Catalyst for methane reforming and manufacturing method thereof

A Ni-B-Mg catalyst with a specific B content range, produced via hydrothermal synthesis, addresses the instability and activity issues of existing methane reforming catalysts by forming a stable Ni-B intermetallic compound, ensuring sustained catalytic performance and reduced coke deposition during high-temperature reactions.

WO2024225636A1PCT designated stage expired Publication Date: 2024-10-31HANWHA SOLUTIONS CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004220
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-02
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Catalysts for methane reforming using carbon dioxide suffer from instability and low activity due to sintering and coke deposition, especially at high temperatures, necessitating the development of a catalyst with improved structural stability and dispersion.

Method used

A catalyst comprising nickel (Ni), boron (B), and magnesium (Mg) is produced using hydrothermal synthesis, with a specific B content range to form a Ni-B intermetallic compound, enhancing structural stability and preventing sintering and coke deposition, thereby maintaining high catalytic activity during methane reforming reactions.

Benefits of technology

The catalyst exhibits excellent structural stability and catalytic performance by suppressing sintering and coke deposition, maintaining high dispersion and activity even after 48 hours of reaction, with a high BET specific surface area and efficient methane and carbon dioxide processing speeds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004220_31102024_PF_FP_ABST
    Figure KR2024004220_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst for a methane reforming reaction and a manufacturing method thereof. More particularly, the objective of the present invention is to provide a highly dispersed nickel catalyst with secured structural stability that can be used in a methane reforming reaction utilizing carbon dioxide, and a manufacturing method thereof, wherein the nickel is highly dispersed and has excellent structural stability during the methane reforming reaction, thereby providing a nickel catalyst that exhibits excellent catalytic performance in a methane reforming reaction utilizing carbon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst for methane reforming and method for producing the same

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0055933, filed April 28, 2023, the entire contents of which are incorporated herein by reference.

[0003]

[0004] The present invention relates to a catalyst for methane reforming and a method for producing the same. In particular, the present invention relates to a catalyst for methane reforming with guaranteed structural stability that can be used in a methane reforming reaction utilizing carbon dioxide, and a method for producing the same.

[0005]

[0006] As rising atmospheric carbon dioxide concentrations pose various challenges, active efforts are being made to convert carbon dioxide into useful substances. Among these, methane reforming using carbon dioxide involves reacting carbon dioxide and methane with a catalyst at high temperatures to produce industrially useful synthesis gases, such as a mixture of hydrogen and carbon monoxide. This synthesis gas offers the advantage of being directly applicable to reactions that synthesize various chemicals or hydrocarbons. However, despite these advantages, the catalysts used for reforming are unstable and have low activity, making practical application difficult.

[0007] In addition, since the methane reforming reaction using carbon dioxide shows a higher conversion as the temperature increases, the reaction must be carried out at a high temperature to obtain a high-purity product. However, in general, when the catalyst is exposed to high temperatures for a long time, the active metal sinters, reducing the active surface, or carbon (e.g., coke), a side reaction product, covers the surface of the active metal, causing a decrease in activity over time. Therefore, a method of using precious metals to minimize side reactions and sintering has been considered, but for economic reasons, a catalyst that can replace precious metals is currently needed.

[0008] Accordingly, a method of manufacturing a catalyst by impregnating an MgO carrier with nickel and molybdenum as active materials was devised, but there are still problems of reduction in active surface area and coke deposition due to calcination.

[0009]

[0010] The present invention provides a catalyst for methane reforming and a method for producing the same. In particular, the present invention provides a methane reforming catalyst with guaranteed structural stability that can be used in a methane reforming reaction utilizing carbon dioxide, and a method for producing the same.

[0011]

[0012] A catalyst for methane reforming according to one embodiment of the present invention is a catalyst comprising nickel (Ni), boron (B) and magnesium (Mg), wherein the B content may be greater than 1 mol part and less than 35 mol parts with respect to 100 mol parts of Mg.

[0013]

[0014] In addition, the method for producing a catalyst for methane reforming of one embodiment of the present invention comprises the steps of: preparing an aqueous solution mixture by mixing MgO, a Ni precursor, and a B precursor (step 1); hydrothermally synthesizing the mixture of step 1 (step 2); and drying and calcining the hydrothermally synthesized composition of step 2 (step 3); wherein in step 1, the B precursor can be mixed in an amount such that the B content is more than 1 mol part and less than 35 mol parts with respect to 100 mol parts of Mg content.

[0015]

[0016] According to the present invention, excellent structural stability is achieved before and after the methane reforming reaction by introducing dual metals, and high dispersion can be maintained by suppressing sintering of Ni nanoparticles during the reforming reaction. Therefore, the present invention can provide a nickel catalyst that exhibits excellent catalytic performance by suppressing sintering and coke deposition in a methane reforming reaction utilizing carbon dioxide.

[0017]

[0018] Figure 1 illustrates the results of nitrogen adsorption analysis of Examples 1 to 3 of the present disclosure and Comparative Example 1.

[0019] Figure 2 shows the TEM and EDS mapping image results after the methane reforming reaction of Example 3 of the present disclosure.

[0020] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.

[0021] In this specification, it should be understood that terms such as “include,” “comprising,” or “having” are intended to specify the presence of a feature, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, steps, components, or combinations thereof.

[0022] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0023] Hereinafter, the present invention will be described in detail.

[0024]

[0025] Although Ni-MgO catalysts are known to have high activity in methane reforming reactions using existing carbon dioxide, there was a problem that deactivation occurred quickly due to sintering of metal particles and coke formation under high-temperature reaction conditions.

[0026] Accordingly, a method using hydrothermal synthesis was proposed. Ni-MgO catalysts manufactured using hydrothermal synthesis had the advantage of achieving high dispersion of Ni and suppressing coke deposition during the reaction compared to catalysts manufactured through other synthetic methods (e.g., impregnation, co-precipitation, etc.).

[0027] However, when Ni nanoparticles form large particles through sintering, there is a problem in that this promotes coke formation during the reforming reaction, significantly reducing catalytic activity during the reaction. Therefore, suppressing sintering of Ni nanoparticles during the reforming reaction and maintaining high dispersion are crucial for maintaining catalytic activity.

[0028] To overcome this, a double metal (B) was introduced during the hydrothermal synthesis of a Ni-MgO catalyst to form a Ni-B intermetallic compound structure, thereby aiming to manufacture a catalyst with improved structural stability and performance. The catalyst of the present disclosure achieves superior structural stability during methane reforming compared to the previously known Ni-MgO (hydrothermal synthesis) and Ni-MgAl2O4 (co-precipitation) catalysts, and thus exhibits superior catalytic performance in a methane reforming reaction utilizing carbon dioxide.

[0029]

[0030] The catalyst of the present disclosure is a catalyst comprising nickel (Ni), boron (B), and magnesium (Mg), wherein the B content may be greater than 1 molar part and less than 35 molar parts relative to 100 molar parts of Mg. Specifically, the B content may be greater than 1 molar part, greater than 5 molar parts, greater than 10 molar parts, greater than 15 molar parts, greater than 20 molar parts, or greater than 25 molar parts and less than 35 molar parts, less than 34 molar parts, less than 33 molar parts, less than 32 molar parts, less than 31 molar parts, or less than 30 molar parts relative to 100 molar parts of Mg.

[0031] The boron (B) content must satisfy the above range to form a Ni-B intermetallic compound, i.e., an alloy structure, to be achieved in the present disclosure, thereby ensuring catalyst structural stability in the methane reforming reaction process, and boron can be highly dispersed in the carrier MgO lattice to form a solid solution (alloy).

[0032] In the case of catalysts containing nickel (Ni) in alumina (Al2O3), coke deposition (i.e., coking) occurs on the catalyst surface during reforming or dehydrogenation reactions, which reduces catalytic activity during the reaction. Therefore, it has been reported that the addition of boron suppresses coke deposition on the catalyst surface due to changes in the electronic structure and improved dispersion of Ni nanoparticles.

[0033] However, if the boron content is too high, a B2O3 crystal structure is formed on the catalyst surface, blocking the active sites where the reaction occurs, which can significantly reduce the catalytic activity.

[0034]

[0035] The Mg (magnesium) in the above methane reforming catalyst may exist as a carrier in the form of MgO (magnesium oxide). Specifically, the catalyst of one embodiment of the present invention may be in the form of a Ni-B intermetallic compound dispersed as nanoparticles on MgO.

[0036]

[0037] The Ni content may be 2 to 10 parts by weight relative to 100 parts by weight of the total catalyst for methane reforming. Specifically, the Ni content may be 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, or 5 parts by weight or more to 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, or 6 parts by weight or less relative to the total weight of the catalyst.

[0038] When the Ni (nickel) content satisfies the above range, nickel can be suppressed from forming excessively large particles and promoting coke formation, thereby preventing adverse effects on catalytic activity, and a sufficient amount of nickel active phase required for the methane reforming reaction can be secured.

[0039] If the Ni content is too excessive, nickel may form large particles, which may promote coke formation and significantly reduce catalytic activity. If the Ni content is too small, the amount of nickel active phase required for the reaction may be insufficient, which may result in a problem of catalytic activity not being secured.

[0040]

[0041] In addition, the catalyst of the present disclosure may have a balance of MgO as a carrier, excluding the B (boron) content and the Ni (nickel) content, based on the total weight of the catalyst.

[0042] Specifically, the catalyst of the present disclosure may include only B (boron), Ni (nickel), and Mg (magnesium) as metal elements.

[0043]

[0044] In addition, in the case of existing methane reforming catalysts containing Ni (nickel) on an alumina (Al2O3) support, there is a problem that the alumina has acid points, which causes coke deposition on the catalyst surface during the reforming reaction, that is, coking, and thus the catalytic activity decreases during the reaction. However, the catalyst of the present disclosure does not contain alumina, but instead contains MgO. Compared to alumina, MgO has very few acid points, that is, it can be considered to have no acid points, and therefore, coking occurs relatively less, which has the advantage of maintaining catalytic activity. In addition, MgO has excellent basicity, so it has excellent adsorption of reactants, resulting in good reactivity. However, in the case of manufacturing using the existing impregnation method, there is a problem that the nickel dispersion is low and the surface area is small. Therefore, the present disclosure intends to provide a manufacturing method including a hydrothermal synthesis method.

[0045]

[0046] The catalyst may have a size of Ni-B nanoparticles of 3.0 to 8.0 nm upon reduction. In addition, the catalyst may have a size of 5 to 17 nm after 48 hours of methane reforming. Specifically, the catalyst may have a size of 5 to 17 nm after 48 hours of methane reforming.

[0047] Since the catalyst of the present invention does not observe any crystallization of Ni when it goes through only the calcination step, the size of the nanoparticles can be observed by reducing it in a hydrogen atmosphere to confirm the structural stability before and after the methane reforming reaction.

[0048] When Ni-B forms large particles, this can promote coke formation during the reforming reaction, significantly reducing catalytic activity. In addition, the catalyst of the present invention maintains structural stability and catalytic efficiency by not increasing the size of the Ni-B nanoparticles before and after use in the reforming reaction.

[0049] In addition, since in the present invention, Ni-B is highly dispersed on MgO to achieve high efficiency, even when used in a methane reforming reaction utilizing high-temperature carbon dioxide, the catalyst does not sinter or coke is deposited on the catalyst surface, thereby reducing the catalytic efficiency.

[0050]

[0051] The above catalyst has a BET specific surface area of ​​10 m measured using the nitrogen adsorption method. 2 / g to 50 m 2 / g may be.

[0052] Specifically, the specific surface area of ​​the above catalyst is 10 m 2 / g or more, 20 m 2 / g or more, 30 m 2 / g or more, or 40 m 2 / g or more to 50 m 2 / g or less, 49 m 2 / g or less, 48 ​​m 2 / g or less, 47 m 2 / g or less, 46 m2 / g or less or 45 m 2 / g can be less.

[0053] The above catalyst may be used in a methane reforming reaction utilizing carbon dioxide. The catalyst according to one embodiment of the present invention has a high BET specific surface area, and thus, when used in a methane reforming reaction utilizing carbon dioxide that is carried out at high temperatures, it has the advantages of a fast methane reforming process speed, a large throughput, no or little sintering of other catalysts as the reaction progresses, and a small amount of coke deposition, so that the catalytic efficiency does not decrease during the reaction.

[0054]

[0055] In addition, the catalyst may have a lattice constant of MgO of 4.1 Å to 4.2 Å as determined by X-ray diffraction analysis. This is a value at which MgO lattice shrinkage occurs by introducing a double metal (B). As MgO lattice shrinkage occurs, it can affect the electronic structure and oxidation / reduction characteristics of the catalyst surface, and can affect the dispersion degree of the supported Ni.

[0056]

[0057] The methane reforming catalyst of the present invention has excellent structural stability by introducing a dual metal (B) during the hydrothermal synthesis process of a Ni-MgO catalyst. Accordingly, compared to existing Ni-MgO catalysts manufactured by a hydrothermal synthesis method without introducing a dual metal, the catalyst of the present invention with the introduction of a dual metal (B) does not show a decrease in the rate of processing methane and carbon dioxide before and after a 48-hour methane reforming reaction.

[0058] This is because boron (B) is highly dispersed in the carrier MgO lattice to form a solid solution (alloy). At this time, MgO lattice shrinkage occurs, which can affect the electronic structure and redox properties of the catalyst surface and the dispersion of the supported Ni. During the reforming reaction, boron (B), a double metal, forms an intermetallic compound with nickel, and coke deposition on the catalyst surface can be suppressed due to the change in the electronic structure and improved dispersion of Ni nanoparticles.

[0059]

[0060] In addition, one embodiment of the present invention provides a method for preparing a catalyst, comprising the steps of: preparing an aqueous solution by mixing MgO, a Ni precursor, and a B precursor (step 1); hydrothermally synthesizing the mixture of step 1 (step 2); and drying and calcining the hydrothermally synthesized composition of step 2 (step 3).

[0061]

[0062] In the above step 1, the B precursor can be mixed in an amount such that the B content is more than 1 mol part and less than 35 mol parts with respect to 100 mol parts of the Mg content. That is, the B precursor can be added to the final product, the catalyst, in an amount such that the B content is more than 1 mol part and less than 35 mol parts with respect to 100 mol parts of the Mg content. Specifically, the B precursor can be mixed in an amount such that the B content is more than 1 mol part, 5 mol parts or more, 10 mol parts or more, 15 mol parts or more, 20 mol parts or more, or 25 mol parts or more and less than 35 mol parts, 34 mol parts or less, 33 mol parts or less, 32 mol parts or less, 31 mol parts or less, or 30 mol parts or less with respect to 100 mol parts of the Mg content.

[0063] The B (boron) precursor content must satisfy the above range to ensure catalyst structural stability in the methane reforming reaction process to be achieved in the present disclosure, and boron can be highly dispersed in the carrier MgO lattice to form a solid solution (alloy).

[0064]

[0065] In the above step 1, the Ni precursor can be mixed in an amount such that the Ni content is 2 to 10 parts by weight based on 100 parts by weight of the entire catalyst. That is, the Ni precursor can be added to the final product, the catalyst, in an amount such that the Ni content is 2 to 10 parts by weight based on 100 parts by weight of the entire catalyst. Specifically, the Ni precursor can be mixed in an amount such that the Ni content is 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, or 5 parts by weight or more, and 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, or 6 parts by weight or less based on 100 parts by weight of the entire catalyst.

[0066] The content of the Ni precursor must satisfy the above range so that nickel can form excessively large particles, thereby preventing coke formation and adverse effects on catalytic activity, and a sufficient amount of nickel active phase required for the methane reforming reaction can be secured.

[0067]

[0068] The B precursor of the above step 1 may be at least one selected from the group consisting of H3BO3, BI3, BN, BF3, BCl3, B2O3, CB4, BF3·2H2O, BBr3, and LiBH4. Specifically, the B precursor of the step 1 may be H3BO3.

[0069]

[0070] The Ni precursor of the above step 1 may be at least one selected from the group consisting of Ni(CH3COO)2·4H2O), NiCl2, NiCl2·6H2O, Ni(NO3)2, NiSO4, (NH4)2Ni(SO4)2·6H2O, NiBr2, NiCO3, NiF2, NiI2, NiC2O4·2H2O and Ni(ClO4)2·6H2O. Specifically, the Ni precursor of the step 1 may be Ni(CH3COO)2·4H2O).

[0071]

[0072] Additionally, step 1 may include a step of preparing a MgO suspension; a step of preparing a Ni precursor aqueous solution; a step of preparing a B precursor aqueous solution; a step of adding the Ni precursor aqueous solution dropwise to the MgO suspension; and a step of adding the B precursor aqueous solution dropwise to the MgO and Ni precursor mixed solution and stirring.

[0073]

[0074] The hydrothermal synthesis in step 2 can be carried out at a temperature of 100 to 300°C for 12 to 48 hours. Specifically, the hydrothermal synthesis can be carried out at a temperature of 100°C or higher, 110°C or higher, 120°C or higher, or 150°C or higher to 300°C or lower, 250°C or lower, or 200°C or lower.

[0075] Hydrothermal synthesis is a method of synthesizing a material using an aqueous solution under high temperature and high pressure. It is a single crystal synthesis method that depends on the solubility of the material, and performs material synthesis through heat treatment at a temperature higher than the boiling point of a commonly used solvent. Hydrothermal synthesis is a method that can be adopted to produce a solid solution in which Ni is uniformly dispersed on MgO, as in the present invention, because the particles are highly dispersed in the solution. In the present invention, in the synthesis step, a mixture of MgO and an aqueous solution of Ni precursor reacts, so that Ni is highly dispersed on MgO to form a solid solution, and MgO forms pores to increase the BET specific surface area.

[0076] Specifically, the hydrothermal synthesis of the present invention can be carried out at a temperature of 120 to 200°C for 22 to 26 hours.

[0077]

[0078] The mixture synthesized in step 2 can undergo the drying and calcination steps of step 3.

[0079] Drying in step 3 can be carried out at 50 to 150°C for 2 to 24 hours, specifically at 70 to 110°C for 10 to 16 hours.

[0080] The firing in step 3 above can be performed at 600 to 1000°C for 2 to 6 hours, specifically at 700 to 900°C for 3 to 5 hours.

[0081]

[0082] As described in the catalyst section above, the method for manufacturing the catalyst of the present invention uses a hydrothermal synthesis method, and thus, compared to an impregnation method such as a prior art, the manufactured catalyst is characterized in that the catalyst does not undergo calcination even in a high-temperature reforming reaction, there is no coke deposition on the surface, and the catalytic activity is maintained, and structural stability is maintained even when a methane reforming reaction is performed.

[0083]

[0084] Hereinafter, the present invention will be described in more detail with reference to the following experimental examples. However, the following experimental examples are intended only to illustrate the present invention and the scope of the present invention is not limited to these examples.

[0085]

[0086] [Experimental Example]

[0087]

[0088] <Example 1>

[0089] A Ni-B-MgO catalyst was prepared using Ni, B precursors and MgO raw materials.

[0090] First, 4 g of magnesium oxide [MgO] was added to 140 mL of distilled water and stirred at room temperature (500 rpm) to prepare an MgO suspension.

[0091] At the same time, 0.893 g of nickel acetate tetrahydrate [Ni(CH3COO)2·4H2O], which has a Ni content of 5 parts by weight per 100 parts by weight of the total catalyst, was added to 20 mL of distilled water and stirred to dissolve, thereby preparing a Ni precursor aqueous solution.

[0092] Next, the Ni precursor solution was added dropwise to the stirred MgO suspension using a pipette, and stirred at the same speed at room temperature for 30 minutes.

[0093] At the same time, 0.306 g of boric acid [H3BO3], which makes the B content 5 molar parts per 100 molar parts of Mg of the catalyst, was added to 20 mL of distilled water and stirred to dissolve, thereby preparing a B precursor aqueous solution.

[0094] Afterwards, the B precursor solution was added dropwise to the stirred Ni and MgO suspension using a pipette, and stirred at the same speed at room temperature for 2 hours.

[0095] The suspension after stirring was subjected to hydrothermal synthesis at 200°C for 24 hours in a Teflon-lined autoclave.

[0096] The resulting suspension was filtered and washed four times with distilled water through a filter device, and then dried at 100°C for 12 hours to remove moisture. The dried sample was calcined in an air atmosphere at 900°C (heating rate: 2°C / min) for 4 hours.

[0097]

[0098] <Example 2>

[0099] The same method as Example 1 was performed, except that 0.612 g of boric acid [H3BO3] was used so that the B content was 10 molar parts per 100 molar parts of Mg in the catalyst.

[0100]

[0101] <Example 3>

[0102] The same method as Example 1 was performed except that 1.224 g of boric acid [H3BO3] was used so that the B content was 20 molar parts per 100 molar parts of Mg in the catalyst.

[0103]

[0104] <Example 4>

[0105] The same method as Example 1 was performed except that 1.836 g of boric acid [H3BO3] was used so that the B content was 30 molar parts per 100 molar parts of Mg in the catalyst.

[0106]

[0107] <Comparative Example 1>

[0108] The same procedure as Example 1 was followed except that boric acid [H3BO3] was not used.

[0109]

[0110] <Comparative Example 2>

[0111] The same method as Example 1 was performed, except that 0.061 g of boric acid [H3BO3] was used so that the B content was 1 molar part per 100 molar parts of Mg in the catalyst.

[0112]

[0113] <Comparative Example 3>

[0114] The same method as Example 1 was performed except that 2.142 g of boric acid [H3BO3] was used so that the B content was 35 molar parts per 100 molar parts of Mg in the catalyst.

[0115]

[0116] <Comparative Example 4>

[0117] In a different manner from the examples, a Ni-B-MgO-IP catalyst was prepared using an impregnation method as follows. 0.893 g of nickel acetate tetrahydrate [Ni(CH3COO)2·4H2O] and 1.224 g of boric acid [H3BO3] were added to 0.5 mL of distilled water and sonicated to dissolve such that the Ni content was 5 parts by weight per 100 parts by weight of the total catalyst and the B content was 20 parts by mole per 100 parts by mole of Mg. Then, the Ni and B precursor solutions were supported on 4 g of MgO using the initial wetness impregnation method, and the supported sample was dried and calcined in the same manner as in Example 1.

[0118]

[0119] Comparative Example 5

[0120] The same method as Comparative Example 4 was performed except that boric acid [H3BO3] was not used.

[0121]

[0122] Experimental Example 1

[0123] To determine the specific surface area and pore structure of the examples and comparative examples, nitrogen adsorption analysis was performed using a Tristar 2 3020 device. Prior to nitrogen adsorption analysis, the samples were pretreated in a vacuum at 150°C for 8 hours.

[0124] The BET surface area was calculated using the BET surface area S formula. From the graph of Adsorbed amout(v) / P / P0(A), 0.15 <A<0.3 범위에서 y 축을 1 / v(1-A), x축을 A로 plot 했을 때 기울기가 1 / vm이다. vm은 촉매의 표면을 덮는 N2분자의 부피이다. N2분자 하나당 0.162 nm를 차지하며, BET 비표면적 S식은 S=(vm x N x s) / mv와 같고, N은 아보가드로 숫자(6.02*10 23 ), s is 0.162 nm 2(crosssection area), mv is the volume per mole of gas molecules (molar volume).

[0125] The BET surface area values ​​are shown in Table 1 below.

[0126]

[0127] Experimental Example 2

[0128] To confirm the crystal structure and lattice information of the examples and comparative examples, X-ray diffraction analysis was performed using RIGAKU SmartLab equipment. The catalyst samples were placed in a glass holder with a depth of 0.2 mm and irradiated with Cu Kα radiation at a wavelength of 1.5406 nm. The X-ray scan was performed at 5° min. -1 The measurements were made from 20° to 80° at an interval of 0.01° at a speed of . The lattice constant of MgO was calculated using Bragg's law, and when the X-ray wavelength λ and the incident angle θ of the X-ray were determined using the equation λ = 2d·sinθ, the interplanar spacing d of the crystal lattice could be calculated using the diffraction pattern. Based on the diffraction pattern with a plane index of 200, d 200 is a 200 / 2, and therefore the MgO lattice constant a 200 was calculated as λ / sinθ.

[0129]

[0130] Experimental Example 3

[0131] To confirm the activity and stability of the examples and comparative examples, a methane reforming reaction using carbon dioxide was performed. Specifically, 8 mg of catalyst particles (200-300 μm) were mixed with SiO2 at a mass ratio of 9:1 and placed in a cylindrical quartz reactor (inner diameter: 10 mm). Then, the temperature was increased to 900°C (heating rate: 10°C / min) in a 100% hydrogen atmosphere for catalyst reduction.

[0132] After maintaining the hydrogen atmosphere for 2 hours, purging was performed in a nitrogen atmosphere for 30 minutes, and then the methane-carbon dioxide mixed gas concentration was injected together with nitrogen gas (45.5 kPa CH4; 45.5 kPa CO2; 9.1 kPa N2), which is an internal standard gas, so that it was 90% of the total feed gas flow rate.

[0133] After fixing the Gas Hourly Space Velocity (GHSV) to 1,200 L / gh based on the reactants, methane reforming reaction using carbon dioxide was performed for 48 hours, and the products (H2, CO) and residual reactants (CH4, CO2) were quantified through gas chromatography (GC) equipped with a TCD detector and a carboxen-1000 column, and are shown in Table 1 below.

[0134] The CH4 and CO2 treatment rates were calculated using the equation (treatment rate = GHSV x reactant concentration x conversion rate). After 48 hours of reaction, the amount of coke deposition on the catalyst was measured using elemental analysis.

[0135]

[0136] Experimental Example 4

[0137] The structural size of the Ni-B intermetallic compound of the examples and comparative examples was measured by TEM images before and after 48 hours of methane reforming. Since the catalyst of the present invention does not observe any crystallization of Ni when it goes through only the calcination step, the size of the nanoparticles was observed by reducing it in a hydrogen atmosphere to confirm the structural stability before and after the methane reforming reaction.

[0138]

[0139] Unit of classification Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Ni content (relative to 100 parts by weight of catalyst) Weight parts 5 5 5 5 5 5 5 5 B content (relative to 100 parts by mole of Mg) Molar parts 5 1 0 2 0 3 0 1 3 5 2 0 BET specific surface area m2 / g4948454155543856MgO lattice constant (a 200 )Å4.1674.1424.1284.1154.2314.2184.1094.2144.225Ni-B crystallite size (before 48 h reaction, after hydrogen reduction)nm5.35.55.45.65.35.56.114.315.6Ni-B crystallite size (after 48 h reaction)nm14.412.810.511.320.119.317.239.742.5Coke production (after 24 h reaction)wt%0.170.110.040.090.720.680.431.321.93CH4Processing rate (initial reaction, 0 h)L / g·h507.1504.8502.2501.4513.0512.2510.7432.0442.8CO2 treatment rate (initial reaction, 0 h)L / g·h509.2506.4504.3503.5517.2515.6512.3434.1445.7CH4 treatment rate (after 48 h reaction)L / g·h511.9514.2515.7513.6496.8497.5503.5437.4410.4CO2 treatment rate (after 48 h reaction)L / g·h513.1516.3518.2514.7498.1499.8505.2439.2412.5Total CH4 treatment amount L / g 2 4 4 5 6 2 4 5 6 2 4 4 3 0 2 4 3 6 0 2 4 2 3 5 2 4 2 3 3 2 4 3 4 1 2 0 8 6 6 2 0 4 7 7 Total CO2 treatment amount L / g 2 4 5 3 5 2 4 5 4 5 2 4 5 4 0 2 4 4 3 7 2 4 3 6 7 2 4 3 7 0 2 4 4 2 0 2 0 9 5 9 2 0 5 9 7

[0140] As a result of the reaction progress for 48 hours, the initial CH4 treatment rate of the example was 501 L / g·h to 508 L / g·h, and the CO2 treatment rate was 503 L / g·h to 510 L / g·h. The CH4 treatment rate of the example after 48 hours was 511 L / g·h to 516 L / g·h, and the CO2 treatment rate was 513 L / g·h to 519 L / g·h, showing higher activity than the comparative example. In particular, it was confirmed that the treatment rate of the comparative example decreased after 48 hours of reforming reaction, and the catalytic performance was not maintained but deteriorated as the reforming reaction progressed. In addition, the coke production amount of the example after 48 hours was 0.2 wt% or less, and a smaller amount of coke was deposited than the comparative example.

[0141] In the case of the example, the processing speed of the reactants increased after 48 hours of reaction, and it was confirmed that this was because boron (B), a double metal, formed an intermetallic compound with nickel during the reforming reaction, and coke deposition on the catalyst surface was suppressed due to changes in the electronic structure and improved dispersity of Ni nanoparticles, thereby improving the catalytic performance compared to the initial stage of the reaction.

[0142] The BET surface area of ​​the example is 40 m 2 / g to 50 m 2 / g, it was confirmed that it had a wider specific surface area than Comparative Example 4 using the impregnation method. In addition, the MgO lattice constant of the example was 4.1 Å to 4.2 Å, which was smaller than that of the comparative example, and it was confirmed that the lattice shrinkage of MgO occurred due to the addition of B.

[0143] After a methane reforming reaction at 900°C for 48 hours, TEM and EDS mapping images showed that the Ni-B intermetallic compound structure was maintained after the methane reforming reaction, and Ni particles with a size of 10 to 15 nm, which was smaller than that of the comparative example, were observed. Consequently, it was confirmed that Examples 1 to 4 enabled higher activity and structural stability compared to the comparative example.

Claims

1. A catalyst containing nickel (Ni), boron (B) and magnesium (Mg), B content is more than 1 mol part and less than 35 mol parts per 100 mol parts of Mg content, Catalyst for methane reforming.

2. In paragraph 1, In the above methane reforming catalyst, Mg exists in the form of MgO as a carrier. Catalyst for methane reforming.

3. In paragraph 1, The Ni content is 2 to 10 parts by weight based on 100 parts by weight of the total methane reforming catalyst. Catalyst for methane reforming.

4. In paragraph 1, The above methane reforming catalyst has a BET specific surface area of ​​10 m using nitrogen adsorption method. 2 / g to 50 m 2 / g person, Catalyst for methane reforming.

5. In paragraph 1, The above methane reforming catalyst has a lattice constant of MgO of 4.1 Å to 4.2 Å using X-ray diffraction analysis. Catalyst for methane reforming.

6. In paragraph 1, The above methane reforming catalyst comprises a Ni-B intermetallic compound structure having a size of 5 nm to 17 nm after 48 hours of methane reforming reaction. Catalyst for methane reforming.

7. In paragraph 1, The above catalyst is used in a methane reforming reaction using carbon dioxide. Catalyst for methane reforming.

8. A step of preparing an aqueous solution mixture by mixing MgO, Ni precursor and B precursor (step 1); A step of synthesizing the mixture of step 1 above (step 2); and A step of drying and calcining the composition synthesized in the above step 2 (step 3); Including, In the above step 1, the B precursor is mixed in an amount such that the B content is more than 1 mol part and less than 35 mol parts with respect to 100 mol parts of Mg content. Method for producing a catalyst for methane reforming.

9. In paragraph 8, In the above step 1, the Ni precursor is mixed in an amount such that the Ni content is 2 to 10 parts by weight based on 100 parts by weight of the total catalyst for methane reforming. Method for producing a catalyst for methane reforming.

10. In paragraph 8, The B precursor of the above step 1 is at least one selected from the group consisting of H3BO3, BI3, BN, BF3, BCl3, B2O3, CB4, BF3·2H2O, BBr3, LiBH4. Method for producing a catalyst for methane reforming.

11. In paragraph 8, The Ni precursor of the above step 1 is at least one selected from the group consisting of Ni(CH3COO)2·4H2O), NiCl2, NiCl2·6H2O, Ni(NO3)2, NiSO4, (NH4)2Ni(SO4)2·6H2O, NiBr2, NiCO3, NiF2, NiI2, NiC2O4·2H2O and Ni(ClO4)2·6H2O. Method for producing a catalyst for methane reforming.

12. In paragraph 8, The hydrothermal synthesis in step 2 is carried out at a temperature of 100 to 300°C for 12 to 48 hours. Method for producing a catalyst for methane reforming.

13. In paragraph 8, The drying in step 3 above is carried out at 50 to 150°C for 2 to 24 hours. Method for producing a catalyst for methane reforming.

14. In paragraph 8, The firing of the above step 3 is carried out at 600 to 1000℃ for 2 to 6 hours. Method for producing a catalyst for methane reforming.

Citation Information

Patent Citations

  • Molded object of Ni-based Catalyst for Steam Methane Reforming and use thereof

    KR101794316B1

  • Synthesis method of 2-dimensional Nickel silicate molecular sieve catalyst for dry reforming of methane and 2-dimensional Nickel silicate molecular sieve catalyst for dry reforming of methane made thereby

    KR102408100B1

  • KR20210004650A

  • KR20220034712A