Coating composition for primer
The mid-coat paint composition, comprising specific resins and a curing agent, addresses the limitations of conventional compositions by providing excellent mechanical and appearance properties and eco-friendliness through low-temperature curing and reduced VOCs, enhancing the automotive painting process.
Patent Information
- Application Number
- PCT/KR2024/005493
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional intermediate paint compositions for automotive bodies in the 3-coat 1-bake method lack sufficient mechanical properties and are limited by high volatile organic compound (VOC) emissions, requiring a composition that can be cured at low temperatures with excellent appearance and eco-friendly characteristics.
A mid-coat paint composition combining an acrylic emulsion resin, polyurethane dispersion resin, and an isocyanate-based curing agent, with specific hydroxyl values and molecular weights to enhance curing, mechanical properties, and reduce VOCs through high solidification, allowing for low-temperature curing below 120°C.
The composition achieves excellent appearance and mechanical properties, such as impact resistance and water resistance, while reducing VOC emissions and lowering production costs by enabling low-temperature curing, making it suitable for automotive painting.
Smart Images

Figure PCTKR2024005493-APPB-IMG-000001 
Figure PCTKR2024005493-APPB-IMG-000002 
Figure PCTKR2024005493-APPB-IMG-000003
Abstract
Description
Intermediate paint composition
[0001] The present invention relates to a mid-coating paint composition, and more particularly, to a mid-coating paint composition comprising an acrylic emulsion resin, a polyurethane dispersion resin, a polyester resin, and an isocyanate-based curing agent.
[0002] Automobile bodies typically undergo a process of electrodeposition painting, intermediate painting, base painting, and clear painting to protect the surface from external factors and external influences. For example, an electrodeposition paint is applied to the body, then cured, followed by an intermediate paint, which is then cured. A common automotive painting system involves successively applying a base coat and a clear coat over the intermediate coating, followed by curing. Furthermore, the aforementioned automotive painting process typically employs the 3-coat-2-bake (3C2B) method, which involves first curing the intermediate coat, followed by the base coat and clear coat, followed by a second curing.
[0003] However, in order to reduce the cost of equipment investment, equipment management, and painting costs in the painting process and to improve the eco-friendliness of the paint, the 3-coat-1-bake (3C1B) painting method and the intermediate-coat deletion painting method have been proposed. The 3-coat-1-bake painting method consists of electrodeposition, intermediate coat, base coat, and clear coat, and is a method in which the intermediate paint is applied, but the base coat and clear coat are painted wet-on-wet without primary curing after the intermediate coat. In addition, the intermediate-coat deletion painting method consists of electrodeposition, base, and clear coat, and is a painting method in which the intermediate coat itself is deleted and the function of the intermediate coat is implemented in the base coat film.
[0004] In this regard, Korean Patent No. 10-1806580 (Patent Document 1) discloses a multi-coat paint system comprising an anhydrous composition comprising an epoxy-modified polyester, an acrylate polymer or a polyurethane polymer, polymer microparticles, a polymer having an isocyanate or amino group, a pigment, an organic solvent and an additive, and a functional layer manufactured therefrom. In addition, the paint system uses a wet-on-wet, 3-coat-1-bake coating method. However, as in Patent Document 1, the conventional intermediate coating composition for the 3-coat-1-bake coating method had insufficient mechanical properties of the manufactured coating film, so that it had limitations in application as a paint for automobile bodies.
[0005] Therefore, there is a need for research and development of an intermediate coating composition that has excellent appearance properties of the manufactured coating film, can be cured at a low temperature of 120°C or lower, and is environmentally friendly and economical due to the effect of reducing volatile organic compounds (VOCs) through high solidification.
[0006] [Patent Document]
[0007] (Patent Document 1) Korean Patent No. 10-1806580 (December 1, 2017)
[0008] The present invention aims to provide an intermediate coating composition that has excellent appearance characteristics of a manufactured coating film, can be cured at a low temperature of 120°C or lower, and is environmentally friendly and economical due to the effect of reducing volatile organic compounds (VOCs) through high solidification.
[0009] The present invention provides a mid-coating paint composition comprising an acrylic emulsion resin, a polyurethane dispersion resin, a polyester resin, and an isocyanate-based curing agent, wherein the acrylic emulsion resin has a hydroxyl value of 110 to 140 mgKOH / g and a weight average molecular weight of 22,000 to 26,000 g / mol, the polyurethane dispersion resin has a hydroxyl value of 110 to 140 mgKOH / g, and the polyester resin has a hydroxyl value of 90 to 105 mgKOH / g.
[0010] The intermediate coating composition according to the present invention can be cured at a low temperature of 120°C or lower and can produce a coating film with excellent appearance characteristics and mechanical properties, and is therefore suitable as a paint for automobile parts and body painting.
[0011] In addition, the intermediate coating composition according to the present invention is environmentally friendly and economical due to its high solid content and VOC reduction effect.
[0012] The present invention is described in detail below.
[0013] In this specification, “weight average molecular weight (Mw)” and “number average molecular weight (Mn)” are measured by methods commonly known in the technical field to which the present invention belongs, and can be measured by methods such as GPC (gel permeation chromatography).
[0014] In this specification, the “glass transition temperature (Tg)” is measured by a method commonly known in the technical field to which the present invention belongs, and can be measured by, for example, differential scanning calorimetry (DSC).
[0015] In this specification, functional groups such as “acid value (Av)” and “hydroxyl value (OHv)” are measured by methods commonly known in the technical field to which the present invention belongs, and can be measured by methods such as titration, for example.
[0016] The intermediate coating composition according to the present invention comprises an acrylic emulsion resin, a polyurethane dispersion resin, a polyester resin, and an isocyanate-based curing agent, wherein the acrylic emulsion resin has a hydroxyl value of 110 to 140 mgKOH / g and a weight average molecular weight of 22,000 to 26,000 g / mol, the polyurethane dispersion resin has a hydroxyl value of 110 to 140 mgKOH / g, and the polyester resin has a hydroxyl value of 90 to 105 mgKOH / g.
[0017] As described above, when an acrylic emulsion resin having a specific range of hydroxyl value and weight average molecular weight is used, the curing reaction speed and crosslinking density with a rapidly reactive isocyanate curing agent are controlled, thereby improving not only the appearance characteristics of the coating film but also mechanical properties such as impact resistance and water resistance, and there is an effect of being able to be cured at a low temperature of 120°C or lower.
[0018] In addition, when using a polyurethane dispersion resin and polyester resin having a specific range of hydroxyl groups, the surface tension is controlled in the curing reaction of the rapidly reactive isocyanate curing agent and the acrylic emulsion resin, thereby improving the smoothness of the coating film and forming a soft coating film, thereby improving the mechanical properties such as chipping resistance and impact resistance of the coating film.
[0019] Acrylic emulsion resin
[0020] Acrylic emulsion resin serves to improve the appearance characteristics and mechanical properties of a coating film manufactured from a composition containing the same.
[0021] The acrylic emulsion resin may be synthesized directly using a known method, or a commercially available product may be used. For example, the acrylic emulsion resin may include units derived from one or more monomers selected from the group consisting of allyl methacrylate (AMA), methyl methacrylate (MMA), ethyl acrylate (EA), hydroethyl acrylate (HEA), and methacrylic acid (MAA).
[0022] The acrylic emulsion resin may be prepared from a mixture comprising monomers such as allyl methacrylate (AMA), methyl methacrylate (MMA), ethyl acrylate (EA), hydroethyl acrylate (HEA), and methacrylic acid (MAA). The mixture may further comprise a divalent acrylic monomer. Divalent acrylic monomers include, for example, 1,4-Butanediol diacrylate, 1,4-Butanediol dimethacrylate, 1,5-pentanediol dimethacrylate, 1,6-Hexanediol diacrylate, 1,6-Hexanediol dimethacrylate, 1,9-Nonanediol dimethacrylate, 1,10-Decanediol dimethacrylate, ethylene glycol diacrylate, Examples include ethylene glycol dimethacrylate.
[0023] The acrylic emulsion resin may have a solid content (NV) of 30 to 50 wt%, or 35 to 45 wt%, based on the total weight of the resin. When the solid content of the acrylic emulsion resin is within the above range, the storage stability of the resin is improved, workability is excellent, and high gloss can be achieved. When the solid content of the acrylic emulsion resin is less than the above range, the viscosity is excessively low, which causes a problem in that the workability of the intermediate coating composition containing the same is insufficient, and when the solid content of the acrylic emulsion resin exceeds the above range, the viscosity of the acrylic emulsion resin is excessively high, which reduces stability during reaction and deteriorates dispersion stability, which may cause agglomeration over time.
[0024] Meanwhile, the acrylic emulsion resin may be in the form of an emulsion dispersed in a solvent such as deionized water. When the acrylic emulsion resin is in the form of an emulsion dispersed in deionized water, it has the effect of reducing the volatile organic compound (VOC) content of the paint.
[0025] The acrylic emulsion resin may have a glass transition temperature (Tg) of 65 to 76°C, or 69 to 73°C. When the glass transition temperature of the acrylic emulsion resin is within the above range, the hardness and solvent resistance of a coating film manufactured from a composition containing the same are improved. When the glass transition temperature of the acrylic emulsion resin is below the above range, the drying speed and crosslinking density of the coating film are reduced, which causes a problem in that the hardness and solvent resistance of the manufactured coating film are insufficient, and when it exceeds the above range, the coating film becomes brittle, which may result in insufficient appearance characteristics and chipping resistance of the manufactured coating film.
[0026] The acrylic emulsion resin may have a viscosity of 800 to 1,800 cps, or 880 to 1,760 cps at 25°C. When the viscosity of the acrylic emulsion resin at 25°C is within the above range, the viscosity of the intermediate coating composition is appropriate, thereby improving workability, high appearance, and durability. When the viscosity of the acrylic emulsion resin at 25°C is less than the above range, the viscosity of the composition is too low, which may cause problems such as poor formation of the produced coating film, resulting in poor paint flow, adhesion, and scratch resistance. When the viscosity exceeds the above range, the workability of the composition may be insufficient, which may cause problems such as poor appearance characteristics of the produced coating film.
[0027] The acrylic emulsion resin may have an acid value (Av) of 0.01 to 2 mgKOH / g, or 0.1 to 1.9 mgKOH / g. When the acid value of the acrylic emulsion resin is within the above range, the reactivity of a composition containing the same can be controlled to improve the appearance properties of a coating film manufactured therefrom, and the leveling (long wave) of the paint can be improved. When the acid value of the acrylic emulsion resin is below the above range, the resin stability is lowered, which causes a problem of lowering the storage properties of the manufactured paint composition, and when it exceeds the above range, the viscosity of the composition increases due to increased resin cohesion, which can cause problems of lowering workability and water resistance of the paint film.
[0028] The acrylic emulsion resin may have a hydroxyl value (OHv) of 110 to 140 mgKOH / g, or 115 to 130 mgKOH / g. When the hydroxyl value of the acrylic emulsion resin is within the above range, the reactivity of the composition containing it is controlled, thereby improving the appearance properties of the coating film manufactured therefrom and having an effect of improving the orange peel of the paint. When the hydroxyl value of the acrylic emulsion resin is below the above range, the resin stability is lowered, which may cause a problem of lowering the storage properties of the manufactured paint composition, and when it exceeds the above range, the viscosity of the composition may increase due to increased resin cohesion, which may cause a problem of lowering the workability and the water resistance of the coating film.
[0029] The acrylic emulsion resin may have a weight average molecular weight (Mw) of 22,000 to 26,000 g / mol, or 23,000 to 25,000 g / mol. When the weight average molecular weight of the acrylic emulsion resin is within the above range, the manufactured coating film has excellent long-term physical properties such as durability, adhesion, hardness, and weather resistance, and the leveling property of the paint can be improved. When the weight average molecular weight of the acrylic emulsion resin is less than the above range, the molecular weight is small, so the manufactured coating film has insufficient water resistance, impact resistance, and cold chipping resistance, and when it exceeds the above range, the flowability is reduced due to the increase in molecular weight, so that the workability of the intermediate coating composition containing it is poor, and the surface smoothness is poor, which may cause a problem that it is difficult to manufacture a coating film having an excellent appearance.
[0030] The acrylic emulsion resin may be included in the composition in an amount of 37 to 47 wt%, or 40 to 45 wt%, based on the total weight of the intermediate coating composition. When the acrylic emulsion resin is included within the above content range, there is an effect of improving the appearance characteristics and gloss. When the content of the acrylic emulsion resin is less than the above range, there is a problem that the drying property is reduced, which reduces the adhesion, gloss, hardness, and durability of the coating film, and when it exceeds the above range, the drying proceeds quickly, which may cause the painting workability and paint flow of the composition to be insufficient, which may cause a problem that the appearance and scratch resistance of the coating film are reduced.
[0031] polyurethane dispersion resin
[0032] The polyurethane dispersion resin improves the drying properties of a mid-coating composition containing the polyurethane dispersion resin and improves the flexibility of a coating film produced from the composition.
[0033] The polyurethane dispersion resin may be a polyester-polycarbonate derived polyurethane dispersion resin. For example, the polyurethane dispersion resin may be a polyester-polycarbonate diol derived polyurethane dispersion resin.
[0034] The polyurethane dispersion resin may have a solid content (NV) of 30 to 40 wt%, or 32 to 38 wt%, based on the total weight of the resin. When the solid content of the polyurethane dispersion resin is within the above range, the storage stability of the resin and the storage stability of the intermediate coating composition may be improved, and workability may be excellent. When the solid content of the polyurethane dispersion resin is less than the above range, the viscosity may be excessively low, which may cause a problem in that the workability of the intermediate coating composition containing the same may be insufficient, and when the solid content of the polyurethane dispersion resin is greater than the above range, the viscosity of the polyurethane dispersion resin may be excessively high, which may result in poor stability during reaction, and poor dispersion stability, which may cause agglomeration over time.
[0035] Polyurethane dispersion resin can be a form in which polyurethane resin is dispersed in a solvent. The aqueous medium for dispersing the polyurethane resin can be an aqueous solvent or a mixed medium of water and a hydrophilic organic solvent. For example, the aqueous solvent can be tap water, ion-exchanged water, distilled water, ultrapure water, etc. In particular, ion-exchanged water can be used to prevent particle instability due to the ease of obtaining water or the influence of salts. In addition, the hydrophilic organic solvent can be a lower monohydric alcohol such as methanol, ethanol, or propanol; a polyhydric alcohol such as ethylene glycol or glycerin; or an aprotic hydrophilic organic solvent such as N-methylmorpholine, dimethyl sulfoxide, or dimethylformamide.
[0036] The polyurethane dispersion resin may have a viscosity of 5 to 50 cps, or 10 to 40 cps, at 25°C. When the viscosity of the polyurethane dispersion resin at 25°C is within the above range, the viscosity of the intermediate coating composition is appropriate, thereby improving workability. When the viscosity of the polyurethane dispersion resin at 25°C is less than the above range, the viscosity of the composition is too low, which may cause problems such as poor formation of the produced coating film, resulting in poor paint flowability, adhesion, and scratch resistance. When the viscosity exceeds the above range, the workability of the composition may be insufficient, which may cause problems such as poor appearance properties of the produced coating film.
[0037] The polyurethane dispersion resin may have an acid value (Av) of 18 to 25 mgKOH / g, or 20 to 23 mgKOH / g. When the acid value of the polyurethane dispersion resin is within the above range, the reactivity of a composition containing the same can be controlled, thereby improving the appearance properties of a coating film manufactured therefrom. When the acid value of the polyurethane dispersion resin is below the above range, the resin stability may be lowered, which may cause a problem of lowering the storability of the manufactured coating composition. When the acid value exceeds the above range, the viscosity of the composition may be increased due to increased resin cohesion, which may cause problems of lowering workability and water resistance of the coating film.
[0038] The polyurethane dispersion resin may have a hydroxyl value (OHv) of 110 to 140 mgKOH / g, or 115 to 130 mgKOH / g. When the hydroxyl value of the polyurethane dispersion resin is within the above range, the reactivity of a composition containing the same can be controlled, thereby improving the appearance properties of a coating film manufactured therefrom. When the hydroxyl value of the polyurethane dispersion resin is below the above range, the resin stability may be lowered, which may cause a problem of lowering the storability of the manufactured coating composition, and when it exceeds the above range, the viscosity of the composition may be increased due to increased resin cohesion, which may cause a problem of lowering the workability and the water resistance of the coating film.
[0039] The polyurethane dispersion resin may have a weight average molecular weight of 18,500 to 22,500 g / mol, or 19,000 to 22,000 g / mol. When the weight average molecular weight of the polyurethane dispersion resin is within the above range, the intermediate coating composition has excellent drying properties, cold chipping resistance, and impact resistance. When the weight average molecular weight of the polyurethane dispersion resin is less than the above range, there is a problem that the mechanical properties of the produced coating film are deteriorated due to the small molecular weight, and when it exceeds the above range, the flowability is deteriorated due to the increase in molecular weight, so that the coating film becomes brittle, reducing smoothness and reducing scratch resistance.
[0040] The polyurethane dispersion resin may be included in the composition in an amount of 5 to 15 wt%, or 7 to 13 wt%, based on the total weight of the intermediate coating composition. When the polyurethane dispersion resin is included within the above content range, it has the effect of improving tensile strength, flexibility, elongation, adhesion, abrasion resistance, scratch resistance, and film smoothness. When the content of the polyurethane dispersion resin in the composition is less than the above range, there is a problem that flexibility is reduced, resulting in reduced tensile strength and scratch resistance, and when it exceeds the above range, the viscosity of the composition becomes excessively high, resulting in reduced workability and drying properties, which may cause problems of reduced appearance and mechanical properties.
[0041] polyester resin
[0042] Polyester resin plays a role in forming the appearance characteristics and physical properties of a coating film manufactured from a composition containing it.
[0043] A polyester resin can be prepared by reacting a carboxylic acid compound with a diol compound. For example, the polyester resin can be prepared by reacting at least one carboxylic acid compound selected from the group consisting of adipic acid (AA), isophthalic acid (IPA), trimaletic anhydride (TMA), alicyclic acids, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, and derivatives thereof; and at least one diol compound selected from the group consisting of 1,6-hexanediol (1,6-HD), neopentyl glycol (NPG), trimethylol propane (TMP), ethylene glycol, propylene glycol, diethylene glycol, butanediol, 1,4-hexanediol, and 3-methylpentanediol.
[0044] The polyester resin may have a solid content (NV) of 70 to 80 wt%, or 72 to 78 wt%, based on the total weight of the resin. When the solid content of the polyester resin is within the above range, the storage stability of the resin is improved, workability is excellent, and gloss and curing reactivity are improved. When the solid content of the polyester resin is below the above range, the viscosity is excessively low, which may cause a problem in that the workability of the intermediate coating composition containing it is insufficient, and when it exceeds the above range, the viscosity of the polyester resin is excessively high, which may reduce stability during reaction.
[0045] The polyester resin may have a viscosity of 2,100 to 2,400 cps, or 2,200 to 2,300 cps at 25°C. When the viscosity of the polyester resin at 25°C is within the above range, the viscosity of the intermediate coating composition is appropriate, thereby improving workability, and the solid content increases, thereby improving the SVR (Solid Volume Ratio) of the paint. When the viscosity of the polyester resin at 25°C is less than the above range, the viscosity of the composition is too low, which may cause problems such as poor formation of a manufactured coating film, resulting in poor paint flowability, adhesion, and scratch resistance. When the viscosity exceeds the above range, the workability of the composition may be insufficient, which may cause problems such as poor appearance characteristics of the manufactured coating film.
[0046] The polyester resin may have an acid value (Av) of 24 to 30 mgKOH / g, or 26 to 28 mgKOH / g. When the acid value of the polyester resin is within the above range, the composition containing it has the effect of improving the crosslinking density and curing reactivity. When the acid value of the polyester resin is below the above range, the resin stability may be reduced, which may cause a problem of reduced storage properties of the manufactured paint composition. When the acid value exceeds the above range, the viscosity of the composition may be increased due to increased resin cohesion, which may cause problems of reduced workability and water resistance of the coating film.
[0047] The polyester resin may have a hydroxyl value (OHv) of 90 to 105 mgKOH / g, or 95 to 100 mgKOH / g. When the hydroxyl value of the polyester resin is within the above range, the composition containing it has the effect of low-temperature curing and improving crosslinking density. When the hydroxyl value of the polyester resin is below the above range, the resin stability may be lowered, which may cause a problem of lowering the storage property of the manufactured paint composition. When the hydroxyl value exceeds the above range, the viscosity of the composition may be increased due to increased resin cohesion, which may cause a problem of lowering the workability and water resistance of the coating film.
[0048] The polyester resin may have a weight average molecular weight of 2,000 to 4,000 g / mol, or 2,500 to 3,500 g / mol. When the weight average molecular weight of the polyester resin is within the above range, the solid content increases, thereby improving the SVR (Solid Volume Ratio) of the paint. When the weight average molecular weight of the polyester resin is less than the above range, the molecular weight is small, so that the water resistance, weather resistance, and scratch resistance of the produced coating film are insufficient, and when the weight average molecular weight exceeds the above range, the flowability is reduced due to the increase in molecular weight, so that the workability of the intermediate coating composition containing it is poor, and the surface smoothness is poor, which may cause a problem that it is difficult to produce a coating film having an excellent appearance.
[0049] The polyester resin may be included in the composition in an amount of 5 to 15 wt%, or 7 to 13 wt%, based on the total weight of the intermediate coating composition. When the polyester resin is included within the above content range, the paint can have high gloss, and the impact resistance and chipping resistance are improved. When the content of the polyester resin is less than the above range, the drying property is reduced, which may cause problems such as reduced adhesion, gloss, hardness, and durability of the coating film. When the content exceeds the above range, the drying proceeds quickly, which may cause problems such as reduced painting workability and paint flow of the composition, which may cause reduced coating film appearance and scratch resistance.
[0050] Isocyanate curing agent
[0051] Isocyanate-based curing agents act to cure by cross-linking with each component of an intermediate coating composition, thereby improving the appearance and gloss of a coating film produced from an intermediate coating composition containing the same. For example, the isocyanate group of an isocyanate-based curing agent reacts with the hydroxyl groups of other components in the coating composition to form a urethane bond, thereby curing the coating composition.
[0052] Non-limiting examples of isocyanate curing agents include methylenediphenyl diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, tetramethylxylene diisocyanate, polyisocyanate, etc., and these may be used alone or in combination of two or more.
[0053] The isocyanate-based curing agent may have a solid content (NV) of 90 to 100 wt%, or 95 to 100 wt%, based on the total weight of the curing agent. When the solid content of the isocyanate-based curing agent is within the above range, it has the effect of improving the crosslinking density, thereby improving the adhesion and hardness of the produced coating film, and enabling curing at a low temperature of 120°C or lower. When the solid content of the isocyanate-based curing agent is below the above range, a problem of deterioration in hardness and appearance characteristics due to reduced curing may occur, and when it exceeds the above range, a problem of deterioration in adhesion, impact resistance, and scratch resistance may occur due to brittleness of the coating film due to excessive curing.
[0054] The isocyanate-based curing agent may have a viscosity at 25°C of 2,500 to 4,500 cps, or 3,000 to 4,000 cps. When the viscosity of the isocyanate-based curing agent at 25°C is within the above range, it has excellent gloss and appearance effects. When the viscosity of the isocyanate-based curing agent at 25°C is lower than the above range, there is a problem that the adhesion and scratch resistance of the coating film are reduced due to the low viscosity and the coating film is not formed, and when it exceeds the above range, the workability of the composition is poor, which may cause a problem that the appearance characteristics of the manufactured coating film are insufficient.
[0055] The isocyanate curing agent may have an NCO content of 18 to 23%, or 20 to 21%.
[0056] When the NCO content of the isocyanate-based curing agent is within the above range, it has an appropriate reactivity with the resin of the composition, so it can be cured at low temperatures and has excellent mechanical properties. When the NCO content of the isocyanate-based curing agent is below the above range, the reactivity of the composition is insufficient, resulting in a low crosslinking density, which may prolong the drying time. When the NCO content of the isocyanate-based curing agent is above the above range, the drying time is shortened, but the flexibility of the coating film may be reduced due to the rapid reaction rate.
[0057] The isocyanate-based curing agent may be included in the composition in an amount of 5 to 15 wt%, or 7 to 13 wt%, based on the total weight of the intermediate coating composition. When the isocyanate-based curing agent is included within the above content range, it has the effect of improving the crosslinking density, thereby improving the adhesion and hardness of the produced coating film, and enabling curing at a low temperature of 120°C or lower.
[0058] If the content of the isocyanate-based hardener is below the above range, there is a problem of deterioration in hardness and appearance characteristics due to reduced hardening, and if it exceeds the above range, there is a problem of deterioration in adhesion, impact resistance, and scratch resistance due to brittleness of the coating film due to excessive hardening.
[0059] solvent
[0060] The intermediate coating composition according to the present invention may additionally include a solvent. The solvent controls the viscosity of the composition and serves to reduce the generation of volatile organic compounds (VOCs). For example, the solvent may include one or more types of water selected from the group consisting of deionized water, pure water, ultrapure water, and distilled water. In addition to water, the solvent may additionally include an organic solvent.
[0061] The solvent may be included in the composition in an amount of 15 to 40 wt%, or 20 to 35 wt%, based on the total weight of the intermediate coating composition. When the solvent content in the composition is within the above range, problems such as reduced water dispersibility of resins in the composition, reduced environmental friendliness, which is an advantage of water-based paints, and insufficient evaporation of water, resulting in coating defects such as pinholes and stains in the final coating film can be prevented.
[0062] additives
[0063] The intermediate coating composition according to the present invention may additionally include one or more additives selected from the group consisting of a softener, a neutralizer, a catalyst, an ultraviolet absorber, a leveling agent, an antifoaming agent, a wetting agent, and a wax.
[0064] The additive may be included in the composition in an amount of 1 to 10 wt%, or 3 to 8 wt%, based on the total weight of the intermediate coating composition.
[0065] The solvent affects the smoothness of the coating film being manufactured, provides storage stability to the intermediate coating composition, lowers the minimum coating film formation temperature, and controls the volatility of the solvent during the coating process. Examples of the solvent include, but are not limited to, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, propylene glycol, N-methyl-2-pyrrolidone, n-propyl alcohol, i-propyl alcohol, n-butanol, propylene glycol monomethyl ether, butyl glycol, hexyl glycol, 2-ethylhexyl alcohol, and butyl carbitol.
[0066] Neutralizers improve the storage stability of intermediate coating compositions and control the pH (to a pH level of 7.5 to 9.0). Neutralizers include, for example, trialkylamines such as trimethylamine, triethylamine, and tributylamine; N,N-dialkylalkanolamines such as N,N-dimethylethanolamine, N,N-dimethylpropanolamine, N,N-dipropylethanolamine, and 1-dimethylamino-2-methyl-2-propanol; N-alkyl-N,N-dialkanolamines; and trialkanolamines such as triethanolamine; tertiary amine compounds such as ammonia; trimethylammonium hydroxide; sodium hydroxide; potassium hydroxide; and lithium hydroxide.
[0067] Catalysts prevent incomplete curing of intermediate coating compositions and improve the mechanical properties of the coating film produced from them. Examples of catalysts include amine-containing phosphate compounds.
[0068] The UV absorber blocks ultraviolet rays from reaching the manufactured coating film and improves the weather resistance of the final coating film. The UV absorber may be a benzotriazole-based UV absorber. For example, the benzotriazole-based UV absorber is α-[3-[3-(2H-Benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-hydroxypoly(oxy-1,2-ethanediyl)). α-[3-[3-(2H-Benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxapropyl]-ω-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxapropoxy]poly(oxy-1,2-ethanediyl)(α-[3-[3-(2H-Benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropoxy]poly(oxy-1,2-ethanediyl)), Examples include 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-methyl ester.
[0069] Leveling agents serve to impart leveling and wettability to the manufactured coating film. Leveling agents may be cationic, anionic, or nonionic surfactants, and may include, for example, nonionic surfactants.
[0070] Defoaming agents suppress the formation of bubbles during paint production and suppress or eliminate pinholes and popping that occur during film formation. Any conventional defoaming agent suitable for use in paint compositions may be used without particular restrictions. Examples of commercially available defoaming agents include BYK-011, BYK-015, and BYK-072, Air Products' DF-21, Munzing's agitan 281, and Sannopco's Foamster-324.
[0071] Wetting agents serve to improve the leveling and wettability of a coating film prepared from a composition containing them, and are not particularly limited as long as they are commonly used in paint compositions. For example, wetting agents may include polyether-modified polysiloxane-based or acetylene alcohol-based wetting agents.
[0072] Wax serves to prevent problems such as sagging caused by slow drying of a coating film manufactured from a composition containing it, and is not particularly limited as long as it is commonly used in paint compositions. For example, waxes may include ethylene-vinyl-acetate waxes.
[0073] Two-component paint composition
[0074] The intermediate coating composition may be a two-component coating composition comprising a main component and a hardener component. For example, the intermediate coating composition may comprise a main component comprising an acrylic emulsion resin, a polyurethane dispersion resin, a polyester resin, a solvent, and an additive; and a hardener component comprising an isocyanate-based hardener. In addition, the intermediate coating composition may be used after mixing the main component and the hardener component prior to application.
[0075] The above intermediate coating composition may have a solid content of 40 to 60 wt%, or 45 to 55 wt%. When the solid content of the intermediate coating composition is within the above range, the composition has the advantage of providing appropriate painting workability.
[0076] The above intermediate coating composition can be cured at 70°C to 120°C, 80°C to 110°C, or 90°C to 100°C. Since the intermediate coating composition can be cured within the above temperature range, it is economical because it can reduce the cost required for the painting process, and since the body and the material parts attached thereto can be painted as a single unit, it can prevent the problem of the parts and the body having different colors after painting. In addition, since the body and parts can both be painted in a single painting process, it is possible to reduce the hassle and cost loss in the process.
[0077] The above intermediate coating composition may have a Ford Cup viscosity of 30 to 50 seconds, or 35 to 45 seconds, based on Ford Cup No. 4 at 25°C. If the viscosity of the intermediate coating composition at 25°C is below the above range, problems such as vertical surface run-off may occur, and if it exceeds the above range, the viscosity of the composition may be high, which may deteriorate the appearance characteristics of a coating film produced therefrom or may cause a load on the coating machine, resulting in a malfunction of the coating machine.
[0078] As described above, the intermediate coating composition according to the present invention can perform the heat curing temperature of the painting process at a low temperature of 120°C or lower, which is lower than the conventional temperature, thereby reducing the cost required for the painting process and being economical. In addition, the intermediate coating composition according to the present invention can produce a coating film having excellent appearance characteristics and mechanical properties, making it suitable as a paint for painting automobile parts and bodywork. Furthermore, the intermediate coating composition according to the present invention is environmentally friendly and economical due to the VOC reduction effect caused by the high solid content.
[0079] Hereinafter, the present invention will be described in more detail through examples. However, these examples are provided solely to aid understanding of the present invention and are not intended to limit the scope of the present invention in any way.
[0080] [Example]
[0081] Examples 1 to 21 and Comparative Examples 1 to 11. Preparation of intermediate coating compositions
[0082] An intermediate paint composition was prepared by stirring and mixing each component as described in Tables 1 to 3 below, so that the viscosity was 40 seconds at 25°C based on Ford Cup No. 4.
[0083]
[0084]
[0085]
[0086] Below, the manufacturers and product names of each component used in the comparative examples and examples are shown in Table 4 below.
[0087]
[0088] [Test Example] Evaluation of the characteristics of manufactured coating films
[0089] After applying the intermediate coating compositions of Examples and Comparative Examples on the electrodeposition-coated specimens, they were dried at room temperature for 15 minutes to form an intermediate coating film having a thickness of 20 μm. Thereafter, a base coat (manufacturer: KCC, product name: WT3062, dry film thickness: 35 μm) and a clear coat (manufacturer: KCC, product name: TT6830, dry film thickness: 40 μm) were applied, and the final coating film was produced by drying and curing at 90°C for 20 minutes.
[0090] The appearance characteristics and physical properties of the final coating were measured using the following methods, and the results are shown in Table 5.
[0091] (1) Painting workability
[0092] The painting workability of the intermediate paint composition was evaluated by looking at the spray state of the composition during bell painting, and the spray state was judged and compared and evaluated according to the atomization state.
[0093] (2) Exterior of the coating
[0094] The CF value of the final coating was measured using an automotive exterior measuring device, Wave Scan DOI (BYK Gardner), and the higher the CF value, the better the exterior properties of the coating. Specifically, a CF value of 65 or higher was evaluated as excellent (◎), 60 or higher but lower than 65 as good (○), 55 or higher but lower than 60 as average (△), and less than 55 as poor (×).
[0095] (3) Gloss
[0096] The 20° gloss of the final coating was measured, and if the measured gloss value was 90 or higher, it was evaluated as excellent (◎), if it was 88 or higher but less than 90, it was evaluated as good (○), if it was 86 or higher but less than 88, it was evaluated as average (△), and if it was less than 86, it was evaluated as poor (×).
[0097] (4) Adhesion
[0098] After painting and curing the intermediate paint compositions of the examples and comparative examples, the adhesion was evaluated using the baduk method.
[0099] Specifically, the above-mentioned Baduk method measured the adhesion by drawing 100 squares (2 mm wide × 2 mm high) horizontally and vertically on the repainted film with a blade and removing them using tape. At this time, if 100% of the 100 squares were completely attached, it was evaluated as excellent (◎), if 70% or more but less than 100% of the remaining squares were attached, it was evaluated as good (○), if 50% or more but less than 70% of the remaining squares were attached, it was evaluated as average (△), and if less than 50% of the remaining squares were attached, it was evaluated as poor (×).
[0100] (5) Impact resistance
[0101] When a 500g weight was dropped from a height of 30cm onto the final coating, the impact resistance was evaluated by observing the surface of the final coating. Specifically, if there was no crack or trace of impact on the surface, it was evaluated as (◎), if there was a trace, it was evaluated as average (△), and if the final coating was cracked or split, it was evaluated as poor (×).
[0102] (6) Water resistance
[0103] After the final coating was immersed in a 40℃ constant temperature bath for 10 days, the adhesion was measured using the same method as the baduk method in item (4), and the water resistance of the coating was evaluated using the same evaluation criteria.
[0104] (7) Fluidity
[0105] A specimen having an electrodeposited coating formed on a steel plate with a hole of 5 mm in diameter was hung vertically, and the intermediate coating compositions of the examples and comparative examples were applied in the same manner as described above, dried and cured, and the surface of the produced coating was observed to evaluate the paint flowability of the composition.
[0106] Specifically, we observed that paint formed at the bottom of the hole. The thickness (㎛) of the film at the starting point where flow occurrence was observed was recorded as the flow limit film thickness. At this time, the lower the measured flow limit film thickness, the more insufficient the paint flowability was judged. At this time, if the flow limit film thickness was 25㎛ or more, it was evaluated as excellent (◎), if it was 20㎛ or more but less than 25㎛, it was evaluated as good (○), if it was 15㎛ or more but less than 20㎛, it was evaluated as average (△), and if it was less than 15㎛, it was evaluated as poor (×).
[0107] (8) Cold-resistant chipping resistance
[0108] After leaving the final coating at -20℃ for 3 hours, a 50g chipping stone was pushed out at a pressure of 4 bar to strike the surface of the final coating. At this time, if the damaged area of the final coating is 1mm or less, it is evaluated as excellent (◎), if it is between 1mm and 2mm, it is evaluated as good (○), if it is between 2mm and 3mm, it is evaluated as average (△), and if it is between 3mm and 3mm, it is evaluated as poor (×).
[0109] (9) Repainting adhesion
[0110] After stripping the base coat and clear coat from the final coating, the intermediate coating compositions and clear paints of the examples and comparative examples were recoated and cured in the same manner as described above to produce a recoated film. Thereafter, the adhesion of the recoated film was measured using the Go-Mok method.
[0111] Specifically, the above-mentioned Baduk method measured the adhesion by drawing 100 squares (2 mm wide × 2 mm high) horizontally and vertically on the repainted film with a blade and removing them using tape. At this time, if 100% of the 100 squares were completely attached, it was evaluated as excellent (◎), if 70% or more but less than 100% of the remaining squares were attached, it was evaluated as good (○), if 50% or more but less than 70% of the remaining squares were attached, it was evaluated as average (△), and if less than 50% of the remaining squares were attached, it was evaluated as poor (×).
[0112]
[0113]
[0114]
[0115] As shown in Tables 5 to 7, the intermediate coating composition of the example has excellent painting workability and paint flowability, and the coating film manufactured therefrom also has excellent mechanical properties such as appearance characteristics, gloss, repainting adhesion, impact resistance, water resistance, and cold chipping resistance.
[0116] On the other hand, Comparative Example 1, which did not contain acrylic emulsion resin, had poor film appearance, gloss, and impact resistance, and Comparative Example 2, which did not contain polyurethane dispersion resin, had poor impact resistance and cold chipping resistance.
[0117] Comparative Example 3, which did not contain polyester resin, had poor coating film appearance, adhesion, impact resistance, water resistance, cold chipping resistance, and repainting adhesion.
[0118] Comparative Example 4, in which the hydroxyl value of the acrylic emulsion resin was below the numerical range of the present invention, had poor impact resistance, water resistance, and cold chipping resistance, and Comparative Example 5, in which the hydroxyl value of the acrylic emulsion resin was above the numerical range of the present invention, had poor film appearance, gloss, and cold chipping resistance.
[0119] Comparative Example 6, in which the weight average molecular weight of the acrylic emulsion resin was below the numerical range of the present invention, had poor impact resistance, water resistance, and cold chipping resistance, and Comparative Example 7, in which the weight average molecular weight of the acrylic emulsion resin was above the numerical range of the present invention, had poor film appearance, gloss, and cold chipping resistance.
[0120] Comparative Example 8, in which the hydroxyl value of the polyurethane dispersion resin was below the numerical range of the present invention, had poor adhesion, impact resistance, water resistance, and cold chipping resistance, and Comparative Example 9, in which the hydroxyl value of the polyurethane dispersion resin was above the numerical range of the present invention, had poor coating workability, coating appearance, gloss, and impact resistance.
[0121] Comparative Example 10, in which the hydroxyl value of the polyester resin was below the numerical range of the present invention, had poor film appearance, gloss, impact resistance, water resistance, and cold chipping resistance, and Comparative Example 11, in which the hydroxyl value of the polyester resin exceeded the numerical range of the present invention, had poor film appearance, adhesion, impact resistance, and repainting adhesion.
[0122] [Test Example] Evaluation of the characteristics of manufactured coatings according to curing temperature
[0123] Example 22
[0124] The intermediate coating composition of Example 1 was applied onto the electrodeposition-coated specimen, and dried at room temperature for 15 minutes to form an intermediate coating film having a thickness of 20 μm. Thereafter, a base coat (manufacturer: KCC, product name: WT3062, dry film thickness: 35 μm) and a clear coat (manufacturer: KCC, product name: TT6830, dry film thickness: 40 μm) were applied, and the final coating film was produced by drying and curing at 100°C for 20 minutes.
[0125] Example 23
[0126] The final coating film was manufactured in the same manner as in Example 22 above, except that the curing temperature was changed to 70°C.
[0127] Example 24
[0128] The final coating film was manufactured in the same manner as in Example 22 above, except that the curing temperature was changed to 120°C.
[0129] Example 25
[0130] The final coating film was manufactured in the same manner as in Example 22 above, except that the curing temperature was changed to 60°C.
[0131] Example 26
[0132] The final coating film was manufactured in the same manner as in Example 22 above, except that the curing temperature was changed to 130°C.
[0133] The appearance characteristics and physical properties of the final coating were measured using the same method as above, and the results are shown in Table 8.
[0134]
[0135] As shown in Table 8, in the cases of Examples 22 to 24 where the curing temperature of the manufactured coating was within the range of 70°C to 120°C, the properties of the coating were all excellent or good.
[0136] In the case of Example 25, where the curing temperature of the coating was 60°C, the coating appearance, gloss, adhesion, and impact resistance were average, and in the case of Example 26, where the curing temperature was 130°C, the painting workability, coating appearance, adhesion, impact resistance, and cold chipping resistance were average.
[0137] Hereinafter, various embodiments of the present invention will be described.
[0138] [Item 1] A paint composition for intermediate use, comprising an acrylic emulsion resin, a polyurethane dispersion resin, a polyester resin, and an isocyanate-based curing agent, wherein the acrylic emulsion resin has a hydroxyl value of 110 to 140 mgKOH / g and a weight average molecular weight of 22,000 to 26,000 g / mol, the polyurethane dispersion resin has a hydroxyl value of 110 to 140 mgKOH / g, and the polyester resin has a hydroxyl value of 90 to 105 mgKOH / g.
[0139] [Item 2] In Item 1, the acrylic emulsion resin has an acid value of 0.01 to 2 mgKOH / g, a solid content of 30 to 50 wt% based on the total weight of the resin, a glass transition temperature of 65 to 76°C, and a viscosity at 25°C of 800 to 1,800 cps, a paint composition for intermediate use.
[0140] [Item 3] In Item 1, a polyurethane dispersion resin has an acid value of 18 to 25 mgKOH / g, a solid content of 30 to 40 wt% based on the total weight of the resin, a weight average molecular weight of 18,500 to 22,500 g / mol, and a viscosity at 25°C of 5 to 50 cps, a paint composition for intermediate use.
[0141] [Item 4] In Item 1, a mid-coating composition, wherein the polyester resin has an acid value of 24 to 30 mgKOH / g, a solids content of 70 to 80 wt% based on the total weight of the resin, a weight average molecular weight of 2,000 to 4,000 g / mol, and a viscosity at 25°C of 2,100 to 2,400 cps.
[0142] [Item 5] In Item 1, an intermediate coating composition in which the isocyanate-based curing agent has a solid content of 90 to 100 wt% based on the total weight of the resin, a viscosity at 25°C of 2,500 to 4,500 cps, and an NCO content of 18 to 23%.
[0143] [Item 6] A mid-coating composition comprising, based on the total weight of the mid-coating composition of Item 1, 37 to 47 wt% of acrylic emulsion resin, 5 to 15 wt% of polyurethane dispersion resin, 5 to 15 wt% of polyester resin, and 5 to 15 wt% of isocyanate-based curing agent.
[0144] [Item 7] In item 1, the intermediate coating composition is cured at 70°C to 120°C.
Claims
1. Contains acrylic emulsion resin, polyurethane dispersion resin, polyester resin, and isocyanate curing agent. The acrylic emulsion resin has a hydroxyl value of 110 to 140 mgKOH / g and a weight average molecular weight of 22,000 to 26,000 g / mol. The polyurethane dispersion resin has a hydroxyl value of 110 to 140 mgKOH / g. A mid-coating paint composition, wherein the polyester resin has a hydroxyl value of 90 to 105 mgKOH / g.
2. In claim 1, An intermediate coating composition, wherein the acrylic emulsion resin has an acid value of 0.01 to 2 mgKOH / g, a solid content of 30 to 50 wt% based on the total weight of the resin, a glass transition temperature of 65 to 76°C, and a viscosity at 25°C of 800 to 1,800 cps.
3. In claim 1, A mid-coating composition, wherein the polyurethane dispersion resin has an acid value of 18 to 25 mgKOH / g, a solid content of 30 to 40 wt% based on the total weight of the resin, a weight average molecular weight of 18,500 to 22,500 g / mol, and a viscosity at 25°C of 5 to 50 cps.
4. In claim 1, A mid-coating composition, wherein the polyester resin has an acid value of 24 to 30 mgKOH / g, a solid content of 70 to 80 wt% based on the total weight of the resin, a weight average molecular weight of 2,000 to 4,000 g / mol, and a viscosity at 25°C of 2,100 to 2,400 cps.
5. In claim 1, An intermediate coating composition, wherein the isocyanate-based curing agent has a solid content of 90 to 100 wt% based on the total weight of the resin, a viscosity at 25°C of 2,500 to 4,500 cps, and an NCO content of 18 to 23%.
6. In claim 1, A mid-coating composition comprising, based on the total weight of the mid-coating composition, 37 to 47 wt% of an acrylic emulsion resin, 5 to 15 wt% of a polyurethane dispersion resin, 5 to 15 wt% of a polyester resin, and 5 to 15 wt% of an isocyanate-based curing agent.
7. In claim 1, The above intermediate coating composition is a intermediate coating composition that is cured at 70°C to 120°C.
Citation Information
Patent Citations
Aqueous paint compositions for automotive surface coating and method of coating automobiles using the same
KR1020170091226A
Liquid toothpaste composition for orthodontic teeth, which uses fullerene C60 as the main ingredient
KR1020210142423A
Rotor core of motor and assembling method thereof
KR1020220055252A
Cathode active material for lithium secondary battery, manufacturing method of the same, and lithium secondary battery comprising the same
KR1020240056313A
Aqueous coating composition based on a binder mixture as base coat