Separator for sodium battery, secondary battery, and electrical apparatus
By designing a gradient-changing porosity structure, the isolation film for sodium batteries solves the problem of battery cycle life attenuation caused by volume expansion in the sodium batteries, achieving effective infiltration and compression resistance of the electrolyte, and extending the service life of the battery.
Patent Information
- Application Number
- PCT/CN2024/072054
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2024-01-12
- Publication Date
- 2024-11-07
AI Technical Summary
The isolation film is compressed due to the volume expansion and deformation of the positive and negative electrode materials of sodium batteries, and the battery circulation performance is rapidly attenuated, making the existing isolation film difficult to effectively resist and recover.
Design a separator film for sodium batteries, whose porosity decreases in gradient along its own thickness direction, has a certain stiffness and compression, and can fully immerse the electrolyte before being compressed, and release it in time after being compressed, so as to alleviate the volume expansion belt The battery cycle life is attenuated.
Through the gradient-changing porosity structure, the isolation film can effectively resist the expansion and deformation of the positive and negative electrode sheets, extend the circulation life of the sodium battery, and improve the circulation performance of the battery.
Smart Images

Figure CN2024072054_07112024_PF_FP_ABST
Abstract
Description
Separator film for sodium battery, secondary battery and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 2023104909281, filed on May 4, 2023, entitled “Separator membrane for sodium battery, secondary battery and electrical device”, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of batteries, and in particular to an isolation membrane for sodium batteries, a secondary battery, and an electrical device. Background Art
[0004] As the application of lithium-ion battery technology in markets such as consumer electronics, electric vehicles, and energy storage continues to expand, the issue of lithium resource shortages has become increasingly prominent. Sodium batteries, due to their abundant sodium reserves, have gradually attracted attention and hold a strategic position in cost-sensitive applications such as energy storage. Furthermore, sodium batteries offer higher conductivity than lithium batteries at the same electrolyte concentration, further reducing production costs.
[0005] However, due to the higher reduction potential and larger relative molecular mass of metallic sodium compared to metallic lithium, the energy density of sodium batteries with similar working principles is significantly lower than that of lithium batteries. At the same time, sodium ions have a larger ionic radius than lithium ions, which also makes the volume expansion associated with their embedding and extraction in the positive and negative electrode materials larger. Some irreversible expansion can easily cause the isolation membrane to be compressed, and the battery's cycle performance rapidly decays.
[0006] Summary of the Invention
[0007] In view of the above problems, the present application provides a sodium battery separator, a secondary battery and an electrical device, which can alleviate the problem of rapid attenuation of battery cycle life due to volume expansion during the use of sodium batteries.
[0008] In a first aspect, the present application provides a separator for a sodium battery, wherein the separator has a first surface and a second surface along its thickness direction, and the porosity of the separator decreases gradually as it extends from the first surface to the second surface.
[0009] The isolation membrane containing this structure has a certain rigidity, which is conducive to its ability to resist the expansion and deformation of the positive and negative electrode plates to a certain extent. The isolation membrane also has a certain compressibility, which can achieve full and effective infiltration of the electrolyte before being compressed, and can effectively and timely release the electrolyte after being compressed, which can alleviate the problem of rapid attenuation of battery cycle life caused by volume expansion during the use of sodium batteries.
[0010] In some embodiments, the porosity of the first surface is greater than or equal to 50% and less than or equal to 70%, and the porosity of the second surface is greater than or equal to 30% and less than 50%.
[0011] In addition to ensuring that the isolation membrane has the function of conducting internal ions and isolating direct contact between the positive and negative pole pieces, it also needs to meet the gradient change of porosity along its own thickness direction. Affected by many factors such as material, preparation process and the isolation membrane's own performance, the porosity of the first surface of the isolation membrane is greater than or equal to 50% and less than or equal to 70%, and the porosity of the second surface is greater than or equal to 30% and less than 50%.
[0012] In some embodiments, the thickness H of the isolation film is 5 μm to 30 μm.
[0013] Within this thickness range, it is easier to design the porosity of the isolation membrane to change gradually along the thickness direction.
[0014] In some embodiments, the porosity of the isolation membrane is q, and the full-fill thickness rebound rate of the isolation membrane is α, which satisfies any of the following conditions: (1) 30%≤q≤40%, α≤100%; (2) 40%<q<60%, 100%<α<200%; (3) 60%≤q≤70%, α≥200%.
[0015] The separator of the present application expands after the battery is fully charged, which can inhibit the expansion of the negative electrode to a certain extent.
[0016] In some embodiments, the isolation membrane includes a base membrane, and the porosity of the base membrane decreases gradually along the thickness direction of the base membrane.
[0017] When the isolation membrane only includes a base membrane, the porosity of the base membrane can be designed to vary gradually along its thickness direction, if the material and preparation process permit.
[0018] In some embodiments, the isolation membrane includes a base membrane and a composite layer located on one surface of the base membrane, and the porosity of the base membrane is smaller than the porosity of the composite layer.
[0019] When the isolation membrane includes both a base membrane and a composite layer, in order to meet the requirement that the porosity of the isolation membrane is designed to change gradiently along the thickness direction, the porosity of the base membrane is inconsistent with the porosity of the composite layer. Further considering the preparation process, the porosity of the base membrane is designed to be smaller than the porosity of the composite layer, which is technically easier to achieve.
[0020] In some embodiments, the composite layer comprises more than one coating layer.
[0021] In some embodiments, the composite layer comprises a coating layer having a third surface adjacent to the base film, wherein the porosity of the coating layer decreases gradually from the first surface to the third surface.
[0022] When the composite layer includes a coating, under the premise that the porosity of the base film is less than the porosity of the coating, the porosity of the coating is designed to change in a gradient, which makes the preparation process easier to operate and realize.
[0023] In some embodiments, the porosity q1 of the base film is 30% to 40%, and the base film has a full-fill thickness rebound rate α1 ≤ 100%;
[0024] and / or;
[0025] The porosity q2 of the coating is 40% to 70%, and the full-fill thickness rebound rate α2 of the coating is ≥100%.
[0026] In some embodiments, the composite layer comprises two or more coating layers, and the porosity of the base film is smaller than the porosity of the coating layer close to the base film, and the porosity of the coating layer close to the base film is smaller than the porosity of the coating layer far from the base film.
[0027] When the composite layer includes two or more coatings, since the layer structure of the isolation membrane includes more than three layers, the porosity of each layer is designed to be different, which is both convenient to implement and meets the requirement that the porosity of the isolation membrane is designed to change gradiently along the thickness direction.
[0028] In some embodiments, the original material of the base film includes but is not limited to any conventional material in the art, such as one or more of polypropylene, polyethylene, polyimide, polyamide, polyethylene terephthalate, polyvinylidene fluoride or cellulose substrate.
[0029] In some embodiments, the porosity q1' of the base film is 30% to 40%, and the full-fill thickness rebound rate α1' of the base film is ≤100%;
[0030] and / or;
[0031] The porosity q2' of the coating close to the base film is 35% to 50%, and the full-fill thickness rebound rate of the coating close to the base film is 90%≤α2'≤180%;
[0032] and / or;
[0033] The porosity q3' of the coating layer away from the base film is 50% to 70%, and the full-fill thickness rebound rate α2' of the coating layer away from the base film is ≥180%.
[0034] In some embodiments, the thickness D of the composite layer and the thickness H of the isolation film satisfy: D<0.5×H.
[0035] The thickness of the composite layer in this application is designed to be less than half the thickness of the separator. This is because the separator relies primarily on the base film to conduct internal ions and isolate the positive and negative electrodes from direct contact. The composite layer only serves the technical purpose of improving performance, such as cycle performance. If the composite layer is designed to be thicker than the base film, it will not be conducive to the base film's ability to perform its own functions.
[0036] In some embodiments, the raw material of the coating includes but is not limited to any conventional form in the art, for example, the coating includes a film layer formed on the surface of the base film by at least one of inorganic particles, organic particles, and organic-inorganic hybrid particles, and the inorganic particles include but are not limited to boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, magnesium aluminum silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate, barium titanate, etc. The organic particles include but are not limited to at least one of polyethylene particles, polypropylene particles, polystyrene particles, polyvinylidene fluoride particles, cellulose, cellulose modifiers (such as carboxymethyl cellulose), melamine resin particles, phenolic resin particles, polyester particles (such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate), silicone resin particles, polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles, polyaryletherketone particles, and copolymers of butyl acrylate and ethyl methacrylate (such as cross-linked polymers of butyl acrylate and ethyl methacrylate).
[0037] In a second aspect, the present application provides a secondary battery, comprising:
[0038] Positive electrode;
[0039] negative electrode;
[0040] electrolyte;
[0041] and the isolation film described in the first aspect;
[0042] The first surface of the isolation film is close to the negative electrode plate, and the second surface is close to the positive electrode plate.
[0043] The present application selects a first surface with a porosity greater than a second surface porosity, and the first surface faces the negative electrode sheet, while the second surface faces the positive electrode sheet. This is because during the battery cycle, a portion of sodium ions cannot be completely released from the negative electrode and are deposited on the surface of the negative electrode sheet as insoluble byproducts. On the one hand, the insoluble byproducts require continuous consumption of electrolyte. On the other hand, the increase in the thickness of the negative electrode sheet will inevitably cause the isolation membrane to have a poorer ability to retain liquid after being squeezed. When the end of the isolation membrane with a relatively large porosity faces the negative electrode sheet, the relatively large porosity is first used to store electrolyte, and the electrolyte can be released in time after being squeezed and deformed, which can alleviate the adverse effects of electrolyte reduction.
[0044] When the volume expansion of the positive and negative electrode sheets exerts external force on the isolation membrane, the isolation membrane first relies on its own elastic modulus to have a certain degree of compression resistance. As the degree of extrusion from the positive and negative electrode sheets increases, the isolation membrane is compressed by its own elastic modulus and its thickness decreases. As the positive and negative electrode materials continue to be ejected and embedded, the degree of extrusion of the positive and negative electrode sheets will decrease again. The isolation membrane relies on its own elastic modulus to effectively restore its thickness and achieve full and effective infiltration of the electrolyte, thereby alleviating the problem of rapid attenuation of battery cycle life caused by volume expansion during the use of sodium batteries and improving the cycle service life of sodium batteries.
[0045] In a third aspect, the present application provides an electrical device, which includes the isolation membrane described in the first aspect or the secondary battery described in the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to denote the same components. In the drawings:
[0047] FIG1 is a schematic structural diagram of an isolation membrane in some embodiments of the present application;
[0048] FIG2 is a schematic diagram of the structure of an isolation membrane in some embodiments of the present application;
[0049] FIG3 is a schematic structural diagram of an isolation membrane in some embodiments of the present application;
[0050] FIG4 is a schematic structural diagram of an isolation membrane in some embodiments of the present application;
[0051] FIG5 is a schematic structural diagram of an isolation membrane in some embodiments of the present application;
[0052] FIG6 is a schematic diagram showing the positional relationship between the separator and the negative electrode sheet and the positive electrode sheet in some embodiments of the present application;
[0053] The accompanying drawings in the specific implementation manner are as follows:
[0054] 100, separator; 200, negative electrode; 300, positive electrode;
[0055] 101, first surface; 102, second surface; 103, third surface;
[0056] 110, base film; 120, composite layer;
[0057] 1201, coating; 1202, first coating; 1203, second coating;
[0058] Coordinate axis x direction: thickness direction of the isolation film;
[0059] Coordinate axis y direction: the length or width direction of the isolation membrane. DETAILED DESCRIPTION
[0060] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.
[0061] Unless otherwise defined, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including", "having", "having", etc. in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0062] In the description of the embodiments of the present application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined. Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0063] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0064] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0065] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.
[0066] In the description of the embodiments of the present application, the technical terms "composite" or "composite layer" include any composite form in the field of materials that forms a composite layer. For those skilled in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0067] Lithium accounts for only 0.0065% of the Earth's crust, while sodium accounts for a whopping 2.64%, giving sodium batteries a natural cost advantage over lithium batteries. However, sodium's standard electrode potential is 0.33V higher than lithium's, and its atomic weight and ionic radius are also larger than lithium's. During the charge and discharge cycles of sodium batteries, irreversible reactions occur during the insertion and removal of positive and negative electrode materials. These reaction products, as insoluble byproducts, deposit on the surface of the negative electrode, causing irreversible expansion of the battery.
[0068] When packaging the battery cells, the dimensions of the core or laminated core are properly matched to the cell casing. For example, the thicknesses are within a certain tolerance range. However, the aforementioned irreversible expansion will inevitably lead to the expansion of the core or laminated core. When this expansion is subjected to stress from the cell casing, the separator in the core or laminated core will be squeezed, resulting in a reduction in thickness. The separator used in existing sodium batteries cannot effectively recover after being squeezed, accompanied by the removal and embedding of the positive and negative electrode materials. If the separator cannot be recovered for a long time, its wettability with the electrolyte will inevitably be affected, causing the sodium battery's cycle performance to rapidly decay.
[0069] Currently, the separators used in sodium batteries are being modified in material or structurally improved to enable them to resist the expansion and deformation of the positive and negative electrodes. Research has found that for porous materials with uniform porosity, such as separators, if their porosity is high, their wettability to the electrolyte is improved, but their ability to resist the expansion and deformation of the positive and negative electrodes is reduced. If their porosity is low, although their ability to resist the expansion and deformation of the positive and negative electrodes is improved, the degree of electrolyte wettability cannot be guaranteed. Exploring separators with appropriate porosity places extremely high demands on materials and preparation processes. Further research has found that if the porosity of the separator used in sodium batteries is designed to change in a gradient along a certain direction, for example, the porosity on one side of the separator is larger and the porosity on the other side along a certain direction is smaller, then the separator containing this structure can take into account both its wettability to the electrolyte and a certain ability to resist the expansion and deformation of the positive and negative electrodes.
[0070] Based on the above considerations, in order to alleviate the problem of rapid attenuation of battery cycle life due to volume expansion during the use of sodium batteries. This application designs a separator for sodium batteries, which has a first surface and a second surface along its own thickness direction, and the porosity of the separator decreases gradually when extending from the first surface to the second surface. The porosity of the separator has a gradient-decreasing variation law along its own thickness direction. The separator containing this structure itself has a certain rigidity. When the separator is used in a sodium battery, it is beneficial to achieve its ability to resist the expansion and deformation of the positive and negative pole pieces to a certain extent. Secondly, the separator also has a certain compressibility, which can achieve full and effective infiltration of the electrolyte before being compressed, and can effectively and timely release the electrolyte after being compressed. Therefore, the separator designed in this application can alleviate the problem of rapid attenuation of battery cycle life due to volume expansion during the use of sodium batteries.
[0071] According to some embodiments of the present application, a sodium battery separator 100 is provided, as shown in FIG1 . The separator 100 includes a first surface 101 and a second surface 102 along its thickness direction, where the thickness direction may be the x-axis shown in FIG1 . The first surface 101 and the second surface 102 are disposed opposite each other, and the first surface 101 and / or the second surface 102 are respectively configured to form an interface with the positive and negative electrode sheets. The porosity of the separator 100 decreases gradually as it extends from the first surface 101 to the second surface 102.
[0072] The definition of porosity includes the definition in the field of materials. In the drawings of this application, the number of pores is used to represent the porosity, but the drawings are only schematic diagrams and do not represent the actual number. The porosity can be measured by the following test method or by other conventional methods in the field.
[0073] For example, the dried isolation film sample is cut into a square sample of about 20mm×20mm, and the thickness and actual side length are measured by a digital micrometer and a vernier caliper, and its volume is calculated as V, and its weight is weighed M0. Then, the square sample is immersed in the electrolyte, soaked in the air atmosphere at room temperature for 2 hours, and then taken out, the electrolyte liquid adsorbed on the surface is absorbed, and then its weight is weighed M t , then the porosity of the isolation membrane satisfies the following mathematical relationship:
[0074] The ρ in the above mathematical relationship is the density of the electrolyte, in mm 3 / g, V is the volume of the square sample of the isolation membrane, the unit is mm 3 , weight M0 and M t The unit is g, the weight measuring instrument is a thousandth balance, and the models of the thousandth balance, digital display micrometer, and vernier caliper include but are not limited to any conventional models in the art.
[0075] The gradient reduction includes the change law of the porosity of the isolation membrane along its own thickness direction, wherein the gradient includes a linear relationship or a nonlinear relationship. For example, linear reduction includes but is not limited to any form of linear change conventional in this field, such as, the rate of decrease of the porosity of the isolation membrane along the thickness direction is uniform and constant. For example, nonlinear reduction includes but is not limited to any form of nonlinear reduction conventional in this field, such as exponential decrease, the rate of decrease of the porosity of the isolation membrane along the thickness direction is first relatively large and then relatively small, and for example, logarithmic change, the rate of decrease of the porosity of the isolation membrane along the thickness direction is first relatively small and then relatively large.
[0076] The isolation membrane containing this structure has a certain rigidity. Under this rigidity, the isolation membrane can resist the external force caused by the expansion and deformation of the positive and negative electrode sheets to a certain extent during use. Secondly, the isolation membrane also has a certain compressibility. Before being compressed, it can achieve full and effective infiltration of the electrolyte, and after being compressed, it can effectively and timely release the electrolyte. For example, when the volume expansion of the positive and negative electrode sheets exerts external force on the isolation membrane during use, the isolation membrane first relies on its own rigidity to have a certain degree of compression resistance. As the degree of extrusion from the positive and negative electrode sheets increases, the isolation membrane is compressed and its thickness decreases. As the positive and negative electrode materials continue to be ejected and embedded, the degree of extrusion of the positive and negative electrode sheets will decrease again. The isolation membrane relies on its own compression resistance to effectively restore its thickness and achieve full and effective infiltration of the electrolyte, thereby alleviating the problem of rapid attenuation of the battery cycle life caused by volume expansion during the use of the sodium battery, and improving the cycle service life of the sodium battery.
[0077] According to some embodiments of the present application, the porosity of the first surface is greater than or equal to 50% and less than or equal to 70%; the porosity of the second surface is greater than or equal to 30% and less than 50%.
[0078] The porosity of the first surface and the porosity of the second surface can be determined by slicing to obtain a slice sample, obtaining an image of the slice sample and the pore volume of the slice sample by means of a CCD camera / scanning electron microscope, etc., and obtaining the porosity of the slice sample by calculation; slice samples of a certain thickness can also be obtained by slicing and calculated using the above-mentioned isolation membrane porosity test method. The present application also includes other methods of obtaining the porosity of the first surface and the porosity of the second surface.
[0079] The present application selects a porosity of the first surface greater than that of the second surface, wherein the relatively large porosity at the first surface is beneficial to the infiltration of the electrolyte by the isolation membrane, and the relatively small porosity at the second surface is beneficial to a certain extent resisting the external force caused by the expansion and deformation of the positive and negative pole pieces.
[0080] This application specifically selects a first surface porosity of greater than or equal to 50% and less than or equal to 70%, based on multiple factors, including the material, preparation process, and functional requirements of the isolation membrane. If the first surface porosity is less than 50%, it is not conducive to designing a gradient porosity of the isolation membrane, as the porosity of isolation membranes is typically between 30% and 50%. If the first surface porosity is greater than 70%, the preparation process becomes more difficult to implement.
[0081] According to some embodiments of the present application, the thickness H of the isolation film is 5 μm to 30 μm.
[0082] As shown in FIG1 , the thickness H of the isolation film 100 is the distance between the first surface 101 and the second surface 102. This thickness can be obtained by direct measurement, such as using a micrometer to measure the film thickness. In the present application, the thickness H of the isolation film can be selected to be any one of 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, and 30μm, or any one of the values within the above range. If the thickness of the isolation membrane is less than 5μm, it may affect the realization of its own function. If the thickness of the isolation membrane is greater than 30μm, the selection requirements for the composite layer and the limitations on the preparation process will become more stringent. This application finally selects the thickness H of the isolation membrane to be 5μm to 30μm. Within this thickness range, it is easier to design the porosity of the isolation membrane to change gradually along the thickness direction.
[0083] According to some embodiments of the present application, the porosity of the isolation membrane is q, and the full-fill thickness rebound rate of the isolation membrane is α, which satisfies any of the following conditions: (1) 30%≤q≤40%, α≤100%; (2) 40%<q<60%, 100%<α<200%; (3) 60%≤q≤70%, α≥200%.
[0084] The porosity q of the isolation membrane in the present application includes the average porosity of the isolation membrane, and the average porosity can be directly measured using the above-mentioned measurement method.
[0085] The full-charge thickness rebound rate in this application includes measurements made using conventional methods in the art. For example, the original thickness of the separator is measured as H0. Then, after fully charging the assembled battery, the assembled battery is disassembled and the thickness of the separator after full charge is measured, which is recorded as H1. The separator thickness rebound rate α = (H1 H0) / H0 × 100%.
[0086] From the above, it can be seen that the isolation membrane of the present application expands after the battery is fully charged, which can suppress the expansion of the negative electrode to a certain extent. Therefore, the isolation membrane has the ability to resist the expansion and deformation of the positive and negative electrode plates, and can also take into account its infiltration into the electrolyte, which is beneficial to alleviate the problem of rapid attenuation of the battery cycle life due to volume expansion during the use of sodium batteries.
[0087] According to some embodiments of the present application, the isolation film includes a base film. As shown in FIG2 , the isolation film 100 includes only the base film 110, wherein the base film 110 has a first surface 101 and a second surface 102 along its thickness direction. The porosity of the base film 110 decreases gradually as it extends from the first surface 101 to the second surface 102. The gradient here has the same meaning as described above.
[0088] Since the isolation membrane 100 only includes the base membrane 110, the thickness H of the isolation membrane 100 is the thickness of the base membrane 110. In conjunction with Figure 2, it can be seen that the porosity at a position with a certain distance h1 from the first surface 101 of the isolation membrane 100 is between the porosity of the first surface and the porosity of the second surface. In addition, the material of the base membrane 110 includes but is not limited to any conventional material in the art, such as polypropylene, polyethylene, polyimide, polyamide, polyethylene terephthalate, polyvinylidene fluoride or cellulose substrate, etc. The listed materials include any conventional manufacturers, models, etc. in the art. The present application starts from the fact that a gradient pore structure with the above-mentioned characteristics is easily formed in the base membrane. The base membrane material includes but is not limited to any one of polypropylene, polyethylene, polyimide, and polyethylene terephthalate.
[0089] Regarding the preparation process of the isolation membrane shown in Figure 2, this application includes but is not limited to the use of conventional dry or wet processes in the field, and repeated stretching is adopted during stretching to achieve a gradient change in the porosity of the isolation membrane along its own thickness direction.
[0090] According to some embodiments of the present application, the isolation film not only includes a base film. As shown in Figure 3, the isolation film 100 includes a base film 110 and a composite layer 120 located on one surface of the base film 110, wherein the thickness of the isolation film 100 is H, the thickness of the composite layer 120 is D, and D and H satisfy: D<0.5×H, and the porosity of the composite layer 120 is greater than the porosity of the base film 110.
[0091] The thickness of the composite layer in this application is designed to be less than half the thickness of the separator. This is because the separator relies primarily on the base film to conduct internal ions and isolate the positive and negative electrodes from direct contact. The composite layer only serves the technical purpose of improving performance, such as cycle performance. If the composite layer is designed to be thicker than the base film, it will not be conducive to the base film's ability to perform its own functions.
[0092] As shown in FIG3 , the composite layer 120 includes one or more coating layers 1201, which are formed on one side of the base film 110 by coating, but are not limited to coating. The “…” in the coating layer 1201 in FIG3 indicates a coating layer that may be included but is not specifically listed. The material of the coating layer 1201 includes but is not limited to any conventional form in the art, such as a film layer formed on the surface of the base film by at least one of inorganic particles, organic particles, and organic-inorganic hybrid particles. The inorganic particles include but are not limited to boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, magnesium aluminum silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate, barium titanate, and the like. The organic particles include but are not limited to at least one of polyethylene particles, polypropylene particles, polystyrene particles, polyvinylidene fluoride particles, cellulose, cellulose modifiers (such as carboxymethyl cellulose), melamine resin particles, phenolic resin particles, polyester particles (such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate), silicone resin particles, polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles, polyaryletherketone particles, and copolymers of butyl acrylate and ethyl methacrylate (such as cross-linked polymers of butyl acrylate and ethyl methacrylate).
[0093] The coating materials listed above are all suitable for this application as long as the formation process allows and they can easily form an isolation membrane that satisfies the gradient porosity change.
[0094] The coating material of this application is a film layer formed by organic-inorganic hybrid particles on the surface of the base film, wherein the organic particles include but are not limited to polyvinylidene fluoride particles, and the inorganic particles include but are not limited to any one of aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, and magnesium oxide. The mass ratio between the organic particles and the inorganic particles is (90-95): (10-5). Due to the limitations of the preparation process, this application specifically explores the changes in the porosity of the coating formed when the mass ratio between the organic particles and the inorganic particles is (90-95): (10-5).
[0095] The composite layer is used to describe the film layer formed on the surface of one side of the base film, and the composite method of the composite layer of the present application includes but is not limited to any conventional form in the art, such as coating, deposition, etc. The listed coating, deposition and other processes include any conventional form in the art.
[0096] By designing the porosity of the base film 110 to be inconsistent with the porosity of the composite layer 120, it is beneficial to achieve that the isolation film not only takes into account its degree of wettability to the electrolyte, but also has a certain ability to resist the expansion and deformation of the positive and negative electrode sheets.
[0097] According to some embodiments of the present application, as shown in FIG. 4 , an isolation film 100 includes a base film 110 and a coating 1201 located on one surface of the base film 110. The coating 1201 includes a third surface 103 proximal to the base film 110 and a first surface 101 of the isolation film 100 at an end surface distal to the base film 110. The porosity of the coating 1201 decreases gradually as it extends from the first surface 101 to the third surface 103. The term "gradient" here has the same meaning as described above.
[0098] The preparation process of the isolation membrane shown in Figure 4 includes but is not limited to the use of conventional dry or wet processes in the field to prepare the base membrane, and also includes coating one side surface of the base membrane with a slurry to prepare a coating, and controlling the different solid contents of the slurry to achieve a gradient change in the porosity of the coating. The solid content of the slurry refers to the mass percentage of the remaining part of the slurry after drying under specified conditions, which can be obtained by experimental calculation. The coating method includes but is not limited to any conventional form in the field, such as gravure roller coating. Among them, in this embodiment, the present application is easier to implement from the perspective of the preparation process by performing a gradient design on the porosity of the composite layer, and at the same time, this design method has a relatively small impact on the isolation membrane to achieve its own other properties in the battery.
[0099] The present application discloses in some embodiments that, when a coating is included, the porosity q1 of the base film is 30% to 40%, and the base film has a full thickness rebound rate α1 ≤ 100%;
[0100] and / or;
[0101] The porosity q2 of the coating is 40% to 70%, and the full-fill thickness rebound rate α2 of the coating is ≥100%. According to some embodiments of the present application, in combination with Figure 5, it can be seen that the isolation film 100 includes a base film 110 and two coatings 1201 located on one side of the base film 110, namely a first coating 1202 and a second coating 1203, wherein the first coating 1202 is arranged close to the base film 110, and the second coating 1203 is arranged away from the base film 110, and the porosity of the base film 110 is less than the porosity of the first coating 1202, and the porosity of the first coating 1202 is less than the porosity of the second coating 1203. The isolation film preparation process designed in this embodiment includes but is not limited to preparing the base film using a conventional dry process or wet process in the field, and then preparing coating slurries with different solid contents, and sequentially coating the coating slurries with different solid contents on one side of the base film under the condition of satisfying the porosity distribution.
[0102] The present application discloses in some embodiments that, when two coating layers are included, the porosity q1' of the base film is 30% to 40%, and the full-fill thickness rebound rate α1' of the base film is ≤100%;
[0103] and / or;
[0104] The porosity q2' of the first coating is 35% to 50%, and the full-fill thickness rebound rate of the first coating is 90% ≤ α2' ≤ 180%;
[0105] and / or;
[0106] The porosity q3' of the second coating layer is 50% to 70%, and the full-fill thickness rebound rate α2' of the second coating layer is ≥180%.
[0107] This application also includes forming three or more coatings on one side of the base film, and the design method is consistent with the above two coatings. This application achieves a gradient porosity change in the composite layer composed of the coatings by controlling the solid content of the different coating slurries. The gradient here is consistent with the above meaning.
[0108] In a second aspect, the present application also discloses a secondary battery, which includes a positive electrode sheet, a negative electrode sheet and an electrolyte, and also includes the separator described in the first aspect; wherein the first surface of the separator is close to the negative electrode sheet, and the second surface is close to the positive electrode sheet. The present application chooses to place the end of the separator with a relatively large porosity facing the negative electrode sheet, and the end of the separator with a relatively small porosity facing the positive electrode sheet. This is because during the battery cycle, there is always a part of the sodium ions that cannot be completely released from the negative electrode and are deposited on the surface of the negative electrode sheet as insoluble by-products. On the one hand, the insoluble by-products need to continuously consume the electrolyte, and on the other hand, the increase in the thickness of the negative electrode sheet will inevitably cause the separator to have a poorer liquid retention capacity after being squeezed. When the end of the separator with a relatively large porosity faces the negative electrode sheet, the relatively large porosity is first used to store the electrolyte, and the electrolyte can be released in time after being squeezed and deformed, which can alleviate the adverse effects of the reduction in electrolyte.
[0109] As shown in FIG6 , by arranging the first surface 101 of the isolation membrane 100 close to the negative electrode sheet 200 and the second surface 102 close to the positive electrode sheet 300, that is, the end face with larger porosity in the isolation membrane 100 is arranged close to the negative electrode sheet 200, and the end face with smaller porosity is arranged close to the positive electrode sheet 300, it is beneficial to resist the external force caused by the expansion and deformation of the positive and negative electrode sheets to a certain extent, and is also beneficial to the infiltration of the isolation membrane into the electrolyte.
[0110] The isolation membrane containing this structure has a certain degree of rigidity and compressibility, so that it can resist a certain degree of extrusion from the positive and negative electrode sheets, and can fully and effectively infiltrate the electrolyte. For example, when the isolation membrane is subjected to a certain degree of extrusion from the negative electrode sheet, it first relies on its own rigidity to resist the extrusion. As the degree of extrusion of the negative electrode sheet increases, the isolation membrane is compressed and its thickness decreases. As the positive and negative electrode materials are released and embedded, the degree of extrusion of the negative electrode sheet will decrease again. The isolation membrane relies on its own elastic modulus to effectively restore its thickness and achieve full and effective infiltration of the electrolyte, thereby alleviating the problem of rapid attenuation of the battery cycle life due to volume expansion during the use of the sodium battery and improving the cycle service life of the sodium battery.
[0111] According to some embodiments of the present application, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into a secondary battery by a winding process or a lamination process, wherein the winding process or the lamination process includes but is not limited to any conventional process in the art.
[0112] The secondary battery preparation process provided in this application does not change the existing sodium battery preparation process and production line, and the design method is highly flexible.
[0113] According to some embodiments of the present application, the positive electrode sheet of the secondary battery includes a positive electrode active material, which is at least one of a sodium transition metal oxide, a polyanion compound, and a Prussian blue compound. Among them, the transition metal in the sodium transition metal oxide can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. The sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1. Polyanionic compounds include one or more of sodium vanadium trifluorophosphate Na3V2(PO4)2F3, sodium vanadium fluorophosphate NaVPO4F, sodium vanadium phosphate Na3V2(PO4)3, Na4Fe3(PO4)2P2O7, NaFePO4, and Na3V2(PO4)3. Prussian blue compounds are Na x M1M2(CN)6, wherein M1 and M2 are one or more of Fe, Mn, Co, Ni, Cu, Zn, Cr, Ti, V, Zr, and Ce, and 0<x≤2.
[0114] A binder and / or a conductive agent may also be added to the positive electrode active material. There is no limitation on the types of the binder and the conductive agent, and those skilled in the art may select them according to actual needs. For example, the binder may be one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), polyvinyl alcohol (PVA), and styrene-butadiene rubber (SBR). The conductive agent may be one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, and carbon nanofibers.
[0115] The negative electrode plates that make up the secondary battery include carbon-based negative electrode materials, titanium-based oxide negative electrode materials, metal and alloy negative electrode materials, and non-metallic elements. Among them, the carbon-based negative electrode materials include hard carbon and soft carbon, the titanium-based oxide negative electrode materials include titanium dioxide and other optimized materials, the metal and alloy negative electrode materials can be tin, antimony, germanium and lead, etc., and the non-metallic elements include carbon elements, etc.
[0116] According to some embodiments of the present application, the electrolyte constituting the secondary battery includes a sodium salt and an organic solvent. Specifically, there is no particular restriction on the organic solvent in the electrolyte, and the organic solvent can be an organic solvent commonly used in the art for electrolytes. As an example, the organic solvent can be selected from at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate, methyl acetate, ethyl propionate, fluoroethylene carbonate, ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and methyl tert-butyl ether. Ether solvents are preferably used to adjust the sodium ion deposition morphology, thereby inhibiting the massive growth of sodium dendrites. In the secondary battery of the present application, there is no particular restriction on the sodium salt in the electrolyte, and the sodium salt can be a sodium salt commonly used in the art for electrolytes. As an example, the sodium salt may be selected from at least one of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate, and sodium chloride.
[0117] The secondary battery provided in this application can be used to manufacture electrical equipment, which can be used as a power source or as an energy storage unit. The electrical equipment has good application prospects in the power field, such as two-wheeled electric vehicles, low-speed electric vehicles, electric ships, buses / coaches, etc., and / or energy storage fields, such as home / industrial energy storage, 5G communication base stations, data centers, renewable energy access, etc., but is not limited to the above-mentioned fields.
[0118] In order to make the purpose, technical solutions and advantages of the present application clearer, the separator used in the secondary battery protected by the present application and the secondary battery are described in detail below with reference to specific embodiments.
[0119] Examples 1 to 4
[0120] Provided is an isolation membrane comprising only a base membrane, wherein the base membrane is made of polyethylene, and wherein the thickness H of the isolation membrane is between 5 μm and 30 μm. The porosity of a first surface of the isolation membrane is greater than or equal to 50% and less than or equal to 70%, and the porosity of a second surface of the isolation membrane is greater than or equal to 30% and less than 50%. Specific parameters of various embodiments are shown in Table 1 below.
[0121] Table 1 List of isolation membrane parameters of Examples 1 to 4
[0122] Examples 5 to 10
[0123] Provided is an isolation membrane having a thickness H of 5 μm to 30 μm. The isolation membrane comprises a base membrane and a coating located on one surface of the base membrane. The coating constitutes a composite layer. The thickness D of the composite layer satisfies: D < 0.5 × H. The base membrane material is a polyimide-formed membrane layer having a porosity of 40%. The coating material is a membrane layer formed by polyvinylidene fluoride particles on the polyimide surface. The membrane layer is filled with aluminum oxide particles, and the mass ratio is 90:10.
[0124] The specific parameters of each embodiment are shown in Table 2 below;
[0125] Table 2 List of isolation membrane parameters of Examples 5 to 10
[0126] In Table 2, the distance h1 from the first surface satisfies: h1 = 0.5×D.
[0127] Examples 11 to 14
[0128] Provided is an isolation membrane having a thickness H of 5 μm to 30 μm. The isolation membrane comprises a base membrane and two coatings located on one surface of the base membrane. The two coatings constitute a composite layer. The thickness D of the composite layer satisfies: D < 0.5 × H. The base membrane material is a polyimide-formed membrane layer with a porosity of 30%. The first coating material is a membrane layer formed by polyvinylidene fluoride particles on the surface of the polyimide. The membrane layer is filled with silicon oxide particles at a mass ratio of 95:5. The second coating material is a membrane layer formed by polyvinylidene fluoride particles on the surface of the first coating layer. The membrane layer is filled with aluminum oxide particles at a mass ratio of 90:10.
[0129] The specific parameters of each embodiment are shown in Table 3 below;
[0130] Table 3 List of isolation membrane parameters of Examples 11 to 14
[0131] The isolation membrane prepared in the above embodiment is selected to prepare a sodium battery;
[0132] Layered oxide is selected as the positive electrode active material of the positive electrode plate, and CNT coating is selected as the negative electrode plate. The isolation membrane, layered oxide positive electrode plate, and CNT coating negative electrode plate are assembled together according to the stacking process, and the electrolyte sodium hexafluorophosphate + triethylene glycol dimethyl ether is injected to form a secondary battery.
[0133] Positive electrode preparation:
[0134] The positive electrode slurry was prepared by mixing Na3V2(PO4)3 material as the positive electrode, polyvinylidene fluoride as the binder, and conductive carbon black as the conductive agent in a mass ratio of 90%:5%:5% in N-methylpyrrolidone solvent. The positive electrode slurry was prepared by extrusion coating machine at a unit area mass of 30 mg / cm 2 It is required to coat the positive electrode slurry on the surface of the aluminum foil and dry it, and then use a cold press to press the coated electrode at a pressure of 2.5g / cm 3 The design is compacted and cold pressed.
[0135] Preparation of negative electrode sheet: A perforated aluminum foil with a thickness of 10 μm is used as the negative electrode current collector, a CNT coating is applied on the surface of the negative electrode current collector, and a conductive slurry is applied on the perforated current collector using a gravure coater and dried to obtain the final negative electrode sheet.
[0136] Preparation of electrolyte: NaPF6 was dissolved in triethylene glycol dimethyl ether as electrolyte.
[0137] Secondary battery assembly: The positive electrode sheet, negative electrode sheet and isolation film are overlapped together according to the winding process to form a square bare cell. The bare cell is baked at 100°C to remove water, then injected with electrolyte and sealed. After that, the secondary battery is obtained through processes such as static standing, hot and cold pressing, formation, aging, shaping, and capacity testing.
[0138] Test of the rebound rate of the full-fill thickness of the isolation film:
[0139] The original thickness of the separator was measured as H0. The assembled battery was then fully charged and disassembled. The thickness of the separator after full charge was measured and recorded as H1. The separator thickness rebound rate α = (H1 H0) / H0 × 100%. The test results are shown in Table 4.
[0140] Test of the porosity of the isolation membrane:
[0141] The dried isolation film sample was cut into a square sample of about 20mm×20mm. The thickness and actual side length were measured by a digital micrometer and a vernier caliper. The volume V was calculated and the weight M0 was weighed. The square sample was then immersed in the electrolyte and soaked in air at room temperature for 2 hours. After that, it was taken out and the electrolyte liquid adsorbed on the surface was sucked off. Then the weight M was weighed. t , then the porosity of the isolation membrane satisfies the following mathematical relationship:
[0142] Table 4 Isolation film performance list
[0143] "-" in Table 4 indicates absence.
[0144] Battery performance test:
[0145] (1) Capacity retention after 300 cycles at 25°C: At 25°C, the first charge and discharge were performed. The battery was first charged to 3.65 V at a charging current of 1 C. Then, the battery was charged at a constant voltage of 3.65 V to a current of 0.5 C. After standing for 5 minutes, the battery was discharged at 1 C to 1.5 V. The obtained capacity was recorded as the discharge capacity of the first cycle. The charge and discharge cycles were then repeated, and the discharge capacity of the 300th cycle was recorded.
[0146] According to the formula: cycle capacity retention rate = (discharge capacity of the 300th cycle / discharge capacity of the first cycle) × 100%, the capacity retention rate of the battery before and after cycling was calculated, as shown in Table 5;
[0147] (2) Specific capacity after 300 cycles at 25°C: According to the above-mentioned test method for cycle capacity retention, the discharge capacity after the 300th cycle is the battery specific capacity. The specific values are shown in Table 5.
[0148] Table 5 Battery performance list of Examples 1 to 14
[0149] "-" in Table 5 indicates absence.
[0150] Comparative Examples 1 to 6
[0151] An isolation membrane is provided, which is different from the above embodiment in that the pore structure of the isolation membrane is uniformly distributed inside.
[0152] The difference between Comparative Example 1 and Example 4 is that the porosity is 40%.
[0153] Comparative Example 2 differs from Example 9 in that the porosity is 40%.
[0154] Comparative Example 3 differs from Example 14 in that the porosity is 30%.
[0155] Comparative Example 4 differs from Example 14 in that the composite layer has a thickness of 15 μm and a porosity of 30%;
[0156] Comparative Example 5 differs from Example 14 in that the composite layer has a thickness of 17 μm and a porosity of 30%.
[0157] The difference between Comparative Example 6 and Example 14 is that the thickness of the composite layer is 20 μm and the porosity is 40%.
[0158] The specific parameters are listed in Table 6. Using the same assembly and testing methods as above, the battery performance is obtained as shown in Table 7.
[0159] Table 6 List of parameters of isolation membranes of comparative examples 1 to 6
[0160] The separators of Comparative Examples 1 to 6 were subjected to the same battery assembly technology and performance tests as in the examples, and the performances shown in Table 7 below were obtained.
[0161] Table 7 Battery performance list of comparative examples 1 to 6
[0162] Combining Tables 4 to 7, it can be seen that for separators with a porosity gradient distribution, the rebound rate of the separator increases after full charge, that is, the expandability of the separator increases, which can inhibit the expansion of the negative electrode to a certain extent. The secondary battery containing the separator of the present application has a certain improvement in cycle life compared to the secondary battery without the separator of the present application. This may be because the separator has a certain rigidity, which not only helps to achieve a certain degree of resistance to the expansion and deformation of the positive and negative electrode sheets, but also has a certain degree of compressibility and can effectively achieve sufficient electrolyte infiltration, which can alleviate the problem of rapid battery cycle life degradation caused by volume expansion during the use of sodium batteries.
[0163] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A separator for a sodium battery, characterized in that: The isolation film has a first surface and a second surface along the thickness direction thereof, and the porosity of the isolation film decreases gradually when extending from the first surface to the second surface.
2. The isolation film according to claim 1, characterized in that: The porosity of the first surface is greater than or equal to 50% and less than or equal to 70%, and the porosity of the second surface is greater than or equal to 30% and less than 50%.
3. The separator according to any one of claims 1 to 2, characterized in that: The thickness H of the isolation film is 5 μm to 30 μm.
4. The separator according to any one of claims 1 to 3, characterized in that: The porosity of the isolation membrane is q, and the full-fill thickness rebound rate of the isolation membrane is α, which satisfies any of the following conditions: (1)30%≤q≤40%,α≤100%; (2)40%<q<60%,100%<α<200%; (3)60%≤q≤70%,α≥200%。 5. The separator according to any one of claims 1 to 4, characterized in that: The isolation film includes a base film.
6. The separator according to any one of claims 1 to 5, characterized in that: The isolation film comprises a base film and a composite layer located on one surface of the base film, and the porosity of the base film is smaller than the porosity of the composite layer.
7. The isolation film according to claim 6, characterized in that: The composite layer comprises more than one coating layer.
8. The separator according to any one of claims 6 to 7, characterized in that: The composite layer includes a coating layer having a third surface close to the base film, and the porosity of the coating layer decreases gradually when extending from the first surface to the third surface.
9. The isolation film according to claim 8, characterized in that: The porosity q1 of the base film is 30% to 40%, and the full-fill thickness rebound rate α1 of the base film is ≤100%; and / or; The porosity q2 of the coating is 40% to 70%, and the full-fill thickness rebound rate α2 of the coating is ≥100%.
10. The separator according to any one of claims 6 to 7, characterized in that: The composite layer comprises two or more coating layers, and the porosity of the base film is smaller than the porosity of the coating layer close to the base film, and the porosity of the coating layer close to the base film is smaller than the porosity of the coating layer far from the base film.
11. The isolation film according to claim 10, characterized in that: The porosity q1' of the base film is 30% to 40%, and the full-fill thickness rebound rate α1' of the base film is ≤100%; and / or; The porosity q2' of the coating close to the base film is 35% to 50%, and the full-fill thickness rebound rate of the coating close to the base film is 90%≤α2'≤180%; and / or; The porosity q3' of the coating layer far from the base film is 50% to 70%, and the full-fill thickness rebound rate α2' of the coating layer far from the base film is ≥180%.
12. The separator according to any one of claims 5 to 11, characterized in that: The thickness D of the composite layer and the thickness H of the isolation film satisfy: D<0.5×H.
13. A secondary battery, characterized in that: The secondary battery comprises: Positive electrode; Negative electrode; Electrolyte; and the isolation film according to any one of claims 1 to 12; The first surface of the isolation film is close to the negative electrode plate, and the second surface is close to the positive electrode plate.
14. An electrical device, characterized in that: The electric device comprises the separator according to any one of claims 1 to 12 or the secondary battery according to claim 13.
Citation Information
Patent Citations
Battery separators with variable porosity
CN102544417A
Lithium-ion battery
CN106654351A
Sodium ion battery and preparation method thereof
CN114583174A
Isolating membrane, isolating membrane preparation method and isolating membrane preparation device
CN114784462A
Isolating membrane, preparation method thereof, secondary battery comprising isolating membrane and electric device
CN115810874A
Cited By
Lithium battery diaphragm with gradient pore structure and preparation method thereof
CN119812677A
Negative electrode-free battery cell, battery apparatus, and electric apparatus
WO2026158058A1