Multilayer film, vapor-deposited multilayer film, multilayer structure, packaging material, recovery composition, method for recovering multilayer structure, and method for producing multilayer film

The multilayer film structure, featuring EVOH with 20-50 mol% ethylene units and polyvalent metal ions, addresses the challenge of maintaining appearance and gas barrier properties at wider widths by reducing stress and interface disorder, ensuring excellent performance and recyclability.

WO2024225423A1PCT designated stage expired Publication Date: 2024-10-31KURARAY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016391
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Multilayer films with EVOH as the outermost layer face challenges in maintaining excellent appearance characteristics and gas barrier properties, especially when produced with a width of 500 mm or more, due to increased shear stress and residence time, leading to viscosity changes and deterioration.

Method used

A multilayer film structure with an EVOH layer as the outermost layer, containing 20-50 mol% ethylene units and a saponification degree of 90 mol% or more, combined with polyvalent metal ions and an adhesive resin, improves slipperiness and reduces stress at the interface, enhancing appearance and gas barrier properties.

Benefits of technology

The proposed multilayer film achieves excellent appearance characteristics and gas barrier properties while maintaining recyclability, even at wider widths, by reducing stress and interface disorder through the use of polyvalent metal ions and appropriate resin composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a multilayer film that is exceptional in appearance characteristics, gas barrier properties, and recyclability even when a film width is 500 mm or greater. This multilayer film has a layer (X) as an outermost layer and has a configuration in which the layer (X), a layer (Y), and a layer (Z) are laminated adjacently in the stated order, the layer (X) being composed of only a resin composition (A) that contains an EVOH (a1) having an ethylene unit content of 20-50 mol% and a saponification degree of 90 mol% or greater, and polyvalent metal ions (a2), the layer (Y) containing an adhesive resin (B) having a melting point of less than 170°C as a main component, the layer (Z) containing a polyolefin resin (C) having a melting point of less than 170°C as a main component, the resin composition (A) containing 350-2000 ppm of the polyvalent metal ions (a2), the polyvalent metal ions (a2) being at least one selected from the group consisting of magnesium ions, calcium ions, zinc ions, cobalt ions, and manganese ions, and the width of the multilayer film being 500 mm or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer film, vapor-deposited multilayer film, multilayer structure, packaging material, recovered composition, recovery method for multilayer structure, and method for producing multilayer film

[0001] The present invention relates to a multilayer film, a vapor-deposited multilayer film, a multilayer structure, and a packaging material, a recovery composition, and a recovery method using the same.

[0002] Packaging materials for long-term storage of foods and other foods often require gas barrier properties, including oxygen barrier properties. The use of packaging materials with high gas barrier properties can prevent oxidative deterioration of foods and other foods due to oxygen intrusion and the proliferation of microorganisms. Metal foils or metal vapor-deposited layers such as aluminum, and inorganic oxide vapor-deposited layers such as silicon oxide and aluminum oxide are widely used as layers for improving gas barrier properties. Meanwhile, resin layers with gas barrier properties, such as vinyl alcohol polymers and polyvinylidene chloride, are also widely used. Vinyl alcohol polymers exhibit gas barrier properties by crystallizing and densifying due to hydrogen bonding between hydroxyl groups in the molecules. Among these, ethylene-vinyl alcohol copolymers (hereinafter sometimes abbreviated as "EVOH") are suitable for melt molding due to their excellent thermal stability. Therefore, with the development of coextrusion technology, multilayer films with an EVOH layer as an intermediate layer have become widely used as gas barrier packaging materials (Patent Document 1).

[0003] Furthermore, in recent years, driven by environmental and waste issues, there has been a growing global demand for post-consumer recycling (hereinafter sometimes simply referred to as "recycling"), which involves recovering and recycling packaging materials consumed in the market. Recycling typically involves shredding recovered packaging materials, separating and cleaning them as necessary, and then melt-mixing them using an extruder. The pellets obtained in this manner are then used to manufacture various molded products. In this regard, packaging materials are required to be composed of as single a material as possible (mono-materialization), which allows for the production of high-purity, high-quality recycled resins. To this end, there has been an increasing demand for barrier films primarily made of polyolefins, which are widely used as packaging materials. To achieve extremely high gas barrier properties, a vapor-deposited multilayer film has also been proposed (Patent Document 2), in which an inorganic vapor-deposited layer is laminated on the surface of an EVOH layer of a polyolefin-based multilayer film, the outermost layer of which is EVOH.

[0004] International Publication No. 2020 / 071513 International Publication No. 2021 / 261560

[0005] When a multilayer film having an EVOH layer as the outermost layer is produced by melt molding, the EVOH experiences large shear stress with the metal wall surface in the extrusion channel, which can adversely affect the appearance of the resulting multilayer film. Particularly in films with a width of 500 mm or more, the resin at the film edge spends a long time in the extrusion channel, and the EVOH tends to stagnate inside the die, causing viscosity changes and the generation of degraded products, resulting in a significant deterioration of the appearance of the multilayer film.

[0006] In view of these circumstances, a first object of the present invention is to provide a multilayer film that has excellent appearance characteristics, gas barrier properties, and recyclability even when the film width is 500 mm or more, and a method for producing the same. A second object of the present invention is to provide, using the multilayer film, a vapor-deposited multilayer film that has excellent appearance characteristics, gas barrier properties, and recyclability, a multilayer structure, and a packaging material containing the multilayer structure. A third object of the present invention is to provide a recovered composition containing recovered material from the multilayer structure, and a method for recovering the same.

[0007] According to the present invention, the above-mentioned object is achieved by providing a multilayer film having a width of 500 mm or more, wherein: [1] the multilayer film has a constitution in which a layer (X) is an outermost layer, and a layer (X), a layer (Y), and a layer (Z) are laminated adjacent to each other in this order, the layer (X) being a layer made only of a resin composition (A) containing an ethylene-vinyl alcohol copolymer (a1) (hereinafter sometimes abbreviated as "EVOH (a1)") having an ethylene unit content of 20 to 50 mol% and a saponification degree of 90 mol% or more and a polyvalent metal ion (a2), the layer (Y) containing an adhesive resin (B) having a melting point of less than 170°C as a main component, and the layer (Z) containing a polyolefin resin (C) having a melting point of less than 170°C as a main component, the resin composition (A) containing 350 to 2000 ppm of the polyvalent metal ion (a2), the polyvalent metal ion (a2) being at least one selected from the group consisting of magnesium ions, calcium ions, zinc ions, cobalt ions, and manganese ions; [2] The multilayer film of [1], wherein the adhesive resin (B) is acid-modified polyethylene or acid-modified polypropylene; [3] The multilayer film of [1] or [2], wherein the polyolefin resin (C) is polyethylene or polypropylene; [4] Any of the multilayer films of [1] to [3], wherein the resin composition (A) contains 40 ppm or more and 500 ppm or less of alkali metal ions (a3); [5] Any of the multilayer films of [1] to [4], wherein the resin composition (A) contains alkali metal ions (a3) ​​in an amount of 40 ppm or more and 500 ppm or less; [6] Any of the multilayer films of [1] to [5], wherein the resin composition (A) contains alkali metal ions (a3) ​​in an amount of 40 ppm or more and 500 ppm or less; [7] Any of the multilayer films of [1] to [4], wherein the resin composition (A) contains alkali metal ions (a3) ​​in an amount of 40 ppm or more and 500 ppm or less of alkali metal ions (a3); [7] Any of the multilayer films of [1] to [6], in which the weight loss W of the resin composition (A) when maintained at 200°C in a nitrogen atmosphere for 30 minutes in thermogravimetry (TG) is 0.01 to 0.3%; [8] Any of the multilayer films of [1] to [7], which does not have a layer containing, as a main component, a resin having a melting point of 200°C or higher and a metal layer with an average thickness of 1 µm or more; [9] Any of the multilayer films of [1] to [8], in which the average thickness of the layer (X) is 0.2 µm or more and less than 20 µm, and the ratio of the average thickness of the layer (X) to the average thickness of the multilayer film is less than 25%;

[10] Any of the multilayer films [1] to [9], wherein the width of the multilayer film is 1000 mm or more;

[11] Any of the multilayer films [1] to

[10] , wherein the multilayer film is not stretched;

[12] Any of the multilayer films [1] to

[10] , wherein the multilayer film is stretched uniaxially by 3 times or more but less than 12 times;

[13] Any of the multilayer films [1] to

[10] , wherein the multilayer film is stretched biaxially by 3 times or more but less than 12 times;

[14] Any of the multilayer films [1] to

[13] , wherein the ratio of the total average thickness of layers containing polyethylene-based resin or polypropylene-based resin as the main component is 75% or more;

[15] Any of the multilayer films [1] to

[13] , wherein the ratio of the total average thickness of layers containing polyethylene-based resin or polypropylene-based resin as the main component is 75% or more;

[16] Any of the multilayer films [1] to

[16] , wherein the ratio of the total average thickness of layers containing polyethylene-based resin or polypropylene-based resin as the main component is 75% or more;

[17] Any of the multilayer films [1] to

[17] , wherein the ratio of the total average thickness of layers containing polyethylene-based resin or polypropylene-based resin as the main component is 75% or more;

[18] Any of the multilayer films [1] to

[18] , wherein the ratio of the total average thickness of layers containing polyethylene-based resin or polypropylene-based resin as the main component is 75% or more;

[19] Any of the multilayer films

[20] to

[22] , wherein the ratio of the total average thickness of layers containing polyethylene-based resin or polypropylene-based resin as the main component is 75% or more;

[21] Any of the multilayer films

[21] to

[22] , wherein the ratio of the total average thickness of layers containing polyethylene-based resin or polypropylene-based resin as the main Image clarity C measured in accordance with K7374 (2007, transmission method) when the longitudinal direction of the multilayer film is the vertical direction at an optical comb width of 2.0 mm; MD and image clarity C when the width direction is the vertical direction TD are all 60% or more, and the image clarity C measured at the measurement position MD Standard deviation of image clarity C TD

[16] The multilayer film of any one of [1] to

[14] , wherein the standard deviation of each of the values ​​of the image clarity of the multilayer film is 10% or less, when the position of one end in the width direction of the multilayer film is 0% and the position of the other end is 100%, and the image clarity of the multilayer film is measured in accordance with JIS K7374 (2007, transmission method) with the longitudinal direction as the vertical direction, with the image clarity C of the multilayer film at an optical comb width of 2.0 mm, centered at 10%, 50%, and 90% positions. MD and image clarity C when the width direction is the vertical direction TD The ratio of the average values ​​of the MD / Average sharpness C TD

[17] A vapor-deposited multilayer film comprising the multilayer film of any one of [1] to

[16] and an inorganic vapor-deposited layer (I) laminated on the exposed surface side of the layer (X) in the multilayer film;

[18] A vapor-deposited multilayer film of

[17] , wherein the inorganic vapor-deposited layer (I) is a metal vapor-deposited layer containing aluminum as the main component or an inorganic oxide vapor-deposited layer containing alumina or silica as the main component;

[19] A vapor-deposited multilayer film having an oxygen transmission rate of 60 cc / (m) at 20°C and 65% RH as measured in accordance with JIS K7126-2 (2006) 2

[20] A multilayer structure obtained by laminating a multilayer film or a vapor-deposited multilayer film according to any one of [1] to

[19] and at least one resin layer (R) containing a thermoplastic resin (D) as a main component;

[21] The multilayer structure according to

[20] , wherein the thermoplastic resin (D) is polyethylene or polypropylene;

[22] A packaging material having the multilayer structure according to

[20] or

[21] ;

[23] A recovered composition comprising a recovered product of the multilayer structure according to

[20] or

[21] ;

[24] A method for recovering a multilayer structure, comprising a step of crushing the multilayer structure according to

[20] or

[21] and then melt-molding the crushed multilayer structure;

[25] A method for producing a multilayer film according to any one of [1] to

[16] , comprising a step of melt-kneading EVOH (a1) and polyvalent metal ions (a2) to obtain resin composition (A) pellets, and a step of melt-molding the resin composition (A) pellets to form a layer (X); This is achieved by providing

[0008] According to the present invention, a multilayer film having excellent appearance characteristics, gas barrier properties, and recyclability can be provided, even when the width is 500 mm or more. Furthermore, by using this multilayer film, a vapor-deposited multilayer film, a multilayer structure, and a packaging material using the same can be provided, each having excellent appearance characteristics, gas barrier properties, and recyclability. Furthermore, because the multilayer structure has good recyclability, a recovered composition containing recovered material from the multilayer structure and a method for recovering the same can be provided. Here, "appearance characteristics" can be evaluated by visually observing the appearance of the multilayer film, particularly the state of streaks in the multilayer film, and by observing the appearance characteristics using an image clarity measuring device. Specifically, this can be evaluated by the method described in the Examples. Furthermore, in this specification, "recyclability" means that when the recovered material from the multilayer structure or packaging material of the present invention is melt-kneaded to produce a recovered composition, gelation of the resin is suppressed, allowing for the efficient production of a recovered composition with excellent appearance. Specifically, this can be evaluated by the method described in the Examples.

[0009] Hereinafter, embodiments of the present invention will be described. Note that in the following description, specific materials (compounds, etc.) that exhibit specific functions may be exemplified, but the present invention is not limited to embodiments using such materials. Furthermore, the exemplified materials may be used alone or in combination, unless otherwise specified.

[0010] The multilayer film of the present invention has a configuration in which Layer (X) is an outermost layer, and Layer (X), Layer (Y), and Layer (Z) are laminated adjacently in this order, Layer (X) is a layer consisting solely of a resin composition (A) containing EVOH (a1) having an ethylene unit content of 20 to 50 mol% and a saponification degree of 90 mol% or more and polyvalent metal ions (a2), Layer (Y) contains, as a main component, an adhesive resin (B) having a melting point of less than 170°C, Layer (Z) contains, as a main component, a polyolefin resin (C) having a melting point of less than 170°C, Resin composition (A) contains 350 to 2000 ppm of polyvalent metal ions (a2), and the polyvalent metal ions (a2) are at least one selected from the group consisting of magnesium ions, calcium ions, zinc ions, cobalt ions, and manganese ions, and the width is 500 mm or greater.

[0011] EVOH (a1) has excellent gas barrier properties, and the multilayer film of the present invention having layer (X) as the outermost layer can achieve high gas barrier properties. Furthermore, since the EVOH (a1) in the outermost layer has a high affinity with the inorganic vapor-deposited layer (I) described below, the vapor-deposited film of the present invention tends to exhibit stable high gas barrier properties. On the other hand, EVOH (a1) has a high affinity with the metal surface of an extruder or the like, which may be why its appearance is prone to deteriorate during multilayer film production. Particularly, when producing multilayer films with a width of 500 mm or more, the resin residence time in the extrusion flow path at the film edge becomes long, and EVOH (a1) is prone to residence inside the die, causing viscosity changes and the generation of degraded products, resulting in a significant deterioration in the appearance of the multilayer film. It has been difficult to achieve both the production of a multilayer film having EVOH (a1) in the outermost layer and the stable production of a multilayer film with excellent appearance, particularly for multilayer films with a width of 500 mm or more. Therefore, the present inventors have conducted extensive research and have found that, in a resin composition (A) containing EVOH (a1) and polyvalent metal ions (a2), use of a resin composition (A) containing 350 to 2000 ppm of polyvalent metal ions (a2) improves the slipperiness between the metal surface of an extruder or the like and the molten resin during the production of a multilayer film, and reduces unevenness in the thickness of the EVOH layer (layer (X)) and disorder at the layer interface, possibly due to a reduction in the interfacial stress between the EVOH layer (layer (X)) and the adhesive resin layer (layer (Y)), thereby suppressing deterioration in appearance characteristics during production.

[0012] In this specification, "Layer (X), Layer (Y), and Layer (Z) are laminated adjacently in this order" means that adjacent layers are directly laminated. Specifically, it means that Layer (X), Layer (Y), and Layer (Z) are laminated in this order, with Layer (X) and Layer (Y) directly laminated, and Layer (Y) and Layer (Z) directly laminated. "Major component" refers to a component present in an amount of more than 50% by mass. Unless otherwise specified, the "average thickness" of each layer refers to the average thickness measured at any five locations. "ppm" refers to the mass content (ppm by mass). "Polyethylene" refers to ethylene homopolymers, copolymers of 80 mol% or more ethylene and 20 mol% or less α-olefin monomers, and copolymers of 90 mol% or more ethylene and less than 10 mol% non-olefin monomers whose functional groups contain atoms other than carbon, oxygen, and hydrogen atoms. "Polypropylene" refers to a propylene homopolymer, a copolymer of 80 mol% or more propylene and 20 mol% or less α-olefin monomer, and a copolymer of 90 mol% or more propylene and less than 10 mol% non-olefin monomer whose functional groups contain no atoms other than carbon, oxygen, and hydrogen atoms. "Acid-modified polyethylene" refers to a polymer obtained by modifying polyethylene with acid. Acid-modified polyethylene may be a polymer in which at least one of an acidic group and an acid anhydride group has been introduced into polyethylene. "Acid-modified polypropylene" refers to a polymer obtained by modifying polypropylene with acid. Acid-modified polypropylene may be a polymer in which at least one of an acidic group and an acid anhydride group has been introduced into polypropylene. "Polyethylene-based resin" refers to polyethylene and modified polyethylene (such as acid-modified polyethylene). Modified polyethylene refers to a polymer obtained by modifying polyethylene. "Polypropylene-based resin" refers to polypropylene and modified polypropylene (such as acid-modified polypropylene). Modified polypropylene refers to a polymer obtained by modifying polypropylene. Furthermore, the term "surface (or surface layer)" in a multilayer film or a multilayer structure does not refer to the front or back, but refers to the exposed surface. In other words, a multilayer film or a multilayer structure has two surfaces.Similarly, multilayer films and multilayer structures have two outermost layers. In this specification, "consisting essentially of" means that optional components may be included to the extent that they do not affect the effects of the present invention, and "consisting only of" means that optional components other than impurities that are inevitably included are excluded. In this specification, a numerical range described using "to" means that the numerical values ​​before and after "to" are included as the lower and upper limits.

[0013] <Layer (X)> The multilayer film constituting the multilayer film of the present invention has, as its outermost layer, a layer (X) made of a resin composition (A) containing EVOH (a1) having an ethylene unit content of 20 to 50 mol% and a saponification degree of 90 mol% or more and a polyvalent metal ion (a2).

[0014] <EVOH (a1)> EVOH (a1) is typically obtained by saponifying an ethylene-vinyl ester copolymer obtained by polymerizing ethylene and a vinyl ester. The ethylene unit content of EVOH (a1) is 20 to 50 mol%. An ethylene unit content of 20 mol% or more improves the melt moldability of EVOH (a1) and the pulverized product of a multilayer film or multilayer structure containing EVOH (a1). The ethylene unit content is preferably 23 mol% or more, more preferably 26 mol% or more, and may be 29 mol% or more. On the other hand, an ethylene unit content of 50 mol% or less improves the gas barrier properties of the multilayer film of the present invention. The ethylene unit content is preferably 46 mol% or less, more preferably 42 mol% or less, and may be 38 mol% or less. The ethylene unit content is the content (mol%) of ethylene units relative to all monomer units constituting EVOH.

[0015] The saponification degree of EVOH (a1) is 90 mol% or more. The saponification degree means the ratio of the number of vinyl alcohol units to the total number of vinyl alcohol units and vinyl ester units in EVOH (a1). When the saponification degree is 90 mol% or more, the gas barrier property of the multilayer film of the present invention is improved. The saponification degree is preferably 95 mol% or more, more preferably 99 mol% or more, and even more preferably 99.9 mol% or more. The upper limit of the saponification degree of EVOH (a1) may be 100 mol%. The ethylene unit content and saponification degree of EVOH (a1) are 1 It is determined by H-NMR measurement.

[0016] EVOH (a1) may be a mixture of two or more types of EVOH having different ethylene unit contents. In this case, the difference in ethylene unit content between the EVOHs having the most different ethylene unit contents is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 15 mol% or less, and may be 3 mol% or more. Similarly, EVOH (a1) may be a mixture of two or more types of EVOH having different saponification degrees. In this case, the difference in saponification degree between the EVOHs having the most different ethylene unit contents is preferably 7 mol% or less, more preferably 5 mol% or less, and may be 0.5 mol% or more. When it is desired to achieve both thermoformability and gas barrier property at a higher level, it is preferred to use as EVOH (a1) an EVOH (low ethylene) having an ethylene unit content of 24 mol% or more and less than 34 mol% and a degree of saponification of 99 mol% or more and an EVOH (high ethylene) having an ethylene unit content of 34 mol% or more and less than 50 mol% and a degree of saponification of 99 mol% or more mixed in a blending mass ratio (low ethylene / high ethylene) of 60 / 40 to 90 / 10.

[0017] The EVOH (a1) may be an EVOH (a'1) having a melting point of less than 150°C. The melting point of the EVOH (a'1) is less than 150°C, which may improve the appearance and interlayer adhesion of a multilayer film having a layer (X) mainly composed of EVOH (a'1) as the outermost layer. This is thought to be because the melting point of the EVOH (a'1) is less than 150°C, which improves the fluidity of polymer chains. This allows effective stress relaxation even at relatively low temperatures during melt molding or secondary processing such as stretching, and maintains adhesive reaction activity with adjacent layers. From the viewpoint of making the effects of the present invention more pronounced, the melting point of the EVOH (a'1) is preferably less than 140°C, more preferably less than 130°C, and may be less than 125°C or less than 120°C. On the other hand, from the viewpoint of processability during melt molding and secondary processing such as stretching, and from the viewpoint of heat resistance as a packaging material, the melting point of EVOH (a'1) is preferably 80°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher. The melting point of EVOH (a'1) can be controlled by the following measures alone or in combination, and in the present invention, the following method (3) can be preferably exemplified: (1) Changing the ethylene unit content (increasing the ethylene unit content decreases the melting point). (2) Changing the degree of saponification (decreasing the degree of saponification decreases the melting point). (3) Introducing a modifying group containing a primary hydroxyl group (introducing a modifying group containing a primary hydroxyl group decreases the melting point).

[0018] The primary hydroxyl group-containing modifying group used in (3) above is preferably a primary hydroxyl group-containing modifying group represented by the following general formula (I). The degree of melting point reduction per introduction rate of the modifying group varies depending on the structure of the primary hydroxyl group-containing modifying group introduced. However, the introduction of 1 mol % of the primary hydroxyl group-containing modifying group represented by the following general formula (I) generally reduces the melting point by approximately 6 to 9°C. Controlling the melting point in this manner can lower the melting point while relatively maintaining gas barrier properties and thermal stability. Furthermore, deterioration in interlayer adhesion with the layer (Y) and inorganic vapor deposition layer (I), described below, is also suppressed, resulting in a multilayer film with particularly excellent quality and performance. This is thought to be due to the fact that the melting point can be lowered while maintaining the hydroxyl group content, and the primary hydroxyl group has high adhesive reactivity with the layer (Y) and inorganic vapor deposition layer (I), described below. The content of the modifying group containing a primary hydroxyl group in EVOH (a'1) may be adjusted as appropriate, taking into consideration the balance between the melting point and various physical properties; however, a content of 2 mol % or more and less than 20 mol % often results in a good balance of physical properties. The lower limit of the content of the modifying group containing a primary hydroxyl group in EVOH (a'1) is more preferably 3 mol %. On the other hand, the upper limit of the content of the modifying group containing a primary hydroxyl group in EVOH (a'1) is more preferably 10 mol %, and even more preferably 8 mol %. The modifying group containing a primary hydroxyl group can be introduced by copolymerization or a polymer reaction. The "content of the modifying group containing a primary hydroxyl group in EVOH (a'1)" may be the content (mol %) of the monomer unit containing a primary hydroxyl group relative to all the monomer units constituting EVOH (a'1).

[0019] [wherein X is a hydrogen atom, a methyl group, or R 2 represents a group represented by —OH. 1 and R 2 each independently represents a single bond, an alkylene group having 1 to 9 carbon atoms, or an alkyleneoxy group having 1 to 9 carbon atoms, and the alkylene group and the alkyleneoxy group may contain a hydroxyl group, an alkoxy group, or a halogen atom.]

[0020] In general formula (I), X is preferably a hydrogen atom or R 2 R is a group represented by —OH, and more preferably a hydrogen atom. 1is preferably a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkyleneoxy group having 1 to 5 carbon atoms, and more preferably a methylmethyleneoxy group (—O—C(CH 3 )H)-). R 1 When is an alkyleneoxy group, the oxygen atom of the alkyleneoxy group is usually bonded to a carbon atom of the main chain.

[0021] EVOH (a1) may contain other monomer units other than ethylene units, vinyl ester units, vinyl alcohol units, and the modifying group containing a primary hydroxyl group, as long as the effects of the present invention are not impaired. The content of other monomer units is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably substantially none. Examples of such other monomers include α-olefins such as propylene, n-butene, isobutylene, and 1-hexene; acrylic acid and its salts; unsaturated monomers having an acrylic ester group; methacrylic acid and its salts; unsaturated monomers having a methacrylic ester group; acrylamide, N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, acrylamidopropanesulfonic acid and its salts, acrylamidopropyldimethylamine and its salts (e.g., quaternary salts); methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, methacrylamidopropanesulfonic acid and its salts, methacrylamidopropyldimethylamine and its salts (e.g., quaternary salts); methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether vinyl halides such as vinyl chloride and vinyl fluoride; vinylidene halides such as vinylidene chloride and vinylidene fluoride; allyl compounds such as allyl acetate, 2,3-diacetoxy-1-allyloxypropane and allyl chloride; unsaturated dicarboxylic acids and salts or esters thereof such as maleic acid, itaconic acid and fumaric acid; vinylsilane compounds such as vinyltrimethoxysilane; isopropenyl acetate, 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane and 1,3-dibutyronyloxy-2-methylenepropane.

[0022] The EVOH (a1) may be post-modified by a technique such as urethanization, acetalization, cyanoethylation, or oxyalkylenation.

[0023] The MFR (190°C, under a load of 2.16 kg) of EVOH (a1), measured in accordance with JIS K7210 (2014), is preferably 0.2 to 20 g / 10 min. The MFR of EVOH (a1) is more preferably 0.5 g / 10 min or more, and even more preferably 0.8 g / 10 min or more. On the other hand, the MFR of EVOH (a1) is more preferably 15 g / 10 min or less, even more preferably 10 g / 10 min or less, even more preferably 5 g / 10 min or less, and particularly preferably 3 g / 10 min or less. When the MFR of EVOH (a1) is within the above range, the melt moldability of EVOH (a1) and pulverized products of multilayer films and multilayer structures containing EVOH (a1) is improved.

[0024] <Polyvalent Metal Ion (a2)> The content of polyvalent metal ion (a2) contained in the resin composition (A) is 350 ppm or more and 2000 ppm or less. If the content of polyvalent metal ion (a2) is less than 350 ppm, the stress that layer (X) receives from the wall surface of the extrusion channel and the stress acting between layer (X) and layer (Y) during molding of the multilayer structure increase, resulting in a deterioration in the appearance of the multilayer film. The content of polyvalent metal ion (a2) is more preferably 380 ppm or more, even more preferably 450 ppm or more, particularly preferably 550 ppm or more, and may even be 650 ppm or more. On the other hand, if the content of polyvalent metal ion (a2) exceeds 2000 ppm, the viscosity decreases significantly when melt-kneaded for a long time, which may result in a deterioration in stable moldability or insufficient interlayer adhesion between layer (X) and layer (Y). The content of the polyvalent metal ion (a2) is more preferably 1500 ppm or less, and even more preferably 1250 ppm or less.

[0025] The polyvalent metal ion (a2) is at least one selected from the group consisting of magnesium ions, calcium ions, zinc ions, cobalt ions, and manganese ions. By including the polyvalent metal ion (a2) in the resin composition (A), the appearance characteristics of the multilayer film are improved, and the viscosity stability during melt molding is excellent. From the viewpoint of the reduced occurrence of discoloration in the resulting multilayer structure, magnesium ions, calcium ions, and zinc ions are more preferred as the polyvalent metal ion (a2), and from the viewpoint of the appearance of the resulting multilayer structure, calcium ions and magnesium ions are even more preferred, with calcium ions being particularly preferred.

[0026] Examples of polyvalent metal compounds that provide the polyvalent metal ions (a2) include aliphatic carboxylates, aromatic carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, hydroxides, metal complexes, etc. Among these, aliphatic carboxylates and hydroxides are more preferred because they are easily available and easy to handle, and aliphatic carboxylates are even more preferred because they easily maintain the viscosity stability of the resin composition (A). Preferred aliphatic carboxylates are acetates, caprylates, and stearates.

[0027] <Alkali Metal Ions (a3)> The resin composition (A) preferably contains 40 to 500 ppm of alkali metal ions (a3). When the resin composition (A) contains alkali metal ions (a3) ​​in the above range, the interlayer adhesion with the layer (Y), which will be described later, tends to be significantly improved. When the alkali metal ions (a3) ​​are 40 ppm or more, the recyclability tends to be improved. On the other hand, when the content of alkali metal ions (b) is 500 ppm or less, the recyclability and the hue of the recovered composition tend to be improved. The lower limit of the content of alkali metal ions (a3) ​​is more preferably 80 ppm, and even more preferably 120 ppm. The upper limit of the content of alkali metal ions (a3) ​​is more preferably 400 ppm, and even more preferably 300 ppm. Furthermore, by controlling the content ratio of the alkali metal ions (a3) ​​to the carboxylic acid, which will be described later, the melt moldability and color resistance of the resulting resin composition can be further improved.

[0028] Examples of the alkali metal ion (a3) ​​include ions of lithium, sodium, potassium, rubidium, cesium, etc., but sodium or potassium ions are preferred from the viewpoint of industrial availability. These ions may be used alone or in combination of two or more.

[0029] Examples of alkali metal compounds that provide the alkali metal ions (a3) ​​include aliphatic carboxylates, aromatic carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, hydroxides, and metal complexes of alkali metals. Among these, aliphatic carboxylates and phosphates are more preferred because of their ease of availability and handling. Preferred aliphatic carboxylates are acetates, caprylates, and stearates.

[0030] <Higher Aliphatic Carboxylic Acid (a4)> The resin composition (A) preferably contains 100 to 4,000 ppm of a higher aliphatic carboxylic acid (a4) having 8 to 30 carbon atoms. The higher aliphatic carboxylic acid (a4) may be contained in part or in whole in the form of a salt, or as a salt of a polyvalent metal ion (a2) or an alkali metal ion (a3). The higher aliphatic carboxylic acid (a4) is preferably caprylic acid or stearic acid. The multilayer film of the present invention has a layer (X) made of the resin composition (A) as the outermost layer. It is believed that the higher aliphatic carboxylic acid (a4) acts as a lubricant for the die metal surface in the die, thereby suppressing poor appearance due to uneven thickness of the multilayer film and the occurrence of gels and bumps due to retained resin. For this reason, the resin composition (A) preferably contains 100 ppm or more of the higher aliphatic carboxylic acid (a4). On the other hand, if the content of the higher aliphatic carboxylic acid (a4) is 4000 ppm or less, thickening of the resin composition (A) during melt molding tends to be suppressed and interlayer adhesion with the layer (Y) described below tends to be maintained. From these viewpoints, the content of the higher aliphatic carboxylic acid (a4) is more preferably 200 to 3000 ppm, and even more preferably 300 to 2500 ppm.

[0031] The resin composition (A) may contain other components in addition to the EVOH (a1), polyvalent metal ions (a2), alkali metal ions (a3), and higher aliphatic carboxylic acids (a4), as long as the effects of the present invention are not impaired. Examples of other components include alkaline earth metal ions and transition metal ions other than the polyvalent metal ions (a2), carboxylic acids (monocarboxylic acids, polycarboxylic acids) other than the higher aliphatic carboxylic acids (a4), thermoplastic resins other than the EVOH (a1), phosphoric acid compounds, boron compounds, antioxidants (hindered phenol compounds, etc.), plasticizers, heat stabilizers (melt stabilizers), photoinitiators, deodorizers, UV absorbers, antistatic agents, lubricants, colorants, fillers, desiccants, bulking agents, pigments, dyes, processing aids, flame retardants, and antifogging agents. From the viewpoint of suppressing coloration during melt molding of the pulverized multilayer structure containing the resin composition (A), it is preferable to contain a carboxylic acid and / or a phosphoric acid compound. Furthermore, by including a boron compound, the melt viscosity of the resin composition (A) and the pulverized product of the multilayer structure containing the resin composition (A) can be controlled.

[0032] <Carboxylic Acid> The resin composition (A) preferably contains a carboxylic acid other than the higher aliphatic carboxylic acid (a4). The lower limit of the carboxylic acid content is preferably 50 ppm, more preferably 100 ppm. On the other hand, the upper limit of the carboxylic acid content is preferably 400 ppm, more preferably 350 ppm. When the carboxylic acid content is 50 ppm or more, the coloring resistance tends to be improved. On the other hand, when the carboxylic acid content is 400 ppm or less, the interlayer adhesion tends to be maintained and the generation of odor tends to be suppressed.

[0033] The pKa of the carboxylic acid is preferably 3.5 to 5.5. When the pKa of the carboxylic acid is within this range, the pH buffering ability of the resulting resin composition (A) is enhanced, further improving the melt moldability and further improving the coloration caused by acidic or basic substances.

[0034] The carboxylic acid may be a monocarboxylic acid. These may be used alone or in combination of two or more. A monocarboxylic acid is a compound having one carboxyl group in the molecule. Monocarboxylic acids having a pKa in the range of 3.5 to 5.5 are not particularly limited, and examples thereof include formic acid (pKa = 3.77), acetic acid (pKa = 4.76), propionic acid (pKa = 4.85), and acrylic acid (pKa = 4.25). These carboxylic acids may further have a substituent such as a hydroxyl group, an amino group, or a halogen atom. Among these, acetic acid is preferred because of its high safety and ease of availability and handling.

[0035] The carboxylic acid may be a polycarboxylic acid. When the carboxylic acid is a polycarboxylic acid, the discoloration resistance of the resin composition (A) at high temperatures and the discoloration resistance of the melt-molded product of the crushed material of the resulting multilayer structure may be further improved. It is also preferable that the polycarboxylic acid compound has three or more carboxyl groups. In this case, discoloration resistance may be more effectively improved. The polycarboxylic acid is a compound having two or more carboxyl groups in the molecule. In this case, it is preferable that the pKa of at least one carboxyl group is in the range of 3.5 to 5.5, and examples thereof include oxalic acid (pKa2=4.27), succinic acid (pKa1=4.20), fumaric acid (pKa2=4.44), malic acid (pKa2=5.13), glutaric acid (pKa1=4.30, pKa2=5.40), adipic acid (pKa1=4.43, pKa2=5.50), and the like. 2=5.41), pimelic acid (pKa1=4.71), phthalic acid (pKa2=5.41), isophthalic acid (pKa2=4.46), terephthalic acid (pKa1=3.51, pKa2=4.82), citric acid (pKa2=4.75), tartaric acid (pKa2=4.40), glutamic acid (pKa2=4.07), aspartic acid (pKa=3.90), etc.

[0036] <Phosphate Compound> The resin composition (A) may further contain a phosphate compound. The lower limit of the content of the phosphate compound is preferably 5 ppm in terms of phosphate radicals. On the other hand, the upper limit of the content of the phosphate compound is preferably 100 ppm in terms of phosphate radicals. By containing the phosphate compound in this range, coloration of the resulting resin composition (A) and a melt-molded product of the pulverized product of the resulting multilayer structure may be suppressed, and thermal stability may be improved.

[0037] As the phosphate compound, various acids such as phosphoric acid and phosphorous acid and their salts can be used. The phosphate may be any of primary phosphate, secondary phosphate, and tertiary phosphate. The cation species of the phosphate is not particularly limited, but the cation species is preferably an alkali metal or alkaline earth metal. Among them, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate are preferred as the phosphate compound.

[0038] <Boron Compound> The resin composition (A) may further contain a boron compound. When a boron compound is contained, the lower limit of the content in the resin composition (A) is preferably 50 ppm, more preferably 100 ppm, in terms of elemental boron. On the other hand, the upper limit of the content of the boron compound in the resin composition (A) is preferably 400 ppm, more preferably 200 ppm, in terms of elemental boron. By containing the boron compound within this range, the thermal stability of the resin composition (A) and the pulverized product of the resulting multilayer structure during melt molding may be improved, and the occurrence of gels and lumps may be suppressed. In addition, the drawdown resistance and neck-in resistance during film formation may be improved, and the mechanical properties of the resulting molded product may be improved. These effects are presumed to be due to the occurrence of a chelating interaction between the EVOH (a1) and the boron compound.

[0039] Examples of boron compounds include boric acid, boric acid esters, borate salts, and boron hydrides. 3 BO 3boric acid such as tetraboric acid, metaboric acid, and the like; boric acid esters such as trimethyl borate and triethyl borate; alkali metal salts or alkaline earth metal salts of the above boric acid; and boric acid salts such as borax. Of these, orthoboric acid is preferred.

[0040] <Hindered phenol compound> The resin composition (A) may further contain a hindered phenol compound as an antioxidant. When a hindered phenol compound is contained, the content of the hindered phenol compound in the resin composition (A) is preferably 1,000 to 10,000 ppm. When the content is 1,000 ppm or more, coloration, thickening, and gelation of the resin can be suppressed when the pulverized product of the multilayer structure is melt-molded. The content of the hindered phenol compound is more preferably 2,000 ppm or more. On the other hand, when the content of the hindered phenol compound is 10,000 ppm or less, coloration and bleed-out resulting from the hindered phenol compound can be suppressed. The content of the hindered phenol compound is more preferably 8,000 ppm or less.

[0041] The hindered phenol compound has at least one hindered phenol group. A hindered phenol group is a group in which a bulky substituent is bonded to at least one carbon atom adjacent to the carbon atom to which the hydroxyl group of a phenol is bonded. The bulky substituent is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably a t-butyl group.

[0042] The hindered phenol compound is preferably in a solid state at around room temperature. From the viewpoint of suppressing bleed-out of the compound, the melting point or softening temperature of the hindered phenol compound is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. From the same viewpoint, the molecular weight of the hindered phenol compound is preferably 200 or higher, more preferably 400 or higher, and even more preferably 600 or higher. Meanwhile, the molecular weight is usually 2000 or lower. Furthermore, from the viewpoint of facilitating mixing with EVOH (a1), the melting point or softening temperature of the hindered phenol compound is preferably 200°C or lower, more preferably 190°C or lower, and even more preferably 180°C or lower.

[0043] The hindered phenol compound preferably has an ester bond or an amide bond. Examples of the hindered phenol compound having an ester bond include esters of aliphatic carboxylic acids having a hindered phenol group and aliphatic alcohols, and examples of the hindered phenol compound having an amide bond include amides of aliphatic carboxylic acids having a hindered phenol group and aliphatic amines. Among these, it is preferable that the hindered phenol compound has an amide bond.

[0044] Specific structures of hindered phenol compounds having an ester bond or an amide bond include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available from BASF as Irganox 1010, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate commercially available from Irganox 1076, 2,2'-thiodiethylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available from Irganox 1035, and 2,2'-thiodiethylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available from Irganox 1135. Examples of such an acid include octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanoate, which is commercially available; ethylene bis(oxyethylene)(3-tert-butyl-4-hydroxy-5-methylbenzenepropanoate), which is commercially available as Irganox 245; 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], which is commercially available as Irganox 259; and N,N'-hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide], which is commercially available as Irganox 1098. Among these, N,N'-hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide] commercially available as Irganox 1098 and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available as Irganox 1010 are preferred, with the former being more preferred.

[0045] The resin composition (A) may further contain a thermoplastic resin other than EVOH (a1). Examples of the thermoplastic resin other than EVOH (a1) include various polyolefins (polyethylene, polypropylene, poly(1-butene), poly(4-methyl-1-pentene), ethylene-propylene copolymers, copolymers of ethylene and an α-olefin having 4 or more carbon atoms, copolymers of polyolefins and maleic anhydride, ethylene-vinyl ester copolymers, ethylene-acrylic acid ester copolymers, and modified polyolefins obtained by graft-modifying these with unsaturated carboxylic acids or derivatives thereof), various polyamides (nylon 6, nylon 6,6, nylon 6 / 66 copolymer, nylon 11, nylon 12, polymetaxylylene adipamide, etc.), various polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyvinyl chloride, polyvinylidene chloride, polystyrene, polyacrylonitrile, polyurethane, polycarbonate, polyacetal, polyacrylate, and modified polyvinyl alcohol resins. The content of the thermoplastic resin in the resin composition (A) is usually less than 40% by mass, preferably less than 30% by mass, more preferably less than 20% by mass, even more preferably less than 10% by mass, and may be less than 5% by mass or even less than 1% by mass, and it is particularly preferable that the resin composition (A) is substantially free of the thermoplastic resin.

[0046] The proportion of EVOH (a1) in the resin constituting resin composition (A) is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, from the viewpoint of more significantly achieving the effects of the present invention. The resin constituting resin composition (A) may be essentially EVOH (a1) alone, or the resin constituting resin composition (A) may consist solely of EVOH (a1). Furthermore, the proportion of EVOH (a1) in resin composition (A) is usually more than 50% by mass. From the viewpoint of more significantly achieving the effects of the present invention, the proportion of EVOH (a1) in resin composition (A) is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and may be 98% by mass or more or 99% by mass or more. The resin composition (A) may consist essentially of the EVOH (a1) and the polyvalent metal ion (a2).

[0047] In thermogravimetry (TG), the resin composition (A) preferably exhibits a weight loss W of 0.01 to 0.3% when maintained at 200°C in a nitrogen atmosphere for 30 minutes. This reflects the low-molecular-weight components inherent in the resin composition (A) and the thermal decomposition characteristics of the EVOH (a1). When the layer (X) is made of a resin composition (A) that satisfies the specific TG conditions, a multilayer film with excellent appearance properties can be stably produced over an extended period of time. From the viewpoint of stably producing a multilayer film with even more excellent appearance properties, the weight loss W when maintained at 200°C in a nitrogen atmosphere for 30 minutes is preferably 0.02 to 0.15%, more preferably 0.03 to 0.10%, and even more preferably 0.04 to 0.08%. W1 can be controlled by the ethylene unit content and degree of saponification of EVOH (a1), the types and contents of polyvalent metal ions (a2), alkali metal ions (a3), higher aliphatic carboxylic acids (a4) and other components, and the production conditions (particularly thermal history such as temperature and time) when producing resin composition (A). For example, when producing resin composition (A) by melt-kneading, the weight loss W tends to be small by performing melt-kneading while removing gas components using a vent device or the like.

[0048] Resin composition (A) preferably satisfies the following formula (a), where S (mol %) is the ethylene unit content of EVOH (a1) and T (ppm) is the amount of polyvalent metal ions (a2): -4.17S + 560≦T≦-29.2S + 2600 (I) When T is equal to or greater than the lower limit of formula (a), the appearance characteristics of the multilayer film tend to be improved, and viscosity stability during melt molding tends to be excellent. Furthermore, when T is equal to or less than the upper limit of formula (a), the interlayer adhesion between layer (X) and layer (Y) tends to be excellent. The lower limit of formula (a) is more preferably -6.26S + 760, and even more preferably -8.33S + 920. Furthermore, the upper limit of formula (a) is more preferably -19.4S + 1920, and even more preferably -16.7S + 1580. The formula (a) means that the more suitable content of the polyvalent metal ion (a2) varies depending on the ethylene unit content of the EVOH (a1).

[0049] The method for producing the resin composition (A) is not particularly limited, but it can be produced by melt-kneading EVOH (a1) and polyvalent metal ions (a2), and, if necessary, other components such as alkali metal ions (a3) ​​and higher aliphatic carboxylic acids (a4). Each component may be blended as a solid, such as a powder, or as a melt. They may also be blended as solutes in a solution or dispersoids in a dispersion. An aqueous solution and an aqueous dispersion are preferred as the solution and dispersion, respectively. For melt-kneading, known mixing or kneading devices such as a kneader-ruder, extruder, mixing roll, or Banbury mixer can be used. The temperature range during melt-kneading can be adjusted appropriately depending on the EVOH (a1) used and the melting points of each component, and is typically 150 to 250°C. Alternatively, the resin composition (A) may be produced by adding some components to EVOH (a1) in advance and then melt-kneading the additional components as described above. An example of a method for pre-adding some components to EVOH (a1) is a method in which EVOH (a1) is immersed in the form of pellets or powder in a solution in which the added components are dissolved. An aqueous solution is preferred as the solution. From the viewpoint of the appearance properties of the multilayer film, it is particularly preferred to include a step of melt-kneading EVOH (a1) and polyvalent metal ions (a2) to obtain pellets of the resin composition (A). Furthermore, it is preferred that the layer (X) be a layer obtained by melt-molding pellets consisting of only the resin composition (A).

[0050] <Layer (Y)> The multilayer film of the present invention has a layer (Y) containing, as a main component, an adhesive resin (B) having a melting point of less than 170°C. The inclusion of layer (Y) in the multilayer film of the present invention tends to result in a multilayer film with excellent appearance and interlayer adhesion. Furthermore, the inclusion of layer (Y) improves the compatibility between layer (X) and layer (Z) during recycling, thereby tending to improve recyclability. Examples of adhesive resin (B) include acid-modified polyolefins obtained by treating a polyolefin with an acid. More specifically, examples include acid-modified polyolefin resins obtained by graft polymerizing an unsaturated carboxylic acid such as maleic anhydride or a derivative thereof onto a polyolefin resin. The melting point of adhesive resin (B) mainly depends on the polyolefin resin before acid modification. Regarding the polyolefin resin, the description of the unmodified polyolefin resin (C) described below can be applied as is. However, adhesive resin (B) is preferably acid-modified polyethylene or acid-modified polypropylene. The acid-modified polyolefin resin may be a carboxylic acid-modified polyolefin resin. The acid-modified polyethylene may be a carboxylic acid-modified polyethylene, and the acid-modified polypropylene may be a carboxylic acid-modified polypropylene.

[0051] The proportion of the acid-modified polyolefin resin in the adhesive resin (B) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and the layer (Y) may be substantially composed of the acid-modified polyolefin resin alone, or may be composed of the acid-modified polyolefin resin alone. The proportion of the adhesive resin (B) in the layer (Y) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and the layer (Y) may be substantially composed of the adhesive resin (B) alone, or may be composed of the adhesive resin (B) alone.

[0052] <Layer (Z)> The multilayer film of the present invention has a layer (Z) containing, as a main component, a polyolefin resin (C) having a melting point of less than 170° C. The polyolefin resin (C) is not particularly limited as long as it is a polyolefin having a melting point of less than 170° C. Examples of the polyolefin resin (C) include polyethylene resins such as linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, and high-density polyethylene; polypropylene resins such as homopolypropylene, random polypropylene, and block polypropylene; vinyl ester resins; ethylene-propylene copolymers; propylene-α-olefin copolymers (α-olefins having 4 to 20 carbon atoms); olefin homopolymers or copolymers thereof such as polybutene and polypentene; and chlorinated polyethylene.

[0053] The lower limit of the content of olefin units relative to all monomer units in the polyolefin resin (C) is preferably 60 mol%, more preferably 70 mol%, even more preferably 80 mol%, even more preferably 90 mol%, and may be 95 mol%, 98 mol%, 99 mol%, or 99.9 mol%. The upper limit of the content of olefin units relative to all monomer units in the polyolefin resin (C) may be 100 mol%. The polyolefin resin (C) may be modified, such as by acid modification, or may be unmodified, but is preferably unmodified.

[0054] From the viewpoint of improving the recyclability of a multilayer structure containing polyolefin resin (C), the polyolefin resin (C) preferably contains a polyethylene-based resin or a polypropylene-based resin as a main component, more preferably polyethylene or polypropylene, and even more preferably polyethylene. Polyethylene-based resins and polypropylene-based resins are widely used in packaging materials regardless of whether they have gas barrier properties, and therefore recycling infrastructures for them have been widely established in various countries. When polyolefin resin (C) contains polyethylene as a main component, the polyethylene is preferably at least one selected from linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, and high-density polyethylene, and more preferably at least one selected from linear low-density polyethylene and low-density polyethylene, or a mixture of at least one selected from linear low-density polyethylene and low-density polyethylene with high-density polyethylene.

[0055] From the viewpoint of making the effects of the present invention more pronounced, the melting point of the polyolefin resin (C) is preferably less than 160 ° C, more preferably less than 150 ° C, and may be less than 140 ° C or less than 130 ° C. On the other hand, from the viewpoint of processability during secondary processing such as melt molding and stretching, and from the viewpoint of heat resistance as a packaging material, the melting point of the polyolefin resin (C) is preferably 80 ° C or higher, more preferably 90 ° C or higher. Furthermore, from the viewpoint of improving melt moldability, the melt flow rate (MFR) (190 ° C, under a load of 2160 g) of the polyolefin resin (C) measured in accordance with the method described in JIS K7210 (2014) is preferably 0.1 to 30 g / 10 min, more preferably 0.3 to 25 g / 10 min, and even more preferably 0.5 to 20 g / 10 min.

[0056] When the polyolefin resin (C) contains a polyethylene resin or a polypropylene resin as a main component, the content of the polyethylene resin or the polypropylene resin in the polyolefin resin (C) is more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 95% by mass or more, and the polyolefin resin (C) may be essentially composed of a polyethylene resin or a polypropylene resin alone, or the polyolefin resin (C) may be composed of a polyethylene resin or a polypropylene resin alone. Furthermore, the proportion of the polyolefin resin (C) in the layer (Z) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and the layer (Z) may be essentially composed of a polyolefin resin (C) alone, or the layer (Z) may be composed of a polyolefin resin (C) alone.

[0057] Layer (Y) and layer (Z) contain adhesive resin (B) and polyolefin resin (C) as main components, respectively, but these layers may also contain other components such as antioxidants, plasticizers, heat stabilizers (melt stabilizers), photoinitiators, deodorizers, UV absorbers, antistatic agents, lubricants, colorants, fillers, desiccants, bulking agents, pigments, dyes, processing aids, flame retardants, and antifogging agents, as long as the effects of the present invention are not impaired. However, the total amount of these components is less than 50% by mass of each layer, preferably less than 40% by mass, more preferably less than 30% by mass, even more preferably less than 20% by mass, and particularly preferably less than 10% by mass, and may be less than 5% by mass, less than 3% by mass, or less than 1% by mass.

[0058] <Multilayer Film> The multilayer film of the present invention has a layer (X) as the outermost layer, and has a configuration in which at least layer (X), layer (Y), and layer (Z) are laminated adjacently in this order. The multilayer film may have a plurality of layers each of layer (X), layer (Y), and layer (Z). When there are a plurality of layers (X), it is sufficient that at least one layer (X) is located as the outermost layer. In other words, when there are a plurality of layers (X), it is also possible that there is a layer (X) that is not located as the outermost layer. Furthermore, when there are a plurality of layers of at least one of layers (X), layer (Y), and layer (Z), there may be a layer that does not constitute the laminate structure of layers (X), layer (Y), and layer (Z). In other words, it is sufficient that the multilayer film has a laminate structure of at least one set of layers (X), layer (Y), and layer (Z).

[0059] The multilayer film of the present invention may have layers other than the layer (X), the layer (Y), and the layer (Z). However, as one embodiment of the present invention, the multilayer film of the present invention may not have layers other than the layer (X), the layer (Y), and the layer (Z).

[0060] The layer structure of the multilayer film of the present invention may be X / Y / Z, X / Y / Z / Y / X, X / Y / Z / Y / X / Y / Z, X / Y / Z / Y / X / Y / Z, X / Y / Z / Y / X / Y / Z / Y / X / Y / Z / Y / X, etc., where X represents layer (X), Y represents layer (Y), and Z represents layer (Z), and " / " indicates that the layers are directly laminated.

[0061] From the viewpoints of gas barrier properties, recyclability, and economy, the average thickness of layer (X) in the multilayer film is preferably 0.2 μm or more and less than 20 μm. It is also preferable that the ratio of the average thickness of layer (X) to the average thickness of the multilayer film is less than 25%. The average thickness of layer (X) is more preferably 0.4 μm or more and less than 16 μm, and even more preferably 0.6 μm or more and less than 12 μm. The ratio of the average thickness of layer (X) to the average thickness of the multilayer film is more preferably less than 20%, and even more preferably less than 15%. The ratio of the average thickness of layer (X) to the total average thickness of the multilayer film may be 1% or more. When multiple layers (X) are present, the average thickness of layer (X) is the sum of the average thicknesses of the layers (X). The average thickness of the multilayer film is equal to the sum of the average thicknesses of each layer of the multilayer film.

[0062] From the viewpoints of interlayer adhesion, recyclability, and economy, the average thickness of layer (Y) in the multilayer film is preferably 0.2 μm or more and less than 20 μm. It is also preferable that the ratio of the average thickness of layer (Y) to the average thickness of the multilayer film is less than 25%. The average thickness of layer (Y) is more preferably 0.4 μm or more and less than 16 μm, and even more preferably 0.6 μm or more and less than 12 μm. The ratio of the average thickness of layer (Y) to the average thickness of the multilayer film is more preferably less than 20%, and even more preferably less than 15%. The ratio of the average thickness of layer (Y) to the average thickness of the multilayer film may be 1% or more. When a plurality of layers (Y) are present, the average thickness of layer (Y) is the sum of the average thicknesses of the layers (Y).

[0063] From the viewpoint of recyclability, the average thickness of the layer (Z) in the multilayer film is preferably 1 μm or more and less than 200 μm. It is also preferable that the ratio of the average thickness of the layer (Z) to the average thickness of the multilayer film is more than 55%. The average thickness of the layer (Z) is more preferably 5 μm or more, even more preferably 10 μm or more, and may be 20 μm or more. The average thickness of the layer (Z) is more preferably 100 μm or less, and may be 50 μm or less. The ratio of the average thickness of the layer (Z) to the average thickness of the multilayer film is more preferably more than 60%, even more preferably more than 70%. The ratio of the average thickness of the layer (Z) to the average thickness of the multilayer film may be 98% or less. When a plurality of layers (Z) are present, the average thickness of the layer (Z) is the sum of the average thicknesses of the layers (Y).

[0064] The average thickness of the multilayer film is usually from 10 μm to less than 200 μm, preferably from 10 μm to less than 150 μm. In the case of a stretched multilayer film described below, the average thickness of the stretched multilayer film is preferably from 10 μm to less than 50 μm, more preferably from 10 μm to less than 40 μm.

[0065] The multilayer film may be an unstretched multilayer film, or may be a stretched multilayer film stretched uniaxially or biaxially (at least uniaxially). An unstretched multilayer film refers to a multilayer film that has not been stretched, but slight orientation during film formation (e.g., orientation as if stretched 1.01 times) is considered to be unstretched. Furthermore, a uniaxially stretched multilayer film that has been stretched only uniaxially is considered to be uniaxially stretched, ignoring slight orientation in other axial directions during film formation (e.g., orientation as if stretched 1.01 times). Unstretched multilayer films have excellent impact resistance and can be suitably used as heat-sealable films. On the other hand, uniaxial or biaxial stretching can improve the mechanical properties and gas barrier properties of the resulting multilayer film. From the viewpoint of economy and ease of tearing the multilayer film (making it easy to open the packaging material when used as a packaging material), the multilayer film is preferably a uniaxially stretched multilayer film. From the viewpoint of obtaining a film with little anisotropy in mechanical properties and a strong film, the multilayer film is preferably a biaxially stretched multilayer film. From the viewpoint of thickness uniformity and mechanical strength of the resulting multilayer film, the multilayer film is preferably stretched at least 3 times but less than 12 times in one axial direction. In the case of a uniaxially stretched multilayer film, it is preferably stretched 3 times or more but less than 12 times in one axial direction, and more preferably stretched 4 times or more but less than 10 times. Furthermore, in the case of a uniaxially stretched multilayer film, the stretching axis is preferably in the machine direction (longitudinal direction, MD direction) or a direction perpendicular to the machine direction, i.e., the width direction (TD direction), and more preferably in the longitudinal direction (MD direction). In the case of a biaxially stretched multilayer film, it is preferably stretched 3 times or more but less than 12 times in each of the two axial directions, and more preferably stretched 4 times or more but less than 10 times.

[0066] The lower limit of the ratio of the total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin in the multilayer film of the present invention (the ratio of the total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin to the average thickness of the multilayer film) is preferably 75%, more preferably 80%, even more preferably 85%, and even more preferably 88%. Increasing the ratio of the total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin in the multilayer film can improve recyclability. The upper limit of the ratio of the total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin in the multilayer film is preferably 99.5%, more preferably 99%, and may even be 98%. The "total average thickness of layers primarily composed of polyethylene-based resin or polypropylene-based resin" refers to the combined average thickness of layers primarily composed of polyethylene-based resin and layers primarily composed of polypropylene-based resin. Examples of layers primarily composed of polyethylene-based resin or polypropylene-based resin include layer (Y) when the adhesive resin (B) is, for example, acid-modified polyethylene or acid-modified polypropylene, and layer (Z) when the polyolefin resin (C) is polyethylene or polypropylene. The adhesive resin (B) and the polyolefin resin (C) may be the same type of resin or different types of resins.

[0067] For example, the lower limit of the ratio of the total average thickness of the layers containing a polyethylene-based resin as a main component in the multilayer film of the present invention is preferably 75%, more preferably 80%, even more preferably 85%, and even more preferably 88%. The upper limit of the ratio of the total average thickness of the layers containing a polyethylene-based resin as a main component in the multilayer film is preferably 99.5%, more preferably 99%, or even 98%. Furthermore, the lower limit of the ratio of the total average thickness of the layers containing a polypropylene-based resin as a main component in the multilayer film of the present invention is preferably 75%, more preferably 80%, even more preferably 85%, and even more preferably 88%. The upper limit of the ratio of the total average thickness of the layers containing a polypropylene-based resin as a main component in the multilayer film is preferably 99.5%, more preferably 99%, or even 98%.

[0068] The multilayer film of the present invention preferably does not have a layer containing as its main component a resin having a melting point of 200°C or higher, or a metal layer having an average thickness of 1 μm or higher. Furthermore, layer (X) preferably does not contain as its main component a resin having a melting point of 200°C or higher. By not having a layer containing as its main component a resin having a melting point of 200°C or higher, or a metal layer having an average thickness of 1 μm or higher, it is possible to prevent the pulverized multilayer film from being mixed with other components in a non-uniform manner when the film is melt-molded. Here, the metal layer refers to a layer having continuous and discontinuous surfaces made of metal, such as aluminum foil.

[0069] The multilayer film of the present invention has a width of 500 mm or more. Here, the width of the multilayer film refers to the distance from one end to the other end in the short direction of the film. In the case of a film stretched in the short direction, the width of the multilayer film refers to the width of the multilayer film before stretching. In the case of a film that has been trimmed, the width refers to the width of the multilayer film before trimming. Furthermore, in the case of a film formed by inflation molding, the width of the multilayer film is defined as twice the width at the time of winding. The actual width of the multilayer film (e.g., the width after trimming) may be 500 mm or more. The wider the multilayer film, the longer the residence time of the resin at the film edge in the extrusion flow path, which makes the EVOH (a1) more likely to remain inside the die, resulting in viscosity changes and the generation of degradation products, resulting in more pronounced defects in the appearance of the multilayer film. The width of the multilayer film is preferably 1,000 mm or more from the viewpoint of achieving more pronounced effects on appearance properties. The width of the multilayer film may also be 5,000 mm or less.

[0070] The image clarity C is measured in accordance with JIS K7374 (2007, transmission method) with the position of one end of the multilayer film in the width direction as 0% and the position of the other end as 100%, with the 10%, 50%, and 90% positions as the center, when the longitudinal direction of the multilayer film is perpendicular to the optical comb width of 2.0 mm. MD and image clarity C when the width direction is the vertical direction TDis preferably 60% or more, more preferably 70% or more, and even more preferably 75% or more. MD Standard deviation of image clarity C TD The standard deviation of each of the image clarity C is preferably 10% or less, and more preferably 5% or less. TD The average value of (average C TD ) Image clarity C MD The average value of (average C MD ) ratio (average C MD / Average C TD ) is preferably 0.80 to 1.15, more preferably 0.85 to 1.05, and even more preferably 0.90 to 1.00. Such a multilayer film is particularly useful as a film with excellent appearance properties. MD and image clarity C TD can be adjusted by the composition of each layer of the multilayer film as well as the production conditions (for example, the take-up speed during film production).

[0071] <Method for Producing a Multilayer Film> The method for producing a multilayer film (film formation method) is not particularly limited. Generally, a conventional coextrusion method can be used, in which each resin is extruded through a separate die or a common die and laminated. Either a circular die or a T-die can be used as the die. The method for uniaxial or biaxial stretching is also not particularly limited. The film can be produced by stretching in the machine direction and / or the direction perpendicular to the machine direction, i.e., the width direction, using a conventional stretching method such as roll-type uniaxial stretching, tenter-type uniaxial stretching, tubular-type simultaneous biaxial stretching, tenter-type sequential biaxial stretching, or tenter-type simultaneous biaxial stretching. Furthermore, tenter-type sequential biaxial stretching may use a tenter for both axes, or may be a combination of roll-type stretching and tenter-type stretching. The effects of the present invention are particularly pronounced in the case of a multilayer film produced by tenter-type sequential biaxial stretching, which is a combination of roll-type stretching and tenter-type stretching. From the viewpoint of processability, the temperature during stretching is usually 40 to 170° C., and more preferably 50 to 160° C. If necessary, after stretching, it is preferable to carry out a heat treatment at a temperature equal to or higher than the glass transition point and lower than the melting point, thereby increasing the crystallinity and fixing the orientation of the molecular chains, which is called heat setting.

[0072] From the viewpoint of appearance properties, the method for producing a multilayer film preferably includes the steps of melt-kneading EVOH (a1) and polyvalent metal ions (a2) to obtain pellets of resin composition (A), and melt-molding the pellets of resin composition (A) to form layer (X). Specific methods for obtaining pellets of resin composition (A) are as described above.

[0073] <Vapor-deposited multilayer film> The vapor-deposited multilayer film of the present invention comprises the multilayer film of the present invention and an inorganic vapor-deposited layer (I) laminated on the exposed surface of layer (X) of the multilayer film. That is, the multilayer film of the present invention may be used by laminating the inorganic vapor-deposited layer (I) on the surface of layer (X). The inorganic vapor-deposited layer (I) is preferably laminated on the exposed surface of layer (X) of the multilayer film directly or via another layer such as an adhesive layer, and is preferably laminated directly on the exposed surface of layer (X). The inorganic vapor-deposited layer (I) refers to a layer made of an inorganic substance such as a metal or inorganic oxide and having gas barrier properties against oxygen and water vapor. Layer (X) has a higher affinity with metals and inorganic oxides than ordinary thermoplastic resins, allowing the formation of a dense, defect-free inorganic vapor-deposited layer (I). The resulting vapor-deposited multilayer film has good interlayer adhesion between layer (X) and inorganic vapor-deposited layer (I). Furthermore, because layer (X) has gas barrier properties, deterioration of gas barrier properties can be suppressed even when defects occur in the inorganic vapor-deposited layer (I) due to bending or the like. The inorganic vapor-deposited layer (I) generally has an average thickness of less than 500 nm. When the average thickness is less than 500 nm, the viscosity of the vapor-deposited multilayer film or multilayer structure containing the inorganic vapor-deposited layer (I) is stable during melt molding, and the occurrence of gels or lumps can be suppressed.

[0074] The inorganic vapor deposition layer (I) is preferably either a metal vapor deposition layer containing aluminum as a main component or an inorganic oxide vapor deposition layer containing alumina or silica as a main component. A metal vapor deposition layer is preferred when light-shielding properties are to be imparted, but an inorganic oxide vapor deposition layer is preferred from the viewpoints of visibility of the contents as a packaging material, microwave suitability, and suppression of gels and lumps when pulverized materials are melt-molded. Furthermore, an inorganic oxide vapor deposition layer is preferred from the viewpoint of suppressing coloration during recycling of the multilayer structure of the present invention.

[0075] The aluminum atom content in the metal vapor-deposited layer is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably 95 mol% or more. The average thickness of the metal vapor-deposited layer is preferably 120 nm or less, more preferably 100 nm or less, and even more preferably 90 nm or less. The average thickness of the metal vapor-deposited layer is preferably 25 nm or more, more preferably 35 nm or more, and even more preferably 45 nm or more. The average thickness of the metal vapor-deposited layer is the average value of thicknesses at any 10 points on the cross section of the metal vapor-deposited layer measured using an electron microscope. When the vapor-deposited multilayer film of the present invention has a metal vapor-deposited layer, the light transmittance at a wavelength of 600 nm can be 10% or less, and the film has excellent light-blocking properties.

[0076] In a metal vapor deposition layer containing aluminum as a main component, oxidation may occur irreversibly, and aluminum oxide may be partially contained. In a metal vapor deposition layer containing aluminum as a main component (inorganic vapor deposition layer (I)), the molar ratio of the oxygen atom content to the aluminum atom content (O mol / Al mol) is preferably 0.5 or less, more preferably 0.3 or less, and even more preferably 0.1 or less.

[0077] The average thickness of the inorganic oxide vapor-deposited layer is preferably 60 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less. The average thickness of the inorganic oxide vapor-deposited layer is preferably 10 nm or more, more preferably 15 nm or more, and even more preferably 20 nm or more. The average thickness of the inorganic oxide vapor-deposited layer is the average value of thicknesses at any 10 points on a cross section of the inorganic oxide vapor-deposited layer measured using an electron microscope. When the vapor-deposited multilayer film of the present invention has an inorganic oxide vapor-deposited layer, the light transmittance at a wavelength of 600 nm can be increased to 80% or more, thereby providing excellent visibility of the contents when used as a packaging material. To further improve visibility, the light transmittance at a wavelength of 600 nm is more preferably 90% or more. The light transmittance can be increased, for example, by suppressing thickness unevenness of the multilayer film used in the production of the multilayer film. One example of a means for further suppressing thickness unevenness of the multilayer film is stretching the film in at least one direction. The light transmittance of the vapor-deposited multilayer film at a wavelength of 600 nm is preferably 80% or more, more preferably 90% or more.

[0078] The inorganic vapor deposition layer (I) can be formed by a known physical vapor deposition method or chemical vapor deposition method. Specific examples include vacuum deposition, sputtering, ion plating, ion beam mixing, plasma CVD, laser CVD, MO-CVD, and thermal CVD. Physical vapor deposition is preferred, and vacuum vapor deposition is more preferred. The upper limit of the surface temperature of layer (X) during the formation of inorganic vapor deposition layer (I) is preferably 60°C, more preferably 55°C, and even more preferably 50°C. The lower limit of the surface temperature of layer (X) during the formation of inorganic vapor deposition layer (I) is not particularly limited, but is preferably 0°C, more preferably 10°C, and even more preferably 20°C. The exposed surface of layer (X) may be plasma-treated before film formation. This plasma treatment can be performed by a known method, and atmospheric pressure plasma treatment is preferred. In atmospheric pressure plasma treatment, nitrogen, helium, neon, argon, krypton, xenon, radon, or the like is used as a discharge gas. Among these, nitrogen, helium, and argon are preferably used, and nitrogen is particularly preferred because it can reduce costs. A known protective layer or the like may be provided on the inorganic vapor deposition layer (I) to improve flex resistance.

[0079] The multilayer film or vapor-deposited multilayer film of the present invention has an oxygen transmission rate (under conditions of 20°C and 65% RH) of 60 cc / (m) as measured in accordance with the method described in JIS K7126-2 (isobaric method; 2006). 2 ·day·atm), and 2 ·day·atm), and more preferably less than 3 cc / (m 2 ·day·atm), and more preferably less than 0.5 cc / (m 2 A multilayer film or a vapor-deposited multilayer film having an oxygen transmission rate within the above range has excellent gas barrier properties.

[0080] <Multilayer structure, recovered composition, method for recovering multilayer structure, and packaging material> The multilayer film or vapor-deposited multilayer film of the present invention can itself be used as a packaging material having gas barrier properties, but by laminating at least one resin layer (R) containing a thermoplastic resin (D) as a main component to form a multilayer structure, it is possible to impart various functions as a packaging material, such as designability and heat-sealability. In other words, the multilayer structure of the present invention is formed by laminating the multilayer film or vapor-deposited multilayer film of the present invention with at least one resin layer (R) containing a thermoplastic resin (D) as a main component.

[0081] The thermoplastic resin (D) is not particularly limited, and examples thereof include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, vinyl ester resin, ethylene-propylene copolymer, polypropylene, propylene-α-olefin copolymer (α-olefin having 4 to 20 carbon atoms), polybutene, polypentene, and other olefin homopolymers or copolymers thereof, polyamides such as nylon 6 and nylon 6,6, polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polystyrene, polyvinyl chloride, polyvinylidene chloride, acrylic resin, polycarbonate, chlorinated polyethylene, chlorinated polypropylene, etc. Among these, polyolefins are preferred from the viewpoints of excellent moisture resistance, mechanical properties, economical efficiency, heat sealability, etc., and polyamides and polyesters are preferred from the viewpoints of excellent mechanical properties, heat resistance, etc. In order to obtain a multilayer structure having particularly excellent recyclability, the thermoplastic resin (D) is preferably the same type as the polyolefin resin (C), i.e., a polyolefin resin having a melting point of less than 170°C, more preferably a polyethylene-based resin or a polypropylene-based resin as the main component, even more preferably polyethylene or polypropylene, and particularly preferably polyethylene. Therefore, in order to obtain a multilayer structure having excellent recyclability, the polyolefin resin (C) and the thermoplastic resin (D) preferably contain a polyethylene-based resin or a polypropylene-based resin as the main component, more preferably polyethylene or polypropylene, and even more preferably polyethylene. Such a resin layer (R) may be unstretched, or may be uniaxially or biaxially stretched or rolled. From the viewpoint of improving mechanical strength, a biaxially stretched layer is preferred, and from the viewpoint of improving heat sealability, a non-stretched layer is preferred.

[0082] The method for producing the resin layer (R) is not particularly limited, but it is generally produced by melt extrusion using an extruder. Either a circular die or a T-die can be used as the die. The method for uniaxial or biaxial stretching is also not particularly limited, and the film can be produced by stretching the film in the machine direction and / or the direction perpendicular to the machine direction, i.e., the width direction, using a conventionally known stretching method such as roll-type uniaxial stretching, tubular-type simultaneous biaxial stretching, tenter-type sequential biaxial stretching, or tenter-type simultaneous biaxial stretching. From the viewpoint of the thickness uniformity and mechanical strength of the resulting layer, the area ratio is preferably 8 to 60 times. The area ratio is more preferably 55 times or less, and even more preferably 50 times or less. Furthermore, the area ratio is more preferably 9 times or more. If the area ratio is less than 8 times, stretching unevenness may remain, and if it exceeds 60 times, the layer may be more likely to break during stretching.

[0083] The average thickness of the resin layer (R) is preferably 10 to 200 μm from the viewpoint of industrial productivity. Specifically, the average thickness is more preferably 10 to 150 μm in the case of an unstretched layer, and more preferably 10 to 50 μm in the case of a biaxially stretched layer.

[0084] The average thickness of the multilayer structure of the present invention is preferably 300 μm or less. With an average thickness within this range, the multilayer structure of the present invention is lightweight and flexible, making it suitable for use in flexible packaging. Furthermore, the amount of resin used in the multilayer structure is small, thereby reducing the environmental impact.

[0085] The average thickness of each layer in the multilayer structure of the present invention may be adjusted appropriately depending on the application, but from the viewpoints of suppressing discoloration during melt molding of the pulverized material, improving thermal stability during melt molding, and suppressing the occurrence of lumps, at least one of the layer (Z) and the resin layer (R) contains a polyethylene resin or a polypropylene resin as a main component, and the ratio of the total average thickness of the layers containing a polyethylene resin or a polypropylene resin as a main component to the average thickness of the multilayer structure is preferably 80% or more, more preferably 85% or more. On the other hand, from the viewpoint of improving gas barrier properties, this ratio is preferably 99.7% or less, more preferably 99.5% or less, and may be 99.3% or less.

[0086] For example, the lower limit of the ratio of the total average thickness of the layers containing a polyethylene-based resin as the main component in the multilayer structure of the present invention is preferably 80%, more preferably 85%. The upper limit of the ratio of the total average thickness of the layers containing a polyethylene-based resin as the main component in the multilayer structure is preferably 99.7%, more preferably 99.5%, or even 99.3%. Furthermore, the lower limit of the ratio of the total average thickness of the layers containing a polypropylene-based resin as the main component in the multilayer structure of the present invention is preferably 80%, more preferably 85%. The upper limit of the ratio of the total average thickness of the layers containing a polypropylene-based resin as the main component in the multilayer structure is preferably 99.7%, more preferably 99.5%, or even 99.3%.

[0087] The method for laminating the resin layer (R) on the multilayer film or vapor-deposited multilayer film of the present invention is not particularly limited, and examples include extrusion lamination, coextrusion lamination, dry lamination, etc. An adhesive layer may be provided when laminating the resin layer (R) on the multilayer film or vapor-deposited multilayer film. Furthermore, each layer constituting the multilayer structure of the present invention may be laminated via an adhesive layer, if necessary. However, it is preferable that no adhesive layer is present between layer (X) and layer (Y) or between layer (Y) and layer (Z) of the multilayer film or vapor-deposited multilayer film. The adhesive layer can be formed by applying and drying a known adhesive. The adhesive is preferably a two-component reactive polyurethane adhesive in which a polyisocyanate component and a polyol component are mixed and reacted. The average thickness of the adhesive layer is not particularly limited, but is preferably 1 to 5 μm, more preferably 2 to 4 μm.

[0088] The multilayer structure of the present invention is not particularly limited, and from the viewpoint of obtaining a multilayer structure with excellent recyclability, for example, the following layer configuration is preferred. In the following layer configurations, layer (X) is represented as X, layer (Y) as Y, layer (Z) as Z, inorganic vapor deposition layer (I) as I, and layer (R) as R, and " / " means that they are directly laminated, and " / / " means that they are laminated via an adhesive layer or that they are directly laminated, with laminated via an adhesive layer being a preferred embodiment. (1) Z / Y / X / I / / R (2) R / / Z / Y / X / I / / R (3) Z / Y / X / / R (4) R / / Z / Y / X / / R

[0089] In the layer structure, the layers (X), (Y), and (Z) may be uniaxially stretched, biaxially stretched, or unstretched. The layers (Z) and (R) are preferably polyethylene-based resins or polypropylene-based resins, and the layer (Y) is preferably maleic anhydride-modified polyethylene-based resins or maleic anhydride-modified polypropylene-based resins. Furthermore, when recycling the packaging material of the present invention, the outermost layers of the multilayer structure of the present invention preferably have layers containing a polyethylene-based resin or a polypropylene-based resin as a main component, so that the pulverized product obtained by pulverizing the packaging material can be recovered as a composition mainly containing a polyethylene-based resin or a polypropylene-based resin. That is, when the resin layers (R) are disposed on both outermost layers, the resin layers (R) are preferably layers mainly containing a polyethylene resin or a polypropylene resin. When the layers (Z) and (R) are disposed on both outermost layers, the resin layers (Z) and (R) are preferably layers mainly containing a polyethylene-based resin or a polypropylene-based resin. Of the layers arranged as the outermost layers, it is preferable that one is an unstretched layer and the other is a layer stretched in at least one direction, which may be preferable from the viewpoint of obtaining a multilayer structure that has both heat sealability and mechanical properties.

[0090] The multilayer structure of the present invention may have layers other than those described above, provided that the effects of the present invention are not impaired. An example of such layers is a recovery layer. It is particularly preferable to reuse a recovered composition containing recovered materials from the multilayer structure of the present invention, as described below, as part or all of the recovery layer. Another example of such layers is a printed layer. The printed layer may be included at any position in the multilayer structure of the present invention. Examples of the printed layer include a film obtained by applying a solution containing a pigment or dye, and optionally a binder resin, followed by drying. Examples of methods for applying the printed layer include gravure printing and various other application methods using a wire bar, spin coater, die coater, etc. The average thickness of the ink layer is not particularly limited, but is preferably 0.5 to 10 μm, more preferably 1 to 4 μm.

[0091] It is preferable to reuse the recovered end portions and defective products generated during the production of the multilayer structure of the present invention. A method for recovering a multilayer structure of the present invention, which comprises a step of crushing the multilayer structure of the present invention and then melt-molding it, and a recovered composition containing the recovered multilayer structure of the present invention are also preferred embodiments of the present invention.

[0092] When recovering the multilayer structure of the present invention, the recovered multilayer structure of the present invention is first pulverized. The pulverized recovered material may be melt-molded directly to obtain a recovered composition, or may be melt-molded together with other components as needed to obtain a recovered composition. A preferred component to be added to the recovered material is a polyolefin resin, and a polyethylene-based resin or a polypropylene-based resin is more preferred. The polyolefin resin used is the same type as the polyolefin resin (C) described above for use in the multilayer film of the present invention. The pulverized recovered material may be directly used to produce a molded product such as a multilayer structure, or the pulverized recovered material may be melt-molded to obtain pellets of the recovered composition, and the pellets may then be used to produce a molded product.

[0093] The mass ratio of the resin composition (A) to the polyolefin resin in the recovered composition [resin composition (A) / polyolefin resin] is preferably 0.01 / 99.99 to 20 / 80. When the mass ratio is 0.01 / 99.99 or more, there is less need to use polyolefin resins other than the recovered material in the multilayer structure, and the proportion of recovered material used is increased. On the other hand, when the mass ratio is 20 / 80 or less, the melt-moldability and mechanical properties of the recovered composition are improved. From the viewpoint of improving the melt-moldability and mechanical properties of the resulting recovered composition, the mass ratio is more preferably 15 / 85 or less, even more preferably 10 / 90 or less, and may even be 5 / 95 or less.

[0094] The multilayer structure of the present invention has gas barrier properties and recyclability, and therefore can be suitably used as a material for various types of packaging, such as food packaging, pharmaceutical packaging, industrial chemical packaging, and agricultural chemical packaging. In particular, packaging materials comprising the multilayer structure of the present invention can be suitably used as packaging materials with excellent recyclability. The multilayer film and vapor-deposited multilayer film of the present invention can also be suitably used as packaging materials.

[0095] The present invention will be explained in more detail below using examples, but the present invention is not limited to these examples in any way.

[0096] [Materials Used] EVOH (a1) EVOH (a1-1): EVOH (ethylene (Et) unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 180 ppm of sodium acetate in terms of sodium ions, 30 ppm of phosphate ions in terms of phosphate radicals, and 150 ppm of boric acid in terms of boron element, but does not contain polyvalent metal ions.) EVOH (a1-1A): EVOH (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 30 ppm of phosphate ions calculated as phosphate radicals, and 150 ppm of boric acid calculated as boron element, but does not contain alkali metal ions or polyvalent metal ions.) EVOH (a1-1B): EVOH (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 100 ppm of sodium acetate in terms of sodium ions, 30 ppm of phosphate ions in terms of phosphate radicals, and 150 ppm of boric acid in terms of boron element, but does not contain polyvalent metal ions.) EVOH (a1-1C): EVOH (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 250 ppm of sodium acetate in terms of sodium ions, 30 ppm of phosphate ions in terms of phosphate radicals, and 150 ppm of boric acid in terms of boron element, but does not contain polyvalent metal ions.) EVOH (a1-1D): EVOH (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 1.6 g / 10 min, melting point 183°C, volatile content 0.8%, contains 550 ppm of sodium acetate in terms of sodium ions, 30 ppm of phosphate ions in terms of phosphate radicals, and 150 ppm of boric acid in terms of boron element, but does not contain polyvalent metal ions.EVOH (a1-2): EVOH (ethylene unit content 27 mol%, saponification degree 99.99 mol%, MFR (210°C, 2.16 kg load) 4.0 g / 10 min, melting point 191°C, volatile content 0.8%, contains 180 ppm of sodium acetate calculated as sodium ions, 30 ppm of phosphate ions calculated as phosphate radicals, and 150 ppm of boric acid calculated as boron element, but does not contain polyvalent metal ions. EVOH (a1-3): EVOH (ethylene unit content 44 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 1.9 g / 10 min, melting point 165°C, volatile content 0.8%, contains 180 ppm of sodium acetate calculated as sodium ions, 30 ppm of phosphate ions calculated as phosphate radicals, and 150 ppm of boric acid calculated as boron element, but does not contain polyvalent metal ions. EVOH (a1-2 / 3): EVOH (a1-2) and EVOH (a1-3) mixed (dry blended) at a mass ratio of 75 / 25 EVOH (a1-4): EVOH (ethylene unit content 48 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 6.4 g / 10 min, melting point 158°C, volatile content 0.8%, contains 180 ppm of sodium acetate in terms of sodium ions, 50 ppm of phosphate ions in terms of phosphate radicals, and does not contain polyvalent metal ions.) EVOH (a1-5): EVOH (ethylene unit content 44 mol%, saponification degree 99.99 mol%, epoxypropane modification degree 4.6 mol%, MFR (190°C, 2.16 kg load) 5.6 g / 10 min, volatile content 0.8%, melting point 119°C, contains 220 ppm of sodium acetate calculated as sodium ions and 30 ppm of phosphate ions calculated as phosphate radicals). The epoxypropane modification degree refers to the content of monomer units modified with epoxypropane relative to the total monomer units. (Method for Producing EVOH (a-5)) 28 parts by mass of zinc acetylacetonate monohydrate was mixed with 957 parts by mass of 1,2-dimethoxyethane to obtain a mixed solution. 15 parts by mass of trifluoromethanesulfonic acid was added to the obtained mixed solution with stirring to obtain a catalyst solution.Next, EVOH having an ethylene unit content of 44 mol% and a degree of saponification of 99.99 mol% or more (but containing no alkali metal ions and 30 ppm of phosphate ions) was charged into a TEM-35BS extruder (37 mmφ, L / D = 52.5) ​​manufactured by Toshiba Machine Co., Ltd., and operated under the following conditions: barrel C1 was water-cooled, barrels C2 to C3 were cooled to 200°C, barrels C4 to C15 were cooled to 240°C, and a screw rotation speed of 250 rpm. Epoxypropane (1.5 kg / hr) and the catalyst solution were added through pressure inlet 1 of C8. Next, an aqueous sodium acetate solution was added through pressure inlet 2 of C13. The discharged strand was cooled and solidified in a cooling tank, cut, and then dried to obtain EVOH (a-5). In this step, the amount of catalyst solution added was adjusted so that the melting point of the resulting EVOH (a-5) would be 119°C. The amount of the aqueous sodium acetate solution added was adjusted appropriately so that the content of sodium ions in EVOH (a-5) was as described above.

[0097] Example 1 (1) Preparation of Resin Composition (A) Pellets 100 parts by mass of EVOH (a1-1) pellets and calcium stearate were dry-blended so that the calcium ion content in the resulting resin composition was 1,000 ppm, and then melt-kneaded to obtain resin composition (A) pellets for layer (X). The extruder used for melt-kneading was a twin-screw extruder with a D (mm) of 25 and a co-rotating, fully intermeshing screw with an L / D of 30. A mixing zone consisting of a feed-type kneading disc, a neutral-type kneading disc, and a return-type kneading disc in succession was located midway through the screw, and a vacuum vent was located downstream of the zone. During melt-kneading, the pressure was reduced using the vacuum vent. The resin temperature was maintained at 230°C.

[0098] (2) Thermogravimetry (TG) of Resin Composition (A) Pellets Thermogravimetry (TG) was performed on the obtained resin composition (A) pellets under conditions of holding at 200°C for 30 minutes in a nitrogen atmosphere to measure the weight loss W. The results are shown in Table 1.

[0099] (3) Resin composition containing adhesive resin (B) for layer (Y) Maleic anhydride-modified polyethylene "ADMER (trademark) NF518" (MFR (190°C, 2.16 kg load) 3.1 g / 10 min, density 0.91 g / cm) manufactured by Mitsui Chemicals, Inc. 3 , b-1) was used as adhesive resin (B) as resin composition pellets for layer (Y). In this specification, a substance consisting essentially of only one component is also referred to as a composition.

[0100] (4) Resin composition containing polyolefin resin (C) for layer (Z) Low-density polyethylene "INNATE (trademark) TF80" (MFR (190°C, 2.16 kg load) 1.6 g / 10 min, melting point 124°C, density 0.926 g / cm) manufactured by DOW 3 ) was used as polyolefin resin (C) as resin composition pellets for layer (Z).

[0101] (5) Preparation of Multilayer Films Using the resin composition pellets obtained in (1), (3), and (4) above, multilayer films having an average thickness and layer structure of (X) / (Y) / (Z) = 4 μm / 4 μm / 32 μm = EVOH4 / Tie4 / PE32 were prepared using coextrusion film-forming equipment. Each extruder was a single-screw extruder with a D (mm) of 30, and a full-flight screw with an L / D of 28 and a compression ratio of 3.0 was used. A 600 mm wide feedblock lamination type T-die was used as the die. The temperature conditions used were as follows. The ratio of the total average thickness of the layers primarily composed of polyethylene-based resin in the multilayer film was 90%. Extrusion temperature of resin composition (A): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220°C Extrusion temperature of resin composition containing adhesive resin (B): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220°C Extrusion temperature of resin composition containing polyolefin resin (C): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220°C Die temperature: 240°C Chill roll temperature: 50°C Take-up speed: 6.0 m / min

[0102] (6) Appearance Evaluation The image clarity of the multilayer film obtained in (5) above was measured at an optical comb width of 2.0 mm in accordance with JIS K7374 (2007, transmission method), and the appearance of the multilayer film was evaluated according to the following criteria: When streaks occur in the multilayer film of the present invention, streaks in the machine direction tend to occur together mainly at the edges in the width direction of the multilayer film, and in the evaluation criteria below, the range where such streaks occur together is expressed as a "region." Specifically, an image clarity tester ("IC-T" manufactured by Suga Test Instruments Co., Ltd.) was used to measure image clarity at the following positions: 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, and 90% of the width of the multilayer film, with one end of the multilayer film at 0% and the other end at 100%. The image clarity was measured with the longitudinal direction (MD) of the multilayer film as the vertical direction. The incidence of streaks was evaluated based on the image clarity measurements. A rating of E was deemed to indicate poor appearance. The results are shown in Table 3. Rating: Criteria A: Slight streaks were observed in an area less than 50% of the total width of the film, and the area where mild to severe streaks were observed was less than 10%. B: Slight streaks were observed in an area of ​​50% or more of the total width of the film, and mild to severe streaks were observed in less than 10% of the area. C: Not applicable to B, slight or mild streaks were observed in an area of ​​50% or more of the total width of the film, and moderate to severe streaks were observed in less than 10% of the area. D: Not applicable to B and C, slight to moderate streaks were observed in an area of ​​50% or more of the total width of the film, and severe streaks were observed in less than 10% of the area. E: Not applicable to B to D, slight to severe streaks were observed in an area of ​​50% or more of the total width of the film, or severe streaks were observed in an area of ​​10% or more of the total width of the film.

[0103] (7) Measurement of Image Clarity The image clarity of the multilayer film obtained in (5) above was measured at an optical comb width of 2.0 mm in accordance with JIS K7374 (2007, transmission method). Specifically, the image clarity was measured using an image clarity measuring instrument ("IC-T" manufactured by Suga Test Instruments Co., Ltd.) at positions of 10%, 50%, and 90% when the position of one end in the width direction of the multilayer film was 0% and the position of the other end was 100%, with the longitudinal direction (MD direction) of the multilayer film being the vertical direction. MD , image clarity C when the width direction (TD direction) of the multilayer film is perpendicular to the light source TD The average value of the three measured values ​​(average image clarity C MD and average clarity C TD ) was calculated. MD and average image clarity C TD Ratio of average clarity C MD / Average sharpness C TD ) was calculated. MD and C TD The standard deviation was calculated for the measured values. The results are shown in Table 3.

[0104] (8) Evaluation of Adhesion of Multilayer Films The adhesion of the multilayer films obtained in (5) above was evaluated. Specifically, strip-shaped test pieces measuring 200 mm in the longitudinal direction (MD) and 15 mm in the width direction (TD) were cut out of the resulting test pieces. The interface between layer (X) and layer (Y) was then peeled off, and the T-peel strength (gf / 15 mm) was measured using an Autograph AGS-H manufactured by Shimadzu Corporation under conditions of a chuck spacing of 50 mm and a tensile speed of 250 mm / min. Measurements were performed on five test pieces (test pieces centered at 10%, 25%, 50%, 75%, and 90% positions, with one end position in the width direction of the multilayer film being 0% and the other end position being 100%), and the adhesion was evaluated based on the average value according to the following criteria. Note that a rating of E was deemed to indicate poor adhesion. The results are shown in Table 3. Judgment: Criteria A: 250gf / 15mm or more B: 150gf / 15mm or more and less than 250gf / 15mm C: 100gf / 15mm or more and less than 150gf / 15mm D: 50gf / 15mm or more and less than 100gf / 15mm E: Less than 50gf / 15mm

[0105] (9) Oxygen Transmission Rate of Multilayer Film The oxygen transmission rate of the multilayer film obtained in (5) above was measured in accordance with the method described in JIS K 7126-2 (isobaric method; 2006) with layer (Z) as the oxygen supply side. Specifically, the oxygen transmission rate (unit: cc / (m)) was measured using an oxygen transmission rate measuring device ("MOCON OX-TRAN2 / 21" manufactured by Modern Control Co., Ltd.) under the conditions of a temperature of 20°C, a humidity of 65% RH on the oxygen supply side, a humidity of 65% RH on the carrier gas side, an oxygen pressure of 1 atmosphere, and a carrier gas pressure of 1 atmosphere. 2 The gas barrier properties were evaluated based on the following criteria: Nitrogen gas containing 2% by volume of hydrogen gas was used as the carrier gas. When the evaluation was E, it was determined that the gas barrier properties were poor. The results are shown in Table 3. Evaluation: Criteria A: 1 cc / (m 2 ・day・atm) B: 1cc / (m 2 ・day・atm) or more, 3cc / (m 2 ・day・atm) C: 3cc / (m 2 ・day・atm) or more, 10cc / (m 2 · day · atm) less than D: 10cc / (m 2 ・day・atm) or more, 60cc / (m 2 ・day・atm) Less than E: 60cc / (m 2 ・day・atm) or more

[0106] (10) Preparation of multilayer structure A two-component reactive polyurethane adhesive (24 parts by mass of "Takelac™ A-520" manufactured by Mitsui Chemicals, Inc. and 4 parts by mass of "Takenate™ A-50") was mixed with 37 parts by mass of ethyl acetate to prepare an adhesive solution. Next, the adhesive solution was applied to the corona-treated surface of a resin layer (R) (an LLDPE film having an average thickness of 50 μm ("Unilux™ LS-760C" manufactured by Idemitsu Unitech Co., Ltd.)) with a wire bar so that the average thickness after drying was 2 μm. The solution was then dried at 100 ° C. for 5 minutes and laminated with the multilayer film obtained in (5) to prepare a multilayer structure having an average thickness and layer structure of (R) / adhesive / (X) / (Y) / (Z) = 50 μm / 2 μm / 4 μm / 4 μm / 32 μm. The adhesion temperature (heat roll temperature) during lamination was 80°C, and then aging was carried out at 40°C for 3 days.

[0107] (11) Evaluation of coloration and recyclability of recovered multilayer structure The multilayer structure obtained in (10) was crushed into a size of 4 mm square or less, and the crushed product was mixed with low-density polyethylene (LDPE) "Novatec (trademark) LD LJ400" (MFR (190 ° C, 2.16 kg load) 1.5 g / 10 min, melting point 111 ° C, density 0.921 g / cm) manufactured by Japan Polyethylene Co., Ltd. 3) were dry-blended in a mass ratio (recycled material / low-density polyethylene) of 50 / 50, and a monolayer film (recycled material) with an average thickness of 100 μm was obtained by extrusion under the following conditions. Furthermore, as a control, a monolayer film with an average thickness of 100 μm was obtained in the same manner using only the low-density polyethylene (hereinafter, sometimes simply referred to as "control"). The extruder was a single-screw extruder with D (mm) = 20, and a full-flight screw with L / D = 20 and a compression ratio of 3.5 was used. A 300 mm wide T-die was used as the die. The average thickness of the monolayer film was adjusted by appropriately changing the screw rotation speed and take-up roll speed. The temperature conditions used here are shown below. : Extrusion temperature: feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220°C Die temperature: 220°C Chill roll temperature: 80°C The coloration and defects of the obtained monolayer film (recycled material) were visually compared with the control and judged according to the following criteria. A defect rating of E was determined to be insufficient in recyclability. The results are shown in Table 3. Coloration judgment: Criteria A: The degree of hue change was small compared to the control. B: Slight coloration was observed compared to the control. C: Moderate coloration was observed compared to the control. D: Significant coloration was observed compared to the control. E: Significant coloration was observed compared to the control, and unevenness was also observed. Defect (recyclability) judgment: Criteria A: The amount of particles was almost the same as that of the control. B: The amount of small particles was slightly higher compared to the control. C: The amount of small particles was higher compared to the control. D: The amount of large particles was higher compared to the control. E: Compared to the control, there was a significantly greater amount of large particles.

[0108] Examples 2 to 19 and Comparative Examples 2 to 4 Resin composition pellets, multilayer films, and multilayer structures were prepared and evaluated in the same manner as in Example 1, except that the type of EVOH (a1), the type and content of polyvalent metal ions (a2), and the content of alkali metal ions (a3) ​​were as shown in Table 1 or Table 2. The results are shown in Table 3 or Table 4. In Example 14, magnesium stearate was used instead of calcium stearate, and in Example 15, zinc stearate was used instead of calcium stearate. In Comparative Example 2, the same operations as in Example 1 were performed, except that calcium stearate was not added during the melt-kneading step in the preparation of (1) resin composition (A) pellets.

[0109] Example 20 Resin composition pellets, a multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 1, except that a dry blend prepared by dry-blending 100 parts by mass of EVOH (a1-1) pellets and 1.5 parts by mass of calcium stearate (calcium ion content in the dry blend: 1,000 ppm) was used as the resin composition for layer (X). The results are shown in Table 3.

[0110] Example 21 Resin composition pellets and a multilayer film were prepared in the same manner as in Example 1, except that an open vent was used instead of a vacuum vent when preparing resin composition (A) pellets for layer (X), and various measurements and evaluations were carried out. The results are shown in Table 4.

[0111] Example 22 Resin composition pellets and a multilayer film were prepared in the same manner as in Example 1, except that a vacuum vent was not used when preparing the resin composition (A) pellets for layer (X), and various measurements and evaluations were carried out. The results are shown in Table 4.

[0112] Example 23 An alumina (AlOx) vapor-deposited layer (inorganic vapor-deposited layer (I)) having an average thickness of 30 nm was laminated by a known vacuum vapor deposition method on the surface of layer (X) of the multilayer film obtained in (5) above to prepare a vapor-deposited multilayer film. Resin composition pellets, a multilayer film, a vapor-deposited multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 1, except that the vapor-deposited multilayer film was used instead of the multilayer film to prepare the multilayer structure. The results are shown in Table 4. The oxygen transmission rate was measured for the vapor-deposited multilayer film.

[0113] Example 24: Resin composition pellets, a multilayer film, a vapor-deposited multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 23, except that the alumina vapor-deposited layer was replaced with a silica (SiOx) vapor-deposited layer. The results are shown in Table 4.

[0114] Example 25: Resin composition pellets, a multilayer film, a vapor-deposited multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 23, except that the alumina vapor-deposited layer was replaced with an aluminum (Al) vapor-deposited layer having an average thickness of 50 nm. The results are shown in Table 4.

[0115] Example 26 Resin composition pellets, a multilayer film, and a multilayer structure were prepared in the same manner as in Example 1, except that the average thickness of each layer of the multilayer film was changed as shown in Table 2, and various measurements and evaluations were carried out. The results are shown in Table 4.

[0116] Example 27 Using each of the resin composition pellets obtained in (1), (3), and (4), a co-extruded film having an average thickness and layer structure of (X) / (Y) / (Z) = 20 μm / 20 μm / 160 μm = EVOH20 / Tie20 / PE160 was produced, and this was stretched 5 times in the longitudinal direction (MD direction) to produce a multilayer film having an average thickness and layer structure of 4 μm / 4 μm / 32 μm = EVOH4 / Tie4 / PE32. Resin composition pellets, multilayer films, and multilayer structures were produced and evaluated in the same manner as in Example 1, except that this was used instead of the multilayer film of Example 1. The results are shown in Table 4.

[0117] Example 28 Resin composition (A) pellets were prepared in the same manner as in Example 1, except that EVOH (a-5) was used instead of EVOH (a-1), and the resulting resin composition pellets and the resin composition pellets obtained in (3) and (4) above were used to prepare a co-extruded film having an average thickness and layer structure of (X) / (Y) / (Z) = 128 μm / 128 μm / 1024 μm = EVOH128 / Tie128 / PE1024. The film was stretched 4 times in the longitudinal direction (MD direction) and then 8 times in the transverse direction (TD direction) to produce a multilayer film having an average thickness and layer structure of 4 μm / 4 μm / 32 μm = EVOH4 / Tie4 / PE32. Except for this, resin composition pellets, multilayer films, and multilayer structures were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 4.

[0118] Example 29 As the adhesive resin (B), a maleic anhydride-modified polypropylene "ADMER (trademark) QF551" (MFR (230 ° C, 2.16 kg load) 5.7 g / 10 min, density 0.89 g / cm) manufactured by Mitsui Chemicals, Inc. was used. 3 , b-2) was used as polyolefin resin (C), and polypropylene "Novatec (trademark) PP EA7AD" (MFR (230°C, 2.16 kg load) 1.4 g / 10 min, melting point 161°C, density 0.90 g / cm) manufactured by Japan Polypropylene Corporation was used. 3 ) was used as the resin layer (R), a polypropylene film having an average thickness of 50 μm was used, and resin composition pellets, a multilayer film, and a multilayer structure were produced and evaluated in the same manner as in Example 1, except that the conditions for producing the multilayer film were changed as follows. The results are shown in Table 4. (Conditions for producing the multilayer film) Extrusion temperature of resin composition (A): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 230°C Extrusion temperature of resin composition containing adhesive resin (B): feeding section / compression section / metering section / adapter = 175 / 230 / 230 / 230°C Extrusion temperature of resin composition containing polyolefin resin (C): feeding section / compression section / metering section / adapter = 175 / 230 / 230 / 230°C Die temperature: 240°C Chill roll temperature: 50°C Take-up speed: 6.0 m / min

[0119] Example 30 As the adhesive resin (B), maleic anhydride-modified polyethylene "BYNEL (trademark) 41E687" manufactured by Dow (MFR (190 ° C, 2.16 kg load) 1.7 g / 10 min, density 0.91 g / cm 3 , b-3) was used, resin composition pellets, a multilayer film and a multilayer structure were produced and evaluated in the same manner as in Example 1. The results are shown in Table 4.

[0120] Example 31 As the adhesive resin (B), a maleic anhydride-modified polyethylene "ADMER (trademark) AT1955T" (MFR (190 ° C, 2.16 kg load) 2.6 g / 10 min, density 0.89 g / cm) manufactured by Mitsui Chemicals, Inc. was used. 3 , b-4) was used, resin composition pellets, a multilayer film and a multilayer structure were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 4.

[0121] Example 32 As the adhesive resin (B), a maleic anhydride-modified polyethylene "ADMER (trademark) AT1955T" (MFR (190 ° C, 2.16 kg load) 2.6 g / 10 min, density 0.89 g / cm) manufactured by Mitsui Chemicals, Inc. was used. 3 , b-4) was used as polyolefin resin (C), and polypropylene "Novatec (trademark) PP EA7AD" (MFR (230°C, 2.16 kg load) 1.4 g / 10 min, melting point 161°C, density 0.90 g / cm) manufactured by Japan Polypropylene Corporation was used. 3 ) was used as the resin layer (R), a polypropylene film having an average thickness of 50 μm was used, and resin composition pellets, a multilayer film, and a multilayer structure were produced and evaluated in the same manner as in Example 1, except that the conditions for producing the multilayer film were changed as follows. The results are shown in Table 4. (Conditions for producing the multilayer film) Extrusion temperature of resin composition (A): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 230°C Extrusion temperature of resin composition containing adhesive resin (B): feeding section / compression section / metering section / adapter = 175 / 230 / 230 / 230°C Extrusion temperature of resin composition containing polyolefin resin (C): feeding section / compression section / metering section / adapter = 175 / 230 / 230 / 230°C Die temperature: 240°C Chill roll temperature: 50°C Take-up speed: 6.0 m / min

[0122] Example 33 Resin composition pellets, a multilayer film, and a multilayer structure were produced and evaluated in the same manner as in Example 1, except that the take-up speed during production of the multilayer film was changed to 12 m / min. The results are shown in Table 4.

[0123] Comparative Example 1 A multilayer film (single layer film) and a multilayer structure were produced and evaluated in the same manner as in Example 1, except that a layer (Z) (single layer film) having an average thickness of 40 μm was used instead of the multilayer film. The layer (Z) having an average thickness of 40 μm was produced by extruding only a polyolefin resin (C)-containing resin composition (low-density polyethylene "INNATE (trademark) TF80" manufactured by DOW) without simultaneously extruding the resin composition (A) and adhesive resin (B) when producing the multilayer film in Example 1, and adjusting the average thickness. The results are shown in Table 4.

[0124] Comparative Example 5: Calcium stearate was not added, and the adhesive resin (B) was a maleic anhydride-modified polyethylene "ADMER (trademark) NF518" manufactured by Mitsui Chemicals, Inc. (MFR (190°C, 2.16 kg load) 3.1 g / 10 min, density 0.91 g / cm 3 Resin composition pellets, a multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Example 1, except that layer (Y) was formed using pellets obtained by dry-blending 20 parts by mass of the resin composition (b-1), b-2) and 80 parts by mass of a low-density polyethylene "INNATE (trademark) TF80" manufactured by Dow. The results are shown in Table 4.

[0125] Comparative Example 6 Resin composition pellets, a multilayer film, and a multilayer structure were prepared and evaluated in the same manner as in Comparative Example 5, except that the amount of calcium stearate added was changed so that the content of polyvalent metal ion (a2) was as shown in Table 2. The results are shown in Table 4.

[0126] Reference Example 1 Resin composition pellets, a multilayer film, and a multilayer structure were produced and evaluated in the same manner as in Comparative Example 3, except that the die used in producing the multilayer film was changed to a 300 mm wide feedblock lamination type T-die. The results are shown in Table 4. The only difference from Comparative Example 3 was the width. Comparative Example 3, in which the multilayer film width was 600 mm, showed a deterioration in appearance, whereas Reference Example 1, in which the multilayer film width was 300 mm, showed no deterioration in appearance. This shows that the problem of deterioration in appearance in the multilayer film of the present invention only arises when the multilayer film has a width of a certain amount or more (500 mm or more).

[0127]

[0128]

[0129]

[0130]

Claims

1. A multilayer film having a structure in which a layer (X) is an outermost layer, and a layer (X), a layer (Y) and a layer (Z) are laminated adjacent to each other in this order, the layer (X) being a layer consisting only of a resin composition (A) containing an ethylene-vinyl alcohol copolymer (a1) having an ethylene unit content of 20 to 50 mol% and a saponification degree of 90 mol% or more and a polyvalent metal ion (a2), the layer (Y) containing an adhesive resin (B) having a melting point of less than 170°C as a main component, the layer (Z) containing a polyolefin resin (C) having a melting point of less than 170°C as a main component, the resin composition (A) containing 350 to 2000 ppm of the polyvalent metal ion (a2), the polyvalent metal ion (a2) being at least one selected from the group consisting of magnesium ions, calcium ions, zinc ions, cobalt ions and manganese ions, and having a width of 500 mm or more.

2. The multi-layer film according to claim 1, wherein the adhesive resin (B) is an acid-modified polyethylene or an acid-modified polypropylene.

3. The multi-layer film according to claim 2, wherein the polyolefin resin (C) is polyethylene or polypropylene.

4. A multilayer film according to any one of claims 1 to 3, wherein the resin composition (A) contains 40 ppm or more and 500 ppm or less of alkali metal ions (a3).

5. The multilayer film according to any one of claims 1 to 4, wherein the following formula (a) is satisfied, where S (mol%) is the ethylene unit content of the ethylene-vinyl alcohol copolymer (a1) and T (ppm) is the amount of the polyvalent metal ion (a2): -4.17S + 560≦T≦-29.2S + 2600 (a) 6. The multilayer film according to any one of claims 1 to 5, wherein the layer (X) is a layer formed by melt molding pellets consisting of only the resin composition (A).

7. The multilayer film according to any one of claims 1 to 6, wherein in thermogravimetry (TG) of the resin composition (A), the weight loss W when held at 200°C for 30 minutes in a nitrogen atmosphere is 0.01 to 0.3%.

8. The multilayer film according to any one of claims 1 to 7, which does not have a layer containing as a main component a resin having a melting point of 200°C or higher and a metal layer having an average thickness of 1 µm or more.

9. The multilayer film according to any one of claims 1 to 8, wherein the average thickness of the layer (X) is 0.2 µm or more and less than 20 µm, and the ratio of the average thickness of the layer (X) to the average thickness of the multilayer film is less than 25%.

10. The multilayer film according to any one of claims 1 to 9, wherein the width of the multilayer film is 1000 mm or more.

11. The multilayer film of any one of claims 1 to 10, wherein the multilayer film is not oriented.

12. The multilayer film according to any one of claims 1 to 10, wherein the multilayer film is stretched uniaxially only by a factor of 3 to less than 12.

13. The multilayer film according to any one of claims 1 to 10, wherein the multilayer film is stretched in each of two axial directions by a factor of 3 or more and less than 12.

14. The multilayer film according to any one of claims 1 to 13, wherein the ratio of the total average thickness of layers mainly composed of a polyethylene resin or a polypropylene resin is 75% or more.

15. The image clarity C of the multilayer film when the longitudinal direction of the multilayer film is the vertical direction at an optical comb width of 2.0 mm is measured in accordance with JIS K7374 (2007, transmission method) with the positions of 10%, 50% and 90% as the center, assuming that the position of one end of the multilayer film in the width direction is 0% and the position of the other end is 100%. MD and image clarity C when the width direction is the vertical direction TD is 60% or more, and the image clarity C measured at the measurement position MD Standard deviation of and image clarity C TD The multilayer film according to any one of claims 1 to 14, wherein the standard deviation of each of the above is 10% or less.

16. The image clarity of the multilayer film at an optical comb width of 2.0 mm is measured in accordance with JIS K7374 (2007, transmission method) with the position of one end of the multilayer film in the width direction as 0% and the position of the other end as 100%, with the positions of 10%, 50% and 90% as the center, and the image clarity C when the longitudinal direction is the vertical direction. MD and image clarity C when the width direction is the vertical direction TD The ratio of the average values ​​of each of the above (average clarity C MD / Average sharpness C TD 16. The multilayer film according to claim 1, wherein the saturation coefficient (S) is 0.80 to 1.

15.

17. A vapor-deposited multilayer film comprising: the multilayer film according to any one of claims 1 to 16; and an inorganic vapor-deposited layer (I) laminated on the exposed surface side of the layer (X) in the multilayer film.

18. The vapor-deposited multilayer film according to claim 17, wherein the inorganic vapor-deposited layer (I) is a vapor-deposited metal layer mainly composed of aluminum or a vapor-deposited inorganic oxide layer mainly composed of alumina or silica.

19. The oxygen transmission rate measured in accordance with JIS K7126-2 (2006) under conditions of 20°C and 65% RH is 60 cc / (m 2 The multilayer film or vapor-deposited multilayer film according to any one of claims 1 to 18, wherein the viscosity is less than 1 / day atm.

20. A multilayer structure comprising the multilayer film or vapor-deposited multilayer film according to any one of claims 1 to 19 laminated with at least one resin layer (R) containing a thermoplastic resin (D) as a main component.

21. The multilayer structure of claim 20, wherein the thermoplastic resin (D) is polyethylene or polypropylene.

22. A packaging material comprising the multilayer structure according to claim 20 or 21.

23. A recycled composition comprising a recycled multi-layer structure according to claim 20 or 21.

24. A method for recovering a multi-layer structure, comprising the steps of crushing the multi-layer structure according to claim 20 or 21 and then melt-molding the crushed multi-layer structure.

25. A method for producing a multilayer film according to any one of claims 1 to 16, comprising the steps of melt-kneading an ethylene-vinyl alcohol copolymer (a1) and a polyvalent metal ion (a2) to obtain pellets of a resin composition (A), and melt-molding the pellets of the resin composition (A) to form a layer (X).

Citation Information

Patent Citations

  • Resin composition

    JP1985238345A

  • Ethylene vinyl alcohol composition containing a metal carboxylate salt

    JP2012504689A

  • Epoxy-terminated polybutadiene as an oxygen scavenger

    JP2017511747A

  • Silage film

    JP2018062115A

  • Multilayer film and multilayer structure using the same

    JP7025605B1