Electrode for lithium secondary battery, manufacturing method therefor, and lithium secondary battery including electrode

The electrode for lithium secondary batteries, featuring a porous layer with a specific copolymer and inorganic fine particles, addresses the stability issues at high temperatures by providing dense bonding and flexibility, thereby enhancing durability and safety.

WO2024225634A1PCT designated stage expired Publication Date: 2024-10-31LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004167
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-28
Filing Date
2024-04-01
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Lithium secondary batteries face issues with stability and longevity at high temperatures due to extreme heat shrinkage of porous separators, leading to potential short circuits between the anode and cathode, which can cause explosions.

Method used

An electrode for lithium secondary batteries is developed with a porous layer containing a polymer binder comprising a copolymer with a hard segment and a soft segment, along with inorganic fine particles, which provides dense bonding and high flexibility, enhancing durability during charging and discharging.

Benefits of technology

The electrode exhibits excellent durability and stability at high temperatures, reducing the risk of short circuits and improving the overall performance and safety of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004167_31102024_PF_FP_ABST
    Figure KR2024004167_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an electrode for a lithium secondary battery, a manufacturing method therefor, and a lithium secondary battery including the electrode. According to the present invention, provided are an electrode for a lithium secondary battery, a manufacturing method therefor, and a lithium secondary battery including the electrode, in which the electrode exhibits excellent durability during charging and discharging, since a porous layer and an electrode active material layer are tightly bound to each other and the porous layer also has high flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode for lithium secondary battery, method for manufacturing same, and lithium secondary battery including same

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority to Republic of Korea Patent Application No. 10-2023-0053337, filed April 24, 2023, and Republic of Korea Patent Application No. 10-2024-0042820, filed March 28, 2024, the entire contents of which are incorporated herein by reference.

[0003]

[0004] The present invention relates to an electrode for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery including the same.

[0005]

[0006] With the recent technological development and increasing demand for mobile devices, the demand for rechargeable secondary batteries as an energy source is rapidly increasing. Consequently, extensive research is being conducted on secondary batteries that can meet diverse needs. Furthermore, secondary batteries are attracting attention as power sources for electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), which are being proposed as solutions to address air pollution caused by existing gasoline and diesel vehicles that use fossil fuels.

[0007] Lithium secondary batteries can experience extreme heat generation and explosion when a short circuit occurs due to contact between the positive and negative electrodes. Porous separators have been applied to lithium arch batteries to address this issue. However, due to their material properties and the manufacturing process, which involves stretching, porous separators in secondary batteries exhibit extreme thermal shrinkage at temperatures above approximately 100°C, potentially causing a short circuit between the positive and negative electrodes.

[0008] Accordingly, research is needed on lithium secondary batteries that can implement stability and long battery life characteristics at high temperatures and include a separator with excellent coating properties.

[0009]

[0010] The present invention provides an electrode for a lithium secondary battery having excellent bonding durability between a porous layer and an electrode substrate.

[0011] The present invention provides a method for manufacturing an electrode for a lithium secondary battery.

[0012] And, the present invention provides a lithium secondary battery including the electrode.

[0013]

[0014] According to one embodiment of the invention,

[0015] It includes an electrode active material layer and a porous layer laminated on an electrode current collector layer,

[0016] The porous layer comprises a polymer binder including a copolymer including a hard segment of the following chemical formula 1 and a soft segment of the following chemical formula 2, and inorganic fine particles dispersed on the polymer binder.

[0017] An electrode for a lithium secondary battery is provided:

[0018] [Chemical Formula 1]

[0019]

[0020] In the above chemical formula 1,

[0021] R 1 and R 3 are each independently , , or and; A 1 Inland A 3 are each independently hydrogen or an alkyl group having 1 to 3 carbon atoms; L 1 is a chemical bond or a methylene group;

[0022] R2 is an alkylene group having 1 to 5 carbon atoms;

[0023] [Chemical Formula 2]

[0024]

[0025] In the above chemical formula 2,

[0026] R 4 is an alkylene group having 3 to 6 carbon atoms.

[0027]

[0028] According to another embodiment of the invention,

[0029] A step of forming an electrode active material layer by applying an electrode material composition including an electrode active material on an electrode current collector layer;

[0030] A step of preparing an inorganic fine particle dispersion by dispersing inorganic fine particles and a dispersant in a solvent;

[0031] A step of preparing a binder solution by dissolving a polymer binder including a copolymer including a hard segment of the above chemical formula 1 and a soft segment of the above chemical formula 2 in a solvent;

[0032] A step of preparing a slurry for forming a porous layer by mixing the binder solution into the inorganic fine particle dispersion; and

[0033] A step of forming a porous layer by applying the slurry for forming the porous layer on the electrode active material layer.

[0034] A method for manufacturing an electrode for a lithium secondary battery, including the above, is provided.

[0035]

[0036] According to another embodiment of the invention, a slurry for forming a porous layer of an electrode for a lithium secondary battery is provided, the slurry comprising the polymer binder and inorganic fine particles dispersed on the polymer binder.

[0037]

[0038] According to another embodiment of the invention, a lithium secondary battery including the electrode for the lithium secondary battery is provided.

[0039]

[0040] Hereinafter, the electrode for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery including the same according to embodiments of the invention will be described in more detail.

[0041]

[0042] The terms and words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted with meanings and concepts that conform to the technical idea of ​​the invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0043] Unless otherwise defined herein, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein is for the purpose of describing specific embodiments only and is not intended to be limiting.

[0044] As used herein, the singular forms also include the plural forms unless the context clearly dictates otherwise.

[0045] As used herein, the term "including" means specifying a particular characteristic, region, integer, step, operation, element and / or component, but does not exclude the presence or addition of other particular characteristics, regions, integers, steps, operations, elements, components and / or groups.

[0046] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and scope of the invention.

[0047] In this specification, when the positional relationship between two parts is described as, for example, ‘on top of’, ‘upper part of’, ‘lower part of’, ‘next to’, etc., one or more other parts may be located between the two parts unless the expression ‘right’ or ‘directly’ is used.

[0048] In this specification, when a temporal relationship is described as, for example, ‘after’, ‘following’, ‘next to’, or ‘before’, it may also include cases where it is not continuous, unless the expression ‘immediately’ or ‘directly’ is used.

[0049] The term 'at least one' in this specification should be understood to include all possible combinations of one or more associated items.

[0050] In the present invention, when it is said that any one layer is connected to another layer “via” another layer, it means that the one layer and the other layer are connected by being laminated by the other layer interposed in at least some area between the one layer and the other layer.

[0051]

[0052] According to one embodiment of the invention,

[0053] It includes an electrode active material layer and a porous layer laminated on an electrode current collector layer,

[0054] The porous layer comprises a polymer binder including a copolymer including a hard segment of the following chemical formula 1 and a soft segment of the following chemical formula 2, and inorganic fine particles dispersed on the polymer binder.

[0055] An electrode for a lithium secondary battery is provided:

[0056] [Chemical Formula 1]

[0057]

[0058] In the above chemical formula 1,

[0059] R 1 and R 3 are each independently , , or and; A 1 Inland A 3 are each independently hydrogen or an alkyl group having 1 to 3 carbon atoms; L 1 is a chemical bond or a methylene group;

[0060] R 2 is an alkylene group having 1 to 5 carbon atoms;

[0061] [Chemical Formula 2]

[0062]

[0063] In the above chemical formula 2,

[0064] R 4 is an alkylene group having 3 to 6 carbon atoms.

[0065]

[0066] As a result of the inventors' continued research, it was confirmed that an electrode for a lithium secondary battery satisfying the above configuration can exhibit excellent durability during charge and discharge by providing high flexibility to the porous layer while ensuring dense bonding between the porous layer and the electrode active material layer.

[0067]

[0068] According to one embodiment of the invention, the electrode for the lithium secondary battery may be a negative electrode or a positive electrode.

[0069]

[0070] The electrode current collector layer may be formed of an electrode current collector known in the art to which the present invention pertains to have conductivity without causing chemical changes in a lithium secondary battery. For example, the electrode current collector may be formed of stainless steel; aluminum; nickel; titanium; sintered carbon; or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, or the like.

[0071] Preferably, the electrode current collector may have a thickness of 3 μm to 500 μm. In order to increase adhesion to the electrode material, the electrode current collector may have fine unevenness formed on its surface. The electrode current collector may have various forms, such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0072]

[0073] The above electrode active material layer includes an electrode material composition which is a mixture of an electrode active material, a conductive material, and a binder.

[0074] The above conductive material can be used to impart electronic conductivity to the electrode.

[0075] As the conductive material, any material that has electronic conductivity and does not cause a chemical change in the lithium secondary battery may be used without particular limitation. Non-limiting examples thereof include carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; graphite such as natural graphite or artificial graphite; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; or conductive polymers such as polyphenylene derivatives. The conductive material may be one or a mixture of two or more of the above-described examples.

[0076] The content of the conductive material can be adjusted within a range that exhibits an appropriate level of conductivity while not causing a decrease in the capacity of the lithium secondary battery. Preferably, the content of the conductive material may be 1 wt% to 10 wt% or 1 wt% to 5 wt% relative to the total weight of the electrode material composition.

[0077]

[0078] The above binder is used to properly attach the electrode material composition to the electrode current collector.

[0079] As non-limiting examples, the binder may be a polymer including polyvinyl alcohol, polyacrylate, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon resin, etc. The binder may be one or a mixture of two or more of the above-described examples.

[0080] The content of the binder can be adjusted within a range that exhibits an appropriate level of adhesiveness while not causing a decrease in the capacity of the lithium secondary battery. Preferably, the content of the binder may be 1 wt% to 10 wt% or 1 wt% to 5 wt% relative to the total weight of the electrode material composition.

[0081]

[0082] When the above lithium secondary battery electrode is a positive electrode, any material capable of reversible insertion and de-insertion of lithium ions can be used as the positive electrode active material without any special restrictions.

[0083] For example, the positive electrode active material may be a composite oxide or phosphate containing lithium and a metal such as cobalt, manganese, nickel, iron, or a combination thereof.

[0084] As another example, the positive electrode active material may be a compound represented by any one of the following chemical formulas: Li a A 1-b R b D2(0.90≤a≤1.8, 0≤b≤0.5); Li a E 1-b R b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); LiE 2-b R b O 4-c D c (0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b R c D d (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0 <d≤2); Li a Ni 1-b-c Co b R c O 2-d Z d (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0 <d<2); Li a Ni 1-b-c Co b R c O 2-d Z2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0 <d<2); Li a Ni 1-b-c Mn b R c D d (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0 <d≤2); Li a Ni 1-b-c Mn b R c O 2-d Z d (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0 <d<2); Li a Ni 1-b-c Mn b R c O 2-dZ2(0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0 <d<2); Li a Ni b E c G d O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1.); Li a Ni b Co c Mn d G e O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0.001≤e≤0.1); Li a NiG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a MnG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn2G b O4(0.90≤a≤1.8, 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiTO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2); Li (3-f) Fe2(PO4)3(0≤f≤2); and LiFePO4.

[0085] In the above chemical formula, A is Ni, Co, Mn or a combination thereof; R is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; Z is F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; T is Cr, V, Fe, Sc, Y or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0086] A positive electrode active material having a coating layer on the surface thereof may also be used, or a positive electrode active material having a coating layer may be mixed and used. As the coating element included in the coating layer, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof may be used.

[0087] According to one embodiment, the positive electrode active material may be included in an amount of 80 wt% to 95 wt% based on the total weight of the electrode material composition. Preferably, the content of the positive electrode active material may be 82 wt% to 95 wt%, or 82 wt% to 93 wt%, or 85 wt% to 93 wt%, or 85 wt% to 90 wt% based on the total weight of the electrode material composition.

[0088]

[0089] When the electrode for the above lithium secondary battery is a negative electrode, the negative electrode active material may include a material capable of reversibly intercalating and deintercalating lithium ions, a lithium metal, an alloy of a lithium metal, a material capable of doping and dedoping lithium, and a transition metal oxide.

[0090] Examples of the material capable of reversibly intercalating and deintercalating the lithium ions include carbonaceous materials such as crystalline carbon, amorphous carbon, or mixtures thereof. Specifically, the carbonaceous material may be natural graphite, artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitches, mesophase pitch-based carbon fiber, meso-carbon microbeads, petroleum or coal tar pitch derived cokes, soft carbon, and hard carbon.

[0091] The above lithium metal alloy may be an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, Sn, Bi, Ga, and Cd.

[0092] The above lithium doping and dedoping materials include Si, Si-C complex, SiOx (0 <x<2), Si-Q 합금(상기 Q는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 15족 원소, 16족 원소, 전이 금속, 희토류 원소, 및 이들의 조합으로 이루어진 군에서 선택되는 원소이다; 단, Si는 제외한다), Sn, SnO2, Sn-R 합금(상기 R은 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 15족 원소, 16족 원소, 전이 금속, 희토류 원소, 및 이들의 조합으로 이루어진 군에서 선택되는 원소이다; 단, Sn은 제외한다.) 등일 수 있다. 그리고, 상기 리튬에 도프 및 탈도프 가능한 물질로는 상기 예들 중 적어도 하나와 SiO2를 혼합하여 사용할 수 있다. 상기 Q 및 R은 Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po 등일 수 있다.

[0093] And, the transition metal oxide may be vanadium oxide, lithium vanadium oxide, lithium titanium oxide, etc.

[0094] Preferably, the negative electrode active material may include at least one compound selected from the group consisting of carbonaceous materials and silicon compounds. Here, the carbonaceous material is at least one material selected from the group consisting of natural graphite, artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch, mesophase pitch-based carbon fiber, carbon microspheres, petroleum or coal-based coke, softened carbon, and hardened carbon, as exemplified above. And, the silicon compound is a compound including Si as exemplified above, i.e., Si, Si-C composite, SiOx (0 <x<2), 상기 Si-Q 합금, 이들의 혼합물, 또는 이들 중 적어도 하나와 SiO2의 혼합물일 수 있다.

[0095] According to one embodiment, the negative active material may be included in an amount of 85 wt% to 98 wt% based on the total weight of the electrode material composition. Preferably, the content of the negative active material may be 85 wt% to 97 wt%, or 87 wt% to 97 wt%, or 87 wt% to 95 wt%, or 90 wt% to 95 wt% based on the total weight of the negative electrode material.

[0096]

[0097] According to one embodiment, the thickness of the electrode active material layer is preferably controlled in the range of 5 µm to 500 µm, or 5 µm to 450 µm, or 10 µm to 450 µm to achieve appropriate performance.

[0098]

[0099] Meanwhile, the electrode for the lithium secondary battery includes a porous layer laminated on an electrode current collector layer.

[0100] According to one embodiment, the porous layer comprises a polymer binder and inorganic fine particles dispersed on the polymer binder.

[0101] In particular, the polymer binder comprises a copolymer including a hard segment of the following chemical formula 1 and a soft segment of the following chemical formula 2:

[0102] [Chemical Formula 1]

[0103]

[0104] In the above chemical formula 1,

[0105] R 1 and R 3 are each independently , , or and; A 1 Inland A 3 are each independently hydrogen or an alkyl group having 1 to 3 carbon atoms; L 1 is a chemical bond or a methylene group;

[0106] R 2 is an alkylene group having 1 to 5 carbon atoms;

[0107] [Chemical Formula 2]

[0108]

[0109] In the above chemical formula 2,

[0110] R 4 is an alkylene group having 3 to 6 carbon atoms.

[0111]

[0112] The copolymer has a hard segment capable of hydrogen bonding with the electrode active material layer and a soft segment that imparts high flexibility to the copolymer. Accordingly, the porous layer and the electrode active material layer are tightly bonded, while the porous layer is imparted with high flexibility, thereby exhibiting excellent durability during charge and discharge.

[0113]

[0114] In the above copolymer, the R 1 and R 3 are each independently , , or am.

[0115] Here, the above A 1 Inland A 3 are each independently hydrogen or an alkyl group having 1 to 3 carbon atoms, and L 1 is a chemical bond or a methylene group. Preferably, the above A 1 Inland A 3 Each of them can be hydrogen, a methyl group, or an ethyl group. Preferably, the L 1 may be a methylene group.

[0116]

[0117] In one embodiment, the R 1 and R 3 may have the above structures derived from 4,4'-diphenylmethane diisocyanate (4,4'-MDI), 1,4-phenylene diisocyanate, 1,3-phenylene diisocyanate, 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), or 1,5-naphthalene diisocyanate, respectively.

[0118] In one embodiment, the R 1 and R 3 are each independently , , , , , , or It could be.

[0119] In one embodiment, the R 1 and R 3 are derived from 4,4'-diphenylmethane diisocyanate (4,4'-MDI), respectively. It can have a structure.

[0120]

[0121] In the above copolymer, the R 2 is an alkylene group having 1 to 5 carbon atoms. According to one embodiment, the R 2may have the above structure derived from methylene diamine, ethylene diamine, 1,3-diaminopropane, 1,4-diaminobutane, or 1,5-diaminopentane. Preferably, the R 2 may be a methylene group (*-CH2-*), an ethylene group (*-CH2-CH2-*), or a propylene group (*-CH2-CH2-CH2-*). According to one embodiment, the R 2 It may have a structure of an ethylene group (*-CH2-CH2-*) derived from ethylene diamine (EDA).

[0122]

[0123] In the above chemical formula 2, the R 4 is an alkylene group having 3 to 6 carbon atoms. Preferably, the R 4 may be a propylene group (*-CH2-CH2-CH2-*) or a butylene group (*-CH2-CH2-CH2-CH2-*). According to one embodiment, the R 4 may have the above structure derived from polytrimethylene ether glycol or polytetramethylene ether glycol. In one embodiment, the R 4 It may have a structure of a butylene group (*-CH2-CH2-CH2-CH2-*) derived from polytetramethylene ether glycol (PTMEG).

[0124]

[0125] As a non-limiting example, the copolymer may comprise R in the hard segment of the above chemical formula 1. 1 and R 3 Each of which is derived from 4,4'-diphenylmethane diisocyanate (4,4'-MDI). The structure is R 2 is the structure of an ethylene group (*-CH2-CH2-*) derived from ethylene diamine (EDA); in the soft segment of the above chemical formula 2, the R 4It may be a copolymer having a structure of butylene groups (*-CH2-CH2-CH2-CH2-*) derived from polytetramethylene ether glycol (PTMEG).

[0126]

[0127] According to one embodiment, the copolymer may comprise the hard segment and the soft segment in a molar ratio of 80:20 to 95:5.

[0128] In order to ensure adhesion to the electrode active material layer while imparting appropriate mechanical properties to the polymer binder including the copolymer, the molar ratio of the hard segment to the soft segment is preferably 80:20 or more. In addition, in order to impart high flexibility to the porous layer, the molar ratio of the hard segment to the soft segment is preferably 95:5 or less.

[0129] Specifically, the molar ratio of the hard segment and the soft segment may be 80:20 or more or 85:15 or more; and 95:5 or less or 90:10 or less.

[0130] Preferably, the molar ratio of the hard segment and the soft segment may be 80:20 to 95:5, or 85:15 to 95:5, or 85:15 to 90:10.

[0131]

[0132] In one embodiment, the copolymer has a weight average molecular weight (Mw) of 100,000 g / mol to 1,000,000 g / mol.

[0133] In order to realize the improvement effect according to the application of the copolymer, the weight average molecular weight (Mw) of the copolymer may be 100,000 g / mol or more, or 150,000 g / mol or more; and 1,000,000 g / mol or less, or 800,000 g / mol or less, or 600,000 g / mol or less, or 400,000 g / mol or less. Preferably, the weight average molecular weight (Mw) of the copolymer is 100,000 g / mol to 1,000,000 g / mol; or 150,000 g / mol to 1,000,000 g / mol; or 150,000 g / mol to 800,000 g / mol; or 150,000 g / mol to 600,000 g / mol; Alternatively, it may be 150,000 g / mol to 400,000 g / mol.

[0134] As a non-limiting example, the weight average molecular weight (Mw) can be measured using an Agilent PL-GPC 220 instrument equipped with a 300 mm long PolarGel MIXED-L column (Polymer Laboratories). The measurement temperature is 65°C, tetrahydrofuran or dimethylformamide is used as a solvent, and the flow rate is measured at a rate of 1 mL / min. The sample is prepared at a concentration of 10 mg / 10 mL and then supplied in an amount of 100 μL. The Mw and Mn values ​​are derived with reference to a calibration curve formed using polystyrene standards. The molecular weights (g / mol) of the polystyrene standards are 8 types: 580 / 3,940 / 8,450 / 31,400 / 70,950 / 316,500 / 956,000 / 4,230,000.

[0135]

[0136] According to one embodiment, the copolymer may be manufactured to meet the above-described structure and weight average molecular weight or may be applied to a commercial product (e.g., spandex, etc.).

[0137]

[0138] And, the polymer binder is polyetherimide, polyvinylidene fluoride, poly(vinylidene fluoride-co-trichloroethylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), poly(vinylidene fluoride-co-trifluoroethylene), poly(vinylidene fluoride-co-tetrafluoroethylene), poly(vinylidene fluoride-co-hexafluoropropylene), butylacrylate, polymethylmethacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene vinyl acetate copolymer, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethylated polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, It may further include at least one compound selected from the group consisting of acrylonitrile-styrene-butadiene copolymers, ethylene-propylene-diene terpolymers, sulfonated ethylene-propylene-diene terpolymers, styrene butadiene rubbers, fluoroelastomers, and polyimides.

[0139]

[0140] According to one embodiment, in order to enable the improvement effect to be expressed by application of the copolymer, the polymer binder is preferably included in an amount of 10 wt% or more, or 10 wt% to 100 wt%, or 30 wt% to 100 wt%, or 50 wt% to 100 wt%, based on the total weight of the polymer binder including the copolymer including the hard segment of the chemical formula 1 and the soft segment of the chemical formula 2.

[0141]

[0142] The above inorganic fine particles form micropores due to empty spaces between particles, maintain their physical form at high temperatures, and are electrochemically stable.

[0143] It is preferable that the above-mentioned inorganic fine particles do not undergo oxidation and / or reduction reactions within the operating voltage range of the secondary battery (e.g., 0 to 5 V based on Li / Li+). It is preferable that the above-mentioned inorganic fine particles have a high electrolyte ion transfer capability. In order to be well dispersed within the polymer binder, it is preferable that the above-mentioned inorganic fine particles have as low a density as possible. In addition, in order to contribute to increasing the dissociation of the electrolyte salt within the electrolyte, it is preferable that the above-mentioned inorganic fine particles have a high dielectric constant.

[0144] Preferably, the inorganic fine particles may be at least one selected from the group consisting of inorganic particles having a dielectric constant of 1 or more, inorganic particles having piezoelectricity, and inorganic particles having lithium ion transfer capability.

[0145] For example, inorganic particles such as SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, boehmite (AlO(OH)), Al(OH)3, TiO2, and SiC have a dielectric constant of 1 or greater and can be preferably applied as the inorganic fine particles.

[0146] As another example, the piezoelectric inorganic particle is a material that is an insulator at normal pressure, but exhibits conductivity due to a change in its internal structure when a certain pressure is applied. The piezoelectric inorganic particle has a high dielectric constant of 100 or more. In addition, when the piezoelectric inorganic particle is stretched or compressed by applying a certain pressure, a charge is generated, so that one side is charged positively (+) and the opposite side is charged negatively (-), thereby generating a potential difference between the two sides. Due to the above-described characteristics of the piezoelectric inorganic particle, when an internal short circuit occurs in the electrode of a secondary battery due to an external impact, direct contact between the positive and negative electrodes can be prevented, and a gradual decrease in voltage and improved safety can be achieved. Examples of the piezoelectric inorganic particle include BaTiO3, Pb(Zr,Ti)O3(PZT), Pb1-x La x Zr 1-y Ti y O3(PLZT), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), and inorganic particles such as HfO2 can be preferably applied.

[0147] As another example, the inorganic particles having the lithium ion transport capability refer to inorganic particles that contain lithium elements but have the function of transporting lithium ions without storing lithium. The inorganic particles having the lithium ion transport capability enable improvement of lithium ion conductivity in a battery. Such inorganic particles include Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x< 2, 0<y<1, 0<z<3), (LiAlTiP) x O y (0 <x<4, 0<y<13), Li x La y TiO3(0 <x<2, 0<y<3), Li x Ge y P z S w (0 <x<4, 0<y<1, 0<z<1, 0<w<5), Li x N y (0 <x<4, 0<y<2), Li x Si y S z (0 <x<3, 0<y<2, 0<z< 4), 및 Li x P y S z (0 <x<3, 0<y<3, 0<z<7) 와 같은 무기 입자를 예로 들 수 있다.

[0148] Preferably, the inorganic fine particles are SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, AlO(OH), Al(OH)3, TiO2, SiC, BaTiO3, Pb(Zr,Ti)O3, Pb 1-x La x Zr 1-y Ti y O3, Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3, HfO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x< 2, 0<y<1, 0<z<3), (LiAlTiP) x O y (0 <x<4, 0<y<13), Li x La y TiO3(0 <x<2, 0<y<3), Li x Ge y P z S w (0 <x<4, 0<y<1, 0<z<1, 0<w<5), Li x N y (0 <x<4, 0<y<2), Li x Si y S z (0 <x<3, 0<y<2, 0<z< 4), 및 Li x P y S z (0 <x<3, 0<y<3, 0<z<7)로 이루어진 군에서 선택된 1종 이상일 수 있다.

[0149] The above-mentioned inorganic fine particles preferably have a particle size of 0.001 ㎛ to 10 ㎛. In order to secure dispersibility in the above-mentioned porous layer, the above-mentioned inorganic fine particles preferably have a particle size of 0.001 ㎛ or more. However, if the particle size of the above-mentioned inorganic fine particles is too large, the thickness of the above-mentioned porous layer increases, resulting in a deterioration in mechanical properties, and an excessively large pore size may cause an internal short circuit during charging and discharging of the secondary battery. Therefore, the above-mentioned inorganic fine particles preferably have a particle size of 10 ㎛ or less.

[0150]

[0151] According to one embodiment, the porous layer may comprise 0.5 to 45 wt% of the polymer binder and 55 to 99.5 wt% of the inorganic fine particles.

[0152] In order to provide the porous layer with an appropriate porosity and insulation, the inorganic fine particles are preferably included in an amount of 55 wt% or more, or 60 wt% or more, or 65 wt% or more, or 70 wt% or more, or 75 wt% or more, or 80 wt% or more. However, if the inorganic fine particles are included in an excessive amount, the mechanical properties of the porous layer may deteriorate due to weakened adhesiveness. Therefore, the inorganic fine particles are preferably included in an amount of 99.5 wt% or less, or 99 wt% or less, or 95 wt% or less.

[0153] Specifically, the porous layer may comprise 55 to 99.5 wt%, or 60 to 99.5 wt%, or 65 to 99.5 wt%, or 70 to 99.5 wt%, or 75 to 99.5 wt%, or 80 to 99.5 wt%, or 80 to 99 wt%, or 80 to 95 wt% of the inorganic fine particles and the remainder of the polymer binder.

[0154]

[0155] According to one embodiment, the porosity of the porous layer may be 40 to 80%.

[0156] In terms of securing lithium ion permeability, the porosity of the porous layer is preferably 40% or more, or 45% or more, or 50% or more. However, if the porosity of the porous layer is too large, it may be difficult to secure adhesion between the porous layer and the electrode, and an internal short circuit may occur during charging and discharging of the lithium secondary battery. Therefore, the porosity of the porous layer is preferably 80% or less, or 75% or less, or 70% or less.

[0157] Specifically, the porosity of the porous layer may be 40 to 80%, or 45 to 80%, or 45 to 75%, or 50 to 75%, or 50 to 70%.

[0158] The above porosity can be measured by preparing the slurry for forming the porous layer and then applying it to a release film to produce an independent porous layer. In other words, the composition and process conditions that can secure the porosity in the above range can be established experimentally and applied to actual manufacturing.

[0159] The porosity can be measured using a scanning electron microscope (SEM) image, using an adsorbed gas such as nitrogen and a BET device, or using a method such as mercury intrusion porosimetry or capillary flowporosimetry. Alternatively, the porosity can be calculated from the thickness, weight, and theoretical density of the obtained porous layer.

[0160]

[0161] The porous layer preferably has a porosity within an appropriate range to achieve the desired characteristics. If the porosity of the porous layer is too high, an internal short circuit may occur during charging and discharging of the lithium secondary battery. Therefore, the porosity of the porous layer is preferably 60% or less.

[0162]

[0163] According to one embodiment, the thickness of the porous layer is preferably controlled in the range of 5 μm to 100 μm, or 5 μm to 50 μm, or 10 μm to 50 μm to achieve appropriate performance.

[0164]

[0165] Meanwhile, an interface layer in which an electrode material composition included in the electrode active material layer and a porous composition included in the porous layer are mixed may exist in the entire area between the electrode active material layer and the porous layer.

[0166] For example, the interfacial layer is a layer composed of the electrode material composition in an amount of more than 0 wt% and less than 100 wt% and the porous composition in an amount of less than 100 wt% and more than 0 wt%.

[0167]

[0168]

[0169] According to another embodiment of the invention,

[0170] A step of forming an electrode active material layer by applying an electrode material composition including an electrode active material on an electrode current collector layer;

[0171] A step of preparing an inorganic fine particle dispersion by dispersing inorganic fine particles and a dispersant in a solvent;

[0172] A step of preparing a binder solution by dissolving a polymer binder including a copolymer including a hard segment of the above chemical formula 1 and a soft segment of the above chemical formula 2 in a solvent;

[0173] A step of preparing a slurry for forming a porous layer by mixing the binder solution into the inorganic fine particle dispersion; and

[0174] A step of forming a porous layer by applying the slurry for forming the porous layer on the electrode active material layer.

[0175] A method for manufacturing an electrode for a lithium secondary battery according to the above is provided.

[0176]

[0177] The electrode for a lithium secondary battery described above can be provided through the above manufacturing method.

[0178] First, a step of forming an electrode active material layer by applying an electrode material composition including an electrode active material onto an electrode current collector layer may be performed. In this step, the electrode current collector and the electrode material composition are each replaced with the previously described content. The electrode active material layer may be formed by applying the electrode material composition onto the electrode current collector layer and drying it.

[0179]

[0180] Separately from the above steps, a step of preparing an inorganic fine particle dispersion by dispersing inorganic fine particles and a dispersant in a solvent; a step of preparing a binder solution by dissolving a polymer binder in a solvent; and a step of preparing a slurry for forming a porous layer by mixing the binder solution into the inorganic fine particle dispersion may be performed.

[0181] The inventors' ongoing research has revealed that, when preparing the slurry for forming the porous layer, the order and method of mixing the components can affect the agglomeration of the inorganic fine particles and the distribution of the polymer binder and inorganic fine particles. Furthermore, it has been confirmed that the distribution of the polymer binder and inorganic fine particles can significantly impact the bonding strength of the porous layer and the electrode active material layer.

[0182] For example, when preparing a slurry for forming a porous layer by preparing a binder solution by dissolving a polymer binder in a solvent and then adding inorganic fine particles thereto, the dispersibility of the inorganic fine particles is significantly reduced, making it impossible to provide an electrode for a lithium secondary battery that satisfies the above characteristics.

[0183] According to one embodiment, the manufacturing method of the present invention is performed by the steps of preparing the inorganic fine particle dispersion; preparing the binder solution; and preparing a slurry for forming a porous layer by mixing the binder solution with the inorganic fine particle dispersion, thereby providing an electrode for a lithium secondary battery in which the porous layer and the electrode active material layer are densely bonded while the porous layer is provided with high flexibility.

[0184] In the above steps, the inorganic fine particles and polymer binder are replaced with the previously described contents.

[0185] As the above dispersant, a compound known to be suitable for dispersing inorganic fine particles in the technical field to which the present invention pertains, such as a carboxylic acid-modified polyester copolymer and acetic acid, can be used.

[0186] And, a non-aqueous organic solvent can be used as the solvent. Specifically, the non-aqueous organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether and tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as N-methyl-2-pyrrolidone (NMP), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, which may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolane. Among the above examples, the carbonate-based solvent suitable for dispersing inorganic fine particles in the non-aqueous organic solvent can be preferably used.

[0187]

[0188] According to one embodiment, the slurry for forming the porous layer preferably has a solid content including the inorganic fine particles of 30 wt% to 95 wt%.

[0189] If the solid content of the porous slurry is too high, it may cause an increase in viscosity, which may prevent it from easily penetrating into the pore region of the electrode active material layer, and thus prevent an interface layer (25) with an appropriate structure from being formed. However, if the solid content of the porous slurry is too low, a pin-hole phenomenon may occur when applied onto the electrode active material layer.

[0190] Specifically, the solids content of the porous slurry may be 30 wt% or more, or 35 wt% or more, and 95 wt% or less, or 90 wt% or less. Preferably, the solids content of the porous slurry may be 30 wt% to 95 wt%, or 30 wt% to 90 wt%, or 35 wt% to 90 wt%.

[0191]

[0192] Next, a step of forming a porous layer by applying the slurry for forming a porous layer onto the electrode active material layer is performed. The porous layer can be formed by applying the slurry for forming a porous layer onto the electrode active material layer and drying it. This step can be performed taking into account the thickness of the electrode active material layer and the porous layer described above.

[0193]

[0194] In the above steps, drying is preferably performed at a temperature of 50°C to 150°C, or 60°C to 150°C, or 60°C to 120°C, or 65°C to 110°C, respectively. If the drying temperature does not meet the above range, the drying efficiency may decrease or the shape of each layer may change, resulting in defects.

[0195]

[0196]

[0197] According to another embodiment of the invention, a slurry for forming a porous layer of an electrode for a lithium secondary battery is provided, the slurry comprising the polymer binder and inorganic fine particles dispersed on the polymer binder.

[0198] In the slurry for forming the above porous layer, the polymer binder and the inorganic fine particles are each replaced with the contents described above.

[0199] The slurry for forming the porous layer can be obtained through the steps of preparing an inorganic fine particle dispersion liquid by dispersing inorganic fine particles and a dispersant in a solvent as described above; preparing a binder solution by dissolving a polymer binder including a copolymer including the hard segment of the chemical formula 1 and the soft segment of the chemical formula 2 in a solvent; and preparing a slurry for forming the porous layer by mixing the binder solution into the inorganic fine particle dispersion liquid.

[0200]

[0201] According to another embodiment of the invention, a lithium secondary battery including the above-described electrode is provided.

[0202] For example, the lithium secondary battery may include an electrode assembly including a counter electrode disposed on a porous layer of the electrode; an electrolyte impregnated in the electrode assembly; and a battery case that seals and houses the electrode assembly and the electrolyte.

[0203] The above lithium secondary battery can exhibit excellent durability and stable performance by having the above-described electrode assembly.

[0204] The above lithium secondary battery can have various shapes such as square, cylindrical, and pouch shapes.

[0205] The above lithium secondary battery can be used as an energy source with improved performance and safety in the field of portable electronic devices such as mobile phones, laptop computers, tablet computers, mobile batteries, and digital cameras; and in the field of transportation means such as electric vehicles, electric motorcycles, and personal mobility devices.

[0206]

[0207] According to one embodiment, the electrolyte may be used without particular limitation as long as it is known in the technical field to which the present invention pertains to be applicable to lithium secondary batteries. For example, the electrolyte may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc.

[0208] Specifically, the electrolyte may include a non-aqueous organic solvent and a lithium salt.

[0209] Any non-aqueous organic solvent that can serve as a medium through which ions involved in the electrochemical reaction of the battery can move may be used without any particular restrictions.

[0210] Specifically, the non-aqueous organic solvent includes ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether and tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); Alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched or cyclic hydrocarbon group, which may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolane.

[0211] Among the above examples, a carbonate solvent can be preferably used as the non-aqueous organic solvent.

[0212] In particular, considering the charge / discharge performance of the battery and compatibility with the positive electrode material, a mixture of a cyclic carbonate (e.g., ethylene carbonate, propylene carbonate) having high ionic conductivity and high dielectric constant and a linear carbonate (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate) having low viscosity can be preferably used as the non-aqueous organic solvent. In this case, mixing and using the cyclic carbonate and the linear carbonate in a volume ratio of 1:1 to 1:9 can be advantageous for exhibiting the above-described performance.

[0213] In addition, as the non-aqueous organic solvent, a mixture of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 1:2 to 1:10; or a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 1 to 3:1 to 9:1 can be preferably used.

[0214] The lithium salt included in the electrolyte is dissolved in the non-aqueous organic solvent and acts as a source of lithium ions within the battery, enabling the basic operation of a lithium secondary battery and promoting the movement of lithium ions between the positive and negative electrodes.

[0215] Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiFSI, LiTFSI, LiCl, LiI, and LiB(C2O4)2, etc. Preferably, the lithium salt may be LiPF6, LiFSI, LiTFSI, and mixtures thereof.

[0216] The lithium salt may be included in the electrolyte at a concentration of 0.1 M to 2.0 M. The lithium salt included in the above concentration range enables the electrolyte to exhibit excellent electrolyte performance by providing appropriate conductivity and viscosity to the electrolyte.

[0217] Optionally, the electrolyte may include additives for the purpose of improving the life characteristics of the battery, suppressing battery capacity reduction, and improving the discharge capacity of the battery.

[0218] For example, the additive may be a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, a cyclic ether, ethylene diamine, n-glyme, hexaphosphoric acid triamide, a nitrobenzene derivative, sulfur, a quinone imine dye, an N-substituted oxazolidinone, an N,N-substituted imidazolidine, an ethylene glycol dialkyl ether, an ammonium salt, a pyrrole, 2-methoxyethanol, aluminum trichloride, or the like. The additive may be included in an amount of 0.1 wt% to 5 wt% based on the total weight of the electrolyte.

[0219]

[0220] According to the present invention, an electrode for a lithium secondary battery, in which a porous layer and an electrode active material layer are tightly bonded while the porous layer is provided with high flexibility, thereby exhibiting excellent durability during charge and discharge, a method for manufacturing the same, and a lithium secondary battery including the electrode are provided.

[0221]

[0222] Figure 1 is a scanning electron microscope (SEM) image of an electrode for a lithium secondary battery according to Example 1.

[0223] Figure 2 is an SEM image of an electrode for a lithium secondary battery according to Example 2.

[0224] Figure 3 is an SEM image of an electrode for a lithium secondary battery according to Example 3.

[0225] Figure 4 is an SEM image of an electrode for a lithium secondary battery according to Example 4.

[0226] Figure 5 is an SEM image of an electrode for a lithium secondary battery according to Example 5.

[0227] Figure 6 is an SEM image of an electrode for a lithium secondary battery according to Comparative Example 1.

[0228] Figure 7 is an SEM image of an electrode for a lithium secondary battery according to Comparative Example 1.

[0229]

[0230] The following specific examples of the invention will illustrate its functions and effects in greater detail. However, these examples are provided solely to aid understanding of the invention. The following examples are not intended to limit the scope of the invention in any way, and it will be apparent to those skilled in the art that various modifications and variations are possible within the scope and spirit of the invention.

[0231]

[0232] Example 1

[0233] An electrode material composition was prepared, comprising 95.6 wt% of an active material composed of 90 wt% of a graphite active material in which artificial graphite and natural graphite are mixed in a ratio of 3:7 and 10 wt% of SiO; 1 wt% of acetylene black as a conductive material; and 1.1 wt% of carboxymethyl cellulose (CMC) and 2.3 wt% of styrene butadiene rubber (SBR) as binders. The electrode material composition was applied to one side of a copper current collector having a thickness of 8 μm using a comma coater. This was dried and rolled at 130°C to prepare an anode plate having a laminated anode active material layer. The anode active material layer was formed with a porosity of 24% and a thickness of 44 μm.

[0234] An inorganic fine particle dispersion having a solid content of 40% was prepared by mixing inorganic fine particles, AlO(OH), and a dispersant (BYK, DISPERBYK-111) in N-methyl-2-pyrrolidone (NMP). The particle diameter (D60) of the inorganic fine particles measured using a particle size analyzer was analyzed to be 400 nm.

[0235] A 10 wt% binder solution was prepared by mixing spandex (weight average molecular weight 200,000 g / mol) and poly(vinylidene fluoride-co-hexafluoropropylene) (PVdF-HFP) as a polymer binder in a weight ratio of 50:50 and dissolving them in NMP.

[0236] Here, the spandex is a block copolymer composed of a hard segment of the chemical formula 1 and a soft segment of the chemical formula 2. The spandex is a block copolymer composed of a hard segment of the chemical formula 1 and a soft segment of the chemical formula 2. 1 and R 3 Each of which is derived from 4,4'-diphenylmethane diisocyanate (4,4'-MDI). The structure is R 2 is the structure of an ethylene group (*-CH2-CH2-*) derived from ethylene diamine (EDA); in the soft segment of the above chemical formula 2, the R 4 It is a copolymer having a structure of butylene groups (*-CH2-CH2-CH2-CH2-*) derived from polytetramethylene ether glycol (PTMEG). In the above spandex, the molar ratio of the hard segment and the soft segment is 85:15.

[0237] A slurry for forming a porous layer was obtained by uniformly mixing the inorganic fine particle dispersion and the binder solution using a homogenizer mixer.

[0238] The slurry for forming the porous layer was applied onto the negative electrode active material layer and then dried at 130°C to obtain a negative electrode plate in which a porous layer was formed on the negative electrode active material layer. The composition of the porous layer was 90 wt% of the inorganic fine particles and 10 wt% of the polymer binder. The porous layer was formed to have a thickness of 20 μm.

[0239] The above negative electrode plate was punched to a size of 31 x 43 mm using a die puncher to prepare a negative electrode portion.

[0240]

[0241] A slurry was prepared by uniformly dispersing a mixture of 94 wt% LiNiCoMnO2 (Ni:Co:Mn=8:1:1) as a cathode active material, 3 wt% conductive carbon black (Super P; IMERYS Graphite & Carbon) as a conductive material, and 3 wt% polyvinylidene fluoride as a binder in NMP. The slurry was applied to one surface of an aluminum current collector, dried, and rolled to prepare a cathode plate having a layer of cathode active material laminated thereon. The cathode plate was punched into a size of 30 x 42 mm using a die puncher to prepare a cathode part.

[0242]

[0243] An electrode assembly was manufactured by placing the positive electrode active material layer of the positive electrode portion in contact with the porous layer of the negative electrode portion.

[0244] The above electrode assembly was placed in a pouch to form a small cell, and an electrolyte was injected into the pouch to manufacture five lithium secondary batteries.

[0245] At this time, the electrolyte used was a non-aqueous organic solvent containing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) mixed in a volume ratio of 3:7, in which 1.0 M LiPF6 and 2 wt% vinylene carbonate (VC) were dissolved.

[0246]

[0247] Example 2

[0248] A negative electrode part, a positive electrode part, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that only the spandex was used instead of the mixture of the spandex and PVdF-HFP as the polymer binder.

[0249]

[0250] Example 3

[0251] A negative electrode part, a positive electrode part, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the composition of the slurry for forming the porous layer was adjusted so that the composition of the porous layer was 92 wt% of the inorganic fine particles and 8 wt% of the polymer binder.

[0252]

[0253] Example 4

[0254] A negative electrode part, a positive electrode part, and a lithium secondary battery were manufactured in the same manner as in Example 3, except that only the spandex was used instead of the mixture of the spandex and PVdF-HFP as the polymer binder.

[0255]

[0256] Example 5

[0257] A negative electrode part, a positive electrode part, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the composition of the slurry for forming the porous layer was adjusted so that the composition of the porous layer was 85 wt% of the inorganic fine particles and 15 wt% of the polymer binder.

[0258]

[0259] Comparative Example 1

[0260] A negative electrode part, a positive electrode part, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that a mixture of polyetherimide and PVdF-HFP in a weight ratio of 50:50 was used instead of the mixture of spandex and PVdF-HFP as the polymer binder.

[0261]

[0262] Comparative Example 2

[0263] A negative electrode part, a positive electrode part, and a lithium secondary battery were manufactured in the same manner as in Example 1, except that only PVdF-HFP was used instead of the mixture of spandex and PVdF-HFP as the polymer binder.

[0264]

[0265] Experimental Example 1

[0266] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the copolymer manufactured in the above manufacturing example were measured using gel permeation chromatography (GPC, Waters E2640).

[0267] Specifically, the copolymer was dissolved in HFIP (hexafluoroisopropanol) at a concentration of 2 mg / mL, and 20 μL was injected into GPC. HFIP was used as the mobile phase of GPC, and the flow rate was 1.0 mL / min. The analysis was performed at 40°C. Two Agilent Mixed-B columns were connected in series. An RI Detector was used as the detector. The Mw value was derived using a calibration curve formed using polystyrene standard samples. Nine weight-average molecular weights of polystyrene standard specimens were used: 2,000 g / mol, 10,000 g / mol, 30,000 g / mol, 70,000 g / mol, 200,000 g / mol, 700,000 g / mol, 2,000,000 g / mol, 4,000,000 g / mol, and 10,000,000 g / mol.

[0268]

[0269] Experimental Example 2

[0270] The bending characteristics of the negative electrode plates according to the above examples and comparative examples were evaluated using the mandrel method, and the diameter of the rod where cracks occurred is shown in Table 1 below.

[0271]

[0272] Experimental Example 3

[0273] The negative electrode plates in which the porous layer according to the above examples and comparative examples was formed on the negative electrode active material layer were observed using a scanning electron microscope, and the results are shown in FIGS. 1 (Example 1), 2 (Example 2), 3 (Example 3), 4 (Example 4), 5 (Example 5), 6 (Comparative Example 1), and 7 (Comparative Example 2). In FIGS. 1, 2, 6, and 7, (a) is an SEM image at a magnification of 1000 times, and (b) is an SEM image at a magnification of 5000 times. FIGS. 3, 4, and 5 are SEM images at a magnification of 5000 times, respectively.

[0274] Referring to FIGS. 1 to 5, a uniform surface state without fine cracks could be observed in the cathode plates according to the embodiments.

[0275] Referring to Fig. 6, cracks were easily observed in the negative electrode plate according to Comparative Example 1 due to the inflexible polymer binder properties. Specifically, in Comparative Example 1, the surface was observed to be rougher than in Example 1 and relatively large pores of about 1 μm were observed to be unevenly distributed.

[0276] Referring to Fig. 7, in the cathode plate according to Comparative Example 2, the surface roughness was somewhat reduced compared to Comparative Example 1, but cracks on the surface could still be easily observed.

[0277]

[0278] Experimental Example 4

[0279] For the lithium secondary batteries obtained in the above examples and comparative examples (five samples each), the open circuit voltage (OCV) was measured immediately after production, and the average value of the five samples is shown in Table 1 below.

[0280] The lithium secondary batteries (5 samples each) obtained in the above examples and comparative examples were subjected to a 0.1 C (reference capacity 4.5 mAh / cm) CC-CV mode at 25 ℃. 2 ) was charged until it reached 4.2 V and the voltage was maintained in CV mode until it reached 0.05 C. Afterwards, the formation process was performed by discharging to 2.5 V at 0.1 C, and the discharge capacity (mAh) was shown in Table 1 below as an average value of five samples.

[0281] During the formation process, the number of defective samples that were not properly charged and discharged due to short circuits, etc., among the five samples manufactured in each of the examples and comparative examples were confirmed and are shown in Table 1 below.

[0282]

[0283] Mandrel diameter (Φ) OCV (V) Discharge capacity (mAh) Number of defective (pieces) Example 140.1642.91 Example 220.1850.40 Example 340.1245.01 Example 420.1547.11 Example 520.1948.00 Comparative example 1120.0325.43 Comparative example 260.1029.52

[0284] Referring to the results of the above experimental examples, the lithium secondary batteries of the examples exhibited high discharge capacity while also exhibiting excellent assembly stability without any defects due to short circuit between the negative electrode and positive electrode.

[0285] The lithium secondary battery of Comparative Example 1 above had a low initial open circuit voltage and a failure rate of about 60%, resulting in low assembly stability due to low bending characteristics and surface cracks of the negative electrode plate.

[0286] In addition, the lithium secondary battery of Comparative Example 2 had slightly better bending characteristics and surface cracks of the negative electrode plate than Comparative Example 1, but the initial open circuit voltage was still lower than that of the example, and the failure rate was about 40%, indicating low assembly stability.

[0287]

[0288] Although the present invention has been described above with reference to limited embodiments and drawings, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical idea of ​​the present invention and the equivalent scope of the patent claims to be described below by a person having ordinary skill in the art to which the present invention pertains.

Claims

1. It includes an electrode active material layer and a porous layer laminated on an electrode current collector layer, The porous layer comprises a polymer binder including a copolymer including a hard segment of the following chemical formula 1 and a soft segment of the following chemical formula 2, and inorganic fine particles dispersed on the polymer binder. Electrodes for lithium secondary batteries: [Chemical Formula 1] In the above chemical formula 1, R 1 and R 3 are each independently , , or and; A 1 Inland A 3 are each independently hydrogen or an alkyl group having 1 to 3 carbon atoms; L 1 is a chemical bond or a methylene group; R 2 is an alkylene group having 1 to 5 carbon atoms; [Chemical Formula 2] In the above chemical formula 2, R 4 is an alkylene group having 3 to 6 carbon atoms.

2. In paragraph 1, The above R 1 and R 3 are each independently , , , , , , or Electrode for lithium secondary batteries.

3. In paragraph 1, An electrode for a lithium secondary battery, wherein the copolymer comprises the hard segment and the soft segment in a molar ratio of 80:20 to 95:

5.

4. In paragraph 1, An electrode for a lithium secondary battery, wherein the copolymer has a weight average molecular weight (Mw) of 100,000 g / mol to 1,000,000 g / mol.

5. In paragraph 1, The polymer binder is polyetherimide, polyvinylidene fluoride, poly(vinylidene fluoride-co-trichloroethylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), poly(vinylidene fluoride-co-trifluoroethylene), poly(vinylidene fluoride-co-tetrafluoroethylene), poly(vinylidene fluoride-co-hexafluoropropylene), butylacrylate, polymethylmethacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene vinyl acetate copolymer, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethylated polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethylcellulose, An electrode for a lithium secondary battery, further comprising at least one compound selected from the group consisting of acrylonitrile-styrene-butadiene copolymers, ethylene-propylene-diene terpolymers, sulfonated ethylene-propylene-diene terpolymers, styrene butadiene rubbers, fluororubbers, and polyimides.

6. In paragraph 5, An electrode for a lithium secondary battery, wherein the polymer binder comprises at least 10 wt% of a copolymer including a hard segment of the chemical formula 1 and a soft segment of the chemical formula 2, based on the total weight of the polymer binder.

7. In paragraph 1, The above inorganic fine particles are SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, AlO(OH), Al(OH)3, TiO2, SiC, BaTiO3, Pb(Zr,Ti)O3, Pb 1-x La x Zr 1-y Ti y O3, Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3, HfO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x< 2, 0<y<1, 0<z<3), (LiAlTiP) x O y (0 <x<4, 0<y<13), Li x La y TiO3(0 <x<2, 0<y<3), Li x Ge y P z S w (0 <x<4, 0<y<1, 0<z<1, 0<w<5), Li x N y (0 <x<4, 0<y<2), Li x Si y S z (0 <x<3, 0<y<2, 0<z< 4), 및 Li x P y S z (0 <x<3, 0<y<3, 0<z<7)로 이루어진 군에서 선택된 1종 이상인, 리튬 이차 전지용 전극.

8. In paragraph 1, An electrode for a lithium secondary battery, wherein the above-mentioned inorganic fine particles have a particle size of 0.001 ㎛ to 10 ㎛.

9. In paragraph 1, An electrode for a lithium secondary battery, wherein the porous layer comprises 0.5 to 45 wt% of the polymer binder and 55 to 99.5 wt% of the inorganic fine particles.

10. A step of forming an electrode active material layer by applying an electrode material composition including an electrode active material on an electrode current collector layer; A step of preparing an inorganic fine particle dispersion by dispersing inorganic fine particles and a dispersant in a solvent; A step of preparing a binder solution by dissolving a polymer binder including a copolymer including a hard segment of the following chemical formula 1 and a soft segment of the following chemical formula 2 in a solvent; A step of preparing a slurry for forming a porous layer by mixing the binder solution into the inorganic fine particle dispersion; and A step of forming a porous layer by applying the slurry for forming the porous layer on the electrode active material layer. A method for manufacturing an electrode for a lithium secondary battery according to claim 1, comprising: [Chemical Formula 1] In the above chemical formula 1, R 1 and R 3 are each independently , , or and; A 1 Inland A 3 are each independently an alkyl group having 1 to 3 carbon atoms; L 1 is a chemical bond or a methylene group; R 2 is an alkylene group having 1 to 5 carbon atoms; [Chemical Formula 2] In the above chemical formula 2, R 4 is an alkylene group having 3 to 6 carbon atoms.

11. In paragraph 10, A method for manufacturing an electrode for a lithium secondary battery, wherein the slurry for forming the porous layer has a solid content including the inorganic fine particles of 55 wt% to 99.5 wt%.

12. A polymer binder comprising a copolymer including a hard segment of the following chemical formula 1 and a soft segment of the following chemical formula 2, and inorganic fine particles dispersed on the polymer binder. Slurry for forming a porous layer for an electrode for a lithium secondary battery: [Chemical Formula 1] In the above chemical formula 1, R 1 and R 3 are each independently , , or and; A 1 Inland A 3 are each independently hydrogen or an alkyl group having 1 to 3 carbon atoms; L 1 is a chemical bond or a methylene group; R 2 is an alkylene group having 1 to 5 carbon atoms; [Chemical Formula 2] In the above chemical formula 2, R 4 is an alkylene group having 3 to 6 carbon atoms.

13. In paragraph 12, A slurry for forming a porous layer of an electrode for a lithium secondary battery, wherein the copolymer comprises the hard segment and the soft segment in a molar ratio of 80:20 to 95:

5.

14. In paragraph 12, A slurry for forming a porous layer of an electrode for a lithium secondary battery, wherein the polymer binder and the inorganic fine particles are contained in a ratio of 0.5 to 45 wt%: 55 to 99.5 wt%.

15. A lithium secondary battery comprising an electrode for a lithium secondary battery according to paragraph 1.

Citation Information

Patent Citations

  • Binder for carbon-coated lithium iron phosphate(c-LiFePO4) electrode with high adhesion and electrode including the binder and lithium secondary battery icluding the electrode

    KR101764072B1

  • Electrode havig improved interfacial adhesion withseparator and electrochemical device comprising thesame

    KR1020080010166A

  • Electrode having porous coating layer and electrochemical device containing the same

    KR1020130114926A

  • Separator for lithium sulfur battery and lithium sulfur battery comprising the same

    KR1020170136850A

  • KR20190140819A