —Acidic Group-Containing Monomer Unit— Examples of acidic group-containing monomers that can form acidic group-containing monomer units include carboxylic acid group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, etc. The acidic group contained in the acidic group-containing monomer unit may form a salt with an alkali metal, ammonia, etc.

[0037] Here, examples of carboxylic acid group-containing monomers capable of forming carboxylic acid group-containing monomer units include monocarboxylic acids and their derivatives, dicarboxylic acids and their acid anhydrides, and their derivatives. Examples of monocarboxylic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of monocarboxylic acid derivatives include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, and α-chloro-β-E-methoxyacrylic acid. Examples of dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of dicarboxylic acid derivatives include methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, and maleic acid monoesters such as nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleates. Examples of dicarboxylic acid anhydrides include maleic anhydride, acrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride. Furthermore, as the carboxylic acid group-containing monomer, an acid anhydride that generates a carboxylic acid group upon hydrolysis can also be used.

[0038] Examples of sulfonic acid group-containing monomers capable of forming sulfonic acid group-containing monomer units include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, styrene sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid. In the present invention, "(meth)allyl" means allyl and / or methallyl.

[0039] Furthermore, examples of the phosphate group-containing monomer capable of forming the phosphate group-containing monomer unit include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate. In the present invention, "(meth)acryloyl" means acryloyl and / or methacryloyl.

[0040] Here, the above-mentioned acidic group-containing monomers may be used alone or in combination of two or more. From the viewpoints of increasing the stability of the slurry composition and improving the peel strength of the electrode, the acidic group-containing monomer capable of forming the acidic group-containing monomer unit is preferably a carboxylic acid group-containing monomer, more preferably a monocarboxylic acid or a dicarboxylic acid, still more preferably acrylic acid, methacrylic acid, or itaconic acid, still more preferably methacrylic acid or itaconic acid, and particularly preferably methacrylic acid.

[0041] The content of the acidic group-containing monomer units in the particulate polymer is preferably 2% by mass or more, more preferably 2.5% by mass or more, preferably 9% by mass or less, more preferably 5% by mass or less, and even more preferably 4% by mass or less, when the amount of all monomer units in the particulate polymer is taken as 100% by mass. When the content of the acidic group-containing monomer units in the particulate polymer is equal to or greater than the above-mentioned lower limit, film formation due to aggregation of the particulate polymer can be suppressed. Therefore, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics. On the other hand, when the content of the acidic group-containing monomer units in the particulate polymer is equal to or less than the above-mentioned upper limit, an excessive increase in the viscosity of the binder composition can be suppressed, thereby suppressing film formation. Therefore, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics.

[0042] [Structure of Particulate Polymer] The particulate polymer may be, for example, any of a random copolymer, a block copolymer, an alternating copolymer, etc. From the viewpoints of further suppressing crater formation on the electrode surface and further improving the cycle characteristics while further reducing the internal resistance of the secondary battery, the particulate polymer is preferably a random copolymer.

[0043] Furthermore, the particulate polymer may be a particulate polymer having a uniform monomer unit composition (type and content ratio of monomer units), or a particulate polymer having a non-uniform monomer unit composition. Examples of particulate polymers having a non-uniform monomer unit composition include particulate polymers having a core-shell structure that has a core portion and a shell portion covering at least a part of the outer surface of the core portion, and in which the core portion and the shell portion have different monomer unit compositions, and particulate polymers in which only the core portion has a different monomer unit composition.

[0044] From the viewpoint of further suppressing the formation of craters on the electrode surface and further improving the cycle characteristics while further reducing the internal resistance of the secondary battery, it is preferable that the particulate polymer has a core-shell structure including a core portion made of a copolymer containing aromatic vinyl monomer units and aliphatic conjugated diene monomer units, and a shell portion made of a polymer containing acidic group-containing monomer units. Note that the core-shell structure of the particulate polymer may further include components other than the core portion and the shell portion, but is preferably made of only the core portion and the shell portion.

[0045] The copolymer constituting the core portion of the core-shell structure of the particulate polymer may contain a monomer unit other than an aromatic vinyl monomer unit and an aliphatic conjugated diene monomer unit, or may contain only an aromatic vinyl monomer unit and an aliphatic conjugated diene monomer unit. Examples of the monomer unit other than an aromatic vinyl monomer unit and an aliphatic conjugated diene monomer unit contained in the copolymer constituting the core portion include acidic group-containing monomer units. Furthermore, the shell portion of the core-shell structure of the particulate polymer may be constituted, for example, by a copolymer containing a monomer unit other than an acidic group-containing monomer unit, or may be constituted by a homopolymer containing only acidic group-containing monomer units. From the viewpoint of further suppressing the formation of craters on the electrode surface and further reducing the internal resistance of the secondary battery while further improving the cycle characteristics, the shell portion of the core-shell structure of the particulate polymer is preferably composed of a copolymer containing an acidic group-containing monomer unit and at least one of a nitrile group-containing monomer unit and an ethylenically unsaturated carboxylic acid ester monomer unit, and more preferably composed of a copolymer containing an acidic group-containing monomer unit, a nitrile group-containing monomer unit and an ethylenically unsaturated carboxylic acid ester monomer unit. In addition, the copolymer constituting the shell portion may contain an aromatic vinyl monomer unit such as a styrene unit.

[0046] When the particulate polymer has a core-shell structure, the proportion of the core portion in the particulate polymer is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, and preferably 98% by mass or less, and more preferably 97.5% by mass or less, when the mass of the entire particulate polymer is taken as 100% by mass. If the proportion of the core portion in the particulate polymer is equal to or greater than the lower limit, the formation of craters on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics. On the other hand, if the proportion of the core portion in the particulate polymer is equal to or less than the upper limit, the peel strength of the electrode can be improved.

[0047] When the particulate polymer has a core-shell structure, the proportion of the shell portion in the particulate polymer is preferably 2% by mass or more, more preferably 2.5% by mass or more, preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, when the mass of the entire particulate polymer is taken as 100% by mass. When the proportion of the shell portion in the particulate polymer is equal to or greater than the above-mentioned lower limit, the peel strength of an electrode formed using the binder composition can be improved. On the other hand, when the proportion of the shell portion in the particulate polymer is equal to or less than the above-mentioned upper limit, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics.

[0048] [Properties of Particulate Polymer] -Average Particle Diameter Da Measured by Dynamic Light Scattering Method- The average particle diameter Da of the particulate polymer is preferably 100 nm or more, more preferably 130 nm or more, even more preferably 150 nm or more, preferably 340 nm or less, more preferably 300 nm or less, even more preferably 260 nm or less, and particularly preferably 240 nm or less. The value of the average particle diameter Da measured by dynamic light scattering method is a value that relatively strongly reflects the spatial spread of the molecular chains in the surface layer portion of the particulate polymer. That is, when the particulate polymer has, for example, the above-mentioned core-shell structure, it is presumed that the value of the average particle diameter Da of the particulate polymer depends on the particle diameter of the entire core-shell structure of the particulate polymer. Therefore, the value of the average particle diameter Da of the particulate polymer can be adjusted, for example, by changing the type and amount of the monomer used to form the particulate polymer, and the polymerization method and conditions.

[0049] -Volume average particle diameter Db measured by laser diffraction scattering method- The volume average particle diameter Db of the particulate polymer is preferably 100 nm or more, more preferably 110 nm or more, even more preferably 120 nm or more, and preferably 170 nm or less, more preferably 160 nm or less, and even more preferably 150 nm or less. When the volume average particle diameter Db of the particulate polymer is within the above-mentioned range, the peel strength of the electrode can be improved. Furthermore, when the volume average particle diameter Db of the particulate polymer is equal to or greater than the above-mentioned lower limit, the injectability of the electrolyte solution into the secondary battery can be improved and the internal resistance of the secondary battery can be further reduced. The volume average particle diameter Db measured by laser diffraction scattering method is not significantly affected by the spatial spread of the molecular chains in the surface layer of the particulate polymer. That is, when the particulate polymer has, for example, the core-shell structure described above, the value of the volume average particle diameter Db of the particulate polymer is somewhat affected by the shell portion, but is presumed to be significantly dependent on the particle diameter of the core portion. Therefore, the value of the volume average particle diameter Db of the particulate polymer can be adjusted, for example, by changing the type and amount of the monomer used to form the core portion of the particulate polymer, as well as the polymerization method and conditions.

[0050] -Da / Db- Here, the ratio (Da / Db) of the average particle diameter Da to the volume average particle diameter Db of the particulate polymer is preferably 1.1 or more, more preferably 1.15 or more, even more preferably 1.3 or more, and preferably 2.0 or less, more preferably 1.9 or less, and even more preferably 1.8 or less. If Da / Db is equal to or greater than the above lower limit, when an electrode mixture layer is formed on a current collector using the slurry composition, migration of the particulate polymer to the surface side of the electrode mixture layer (i.e., the side opposite the current collector) is suppressed, and the particulate polymer can be present in a well-dispersed state in the electrode mixture layer. This is presumably because this can improve the peel strength of the electrode. Furthermore, if Da / Db is equal to or less than the above upper limit, excessive increase in the viscosity of the binder composition can be suppressed, thereby suppressing film formation. Therefore, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics.

[0051] [Method for preparing particulate polymer] The method for preparing the particulate polymer is not particularly limited. For example, the particulate polymer can be prepared by polymerizing the monomers that are the origin of the monomer units contained in the particulate polymer in an emulsion. Examples of such polymerization methods include a batch emulsion polymerization method, an emulsion (Em) prop method, and a seed polymerization method, and the batch emulsion polymerization method is preferred.

[0052] The batch emulsion polymerization method can be carried out, for example, by the following procedure. First, the monomers that are the basis of the monomer units contained in the particulate polymer are mixed with water, an emulsifier, and a polymerization initiator. The mixture (emulsion) is heated to carry out a polymerization reaction. When a predetermined polymerization conversion rate is reached, the mixture is cooled to stop the reaction, thereby obtaining a mixture containing the particulate polymer. Unreacted monomers are removed from the mixture to obtain an aqueous dispersion of the particulate polymer.

[0053] Here, when preparing a particulate polymer by a batch emulsion polymerization method, it is preferable to use two-stage polymerization in which the monomers are added in two batches rather than one-stage polymerization in which the monomers are added all at once, from the viewpoint of making it easier to keep the coating amount of the binder composition below a predetermined value. When a particulate polymer is prepared by two-stage polymerization, it is possible to obtain a particulate polymer having a core-shell structure with a core portion composed of monomer units derived from the monomer added in the first stage polymerization and a shell portion composed of monomer units derived from the monomer added in the second stage polymerization.

[0054] In the first polymerization step, the core-forming monomer is mixed with water, an emulsifier, a chain transfer agent, and a polymerization initiator. The mixture is heated to carry out the polymerization reaction until a predetermined polymerization conversion rate is reached, thereby forming a particle polymer comprising the core.

[0055] In the second polymerization step, the monomer for forming the shell portion, and optionally an emulsifier and water, are continuously added to the reaction solution after the first polymerization step to continue the polymerization. When a predetermined polymerization conversion rate is reached, the reaction is stopped by cooling to obtain a mixture containing a particulate polymer. Unreacted monomers are removed from the mixture to obtain an aqueous dispersion of a particulate polymer having a core-shell structure.

[0056] Heating during the polymerization reaction may be carried out, for example, at 40° C. or higher, 45° C. or higher, 50° C. or higher, 55° C. or higher, or 60° C. or higher, and 90° C. or lower, 85° C. or lower, 80° C. or lower, 75° C. or lower, or 70° C. or lower. Unreacted monomers may be removed from the mixture by, for example, heated, reduced-pressure distillation or by blowing in steam.

[0057] Examples of emulsifiers used in preparing the particulate polymer include alkyl diphenyl ether disulfonic acid, dodecyl benzene sulfonic acid, lauryl sulfate, or salts thereof (e.g., potassium salt, sodium salt). Of these, it is preferable to use alkyl diphenyl ether disulfonic acid salts. Examples of polymerization initiators used in preparing the particulate polymer include potassium persulfate, n-butyl lithium, and ammonium persulfate. Of these, it is preferable to use potassium persulfate. Examples of chain transfer agents used in preparing the particulate polymer include α-methylstyrene dimer, tert-dodecyl mercaptan, and 3-mercapto-1,2-propanediol. Of these, it is preferable to use tert-dodecyl mercaptan.

[0058] <Solvent> The binder composition of the present invention is not particularly limited, but typically contains a solvent. For example, the binder composition of the present invention may contain only water as the solvent, or only an organic solvent (e.g., esters, ketones, or alcohols) as the solvent, or the solvent may be a mixture of water and an organic solvent. From the viewpoints of further suppressing crater formation on the electrode surface and further improving the cycle characteristics while further reducing the internal resistance of the secondary battery, it is preferable that the binder composition of the present invention contains water as the solvent.

[0059] Here, the proportion of water in the solvent in the binder composition of the present invention is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass (i.e., the binder composition of the present invention contains only water as the solvent), with the total amount of solvent being 100% by mass. If the proportion of water in the solvent in the binder composition is equal to or greater than the above lower limit, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics.

[0060] <Other Components> In addition to the above-described binder and solvent, the binder composition of the present invention may contain, for example, an acidic water-soluble polymer, an antioxidant, a preservative, etc. The other components may be used alone or in combination of two or more at any ratio.

[0061] The acidic water-soluble polymer that can be contained in the binder composition of the present invention is produced, for example, as a by-product by polymerization from a monomer that is a raw material for the particulate polymer when the particulate polymer is produced by polymerization.

[0062] The weight-average molecular weight of such an acidic water-soluble polymer is preferably 500 or more, more preferably 700 or more, and even more preferably 1,000 or more, and is preferably 20,000 or less, more preferably 15,000 or less, still more preferably 8,000 or less, and particularly preferably 3,500 or less. When the weight-average molecular weight of the acidic water-soluble polymer is equal to or greater than the above-mentioned lower limit, the peel strength of the electrode can be improved. When the weight-average molecular weight of the acidic water-soluble polymer is equal to or less than the above-mentioned upper limit, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics.

[0063] The acidic water-soluble polymer may be in the form of a salt (a salt of the acidic water-soluble polymer). That is, in the present invention, the "acidic water-soluble polymer" also includes the salt of the acidic water-soluble polymer.

[0064] Examples of the antioxidant include hindered phenol-based antioxidants (e.g., 4-[[4,6-bis(octylthio)-1,3,5-triazin-2-yl]amino]-2,6-di-tert-butylphenol, 2,6-di-tert-butyl-p-cresol, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,4,6-tris(3',5'-di-tert-butyl-4'-hydroxybenzyl)mesitylene), oligomeric phenol-based antioxidants (e.g., WINGSTAY (registered trademark) L), phosphite-based antioxidants (e.g., 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 2,2-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite, tris(2,4-di-tert-butylphenyl)phosphite), sulfur-based antioxidants (e.g., didodecyl 3,3′-thiodipropionate), and the like. Among these, oligomeric phenol-based antioxidants are preferred.

[0065] The amount of the antioxidant added is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the particulate polymer.

[0066] Examples of preservatives include known preservatives such as isothiazolinone compounds and 2-bromo-2-nitro-1,3-propanediol. The isothiazolinone compounds are not particularly limited, and examples include those described in JP 2013-211246 A, JP 2005-097474 A, and JP 2013-206624 A. Preservatives may be used alone or in combination of two or more. Preferred preservatives include 1,2-benzisothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one, and 2-bromo-2-nitro-1,3-propanediol, with 1,2-benzisothiazolin-3-one being more preferred.

[0067] The amount of the preservative contained in the binder composition is preferably 0.01 part by mass or more, preferably 0.5 part by mass or less, more preferably 0.4 part by mass or less, and even more preferably 0.3 part by mass or less, relative to 100 parts by mass of the particulate polymer. If the content of the preservative is 0.01 part by mass or more per 100 parts by mass of the particulate polymer, the formation of aggregates in the binder composition after long-term storage can be further suppressed, and if it is 0.5 part by mass or less, the peel strength of the electrode can be ensured to be sufficiently high.

[0068] <<Properties of Binder Composition>> [Coating Amount] Here, the binder composition of the present invention must have a coating amount of 1.3 g or less. The coating amount of the binder composition is preferably 1.0 g or less, more preferably 0.8 g or less, even more preferably 0.7 g or less, even more preferably 0.6 g or less, particularly preferably 0.5 g or less, preferably 0.05 g or more, and more preferably 0.1 g or more. If the coating amount exceeds 1.3 g, the number of craters on the electrode surface increases, the internal resistance of the secondary battery increases, and the cycle characteristics deteriorate. If the coating amount is 1.0 g or less, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics. Furthermore, if the coating amount is 0.05 g or more, the ease of production of the binder composition can be ensured. The coating amount can be adjusted, for example, by changing the type and amount of monomer used in preparing the particulate polymer or the preparation method of the particulate polymer. Specifically, when preparing a particulate polymer by batch emulsion polymerization, the amount of coating can be reduced by using two-stage polymerization instead of one-stage polymerization. In addition, when using two-stage polymerization, the amount of coating can be reduced by adding a nitrile group-containing monomer and / or an ethylenically unsaturated carboxylic acid ester monomer in the second stage polymerization.

[0069] [Viscosity] The binder composition of the present invention preferably has a viscosity of 60 mPa·s or more, more preferably 150 mPa·s or more, even more preferably 250 mPa·s or more, and particularly preferably 350 mPa·s or more, and preferably 3000 mPa·s or less, more preferably 2500 mPa·s or less, even more preferably 2000 mPa·s or less, and particularly preferably 1400 mPa·s or less, when the binder composition has a solid content of 30% by mass. When the viscosity is equal to or greater than the lower limit, the peel strength of the electrode can be improved. When the viscosity is equal to or less than the upper limit, the formation of craters on the electrode surface can be further suppressed, and the peel strength of the electrode can be improved. The viscosity of the binder composition when the binder composition has a solid content of 30% by mass can be adjusted, for example, by changing the pH of the binder composition. Specifically, the viscosity can be reduced by lowering the pH of the binder composition, and the viscosity can be increased by increasing the pH of the binder composition.

[0070] [pH] When the binder composition contains water as a solvent, the pH of the binder composition is preferably 6 or higher, more preferably 7 or higher, preferably 10 or lower, more preferably 9 or lower, and even more preferably 8 or lower. When the pH of the binder composition is above the lower limit, the peel strength of the electrode can be improved. On the other hand, when the pH of the binder composition is below the upper limit, the viscosity of the binder composition is prevented from increasing excessively, thereby suppressing film formation. Therefore, crater formation on the electrode surface can be further suppressed, and the internal resistance of the secondary battery can be further reduced while further improving the cycle characteristics. The pH can be adjusted, for example, by adding an alkali species to the binder composition. Examples of alkali species include lithium hydroxide, sodium hydroxide, potassium hydroxide, and aqueous ammonia. Ammonia water is preferred because it is less likely to generate aggregates due to addition shock during alkali neutralization.

[0071] <Method for Preparing Binder Composition> The method for preparing the binder composition of the present invention is not particularly limited. For example, the aqueous dispersion containing a particulate polymer obtained by the method described above in the section "Method for Preparing a Particulate Polymer" can be used as a binder composition as is. Alternatively, for example, other components can be added to the aqueous dispersion containing a particulate polymer and mixed by a known method to prepare a binder composition. When preparing a binder composition using an aqueous dispersion containing a particulate polymer, the liquid contained in the aqueous dispersion (e.g., water) can be used as a solvent for the binder composition as is. Furthermore, optionally, the pH of the binder composition can be adjusted to be within the above-mentioned preferred pH range, and aggregates can be removed by filtering using a wire mesh or the like.

[0072] (Slurry composition for secondary battery electrode) The slurry composition of the present invention is a slurry composition used to form an electrode mixture layer of an electrode, and contains at least the above-mentioned binder composition and an electrode active material. For example, the slurry composition of the present invention contains an electrode active material and a binder in a solvent such as water, and optionally contains components other than the solvent, electrode active material, and binder (optional components). Since the slurry composition of the present invention contains the above-mentioned binder composition, when an electrode is produced using the slurry composition, it is possible to suppress crater formation on the electrode surface and to reduce the internal resistance of the secondary battery while exhibiting excellent cycle characteristics.

[0073] <Binder composition> The binder composition of the present invention described above is used as the binder composition. The amount of the binder composition in the slurry composition is not particularly limited. For example, the amount of the binder composition can be set so that the amount of the binder is 0.5 parts by mass or more and 15 parts by mass or less in terms of solid content per 100 parts by mass of the electrode active material.

[0074] <Electrode active material> The electrode active material is not particularly limited, and known electrode active materials used in secondary batteries can be used. Specifically, for example, the electrode active material that can be used in the electrode mixture layer of a lithium ion secondary battery, which is an example of a secondary battery, is not particularly limited, and the following electrode active materials can be used.

[0075] [Positive Electrode Active Material] The positive electrode active material to be blended in the positive electrode composite layer of the positive electrode of the lithium ion secondary battery may be, for example, a compound containing a transition metal, such as a transition metal oxide, a transition metal sulfide, or a composite metal oxide of lithium and a transition metal. Examples of the transition metal include Ti, V, Cr, Mn, Fe, Co, Ni, Cu, and Mo. Specifically, the positive electrode active material is not particularly limited, and may be, for example, lithium-containing cobalt oxide (LiCoO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium-containing nickel oxide (LiNiO 2 ), Co—Ni—Mn lithium-containing composite oxide, Ni—Mn—Al lithium-containing composite oxide, Ni—Co—Al lithium-containing composite oxide, olivine-type lithium iron phosphate (LiFePO 4 ), olivine-type lithium manganese phosphate (LiMnPO 4 ), Li 1+x Mn 2-x O 4 (0<X<2) Lithium-excess spinel compound represented by Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O 2 , LiNi 0.5 Mn 1.5 O 4 The above-mentioned positive electrode active materials may be used singly or in combination of two or more.

[0076] [Negative Electrode Active Material] Examples of negative electrode active materials to be incorporated into the negative electrode composite layer of the negative electrode of a lithium ion secondary battery include carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials combining these. Here, the carbon-based negative electrode active material refers to an active material having a carbon skeleton that can insert lithium (also referred to as "dope"). Specific examples of carbon-based negative electrode active materials include carbonaceous materials such as coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fiber, pyrolytic vapor-grown carbon fiber, phenolic resin calcined body, polyacrylonitrile-based carbon fiber, pseudoisotropic carbon, furfuryl alcohol resin calcined body (PFA), and hard carbon, as well as graphitic materials such as natural graphite and artificial graphite. Furthermore, the term "metal-based negative electrode active material" refers to an active material containing a metal, typically containing an element capable of inserting lithium in its structure, and having a theoretical electrical capacity per unit mass of 500 mAh / g or more when lithium is inserted. Examples of metal-based active materials include lithium metal, elemental metals capable of forming lithium alloys (e.g., Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.), and oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. thereof. Further examples include oxides such as lithium titanate. The above-mentioned negative electrode active materials may be used alone or in combination of two or more.

[0077] <Optional Components> Optional components that can be blended into the slurry composition are not particularly limited, and examples thereof include the other components described above in the section "Binder composition for secondary battery electrodes," dispersants, viscosity modifiers (thickeners) such as carboxymethyl cellulose, metal capture agents, conductive materials such as carbon black, etc. Note that the optional components may be used alone or in combination of two or more at any ratio.

[0078] <Preparation of Slurry Composition> The method for preparing the slurry composition is not particularly limited. For example, the binder composition, the electrode active material, and optional components used as needed can be mixed in the presence of a solvent derived from the binder composition to prepare the slurry composition. The mixing method is not particularly limited, and mixing can be performed using a commonly used stirrer or disperser.

[0079] (Secondary battery electrode) The electrode of the present invention includes an electrode mixture layer formed using the above-described slurry composition of the present invention. Therefore, the electrode mixture layer is made of a dried product of the above-described slurry composition, and usually contains an electrode active material and a binder, and may further contain optional components. Note that the components contained in the electrode mixture layer are those contained in the above-described slurry composition, and the preferred abundance ratio of each component is the same as the preferred abundance ratio of each component in the slurry composition. Furthermore, the particulate polymer exists in particulate form in the slurry composition, but may be in particulate form or any other shape in the electrode mixture layer formed using the slurry composition.

[0080] Furthermore, since the electrode of the present invention forms an electrode composite layer using the above-mentioned slurry composition, it is possible to suppress the formation of craters on the electrode surface, and to reduce the internal resistance of the secondary battery while exhibiting excellent cycle characteristics.

[0081] <Method of Forming an Electrode> Here, the electrode mixture layer provided in the electrode of the present invention can be formed using, for example, the following methods. 1) A method of applying the slurry composition of the present invention to the surface of a current collector and then drying it; 2) A method of immersing a current collector in the slurry composition of the present invention and then drying it; and 3) A method of applying the slurry composition of the present invention to a release substrate and drying it to produce an electrode mixture layer, and then transferring the obtained electrode mixture layer to the surface of the current collector. Among these, method 1) is particularly preferred because it makes it easy to control the layer thickness of the electrode mixture layer. Method 1) specifically includes a step of applying the slurry composition to the current collector (application step) and a step of drying the slurry composition applied to the current collector to form an electrode mixture layer on the current collector (drying step).

[0082] [Coating Step] The method for applying the slurry composition to the current collector is not particularly limited, and known methods can be used. Specifically, examples of the coating method include a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, and a brush coating method. In this case, the slurry composition may be applied to only one side of the current collector, or may be applied to both sides. The thickness of the slurry film on the current collector after application and before drying can be appropriately set depending on the thickness of the electrode mixture layer obtained by drying.

[0083] Here, the current collector to which the slurry composition is applied is made of a material that is electrically conductive and electrochemically durable. Specifically, the current collector may be made of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. Note that one of the above materials may be used alone, or two or more may be used in combination in any ratio.

[0084] [Drying Step] The method for drying the slurry composition on the current collector is not particularly limited and any known method can be used, for example, a drying method using warm air, hot air, or low-humidity air, a vacuum drying method, or a drying method using irradiation with infrared rays or electron beams, etc. By drying the slurry composition on the current collector in this manner, an electrode mixture layer can be formed on the current collector, and an electrode including the current collector and the electrode mixture layer can be obtained.

[0085] After the drying step, the electrode mixture layer may be subjected to a pressure treatment using a mold press, a roll press, or the like. The pressure treatment improves the adhesion between the electrode mixture layer and the current collector and also increases the density of the resulting electrode mixture layer. In addition, when the electrode mixture layer contains a curable polymer, it is preferable to cure the polymer after the electrode mixture layer is formed.

[0086] (Secondary battery) The secondary battery of the present invention includes a positive electrode, a negative electrode, an electrolyte, and a separator, and uses the electrode of the present invention described above as at least one of the positive electrode and the negative electrode. The secondary battery of the present invention is manufactured using the electrode of the present invention described above as at least one of the positive electrode and the negative electrode, and therefore has excellent cycle characteristics and reduced internal resistance. In the following, a description will be given of a case where the secondary battery is a lithium-ion secondary battery as an example, but the present invention is not limited to the following example.

[0087] <Electrode> Here, the electrode other than the above-described electrode of the present invention that can be used in the secondary battery of the present invention is not particularly limited, and a known electrode used in the manufacture of secondary batteries can be used. Specifically, an electrode obtained by forming an electrode mixture layer on a current collector using a known manufacturing method can be used as the electrode other than the above-described electrode of the present invention.

[0088] <Electrolyte> As the electrolyte, an organic electrolyte solution in which a supporting electrolyte is dissolved in an organic solvent is usually used. As the supporting electrolyte of a lithium ion secondary battery, for example, a lithium salt is used. As the lithium salt, for example, LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , C.F. 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF is particularly preferred because it is easily soluble in solvents and shows a high degree of dissociation. 6 , LiClO 4 , C.F. 3 SO 3Li is preferred. Note that one type of electrolyte may be used alone, or two or more types may be used in combination at any ratio. Generally, the use of a supporting electrolyte with a higher degree of dissociation tends to result in higher lithium ion conductivity, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.

[0089] The organic solvent used in the electrolyte is not particularly limited as long as it can dissolve the supporting electrolyte. Suitable examples include carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), and vinylene carbonate (VC); esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; and sulfur-containing compounds such as sulfolane and dimethyl sulfoxide. Mixtures of these solvents may also be used. Among these, carbonates are preferred due to their high dielectric constant and wide stable potential range. Generally, the lower the viscosity of the solvent used, the higher the lithium ion conductivity. Therefore, the lithium ion conductivity can be adjusted by the type of solvent. The concentration of the electrolyte in the electrolyte can be adjusted as appropriate. Known additives can also be added to the electrolyte.

[0090] <Separator> The separator is not particularly limited, and for example, those described in JP 2012-204303 A can be used. Among these, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred because it allows the thickness of the entire separator to be thin, thereby increasing the proportion of electrode active material in the secondary battery and increasing the capacity per volume.

[0091] The secondary battery of the present invention can be produced, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, rolling or folding the stack as necessary according to the battery shape, placing the stack in a battery container, injecting an electrolyte into the battery container, and sealing the container. In the secondary battery of the present invention, the electrode of the present invention described above is used as at least one of the positive electrode and negative electrode, preferably the negative electrode. The secondary battery of the present invention may be provided with an overcurrent protection element such as a fuse or a PTC element, an expanded metal, a lead plate, or the like, as necessary to prevent internal pressure buildup, overcharging and overdischarging, and the like. The shape of the secondary battery may be any shape, such as a coin type, a button type, a sheet type, a cylindrical type, a rectangular type, or a flat type.

[0092] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following description, the terms "%" and "parts" used to represent amounts are based on mass unless otherwise specified. In addition, in a polymer produced by polymerizing multiple types of monomers, the proportion of a monomer unit formed by polymerizing a certain monomer in the polymer usually corresponds to the ratio (feed ratio) of the certain monomer to all the monomers used in the polymerization of the polymer, unless otherwise specified. In the examples and comparative examples, the content of each monomer unit in the particulate polymer, the average particle diameter Da and volume average particle diameter Db of the particulate polymer, the viscosity and coating amount of the binder composition, the number of craters on the electrode surface, the peel strength of the electrode, and the internal resistance and cycle characteristics of the secondary battery were evaluated by the following methods.

[0093] <Content ratio of each monomer unit> 1The intensity ratio of the peaks derived from each monomer unit in the particulate polymer was determined by H-NMR (nuclear magnetic resonance) and converted into a mass ratio to determine the content ratio of each monomer unit in the particulate polymer. <Average particle diameter Da of particulate polymer> The average particle diameter Da of the particulate polymer prepared in the examples and comparative examples was measured using a particle size distribution measuring device (manufactured by Otsuka Electronics Co., Ltd., model "nanoSAQLA") that uses dynamic light scattering as its measurement principle. Specifically, the particle size distribution of an aqueous dispersion of the particulate polymer was measured under the following conditions, and the particle diameter (D50) at which the cumulative frequency of the light scattering intensity calculated from the small diameter side in the measured particle size distribution became 50% was determined as the average particle diameter Da (nm) of the particulate polymer. Dispersion medium: ion-exchanged water Measurement temperature: 25±1°C Measurement concentration (solid content concentration): 0.5% by mass Scattering angle: 168.8° Light source laser wavelength: 660 nm <Volume average particle diameter Db of particulate polymer> The volume average particle diameter Db of the particulate polymer prepared in the examples and comparative examples was measured in accordance with JIS Z 8825 using a particle size distribution measuring device (manufactured by Shimadzu Corporation, product name "SALD-2300") that uses a laser diffraction scattering method as its measurement principle. Specifically, an aqueous dispersion in which the solid content concentration of the particulate polymer was adjusted to 0.1% by mass was measured using the above device, and the particle diameter (D50) at which the cumulative volume calculated from the smallest diameter side reached 50% in the obtained particle size distribution (volume basis) was determined as the volume average particle diameter Db (nm) of the particulate polymer. <Coating amount> The solid content concentration of the binder composition prepared in the examples and comparative examples was adjusted to 30% by mass with water to prepare a mixed solution. When the solid content of the binder composition is lower than 30% by mass, the solvent can be distilled off to increase the solid content, thereby obtaining a mixed solution with a solid content of 30% by mass. 10.0 g of the resulting mixed solution was poured into a polytetrafluoroethylene dish with an inner diameter of 10 cm and allowed to stand for 2 hours under conditions of a temperature of 40°C and a humidity of 50% RH. The contents of the dish were then filtered using a stainless steel plain woven wire mesh (mesh: 200, wire diameter: 0.05 mm, opening: 0.077 mm). After filtration, the mass (g) of the material remaining on the wire mesh was measured and used as the coating amount.<Viscosity> After adjusting the solid content concentration of the binder composition prepared in the Examples and Comparative Examples to 30% by mass with water, the viscosity of the binder composition was measured using a Brookfield viscometer (manufactured by Toki Sangyo Co., Ltd., product name "TVB-10", rotation speed: 60 rpm). The temperature during viscosity measurement was 25°C. Note that if the viscosity of the binder composition is 10 mPa·s or more and 3000 mPa·s or less, it can be said that the binder composition has good viscosity. <Number of Craters> The electrodes prepared in the Examples and Comparative Examples were cut into a length of 30 cm and a width of 10 cm, and the surface of the cut electrode facing the electrode mixture layer was observed to count the number of craters with a diameter (inner diameter) of 1 cm or more. This measurement was performed three times, and the average value was calculated, which was used as the number of craters. Note that if the average value was a non-integer value, it was rounded to an integer value. Evaluation was then performed according to the following criteria. A: 0 craters B: 1 to 3 craters C: 4 to 6 craters D: 7 or more craters <Peel Strength> The electrodes prepared in the Examples and Comparative Examples were cut into rectangular shapes measuring 100 mm in length and 10 mm in width to prepare test specimens. The test specimens were placed with the surface of the electrode mixture layer facing downwards, and cellophane tape was attached to the surface of the electrode mixture layer. The cellophane tape used was specified in JIS Z1522. The cellophane tape was fixed to a test table. One end of the current collector was then pulled vertically upward at a pulling rate of 50 mm / min, and the stress when peeled was measured. This measurement was performed three times, and the average value was calculated. This average value was used as the peel strength. Evaluation was then performed according to the following criteria. A: Peel strength of 10 N / m or more B: Peel strength of 7 N / m or more but less than 10 N / m C: Peel strength of 5 N / m or more but less than 7 N / m D: Peel strength of less than 5 N / m <Internal Resistance> To evaluate the internal resistance of the lithium ion secondary batteries produced in the Examples and Comparative Examples, the IV resistance was measured as follows: Each battery was subjected to a conditioning treatment in which it was charged at a temperature of 25°C at a charge rate of 0.1 C until the voltage reached 4.2 V, and then left to rest for 10 minutes, followed by constant current (CC) discharge at a discharge rate of 0.1 C until the voltage reached 3.0 V, which was repeated three times.Subsequently, the batteries were charged to 3.75 V at 1 C (C is a value expressed as rated capacity (mA) / hour (h)) in a −10°C atmosphere, and then charged for 20 seconds and discharged for 20 seconds at 0.5 C, 1.0 C, 1.5 C, and 2.0 C, centered around 3.75 V. For each case, the battery voltage after 15 seconds on the charging side was plotted against the current value, and the slope was calculated as the IV resistance (Ω). The obtained IV resistance values ​​(Ω) were compared with the IV resistance of Comparative Example 1 and evaluated according to the following criteria. The smaller the IV resistance value, the lower the internal resistance of the secondary battery. A: Less than 85% of the IV resistance of Comparative Example 1 B: 85% to less than 95% of the IV resistance of Comparative Example 1 C: 95% or more of the IV resistance of Comparative Example 1 <Cycle Characteristics> After injecting the electrolyte, the lithium-ion secondary batteries fabricated in the Examples and Comparative Examples were allowed to stand at 25°C for 5 hours. Next, the battery was charged to a cell voltage of 3.65 V at a constant current of 0.2 C at 25 ° C, and then aged for 12 hours at 60 ° C. Then, the battery was discharged to a cell voltage of 3.00 V at a constant current of 0.2 C at 25 ° C. Subsequently, constant current (CC)-constant voltage (CV) charging (upper limit cell voltage 4.20 V) was performed at a constant current of 0.2 C, and CC discharging was performed to 3.00 V at a constant current of 0.2 C. This 0.2 C charge-discharge cycle was repeated three times. Then, 100 cycles of charge-discharge were performed at a cell voltage of 4.20-3.00 V and a charge-discharge rate of 1.0 C in a 25 ° C environment. The discharge capacity of the first cycle was defined as X1, and the discharge capacity of the 100th cycle as X2. Using the discharge capacities X1 and X2, the capacity retention rate, ΔC=(X2 / X1)×100(%), was calculated and evaluated according to the following criteria. A larger value of the capacity retention rate ΔC indicates better cycle characteristics: A: ΔC is 93% or more; B: ΔC is 90% or more but less than 93%; C: ΔC is 87% or more but less than 90%; D: ΔC is less than 87%.

[0094] Example 1 Preparation of Negative Electrode Binder Composition First-Stage Polymerization Addition Into a 5 MPa pressure vessel A equipped with a stirrer, 22 parts of styrene (St) as an aromatic vinyl monomer, 70 parts of 1,3-butadiene (BD) as an aliphatic conjugated diene monomer, 1 part of methacrylic acid (MAA) as an acidic group-containing monomer, 0.6 parts of alkyl diphenyl ether disulfonate as an emulsifier, 143 parts of ion-exchanged water, 0.1 parts of tert-dodecyl mercaptan as a chain transfer agent, and 0.3 parts of potassium persulfate as a polymerization initiator were placed, thoroughly stirred, and then heated to 55°C to initiate polymerization and allowed to react for 10 hours. The mixture was then heated to 65°C and allowed to react for an additional 6 hours. [Second-stage polymerization addition] Next, 2 parts of acrylonitrile (AN) as a nitrile group-containing monomer, 2 parts of methyl methacrylate (MMA) as an ethylenically unsaturated carboxylic acid ester monomer, and 3 parts of methacrylic acid (MAA) as an acidic group-containing monomer were added to a pressure-resistant vessel A, heated to 85°C, and allowed to react for an additional 6 hours. Thereafter, unreacted monomers were removed by heating and reduced pressure distillation. As a result, an aqueous dispersion of a particulate polymer having a core-shell structure in which at least a portion of the outer surface of the core formed in the first-stage polymerization was covered with the shell formed in the second-stage polymerization was obtained. [pH adjustment, filtration] The obtained aqueous dispersion of the particulate polymer was neutralized with aqueous ammonia to adjust the pH to 7. After further cooling, 1 part (solids equivalent) of Wingstay L dispersion (manufactured by Chukyo Yushi Co., Ltd., catalog number "K-840") was added as an antioxidant. The mixture was then dried on a polytetrafluoroethylene dish at 40°C for 2 hours, and then filtered using a stainless steel plain woven wire mesh (mesh: 200, wire diameter: 0.05 mm, opening: 0.077 mm) to obtain a binder composition for a negative electrode. Using this binder composition, the content of each monomer unit in the particulate polymer, the average particle diameter Da and volume average particle diameter Db of the particulate polymer, the coating amount, and the viscosity of the binder composition were measured. The results are shown in Table 1. <Preparation of Slurry Composition for Negative Electrode> Artificial graphite (tap density: 0.85 g / cm) was added as a negative electrode active material to a planetary mixer equipped with a disperser. 3A mixture was obtained by adding 100 parts of a binder composition (capacity: 360 mAh / g), 1 part of carbon black (manufactured by TIMCAL, product name "Super C65") as a conductive material, and 1.2 parts of a 2% aqueous solution of carboxymethyl cellulose (manufactured by Daicel Corporation, product name "Daicel 2200") as a thickener, in terms of solid content. The resulting mixture was adjusted to a solid content of 60% with ion-exchanged water and then mixed at 25°C for 60 minutes. Next, the solid content was adjusted to 52% with ion-exchanged water, and then mixed for an additional 15 minutes at 25°C to obtain a mixed solution. 2.0 parts of the binder composition prepared above, in terms of solid content, and ion-exchanged water were added to the resulting mixed solution, and the final solid content was adjusted to 48%. After further mixing for 10 minutes, the mixture was degassed under reduced pressure to obtain a negative electrode slurry composition with good fluidity. <Formation of Negative Electrode> The obtained negative electrode slurry composition was coated on a copper foil having a thickness of 15 μm, which was a current collector, using a comma coater at a speed of 3.6 m / min so that the coating weight after drying was 10.5 mg / cm 2 The copper foil was dried by conveying it at a speed of 3.6 m / min through an oven at 140°C for 20 seconds and then through an oven at 150°C for 20 seconds. The obtained negative electrode blank was rolled with a roll press to reduce the density of the negative electrode composite layer to 1.70 g / cm. 3 The negative electrode was evaluated for the number of craters on the surface and peel strength. The results are shown in Table 1. <Formation of Positive Electrode> A LiCoO film having a median diameter of 12 μm was used as the positive electrode active material. 2 100 parts of the above, 2 parts of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd., product name "HS-100") as a conductive material, 2 parts of polyvinylidene fluoride (manufactured by Kureha Corporation, product name "#7208") as a binder, in terms of solid content, and N-methylpyrrolidone as a solvent were mixed to a total solids concentration of 70%. These were mixed using a planetary mixer to obtain a positive electrode slurry composition. The obtained positive electrode slurry composition was coated using a comma coater on a 20 μm thick aluminum foil current collector so that the basis weight after drying was 23 mg / cm 2The aluminum foil was then coated with the coating and dried so that the density of the positive electrode composite layer became 4.0 g / cm. This drying was performed by conveying the aluminum foil at a speed of 0.5 m / min through an oven at 60°C for 2 minutes. Thereafter, the aluminum foil was heat-treated at 120°C for 2 minutes to obtain a positive electrode blank. The positive electrode blank was then rolled with a roll press to obtain a positive electrode composite layer having a density of 4.0 g / cm. 3 A positive electrode of 1000 W was obtained. <Preparation of Separator> A single-layer polypropylene separator (manufactured by Celgard, product name "Celgard 2500") was prepared as a separator made of a separator substrate. <Preparation of Lithium-Ion Secondary Battery> A laminate was obtained by interposing the pressed positive and negative electrodes prepared as described above and a separator (a 20 μm thick polypropylene microporous film) in a separator / positive electrode / separator / negative electrode configuration. Next, the laminate of the electrode and separator was wound around a core with a diameter of 20 mm to obtain a wound body including a positive electrode, a separator, and a negative electrode. Subsequently, the obtained wound body was compressed in one direction at a speed of 10 mm / sec until it reached a thickness of 4.5 mm, thereby obtaining a flattened body. The obtained flattened body had an elliptical shape in a plan view, and the ratio of its major axis to its minor axis (major axis / minor axis) was 7.7. In addition, a nonaqueous electrolyte (LiPF at a concentration of 1.0 M) was added. 6 A solution (solvent): a mixed solvent of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (mass ratio), further containing 2 volume% vinylene carbonate (VC) as an additive, was prepared. The flat body was then housed in an aluminum laminate case along with the nonaqueous electrolyte solution. After connecting the negative and positive electrode leads to their designated locations, the opening of the laminate case was thermally sealed to produce a laminated lithium-ion secondary battery as a nonaqueous secondary battery. The resulting secondary battery was a pouch-shaped battery measuring 35 mm wide x 48 mm high x 5 mm thick, with a nominal capacity of 700 mAh. The internal resistance and cycle characteristics of this lithium-ion secondary battery were evaluated. The results are shown in Table 1.

[0095] (Example 2) A binder composition for a negative electrode, a slurry composition for a negative electrode, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that, when preparing the binder composition, the aqueous dispersion of the particulate polymer was adjusted with ammonia water to a pH of 6. Evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0096] Example 3 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1. First-stage polymerization: 23 parts of St, 71 parts of BD, 0 part of MAA Second-stage polymerization: 2 parts of AN, 2 parts of MMA, 2 parts of MAA

[0097] Example 4 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1. First-stage polymerization: 22 parts of St, 72 parts of BD, 1 part of MAA Second-stage polymerization: 0 part of AN, 2 parts of MMA, 3 parts of MAA

[0098] Example 5 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1. First-stage polymerization: 22 parts of St, 72 parts of BD, 1 part of MAA Second-stage polymerization: 2 parts of AN, 0 parts of MMA, 3 parts of MAA

[0099] Example 6 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1. First-stage polymerization: 18 parts of St, 70 parts of BD, 1 part of MAA Second-stage polymerization: 2 parts of AN, 2 parts of MMA, 3 parts of MAA, 4 parts of St

[0100] (Example 7) A binder composition for a negative electrode, a slurry composition for a negative electrode, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 3, except that, when preparing the binder composition, the aqueous dispersion of the particulate polymer was adjusted with ammonia water to a pH of 6. Evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0101] Example 8 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1. First-stage polymerization: 19 parts of St, 67 parts of BD, 1 part of MAA Second-stage polymerization: 8 parts of AN, 2 parts of MMA, 3 parts of MAA

[0102] Example 9 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1. First-stage polymerization: 19 parts of St, 67 parts of BD, 1 part of MAA Second-stage polymerization: 2 parts of AN, 8 parts of MMA, 3 parts of MAA

[0103] Comparative Example 1 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 2. First-stage polymerization: 24 parts of St, 72 parts of BD, 1 part of MAA Second-stage polymerization: 3 parts of MAA

[0104] Comparative Example 2 A binder composition for a negative electrode, a slurry composition for a negative electrode, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that, when preparing the binder composition, the aqueous dispersion of the particulate polymer was adjusted with ammonia water to have a pH of 4. Evaluations were then performed in the same manner as in Example 1. The results are shown in Table 2.

[0105] Comparative Example 3 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 2. First-stage polymerization: 16.5 parts of St, 59.5 parts of BD, 1 part of MAA Second-stage polymerization: 10 parts of AN, 10 parts of MMA, 3 parts of MAA

[0106] Comparative Example 4 A binder composition for a negative electrode, a slurry composition for a negative electrode, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that, when preparing the binder composition, the aqueous dispersion of the particulate polymer was adjusted with ammonia water so that the pH was 10. Evaluations were then performed in the same manner as in Example 1. The results are shown in Table 2.

[0107] Comparative Example 5 A binder composition for a negative electrode, a slurry composition for a negative electrode, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the binder composition were changed as follows, and the aqueous dispersion of the particulate polymer was adjusted with aqueous ammonia to a pH of 5. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 2. First-stage polymerization: 19 parts of St, 67 parts of BD, 1 part of MAA Second-stage polymerization: 2 parts of AN, 2 parts of MMA, 9 parts of MAA

[0108] (Comparative Example 6) A negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that a negative electrode binder composition prepared as follows was used. Evaluations were then performed in the same manner as in Example 1. The results are shown in Table 2. <Preparation of negative electrode binder composition> In a 5 MPa pressure vessel A equipped with a stirrer, 22 parts of styrene (St) as an aromatic vinyl monomer, 70 parts of 1,3-butadiene (BD) as an aliphatic conjugated diene monomer, 4 parts of methacrylic acid (MAA) as an acidic group-containing monomer, 2 parts of acrylonitrile (AN) as a nitrile group-containing monomer, 2 parts of methyl methacrylate (MMA) as an ethylenically unsaturated carboxylic acid ester monomer, 0.6 parts of alkyl diphenyl ether disulfonate as an emulsifier, 143 parts of ion-exchanged water, 0.1 parts of tert-dodecyl mercaptan as a chain transfer agent, and 0.3 parts of potassium persulfate as a polymerization initiator were all placed together, thoroughly stirred, and then heated to 55 ° C. to initiate polymerization and reacted for 10 hours. Then, heated to 65 ° C. and further reacted for 6 hours. Thereafter, unreacted monomer was removed by heating and reduced pressure distillation to obtain an aqueous dispersion of a particulate polymer. The resulting aqueous dispersion of the particulate polymer was neutralized with aqueous ammonia to adjust the pH to 7. The mixture was then cooled, and 1 part of a Wingstay L dispersion (equivalent to the solid content) was added as an antioxidant. The mixture was then dried at 40°C for 2 hours on a polytetrafluoroethylene dish, and then filtered using a stainless steel plain-woven wire mesh (mesh: 200, wire diameter: 0.05 mm, opening: 0.077 mm) to obtain a binder composition for a negative electrode.

[0109] Comparative Example 7 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 2. First-stage polymerization: 18 parts of St, 66 parts of BD, 1 part of MAA Second-stage polymerization: 10 parts of AN, 2 parts of MMA, 3 parts of MAA

[0110] Comparative Example 8 A negative electrode binder composition, a negative electrode slurry composition, a negative electrode, a positive electrode, a separator, and a lithium ion secondary battery were prepared or fabricated in the same manner as in Example 1, except that the amounts of each monomer added in the first and second polymerization stages during the preparation of the negative electrode binder composition were changed as follows. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 2. First-stage polymerization: 18 parts of St, 66 parts of BD, 1 part of MAA Second-stage polymerization: 2 parts of AN, 10 parts of MMA, 3 parts of MAA

[0111] In Tables 1 and 2 shown below, "St" represents a styrene unit, "BD" represents a 1,3-butadiene unit, "MAA" represents a methacrylic acid unit, "AN" represents an acrylonitrile unit, "MMA" represents a methyl methacrylate unit, "viscosity" represents the viscosity under the condition of a solid content concentration of 30% by mass, and "Da / Db" represents the ratio of the average particle diameter Da of the particulate polymer measured by dynamic light scattering to the volume average particle diameter Db of the particulate polymer measured by laser diffraction scattering. In Tables 1 and 2, "Da / Db" is expressed as a value rounded to one decimal place.

[0112]

[0113]

[0114] Table 1 shows that in Examples 1 to 9, which used binder compositions with a coating amount equal to or less than a predetermined value, electrodes in which crater formation was suppressed and secondary batteries with reduced internal resistance and excellent cycle characteristics were produced. On the other hand, Table 2 shows that in Comparative Examples 1 and 2 and 4 to 8, which used binder compositions with a coating amount greater than a predetermined value, crater formation on the electrode surface was not sufficiently suppressed, and the internal resistance of the secondary battery increased and the cycle characteristics deteriorated. Table 2 also shows that in Comparative Example 3, which used a binder composition with a coating amount greater than a predetermined value, crater formation on the electrode surface was not sufficiently suppressed, and the cycle characteristics of the secondary battery deteriorated.

[0115] According to the present invention, it is possible to provide a binder composition for a secondary battery electrode and a slurry composition for a secondary battery electrode that can form a secondary battery electrode in which crater formation on the electrode surface is suppressed, and that can reduce the internal resistance of the secondary battery and exhibit excellent cycle characteristics. Furthermore, according to the present invention, it is possible to provide a secondary battery electrode in which crater formation on the electrode surface is suppressed, and that can reduce the internal resistance of the secondary battery and exhibit excellent cycle characteristics. Furthermore, according to the present invention, it is possible to provide a secondary battery in which internal resistance is reduced and excellent cycle characteristics are exhibited.

Claims

1. A binder composition for secondary battery electrodes, comprising a binder, wherein 10.0 g of a mixed solution of the binder composition for secondary battery electrodes and water adjusted to a solids concentration of 30 mass % is poured into a polytetrafluoroethylene petri dish having a diameter of 10 cm, and the amount of the coating film after leaving the mixture at a temperature of 40°C for 2 hours is 1.3 g or less.

2. The binder composition for secondary battery electrodes according to claim 1, wherein the binder comprises a particulate polymer, and the particulate polymer contains nitrile group-containing monomer units in a proportion of 1% by mass or more and 9% by mass or less, and ethylenically unsaturated carboxylic acid ester monomer units in a proportion of 1% by mass or more and 9% by mass or less.

3. The binder composition for secondary battery electrodes according to claim 2, wherein the particulate polymer is a random copolymer.

4. The binder composition for secondary battery electrodes according to claim 2, wherein, when an average particle diameter of the particulate polymer measured by a dynamic light scattering method is Da (nm) and a volume average particle diameter of the particulate polymer measured by a laser diffraction scattering method is Db (nm), the ratio of Da to Db (Da / Db) is 1.1 or more and 2.0 or less.

5. The binder composition for secondary battery electrodes according to claim 1, having a viscosity of 60 mPa·s or more and 3,000 mPa·s or less under the condition of a solid content concentration of 30 mass %.

6. The binder composition for a secondary battery electrode according to claim 1, further comprising water and having a pH of 6 or more and 10 or less.

7. A slurry composition for a secondary battery electrode, comprising an electrode active material and the binder composition for a secondary battery electrode according to any one of claims 1 to 6.

8. A secondary battery electrode comprising an electrode mixture layer formed using the slurry composition for a secondary battery electrode according to claim 7.

9. A secondary battery comprising the electrode for a secondary battery according to claim 8.

Citation Information

Patent Citations

  • Copolymer latex with high long-term storage stability

    JP2005097474A

  • Binder composition for electrode, slurry composition for electrode, electrode and battery

    JP2011076917A

  • Electrode for secondary battery, binder for secondary battery electrode, manufacturing method and secondary battery

    JP2012204303A

  • Composition for battery electrode and binder composition for battery electrode

    JP2013206624A

  • Binder composition for electrode, electrode slurry, electrode, and electricity storage device

    JP2013211246A

Cited By

  • Particulate binder for nonaqueous secondary battery electrode, binder composition for nonaqueous secondary battery electrode, slurry composition for nonaqueous secondary battery electrode, composite particles for nonaqueous secondary battery electrode, electrode for nonaqueous secondary battery, and nonaqueous secondary battery

    WO2026116165A1