Bionic vision restoration material and preparation method therefor, restoration membrane and preparation method therefor, and restoration device

Through the composite of ferroelectric gel or pressure ion gel and photoresponsive material, a soft bionic visual repair material is formed, which solves the difficulties in fitting existing visual prosthesis and equipment complexity problems, and realizes effective stimulation and vision of optic nerve cells recover.

WO2024227312A1PCT designated stage expired Publication Date: 2024-11-07SHENZHEN INST OF ADVANCED TECH
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/100880
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-04
Filing Date
2023-06-16
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing visual prostheses are difficult to fit the eyeballs during surgery, and the equipment is complex and costly. Signal crosstalk and thermal production problems exist, which affects the visual recovery effect.

Method used

Ferroelectric gel or pressure ion gel is used to combine with light-responsive material to form a soft bionic visual repair material, which can generate electrical signals under light or ultrasound, stimulate optic nerve cells, and have the characteristics of adaptively fitting the eyeball.

Benefits of technology

It realizes effective stimulation of optic nerve cells, improves visual recovery effect, reduces surgical difficulty and equipment complexity, and is relatively low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention relates to the technical field of biological materials. Specifically disclosed are a bionic vison restoration material and a preparation method therefor, a restoration membrane and a preparation method therefor, and a restoration device. The bionic vision restoration material comprises a gel material; the gel material is a ferroelectric gel or a piezoelectric gel; the ferroelectric gel is selected from a polyacrylonitrile and / or polyacrylonitrile composite gel; the Young's modulus of the gel material is 10 Pa to 300 MPa; and an electric signal having a current density of 1 pA mm-2 to 100 mA mm-2 and a voltage of 10 mV to 100 V can be generated under illumination of 200 nm to 2500 nm or ultrasonic waves having power of 1 W to 1000 W. The bionic vison restoration material of the present invention is soft, and can be adaptively attached to eyeballs or visual cortex; and under illumination or ultrasonic waves, an electric signal can be generated to stimulate visual nerve cells for vision restoration.
Need to check novelty before this filing date? Find Prior Art

Description

Bionic visual repair material, repair film, preparation method thereof, and repair device Technical Field

[0001] The present invention belongs to the technical field of biomaterials, and in particular relates to a bionic visual restoration material, a restoration film, a preparation method thereof, and a restoration device. Background Art

[0002] Vision is one of the most important ways humans acquire information. Retinal degenerative diseases, such as retinitis pigmentosa and macular degeneration, are the leading causes of blindness in adults, and to date, there are no effective clinical treatments for these diseases. Studies have found that even in blind individuals with retinal degeneration or photoreceptor cell disease, a significant number of neurons in the visual pathway remain functional. Therefore, an artificial retina could be implanted to stimulate these neurons and restore some visual ability.

[0003] Currently, some implantable electronic devices serve as visual prostheses. After processing external image information through a microprocessor, they use microelectrode arrays implanted in the body to apply pulsed current stimulation to neurons in the intact visual nerve pathway, thereby restoring the patient's vision to a certain extent. This type of visual prosthesis has been clinically proven to be effective and has brought good news to blind patients. However, this type of visual prosthesis usually requires an external power supply unit and wireless transmission control, which greatly complicates the implantation surgery. At the same time, the electrode density of the microelectrode array is low, which to some extent affects the spatial resolution of vision. Moreover, the equipment is complex and has problems such as signal crosstalk, excessive heat generation, and packaging difficulties.

[0004] In recent years, passive visual prostheses based on the photoelectric effect have been developed. These prostheses, which eliminate the need for complex structures, directly convert light signals into electrical signals to stimulate retinal ganglion cells, retinal photoreceptors, or the visual cortex. This significantly reduces surgical complexity and offers advantages such as simple structure and low cost, making them considered an ideal solution for artificial retinas. However, current visual prosthetic materials are too hard to adhere to the eyeball, creating close contact and stimulation of the optic nerve, limiting their practical use.

[0005] Summary of the Invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a bionic visual repair material, a repair film, a preparation method thereof, and a repair device, wherein: the bionic visual repair material contains ferroelectric gel or piezoelectric gel or is a composite of a gel material (ferroelectric gel or piezoelectric gel) and a photoresponsive material, and the material has soft properties and can adaptively fit the eyeball or visual cortex. At the same time, the bionic visual repair material of the present invention can generate electricity under light or ultrasound, either by the gel material itself or by the photoelectric effect of the photoresponsive material distributed in the gel material, which can stimulate visual nerve cells and repair vision.

[0007] In order to solve the above technical problems, the first aspect of the present invention provides a bionic visual restoration material, which includes a gel material, wherein the gel material is a ferroelectric gel or a piezoelectric gel, and the ferroelectric gel is selected from polyacrylonitrile and / or polyacrylonitrile composite gel, and the ferroelectric gel has a Young's modulus of 10Pa-300MPa, and can generate a current density of 1pA mm under 200nm-2500nm light or 1W-1000W ultrasonic wave. -2 -100mA mm -2 , an electrical signal with a voltage of 10mV-100V.

[0008] Specifically, the biomimetic visual restoration material of the present invention contains specific ferroelectric gels or piezoelectric ion gels, which impart softness to the material. Due to their low Young's modulus, they conform well to the eyeball or visual cortex. Furthermore, the gel material generates electricity due to the photoelectric effect under light or ultrasound, stimulating retinal ganglion cells, retinal photoreceptors, or the visual cortex to restore vision. Ferroelectric gels, due to their inherent photoelectric effect, can be used independently as biomimetic visual restoration materials under light or ultrasound. Piezoelectric ion gels, on the other hand, generate electric charge due to the directional movement of ions within the gel when subjected to force. Therefore, ultrasound induces stress, generating electricity.

[0009] As a further improvement of the above solution, the bionic visual restoration material further includes a light-responsive material, and the light-responsive material is distributed in the ferroelectric gel.

[0010] Specifically, ferroelectric gels have piezoelectric and pyroelectric properties, generating electricity when heated due to pyroelectricity, and when subjected to force due to piezoelectricity. Therefore, under conditions of light or ultrasound, the photothermal material and photodeformable material distributed within the ferroelectric gel can generate heat or force, thereby generating electricity within the ferroelectric gel. Piezoelectric gels, on the other hand, can generate electricity under ultrasound or with the aid of photoresponsive materials.

[0011] As a further improvement of the above solution, the mass ratio of the gel material to the light-responsive material is (1-100):1.

[0012] As a further improvement of the above solution, the light-responsive material is selected from at least one of ferroelectric materials, semiconductor materials, photothermal materials, and photodeformable materials.

[0013] Specifically, the photothermal material and photodeformable material distributed in the ferroelectric gel will generate heat and force under light, thereby generating electricity in the ferroelectric gel; while the photothermal material distributed in the piezoelectric gel will expand when heated, bringing stress to the gel material, and the photodeformable material will deform under light, bringing stress to the gel material, thereby generating electricity.

[0014] Preferably, the ferroelectric material is selected from polyvinylidene fluoride and its copolymers, nylon with an odd number of carbon atoms, polyacrylonitrile, polyimide, polyvinylidene dicyandiamide and its copolymers, polyurea, polyphenylene cyanoether, polyvinyl chloride, polyvinyl acetate, polypropylene, polytetrafluoroethylene, ferroelectric liquid crystal, lead titanate, barium titanate, potassium niobate, lithium niobate, lithium tantalate, bismuth titanate, bismuth layered perovskite structure ferroelectric, tungsten bronze type ferroelectric, bismuth ferrite, potassium dihydrogen phosphate, triammonium sulfate, Roche salt, perovskite type organic metal halide ferroelectric, strontium ruthenate and at least one of the composites or doped compounds of the above materials.

[0015] Preferably, the semiconductor material is selected from at least one of silicon, cadmium, cadmium sulfide, gallium arsenide and composites thereof.

[0016] Preferably, the photothermal material is selected from at least one of carbon black, carbon nanotubes, graphene, black phosphorus, polydopamine, gold nanoparticles, gold nanorods, gallium-indium alloy liquid metal, black titanium dioxide, supramolecular metal-organic framework (MOF) materials, molybdenum disulfide, transition metal carbide nitride, carbonitride two-dimensional materials, small molecule photothermal agents and composite materials based on the above materials.

[0017] Preferably, the small molecule photothermal agent is selected from fluorine-boron complexes.

[0018] Preferably, the photodeformable material is at least one selected from azobenzene and its composites.

[0019] As a further improvement of the above solution, the ionotropic gel is selected from at least one of a polymer containing anionic monomers, a polymer containing cationic monomers, a polymer containing both anionic and cationic monomers, a polymer containing no ionic monomers but containing small molecule electrolytes, and an ionic natural polymer.

[0020] Preferably, the anionic monomer is selected from at least one of a carboxylate monomer, a sulfonate monomer, and a phosphate monomer.

[0021] Preferably, the carboxylate monomer is selected from acrylic acid and / or acrylic acid salts.

[0022] Preferably, the sulfonate monomer is selected from p-styrene sulfonate and / or 2-acrylamide-2-methylpropane sulfonate.

[0023] Preferably, the phosphate monomer is selected from phosphorylated monomers.

[0024] Preferably, the cationic monomer is selected from quaternary ammonium salt monomers and / or amino monomers.

[0025] Preferably, the quaternary ammonium salt monomer is selected from 3-chloroallylhexamethylenetetramine chloride and / or allyltrimethylammonium chloride.

[0026] Preferably, the amino type monomer is selected from vinylamine.

[0027] Preferably, the anionic and cationic monomers include both the above-mentioned anionic monomers and cationic monomers.

[0028] Preferably, the small molecule electrolyte is selected from at least one of alkali metal salts, ionic liquids, acids, and bases.

[0029] Preferably, the alkali metal salt is at least one selected from lithium fluoride, sodium fluoride, potassium fluoride, lithium chloride, sodium chloride, potassium chloride, lithium bromide, sodium bromide, and potassium bromide.

[0030] Preferably, the ionic liquid is selected from [EMI + ][TFSI - ].

[0031] Preferably, the acid is selected from at least one of phosphoric acid, formic acid, acetic acid and phytic acid.

[0032] Preferably, the base is selected from at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide.

[0033] Preferably, the ionic natural polymer is at least one selected from sodium alginate, chitosan, hyaluronic acid, carrageenan, agar, gelatin, silk fibroin, and modified cellulose.

[0034] The second aspect of the present invention provides a method for preparing a bionic visual restoration material, wherein the method is used to prepare the bionic visual restoration material according to the first aspect of the present invention, comprising the following steps:

[0035] The photoresponsive material is dispersed in a polar solvent, and then the gel material is added and mixed to obtain the bionic vision repair material.

[0036] Preferably, the polar solvent is selected from at least one of dimethyl sulfoxide (DMSO), deionized water, and tetrahydrofuran.

[0037] The third aspect of the present invention provides a bionic visual restoration film, characterized in that the bionic visual restoration film is made of the bionic visual restoration material described in the first aspect of the present invention.

[0038] As a further improvement of the above solution, the surface of the bionic visual repair film has a microstructure or a mesh structure.

[0039] Specifically, the microstructure is a surface layer with a micro-nanoscale lattice structure. Compared with a planar structure, a microstructure or a reticular structure is beneficial for improving the contact effect between the membrane layer and the retinal ganglion cells or retinal photoreceptor cells, thereby improving the photoelectric response efficiency of the cells.

[0040] A fourth aspect of the present invention provides a method for preparing a biomimetic visual repair film, wherein the method is used to prepare the biomimetic visual repair film according to the third aspect of the present invention, and comprises the following steps:

[0041] The bionic vision repair material described in the first aspect of the present invention is poured into a mold to form a film, and then dried to obtain the bionic vision repair film.

[0042] Preferably, the drying is performed at 50-80° C. for 4-8 hours.

[0043] The fifth aspect of the present invention provides a bionic vision restoration device, which includes the bionic vision restoration film described in the third aspect of the present invention.

[0044] Preferably, the bionic vision repair device can be implanted on the retina, under the retina or in the visual cortex, and utilize the photoelectric effect to stimulate the retinal ganglion cells, retinal photoreceptor cells or visual cortex to show excitability, thereby repairing vision.

[0045] Compared with the prior art, the above technical solution of the present invention has at least the following technical effects or advantages:

[0046] The bionic visual restoration material of the present invention includes ferroelectric gel or piezoelectric ion gel, or is composed of a gel material (ferroelectric gel or piezoelectric ion gel) and a light-responsive material. The bionic visual restoration material has soft properties, a Young's modulus of 10Pa-300MPa, and can adaptively fit the eyeball or visual cortex; and under 200nm-2500nm light or 1W-1000W ultrasonic power, it can generate a current density of 1pA mm -2 -100mA mm -2, an electrical signal with a voltage of 10mV-100V can stimulate the retinal ganglion cells, retinal photoreceptor cells or visual cortex, showing excitability to repair vision. DETAILED DESCRIPTION

[0047] The present invention is described in detail below with reference to the examples to facilitate understanding of the present invention by those skilled in the art. It is necessary to point out that the examples are only used to further illustrate the present invention and are not to be construed as limiting the scope of protection of the present invention. Non-essential improvements and adjustments made to the present invention by those skilled in the art based on the above-mentioned invention should still fall within the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods that are not mentioned in detail are all process steps or preparation methods known to those skilled in the art.

[0048] Example 1

[0049] A bionic visual restoration material composed of a composite of ferroelectric gel polyacrylonitrile and barium titanate.

[0050] A method for preparing a bionic visual restoration material comprises the following steps:

[0051] Barium titanate powder was ultrasonically dispersed in dimethyl sulfoxide, followed by the addition of acrylonitrile monomer, sodium p-styrene sulfonate, and N,N'-methylenebisacrylamide, vortexed to dissolve. Ammonium persulfate powder, an initiator, was then added under a nitrogen atmosphere and mixed uniformly to obtain the biomimetic visual restoration material of this embodiment (a mixture of acrylonitrile copolymer prepolymer and barium titanate). The mass ratio of acrylonitrile, sodium p-styrene sulfonate, N,N'-methylenebisacrylamide, and ammonium persulfate was 40:10:3:4, the mass-to-volume ratio (v / w) of the acrylonitrile solution was 1 g / 6 mL, and the mass ratio of barium titanate to polyacrylonitrile was 10:100.

[0052] A method for preparing a bionic visual repair film comprises the following steps:

[0053] The obtained acrylonitrile copolymer prepolymer liquid and barium titanate mixture was poured into a mold to form a film, and then placed in a 60°C oven for reaction for 4 hours to obtain the biomimetic visual repair film (polyacrylonitrile barium titanate composite film) of this embodiment, which has a Young's modulus of 10 MPa and a power of 100 mW mm -2 Under the 400nm wavelength light, the output voltage can be greater than 1V and the output current can be greater than 1pA mm -2 , which can stimulate the retinal ganglion cells to show excitability.

[0054] Example 2

[0055] A bionic visual restoration material composed of ferroelectric gel polyacrylonitrile and polydopamine.

[0056] A method for preparing a bionic visual restoration material comprises the following steps:

[0057] Polydopamine powder was ultrasonically dispersed in dimethyl sulfoxide, and then a certain amount of acrylonitrile monomer, sodium p-styrene sulfonate, and N,N'-methylenebisacrylamide were added and vortexed to dissolve. Then, initiator ammonium persulfate powder was added under a nitrogen atmosphere and mixed evenly to obtain the biomimetic visual restoration material of this embodiment (acrylonitrile copolymer prepolymer and polydopamine mixture), wherein the mass ratio of acrylonitrile, sodium p-styrene sulfonate, N,N'-methylenebisacrylamide, and ammonium persulfate was 40:10:3:4, the mass volume ratio (v / w) of the acrylonitrile solution was 1 g / 6 mL, and the mass ratio of polydopamine to acrylonitrile copolymer was 100:100.

[0058] A method for preparing a bionic visual repair film comprises the following steps:

[0059] The prepared acrylonitrile copolymer prepolymer solution and polydopamine mixture were poured into a mold to form a film, and then placed in a 60°C oven for reaction for 4 hours to obtain the biomimetic visual repair film (polyacrylonitrile polydopamine composite film) of this embodiment, which had a Young's modulus of 5 MPa and a power of 1 mW mm -2 The output voltage can be greater than 2V and the output current can be greater than 10mA under the 2500nm wavelength light. -2 , which can stimulate retinal photoreceptor cells to show excitability.

[0060] Example 3

[0061] A bionic visual restoration material composed of ferroelectric gel polyacrylonitrile and azobenzene.

[0062] A method for preparing a bionic visual restoration material comprises the following steps:

[0063] Azobenzene was ultrasonically dispersed in dimethyl sulfoxide, followed by the addition of a certain amount of acrylonitrile monomer, sodium p-styrene sulfonate, and N,N'-methylenebisacrylamide, vortexed to dissolve. Ammonium persulfate powder, an initiator, was then added under a nitrogen atmosphere and mixed thoroughly to obtain the biomimetic visual restoration material (acrylonitrile copolymer prepolymer and azobenzene mixture) of this embodiment. The mass ratio of acrylonitrile, sodium p-styrene sulfonate, N,N'-methylenebisacrylamide, and ammonium persulfate was 40:10:3:4, the mass-to-volume ratio (v / w) of the acrylonitrile solution was 1 g / 6 mL, and the mass ratio of azobenzene to acrylonitrile copolymer was 50:100.

[0064] A method for preparing a bionic visual repair film comprises the following steps:

[0065] The prepared acrylonitrile copolymer prepolymer liquid and azobenzene mixture was poured into a mold to form a film, and then placed in a 60°C oven for reaction for 4 hours to obtain the biomimetic visual repair film (polyacrylonitrile azobenzene composite film) of this embodiment, which had a Young's modulus of 1 MPa and a power of 100 mW mm -2 The output voltage can be greater than 1V and the output current can be greater than 1mA under 405nm wavelength light. -2 , which can stimulate the visual cortex cells to show excitability.

[0066] Example 4

[0067] A bionic visual restoration material is composed of a composite of piezoelectric ion gel polyacrylic acid and polycrystalline silicon.

[0068] A method for preparing a bionic visual restoration material comprises the following steps:

[0069] Polycrystalline silicon powder was ultrasonically dispersed in deionized water, and then 30 wt% of acrylic acid monomer was added and stirred to dissolve. N,N'-methylenebisacrylamide (a crosslinking agent) and ammonium persulfate (an initiator) were then added and stirred until completely dissolved, yielding the biomimetic visual restoration material (a mixture of polyacrylic acid and polycrystalline silicon) of this embodiment. The weight ratio of acrylic acid monomer to polycrystalline silicon was 100:10, and the weight of the initiator and crosslinker was 0.6% and 0.8% of the acrylic acid monomer, respectively.

[0070] A method for preparing a bionic visual repair film comprises the following steps:

[0071] The mixture of polyacrylic acid and polycrystalline silicon was poured into a mold and reacted in an oven at 80°C under a nitrogen atmosphere for 4 hours to obtain the biomimetic visual repair film (polyacrylic acid polycrystalline silicon composite film) of this embodiment, which had a Young's modulus of 1 kPa and a power of 100 mW mm -2 The output voltage can be greater than 100mV and the output current can be greater than 1mA under 1100nm wavelength light. -2 , which can stimulate retinal photoreceptor cells to show excitability.

[0072] Example 5

[0073] A bionic visual restoration material is composed of a composite of piezoelectric ion gel polyvinylamine and graphene.

[0074] A method for preparing a bionic visual restoration material comprises the following steps:

[0075] Graphene was ultrasonically dispersed in deionized water, and then 15 wt% polyvinylamine was added and stirred to dissolve, thereby obtaining the biomimetic visual restoration material (polyvinylamine and graphene mixture) of this embodiment, wherein the weight ratio of polyvinylamine to graphene was 100:1.

[0076] A method for preparing a bionic visual repair film comprises the following steps:

[0077] The mixture of polyvinylamine and graphene was poured into a mold and dried in an oven at 80°C under a nitrogen atmosphere for 4 hours to obtain the biomimetic visual repair film (polyvinylamine graphene composite film) of this embodiment, which had a Young's modulus of 100 Pa and a power of 100 mW mm -2 The output voltage can be greater than 1V and the output current can be greater than 10μA mm under 808nm wavelength light. -2 , which can stimulate the retinal ganglion cells to show excitability.

[0078] Example 6

[0079] A bionic visual restoration material is composed of a composite of ionotropic ethyleneamine-acrylic acid copolymer and azobenzene.

[0080] A method for preparing a bionic visual restoration material comprises the following steps:

[0081] Azobenzene was ultrasonically dispersed in tetrahydrofuran, and then N-vinylformamide and acrylic acid were added and stirred to dissolve. A 1.1% mol (relative to the molar amounts of N-vinylformamide and acrylic acid) solution of azobisisobutyronitrile in tetrahydrofuran was added dropwise to the mixture to obtain the biomimetic visual restoration material of this embodiment (a mixture of vinylamine-acrylic acid prepolymer and azobenzene). The molar ratio of N-vinylformamide to acrylic acid was 3:1, and the molar concentration of N-vinylformamide was 1M.

[0082] A method for preparing a bionic visual repair film comprises the following steps:

[0083] The mixture of vinylamine-acrylic acid prepolymer and azobenzene was poured into a mold and reacted in an oven at 70°C under a nitrogen atmosphere for 5 hours to obtain the biomimetic visual repair film (polyvinylamine-acrylic acid azobenzene composite film) of this embodiment, which had a Young's modulus of 100 Pa and a power of 100 mW mm -2 The output voltage is greater than 1V and the output current is greater than 10μA mm under 405nm wavelength light. -2 , which can stimulate retinal photoreceptor cells to show excitability.

[0084] Example 7

[0085] A bionic visual restoration material is composed of a composite of poly (sodium p-styrene sulfonate) swollen by a pressure ion gel sodium chloride solution and carbon nanotubes.

[0086] A method for preparing a bionic visual restoration material comprises the following steps:

[0087] The carbon nanotubes were ultrasonically dispersed in deionized water, and then 30 wt% of sodium p-styrene sulfonate monomer was added and stirred to dissolve. The crosslinker, N,N'-methylenebisacrylamide, and the initiator, ammonium persulfate, were added and stirred until completely dissolved, yielding the biomimetic visual restoration material (a mixture of sodium p-styrene sulfonate and carbon nanotubes) of this embodiment. The weight ratio of sodium p-styrene sulfonate monomer to carbon nanotubes was 100:10, and the weight of the initiator and crosslinker was 0.4% and 0.2% of the acrylic acid monomer, respectively.

[0088] A method for preparing a bionic visual repair film comprises the following steps:

[0089] The mixture of sodium polystyrene sulfonate and carbon nanotubes was poured into a mold and reacted in a 50°C oven under a nitrogen atmosphere for 8 hours to obtain the biomimetic visual repair film (sodium polystyrene sulfonate carbon nanotube composite film) of this embodiment. The composite film was immersed in a 0.1M sodium chloride solution for 24 hours, and its Young's modulus was 10Pa. At a power of 100mW mm -2 The output voltage is greater than 1V and the output current is greater than 100μA mm under 808nm wavelength light. -2 , which can stimulate retinal photoreceptor cells to show excitability.

[0090] Example 8

[0091] A bionic visual restoration material composed of a composite of pressure ion gel sodium alginate and azobenzene.

[0092] A method for preparing a bionic visual restoration material comprises the following steps:

[0093] Azobenzene was ultrasonically dispersed in deionized water, and then 2 wt% sodium alginate was added and stirred to dissolve to obtain the biomimetic visual restoration material (a mixture of sodium alginate and azobenzene) of this embodiment, wherein the weight ratio of sodium alginate to azobenzene was 100:10.

[0094] A method for preparing a bionic visual repair film comprises the following steps:

[0095] The mixture of sodium alginate and azobenzene was poured into a mold, immersed in a 1M calcium chloride solution for cross-linking for 2 hours, and then taken out to obtain the biomimetic visual repair film (sodium alginate azobenzene composite film) of this embodiment, which has a Young's modulus of 10Pa and a power of 100mW mm -2 The output voltage can be greater than 1V and the output current can be greater than 1μA mm under 405nm wavelength light. -2 , which can stimulate retinal photoreceptor cells to show excitability.

[0096] Example 9

[0097] A bionic visual restoration material composed of ferroelectric gel polyacrylonitrile.

[0098] A method for preparing a bionic visual restoration material comprises the following steps:

[0099] Acrylonitrile monomer, sodium p-styrene sulfonate, and N,N'-methylenebisacrylamide were vortexed to dissolve, and then ammonium persulfate powder as an initiator was added under a nitrogen atmosphere and mixed thoroughly to obtain the biomimetic visual restoration material (acrylonitrile copolymer prepolymer) of this embodiment. The mass ratio of acrylonitrile, sodium p-styrene sulfonate, N,N'-methylenebisacrylamide, and ammonium persulfate was 40:10:3:4, and the mass-to-volume ratio (v / w) of the acrylonitrile solution was 1 g / 6 mL.

[0100] A method for preparing a bionic visual repair film comprises the following steps:

[0101] The prepared acrylonitrile copolymer prepolymer was poured into a mold to form a film, and then placed in a 60°C oven for reaction for 4 hours to obtain the biomimetic visual repair film (polyacrylonitrile film) of this embodiment, which had a Young's modulus of 10 MPa and could generate an output voltage greater than 1 V and an output current greater than 10 mA mm under an ultrasonic wave with a power of 1 W. -2 , which can stimulate the retinal ganglion cells to show excitability.

[0102] Example 10

[0103] A bionic visual restoration material composed of a composite of ferroelectric gel polyacrylonitrile and barium titanate.

[0104] A method for preparing a bionic visual restoration material comprises the following steps:

[0105] Barium titanate powder was ultrasonically dispersed in dimethyl sulfoxide, followed by the addition of acrylonitrile monomer, sodium p-styrene sulfonate, and N,N'-methylenebisacrylamide, vortexed to dissolve. Ammonium persulfate powder, an initiator, was then added under a nitrogen atmosphere and mixed uniformly to obtain the biomimetic visual restoration material of this embodiment (a mixture of acrylonitrile copolymer prepolymer and barium titanate). The mass ratio of acrylonitrile, sodium p-styrene sulfonate, N,N'-methylenebisacrylamide, and ammonium persulfate was 40:10:3:4, the mass-to-volume ratio (v / w) of the acrylonitrile solution was 1 g / 6 mL, and the mass ratio of barium titanate to polyacrylonitrile was 10:100.

[0106] A method for preparing a bionic visual repair film comprises the following steps:

[0107] The obtained acrylonitrile copolymer prepolymer liquid and barium titanate mixture was poured into a mold to form a film, and then placed in a 60°C oven for reaction for 4 hours to obtain the biomimetic visual repair film (polyacrylonitrile barium titanate composite film) of this embodiment, which has a Young's modulus of 10 MPa and can generate an output voltage greater than 100 V and an output current greater than 100 mA mm under an ultrasonic power of 1000 W. -2 , which can stimulate the retinal ganglion cells to show excitability.

[0108] Example 11

[0109] The invention discloses a bionic visual restoration material composed of pressure ion gel sodium alginate.

[0110] A method for preparing a bionic visual restoration material comprises the following steps:

[0111] 2 wt % sodium alginate was stirred and dissolved to obtain the biomimetic visual restoration material (sodium alginate solution) of this embodiment.

[0112] A method for preparing a bionic visual repair film comprises the following steps:

[0113] The sodium alginate solution was poured into the mold, immersed in a 1M calcium chloride solution for cross-linking for 2 hours, and then taken out to obtain the biomimetic visual repair film (sodium alginate film) of this embodiment. Its Young's modulus was 10Pa, and the output voltage generated under an ultrasonic power of 10W was greater than 1V and the output current was greater than 1μA mm -2 , which can stimulate the retinal ganglion cells to show excitability.

[0114] Example 12

[0115] A bionic visual restoration material composed of a composite of pressure ion gel sodium alginate and azobenzene.

[0116] A method for preparing a bionic visual restoration material comprises the following steps:

[0117] Azobenzene was ultrasonically dispersed in deionized water, and then 2 wt% sodium alginate was added and stirred to dissolve, thereby obtaining the biomimetic visual restoration material (a mixture of sodium alginate and azobenzene) of this embodiment, wherein the weight ratio of sodium alginate to azobenzene was 100:10.

[0118] A method for preparing a bionic visual repair film comprises the following steps:

[0119] The mixture of sodium alginate and azobenzene was poured into a mold, immersed in a 1M calcium chloride solution for cross-linking for 2 hours, and then taken out to obtain the biomimetic visual repair film (sodium alginate azobenzene composite film) of this embodiment. Its Young's modulus was 10 Pa, and the output voltage generated under an ultrasonic power of 10 W was greater than 1 V and the output current was greater than 1 μA mm-2 , which can stimulate the retinal ganglion cells to show excitability.

[0120] Comparative Example 1

[0121] A bionic visual restoration material is prepared by compounding polyvinylidene fluoride-trifluoroethylene (P(VDF-TrFE)) and azobenzene.

[0122] A method for preparing a bionic visual restoration material comprises the following steps:

[0123] Azobenzene was ultrasonically dispersed in dimethyl sulfoxide, and then P(VDF-TrFE) was added and stirred for 12 hours to fully dissolve it, thereby obtaining the biomimetic visual restoration material (a mixture of P(VDF-TrFE) and azobenzene) of this comparative example. The mass-to-volume ratio (v / w) of the P(VDF-TrFE) solution was 100 mg / mL, and the mass ratio of azobenzene to P(VDF-TrFE) was 10:100.

[0124] A method for preparing a bionic visual repair film comprises the following steps:

[0125] The mixture of P(VDF-TrFE) and azobenzene was cast into a film on a silicon wafer, dried in an oven at 80°C for 12 hours, and then dried in a vacuum drying oven at 130°C for 6 hours. After corona poling, the Young's modulus was 1 GPa. -2 Under the 405nm wavelength light, the output voltage can be greater than 60V and the output current can be greater than 100nA mm -2 , but it cannot bend to fit the eyeball, so it cannot stimulate the retinal photoreceptor cells in the body to show excitability.

[0126] For those skilled in the art to which the present invention belongs, a number of simple deductions or substitutions can be made without departing from the concept of the present invention, without having to resort to creative work. Therefore, based on the disclosure of the present invention, simple improvements made by those skilled in the art to the present invention should be within the scope of protection of the present invention. The above embodiments are preferred embodiments of the present invention, and all processes similar to the present invention and equivalent changes made should fall within the scope of protection of the present invention.

Claims

1. A bionic visual restoration material, characterized in that: The bionic visual repair material comprises a gel material, wherein the gel material is a ferroelectric gel or a piezoelectric gel, and the ferroelectric gel is selected from polyacrylonitrile and / or polyacrylonitrile composite gel; the Young's modulus of the gel material is 10Pa-300MPa, and under 200nm-2500nm light or 1W-1000W ultrasound, a current density of 1pA mm -2 -100mA mm -2 , an electrical signal with a voltage of 10mV-100V.

2. The bionic visual restoration material according to claim 1, characterized in that: The bionic vision repair material also includes a light-responsive material, and the light-responsive material is distributed in the gel material.

3. The bionic visual restoration material according to claim 2, characterized in that: The mass ratio of the gel material to the light-responsive material is (1-100):

1.

4. The bionic visual restoration material according to claim 1, characterized in that: The ionotropic gel is selected from at least one of a polymer containing anionic monomers, a polymer containing cationic monomers, a polymer containing both anionic and cationic monomers, a polymer containing no ionic monomers but containing small molecule electrolytes, and an ionic natural polymer.

5. The bionic visual restoration material according to claim 4, characterized in that: The anionic monomer is selected from at least one of a carboxylate monomer, a sulfonate monomer, and a phosphate monomer; The cationic monomer is selected from quaternary ammonium salt monomers and / or amino monomers; The anionic and cationic monomers include both the anionic monomers and the cationic monomers; The small molecule electrolyte is selected from at least one of an alkali metal salt, an ionic liquid, an acid, and a base; The ionic natural polymer is selected from at least one of sodium alginate, chitosan, hyaluronic acid, carrageenan, agar, gelatin, silk fibroin, and modified cellulose.

6. The bionic visual restoration material according to claim 1, characterized in that: The light-responsive material is selected from at least one of ferroelectric materials, semiconductor materials, photothermal materials, and photodeformable materials.

7. The bionic visual restoration material according to claim 6, characterized in that: The ferroelectric material is selected from at least one of polyvinylidene fluoride and its copolymers, nylon with an odd number of carbon atoms, polyacrylonitrile, polyimide, polyvinylidene dicyandiamide and its copolymers, polyurea, polyphenylene cyanoether, polyvinyl chloride, polyvinyl acetate, polypropylene, polytetrafluoroethylene, ferroelectric liquid crystal, lead titanate, barium titanate, potassium niobate, lithium niobate, lithium tantalate, bismuth titanate, bismuth layered perovskite structure ferroelectric, tungsten bronze type ferroelectric, bismuth ferrite, potassium dihydrogen phosphate, triammonium sulfate, Roche salt, perovskite type organic metal halide ferroelectric, strontium ruthenate and composites or doped compounds of the above materials; The semiconductor material is selected from at least one of silicon, cadmium, cadmium sulfide, gallium arsenide and a composite thereof; The photothermal material is selected from carbon black, carbon nanotubes, graphene, black phosphorus, polydopamine, gold nanoparticles, gold nanorods, At least one of gallium-indium alloy liquid metal, black titanium dioxide, supramolecular metal organic framework materials, molybdenum disulfide, transition metal carbide nitrides, carbonitride two-dimensional materials, small molecule photothermal agents, and composite materials based on the above materials; The photodeformable material is selected from at least one of azobenzene and a composite thereof.

8. A method for preparing a bionic visual restoration material, characterized in that: The preparation method is used to prepare the bionic visual restoration material according to any one of claims 1 to 7, comprising the following steps: The photoresponsive material is dispersed in a polar solvent, and then a gel material is added and mixed to obtain the bionic visual repair material.

9. The method for preparing the bionic visual restoration material according to claim 8, characterized in that: The polar solvent is selected from at least one of dimethyl sulfoxide, deionized water and tetrahydrofuran.

10. A bionic visual repair film, characterized in that: The bionic vision repair film is made from the bionic vision repair material according to any one of claims 1 to 7.

11. The bionic visual repair film according to claim 10, characterized in that: The surface of the bionic visual repair film has a microstructure or a mesh structure.

12. A method for preparing a bionic visual repair film, characterized in that: The preparation method is used to prepare the bionic visual repair film according to claim 10 or 11, comprising the following steps: The bionic vision repair material according to any one of claims 1 to 7 is poured into a mold to form a film, and then dried to obtain the bionic vision repair film.

13. The method for preparing the bionic visual repair film according to claim 12, characterized in that: The drying is carried out at 50-80° C. for 4-8 hours.

14. A bionic visual restoration device, characterized in that: The bionic vision restoration device comprises the bionic vision restoration film according to claim 10 or 11.

15. The bionic visual prosthetic device according to claim 14, characterized in that: The bionic visual prosthesis device can be implanted on the retina, under the retina or in the visual cortex.

Citation Information

Patent Citations

  • Photo-responsive gel electrolyte and preparation method and application thereof

    CN105551808A

  • Ionic gel with temperature and light responsiveness, preparation method of ionic gel and application of ionic gel

    CN109897133A

  • Nerve tissue stimulation composite material, composite membrane and nerve tissue prosthesis

    CN111013014A

  • Flexible sensing element of polyvinyl chloride ionic gel, and preparation method thereof

    CN112629399A

  • Near-infrared super-vision flexible artificial retina and manufacturing method thereof

    CN112641534A