High capacity rechargeable all active material electrode lithium-ion batteries with percolated networks of layered oxides
AAM electrodes with a blend of LCO and LNMO materials address the limitations of conventional lithium-ion batteries by enhancing both electronic and ionic conductivity, achieving higher energy density and mechanical stability, particularly in small form factor batteries like 2032-type coin cells.
Patent Information
- Application Number
- PCT/US2024/026021
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional lithium-ion battery electrodes face limitations in energy density due to restricted ionic transport and mechanical stability issues, particularly with increased thickness, which restricts the use of high-capacity electroactive materials and leads to delamination and cracking.
The development of All Active Material (AAM) electrodes, which are thick, sintered, and free of inactive binders and conductive additives, utilizing a blend of high electronic conductivity LiCoO2 (LCO) and high electrochemical capacity LiNi0.5Mn0.5O2 (LNMO) materials to enhance both electronic and ionic conductivity, allowing for higher energy density and mechanical integrity.
AAM electrodes achieve higher energy density and improved rate capability compared to conventional composite electrodes, with the LCO-NCA blend demonstrating the highest capacity and best battery performance, suitable for small form factor applications like 2032-type coin cells.
Smart Images

Figure US2024026021_31102024_PF_FP_ABST
Abstract
Description
HIGH CAPACITY RECHARGEABLE ALL ACTIVE MATERIAL ELECTRODE LITHIUM-ION BATTERIES WITH PERCOLATED NETWORKS OF LAYERED OXIDESCLAIM OF PRIORITY AND CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of priority to U.S. Provisional Patent Application Serial No. 63 / 497,881 entitled “HIGH CAPACITY RECHARGEABLE ALL ACTIVE MATERIAL ELECTRODE LITHIUM-ION BATTERIES WITH PERCOLATED NETWORKS OF LAYERED OXIDES,” filed April 24, 2023, which is incorporated herein in its entirety by reference.STATEMENT OF GOVERNMENT SUPPORT
[0002] This subject matter was made with Government support under 1652488 awarded by the National Science Foundation. The U.S. Government has certain rights in this subject matter.BRIEF DESCRIPTION OF THE FIGURES
[0003] In the drawings, which are not necessarily drawn to scale, like numerals describe substantially similar components throughout the several views. Like numerals having different letter suffixes represent different instances of substantially similar components. The drawings illustrate generally, by way of example, but not by way of limitation, various aspects of the present subject matter.
[0004] FIG. 1 A and FIG. IB comprise schematics showing a 2032-type cell with FIG. 1 A showing more conventional assembly of cell components and FIG. IB showing an assembly with AAM electrodes in this report towards increasing total cell capacity
[0005] FIG. 2A, FIG. 2B, FIG. 2C, and FIG. 2D comprise a series of graphs showing in FIG. 2A Rate capabilities outcomes for discharging cells at the indicated currents (all charge cycles were conducted at 1 mA) for AAM electrode full cells containing Blend, LCO , and NCA AAM cathodes. The discharge rates were at 1, 2, 5, 10, and 1 mA, with 5 cycles at each rate. The anode in all cases was AAM LTO, and the voltage window was 1.0-2.8 V (cell). Discharge voltage profiles are also provided for the 5th (1 mA), 10th (2 mA), 15th (5mA), and 20th (10 mA) cycles in FIG. 2B for LCO, in FIG. 2C for NCA, and in FIG. 4D for Blend.
[0006] FIG. 3 is a graph showing a first discharge dQ / dV profiles for NCA AAM cell, NCA composite cell, and Blend AAM cell. The AAM cells use bottom axis and the composite cell uses the top axis, and the two axes are aligned with a difference of 1.56 V corresponding to the location of the plateau regions for LTO materials.
[0007] FIG. 4 is a schematic comparing total capacity of commercial rechargeable 2032-type coin cells, the Blend rechargeable 2032 coin cells as described herein, and commercial single use (primary) 2032 coin cells.
[0008] FIG. 5 is a graph showing XRD patterns of the surfaces of sintered AAM electrode pellets after thermal treatment of Blend, pure NCA, and pure LCO electrodes. The cutout on the right is an expansion of the (003) peak region for LCO and NCA. Peak assignments were based on ICSD 259670 for NCA and ICSD 51381 for LCO.
[0009] FIG. 6 is a graph showing first cycle charge / discharge profiles for NCA and LCO processed into composite cathodes and paired with lithium metal anodes. The rate for both charge and discharge was C / 20, which corresponded to 106.8 pA cm'2and 15.8 pA cm'2for the NCA and LCO cells, respectively. C rate was assigned based on the cathode active material loading in the cells and assuming a capacity of 200 mAh g'1NCA and 137 mAh g'1LCO.
[0010] FIG. 7 is a graph showing a discharge voltage profile of the AAM NCA cathode at 0.1 mA after the rate capability test the Anode was AAM LTO.
[0011] FIG. 8 is a graph showing AAM electrode geometric pore / void fraction for the different mass loadings of LCO blended with LNMO. Error bars are the standard deviations of the mean of 3 independent experimental measurements on electrode pellets.
[0012] FIG. 9 is a graph showing XRD patterns for synthesized powders of LCO and LNMO.
[0013] FIG. 10 is a graph showing XRD patterns for AAM electrode pellets. The materials were 100%LCO, 60%LCO, 45%LCO, 30%LCO, 15%LCO, and 0%LCO.
[0014] FIG. 11 is a graph showing volume fraction of the AAM electrode which was occupied by LiCoO? (LCO) particles as a function of LCO relative mass loading, based on the measured volume of the electrode, the measured mass of LCO in the electrode, and the crystal density of LCO.
[0015] FIG. 12A, FIG. 12B, FIG. 12C, and FIG. 12D comprise a series of graphs showing a first cycle charge / discharge voltage profiles. In FIG. 12A for LCO and in FIG. 12C for LNMO and corresponding dQ / dV plots. In FIG. 12B for LCO and in FIG. 12D forLNMO processed into conventional composite electrodes and cycled at C / 10 after pairing with Li foil anodes. The solid and dashed curve represent the as-synthesized powder and AAM treated powder. “AAM treated” powder refers to the material undergoing ethanol contact and thermal treatment as is done with AAM electrodes, although there is not hydraulic compression and the resulting powder was processed into a composite electrode.
[0016] FIG. 13 A and FIG. 13B comprise a series of graphs showing in FIG. 13Adischarge voltage profiles at low rate for AAM electrode cells containing LTO anodes and cathodes comprised of 100%LCO, 60%LCO, 45%LCO, 30%LCO, 15%LCO, and 0%LCO. The discharge was at a rate of C / 80, which was the same rate used for the charge cycle and corresponded to -0.282 mA cm'2and in FIG. 13B(b) the corresponding dQ / dV plots calculated from the discharge results shown in FIG. 13 A.
[0017] FIG. 14 is a graph showing discharge capacity (gravimetric on cathode mass basis) from rate capability testing of AAM electrode cells comprised of LTO anodes and cathodes with the indicated relative LCO compositions on the x-axis (balance of electroactive material mass was LNMO). The line at the top indicates the capacity expected based on the mass of active material in the electrodes and their gravimetric capacity in conventional composite electrodes cycled at a relatively low rate of charge / discharge. For reference, -1.13 mA cm'2was used as C / 20 rate for all AAM electrodes.
[0018] FIG. 15 A, FIG. 15B, FIG. 15C, FIG. 15D, FIG. 15E, and FIG 15F comprise a series of graphs showing voltage profiles at C / 20 - C / 2.5 for AAM electrode cells comprised of LTO anodes and cathodes of the composition in FIG. 15A of 0%LCO, in FIG. 15B of 15%LCO, in FIG. 15C of 30%LCO, in FIG. 15D of 45%LCO, in FIG. 15E of 60%LCO, and in FIG. 15F of 100%LCO. Charge and discharge were always performed at the same rate as indicated on the plot. For reference C / 20 corresponded to -1.13 Ma cm'2.
[0019] FIG. 16 is a graph showing discharge capacity during rate capability evaluations for AAM electrode cells with LTO anodes and cathodes with composition of 0%LCO, 15%LCO, 30%LCO, 45%LCO, 60%LCO, and 100%LCO. Charge and discharge were at the same rate as indicated on the plot. For reference C / 20 corresponded to -1.13 Ma cm'2.
[0020] FIG. 17A, FIG. 17B, FIG. 17C, and FIG. 17D comprise a series of graphs showing in FIG. 17A and FIG. 17B voltage profiles and FIG. 17B and FIG 17B overpotential distributions extracted from P2D simulations of AAM electrode cells.
[0021] FIG. 18 is a graph showing electronic conductivities as a function of lithiation used in simulations. LiCoCh (LCO) electronic conductivity as a function of lithiation was based on reported literature.
[0022] FIG. 19A and FIG. 19B comprise a series of graphs showing simulated Li concentration in FIG. 19A of the electrolyte phase and in FIG. 19B of the solid-state electrode phase at C / 20 discharge (1.13 Ma cm'2) following a C / 20 charge cycle for pure LNMO (0%LCO) cell.
[0023] FIG. 20A and FIG. 20B comprise a series of graphs showing simulated Li concentration in the (a) electrolyte phase and (b) electrode phase at C / 20 discharge (1.13 Ma cm'2) following a C / 20 charge cycle for 45%LCO cell.
[0024] FIG. 21 A, FIG. 21B, FIG 21C, FIG. 21D, and FIG. 21E comprise a series of graphs showing simulated change in Li concentration in the LNMO and LCO material as a function of position in the cathode for 45%LCO cell at different stages of discharge at a rate of C / 20 (1.13 mA cm'2). The regions during discharge shown in FIG. 21 A are from 0 to 30 mAh g'1cathode discharged, in FIG. 2 IB are from 30 to 56 mAh g'1cathode discharged, in FIG. 21C are from 56 to 78 mAh g'1cathode discharged, in FIG. 2 ID are from 78 to 110 mAh g'1cathode discharged, and in FIG. 21E are from 110 to 125 mAh g'1cathode discharged.
[0025] FIG. 22A, FIG. 22B, FIG. 22C, FIG. 22D, FIG. 22E, FIG. 22F, FIG. 22G, FIG. 22H, AND FIG. 221 comprise a series of graphs showing in FIG. 22A an Equivalent Circuit Model used for fitting all electrochemical impedance spectroscopy data. Nyquist plots are shown of FIG. 22B fresh cell and after CCCV charge at in FIG. 22Cof 3.8 V, FIG. 22D of 3.9 V, FIG. 22E of 4.0 V, FIG. 22F of 4.1 V, FIG. 22G of 4.2 V, FIG. 22H of 4.3 V, and FIG. 221 of 4.4 V.
[0026] FIG. 23 is a CCCV plot for a AAM LNMO cell paired with Li metal charged at 0.55 mA cm'2and then held at 4.4 V.DETAILED DESCRIPTION
[0027] Reference will now be made in detail to certain aspects of the disclosed subject matter, examples of which are illustrated in part in the accompanying drawings. While the disclosed subject matter will be described in conjunction with the enumerated claims, it will be understood that the exemplified subject matter is not intended to limit the claims to the disclosed subject matter.
[0028] Throughout this document, values expressed in a range format should be interpreted in a flexible manner to include not only the numerical values explicitly recited as the limits of the range, but also to include all the individual numerical values or sub-ranges encompassed within that range as if each numerical value and sub-range is explicitly recited. For example, a range of “about 0.1% to about 5%” or “about 0.1% to 5%” should be interpreted to include not just about 0.1% to about 5%, but also the individual values (e.g., 1%, 2%, 3%, and 4%) and the sub-ranges (e.g., 0.1% to 0.5%, 1.1% to 2.2%, 3.3% to 4.4%) within the indicated range. The statement “about X to Y” has the same meaning as “about X to about Y,” unless indicated otherwise. Likewise, the statement “about X, Y, or about Z” has the same meaning as “about X, about Y, or about Z,” unless indicated otherwise.
[0029] In this document, the terms “a,” “an,” or “the” are used to include one or more than one unless the context clearly dictates otherwise. The term “or” is used to refer to a nonexclusive “or” unless otherwise indicated. The statement “at least one of A and B” has the same meaning as “A, B, or A and B .” In addition, it is to be understood that the phraseology or terminology employed herein, and not otherwise defined, is for the purpose of description only and not of limitation. Any use of section headings is intended to aid reading of the document and is not to be interpreted as limiting; information that is relevant to a section heading may occur within or outside of that particular section.
[0030] All publications, patents, and patent documents referred to in this document are incorporated by reference herein in their entirety, as though individually incorporated by reference. In the event of inconsistent usages between this document and those documents so incorporated by reference, the usage in the incorporated reference should be considered supplementary to that of this document; for irreconcilable inconsistencies, the usage in this document controls.
[0031] In the methods described herein, the acts can be carried out in any order without departing from the principles of the subject matter, except when a temporal or operational sequence is explicitly recited. Furthermore, specified acts can be carried out concurrently unless explicit claim language recites that they be carried out separately. For example, a claimed act of doing X and a claimed act of doing Y can be conducted simultaneously within a single operation, and the resulting process will fall within the literal scope of the claimed process.
[0032] Lithium ion (Li-ion) batteries have found wide applications from electric vehicles to portable electronics due to their exceptional volumetric and gravimetric energydensity. In addition to exploration of material chemistry, optimizing electrode architecture is necessary to maximize energy density at the cell level. Increased thickness of a battery electrode results in increased areal loading of electroactive material, which will increase cell energy density. Increased electrode thickness, however, results in ionic transport and mechanical stability limitations, which leads to conventional composite electrodes generally having thicknesses less than 100 pm. For composite electrodes, the ionic transport in the electrolyte through the tortuous electrode interstitial regions becomes even more restricted due to the inclusion of polymer binders, conductive additives, and electrode calendaring. Mechanical issues for thicker composite electrodes originates from the casting process, where the electroactive material, conductive additives, and polymer binder solution are first blended into slurry and coated onto a current collector. Solvent drying happens at the top air interface and the solid particles redistribute, giving rise to inhomogeneity across the electrode depth which can cause severe electrode delamination and cracking.
[0033] Towards mitigating transport limitations of thick electrodes, one option is to process electrodes containing only electroactive material to remove the extra transport restrictions imposed by inactive binders and conductive additives in the electrode interstitial regions. Previously reported “All Active Material (AAM) electrodes” (in some cases referred as “sintered electrodes”) are comprised of only electroactive material processed via hydraulic compression and mild thermal treatment which burns out binders and increases mechanical integrity of the porous ceramic thin films. AAM electrodes have been reported with thickness over 500 pm and loadings of hundreds of mg cm'2with mechanical stability during the fabrication process and lowered tortuosity compared to conventional composite electrodes. It is noted that the mechanical integrity is provided by the inter-particle connections formed during the mild sintering process, and thus care must be taken to avoid electroactive material with large lattice volume change during electrochemical charge / discharge to mitigate pulverization or particle disconnection. In addition, due to the absence of conductive additives the electronic transport must proceed through the electroactive material, but many Li-ion electroactive cathode materials have relatively low electronic conductivity. An AAM cathode can be made from a blend of LiCoCh (LCO, high electronic conductivity but relatively low electrochemical capacity) and LiNio.5Mno.5O2 (LNMO, with relatively high electrochemical capacity but low electronic conductivity). The blend of cathode materials resulted in the best battery performance due to combining high electronic conductivity fromthe percolated LCO network with the relatively higher gravimetric capacity of the LNMO material.
[0034] Small form factor cells such as 2032-type coin cells can be used for portable or wearable applications depending on power demands. For many small form factor cells, multi-layering or stacking of electrodes can be challenging and thus designs such as AAM electrodes are well suited for these applications. Herein, 2032-type coin cells using the AAM electrode architecture for both anode and cathode with high total loadings will be described. Building on a blended cathode concept, the cathodes reported for these cells will include pure LCO cathode (referred to as “LCO”), pure LiNi0.8Co0.15Al0.05O2 (NCA) cathode (referred to as “NCA”), and a blend of 40 wt% LCO and 60 wt% NCA (referred to as “Blend”). LCO and NCA are both layered phase transition metal oxide cathode materials, with LCO having a much higher electronic conductivity than NCA and NCA having a much higher gravimetric capacity than LCO (NCA also exceeds the gravimetric capacity of the previously investigated AAM electrode LNMO material). An important element of the cells described in this report is that the thickness of the electrodes was maximized even relative to prior reports of AAM electrode 2032 coin cells, and a schematic of the cell changes relative to prior AAM electrode reports can be found in FIG 1. First, all wave springs and explicit current collector spacers typically used in coin cells (FIG la) were removed from the cells. Thus, the AAM electrodes were directly attached to the bottom and top pieces of the coin cells (FIG lb). The other modification relative to more typical Li-ion coin cells and many prior AAM electrode reports is that the separator was glass fiber rather than a porous polymer. While the glass fiber was thicker than a typical polymer separator, the increased thickness helps to further prevent soft shorts from the relatively rough AAM electrodes and has space to compress if necessary to accommodate electrode volume change during cycling. Electroactive materials were selected for the anode and cathode which had relatively small lattice volume change during el ectrochemi cal charge / di scharge .
[0035] According to an aspect of this disclosure, LCO was synthesized via sol-gel method. As further disclosed, LCO can be processed into both composite and sintered electrodes and evaluated electrochemically when paired in half and full cell configurations. The outcomes disclosed herein show that LCO is a suitable material as a sintered anode, providing stable and reversible electrochemical cycling.
[0036] Sintered electrodes have been reported which are free of inactive conductive additives and binders, with high loadings exceeding 150 mg cm'2and thicknesses over 500 pm. The electrode microstructure for sintered electrodes does not contain inactive additives in the interstitial regions between particles, and thus sintered electrodes have lower tortuosity than conventional composite electrodes. However, the electrodes are still very thick, and thus ion transport limitations through the microstructure and electron transport through the electrode matrix can result in high polarization and rate capability limitations. Because electron conduction through the electrode matrix must proceed through the electroactive material itself in sintered electrodes, materials with relatively high electronic conductivity across the range of extents of lithiation experienced during charge / discharge of the cell are desirable.
[0037] According to various examples of the instant disclosure, sintered cathodes or anodes can inlcude LCO, NCA, or a blend thereof. When blended the LCO and NCA can indpendently range from about 5 wt% to about 100 wt% of the cathode or anode, about 40 wt% to about 60 wt%, less than, equal to, or greater than about 5 wt%, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37,38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62,63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87,88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or about 100 w%
[0038] The synthesis of LNMO and LCO powders, as well as their subsequent processing into AAM electrodes, demonstrates a scalable and reproducible method for creating high-capacity electrode materials. The use of a sol-gel method for LCO and a high-temperature lithiation process for LNMO ensures a high degree of purity and phase homogeneity, which is critical for the performance and stability of the resulting AAM electrodes. The ball-milling process applied to LCO powders further refines the particle size, contributing to a more uniform microstructure in the final electrode.
[0039] In view of the foregoing, in accordance with various aspects, an electrochemical storage device can include an electrode. The electrode can include many suitable materials. Examples of suitable materials can include LCO, NCA, and blends thereof. Depending on various aspects, the electrode can be an anode or a cathode. In some examples, the cathode or anode can include at least one dopant, at least two dopants, or any suitable number. The at least one dopant has a 1+, 2+, or 3+oxidation state. As non-limitingexamples, the at least one dopant comprises copper, aluminum, sulfur, potassium, or a mixture thereof.
[0040] The blending of LCO and LNMO powders in various ratios to create AAM electrodes with different compositions allows for the fine-tuning of the electrode's electronic and ionic conductivities. This blending strategy is particularly advantageous for optimizing the electrode architecture to balance the trade-off between high energy density and electronic conductivity. The resulting AAM electrodes exhibit a synergistic effect, where the high electronic conductivity of LCO enhances the overall performance of the LNMO, which contributes to higher energy density.
[0041] The benefits of the electrodes described herein can be achieved when the electrode is a sintered electrode or a composite electrode. In examples where the electrode is a composite. While not so limited, a substrate can include a stainless steel, aluminum, alloys thereof, or mixtures thereof.
[0042] As explained herein, electrode thickness is an important parameter of the electrode. As an example, a thickness of the electrode can be in a range of from about 50 pm to about 2000 pm, about 70 pm to about 400 pm, less than, equal to, or greater than about 50 pm, 60, 70, 80, 90, 100, 110, 120,130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300, 310, 320, 330, 340, 350, 360, 370, 380, 390, 400, 410, 420,430, 440, 450, 460, 470, 480, 490, 500, 510, 520, 530, 540, 550, 560, 570, 580, 590, 600,610, 620, 630, 640, 650, 660, 670, 680, 690, 700, 710, 720, 730, 740, 750, 760, 770, 780,790, 800, 810, 820, 830, 840, 850, 860, 870, 880, 890, 900, 910, 920, 930, 940, 950, 960,970, 980, 990, 1000, 1110, 1120, 1130, 1140, 1150, 1160, 1170, 1180, 1190, 1200, 1210, 1220, 1230, 1240, 1250, 1260, 1270, 1280, 1290, 1300, 1310, 1320, 1330, 1340, 1350, 1360,1370, 1380, 1390, 1400, 1410, 1420, 1430, 1440, 1450, 1460, 1470, 1480, 1490, 1500, 1510,1520, 1530, 1540, 1550, 1560, 1570, 1580, 1590, 1600, 1610, 1620, 1630, 1640, 1650, 1660,1670, 1680, 1690, 1700, 1710, 1720, 1730, 1740, 1750, 1760, 1770, 1780, 1790, 1800, 1810,1820, 1830, 1840, 1850, 1860, 1870, 1880, 1890, 1900, 1910, 1920, 1930, 1940, 1950, 1960,1970, 1980, 1990, or about 2000 pm.
[0043] A porosity of the electrode can be in a range of from about 30% to about 50 %, about 35% to about 40 %, less than, equal to, or greater than about 30%, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, or about 50%. The porosity can alternatively be expressed as a void space of the portion of the electrode that is empty. The pores can be through pores in some examples.
[0044] The porosity of the AAM electrodes plays a significant role in the electrochemical performance of the cells. The geometric pore / void fraction of the electrodes, as determined by experimental measurements, indicates the level of ion transport facilitation through the electrode microstructure. The optimization of porosity is crucial for reducing ionic transport overpotential and improving the rate capability of the AAM electrodes, especially when dealing with thick electrode designs.
[0045] According to various examples, the electrode is substantially free of any conductive additives. For example, the electrode can include about 0 wt% to about 5 wt% conductive additive, about 0 wt% to about 0.50 wt%, less than, equal to, or greater than about 0 wt%, 0.1, 0.2, 0.3. 0.4, .0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, or about 5 wt%. Non limiting examples of conductive additives that the electrode is free of include a polymer binder, a conductive carbon, or a mixture thereof.
[0046] The material(s) and construction of the electrode can control the capacity of the electrode. As an example, the capacity of the electrode can be in a range of from about 7 mAh / cm2to about 200 mAh / cm2, about 10 mAh / cm2to about 50 mAh / cm2, less than, equal to, or greater than about 7 mAh / cm2, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47,48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72,73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97,98, 99, 100, 101, 102, 103, 104, 105, 106, 107. 108, 109, 110, 111, 112, 113, 114, 115, 116,117, 118, 119, 120, 121, 122, 123, 124, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134,135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, 151, 152,153, 154, 155, 156, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170,171, 172, 173, 174, 175, 176, 177, 178, 179, 180, 181, 182, 183, 184, 185, 186, 187, 188,189, 190, 191, 192, 193, 194, 195, 196, 197, 198, 199 or about 200 mAh / cm2.
[0047] The electrode, in some aspects, can be associated with an electrically conductive current collector to facilitate the flow of electrons between the electrode and an exterior circuit. The current collector can include metal, such as a metal foil or a metal grid. In some aspects, the current collector can be formed from nickel, aluminum, stainless steel, copper or the like. The electrode material can be cast as a thin film onto the current collector. The electrode material with the current collector can then be dried, for example in an oven, toremove solvent from the sintered electrode. In some aspects, the dried sintered electrode material in contact with the current collector foil or other structure can be subjected to a pressure, such as, from about 2 to about 10 kg / cm2(kilograms per square centimeter).
[0048] The separator is located between the positive electrode and the negative electrode. The separator is electrically insulating while providing for at least selected ion conduction between the two electrodes. A variety of materials can be used as separators. Commercial separator materials are generally formed from polymers, such as polyethylene and / or polypropylene that are porous sheets that provide for ionic conduction. Commercial polymer separators include, for example, the Celgard® line of separator material from Hoechst Celanese, Charlotte, N.C. Also, ceramic-polymer composite materials have been developed for separator applications. The separator can also be a glass fiber separator. These composite separators can be stable at higher temperatures, and the composite materials can significantly reduce the fire risk. In some further examples the separator can include glass fibers. Glass fiber separators can be especially useful when a sintered electrode is used.
[0049] The use of glass fiber as a separator in AAM electrode cells is a strategic choice that addresses the mechanical stability challenges posed by the rough surface of AAM electrodes. The thickness and compressibility of glass fiber separators not only prevent short-circuiting but also accommodate the volume changes of the electrodes during cycling. This feature is particularly important for maintaining the structural integrity of the cell over multiple charge-discharge cycles.
[0050] The electrolyte includes solvated ions as electrolytes, and ionic compositions that dissolve to form solvated ions in appropriate liquids are referred to as electrolyte salts. Electrolytes for lithium ion batteries can comprise one or more selected lithium salts. Appropriate lithium salts generally have inert anions. Suitable lithium salts include, for example, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium bis(trifluorometh yl sulfonyl imide), lithium trifluoromethane sulfonate, lithium tri s(trifluorom ethyl sulfonyl) methide, lithium tetrafluorob orate, lithium perchlorate, lithium tetrachloroaluminate, lithium chloride, lithium difluoro oxalato borate, and combinations thereof. Traditionally, the electrolyte comprises a 1 M concentration of the lithium salts, although greater or lesser concentrations can be used.
[0051] A non-aqueous liquid can be used to dissolve the lithium salt(s). The solvent generally does not dissolve the electroactive materials. Appropriate solvents include, for example, propylene carbonate, dimethyl carbonate, diethyl carbonate, 2-methyl tetrahydrofuran, dioxolane, tetrahydrofuran, methyl ethyl carbonate, y-butyrolactone,dimethyl sulfoxide, acetonitrile, formamide, dimethyl formamide, triglyme (tri(ethylene glycol) dimethyl ether), diglyme (di ethylene glycol dimethyl ether), DME (glyme or 1,2- dimethyloxyethane or ethylene glycol dimethyl ether), nitromethane and mixtures thereof.
[0052] The electrodes described herein can be incorporated into various commercial battery designs, such as prismatic shaped batteries, wound cylindrical batteries, coin batteries or other reasonable battery shapes. The batteries can comprise a single sintered electrode stack or a plurality of sintered electrodes of each charge assembled in parallel and / or series electrical connection(s). Appropriate electrically conductive tabs can be welded or the like to the current collectors, and the resulting jellyroll or stack structure can be placed into a metal canister or polymer package, with the negative tab and positive tab welded to appropriate external contacts. Electrolyte is added to the canister, and the canister is sealed to complete the battery. Some presently used rechargeable commercial batteries include, for example, the cylindrical 18650 batteries (18 mm in diameter and 65 mm long) and 26700 batteries (26 mm in diameter and 70 mm long), although other battery sizes can be used.
[0053] Another battery that the electrodes described herein can be disposed in is a 2032-type coin cell and other coin / button cell form factors, for example 2025, 2016, 312, and others.
[0054] The sintered electrode can be formed according to many suitable methods. For example, the electroactive material of the electrode is sintered. Sintering can be performed at a temperature in range of from about 500 °C to about 1100 °C, about 700 °C to about 900 °C, less than, equal to, or greater than about 500 °C, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1050, or about 1100 °C. Sintering can be conducted at a constant temperature or at a variable temperature during the sintering process. Sintering can last for any amount of time in a range of from about 0 hours to about 20 hours, about 12 hours to about 18 hours, less than, equal to, or greater than about 0 hours, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or about 20 hours. Sintering can be conducted in one step or across multiple sintering steps.
[0055] Alternatively, a composite electrode can be formed by disposing the electroactive material on a substrate. The electroactive material can be in the form of a slurry mixed with a solvent, carbon source, and any other suitable component. The substrate can be an aluminum foil. After the slurry is disposed on the substrate, the slurry is allowed to dry in an oven to form the electrode.
[0056] As mentioned previously, in some aspects the electrode can include a degree of porosity. The structure and / or arrangement of pores in the sintered electrode microstructure can lead to additional improvements in the energy and power density of the energy storage device to which the electrode is incorporated. As an example, aligning the pores can improve these properties. One method that can be used to accomplish this is to fabricate an electrode using reactants that are capable of forming an anisotropic structure. This can be accomplished by producing an anisotropic precipitate particle that includes a single transition metal or multiple transition metals. The precipitate can be used as a precursor template in formulating battery active material having an anisotropic morphology. Any suitable transition metal can be used to form the precursor template.
[0057] In producing the sintered electrode, there are different strategies to improve or overcome inherent electronic conductivity limitations of electroactive materials. One route is to dope the electroactive material with elements that result in increased electronic conductivity. There are limits to the electronic conductivity improvements via doping methods and at too high of a doping level secondary phases can result. Another option is to carbon coat the electroactive material, and this strategy has been attributed to improving rate capability of other low electronic conductivity electroactive materials such as LiFePCh. Carbon coating of electroactive materials has been broadly reported for improved interfacial stability and electronic conductivity. Sucrose is a common carbon source that also can serve as a particulate binder material. As described herein a carbon coated sintered electrode can be produced using sucrose both as a sacrificial binder for sintered electrode processing and as a carbon source, where the carbon coating process does not require an extra step for treating the electroactive material powder or the sintered porous pellet relative to processing the electrodes without the coating.
[0058] The electrochemical storage device described herein can be disposed in many suitable articles. For example, the electrochemical storage device can be disposed in vehicle (e.g., an electric vehicle) or an electronic device.
[0059] The electrochemical storage device described herein can be adapted for various commercial applications, including but not limited to electric vehicles and portable electronics. The high energy density and customizable architecture of the AAM electrodes make them suitable for integration into different battery form factors, such as prismatic, cylindrical, and coin cells. The ability to scale the electrode thickness and composition allows for the design of batteries that meet specific energy and power requirements for a wide range of applications.Examples
[0060] Various aspects of the present subject matter can be better understood by reference to the following Examples which are offered by way of illustration. The present subject matter is not limited to the Examples given herein.EXAMPLE 1Materials and MethodsMaterial Preparation
[0061] Cathode materials used were NCA and LCO. NCA was received from CAMP (Cell Analysis, Modeling and Prototyping) Facility, Argonne National Laboratory. LCO was synthesized from a precursor oxalate precipitate. 200 mM of each sodium oxalate (Na2C2O4, Fisher) and cobalt sulfate heptahydrate (CoSO^ EEO, Acros Organics) were separately dissolved into deionized (DI) water volumes of 400 mL. The two solutions were preheated to 60 °C before mixing together all at once. The mixed solution continued to be stirred at 300 RPM and was kept at 60 °C for 30 min. After 30 min of allowing coprecipitation to proceed, the precipitate was collected by vacuum filtration and dried at 80 °C overnight. The resulting COC2O4«2H2O was blended with lithium carbonate (Li2CO3, Fisher) with Li:Co ratio of 1.05: 1 using a mortar and pestle by hand for 10 min. The powder mixture was then transferred to a box furnace (Carbolite CWF 1300) and heated with a ramp rate of 1°C min'1to 800 °C without a hold at the target temperature and allowed to cool to room temperature without control over cooling rate. The anode material was Li4TisOi2 (LTO, Nanomyte from NEI) and was used as received. Detailed characterization of the LCO and LTO materials can be found in previous reports.Electrode Preparation
[0062] Composite electrodes: for composite electrodes, NCA electrode was received from CAMP. Circular cathodes with an area of 1.33 cm2were punched out from the electrode sheets. The areal electroactive material loading for the NCA electrode discs was measured to be 10.7 mg cm'2. LCO electrodes were fabricated in the lab. LCO powders were blended with acetylene carbon black (CB, Alfa Aesar) and 3.33 wt% polyvinyl pyrrolidone (PVP, Sigma Aldrich, 360 kDa molecular weight) in ethanol with a weight ratio of 8: 1 : 1 LCO:CB:PVP. The slurry was blended in a mixer (Thinky AR- 100) at 2000 rpm for 4 min, then sonicatedfor 5 min, followed by another slurry mixing process at 2000 rpm for 4 min. PVP, while not as commonly used as a Li-ion electrode binder, was used to keep consistency with the binder used for attachment of the AAM electrode (additional details below). The resulting slurry was coated onto an aluminum foil using a doctor blade with a 400 pm gap height, then vacuum dried at 50 °C for 30 min. Circular cathodes with an area of 1.33 cm2were punched out with an areal electroactive material loading of 2.3 mg cm'2.
[0063] AAM electrodes: Pure LCO or NCA of 1 g was added to a mortar followed by adding 2 mL of 1 wt% polyvinyl butyral (PVB, Pfaltz & Bauer) in ethanol. The suspension was blended using a pestle by hand until dried. For the pure LCO and NCA AAM electrodes, the resulting PVB-coated powder was pressed into a circular pellet using a pellet die with diameter of 16 mm (Carver) under -300 MPa applied pressure for 2 min. For the Blend electrode, PVB-coated LCO and NCA were blended using a mortar and pestle by hand for 5 min with mass ratio of 4:6 LCO:NCA before undergoing the same hydraulic compression step as used for the pure powders. The resulting pellets were transferred to a box furnace and heated with a ramp up rate of 1 °C min'1to the target temperature of 600 °C, held at the target temperature for 1 h, and then cooled to room temperature using a ramp down rate of 1 °C min'1. The final result was AAM porous ceramic thin film pellets. For processing LTO AAM anodes, pure LTO of 1 g was added to the mortar followed by adding 4 mL of 1 wt% PVB in ethanol. The compression and sintering steps were the same as for the AAM cathodes, except that for LTO the target holding temperature was higher at 730 °C. All resulting pellet electrodes had areas of -2 cm2and other detailed dimensions are listed in Table 1. The total combined electrode thickness for cathode and anode was kept between 2500-2600 pm. This total thickness was targeted based on the total cell thickness of 3200 pm (due to 2032-type cell form factor) minus the thicknesses of 500 pm (combined thickness for the top and bottom cell case parts) and minus the thickness of 100-200 pm allowed for the glass fiber after compression. To mitigate interfacial resistance between the AAM electrode and the current collector (cell top / bottom piece), a conductive carbon adhesive buffer layer was applied between the current collector (i.e., top or bottom cell part) and the respective AAM electrode. The buffer layer was made by blending CB and 3.33 wt% PVP solution in ethanol with a mass ratio of 1 : 1 CB:PVP using the slurry mixer for 4 min at 2000 rpm. After attachment of the AAM electrode to the current collector using the wet buffer layer slurry, all components were vacuum dried together at 50 °C for 30 min.Table 1. Electrode specificationsMaterial Characterizations
[0064] X-ray diffraction (XRD) patterns were collected on a PANalytical X’pert ProMPD. Scanning electron micrographs (SEM) and energy dispersive X-ray spectroscopy (EDS) were performed on a FEI Quantum 650.Electrochemical Evaluations
[0065] For composite electrode cells, circular Li foil was punched out with an area of 1.6 cm2as anode. Circular separator (Celgard 2325) with an area of 2.0 cm2was used.Electrolyte (1.2 M LiPFe in 3:7 ethylene carbonate: ethyl methyl carbonate, Gotion) addition and cell (2032 type) assembly was conducted in an argon-filled glove box. Cells were cycled between 2.5-4.3 V (vs. Li / Li+) at C / 20 (137 mAh g'1assumed for LCO with a current density of 16 pA cm’2, and 200 mAh g'1assumed for NCA with a current density of 107 pA cm’2).
[0066] For AAM electrode cells, glass fiber (Fisher) was used as separator and the same electrolyte was used as for the composite electrode cells. AAM cells were cycled between 1.0-2.8 V (cell, LTO anode). The charge rate used was always 1 mA and discharge rates of 1, 2, 5, and 10 mA were used. It is noted that one full charge and discharge cycle for the Blend cell at 1 mA charge / discharge took over one week. On the basis of the amount of solid cathode active material in the AAM electrodes, 1 mA corresponded to -C / 100. All AAM cells had cell balancing which was slightly cathode limiting.Results and DiscussionMaterials Characterization
[0067] The NCA powder had secondary particle size of ~10 pm and primary particle size of ~0.5 pm. The LCO powder did not have obvious secondary particle agglomerates, and most primary particles were less than 1.0 pm in length. After hydraulic compression and mildsintering additional SEM images were taken on the surfaces of electrode pellets. The electrodes appeared smoother / flattened due to the compression process, however, the primary particle sizes appeared unchanged. The porous electrode pellets also maintained relatively high porosity after the mild thermal treatment, where the geometric pore / void fraction for all pellets ranged from 0.32-0.34. Due to the two different composition particles used for the Blend electrode, EDS analysis was also conducted on the top surface of this pellet material. The EDS results suggested segregation of Co-rich particles / regions and Ni-rich particles / regions, which were attributed to LCO particles and NCA particles, respectively. This outcome was consistent with the individual NCA and LCO material particles remaining segregated with minimal inter-diffusion. Similar observations were previously made on different composition layered phase blends of particles where the individual composition particles remained segregated. It is noted that this is not the case for all material systems, as in particular a blends of two particles with different phases and lithium concentrations resulted in the formation of an interfacial material / phase in a previous report using similar processing methods.
[0068] To provide further support for the segregation of the LCO and NCA materials within the AAM electrodes, XRD patterns were obtained using the AAM electrode pellet samples after processing for the pure LCO, pure NCA, and Blend materials. The XRD patterns can be found in FIG 5. For the pure LCO and NCA, both patterns were consistent with layered R-3m phase that has previously been reported for these materials LCO and no impurities were detected. However, while the LCO and NCA have the same symmetry these materials also have slightly different peak locations. In particular, the (003) peak is at a lower 2D value for NCA relative to LCO. For the Blend electrode, XRD features from both the LCO and NCA materials were clearly observed, and there was not a notable shift in the (003) peaks compared with the pure component NCA and LCO (003) peaks. There were also no new impurity peaks observed for the Blend electrode. These results, when combined, suggested the LCO, NCA, and Blend were all consistent with layered phase materials. The lack of impurity phases or shifting of peaks for the Blend suggested that the Blend was a combination of the NCA and LCO constituent particles with no new interfacial phases forming and limited inter-diffusion of transition metals, at least in the bulk material.Electrochemical CharacterizationLCO
[0069] To confirm the intrinsic electrochemical voltage profile of the synthesized LCO material, initial electrochemical evaluation was conducted on composite LCO electrodes paired with lithium metal anodes at relatively low rates of charge / discharge. The first charge and discharge voltage profiles of a LCO composite cell at C / 20 between 2.5-4.3 V (vs. Li / Li+) can be found in Supporting Information, FIG 6. The first discharge capacity was 130 mAh g'1LCO with over -90% of the discharge capacity delivered above 3.9 V (corresponding to -2.3 V relative to the plateau voltage of LTO), which was consistent with previous reports. AAM LCO cell rate capability and representative discharge voltage profiles can be found in FIGs 2a and 2b, respectively. Note that the AAM LCO was paired with a AAM LTO anode, which was why the cell voltage was substantially lower than the composite electrode paired with a Li metal anode. The AAM LCO cell achieved an initial discharge capacity at 1 mA of 88 mAh, which corresponded to 122 mAh g'1LCO. This was close to the composite cell gravimetric capacity, although ion transport limitations in particular may have limited achieving full gravimetric LCO capacity. At higher rate of 10 mA, the capacity dropped below 20 mAh, again consistent with ion transport limitations in these very thick electrode cells. After returning to the 1 mA low rate cycling, the last discharge cycle had a capacity of 79 mAh, or 90% of the initial discharge. This extent of capacity fade has been reported in previous reports with thinner LCO AAM electrodes, and may have been due to some structural collapse of the LCO material.NCA
[0070] As with the LCO, the NCA material was first evaluated in a composite electrode paired with a Li metal anode (FIG 6). The NCA had a first cycle discharge capacity of 185 mAh g'1NCA and over 90% of the capacity was delivered above 3.5 V for charge / discharge at C / 20 between a voltage window of 2.5-4.3 V (vs. Li / Li+). These results for NCA materials were consistent with previous reports. However, in the AAM electrode cell, the first discharge at the lowest rate of 1 mA was only slightly above 82 mAh, corresponding to 130 mAh g'1NCA which was much lower than the composite cathode cell. At a higher discharge rate of 2 mA (charge still 1 mA), the capacity dropped below 50 mAh, and much lower capacity was delivered at higher rates. This capacity retention at increasing rates for the NCA AAM electrode was much lower than for the LCO AAM electrode. Theonly difference in the two fabricated cells was the cathodes, and the cathodes had similar porosity and thickness which suggested factors outside of ion transport resistance played a role in the inferior rate capability for the NCA. It was expected that the cause of the lower rate capability of the AAM NCA relative to AAM LCO was the lower electronic conductivity of NCA material. While LCO has an electronic conductivity over 10 S m'1across most of the range of lithiation experienced by the material in the cell, NCA materials have been reported to have electronic conductivity below 0.1 S m’1. For additional insights into the role of electronic conductivity of NCA in the electrochemical outcomes for the AAM NCA electrode, dQ / dV analysis was conducted on the initial discharge for both composite NCA cells at C / 20 and AAM NCA cells at 1 mA. The dQ / dV plots can be found in FIG 3. For the plots in FIG 3, the x-axis is shown for both Li and LTO as the basis, with the assumption of an offset of 1.56 V for the plateau regions of LTO relative to Li / Li+. Inspection of the dQ / dV plots for composite NCA cells revealed three obvious peaks at 4.1 V, 3.9 V, and 3.7 V (vs. Li / Li+), which were at locations previously reported for phase transitions for NCA materials from H3 to H2, H2 to M, and M to Hl . However, for the AAM cell, the dQ / dV peaks were much weaker and broader. In addition, the largest dQ / dV peak had a shift of 0.16 V, which would be consistent with the limited electronic conductivity of the NCA electroactive material. The last cycle capacity retention was 84%, however, it was speculated that this may have been due to the electronic conductivity limitations of the AAM electrode material. To test this hypothesis, the cell was charged again and then a discharge was conducted at the much lower rate of 0.1 mA (see FIG 7, for the discharge profile). The discharge capacity achieved was 97 mAh, or 154 mAh g'1NCA, compared to 68 mAh for the preceding discharge at 1 mA. This outcome suggested the capacity was not able to be extracted due to the electronic conductivity limitations of the NCA material, which has been reported to be most severe at high extents of discharge / lithiation.Blend
[0071] The final AAM full cell evaluated electrochemically contained a AAM LTO anode and the Blend cathode with both LCO and NCA materials. Building off of a previous concept, the Blend was intended to result in a percolated LCO network to provide efficient electrode matrix electron conduction pathways while incorporating the higher energy density NCA material to increase overall cell capacity. At a rate of 1 mA, the discharge capacity reached 100 mAh, which to the authors’ knowledge is the highest reported for a rechargeable 2032 form factor cell. For reference, most commercial rechargeable 2032-type cells havecapacities ranging between 40-70 mAh (schematic of capacity range shown in FIG 4). It is noted that commercial primary / single use 2032 form factor cells often exceed 200 mAh, so the Blend AAM electrode full cells lie between commercial options for single use or rechargeable coin cells. With regards to rate capability, the Blend cathode AAM cell delivered 40 mAh and 20 mAh at 5 mA and 10 mA discharge rates, respectively. The cell capacity across all discharge rates was greater than the LCO AAM cell, which was consistent with the incorporation of the higher energy density NCA material. Also, the rate capability and material utilization was dramatically improved compared to the NCA AAM cathode cell, consistent with the hypothesis that the LCO provided a lower resistance pathway to overcome the electronic conductivity limitations that hindered the rate capability of the NCA electrodes. There was still loss of capacity with increasing rate of discharge, which was consistent with the ion transport overpotential of very thick electrodes in general. The first discharge dQ / dV curve was also analyzed for the Blend cathode cell (FIG 4). There was a large peak at ~2.3 V (vs. LTO), which was consistent with capacity contributions from the LCO material in the electrode. The remainder of the capacity from lower potentials was likely mostly from the NCA phase. The distinct regions of NCA and LCO capacity in the dQ / dV plot was consistent with the XRD and EDS results that suggested segregated NCA and LCO regions / particles in the electrode. Within the region of the dQ / dV expected to be due to the NCA component of the electrode, the strongest peak was at -2.05 V (vs. LTO), which was only 0.08 V shifted relative to the composite cell. This peak was -80 mV higher than the corresponding peak for the NCA AAM electrode, suggesting a substantial increase in the overall electrode matrix electronic conductivity. The last cycle (back at 1 mA) capacity retention was over 97% relative to the first cycle, the best among the three AAM cells evaluated.Conclusions
[0072] Coin cells were constructed using cathodes containing AAM electrodes with LCO, NCA, and a blend of LCO and NCA. NCA has higher energy density than LCO; however, in AAM electrodes pure AAM had limited capacity utilization which was suspected to result from the low electronic conductivity of NCA. An electrode with Blend of LCO and NCA resulted in the highest energy density battery cell, which was attributed to the LCO particles / phase providing sufficient matrix electronic conductivity and the NCA providing the increased energy density. The electrode with a blend of NCA and LCO achieved a reversible capacity exceeding 90 mAh in a 2032-type coin cell, which exceeds the capacity ofcommercial coin cells in this form factor. Rate capability still has limitations due to ionic transport limitations at the great electrode thicknesses, thus such cells would be suitable to relatively low rate and high energy rechargeable energy storage applications.EXAMPLE 2Methods & MaterialsActive Material Powder Synthesis
[0073] LNMO was synthesized via high temperature lithiation and calcination of a transition metal oxalate precursor. The precursor was synthesized using precipitation methods. 200 mM of sodium oxalate (Na2C2O4) was dissolved into 400 mL of deionized (DI) water within a 1000 mL beaker. 100 mM of manganese sulfate monohydrate (MnC2O4*2H2O, Fisher Chemical) and 100 mM of nickel sulfate hexahydrate (NiSCh’OFLO, Fisher Chemical) were dissolved into 400 mL DI water using a separate 1000 mL beaker. Both solutions were heated to 60 °C before pouring the Mn / Ni sulfate solution into the oxalate solution all at once. The precipitation reaction proceeded for 30 minutes at 60 °C at 300 RPM stirring. Then, the precipitate was collected using vacuum filtration and rinsed with 1.6 L DI water before drying overnight at 80 °C in air. The resulting Nio.5Mno.5C204*2H20 was mixed with LiOH with a target molar ratio of 1 : 1.1 transition metal :Li using mortar and pestle by hand for 10 minutes. The powder mixture was then transferred to a furnace (Carbolite CWF 1300) for calcination. The temperature profile for the thermal process included a hold at 480 °C for 3 hours and then 950 °C for 10 hours in air. Temperature increases occurred at a rate of 1 °C min'1, but the cooling rate back to room temperature was not controlled.
[0074] For LCO, 200 mM each of Na2C2O4 and cobalt sulfate heptahydrate (COSO4*7H2O, Acros Organics) were separately dissolved into 400 mL of DI water in two 1000 mL beakers. The reaction conditions were otherwise the same as the LNMO precursor synthesis. The CoC2O4*2H2O was mixed with Li2COs (Fisher Chemical) with a target molar ratio of 2: 1.05 oxalate precursor: lithium carbonate. The mixture was heated to 800 °C without a hold at the top temperature using a heating rate of 1 °C min'1. Upon reaching the set temperature, cooling proceeded to room temperature without temperature control. The synthesized powder was then ball-milled (Fritsch Pulverisette 7 planetary ball miller) with zirconia beads of 4.8 mm diameter for 5 hours at 300 RPM using a powder to beads mass ratio of 1 :5.AAM Electrode Fabrication
[0075] To fabricate AAM electrode cathodes, the synthesized active material powders of LNMO and LCO were used in isolation or in blends. For AAM anodes, the material was purchased from a commercial vendor and was LiMisOn (LTO, NEI corporation). Material and electrochemical properties for the LCO and LTO materials, both in conventional composite and AAM electrodes. To prepare a AAM electrode, 1 g of active material powder was blended with 2 mL of 1 wt.% polyvinyl butyral (PVB, Pfaltz & Bauer) in ethanol. The suspension was mixed using mortar and pestle by hand until the ethanol evaporated and the powder appeared dry. PVB-coated powder was used for fabricating all the AAM electrodes.
[0076] For AAM cathodes used in battery full cells, PVB-coated LNMO and LCO powder was used and blended at the desired mass ratio by hand using mortar and pestle. The compositions used on a LCO mass percentage basis were 0%, 15%, 30%, 45%, 60%, and 100% (denoted as 0%LCO, 15%LCO, 30%LCO, 45%LCO, 60%LCO, and 100%LCO). 0.2 g of resulting cathode powder was loaded into a pellet die (Carver) with diameter of 13 mm before being hydraulically pressed at 430 MPa for 2 minutes (Carver). The pressed pellet was thermally treated by heating to 600 °C at a rate of 1 °C min'1without a hold and then allowed to cool without control over the cooling rate to room temperature in air. 600 °C was chosen to according to previous studies, as below this temperature the pellets often have lower mechanical stability which impacts processing into functional cells. The AAM cathode pellets had thicknesses ranging from 450 to 550 pm as measured using calipers and loadings ranging from 145 to 150 mg cm'2. Due to the morphology and particle size differences, the pellet geometric void / pore volume fraction for pure LNMO was 0.41 and approximately linearly decreased to 0.33 for pure LCO (Fig. 8). No noticeable shrinkage or expansion was observed before and after the mild sintering for all processed pellets.
[0077] AAM cathodes were also processed and paired with Li metal anodes for experiments where constant current followed by constant voltage (CCCV) charging and electrochemical impedance spectroscopy (EIS) were conducted. For these cathodes, the PVB coated 0%LCO, 45%LCO, or 100%LCO powder of 0.2 g were pressed using a 16 mm diameter pellet die (Carver) at 280 MPa for 2 minutes. The same processing temperature after compression was used, and the same range of porosities were observed (and there was no shrinkage after thermal treatment of the pellets). The increased diameter of 16 mm was chosen to minimize excess electrolyte outside of the pellet region, which was important for analysis of the high frequency resistance. The resulting pellets had loadings 96-99 mg cm'2.
[0078] For AAM LTO anode fabrication for full cell batteries, 0.2 g of PVB-coated LTO was pressed following the same procedures as the cathode powders. For thermal treatment of the electrode, the temperature was increased at a rate of 1 °C min'1to 600 °C, held for 1 h, and the temperature was ramped down at a rate of 1 °C min'1back to room temperature. The AAM LTO electrodes had thickness ranging from 710 - 720 pm and loadings ranging from 148 - 152 mg cm'2, with geometric porosity / void fractions of 0.40.Material Characterization
[0079] Scanning electron micrographs (SEM) were collected using a FEI Quantum 650. Primary particle sizes were measured for 20 particles in SEM images to calculate mean primary particle size. SEMs were taken for both LNMO and LCO as both loose active material powder and after processing into AAM pellets. X-ray diffraction (XRD) patterns were collected on both powders and pellets using a PANalytical X'pert ProMPD.Electrochemical Characterization
[0080] For conventional composite electrode cells, the as-synthesized and “AAM- processed” (same thermal treatment procedure as AAM electrodes without hydraulic compression, and then the resulting powder was processed into a composite electrode) cathode active material powder (LNMO or LCO) was blended with acetylene carbon black (CB, Alfa Aesar), and polyvinyl pyrrolidone (PVP, Sigma Aldrich, 360 kDa molecular weight) using ethanol (Fisher) as solvent with a mass ratio of 8: 1 : 1 electroactive material:CB:PVP. The ethanol solution used in forming the slurry contained 3.33 wt% PVP. The blend was then processed in a slurry mixer (Thinky AR- 100) at 2000 RPM for 4 minutes, sonicated for 5 minutes, and blended in the slurry mixer for an additional 4 minutes at 2000 RPM. The resulting slurry was coated onto an aluminum foil using a doctor blade with a 400 □ m gap thickness. The casted conventional composite electrode was vacuum dried at 80 °C before punching into circular discs with an area of 1.33 cm2and transferring the electrodes into a glove box. The loadings for all conventional composite electrodes were 2-5 mg cm'2. Celgard 2325 punched into circular discs with an area of 1.98 cm2was used as separator and Li foil discs with an area of 1.60 cm2were used as anodes. 1.2 M LiPFe in 3:7 ethylene carb onate: ethyl methyl carbonate (Gotion) was used as electrolyte. Coin cells (2032-type) were assembled and cycled using a multichannel battery cycler (MACCOR) with a voltage range of 2.5 V to 4.4 V (vs. Li / Li+).
[0081] For AAM electrode cells, AAM pellet cathode and anode were adhered to a stainless steel bottom plate and a spacer, respectively, using a custom carbon paste. The carbon paste was made by blending a slurry consisting of by weight 4.76%:4.76%:90.48% CB:PVP: ethanol. The attached pellet electrodes were vacuum dried at 80 °C for 1 h before transferring to the glove box. Glass fiber (Fisher, type G6 circles) was used as a separator for AAM electrode cells and the same electrolyte as for the conventional composite electrode cells was used. Cells were cycled between 1.0 V and 2.85 V (cell voltage relative to LTO anode). Each individual charge and discharge cycle used the same current density, although the current density / rate applied was systematically varied for rate capability testing. Rate capability tests were conducted using C rates varying from C / 20 to C / 2.5, where the C rate was determined by cathode material mass and an assumed gravimetric capacity of 150 mAh g'1cathode. As a frame of reference, C / 20 for AAM electrode cells was -1.13 mA cm'2as loading was -150 mg cm'2.
[0082] The cells assembled for CCCV and EIS measurements were assembled in the glovebox using the same electrolyte as all other cells. The AAM cathode was paired with and circular Li foil of 2 cm2(same area as the AAM cathodes) as anode. Two layers of Celgard separator with diameter of 18 mm were used to prevent shorting during lithium plating. CCCV was performed by first charging the cell at a constant current of 1.1 or 0.55 mA cm'2until reaching a target voltage, and then holding at each target voltage for 20 h. The target voltages were between 3.9 to 4.4 V in 0.1 V increments. The CCCV was accomplished using a MACCOR multichannel battery cycler, and EIS was performed using a Gamry Reference 600 after each voltage hold. The high frequency intercept of the Nyquist plot was fitted using Zview. All cells for electrochemical characterizations were assembled inside the glove box.P2D Simulation
[0083] Simulations were based on the pseudo-two dimensional (P2D) framework originally developed previously, but with two features generally not incorporated in P2D LIB simulations. First, P2D simulations often assume a single and constant electrode matrix electronic conductivity, which is largely due to the conductive additives in the conventional composite. For AAM electrodes there are no conductive additives, and thus matrix electronic conductivity must be provided by the electroactive material itself. Thus, a variable matrix electronic conductivity for the electrode as a function of lithiation was used. The second modification was that for discharge simulations often the cathode and anode are assumed tostart with homogeneous lithium concentrations in the solid and liquid phases throughout a given electrode. However, for the discharge simulations herein the lithium distribution (in both liquid and solid phase) was initially heterogeneous as a function of electrode depth, with the concentration profile being determined by simulation of the preceding charge cycle. Details and discussion of these two modifications for AAM electrode LIB simulations can be found. Simulations were implemented using implicit numerical methods in Python 3.7. To simulate the 45%LCO cathode battery, the solid electrode had two electroactive materials instead of one. At each discretized point, the delithiation / lithiation happened to both electroactive materials. Overpotential distributions were also calculated, which provide insight into the processes that are contributing the most polarization during cell discharge.Results and DiscussionMaterial Characterization
[0084] The XRD patterns for synthesized powders of both LNMO and LCO are shown in Fig. 9. Each peak was assigned based on the expected space group for these materials of R-3m, and no impurity peaks were observed. SEM images of the powders revealed that LCO had an irregular particle morphology and relatively small primary particle size of 300 ± 150 nm, while LNMO had slightly larger primary particles of 420 ± 130 nm with a more rounded morphology (uncertainties were the standard deviation based on 20 randomly selected individual primary particles). Some of the differences in the observed morphology may have originated as a consequence of LCO undergoing a ball-milling process, while LNMO was not ball-milled. Part of the reason why LCO was ball-milled was to be consistent with processes used in prior reports, although for the goal of a blended electrode with percolated LCO finer LCO particles may also be desirable to improve dispersion in the interstitial regions between LNMO particles, though it is noted such morphology impacts on distribution of LCO material was speculative.
[0085] As described in herein, powders were hydraulically compressed and underwent an additional thermal treatment to form AAM electrodes. XRD patterns collected for all AAM electrodes can be found in Fig. 10. The XRD patterns suggested that the mild sintering procedure did not result in any new phases for 0%LCO (pure LNMO) and 100%LCO. With increasing LCO content, the relative peak intensity of the LCO constituent increased (e.g., the (003) peak at a 2theta of 18.96°) as expected. Although the thermal treatment would be expected to result in some interdiffusion between Co and Mn / Ni, from XRD the LCO and LNMO materials appeared to remain segregated and compositionally andstructurally distinct. More specifically, the (003) peak for pure LNMO was distinctly located at 29 of 18.63°, while for LCO the corresponding peak was at 29 of 18.96°. For the blended materials, the relative magnitudes of these peaks changed, but the peak positions did not shift, suggesting that the two materials remained largely compositionally and structurally segregated, at least for the bulk materials responsible for the XRD patterns.
[0086] For pure LCO and LNMO, with the mild thermal treatment conditions applied to the porous ceramic pellets, there was a slight increase in the mean primary particle size, however, the size distribution was wide so it was difficult to explicitly confirm a particle coarsening effect. The primary particle size was 400 ± 80 nm for LCO, and 460 ± 100 nm for LNMO (uncertainties based on standard deviation for 20 independent particle measurements). For the blend pellets, it was noticed that as the LCO content was increased the fraction of smaller particles observed in SEM also increased, consistent with a relative increase of the amount of smaller LCO particles in the electrode pellet.
[0087] Disordered jammed sphere packing, expected to be a reasonable representation of the AAM electrodes, has been reported to have a critical volume fraction to achieve percolation for a given sphere material in the system of 0.199 for a three-dimensional system. Based on the reported crystal density for LNMO and LCO, the LCO volume fraction reached 0.17 for 30%LCO (slightly below the threshold) and 0.27 for 45%LCO (well above the threshold). The calculated volume fraction of LCO for each sample can be found in Fig. 11. To further support the formation of a percolated LCO network, EDS mapping of 15%LCO, 30%LCO, 45%LCO, and 60%LCO AAM electrodes was performed. While the two- dimensional EDS maps cannot confirm that there was three-dimensional continuous connectivity of the LCO particles, it was observed that the LCO particles started to form larger connected regions for 45%LCO, and had a very well-connected structure for the 69%LCO. Due to the two-dimensional limitations of EDS and preferential surface sensitivity of the technique, formation of a percolated network of LCO may have occurred at a lower loading than the observed 45%LCO.Electrochemical CharacterizationPure LCO Cathode Cells Electrochemical Evaluation
[0088] To obtain data most representative of the intrinsic electroactive particle charge / discharge profiles, including any possible impact from the AAM processing withoutthe electronic conductivity and large thickness complications of the AAM electrodes, as- synthesized and “AAM treated” LCO or LNMO powder were first evaluated in conventional composite electrodes paired with Li metal anodes. The AAM treated materials underwent ethanol contact and thermal treatment consistent with AAM electrodes, but did not undergo hydraulic compression and were subsequently processed into composite electrodes. These composite cathode cells were galvanostatically cycled within a voltage window of 2.5 V to 4.4 V (vs. Li / Li+). The as-synthesized LCO electroactive material achieved 174 mAhg'1LCO for the first charge and 138 mAh g'1LCO for the first discharge cycle at a rate of C / 10 (initial charge / discharge cycle polarization curves can be found in Fig. 12a). Such low reversibility was likely from the negative impact from ball-milling, consistent with previous observations for these same materials. The AAM treatment composite LCO achieved 169 mAhg'1LCO for the first charge cycle and 146 mAh g'1LCO for the first discharge cycle. Such improvement in discharge capacity and reversibility was possibly due to the enhanced LCO crystallinity from heat treatment. The corresponding dQ / dV curves (shown in Fig. 12b) for the first cycle at C / 10 had a peak at ~3.9 V (versus Li / Li+) associated with the LCO voltage plateau for both as-prepared and AAM treated composite electrodes. However, for the AAM treated LCO, there were two more pronounced peaks at -4.05 V and -4.15 V, which was another indication of higher crystallinity of this LCO material. LCO processed into conventional composite cathodes exhibited electrochemical charge / discharge curves consistent with previous reports.
[0089] For the AAM LCO electrode (100%LCO) paired with AAM LTO using a voltage window from 1.0 V to 2.85 V (corresponding to approximately 2.56 V to 4.41 V vs. Li / Li+, assuming the OCV of LTO was 1.56 V vs. Li / Li+), the first cycle at a slow charge / discharge rate (C / 80) attained nearly the same gravimetric discharge capacity (139 mAhg'1cathode) as the conventional composite cathode cells (initial discharge voltage profile can be found in Fig. 13a). The AAM electrode cell dQ / dV calculated using the initial discharge curve (Fig. 13b) had a small initial peak at -2.6 V, which corresponded to the small peak at -4.15 V (vs Li / Li+, AAM treated LCO in conventional composite cell, Fig. 12b). There was a strong peak at 2.3 V, which was consistent with the conventional composite cell data. As shown in Fig. 14, at higher rates of C / 20, C / 10, C / 5, and C / 2.5, the AAM electrode cell discharge capacity was 112 mAh g'1, 62 mAhg'1, 29 mAh g'1, and 12 mAhg'1, respectively, on an LCO mass basis. Such decrease in capacity was expected to have originated from the ionic transport limitations though the thick electrode microstructure forthis material pairing, as has been described thoroughly in previous reports. Additional cycling voltage profiles and rate capability outcomes can be found in Fig. 14a and 15.Pure LNMO Cathode Cells Electrochemical Evaluation
[0090] For electrochemical cycling of as-synthesized and AAM treatment LNMO material processed into conventional composite cathode and paired with a Li metal anode, the same voltage window as with LCO of 2.5 V to 4.4 V (vs. Li / Li+) was used. The first discharge cycle at C / 10 reached 162 mAh g'1LNMO and 165 mAh g'1LNMO (see, Fig. 12) before and after AAM treatment, which did not have obvious impact on electrochemical outcomes. Such observation was consistent with previous literature, where ethanol treatment has been applied to layered phase oxides with high nickel amounts such asLiNi0.80Co0.15Al0.05O2 (NCA), and no major structural changes were observed, especially after an additional heat treatment. The dQ / dV of LNMOs for the initial discharge cycle compared to that of LCO had a broader peak located at slightly lower voltage of 3.75 V (see, Fig. 12d).
[0091] For the AAM LNMO cathode cell (0%LCO in Fig. 13), the first discharge at C / 80 (0.282 mA cm’2) only reached 97 mAh g'1cathode (Fig. 14). Based on the conventional composite electrode dQ / dV result and the voltage offset from using LTO in the AAM cell, a peak was expected at 2.16 V; however, a sharp dQ / dV peak was not observed for this discharge (Fig. 13b). The first cycle discharge capacity retention of the AAM cell relative to the conventional composite cathode cell for LNMO was 60%, while for LCO it was 99% at C / 80. Such differences were hypothesized to result from the much lower electronic conductivity of the LNMO, which has been reported with a range from 10'5to 10'6S cm’1for the pristine material before cycling.31,32These electronic conductivity values are more than 4 orders of magnitude lower than LCO, where for over 95% of the lithiation range typically accessed for LCO the electronic conductivity is over 10'1S cm’1. Cells cycled at C / 200 and C / 500 delivered 117 mAh g'1LNMO and 138 mAh g'1LNMO on the first discharge cycle, which was 72% and 85% retention relative to conventional composite electrode initial discharge gravimetric capacity. Interestingly, the first charge capacities at C / 200 and C / 500 were quite similar (169 mAh g'1and 171 mAh g'1), where the differences (2 mAh g'1cathode) were much smaller than that of the discharge (21 mAh g'1cathode). This outcome was consistent with the LNMO material having a variable electronic conductivity as a function of lithiation, where the electronic conductivity increases upon delithiation similar to other layered materials such as LCO. Thus, the charging process may have extracted all availablecapacity from the LNMO active material, facilitated by the improved electronic conductivity as the material was delithiated. However, as more Li intercalated into the LNMO crystal during discharge, the electronic conductivity would have decreased. This severe drop would have resulted in electronic overpotential which likely limited the electrochemical capacity that was able to be discharged. The later P2D simulations section contains a more detailed discussion of the impacts of LNMO electronic conductivity.
[0092] Although LNMO has lower electronic conductivity than LCO, at C / 10 the AAM LNMO discharged 63 mAh g’1, which was greater than the pure AAM LCO. This was likely due to a few contributing factors. First, as mentioned earlier it was suspected that LNMO has an increasing electronic conductivity with delithiation, and thus was able to extract that level of capacity at C / 10 before reaching extents of lithiation during discharge where the electronic conductivity dropped, and the resulting overpotential limited the ability to deliver additional capacity. Second, another factor beyond electronic conductivity was the potential of the electrochemical reactions for the different cathode materials (e.g., thermodynamic, or OCV, factors). LNMO had an overall lower OCV for electrochemical charge / oxidation compared to LCO. As an example, a large charging voltage plateau region for LCO was -0.14 V higher than that of LNMO (see, Fig. 12). The lower charging potential for extracting lithium and capacity means that after reaching an equivalent charging capacity that LNMO has greater potential range remaining before hitting the cutoff voltage, where the cutoff was the same for all AAM electrode full cells. Thus, the relative thermodynamic driving force for extracting additional capacity on charge at greater charging extents was expected to be greater for LNMO relative to LCO. In addition, porosity of AAM LCO electrodes (-0.33) was lower than that of LNMO electrodes (-0.41), likely due to morphology differences for the powders. Thus, the overpotential from ion transport through the electrode microstructure was greater for the LCO electrodes relative to LNMO electrodes. Ion transport through the electrode microstructure has previously been demonstrated to be a major limiting factor for thick AAM electrodes, and the higher porosity for the LNMO would improve the relative ionic conductivity of these electrodes. At higher rates such as C / 5 the AAM LMNO delivered very low capacity (6 mAh g'1), suggesting the low electronic conductivity of LNMO (0%LCO) was too resistive at that rate to facilitate much of the electrode achieving high extents of lithiation. Voltage profiles and rate capability results starting from C / 20 can be found in Figs. 14f and 15.Blended LNMO / LCO Cathode Cells Electrochemical Evaluation
[0093] Discharge capacities at different rates for AAM electrodes with LCO, LNMO, and all evaluated blend compositions can be found in Fig. 14. A dashed line at the top of the Fig. connects the gravimetric discharge capacities of LCO and LNMO in conventional composite electrodes, and was considered as representing the maximum extractable capacities of each composition AAM electrode at low rates and without electrode electronic and ionic conductivity limitations. As the relative LCO content in the AAM electrodes increased, at the slow rate of C / 80, the discharge capacity moved closer to the conventional composite electrode gravimetric limit / line. This outcome was attributed to the increasing electronic matrix conductivity as the LCO relative content was increased. As the relative LCO content was increased from 0%LCO to 15%LCO at the slow rate of C / 80, the gravimetric discharge capacity dramatically increased from -97 to -141 mAh g'1cathode, although the increase in capacity with further increase in LCO electrode content was minimal - the discharge capacity more or less was the same for the different blend compositions. At the higher rates, C / 10 and C / 5 in particular, the greatest discharge capacity was observed for the 45%LCO. This result was speculated to result from a combination of (i) reaching above a threshold LCO fraction for a well-connected LCO electronically conductive percolated network; (ii) still having significant LNMO content with its OCV function that had greater lower voltage capacity and resulted in greater driving force when approaching the higher voltage charging cutoff; and (iii) an intermediate porosity to the pure LCO and LNMO AAM electrodes to at least provide lower ionic overpotential relative to the pure LCO AAM electrodes. In summary, the combination of material (LCO) with relatively higher electronic conductivity and lower gravimetric capacity with material (LNMO) with relative higher gravimetric capacity and porosity but lower electronic conductivity resulted in increased gravimetric discharge capacity than either of these materials used alone in AAM electrodes. Charge / discharge voltage profiles at higher rates for all the material compositions can be found in Fig. 14.
[0094] Closer inspection of the first discharge voltage profile at C / 80 (Fig. 13a) revealed that as the LCO content in the AAM electrodes increased, the average discharge voltage also increased. This was a consequence not only of the higher electronic conductivity of LCO compared to LNMO, but the intrinsic properties of the material with regards to the potentials at which the intercalation reactions occur. The relative impact of the voltage of the electrochemical reactions of the different materials can be further informed by examining thedQ / dV of the first discharge voltage profile at C / 80 (Fig. 13). As mentioned previously, pure LNMO (0%LCO) had a very broad dQ / dV across the voltage range without a sharp peak. However, even the 15%LCO AAM cathode had a clear dQ / dV peak assigned as arising from the LNMO component at 2.16 V (vs. LTO / anode). As the LCO content in the electrodes was increased from 15%LCO towards 100%LCO, the dQ / dV peak that was due to the LCO component (at ~2.3 V) increased while the LNMO dQ / dV peak decreased, as would be expected for their changing relative compositions in the electrodes. However, the LNMO peak intensity change was not proportional to the LNMO content, in particular when comparing the dQ / dV peaks for 15%LCO and 30%LCO. This observation may have been due to the more limited improvement in matrix electronic conductivity at these extents of LCO loading, which then did not enable the LNMO to be fully accessible in the electrode for delivering capacity at these discharge rates.P2D Simulations and AnalysisPure LNMO AAM Electrode Simulation
[0095] Representative simulation of the discharge of AAM cathodes relies on an accurate electronic conductivity as a function of lithiation for the active materials. Previous reports investigating AAM LTO / LCO full cells using both simulation and experiments illustrated the importance of using a variable matrix electronic conductivity of the electrode as a function of lithiation to have better agreement experimentally with not only the voltage profile, but also the lithium intercalation positions / depths during cycling. The lack of LNMO electronic conductivity as a function of lithiation resulted in a poor match between the simulated and experimental voltage profiles. Using the measured value of 9.5 x 10'4S nr1for as synthesized / fabricated LMNO pellets as a constant electronic conductivity in simulation, the predicted voltage curve at C / 20 was not representative of the experimental curve, where the predicted capacity and average discharge voltage were only 18 mAh g'1cathode and 1.70 V, compared to the experimental measurements of 91 mAh g'1cathode and 2.15 V (Fig. 17a). Both LCO and LNMO have a similar layered oxide crystal structure. For LCO, upon delithiation the production of Co4+and the shortened distance between Co-Co has been reported to result in high electronic conductivity. Although for LNMO the transition metals were Mn and Ni instead of Co, it was speculated that decreasing transition metal-transition metal distances would similarly increase the electronic conductivity of LNMO upondelithiation. The LNMO electronic conductivity at high levels of delithiation was assumed to have a plateau similar to LCO, and then taper down to the experimental value measured at full lithiation. The LNMO value for the plateau region (the “high” conductivity) was adjusted until the error relative to the discharge profile at C / 20 was minimized. The corresponding fitted electronic conductivity was plotted and can be found in Fig. 18. The predicted capacity and average voltage for the fitted electronic conductivity profile were 93 mAh g'1cathode and 2.13 V, which had much improved agreement with the experimental values (Fig. 17a).
[0096] An overpotential distribution analysis throughout the discharge simulation was performed (Fig. 17b), and a detailed introduction of the process associated with such analysis can be found in a previous report.14In brief, the overpotentials associated with ionic resistance, electronic resistance, interfacial resistance, and OCV differences are calculated at different depths within the cell during the discharge simulation. These overpotentials are then weighted by the electrochemical current being produced at each location, and then summed. Thus, at any given point in the discharge the relative overpotential for each of the resistances mentioned above for the cathode, anode, and separator were calculated. Such analysis provides insights into the factor(s) responsible for deviations between the discharge potential and the thermodynamic maximum potential for a given extent of discharge capacity delivered. In addition, the electrolyte and electrode Li+concentrations at selected discharge capacities were calculated during the simulation and can be found in Fig. 19.
[0097] Due to the limited electronic conductivity of the solid phase (lower than ionic conductivity of electrolyte phase), the initial condition from discharge simulation included a more delithiated region near the current collector for the LNMO electrode (Fig. 19b). For the first 10 mAh g'1cathode discharged, due to a combination of the OCV difference across the cathode depth due to the lithiation distribution at the end of charge and the limited electronic conductivity, the intercalation was largely confined near the current collector in the LNMO (Fig. 19b). The OCV overpotential contribution was even negative due to the more lithiated LNMO near the current collector, and the low electronic conductivity drove the electronic overpotential to -0.08 V (Fig. 17b). As the discharge proceeded up to 79 mAh g'1cathode, the intercalation preferentially still happened near the current collector side, which was due to the low matrix electronic conductivity arising from the LMNO material. The electronic overpotential reached a plateau of -0.11 V, which notably exceeded the other overpotential sources, including the sum of overpotentials from the separator and anode. The OCV overpotential reached a plateau of —0.09 V and resulted from the material being morelithiated near the current collector side first during discharge, and thus net resulted also due to the low electronic conductivity of the LNMO material. For the rest of the discharge process (concluding at 93 mAh g'1cathode), very little lithiation occurred in the LNMO near the current collector due to the limited capacity still available in this region, which then resulted in more lithiation occurring near the separator. The current had to travel via the electroactive material before reaching the lithiation region near the separator and the electronic conductivity near the current collector had significantly decreased due to that material being near the full lithiation state. These two effects combined to result in the electronic overpotential significantly increasing. In summary, the following processes result in the LNMO cathode full cells having relatively low discharge capacity: (i) the low electronic conductivity drove intercalation / lithiation early in the discharge near the current collector region in the cathode; (ii) once the current collector side reached near its capacity limit, more and more current had to pass through this region which had very low electronic conductivity (due to decreasing electronic conductivity with increasing lithiation); and (iii) the electronic overpotential then severely increased, causing the cell voltage to plummet and reach the lower voltage cutoff.45%LCO AAM Electrode Simulation
[0098] For the 45%LCO AAM electrode, it was assumed that 1) the LCO was at sufficient volume fraction to form a percolated network, and 2) the LCO electronic conductivity as a function of lithiation was the same as for pure LCO. The matrix electronic conductivity effectively followed the LCO material conductivity because the electronic resistance was so much lower relative to the LNMO material. It is noted that the second assumption would require minimal incorporation of the Ni or Mn into the LCO material in the electrode, which was consistent with the XRD results. The electronic conductivity for the LCO as a function of lithiation can be found in Fig. 18. The simulated discharge voltage profile at C / 20 matched the experimental profile well (Fig. 17c), except that at later points in the discharge (over 80 mAh g'1cathode) the simulated voltage was slightly higher. Such deviation was possibly due to (i) inhomogeneous distribution of LCO in the electrode; (ii) the electronic conductivity enhancement from LCO was less effective because further in the discharge the LCO was at near full lithiation state with relatively low electronic conductivity (to be elaborated on later); and (iii) the co-diffusion of Mn, Ni, and Co from mild sinteringwas not detected in the bulk but still sufficiently reduced the electronic conductivity of the percolated LCO network relative to pure LCO.
[0099] The electrochemical potential of the electrode materials provides the driving force for the electrochemical reactions to occur. This can be analyzed in the context of the OCV of the materials in the electrode, which varies as a function of charge / discharge time and location as the reactions proceed. LCO had -90% of its capacity above -3.8 V (versus Li / Li+), where LNMO had only -56% of its capacity above this voltage. Before moving to the same analysis as the one done to the pure LNMO cell, a capacity contribution separately from each material (LNMO and LCO) was extracted from the simulation and can be found in Fig. 6. For the first -30 mAh g'1cathode capacity delivered, both LCO and LNMO contributed roughly similar capacity, which could be attributed to the initially sloped OCV functions for both materials. From -30 until -60 mAh g'1cathode capacity delivered, the LCO started to contribute more capacity because it had much more capacity at -2.3 V (cell voltage, corresponding to the LCO voltage plateau at -3.9 V vs. Li / Li+). From -60 until -115 mAh g'1cathode capacity delivered, the LNMO replaced LCO as the major capacity contributor due to its voltage plateau at -2.1 V (cell voltage, corresponding to the LNMO voltage plateau at -3.7 V vs. Li / Li+). For the final portion of delivered capacity until the end of discharge, both LCO and LNMO approximately equally contributed capacity, due to the sloped OCV function and similar to the early portion of the discharge capacity. It is noted here that the blended electrodes result in the electrochemical lithiation during discharge being more distributed throughout the electrode depth during discharge. In contrast, single component electrodes had more localized electrochemical activity as a function of cell depth. It is speculated that spreading out the reaction as a function of electrode depth may have advantages in accommodating the changes in stress / strain that accompany changes in lithium composition in the AAM electrodes. Such mechanical advantages are speculative, but are intended to be investigated in more detail in future work.
[0100] The same overpotential distribution analysis from the simulation results as was conducted for the LNMO AAM electrode cell was performed for the cell with the 45%LCO cathode and is shown in Fig. 17d. The Li concentration in the electrode for the solid (averaged based on the wt.% of LNMO and LCO) and electrolyte phase can be found in Fig. 20. The change in Li electrode concentration of each of LNMO and LCO at selected delivered capacity points is also provided in Fig. 21. For the first 30 mAh g'1cathode capacity delivered, both LCO and LNMO had slightly more Li intercalated near the separatorregion. This was in contrast to the pure LNMO case where the initial intercalation was near the current collector and was due to the relatively higher electronic conductivity of the blended material solid electrode compared to the ionic conductivity of the electrolyte. The interfacial overpotential from LNMO was slightly greater than that of the LCO, which originated from the smaller interfacial area of LNMO and smaller reaction rate constant used in the simulation. From 30 until 56 mAh g'1cathode capacity delivered, the LCO interfacial overpotential increased but that of LNMO decreased, which was because the LCO was in its voltage plateau regions and thus less capacity was provided by LNMO in this region. Correspondingly, much more Li was intercalated into LCO and also more Li was intercalated near the separator region. From 56 until 78 mAh g'1cathode capacity delivered, the capacity from LCO voltage plateau was nearly depleted. A large amount of Li intercalated into the LCO, but this capacity was concentrated in the current collector region. Such observation was consistent with previous thick AAM electrode reports, where an electrode with a flat OCV curve and relatively higher electronic conductivity (relative to ionic conductivity) resulted in a reaction front which initiated from the separator and propagated towards the current collector. Correspondingly, the ionic overpotential rose and fell depending on whether it was further from or closer to the separator, respectively. From 78 to 110 mAh g'1cathode capacity delivered, the LNMO interfacial overpotential increased but that of LCO decreased, which was because the LNMO started delivering a larger fraction of the capacity due to now being in the LNMO voltage plateau region. In examining the change in Li electrode concentration, the LNMO accepted more Li, but the reaction was not as concentrated as LCO at the separator side. Such behavior may have resulted due to (i) the electrode electronic conductivity was not as high as when LCO was being discharged because the LCO network was now at a much higher extent of lithiation and correspondingly lower electronic conductivity; (ii) LNMO had slightly smaller reaction rate constant and interfacial area than that of LCO; and (iii) LNMO OCV compared to LCO was more sloped (see, Fig. 12), and flatter OCV profiles promote sharper reaction propagation gradients.
[0101] From 110 mAh g'1cathode capacity delivered until the end of discharge, a reaction front in the LNMO similar to that observed for LCO earlier was observed. There was also a similar peak that occurred with regards to the ionic overpotential, and more Li was intercalated into the LNMO at the current collector side. Note that the electronic overpotential throughout the discharge was dramatically suppressed from the electronic conductivity enhancement of the blended LCO. The electronic overpotential started toincrease at -120 mAh g'1cathode capacity due to the decreasing electronic conductivity of LCO phase. Such decrease in electronic conductivity of LCO led to a decreased voltage, and the resulting voltage was lower than observed experimentally suggesting that the electronic conductivity in the simulation may have been underestimated at high extents of lithiation for the LCO.EIS and CCCV analysis
[0102] EIS measurements were also conducted as a function of charging voltage for AAM cathodes. The cathodes were paired with Li metal to avoid effects from the lithiation heterogeneity of the LTO AAM anode. The P2D simulations suggested Li inhomogeneity developed as a function of depth in the thick AAM electrodes, thus the charging profile was CCCV, where a long voltage hold of 20 hours was used at heat voltage where EIS was conducted to minimize lithiation heterogeneity within the electrodes as a function of depth. It was expected that these the high frequency intercept region from these EIS measurements would provide insights into the relative electronic conductivity changes of the AAM cathodes as a function of delithiation. The high frequency intercept (Rceii) from the Nyquist plot was extracted at each 0.1 V increment of the charging process for the cell. At the high frequency, interfacial and slower diffusive processes were excluded, and the current through the AAM electrode could be treated as a transmission line model59, where the current partially travelled through the solid AAM electrode and partially travelled through the liquid electrolyte. The relative passage of current was determined by the relative electronic conductivity of AAM electrode and ionic conductivity of liquid electrode in the interstitial region of the AAM electrode. However, because the electronic conductivity in the AAM electrodes was expected to vary by orders of magnitude, and could swing from orders of magnitude above and below the ionic conductivity of the liquid electrolyte, quantitatively calculating the electronic conductivity was challenging. In addition, it is noted that the high frequency intercept reflects multiple other contributions which could influence interpreting changes in its magnitude, including the change in electrolyte ionic conductivity due to irreversible side reactions which can change electrolyte concentration upon cycling, contact resistance between the current collectors and electrodes, and external cell connections. The Rceii values were fitted using an equivalent circuit model for the lithium half cell, with model and plots shown in, Fig. 22.
[0103] In qualitatively examining the Rceii at different holding voltages (Fig. 7a), all three cells started at -10.6 Q, suggesting the pristine AAM electrode without delithiation had electronic conductivities which were much lower than the electrolyte conductivity, and thus the liquid electrolyte carried the most of the current. Such observation was consistent with the literature reported and measured electronic conductivity data, where the solid LCO and LNMO were both over 2 orders of magnitude lower in electronic conductivity than the ionic conductivity of the liquid electrolyte. Until 3.9 V, the LCO had the largest decrease in Rceii followed by 45%LCO, and the LNMO, implying electronic conductivity increased in all AAM electrodes. Such observation was also consistent with the aforementioned cell data. Between 3.9 V and 4.4V, all Rceii values increased, which may have been due to reductions in the ionic conductivity in the liquid electrolyte. It is expected that the electrolyte would be consumed by side reactions for both the cathode electrolyte interface (CEI) and solid electrolyte interface (SEI) on the Li foil. SEI would be expected to especially consume electrolyte during the lithium plating which occurred during the charging process. Note that the areal AAM loading was on the order of 100 mg cm’2, thus thick SEI should form during charge and change the electrolyte composition dramatically. The LCO and 45%LCO had very similar trends in Rceii values, which supported the speculation that 45%LCO had a percolated LCO network which resulted in an electronic conductivity similar in magnitude to pure LCO. The increase in Rceii for both LCO and 45%LCO at higher voltages had smaller increases than the LNMO AAM electrode cell. This would be consistent with lower electronic conductivity for the LNMO because for that material a higher fraction of the current must travel through the liquid electrolyte, which would result in a greater Rceii increase if the electrolyte concentration changed and the resulting electrolyte conductivity decreased.
[0104] CCCV profiles (Fig. 7b-d) were also evaluated for the different AAM electrode cells. For LCO, only a small capacity was achieved below 3.9 V, which was attributed to the relatively low electronic conductivity at the extent of lithiation below this potential and the relatively low amount of capacity for LCO at this lower redox potential. Above 3.9 V, the charging capacity from during the CC steps in the experiment were much greater, suggesting the increased electronic conductivity of LCO after delithiation had facilitated less polarization from that process within the cell.
[0105] For LNMO, nearly all capacity occurred during the CV step until 4.4 V. One specific observation of note was the CV step at 3.9 V, where there was an initial increase incurrent followed by a decrease. In most cases for a CCCV discharge, the current is supposed to exponentially decay during the CV step. Such observation was additional support that the electronic conductivity increased for LNMO with delithiation. However, this electronic conductivity increase was still insufficient to provide much charge capacity during the subsequent CC step. A separate identically processed cell was charged with CCCV mode all the way to 4.4 V (CCCV profile can be found in Fig. 23) with half of the current density. The voltage initially spiked to ~4.0 V (~0.3 V above the potential from the same material processed into a composite electrode), then decreased down to -3.9 V, and finally more gradually increased to 4.4 V. There was no material activation process in the identical material evaluated in conventional composite electrodes at C / 10 (Fig. 12). Thus, this initial voltage spike and then decline on charge was attributed to the LNMO electronic conductivity effect on the electrode matrix electronic conductivity as a function of the extent of lithiation.
[0106] The 45%LCO AAM electrode had similar CCCV patterns to the LCO AAM electrode, where below 3.9 V there was minimal capacity from CC mode. Above 4.0 V, the charge capacities during CC steps were much greater. These observations were also consistent with the aforementioned trend where 45%LCO was expected to approach LCO AAM electrode electronic conductivity due to LCO material percolation.Conclusions
[0107] In this Example, AAM electrode full cells were fabricated where the cathode was either all LCO, all LNMO, or a blend of the two components. Pure LCO had been previously reported as a AAM cathode material and has advantages particularly with regards to electronic conductivity because within AAM electrodes the electrons must transport through the electroactive material itself in the electrode matrix. LNMO served as a model alternative layered phase metal oxide material, where the gravimetric capacity is higher than LCO, but the electronic conductivity especially at high extents of lithiation is much lower. Pure LNMO AAM electrodes resulted in cells with high polarization and low capacity and rate capability during discharge. Blends of LNMO and LCO were investigated with the aim of forming a percolated network of LCO to conduct the electrons through the cathode matrix. Experimental results suggested the LCO and LMNO remained segregated as separate phase particles during processing, and that the addition of LCO significantly improved the discharge capacity and rate capability of AAM electrode cells containing these cathodes. To provide further support for the role of LCO in the improved electrochemical outcomes for the AAM electrodes, P2D simulations were conducted. The P2D simulations further supportedthat the source of high voltage drops and capacity limitations for pure LNMO AAM electrodes was the limited electronic conductivity of the material. After modification of the electronic conductivity as a function of lithiation, the simulations were able to match the experimental polarization curves well and provide further insights into the discharge process for the blended LCO and LNMO electrodes. Additional EIS and CCCV analyses were performed, which were consistent with the role of electronic conductivity of the AAM electrodes with regards to dependence on electrode composition and extent of delithiation. This study provides support for the use of a percolated secondary phase to enable the use of low electronic conductivity electrode materials in AAM electrode cells at reasonable rates, provided that undesirable interfacial phases do not form during the processing of these multicomponent all active material electrodes.
[0108] The terms and expressions that have been employed are used as terms of description and not of limitation, and there is no intention in the use of such terms and expressions of excluding any equivalents of the features shown and described or portions thereof, but it is recognized that various modifications are possible within the scope of the aspects of the present subject matter. Thus, it should be understood that although the present subject matter has been specifically disclosed by specific aspects and optional features, modification and variation of the concepts herein disclosed may be resorted to by those of ordinary skill in the art, and that such modifications and variations are considered to be within the scope of aspects of the present subject matter.Additional Aspects.
[0109] The following exemplary aspects are provided, the numbering of which is not to be construed as designating levels of importance:
[0110] Aspect 1 provides an electrochemical storage device comprising LiNi0.80Co0.15Al0.05O2 (NCA), LiCoO? (LCO), or a blend thereof.
[0111] Aspect 2 provides the electrochemical storage device of Aspect 1, wherein the electrode is a sintered electrode.
[0112] Aspect 3 provides the electrochemical storage device of any one of Aspects 1 or 2, wherein the electrode is a composite electrode.
[0113] Aspect 4 provides the electrochemical storage device of Aspect 3, wherein the composite electrode comprises a metallic substrate to which the LiNi0.80Co0.15Al0.05O2 (NCA), LiCoO2 (LCO), or blend thereof is applied.
[0114] Aspect 5 provides the electrochemical storage device of Aspect 4, wherein the metallic substrate comprises a stainless steel, aluminum, alloys thereof, or mixtures thereof.
[0115] Aspect 6 provides the electrochemical storage device of any one of Aspects 1-5, wherein a thickness of the electrode is in a range of from about 50 pm to about 2000 pm.
[0116] Aspect 7 provides the electrochemical storage device of any one of Aspects 1-6, wherein a thickness of the electrode is in a range of from about 70 pm to about 400 pm.
[0117] Aspect 8 provides the electrochemical storage device of any one of Aspects 1-7, wherein the electrode is substantially free of a conductive additive.
[0118] Aspect 9 provides the electrochemical storage device of Aspect 8, wherein the conductive additive comprises a polymer binder, a conductive carbon, or a mixture thereof.
[0119] Aspect 10 provides the electrochemical storage device of any one of Aspects 1-9, wherein a porosity of the electrode is in a range of from about 30% to about 50 %.
[0120] Aspect 11 provides the electrochemical storage device of any one of Aspects 1-10, wherein a porosity of the electrode is in a range of from about 35% to about 40 %.
[0121] Aspect 12 provides the electrochemical storage device of any one of Aspects 1-11, wherein a capacity of the electrode is in a range of from about 7 mAh / cm2to about 100 mAh / cm2.
[0122] Aspect 13 provides the electrochemical storage device of any one of Aspects 1-12, wherein a capacity of the electrode is in a range of from about 10 mAh / cm2to about 50 mAh / cm2.
[0123] Aspect 14 provides the electrochemical storage device of any one of Aspects 1-13, wherein the electrode is an anode.
[0124] Aspect 15 provides the electrochemical storage device of any one of Aspects 1-14, wherein the electrode is a cathode.
[0125] Aspect 16 provides the electrochemical storage device of any one of Aspects 1-15, wherein the electrode comprises one dopant.
[0126] Aspect 17 provides the electrochemical storage device of Aspect 16, wherein the electrode comprises at least two dopants.
[0127] Aspect 18 provides the electrochemical storage device of any one of Aspects 16 or 17, wherein the at least one dopant has a 1+, 2+, or 3+oxidation state.
[0128] Aspect 19 provides the electrochemical storage device of any one of Aspects 1-18, wherein the at least one dopant comprises copper, aluminum, sulfur, potassium, or a mixture thereof.
[0129] Aspect 20 provides the electrochemical storage device of any one of Aspects 1-19, wherein the electrode is a battery anode.
[0130] Aspect 21 provides the electrochemical storage device of any one of Aspects 1-20, wherein the electrode is a battery cathode.
[0131] Aspect 22 provides the electrochemical storage device of any one of Aspects 1-22, wherein the electrode is free of a binder, an inactive solid additive, or a mixture thereof.
[0132] Aspect 23 provides the electrochemical storage device of any one of Aspects 1-22, wherein the LiCoCh (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA) independently range from about 5 wt% to about 95 wt% within a blend LiCoO? (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA).
[0133] Aspect 24 provides the electrochemical storage device of Aspect 23, wherein the LiCoO2 (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA) independently range from about 20 wt% to about 70 wt% of a blend LiCoO2 (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA).
[0134] Aspect 25 provides the electrochemical storage device of Aspect 24, wherein the LiCoO2 (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA) independently range from about 40 wt% to about 60 wt% of a blend LiCoO2 (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA).
[0135] Aspect 26 provides a battery comprising: a first electrode corresponding to the electrode of any one of Aspects 1-25; a second electrode spaced apart from the first electrode; and a separator positioned between the first electrode and the second electrode.
[0136] Aspect 27 provides the battery of Aspect 26, wherein the separator comprises a glass fiber or porous polymer.
[0137] Aspect 28 provides the battery of any one of Aspects 26 or 27, wherein the battery is a 2032-type cell or other small form factor geometry.
[0138] Aspect 29 provides an article comprising the electrochemical storage device of any one of Aspects 1-28.
[0139] Aspect 30 provides a method of making the electrode of any one of Aspects 1- 29, the method comprising: contacting components of an electroactive material; blending the components of the electroactive material; and sintering the blended electroactive material to form the sintered electrode.
[0140] Aspect 31 provides the method of Aspect 30, wherein the sintering is performed at a temperature in range of from about 500 °C to about 1100 °C.
[0141] Aspect 32 provides the method of any one of Aspects 30 or 31, wherein the sintering is performed at a temperature in range of from about 700 °C to about 900 °C.
[0142] Aspect 33 provides the method of any one of Aspects 30-32, wherein sintering is performed at a variable temperature.
[0143] Aspect 34 provides the method of any one of Aspects 30-33, wherein sintering is performed over a period of time in a range of from about 0.5 hours to about 20 hours.
[0144] Aspect 35 provides the method of any one of Aspects 30-34, wherein sintering is performed over a period of time in a range of from about 16 hours to about 18 hours.
[0145] Aspect 36 provides the electrochemical storage device of any of Aspects 1-25, wherein the blend comprises LiCoO2 (LCO) and LiNi0.80Co0.15A10.0502 (NCA) in a weight ratio ranging from about 40 wt% to about 60 wt% LCO and from about 60 wt% to about 40 wt% NCA, providing a balance between electronic conductivity and energy density.
[0146] Aspect 37 provides the electrochemical storage device of Aspect 36, wherein the electrode has a porosity in a range of from about 35% to about 40%, which is optimized to facilitate ion transport while maintaining mechanical integrity during charge-discharge cycles.
[0147] Aspect 38 provides the electrochemical storage device of any of Aspects 1-25, wherein the LiCoO2 (LCO) is synthesized using a sol-gel method that ensures a high degree of purity and phase homogeneity, contributing to the stability and performance of the electrode.
[0148] Aspect 39 provides the electrochemical storage device of any of Aspects 1-25, wherein the LiNi0.80Co0.15A10.0502 (NCA) is synthesized through a high-temperature lithiation process that promotes the formation of a well-defined crystal structure, enhancing the electrochemical capacity of the electrode.
[0149] Aspect 40 provides the electrochemical storage device of any of Aspects 1-25, wherein the electrode is characterized by a microstructure that is formed by a blend of electroactive materials processed via hydraulic compression and mild sintering, resulting in an electrode architecture that is free of polymer binders and conductive additives, thereby increasing the active material content and energy density of the electrode.
Claims
CLAIMSWhat is claimed is:
1. An electrochemical storage device comprising an electrode comprising LiNi0.80Co0.15Al0.05O2 (NCA), LiCoO? (LCO), or a blend thereof.
2. The electrochemical storage device of claim 1, wherein the electrode comprises all electroactive materials, electroactive materials facilitate improved electronic conduction through a microstructure matrix of the electrode.
3. The electrochemical storage device of any one of claims 1 or 2, wherein the electrode is a composite electrode or a sintered electrode.
4. The electrochemical storage device of claim 3, wherein the composite electrode comprises a metallic substrate to which the LiNi0.80Co0.15Al0.05O2 (NCA), LiCoO2 (LCO), or blend thereof is applied.
5. The electrochemical storage device of claim 4, wherein the metallic substrate comprises a stainless steel, aluminum, alloys thereof, or mixtures thereof.
6. The electrochemical storage device of any one of claims 1-5, wherein a thickness of the electrode is in a range of from about 50 pm to about 2000 pm.
7. The electrochemical storage device of any one of claims 1-6, wherein a thickness of the electrode is in a range of from about 70 pm to about 400 pm.
8. The electrochemical storage device of any one of claims 1-7, wherein the electrode is substantially free of a conductive additive.
9. The electrochemical storage device of claim 8, wherein the conductive additive comprises a polymer binder, a conductive carbon, or a mixture thereof.
10. The electrochemical storage device of any one of claims 1-9, wherein a porosity of the electrode is in a range of from about 30% to about 50 %.
11. The electrochemical storage device of any one of claims 1-10, wherein a porosity of the electrode is in a range of from about 35% to about 40 %.
12. The electrochemical storage device of any one of claims 1-11, wherein a capacity of the electrode is in a range of from about 7 mAh / cm2to about 100 mAh / cm2.
13. The electrochemical storage device of any one of claims 1-12, wherein a capacity of the electrode is in a range of from about 10 mAh / cm2to about 50 mAh / cm2.
14. The electrochemical storage device of any one of claims 1-13, wherein the electrode is an anode.
15. The electrochemical storage device of any one of claims 1-14, wherein the electrode is a cathode.
16. The electrochemical storage device of any one of claims 1-15, wherein the electrode comprises one dopant.
17. The electrochemical storage device of claim 16, wherein the electrode comprises at least two dopants.
18. The electrochemical storage device of any one of claims 16 or 17, wherein the at least one dopant or two dopants has a 1+, 2+, or 3+oxidation state.
19. The electrochemical storage device of any one of claims 1-18, wherein the at least one dopant or two dopants comprises copper, aluminum, sulfur, potassium, or a mixture thereof.
20. The electrochemical storage device of any one of claims 1-19, wherein the electrode is a battery anode.
21. The electrochemical storage device of any one of claims 1-20, wherein the electrode is a battery cathode.
22. The electrochemical storage device of any one of claims 1-21, wherein the electrode is free of a binder, an inactive solid additive, or a mixture thereof.
23. The electrochemical storage device of any one of claims 1-22, wherein the LiCoCh (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA) independently range from about 5 wt% to about 95 wt% within a blend LiCoO? (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA).
24. The electrochemical storage device of claim 23, wherein the LiCoO2 (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA) independently range from about 20 wt% to about 70 wt% of a blend LiCoO2 (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA).
25. The electrochemical storage device of claim 24, wherein the LiCoO2 (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA) independently range from about 40 wt% to about 60 wt% of a blend LiCoO2 (LCO) and LiNi0.80Co0.15Al0.05O2 (NCA).
26. A battery comprising: a first electrode corresponding to the electrode of any one of claims 1-25; a second electrode spaced apart from the first electrode; and a separator positioned between the first electrode and the second electrode.
27. The battery of claim 26, wherein the separator comprises a glass fiber or porous polymer.
28. The battery of any one of claims 26 or 27, wherein the battery is a 2032-type cell or other small form factor geometry.
29. An article comprising the electrochemical storage device of any one of claims 1-28.
30. A method of making the electrode of any one of claims 1-29, the method comprising: contacting components of an electroactive material; blending the components of the electroactive material; and sintering the blended electroactive material to form the sintered electrode.
31. The method of claim 30, wherein the sintering is performed at a temperature in range of from about 500 °C to about 1100 °C.
32. The method of any one of claims 30 or 31, wherein the sintering is performed at a temperature in range of from about 700 °C to about 900 °C.
33. The method of any one of claims 30-32, wherein sintering is performed at a variable temperature.
34. The method of any one of claims 30-33, wherein sintering is performed over a period of time in a range of from about 0.5 hours to about 20 hours.
35. The method of any one of claims 30-34, wherein sintering is performed over a period of time in a range of from about 16 hours to about 18 hours.
36. The electrochemical storage device of any of claims 1-25, wherein the blend comprises LiCoO2 (LCO) and LiNi0.80Co0.15A10.0502 (NCA) in a weight ratio ranging from about 40 wt% to about 60 wt% LCO and from about 60 wt% to about 40 wt% NCA, providing a balance between electronic conductivity and energy density.
37. The electrochemical storage device of claim 36, wherein the electrode has a porosity in a range of from about 35% to about 40%, which is optimized to facilitate ion transport while maintaining mechanical integrity during charge-discharge cycles.
38. The electrochemical storage device of any of claims 1-25, wherein the LiCoO2 (LCO) is synthesized using a sol-gel method that ensures a high degree of purity and phase homogeneity, contributing to a stability and performance of the electrode.
39. The electrochemical storage device of any of claims 1-25, wherein the LiNi0.80Co0.15A10.0502 (NCA) is synthesized through a high-temperature lithiation process that promotes formation of a well-defined crystal structure, enhancing an electrochemical capacity of the electrode.
40. The electrochemical storage device of any of claims 1-25, wherein the electrode is characterized by a microstructure that is formed by a blend of electroactive materials processed via hydraulic compression and mild sintering, resulting in an electrode architecture that is free of polymer binders and conductive additives, thereby increasing an active material content and energy density of the electrode.
Citation Information
Patent Citations
Non-aqueous electrolyte secondary cell
EP0709906A1
Composite cathode active material, cathode and lithium battery including the composite cathode active material, and preparation method thereof
US20140205898A1