Oil absorbent cloth and method of manufacturing same

The oil absorption cloth, featuring polyester fiber foam, laminated polypropylene fiber sheets, and a water-repellent coating, addresses the challenge of low moisture absorption and high oil absorption, demonstrating enhanced porosity and bulkiness for improved oil absorption performance.

WO2024225863A1PCT designated stage expired Publication Date: 2024-10-31HAN YOUNG INDUSTRIAL CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/095019
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-01-10
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing oil absorbent fabrics face challenges in achieving low moisture absorption while maintaining excellent oil absorption capabilities, particularly in industrial and coastal water applications.

Method used

The development of an oil absorption cloth comprising polyester fiber foam, laminated and bonded polypropylene fiber sheets, and a water-repellent coating, specifically using a mixture of 10-30% 6-denier polyester fibers and 70-90% 20-denier polyester fibers, with a water-repellent agent containing wax, to enhance oil absorption and reduce moisture absorption.

Benefits of technology

The solution results in an oil absorption cloth with improved porosity, bulkiness, and air permeability, achieving superior oil absorption rates while minimizing moisture absorption, thus effectively addressing the limitations of prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024095019_31102024_PF_FP_ABST
    Figure KR2024095019_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an oil absorbent cloth and a method of manufacturing same, and the oil absorbent cloth comprises: a polyester fiber foam; a polypropylene fiber sheet laminated on and bonded to the polyester fiber foam; and a water-repellent agent coated on the polyester fiber foam and the polypropylene fiber sheet. According to the present invention, an oil adsorbent cloth having a low water absorption rate and excellent oil adsorption is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Oil absorbent pad and its manufacturing method

[0001] The present invention relates to an oil absorbent cloth and a method for manufacturing the same, and more particularly, to an oil absorbent cloth having low moisture absorption rate and excellent oil absorption and a method for manufacturing the same.

[0002]

[0003] In general, oil absorbents are widely used for disaster recovery related to oil spills, oil spill accidents from ships operating in coastal waters, and oil contamination removal from various industrial fields.

[0004] As disclosed in Korean Patent Publication No. 10-1032121, etc., existing oil absorbent pads were manufactured by putting feathers of ducks, geese, chickens, etc. in mesh nets or bags, or by mixing feathers with synthetic fibers to make non-woven fabrics.

[0005] Recently, problems such as feather supply and demand have been resolved by manufacturing oil absorbent pads using polypropylene resin. Specifically, oil absorbent pads are manufactured by melt-blown molding of polypropylene resin and fusing a cover with heat, high frequency, or ultrasonic waves. A related prior art is Korean Patent No. 10-1903145. This prior art manufactures an oil absorbent pad by molding an absorbent portion using the melt-blown method and bonding a cover portion to the absorbent portion using ultrasonic waves from a fusing machine.

[0006]

[0007] The purpose of the present invention is to provide an oil absorbent cloth having low moisture absorption rate and excellent oil absorption, and a method for manufacturing the same.

[0008]

[0009] The technical problems to be solved by the present invention are not limited to the technical problems mentioned above, and other technical problems not mentioned can be clearly understood by a person having ordinary skill in the technical field to which the present invention belongs from the description below.

[0010]

[0011] The oil absorbent fabric of the present invention for achieving the above purpose comprises: polyester fiber foam; a polypropylene fiber sheet laminated and bonded to the polyester fiber foam; and a water repellent coated on the polyester fiber foam and the polypropylene fiber sheet.

[0012] More specifically, the polyester fiber foam may be composed of 10 to 30 wt% of 6 denier polyester fiber and 70 to 90 wt% of 20 denier polyester fiber.

[0013]

[0014] The method for manufacturing an oil absorbent pad of the present invention comprises a first step of mixing polyester fibers having different thicknesses; a second step of forming a polyester fiber foam using the mixed fibers and laminating a polypropylene fiber sheet on the polyester fiber foam; a third step of forming an absorbent pad base by laminating the polyester fiber foam and the polypropylene fiber sheet; and a fourth step of coating a water-repellent agent containing wax on the absorbent pad base.

[0015] More specifically, in the first step, 10 to 30 wt% of 6 denier polyester fiber and 70 to 90 wt% of 20 denier polyester fiber can be mixed.

[0016] The above water repellent can be formulated to contain 10 to 15 wt% of the above wax based on the total weight.

[0017]

[0018] According to the present invention, an oil absorbent cloth having low moisture absorption rate and excellent oil absorption is provided.

[0019]

[0020] Fig. 1 is a drawing showing a side view of the oil absorbent fabric of the present invention.

[0021]

[0022] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. Detailed descriptions of well-known functions and configurations that may unnecessarily obscure the gist of the present invention will be omitted.

[0023] The oil absorbent fabric of the present invention is manufactured by a mixing process in which polyester fibers of different deniers are fed into a hopper and mixed, a blending process, a carding process in which the polyester fibers are arranged in a combing manner, a lapping process in which the arranged polyester fibers are spread out and overlapped to adjust the size and thickness of the polyester fibers to form a polyester fiber foam (10) in the form of a fiber web, and at the same time, a laminating process in which a polypropylene fiber sheet (20) is laminated on the formed polyester fiber foam (10), a needle punching process in which the polyester fiber foam (10) and the polypropylene fiber sheet (20) are bound and laminated, an ironing process in which the surface is made even, a metal detecting process, and a wrapping process to create an absorbent fabric, and then coating a water repellent on the absorbent fabric and drying it.

[0024] The oil absorbent fabric of the present invention manufactured through this process is composed of polyester fiber foam (10), a polypropylene fiber sheet (20) laminated and bonded to the polyester fiber foam (10), and a water repellent coated on the polyester fiber foam (10) and the polypropylene fiber sheet (20).

[0025] The polypropylene fiber sheet (20) is made of polypropylene fibers, and since polypropylene fibers have superior strength and elongation than polyester fibers, the polypropylene fiber sheet (20) forms a base layer to support the polyester fiber foam (10) and maintain the shape of the sheet.

[0026] In addition, since polypropylene fibers have a significantly lower specific gravity than polyester fibers and superior floating properties, the polypropylene fiber sheet (20) floats the polyester fiber foam (10) on water, allowing the polyester fiber foam (10) to absorb oil.

[0027] Such a polypropylene fiber sheet (20) may be a spunbond polypropylene nonwoven fabric manufactured by a spunbond method of continuously bonding radiated polypropylene fibers.

[0028] Polyester fiber foam (10) maintains its shape with the support of a polypropylene fiber sheet (20) and absorbs and removes oil. It is preferable that this polyester fiber foam (10) be formed by mixing 10 to 30 wt% of 6-denier polyester fibers of different thicknesses and 70 to 90 wt% of 20-denier polyester fibers.

[0029] When polyester fiber foam (10) is manufactured through the process described above using only 20 denier polyester fibers, the bulkiness is excellent and large voids are formed between the fibers, but the density is low, so the polyester fiber foam (10) cannot maintain its shape and collapses without strength, causing a problem in which the voids collapse.

[0030] When polyester fiber foam (10) is manufactured through the process described above using only 6 denier polyester fibers, the polyester fiber foam (10) has a high density, which is advantageous in maintaining its shape, but there is a problem in that the oil absorption capacity is reduced due to the narrow spacing between fibers and the micropores.

[0031] Therefore, the 6 denier polyester fiber controls the density of the polyester fiber foam (10), allowing the 20 denier polyester fiber to maintain its shape and pores and effectively absorb oil.

[0032] If the 6-denier polyester fiber is less than 10% by weight of the total weight of the polyester fiber foam (10), it is difficult to maintain the shape of the polyester fiber foam (10), and if it exceeds 30% by weight, there is a problem of the oil absorption capacity of the polyester fiber foam (10) being reduced.

[0033] In addition, if the 20-denier polyester fiber is less than 70% by weight of the total weight of the polyester fiber foam (10), there is a problem that the oil absorption capacity of the polyester fiber foam (10) is reduced, and if it exceeds 90% by weight, it is difficult to maintain the shape of the polyester fiber foam (10).

[0034] The polyester fiber constituting the polyester fiber foam (10) may be a 100% recycled polyester fiber using PET flakes (thin solid pieces) made by crushing PET bottles, or may be a polypropylene fiber or a regenerated polypropylene fiber constituting the polypropylene fiber sheet (20).

[0035] In this way, the needle punching process of making an absorbent fabric by bonding and laminating polyester fiber foam (10) and polypropylene fiber sheet (20) made by mixing 10 to 30 weight% of 6 denier polyester fiber and 70 to 90 weight% of 20 denier polyester fiber is preferably performed by changing the conditions of the needle punching process of general nonwoven fabric.

[0036] At this time, it is preferable to make an absorbent fabric by laminating 80 to 85 weight% of polyester fiber foam (10) and 15 to 20 weight% of polypropylene fiber sheet (20) relative to the total weight of the absorbent fabric and then needle punching. It is preferable that the polypropylene fiber sheet (20) have a weight of 40 to 80 g / sqm.

[0037] If the polyester fiber foam (10) is less than 80 wt% or more than 85 wt% of the total weight of the absorbent fabric, the oil absorption capacity or shape retention capacity is reduced, and if the polypropylene fiber sheet (20) is less than 15 wt% or more than 20 wt%, the shape retention capacity and oil absorption capacity are reduced. Preferably, the absorbent fabric is made by combining 80 wt% of the polyester fiber foam (10) with 20 wt% of the polypropylene fiber sheet (20) relative to the total weight of the absorbent fabric.

[0038] When polyester fiber foam (10) and polypropylene fiber sheet (20) are bonded through a general nonwoven needle punching process (15,000 needles in the needle plate, 10 to 12 mm needle depth, 500 to 800 rpm needle punching speed), the mechanical interlocking of fibers constituting the polyester fiber foam (10) and the polypropylene fiber sheet (20) is manufactured densely, so that the density increases, the thickness decreases, and the durability decreases, resulting in a problem in that the oil adsorption capacity of the polyester fiber foam (10) and the buoyancy of the polypropylene fiber sheet (20) are reduced.

[0039] For this reason, it is desirable to arrange the needles diagonally with a needle plate having a number (density) 50% less than that used in a general nonwoven needle punching process, to punch with a needle depth deeper than the existing needle depth, and to punch with a needle punching speed slower than the existing needle punching speed.

[0040] For example, the number of needles in the needle plate is 7,500, which is 50% less than before, the needle depth is 17 to 18.5 mm, which is deeper than before, and the needle punching speed is 300 to 400 rpm, which is slower than before, to bind the polyester fiber foam (10) and the polypropylene fiber sheet (20), thereby greatly improving the void ratio between the fibers of the polyester fiber foam (10), and further enhancing the oil adsorption capacity.

[0041] In addition, two needle punching machines can be arranged, and in order to bind the polyester fiber foam (10) and the polypropylene fiber sheet (20) while minimizing physical damage, it is preferable that the needle punching speed of the first process be 10 to 30% slower than the needle punching speed of the second process. For example, the needle punching speed in the first process can be 30 to 120 rpm, and the needle punching speed in the second process can be 300 to 400 rpm.

[0042] The absorbent fabric manufactured by this needle punching process has greatly improved porosity and bulkiness, and has an air permeability of 300 to 600㎤ / ㎠ / sec, which is the maximum value.

[0043] Meanwhile, the water-repellent agent coated on the absorbent fabric reduces the moisture absorption rate and increases the buoyancy of the absorbent fabric. The water-repellent agent is coated not only on the polyester fiber foam (10) but also on the polypropylene fiber sheet (20), thereby reducing the moisture absorption rate and increasing the buoyancy of the polyester fiber foam (10) and the polypropylene fiber sheet (20).

[0044] When the water repellent is coated on only one of the polyester fiber foam (10) or the polypropylene fiber sheet (20), the uncoated polyester fiber foam (10) or the polypropylene fiber sheet (20) absorbs moisture and increases in weight, so that the polyester fiber foam (10) may be located under the oil layer (oil layer) or submerged in water.

[0045] It is preferable that the water repellent be a non-fluorine water repellent, and preferably a wax such as paraffin wax, microcrystalline wax, polyethylene wax, or polypropylene wax. It is preferable to use a wax with a solid content of 30 to 40% or more.

[0046] It is preferable to dilute such waxes to form a water-repellent composition. For example, a water-repellent composition should preferably contain 10-15% by weight of wax relative to the total weight of the water-repellent composition. If the wax content is less than 10% by weight, the water-repellent effect will be reduced. If it exceeds 15% by weight, the relative oil absorption rate (adsorption rate) will decrease due to the strong water-repellent effect, making it difficult to meet the performance and quality standards of the absorbent pad.

[0047] It is preferable to dilute the wax in water to form a water-repellent agent, and the water-repellent agent can be formed by mixing 10 to 15 wt% of wax and 85 to 90 wt% of water. Such a water-repellent agent can be coated on the polypropylene fiber sheet (20) and polyester fiber foam (10) forming the absorbent fabric by either a spraying or immersion process, thereby reducing the moisture absorption rate of the absorbent fabric and increasing its buoyancy.

[0048] The immersion process can be performed by immersing the absorbent fabric in an immersion tank to allow the water-repellent agent to be absorbed into the polypropylene fiber sheet (20) and polyester fiber foam (10), and then squeezing it with a roller at a constant pressure. As a result, the water-repellent agent is densely deposited and applied between the gaps between the fibers of the polypropylene fiber sheet (20) and polyester fiber foam (10), thereby providing an excellent water-repellent effect.

[0049] The spraying process can be performed by spraying a water-repellent agent onto a polypropylene fiber sheet (20) and a polyester fiber foam (10) through nozzles, respectively. When spraying the water-repellent agent, the water-repellent agent is sprayed in a fan-shaped spray pattern through a fine nozzle, and compressed air is simultaneously sprayed using an air gun so that the water-repellent agent can be uniformly applied and penetrated into the polypropylene fiber sheet (20) and the polyester fiber foam (10). As a result, the water-repellent agent is densely deposited and applied between the pores between the fibers of the polypropylene fiber sheet (20) and the polyester fiber foam (10), thereby providing an excellent water-repellent effect.

[0050]

[0051] <Example 1>

[0052] 20 wt% of 6 denier polyester fiber and 80 wt% of 20 denier polyester fiber were fed into a hopper and mixed to produce polyester fiber foam. Then, a polypropylene fiber sheet was laminated on the polyester fiber foam and then needle-punched to produce an absorbent fabric.

[0053] The number of needles on the needle plate was 7,500, arranged diagonally, and needle punching was performed at a needle depth of 18.5 mm and a punching speed of 400 rpm to produce an absorbent fabric.

[0054] Afterwards, an oil absorbent fabric was manufactured by immersing and coating an absorbent fabric in a water-repellent agent prepared by mixing 15 wt% of wax and 85 wt% of water, and drying the resulting fabric.

[0055]

[0056] <Comparative Example 1>

[0057] 20 wt% of 6 denier polyester fiber and 80 wt% of 20 denier polyester fiber were fed into a hopper and mixed to produce polyester fiber foam. A polypropylene fiber sheet was then laminated on the polyester fiber foam and needle-punched to produce an absorbent fabric. The absorbent fabric was produced by needle-punching in the same manner as the general non-woven needle-punching process.

[0058] Afterwards, an oil absorbent fabric was manufactured by immersing and coating an absorbent fabric in a water-repellent agent prepared by mixing 15 wt% of wax and 85 wt% of water, and drying the resulting fabric.

[0059]

[0060] Comparative Example 2

[0061] I purchased a commercially available oil absorbent pad made of polypropylene fiber.

[0062]

[0063] Experimental Example 1

[0064] The specimens of Example 1 and Comparative Examples 1 and 2, each measuring 10 cm in width × 10 cm in length, were prepared. Each specimen was placed in a water bath formed with a buckwheat oil surface for 5 minutes to measure the oil absorption rate and water absorption rate, and the results are shown in Table 1.

[0065]

[0066] Absorption rate Absorption rate g / gg / ㎤ g / gg / ㎤ Example 1151.20.900.08 Comparative example 190.80.950.10 Comparative example 210.91.10.400.05

[0067]

[0068] As a result of the test, it was proven that Example 1 had a superior oil absorption rate than Comparative Examples 1 and 2.

[0069]

[0070] The present invention has been described above with reference to preferred embodiments. Those skilled in the art will appreciate that they can implement other embodiments of the present invention, other than those described above, within the essential technical scope of the present invention. The essential technical scope of the present invention is set forth in the claims, and all differences within the scope equivalent thereto should be construed as being included in the present invention.

Claims

1. Polyester fiber foam; A polypropylene fiber sheet laminated and bonded to the above polyester fiber foam; and An oil absorbent fabric comprising a water-repellent agent coated on the polyester fiber foam and polypropylene fiber sheet.

2. In paragraph 1, The above polyester fiber foam is an oil-absorbing fabric composed of 10 to 30 wt% of 6-denier polyester fiber and 70 to 90 wt% of 20-denier polyester fiber.

3. The first step is to mix polyester fibers of different thicknesses; A second step of making a polyester fiber foam using the above mixed fibers and laminating a polypropylene fiber sheet on the polyester fiber foam; A third step of making an absorbent fabric by combining the polyester fiber foam and the polypropylene fiber sheet; and A method for manufacturing an oil absorbent pad, comprising a fourth step of coating a water-repellent agent containing wax on the absorbent pad raw material.

4. In paragraph 3, A method for manufacturing an oil absorbent fabric, wherein 10 to 30 wt% of 6 denier polyester fiber and 70 to 90 wt% of 20 denier polyester fiber are mixed in the first step.

5. In paragraph 3, A method for manufacturing an oil absorbent cloth, wherein the water repellent is composed of 10 to 15 wt% of the wax based on the total weight.

Citation Information

Patent Citations

  • Oil absorbent mat

    JP2006218761A

  • Oil adsorption sheet and application method therefor

    JP2018047428A

  • Semiconductor cleaning composition and semiconductor manufacturing method using the same

    KR1020240108709A

  • Eye drive system of humanoid robot

    KR102279096B1

  • Nose bridge for eyeglass frames with seating power and excellent tightness

    KR102565302B1