Phenolic resin foam and method for producing same
By optimizing the water content and composition of lignin in phenolic resin foams, the challenges of high thermal conductivity and prolonged curing times are addressed, achieving low thermal conductivity and high productivity for bio-based insulation.
Patent Information
- Application Number
- PCT/JP2024/016349
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Existing phenolic resin foams with lignin additives suffer from high thermal conductivity and prolonged curing times, which hinder their productivity and insulation performance.
Adjusting the water content of lignin and optimizing the lignin-containing phenolic resin composition to maintain foam curing time and thermal conductivity comparable to foams without lignin, while using plant-derived materials for bio-based insulation.
The approach results in phenolic resin foams with low thermal conductivity and high productivity, maintaining insulation performance and utilizing bio-based materials effectively.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Phenolic resin foam and its manufacturing method CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority to Japanese Patent Application No. 2023-075252, filed on April 28, 2023, the entire disclosure of which is incorporated herein by reference.
[0002] The present invention relates to a phenolic foam and a method for producing the same.
[0003] Acid-cured phenolic resin foams made from resol phenolic resins exhibit excellent heat insulating properties, are flame-resistant, and produce little smoke. Therefore, they have been used for a long time in building materials such as exterior wall materials (e.g., metal siding), interior wall materials (e.g., partition panels), ceiling materials, fire doors, and storm shutters, as well as in cooling and heat insulation materials for industrial plants.
[0004] In recent years, concerns about global warming have made it urgent to reduce greenhouse gas emissions, and the use of plant-derived materials as product raw materials has attracted attention as one way to reduce greenhouse gases such as carbon dioxide emitted during incineration. Foams made from plant-derived materials can be considered to have the same amount of carbon dioxide emitted during incineration as the amount absorbed by the plants, depending on the amount used, and therefore can be considered a carbon-neutral technology that does not affect the increase or decrease of carbon dioxide in the atmosphere.
[0005] Lignin is one of the plant-derived materials that has been considered for potential use. Lignin is a component recovered from plants during the production of pulp. It is classified into woody and herbaceous species based on the plant species used as the raw material, and is further classified into kraft lignin, lignosulfonic acid, soda lignin, etc. based on the method of extraction used in pulp production. Because lignin has a phenolic skeleton in its chemical structure, attempts have been made to produce composites with phenolic resins.
[0006] Patent Document 1 discloses a method for producing a foamed phenolic resin by adding lignin sulfonate to a phenolic resol to control the foaming and curing rate. Patent Document 2 discloses that a bio-based phenolic resin foam can be provided by adding organosolv lignin or pyrolytic lignin to a condensate of a mixture of phenol, formaldehyde, and a basic catalyst.
[0007] Patent No. 1578980 Patent No. 5885855
[0008] However, the phenolic resin foam containing lignin sulfonate in the examples of Patent Document 1 has a high thermal conductivity, which does not take advantage of the inherently low thermal conductivity of the phenolic resin foam. Furthermore, the more the amount of lignin sulfonate added, the longer the curing completion time, which is not preferable from the viewpoint of productivity.
[0009] On the other hand, the phenolic resin foam to which organosolv lignin or pyrolytic lignin is added in Patent Document 2 cannot be said to have sufficient thermal conductivity compared to the phenolic resin foam to which no lignin compound is added, as in Patent Document 1. Furthermore, the phenolic resin foam in Patent Document 2 requires 24 hours or more for foaming and curing, which is undesirable from the viewpoint of productivity.
[0010] Therefore, there has been a demand for a phenolic resin foam containing lignin but having low thermal conductivity. Furthermore, there has been a demand for a technology that can achieve the same low thermal conductivity as a lignin-free phenolic resin foam while exhibiting a foaming and curing time equivalent to that of a lignin-free phenolic resin foam.
[0011] Therefore, the present inventors have conducted extensive research to solve the above-mentioned problems and have developed a technology that allows a lignin-containing phenolic resin foam to exhibit the same foaming and curing time and thermal conductivity as a lignin-free phenolic resin foam by appropriately adjusting the moisture content of the lignin and optimizing the moisture content of the lignin-containing phenolic resin composition.
[0012] [1] A phenolic resin foam in which, in an ion chromatogram obtained by gas chromatography-mass spectrometry of gas components generated by heating at 600°C, the total area X (X = A + B + C) of the area A derived from dihydroxybenzene, the area B derived from dihydroxytoluene, and the area C derived from dihydroxyxylene, which are pyrolysis products, to the area Y of the pyrolysis product exhibiting a structure derived from urea crosslinking, is in the range of the following formula (1), and the thermal conductivity value in an environment of 23°C is 0.0240 W / (m K) or less: 0.035≦Z≦0.715 (1) [2] A density of 10 kg / m 3 More than 50kg / m 3 [3] The phenolic resin foam according to any one of [1] to [2], which has an average cell diameter of 70 μm or more and 250 μm or less. [4] The phenolic resin foam according to any one of [1] to [3], which contains any one of hydrofluoroolefin, hydrocarbon, and chlorinated hydrocarbon. [5] The phenolic resin foam according to any one of [1] to [4], which has a surface material on at least one of one side of the phenolic resin foam and the back side of the one side. [6] The method for producing a phenolic resin foam laminate according to [5], wherein a foamable phenolic resin composition containing lignin is foamed and cured on a facing material, the method comprising at least one of the following steps to obtain the foamable phenolic resin composition: adding lignin to phenols, adding lignin during synthesis of a phenolic resin, adding lignin to a phenolic resin, and adding lignin to a phenolic resin composition, wherein the lignin has a moisture content of 34.0% or less, and the moisture content of the lignin-containing phenolic resin composition in the foamable phenolic resin composition is 1.5% by mass or more and 6.5% by mass or less. [7] The method for producing a phenolic resin foam laminate according to [6], wherein in the step of adding lignin, the median diameter of the lignin powder added is 0.1 μm or more and 300 μm or less.
[0013] By appropriately adjusting the moisture content of the lignin and the moisture content of the phenolic resin composition to which lignin has been added, the phenolic resin foam according to the present invention can maintain the foaming and curing time even when the foam contains lignin, allowing it to be produced without reducing productivity. Furthermore, by suppressing water-induced foaming inhibition and maintaining fine cells, the thermal conductivity and heat insulating performance can be maintained even when the foam contains lignin. Furthermore, by using plant-derived materials, it is possible to provide a bio-based phenolic resin foam.
[0014] The present invention identifies the conditions for adding plant-derived materials, which are necessary to maintain the foaming and curing time and thermal insulation performance, and has discovered a phenolic resin foam that simultaneously satisfies low thermal conductivity, high productivity, and is bio-based, something that has not been possible until now.
[0015] The following describes in detail the embodiments of the present invention (hereinafter referred to as "present embodiments"). The present invention is not limited to the following embodiments and can be modified in various ways within the scope of the present invention. In this specification, a "phenolic resin" to which a surfactant has been added is referred to as a "phenolic resin composition," and a "phenolic resin composition" containing lignin is specifically referred to as a "lignin-containing phenolic resin composition." A "phenolic resin composition" or a "lignin-containing phenolic resin composition" to which a blowing agent, a foam nucleating agent, an acidic curing agent, etc. have been added to impart foamability or both foamability and curability is referred to as a "foamable phenolic resin composition." The resulting foam is referred to as a "phenolic resin foam." A laminate of a phenolic resin foam having a surface material on at least one of one side and the backside of the one side is referred to as a "phenolic resin foam laminate."
[0016] The phenolic resin foam according to the embodiment of the present application contains lignin. Whether or not the phenolic resin foam contains lignin can be determined by subjecting the phenolic resin foam to pyrolysis gas chromatography mass spectrometry, as described below.
[0017] When gas components generated by heating a lignin-containing phenolic resin foam at 600°C are analyzed by gas chromatography-mass spectrometry, where the retention time at which phenol is detected in the resulting total ion chromatogram is t minutes, a pyrolysis product derived from dihydroxybenzene is detected at a retention time of approximately 1.38 × t minutes in the extracted ion chromatogram for m / z = 110, a pyrolysis product derived from dihydroxytoluene is detected at a retention time of approximately 1.46 × t minutes in the extracted ion chromatogram for m / z = 124, a pyrolysis product derived from dihydroxytoluene is detected at a retention time of approximately 1.50 × t minutes in the extracted ion chromatogram for m / z = 138, and a pyrolysis product derived from dihydroxyxylene is detected at a retention time of approximately 1.58 × t minutes in the extracted ion chromatogram for m / z = 138. Phenol is detected at a retention time of approximately 10.0 minutes using the pyrolysis-gas chromatography-mass spectrometry measurement method described below.
[0018] In the extracted ion chromatogram of the obtained pyrolysis product at m / z = 110, the area of the pyrolysis product derived from dihydroxybenzene detected near a retention time of 1.38 × t minutes is designated A; in the extracted ion chromatogram at m / z = 124, the sum of the area of the pyrolysis product derived from dihydroxytoluene detected near a retention time of 1.46 × t minutes and the area of the pyrolysis product derived from dihydroxytoluene detected near a retention time of 1.50 × t minutes is designated B; in the extracted ion chromatogram at m / z = 138, the area of the pyrolysis product derived from dihydroxyxylene detected near a retention time of 1.58 × t minutes is designated C; the sum of A, B, and C is designated X (X = A + B + C). Furthermore, when the area of the pyrolysis product exhibiting a structure derived from urea crosslinking is designated Y, the ratio to X is designated Z (Z = X / Y). The pyrolysis product exhibiting a structure derived from urea crosslinking corresponds to, for example, Peak 9 in [Figure 1] of Japanese Patent No. 4711469, and is detected in the total ion chromatogram at a retention time of approximately 1.50 x t minutes. In the extracted ion chromatogram, the values of areas A, B, and C vary depending on the type of lignin and change depending on the amount of lignin added to the phenolic resin composition. The value of area Y does not change depending on the timing of lignin addition. The areas A, B, C, and Y are calculated using the intersections with the baseline or the inflection points with adjacent peaks as boundaries.
[0019] In the ion chromatogram of the obtained pyrolysis product, Z is 0.035 or more and 0.715 or less, preferably 0.040 or more and 0.40 or less. More preferably, it is 0.055 or more and 0.23 or less, and even more preferably, it is 0.065 or more and 0.18 or less. Most preferably, it is 0.075 or more and 0.11 or less. A Z less than 0.035 indicates a low proportion of plant-derived materials in the phenolic resin foam, making it less valuable as a bio-based material. A Z greater than 0.715 indicates a significantly high proportion of lignin in the phenolic resin foam. However, increasing the lignin proportion is undesirable because it increases the viscosity when added to the phenolic resin. Furthermore, when used as an insulating material, the lignin functions as a thermal bridge, increasing the thermal conductivity.
[0020] The phenolic resin foam of the present invention contains a blowing agent as described below.
[0021] The density of the phenolic resin foam of the present invention may be adjusted to a desired density depending on the intended use of the foam, but is preferably 10 kg / m 3 More than 50kg / m 3 More preferably, it is 20 kg / m or less. 3 More than 50kg / m 3 More preferably, it is 22 kg / m or less. 3 More than 50kg / m 3 or less, and most preferably 24 kg / m 3 Over 45kg / m3 The density is 10 kg / m or less. 3 In the above cases, the decrease in mechanical strength such as compressive strength and the decrease in surface brittleness, which tend to occur due to low density, are small, and strength that does not pose a problem in practical use can be maintained. 3 When the density is below 100%, there is less concern about an increase in thermal conductivity due to the thermal conduction of the phenolic resin portion, which becomes larger due to the high density. The density of the phenolic resin foam can be adjusted by adjusting the filling ratio of the blowing agent in the phenolic resin foam, and can be adjusted to a desired value mainly by changing the amount of blowing agent added to the phenolic resin composition, the temperature of the foamable phenolic resin composition, the timing of pre-molding in the step of discharging the mixed foamable phenolic resin composition, the amount of foam nucleating agent added, the amount of acidic curing agent added, and curing conditions such as temperature and residence time.
[0022] The average cell diameter of the phenolic resin foam of the present invention is preferably 70 μm or more and 250 μm or less, more preferably 70 μm or more and 130 μm or less. It is even more preferably 70 μm or more and 120 μm or less, and most preferably 70 μm or more and 110 μm or less. An average cell diameter of 70 μm or more can suppress the increase in thermal conductivity due to thermal conduction in the phenolic resin portion, which increases with decreasing cell diameter. Furthermore, a cell diameter of 250 μm or less reduces heat conduction due to radiation within the cells, suppressing the increase in thermal conductivity. The average cell diameter of the phenolic resin foam can be adjusted to a desired value by, for example, changing the amount of solid foam nucleating agent added, the temperature of the foamable phenolic resin composition, the timing of pre-molding in the process of discharging the mixed foamable phenolic resin composition onto the lower surface material, the amount of foaming agent added, the amount of acidic curing agent added, and curing conditions such as temperature and residence time.
[0023] The thermal conductivity of the phenolic resin foam of this embodiment at 23°C is 0.024 W / (m K) or less, preferably 0.02330 W / (m K) or less, more preferably 0.02230 W / (m K) or less, even more preferably 0.02150 W / (m K) or less, and most preferably 0.02115 W / (m K) or less.
[0024] Phenolic resin foam laminates can be used alone or bonded to external components for a variety of applications. Examples of external components include board-shaped materials, sheet-shaped / film-shaped materials, and combinations thereof. Suitable board-shaped materials include wood-based boards such as ordinary plywood, structural plywood, particle board, and OSB, as well as wood-cement boards, wood-chip cement boards, gypsum boards, flexible boards, medium-density fiberboards, calcium silicate boards, magnesium silicate boards, and volcanic glass multi-layer boards. Suitable sheet-shaped / film-shaped materials include polyester nonwoven fabrics, polypropylene nonwoven fabrics, inorganic-filled glass fiber nonwoven fabrics, glass fiber nonwoven fabrics, paper, calcium carbonate paper, polyethylene-coated paper, polyethylene film, plastic moisture-proof films, asphalt waterproof paper, and aluminum foil (with or without holes).
[0025] The method for producing the phenolic foam will now be described in more detail.
[0026] <Raw Materials for Phenolic Resin Foam> The phenolic resin used is a resol-type phenolic resin synthesized using alkali metal hydroxides or alkaline earth metal hydroxides. Resole-type phenolic resins are synthesized by heating phenols and aldehydes as raw materials in the presence of an alkali catalyst at temperatures ranging from 40 to 100°C. If necessary, additives such as urea may be added during or after the synthesis of the resol-type phenolic resin. When adding urea, it is preferable to mix urea that has been methylolated with an alkali catalyst into the resol-type phenolic resin. Since synthesized resol-type phenolic resins typically contain excess moisture, the moisture content is adjusted to an appropriate level for foaming during foaming. Furthermore, aliphatic hydrocarbons, high-boiling alicyclic hydrocarbons, or mixtures thereof, viscosity-adjusting diluents such as ethylene glycol and diethylene glycol, and other additives such as dicyandiamide and melamine may also be added to the phenolic resin. If necessary, lignin may be added during or after the synthesis of the resol-type phenolic resin.
[0027] The starting molar ratio of phenols to aldehydes in the synthesis of the phenolic resin is preferably in the range of 1:1 to 1:4.5, more preferably in the range of 1:1.5 to 1:2.5. If necessary, lignin may be dissolved in advance in the phenols used in the synthesis.
[0028] In this embodiment, phenols preferably used in synthesizing the phenolic resin include phenol itself and other phenols, examples of which include resorcinol, catechol, o-, m-, and p-cresol, xylenols, ethylphenols, and p-tert-butylphenol. Dinuclear phenols can also be used.
[0029] The aldehyde may be any compound that can serve as an aldehyde source, and preferred aldehydes include formaldehyde itself, paraformaldehyde that can be depolymerized for use, and other aldehydes and their derivatives. Examples of other aldehydes include glyoxal, acetaldehyde, chloral, furfural, and benzaldehyde.
[0030] The mass average molecular weight of the phenolic resin is preferably 300 or more, more preferably 400 or more, and even more preferably 450 or more. The mass average molecular weight is preferably 2,500 or less, more preferably 2,200 or less, even more preferably 2,050 or less, and most preferably 1,900 or less. When the mass average molecular weight of the phenolic resin is 300 or more, runaway reaction due to the heat of the curing reaction is unlikely to occur, and foam molding can be performed using the reaction heat, resulting in good energy efficiency. Furthermore, when the mass average molecular weight is 2,500 or less, the reaction heat of the polymerization reaction is small, which tends to reduce the bubble diameter. Since the resin is less likely to harden in equipment upstream of the board molding process, piping is less likely to become dirty, and long-term continuous operation is possible. The mass average molecular weight of the phenolic resin can be measured using the method described in the examples of this specification.
[0031] The viscosity of the phenolic resin composition at 40°C is preferably 5,000 mPa·s or more and 100,000 mPa·s or less, more preferably 7,000 mPa·s or more and 50,000 mPa·s or less, and even more preferably 9,000 mPa·s or more and 40,000 mPa·s or less.
[0032] The lignin, surfactant, foaming agent and foam nucleating agent may be added to the phenolic resin composition in advance, or may be added simultaneously with the acidic curing agent.
[0033] Usable lignins include woody and herbaceous lignins, including kraft lignin, lignosulfonic acid, lignosulfonates, soda lignin, organosolv lignin, explosive lignin, sulfuric acid lignin, alkaline lignin, dealkalized lignin, and derivatives, modified products, and decomposition products thereof. These lignins can be used alone or in combination of two or more types.
[0034] The water content of the lignin-containing phenolic resin composition is 1.5% by mass or more and 6.5% by mass or less, preferably 1.5% by mass or more and 5.0% by mass or less. It is more preferably 1.5% by mass or more and 4.8% by mass or less, and even more preferably 1.5% by mass or more and 4.2% by mass or less. It is most preferably 4.0% by mass or less. If the water content is less than 1.5% by mass, the viscosity of the lignin-containing phenolic resin composition increases rapidly, significantly reducing productivity. If the water content is greater than 6.5% by mass, foaming and curing are inhibited, making it impossible to maintain fine cells, resulting in high thermal conductivity.
[0035] The method for adjusting the moisture content of the lignin-containing phenolic resin composition is not particularly limited, but for example, it can be appropriately adjusted by using a thin-film evaporator to control the temperature and the degree of vacuum by steam pressure.
[0036] The moisture content of the lignin added to the phenolic resin composition is 34.0% by mass or less, preferably 11.0% by mass or less. More preferably, it is 7.0% by mass or less, and even more preferably, it is 6.0% by mass or less. Most preferably, it is 5.5% by mass or less. If the moisture content is greater than 34.0% by mass, a large amount of moisture from the lignin dissipates during foaming and curing, leading to coarsening of the foam's cell diameter and an increase in the foam's thermal conductivity. Furthermore, if the moisture content is greater than 34.0% by mass, viscosity increase is unlikely to occur when the lignin-containing phenolic resin composition, blowing agent, and acidic curing agent are mixed in a mixer, reducing the generation of shear heat in the mixer and delaying the foaming and curing time. If the moisture content is 34.0% by mass or less, viscosity increase occurs during mixing, shear heat is generated in the mixer, and the lignin-containing phenolic resin composition is preheated, thereby reducing the curing reaction inhibitory effect of lignin. Therefore, a lignin-containing phenolic resin foam can be produced in the same foaming and curing time as a lignin-free phenolic resin foam, without impairing productivity.
[0037] The method for adjusting the moisture content of the lignin is not particularly limited, but can be appropriately done, for example, by heating or drying the lignin powder using a constant temperature air-blowing dryer.
[0038] The median diameter of the lignin powder is preferably 0.1 μm to 300 μm, more preferably 0.1 μm to 250 μm, even more preferably 0.1 μm to 200 μm, and most preferably 0.1 μm to 150 μm. If the median diameter is greater than 300 μm, the size of the lignin particles in the phenolic resin foam will be significantly larger than the cell diameter of the foam, making the cells more likely to break and increasing the thermal conductivity.
[0039] The method for pulverizing the lignin powder is not particularly limited, but examples include methods using a pulverizer such as a rolling ball mill, a rolling rod mill, a vibrating ball mill, a vibrating rod mill, a pan mill, a roller mill, or a high-speed rotary mill.
[0040] The timing of adding lignin is not particularly limited, and can be determined arbitrarily as long as it is supplied into a mixer that mixes the phenolic resin composition, the blowing agent, and the acidic curing agent. If lignin is added downstream of the mixer, the dispersibility of the lignin in the phenolic resin composition will decrease, resulting in a phenolic resin foam in which lignin is locally present within the foam. When used as a heat insulating material, the lignin will function as a thermal bridge, resulting in high thermal conductivity. Therefore, it is preferable to add lignin in a process upstream of the mixer that mixes the phenolic resin composition.
[0041] The amount of lignin added is preferably 1.0% by mass or more but less than 30.0% by mass, more preferably 1.0% by mass or more but less than 25.0% by mass, based on 100 parts by mass of the phenolic resin composition. It is even more preferably 1.0% by mass or more but less than 12.0% by mass, and most preferably 1.0% by mass or more but less than 8.0% by mass. If the amount of lignin added is less than 1.0% by mass, the proportion of plant-derived materials in the phenolic resin foam is low, resulting in low value as a bio-based material. If the amount of lignin added exceeds 30.0% by mass, the proportion of lignin in the phenolic resin foam increases, which is undesirable because the viscosity increases when added to the phenolic resin. Furthermore, when used as an insulating material, the lignin functions as a thermal bridge, resulting in high thermal conductivity.
[0042] Surfactants commonly used in the production of phenolic resin foams can be used, but nonionic surfactants are particularly effective. Examples include alkylene oxides (copolymers of ethylene oxide and propylene oxide), condensates of alkylene oxides and castor oil, condensation products of alkylene oxides and alkylphenols such as nonylphenol and dodecylphenol, polyoxyethylene alkyl ethers having 14 to 22 carbon atoms in the alkyl ether moiety, fatty acid esters such as polyoxyethylene fatty acid esters, silicone compounds such as polydimethylsiloxane, and polyalcohols. These surfactants may be used alone or in combination of two or more. There are no particular restrictions on the amount used, but a range of 0.3 to 10 parts by weight per 100 parts by weight of phenolic resin is preferred.
[0043] As the blowing agent, hydrofluoroolefins, hydrocarbons and chlorinated hydrocarbons can be used alone or in combination of two or more thereof.
[0044] Hydrofluoroolefins generally have low thermal conductivity, and when used as a blowing agent, they are preferred because they can produce phenolic resin foams with low thermal conductivity. Hydrofluoroolefins include chlorinated hydrofluoroolefins and non-chlorinated hydrofluoroolefins. In the present invention, chlorinated hydrofluoroolefins and non-chlorinated hydrofluoroolefins can also be used in combination.
[0045] Examples of chlorinated hydrofluoroolefins include (Z)-1-chloro-2,3,3,3-tetrafluoropropene (HCFO-1224yd(Z)), 1-chloro-3,3,3-trifluoropropene (HCFO-1233zd, for example, E-isomer (HCFO-1233zd(E)), manufactured by Honeywell Japan Co., Ltd., product name: Solstice™ LBA), and 1,1,2-trichloro-3,3,3-trifluoropropene (HCFO-1224yd(Z)). 13xa), 1,2-dichloro-3,3,3-trifluoropropene (HCFO-1223xd), 1,1-dichloro-3,3,3-trifluoropropene (HCFO-1223za), 1-chloro-1,3,3,3-tetrafluoropropene (HCFO-1224zb), 2,3,3-trichloro-3-fluoropropene (HCFO-1231xf), 2,3-dichloro-3,3-difluoropropene (HCFO-1232xf), 2-chloro- 1,1,3-trifluoropropene (HCFO-1233xc), 2-chloro-1,3,3-trifluoropropene (HCFO-1233xe), 2-chloro-3,3,3-trifluoropropene (HCFO-1233xf), 1-chloro-1,2,3-trifluoropropene (HCFO-1233yb), 3-chloro-1,1,3-trifluoropropene (HCFO-1233yc), 1-chloro-2,3,3-trifluoropropene (HCFO Examples of chlorinated hydrofluoroolefins include 3-chloro-1,2,3-trifluoropropene (HCFO-1233ye), 3-chloro-2,3,3-trifluoropropene (HCFO-1233yf), 1-chloro-1,3,3-trifluoropropene (HCFO-1233zb), and 1-chloro-3,3,3-trifluoropropene (HCFO-1233zd), and these configurational isomers, i.e., E- and Z-configurational isomers, or a mixture thereof, may be used. Further examples include (E)-1-chloro-2,3,3,3-tetrafluoropropene (HCFO-1224yd(E)). In the present invention, two or more of these chlorinated hydrofluoroolefins may be used in combination.
[0046] Examples of non-chlorinated hydrofluoroolefins include 1,3,3,3-tetrafluoroprop-1-ene (HFO-1234ze, for example, the E-form (HFO-1234ze(E)), manufactured by Honeywell Japan Co., Ltd., product name: Solstice™ ze), 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz, for example, the Z-form (HFO-1336mzz(Z)), manufactured by Chemours Inc., Opteon™ 1100), and 2,3,3,3 1,1,3,3,3-tetrafluoro-1-propene (HFO-1234yf), 1,1,3,3,3-pentafluoropropene (HFO-1225zc), 1,3,3,3-tetrafluoropropene (HFO-1234ze), 3,3,3-trifluoropropene (HFO-1243zf), 1,1,1,4,4,5,5,5-octafluoro-2-pentene (HFO-1438mzz), and the like are used as configurational isomers, i.e., E-isomers and Z-isomers, or a mixture thereof. In the present invention, two or more of these non-chlorinated hydrofluoroolefins can also be used as a mixture.
[0047] Preferred hydrocarbons are cyclic or chain alkanes, alkenes, and alkynes having 3 to 7 carbon atoms. Specific examples include normal butane, isobutane, cyclobutane, normal pentane, isopentane, cyclopentane, neopentane, normal hexane, isohexane, 2,2-dimethylbutane, 2,3-dimethylbutane, and cyclohexane. Among these, pentanes such as normal pentane, isopentane, cyclopentane, and neopentane, and butanes such as normal butane, isobutane, and cyclobutane are preferred. In the present invention, these hydrocarbons can also be used in combination with two or more other hydrocarbons. Examples of such mixtures include normal pentane and normal butane, isobutane and isopentane, normal butane and isopentane, isobutane and normal pentane, cyclopentane and normal butane, and cyclopentane and isobutane. A mixture of cyclopentane and isobutane is particularly preferred.
[0048] As the chlorinated hydrocarbon, linear or branched chlorinated aliphatic hydrocarbons having 2 to 5 carbon atoms can be preferably used. The number of bonded chlorine atoms is preferably 1 to 4, and examples thereof include dichloroethane, propyl chloride, 2-chloropropane, butyl chloride, isobutyl chloride, pentyl chloride, and isopentyl chloride. Of these, propyl chloride and 2-chloropropane, which are chloropropanes, are more preferably used. In the present invention, these chlorinated hydrocarbons can also be used in combination of two or more types.
[0049] Furthermore, the other foaming agents are not particularly limited and include, for example, chemical foaming agents such as sodium bicarbonate, sodium carbonate, calcium carbonate, magnesium carbonate, azodicarboxylic acid amide, azobisisobutyronitrile, barium azodicarboxylate, N,N'-dinitrosopentamethylenetetramine, p,p'-oxybisbenzenesulfonylhydrazide, and trihydrazinotriazine. These foaming agents may be used alone or in combination of two or more.
[0050] The amount of blowing agent in the phenolic resin composition varies depending on the type of blowing agent, the compatibility of the blowing agent with the phenolic resin, and the foaming and curing conditions, such as temperature and residence time. Therefore, the amount of blowing agent can be determined arbitrarily based on the desired density of the phenolic resin foam, the foaming conditions, etc. However, the amount of blowing agent is preferably 3.0 to 20 parts by mass, more preferably 4.0 to 18 parts by mass, even more preferably 5.0 to 16 parts by mass, and most preferably 6.0 to 15 parts by mass, per 100 parts by mass of the phenolic resin composition. When the amount of blowing agent per 100 parts by mass of the phenolic resin composition is 3.0 parts by mass or more, the resin foam can be prevented from becoming denser. Furthermore, when the amount of blowing agent per 100 parts by mass of the phenolic resin composition is 20 parts by mass or less, the phenolic resin foam can be prevented from becoming low-density, which can lead to a decrease in mechanical strength, such as compressive strength, and an increase in thermal conductivity.
[0051] In this embodiment, a foam nucleating agent may be used to produce the phenolic resin foam. Examples of the foam nucleating agent include gaseous foam nucleating agents, such as nitrogen, helium, and argon, which have a boiling point 50° C. or more lower than that of the foaming agent. Solid foam nucleating agents may also be used, such as inorganic powders such as aluminum hydroxide powder, aluminum oxide powder, calcium carbonate powder, talc, kaolin, silica stone powder, silica sand, mica, calcium silicate powder, wollastonite, glass powder, glass beads, fly ash, silica fume, gypsum powder, borax, slag powder, alumina cement, and Portland cement, and organic powders such as crushed powder of phenolic resin foam. These may be used alone or in combination of two or more, regardless of whether they are gaseous or solid. The timing of adding the foam nucleating agent can be determined arbitrarily, as long as it is supplied to the mixer used to mix the phenolic resin composition.
[0052] When a gas foam nucleating agent is added, the amount added is preferably 0.2% by mass or more and 1.0% by mass or less, and more preferably 0.3% by mass or more and 0.5% by mass or less, based on 100% by mass of the amount of the foaming agent.
[0053] The amount of the solid foam nucleating agent added is preferably 3.0% by mass or more and 10.0% by mass or less, and more preferably 3.0% by mass or more and 8.0% by mass or less, relative to 100 parts by mass of the phenolic resin composition. When the amount of the solid foam nucleating agent added is 3.0% by mass or more, it becomes easier to suppress the seepage of the foamable phenolic resin composition from the surface material. Furthermore, when the amount of the solid foam nucleating agent added is 10.0% by mass or less, it becomes easier to suppress the emission of a foaming agent with a low boiling point.
[0054] The acidic curing agent may be any acidic curing agent capable of curing the phenolic resin composition, and contains an organic acid as the acid component. The organic acid is preferably an arylsulfonic acid or an anhydride thereof. Examples of arylsulfonic acids and anhydrides thereof include toluenesulfonic acid, xylenesulfonic acid, phenolsulfonic acid, substituted phenolsulfonic acid, xylenolsulfonic acid, substituted xylenolsulfonic acid, dodecylbenzenesulfonic acid, benzenesulfonic acid, naphthalenesulfonic acid, and the like, as well as their anhydrides. These may be used alone or in combination of two or more. In this embodiment, resorcinol, cresol, saligenin (o-methylolphenol), p-methylolphenol, or the like may be added as a curing aid. These acidic curing agents may also be diluted with solvents such as ethylene glycol and diethylene glycol.
[0055] The amount of acidic curing agent used varies depending on the type thereof. When a mixture of 80% by mass of xylene sulfonic acid and 20% by mass of diethylene glycol is used, the amount used is preferably 6 parts by mass or more and 20 parts by mass or less, more preferably 8 parts by mass or more and 15 parts by mass or less, and most preferably 11 parts by mass or more and 13 parts by mass or less, per 100 parts by mass of the phenolic resin composition.
[0056] A flexible surface material (flexible surface material) is used as the surface material disposed on at least one of the surfaces of the phenolic resin foam and the back surface of the phenolic resin foam. Examples of suitable flexible surface materials include nonwoven or woven fabrics primarily composed of polyester, polypropylene, nylon, or the like; paper materials such as kraft paper, glass fiber-blended paper, calcium hydroxide paper, aluminum hydroxide paper, and magnesium silicate paper; and inorganic fiber nonwoven fabrics such as glass fiber nonwoven fabrics. These materials may be mixed (or laminated) together. When peeling the surface material from the resulting phenolic resin foam laminate and using only the base material, inexpensive paper materials that can be disposed of after peeling are preferred. These surface materials are typically provided in roll form. Furthermore, the flexible surface material may contain additives such as flame retardants. The method of bonding the surface material and the phenolic resin foam is not particularly limited, and an adhesive such as an epoxy resin may be used. However, from the viewpoint of production costs and preventing the production process from becoming complicated, it is preferable that the bonding be achieved solely by the adhesive force that occurs when the foamable phenolic resin composition is thermally cured on the surface of the surface material.
[0057] <Method for manufacturing phenolic resin foam and laminate thereof> A phenolic resin foam laminate is manufactured by a continuous manufacturing method including a mixing step of mixing the foamable phenolic resin composition described above in a mixer, a discharging step of discharging the mixed foamable phenolic resin composition onto a lower surface material, and a foam laminate manufacturing step of manufacturing a phenolic resin foam laminate from the foamable phenolic resin composition discharged onto the lower surface material. It is also possible to employ a batch method using a mold in which each step is performed in stages. The phenolic resin foam can also be used without a surface material laminated thereon or by removing the surface material.
[0058] In the continuous manufacturing method, the phenolic resin composition dispensed onto the lower surface material is coated with the upper surface material, and then preformed from above and below while foaming and curing, followed by final molding into a plate while foaming and curing. In the continuous manufacturing method, various methods for preforming and final molding can be used depending on the manufacturing purpose, such as using a slat-type double conveyor, a metal roll or steel plate, or a combination of these. For example, when molding using a slat-type double conveyor, the foamable phenolic resin composition coated with the upper and lower surface materials is continuously guided into the slat-type double conveyor, and then heated and pressure is applied from above and below to adjust the thickness, foaming and curing, and molding into a plate. The temperature of the foamable phenolic resin composition when dispensed onto the lower surface material depends on the boiling point of the foaming agent, but is generally preferably between 32°C and 45°C. When the temperature of the foamable phenolic resin composition is 32°C or higher, the foamable phenolic resin composition is more likely to foam initially, making it easier to prevent the foamable phenolic resin composition from seeping out of the lower surface material. On the other hand, when the temperature of the foamable phenolic resin composition is 45°C or lower, it is easier to prevent diffusion even when a foaming agent with a low boiling point is used, making it easier to prevent a decrease in foaming efficiency and an increase in thermal conductivity due to coarsening of the bubble diameter. The temperature of the foamable phenolic resin composition discharged onto the lower surface material can be adjusted by adjusting the temperature and flow rate of the water temperature control device, the rotation speed, etc. of the mixer that mixes the various compositions.
[0059] <Preforming Step> The heating temperature control conditions for the step of performing preforming on the upper surface material while foaming and curing the foamable phenolic resin composition dispensed onto the lower surface material are preferably 30°C or higher and 80°C or lower. At 30°C or higher, the foaming promotion effect in the preforming step is easily achieved, and curing can be accelerated. Furthermore, at 80°C or lower, the vicinity of the center in the thickness direction is less susceptible to internal heat generation, the temperature at the center is less likely to rise, and thermal conductivity can be maintained for a long period of time. When foaming and curing the foamable phenolic resin composition, in order to efficiently promote curing while suppressing internal heat generation near the center in the thickness direction, it is important to provide a main molding step and a post-curing step following the preforming step, thereby gradually increasing the temperature. The residence time in the preforming step is preferably 1 minute or higher and 20 minutes or lower.
[0060] <Main Molding Process> The heating temperature control conditions for the main molding process following the pre-molding process are preferably 65°C or higher and 100°C or lower. In this section, main molding can be performed using an endless steel belt type double conveyor, a slat type double conveyor, or rolls, etc. Furthermore, since this is the main process in which the foaming and curing reactions occur, the residence time for the main molding process is preferably 5 minutes or higher and 40 minutes or lower. A residence time of 5 minutes or longer can sufficiently promote foaming and curing. A residence time of 2 hours or less can increase the production efficiency of phenolic resin foam laminates. When using conveyors, it is desirable to keep the temperature difference between the upper and lower conveyors to less than 4°C.
[0061] <Post-curing step> After heating and temperature control through the temperature control sections of the pre-molding step and main molding step, the post-curing step is applied. The temperature of the post-curing step is preferably 90°C or higher and 120°C or lower. If the temperature is 90°C or higher, moisture in the foam is easily dissipated, and if the temperature is 120°C or lower, the low thermal conductivity of the product can be maintained for a long period of time. By providing a temperature control section in the post-curing step, moisture in the foamable phenolic resin composition can be dissipated after final molding. The residence time in the post-curing step is preferably 60 minutes or higher and 300 minutes or lower.
[0062] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.
[0063] <Synthesis of phenolic resin> A reactor was charged with 3,500 kg of a 52% by mass aqueous formaldehyde solution (52% by mass formalin) and 2,510 kg of 99% by mass phenol (containing water as an impurity), and the mixture was stirred with a propeller-rotating stirrer. The temperature of the liquid inside the reactor was adjusted to 40°C with a temperature controller. Next, the temperature was raised while adding a 48% by mass aqueous sodium hydroxide solution, and the reaction was carried out. The Ostwald viscosity of the reaction liquid was 110 centistokes (= 110 × 10 -6 m 2 When the reaction temperature reached 100°C (1 / s, measured at 25°C), the reaction solution was cooled, and 398 kg of urea was added. Thereafter, the reaction solution was cooled to 30°C, and neutralized to a pH of 6.4 with a 50% by mass aqueous solution of paratoluenesulfonic acid monohydrate.
[0064] This reaction solution was concentrated at 60° C. to obtain a phenolic resin. The mass average molecular weight and viscosity at 40° C. of the phenolic resin were measured by the following methods, and the mass average molecular weight was 500, the viscosity at 40° C. was 9,730 mPa·s, and the water content was 4.0% by mass.
[0065] <Weight-average molecular weight of phenolic resin> Measurement was performed by gel permeation chromatography (GPC) under the following conditions, and the weight-average molecular weight Mw of the phenolic resin was determined from a calibration curve obtained using standard substances (standard polystyrene, 2-hydroxybenzyl alcohol, and phenol) shown below. Pretreatment: Approximately 10 mg of phenolic resin was dissolved in 1 ml of N,N-dimethylformamide (Fujifilm Wako Pure Chemical Industries, Ltd., for high-performance liquid chromatography), and the solution was filtered through a 0.2 μm membrane filter and used as the measurement solution. Measurement conditions: Measurement device: Shodex System 21 (Showa Denko K.K.) Column: Shodex Asahipak GF-310HQ (7.5 mm I.D. × 30 cm) Eluent: 0.1% by mass of lithium bromide dissolved in N,N-dimethylformamide (Fujifilm Wako Pure Chemical Industries, Ltd., for high-performance liquid chromatography). Flow rate: 0.6 ml / min Detector: RI detector Column temperature: 40°C Standard substances: standard polystyrene (Shodex STANDARD SL-105 manufactured by Showa Denko K.K.), 2-hydroxybenzyl alcohol (Sigma-Aldrich, 99% product), phenol (Kanto Chemical Co., Ltd., special grade)
[0066] <Viscosity Measurement of Phenolic Resin> Using a rotational viscometer (manufactured by BrookField Metek, DVNXHBCBG model, rotor part CPA-52Z), 0.5 ml of phenolic resin was stabilized at 40° C. for 6 minutes, and the measured value was taken as the viscosity of the phenolic resin.
[0067] Example 1 100 parts by mass of phenolic resin was mixed with 3.0 parts by mass of a surfactant composition containing 50% by mass of an ethylene oxide-propylene oxide block copolymer and 50% by mass of polyoxyethylene dodecyl phenyl ether. This composition was designated the phenolic resin composition. As lignin, 8.0% by mass of dealkalized lignin (manufactured by Tokyo Chemical Industry Co., Ltd.) obtained by the sulfite method, which had been previously heat-dried at 120°C for 20 minutes in a constant temperature air dryer and then pulverized, and which had a median diameter of 25.7 μm and a moisture content of 10.2% was added to 100 parts by mass of the surfactant-containing phenolic resin composition. This composition was designated the lignin-containing phenolic resin composition. The lignin-containing phenolic resin composition was concentrated using a thin-film evaporator, and the moisture content was found to be 4.20% by mass. Additionally, 13 parts by weight of a foaming agent consisting of a mixture of 70% by weight of cyclopentane and 30% by weight of isobutane, 0.4% by weight of nitrogen as a gas foam nucleating agent relative to the foaming agent, and 13 parts by weight of a composition consisting of a mixture of 80% by weight of xylene sulfonic acid and 20% by weight of diethylene glycol as an acidic curing agent were added to 100 parts by weight of the lignin-containing phenolic resin composition, and the mixture was fed into a variable-speed mixing head controlled at 17°C. The lignin was kneaded with the phenolic resin composition in a twin-screw extruder before adding the foaming agent and acidic curing agent. The gas foam nucleating agent, foaming agent, and acidic curing agent were then mixed in a mixer, and the resulting foamable phenolic resin composition was distributed through a multi-port distribution pipe and fed onto a moving bottom surface material. The mixer used was the one disclosed in Figure 1 of JP-A-10-225993. Specifically, a mixer was used in which an inlet for the lignin-containing phenolic resin composition and an inlet for the foaming agent were adjacently arranged on the upper side of the mixer, and an inlet for the acidic curing agent was provided on the side near the center of the agitation section where the rotor agitates. The agitation section and the subsequent sections were connected to a nozzle for discharging the foamable phenolic resin composition. The mixer was comprised of a mixing section (pre-stage) up to the acidic curing agent inlet, a mixing section (post-stage) from the acidic curing agent inlet to the agitation end section, and a distribution section from the agitation end section to the nozzle. The distribution section had multiple nozzles at its tip and was designed to uniformly distribute the mixed foamable phenolic resin composition.Furthermore, the distribution section had a jacketed structure, allowing for sufficient heat exchange using temperature-controlled water. The temperature of the temperature-controlled water in the distribution section was set to 17°C. A thermocouple was installed at the outlet of the multi-port distribution pipe to detect the temperature of the foamable phenolic resin composition, and the mixer rotation speed was set to 500 rpm. The temperature of the foamable phenolic resin composition dispensed onto the lower surface material was 34°C. The foamable phenolic resin composition dispensed onto the lower surface material was introduced into a pre-molding process controlled at 40°C, and after 30 seconds, pre-molding was performed using a free roller from above the upper surface material. The residence time in this process was 5 minutes. The composition was then sandwiched between two surface materials and introduced into a slat-type double conveyor heated to 69°C (main molding process). After curing for 15 minutes, it was retained at 100°C for 9 minutes and then cured at 110°C for 2 hours (post-curing process), yielding a phenolic resin foam laminate of Example 1 with a thickness of approximately 30 mm. The surface materials for both the top and bottom surfaces are polyester nonwoven fabric (Asahi Kasei Corporation Eltas E05060, basis weight 60 g / m). 2 ) was used. This production method is shown as Production Method A in Table 2. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to the foaming and curing rate of the lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0068] The properties of the lignin powder used were evaluated by the following method.
[0069] <Measurement of Median Diameter of Lignin Powder> The median diameter of the lignin powder was measured using a laser diffraction light scattering particle size distribution measuring device (Microtrac HRA; 9320-X100, manufactured by Nikkiso Co., Ltd.) after treating the lignin powder with ultrasound for 1 minute to uniformly disperse it in water.
[0070] <Measurement of Moisture Content of Lignin Powder> The moisture content of the lignin powder was calculated using a moisture meter (Shimadzu Corporation, MOC63u) by heating 0.5 g of the powder at 120°C for 20 minutes, and then dividing the difference between the mass before and after heating, M (g), by the mass before heating, according to the following formula: moisture content (mass%) = ((0.5 - M) / 0.5) × 100
[0071] The properties of the phenolic resin composition and the lignin-containing phenolic resin composition used were evaluated by the following methods.
[0072] <Measurement of Moisture Content of Phenolic Resin Composition and Lignin-Containing Phenolic Resin Composition> The moisture content of the phenolic resin composition and the lignin-containing phenolic resin composition was measured using a volumetric titration Karl Fischer moisture meter (Kyoto Electronics Manufacturing Co., Ltd., MKV-710) using Chem-Aqua titrant TR-3 (Kyoto Electronics Manufacturing Co., Ltd.) as the Karl Fischer reagent and Chem-Aqua dehydrating solvent MET (Kyoto Electronics Manufacturing Co., Ltd.) as the dehydrating solvent.
[0073] The properties of the obtained phenolic resin foam and phenolic resin foam laminate were evaluated (identification of the lignin component in the phenolic resin foam, measurement of density, measurement of the thermal conductivity of the phenolic resin foam laminate in an environment of 23°C, measurement of the average cell diameter of the phenolic resin foam, and identification of the type of blowing agent in the phenolic resin foam) by the following methods.
[0074] <Identification of lignin components in phenolic resin foam> A phenolic resin foam laminate was used as a sample. After removing the surface material from the sample, pyrolysis gas chromatography mass spectrometry was performed under the following measurement and analysis conditions to identify the lignin components present in the phenolic resin foam.
[0075] <Conditions for pyrolysis gas chromatography mass spectrometry (GC-MS)> GC apparatus: Agilent Technologies 7890B Column: DB1 (30 m, 0.25 mmφ, liquid phase thickness 0.25 μm) Column temperature: 40°C (5 min) → (heating at 10°C / min) → 320°C (hold for 12 min) Flow rate: 1 ml / min constant flow Injector temperature: 300°C Injection method: split method (split ratio 100:1) MS apparatus: JEOL RESONANCE, JMS-Q1500GC Interface temperature: 300°C Ionization method: EI (electron ionization) method 70 eV (temperature 230°C) Pyrolysis apparatus: Frontier-lab EGA / PY-3030D Pyrolysis temperature: 600°C (under He atmosphere) Scan range: m / z 10-800 Sample amount: 1 mg
[0076] In gas chromatography-mass spectrometry, when the retention time at which phenol is detected in the obtained total ion chromatogram is t minutes, a pyrolysis product derived from dihydroxybenzene is detected at a retention time of approximately 1.38 × t minutes in the extracted ion chromatogram of m / z = 110, a pyrolysis product derived from dihydroxytoluene is detected at a retention time of approximately 1.46 × t minutes in the extracted ion chromatogram of m / z = 124, a pyrolysis product derived from dihydroxytoluene is detected at a retention time of approximately 1.50 × t minutes in the extracted ion chromatogram of m / z = 138, and a pyrolysis product derived from dihydroxyxylene is detected at a retention time of approximately 1.58 × t minutes in the extracted ion chromatogram of m / z = 138. Note that, by the above-mentioned pyrolysis-gas chromatography-mass spectrometry measurement method, phenol was detected at a retention time of approximately 10.0 minutes.
[0077] In the ion chromatogram of the obtained pyrolysis products, the area of the pyrolysis product derived from dihydroxybenzene detected at a retention time of approximately 1.38 × t minutes in the extracted ion chromatogram of m / z = 110 is defined as A; the sum of the area of the pyrolysis product derived from dihydroxytoluene detected at a retention time of approximately 1.46 × t minutes and the area of the pyrolysis product derived from dihydroxytoluene detected at a retention time of approximately 1.50 × t minutes in the extracted ion chromatogram of m / z = 124 is defined as B; the area of the pyrolysis product derived from dihydroxyxylene detected at a retention time of approximately 1.58 × t minutes in the extracted ion chromatogram of m / z = 138 is defined as C; and the sum of A, B, and C is defined as X (X = A + B + C). Furthermore, when the area of a thermal decomposition product corresponding to Peak 9 in [Fig. 1] of Japanese Patent No. 4711469 and exhibiting a structure derived from urea crosslinking, which was detected in the total ion chromatogram at a retention time of approximately 1.50 × t minutes, was defined as Y, the ratio of X to Y was calculated as Z (Z = X / Y). Furthermore, the areas A, B, C, and Y were calculated using the intersection with the baseline or the inflection point with the adjacent peak as the boundary.
[0078] <Measurement of Density of Phenolic Resin Foam> A 200 mm square phenolic resin foam laminate was used as a sample, and after removing the surface material from the sample, the mass and apparent volume were measured according to JIS K7222 to determine the density.
[0079] <Measurement of thermal conductivity of phenolic resin foam laminate in an environment of 23°C> The thermal conductivity of the resin foam laminate in the thickness direction in an environment of 23°C was measured by the following method in accordance with JIS A 1412-2:1999. The specific procedure is as follows.
[0080] The phenolic foam laminate was cut into 300 mm square pieces and placed in an atmosphere at 23±1°C and 50±2% humidity. The weight change over time was then measured every 24 hours, and the condition was checked and adjusted until the weight change after 24 hours was 0.2% by mass or less. The conditioned phenolic foam laminate specimen was then placed in a thermal conductivity measuring device also placed in an atmosphere at 23±1°C and 50±2% humidity. If the thermal conductivity measuring device was not placed in the same room controlled at 23±1°C and 50±2% humidity as the phenolic foam laminate specimen, the specimen whose condition had been checked and adjusted in the aforementioned atmosphere was immediately placed in a polyethylene bag, the bag was closed, and the specimen was removed from the bag within one hour, and the thermal conductivity was immediately measured.
[0081] The thermal conductivity was measured under the conditions of a low temperature plate of 13°C and a high temperature plate of 33°C using a measuring device with a single test piece and a symmetrical configuration (manufactured by Eiko Seiki Co., Ltd., product name "HC-074 / FOX304").
[0082] <Measurement of Average Cell Diameter of Phenolic Resin Foam> The average cell diameter was measured by the following method: A phenolic resin foam laminate was used as a sample, and after removing the surface material from the sample, four photographs of bubbles at approximately the center in the thickness direction of the phenolic resin foam and at approximately the center and the center relative to the front and back surfaces were taken using a scanning electron microscope at 50x magnification, and four straight lines 90 mm long (corresponding to 1,800 μm in the actual cross section of the foam) were drawn on the obtained photographs, avoiding voids, and the number of bubbles was determined for each line based on the number of bubbles crossed by each line, and the average value of these numbers was divided by 1,800 μm to obtain the average cell diameter.
[0083] <Identification of the type of blowing agent in phenolic resin foam> First, the retention times were determined under the following GC / MS measurement conditions using standard gases of halogenated hydrocarbons and hydrocarbons.
[0084] A phenolic foam laminate was used as the sample. After removing the surface material from the sample, a 0.25 mg sample was cut from near the center of the phenolic foam and placed in a dedicated container. 10 ml of chloroform and 12 crushed glass beads were added. The sample was crushed using a homogenizer (IKA ULTRA-TURRAX Tube Drive) at 6000 rpm for 7-11 min to extract the components into chloroform. The extract was then filtered through a 0.45 μm filter and subjected to GC / MS analysis. A standard sample solution of known concentration was prepared by dissolving the target component in chloroform and subjected to GC / MS analysis under the same conditions as the sample.
[0085] The halogenated hydrocarbons and hydrocarbons were identified based on the retention times and mass spectra obtained in advance. The detection sensitivity of each generated gas component was measured separately using a standard gas, and the content of each substance was calculated from the detection area and detection sensitivity of each gas component obtained by GC / MS. The mass percentage of each blowing agent component in the phenolic resin foam was calculated from the content of each identified gas component and the content and molar mass of the blowing agent.
[0086] Example 2 A phenolic resin foam laminate of Example 2 was produced in the same manner as Example 1, except that the lignin was changed to lignin (alkali) (manufactured by Tokyo Chemical Industry Co., Ltd.) obtained by the sulfite method, with a median diameter of 26.8 μm and a moisture content of 5.3 mass%. The moisture content of the lignin-containing phenolic resin composition after concentration was 3.85 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied to the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0087] Example 3 A phenolic resin foam laminate of Example 3 was produced in the same manner as Example 1, except that the lignin was not pulverized and was replaced with lignin sulfonate sodium salt having a median diameter of 238.5 μm and a moisture content of 5.0 mass%. The moisture content of the lignin-containing phenolic resin composition after concentration was 3.83 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied to the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0088] Example 4 A phenolic resin foam laminate of Example 4 was produced in the same manner as in Example 1, except that the lignin was changed to kraft lignin having a median diameter of 23.9 μm and a moisture content of 6.5% by mass. The moisture content of the lignin-containing phenolic resin composition after concentration was 3.93% by mass. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0089] Example 5 A phenolic resin foam laminate of Example 5 was produced in the same manner as in Example 1, except that the amount of lignin added per 100 parts by mass of the phenolic resin composition was 1.0 mass%. The water content of the lignin-containing phenolic resin composition after concentration was 3.80 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0090] Example 6 A phenolic resin foam laminate of Example 6 was produced in the same manner as in Example 1, except that the amount of lignin added per 100 parts by mass of the phenolic resin composition was 12.0 mass%. The water content of the lignin-containing phenolic resin composition after concentration was 4.40 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0091] Example 7 A phenolic resin foam laminate of Example 7 was produced in the same manner as in Example 1, except that the amount of lignin added per 100 parts by mass of the phenolic resin composition was 20.0 mass%. The water content of the lignin-containing phenolic resin composition after concentration was 4.78 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0092] Example 8 A phenolic resin foam laminate of Example 8 was produced in the same manner as in Example 1, except that the amount of lignin added per 100 parts by mass of the phenolic resin composition was 25.0 mass%. The water content of the lignin-containing phenolic resin composition after concentration was 4.99 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0093] Example 9 A phenolic resin foam laminate of Example 9 was produced in the same manner as in Example 1, except that the amount of lignin added per 100 parts by mass of the phenolic resin composition was 29.0 mass%. The water content of the lignin-containing phenolic resin composition after concentration was 5.15 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0094] Example 10 A phenolic resin foam laminate of Example 10 was produced in the same manner as in Example 1, except that the lignin was changed to kraft lignin with a median diameter of 23.9 μm and a moisture content of 6.5% by mass, and the amount of lignin added per 100 parts by mass of the phenolic resin composition was 29.0% by mass. The moisture content of the lignin-containing phenolic resin composition after concentration was 4.33% by mass. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied to the lower surface material was equivalent to that of a lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0095] Example 11 A phenolic resin foam laminate of Example 11 was produced in the same manner as in Example 1, except that 2.7 mass% of water was added to 100 mass parts of the surfactant-containing phenolic resin composition to adjust the water content of the concentrated lignin-containing phenolic resin composition to 6.50 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to that of the lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0096] Example 12 A phenolic resin foam laminate of Example 12 was produced in the same manner as in Example 1, except that (Z)-1-chloro-2,3,3,3-tetrafluoropropene (HCFO-1224yd(Z)) was used as the blowing agent. The water content of the lignin-containing phenolic resin composition after concentration was 4.20 mass%. The foaming and curing rate of the lignin-containing foamable phenolic resin composition supplied onto the lower surface material was equivalent to the foaming and curing rate of the lignin-free foamable phenolic resin composition (Comparative Example 1 described below).
[0097] Example 13: 100 parts by mass of phenolic resin was mixed with 3.0 parts by mass of a surfactant composition containing 50% by mass of an ethylene oxide-propylene oxide block copolymer and 50% by mass of polyoxyethylene dodecyl phenyl ether. This composition was designated the phenolic resin composition. Lignin (dealkalized) obtained by the sulfite method (Tokyo Chemical Industry Co., Ltd.), which had been previously heat-dried at 120°C for 20 minutes in a constant temperature air dryer and then pulverized, and had a median diameter of 25.7 μm and a moisture content of 10.2% was placed in a plastic cup so that the content was 8.0% by mass relative to 100 parts by mass of the surfactant-containing phenolic resin composition. The mixture was then kneaded using a cordless driver drill (Hi-Koki DS 10DAL) equipped with a stirring rod. This composition was designated the lignin-containing phenolic resin composition. The lignin-containing phenolic resin composition was concentrated using a thin-film evaporator, and the moisture content was found to be 4.20% by mass. Additionally, the lignin-containing phenolic resin composition was mixed using a cordless driver drill to obtain 12 parts by weight of normal pentane as a foaming agent per 100 parts by weight of the composition. No gaseous foam nucleating agent was added, but the air entrained during mixing served as the foam nucleating agent. The success of mixing the required amounts of each was confirmed by the change in the weight of the resin composition. The plastic cup containing the foamable phenolic resin composition was then cooled in a refrigerator for 1 hour. After confirming that the temperature of the foamable phenolic resin composition was below 12°C, 13 parts by weight of a composition consisting of a mixture of 80% by weight of xylene sulfonic acid and 20% by weight of diethylene glycol was added as an acidic curing agent, and the mixture was mixed for 2 minutes using a cordless driver drill. The foamable phenolic resin composition was then applied to the bottom of a metal frame (mold) with a spatula in an environment of 23°C. The amount of the foamable phenolic resin composition applied was appropriately adjusted so that the thickness did not extend beyond the frame (mold) after foaming. The metal frame (mold) used here was made of metal with a thickness of 2.0 mm, an inner diameter of 300 mm x 300 mm x height of 30 mm, and the bottom surface was punched with holes of 5 mm diameter at 1 mm intervals. The bottom surface was further covered with polyester nonwoven fabric (Asahi Kasei Corporation Eltas E05060, basis weight 60 g / m 2) was laid as a surface material. The working time from mixing the foamable phenolic resin composition and acidic curing agent to completing the application was 5 minutes. Then, a metal frame (mold) with the same punching specifications as the bottom plate, larger than 300 mm x 300 mm, was used as a top plate. The same surface material as the bottom plate was attached to the metal frame (mold). This top plate was placed on the metal frame (mold) with the surface material facing the foamable phenolic resin side, and the top plate was secured to the metal frame (mold) with clips. This metal frame (mold) was placed in an oven heated to 85°C, and a 25 kg weight heated to 85°C was placed on the center of the top plate of the metal frame (mold). The heat treatment was continued for 1 hour, followed by further curing at 105°C for 1 hour, yielding a 30 mm-thick phenolic resin foam laminate of Example 13. This production method is designated as Production Method B in Table 2. The foaming and curing rate of the foamable phenolic resin composition containing lignin applied to the bottom surface material (Comparative Example 1 described below) was comparable to that of the foamable phenolic resin composition not containing lignin.
[0098] Comparative Example 1 A phenolic resin foam laminate of Comparative Example 1 was produced in the same manner as in Example 1, except that lignin was not kneaded into the phenolic resin composition. The water content of the phenolic resin composition was 3.73 mass%. The foamable phenolic resin composition supplied onto the lower surface material had a foam curing rate that was sufficient to maintain sufficient productivity in the commercial production of phenolic resin foams.
[0099] Comparative Example 2 A phenolic resin foam laminate of Comparative Example 2 was produced in the same manner as in Example 1, except that the lignin was replaced with kraft lignin having a median diameter of 23.7 μm and a moisture content of 34.6% by mass without drying. The moisture content of the lignin-containing phenolic resin composition after concentration was 5.94% by mass. Furthermore, the foaming and curing rate of the lignin-containing foamable phenolic resin composition applied to the lower surface material was reduced compared to the foaming and curing rate of the lignin-free foamable phenolic resin composition (Comparative Example 1), resulting in an insufficiently cured foam. Therefore, a further curing step at 110°C for 4 hours after the post-curing step resulted in a fully cured foam.
[0100] Comparative Example 3 A phenolic resin foam laminate of Comparative Example 3 was produced in the same manner as in Example 1, except that 13.7% by mass of water was added to 100 parts by mass of the surfactant-containing phenolic resin composition, resulting in a water content of 15.70% by mass of the concentrated lignin-containing phenolic resin composition. The foaming and curing rate of the lignin-containing foamable phenolic resin composition applied to the lower surface material was reduced compared to the foaming and curing rate of the lignin-free foamable phenolic resin composition (Comparative Example 1), resulting in an insufficiently cured foam. Therefore, after the post-curing step, the foam was further cured at 110°C for 4 hours to obtain a sufficiently cured foam.
[0101] The types of lignin used in Examples 1 to 13 and Comparative Examples 2 to 3 are shown in Table 1. The above-mentioned measurements and evaluation tests were also carried out on Examples 1 to 13 and Comparative Examples 1 to 3. The measurement results and evaluation results are shown in Tables 2 and 3.
[0102]
[0103]
[0104]
[0105] By appropriately adjusting the water content of the lignin-added phenolic resin composition, the phenolic resin foam according to the present invention can maintain the foaming and curing time even when the foam contains lignin, allowing it to be produced without sacrificing productivity. Furthermore, by suppressing water-induced foaming inhibition and maintaining fine cells, the thermal conductivity and insulating performance of the lignin-containing phenolic resin foam can be maintained. Furthermore, by adding pulverized lignin powder with small particle size, cell destruction due to coarse particles of the lignin powder can be reduced, maintaining fine cells. This allows the thermal conductivity and insulating performance of the lignin-containing phenolic resin foam to be maintained. Furthermore, by using plant-derived materials, it is possible to provide a bio-based phenolic resin foam.
Claims
1. A phenolic resin foam in which, in an ion chromatogram obtained by subjecting gas components generated by heating at 600°C to gas chromatography mass spectrometry, the total area X (X=A+B+C) of the area A derived from dihydroxybenzene, the area B derived from dihydroxytoluene, and the area C derived from dihydroxyxylene, which are pyrolysis products, and the area Y of the pyrolysis product exhibiting a structure derived from urea crosslinking, Z (Z=X / Y), are within the range of the following formula (1), and the thermal conductivity value in an environment of 23°C is 0.0240 W / (m·K) or less. 0.035≦Z≦0.715 (1) 2. Density is 10 kg / m 3 More than 50kg / m 3 2. The phenolic foam of claim 1 , wherein:
3. The phenolic resin foam according to claim 1 or 2, having an average cell diameter of 70 μm or more and 250 μm or less.
4. The phenolic resin foam according to claim 1 or 2, which contains any one of hydrofluoroolefins, hydrocarbons, and chlorinated hydrocarbons.
5. The phenolic resin foam according to claim 1 or 2, which is provided with a surface material on at least one of one side of the phenolic resin foam and the back side of the one side.
6. A method for producing a phenolic resin foam laminate, which comprises foaming and curing a foamable phenolic resin composition, the method comprising at least one of the following steps to obtain the foamable phenolic resin composition: adding lignin to phenols, adding lignin during synthesis of a phenolic resin, adding lignin to a phenolic resin, and adding lignin to a phenolic resin composition, wherein the moisture content of the lignin is 34.0% or less, and the moisture content of the lignin-containing phenolic resin composition in the foamable phenolic resin composition is 1.5 mass% or more and 6.5 mass% or less.
7. The method according to claim 6, wherein the lignin powder added in the step of adding lignin has a median diameter of 0.1 μm or more and 300 μm or less.
Citation Information
Patent Citations
Method for preparing phenolic foam by enzymatic modification of lignin
CN111234455A
Modified phenolic resin for foaming, foamed material, and preparation method and application of modified phenolic resin for foaming
CN111620991A
Smoke-suppression flame-retardant phenolic carbon foam as well as preparation method and application thereof
CN115636406A
Foamed material based on phenolic resin
JP2014533748A
Lignin compositions
US20180273755A1
Cited By
Phenolic resin foam
JP2026161393A