Structure comprising two layers having different electrical natures and method for preparing same
The introduction of a transition zone with specific chemical elements in the structure of MIM type capacitances prevents oxide interface layer formation, addressing the issue of unwanted oxidation and ensuring efficient growth and performance in micro- and nano-electronic devices.
Patent Information
- Application Number
- PCT/FR2024/050582
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2024-05-03
- Publication Date
- 2024-11-07
AI Technical Summary
The manufacture of MIM type capacitances in micro- and nano-electronic devices is hindered by unwanted oxidation of electrical layers, leading to non-conductive oxide interface layers that degrade the electrical response and hinder the growth of metal and/or metal nitride layers on dielectric layers.
A structure comprising a stack of two layers with a transition zone that includes specific chemical elements from both layers, free of oxygen, ensuring continuity of growth and preventing oxide interface layer formation, thereby maintaining the intrinsic properties of the layers.
This approach allows for the creation of efficient MIM type capacitances with controlled growth and reduced degradation, ensuring high performance and efficiency in micro- and nano-electronic devices.
Smart Images

Figure FR2024050582_07112024_PF_FP_ABST
Abstract
Description
[0001] STRUCTURE COMPRISING TWO LAYERS OF DIFFERENT ELECTRICAL NATURE AND ITS PREPARATION METHOD
[0002] DESCRIPTION
[0003] TECHNICAL FIELD
[0004] The invention relates to the field of micro- and nano-structures for micro- and nano-electronic and optronic devices.
[0005] More specifically, the invention relates to a structure comprising two layers of different electrical nature.
[0006] It also relates to a process for preparing a structure as defined above.
[0007] The invention finds particular application in the manufacture of high-density capacitances, for example of the MIM (for “Metal-Insulator-Metal”) type for devices such as digital memories, analog or digital converters or even radiofrequency filters.
[0008] STATE OF THE PRIOR ART
[0009] The advent of connected and intelligent objects is currently the subject of research, particularly research into highly advanced and increasingly complex micro- and nano-electronic devices.
[0010] In addition to developments related to the architecture and design of micro- and nano-electronic components to meet very advanced technological criteria and performance, research is being carried out to enable an increasingly significant reduction in the size of these components.
[0011] MIM-type capacitances represent one of the essential components for such micro- and nano-electronic devices and are obtained, most often, by successive depositions of a first electrical layer, a dielectric layer and a second electrical layer.
[0012] Generally, such layers are deposited by atomic layer deposition (ALD) or plasma-assisted ALD (PEALD), allowing successive deposition of extremely thin and conformable layers, i.e. perfectly matching the surface of the substrate which is intended to support a stack of these layers.
[0013] However, the manufacture of a MIM type capacitance is often assimilated to the manufacture of a MOIM type capacitance (for "Metal-Oxide-Insulator-Metal"), or even MOIOM (for "Metal-Oxide-Insulator-Oxide-Metal"), as described in application EP 3570307-A1 or in patent US 10,319,806-B2.
[0014] Indeed, oxidation of the electrical layers (or so-called metallic layers) can occur in an unwanted and uncontrolled manner, thus introducing non-conductive oxide interface layers between the metallic layer and the dielectric layer. These oxide layers are not desirable in such structures because they are likely to modify the electrical response, or impact the electrical operation, of the MIM-type capacitance.
[0015] Furthermore, the growth of electrical layers, which are generally made of a metal and / or a metal nitride, on a dielectric layer may suffer from delayed growth, or even an absence of growth, due to the nature of the electrical and dielectric layers used.
[0016] In view of the above, the inventors set themselves the goal of overcoming the drawbacks of the prior art, in particular by proposing a structure comprising a stack of two layers of different electrical nature while avoiding the formation of oxide interface layers, thus making it possible to obtain high-performance structures and avoiding their degradation.
[0017] STATEMENT OF THE INVENTION
[0018] The invention aims precisely to provide such a structure.
[0019] The invention therefore relates, firstly, to a structure comprising a substrate covered by a stack comprising a first layer and a second layer, the first layer being electrically conductive (also called first electrode) and comprising a first specific chemical element, the second layer being a dielectric layer or an electrically insulating layer, the second layer comprising a second specific chemical element. The structure comprises a first transition zone between the first layer and the second layer. The first transition zone is in contact with the first layer and the second layer. In other words, no other material is present between the first layer and the first transition zone or between the second layer and the first transition zone.
[0020] The first transition zone includes the first specific chemical element and the second specific chemical element but is free of oxygen.
[0021] It should be noted that the structure may comprise a stack comprising successively, from the substrate, the first layer then the second layer or a stack comprising successively, from the substrate, the second layer then the first layer, preference however being given to the stack comprising successively, from the substrate, the first layer then the second layer.
[0022] Furthermore, it is specified that the second layer may be a unitary dielectric layer, made of a single material, or may comprise several dielectric layers, in the form of an alternation of different unitary layers, to fulfill microelectronic or optronic functionalities, preference being given, however, to a unitary layer.
[0023] The invention is fundamentally distinguished from the prior art by the presence of the first transition zone which makes it possible to guarantee continuity of growth of the first layer and the second layer of the structure, without degrading their intrinsic properties.
[0024] In fact, the first transition zone allows both to finalize the growth of the first layer and to initiate the growth of the second layer, while having a role of barrier to the oxidation of the first layer. The first transition zone therefore makes it possible to avoid the formation of an oxide interface layer.
[0025] It is specified that, in the foregoing and the following, the term "growth" means that the second layer can be deposited and grow on the surface of the first underlying layer, so as to have a desired homogeneous thickness over this entire surface. One of the properties of the first transition zone is linked to its physicochemical affinity with the first layer and with the second layer, this transition zone being in contact with these layers. The composition of such a transition zone is characterized by a mixture comprising at least the first specific chemical element - which the first layer comprises - and at least the second specific chemical element - which the second layer comprises. For example, the first layer may have as its specific chemical element an element called "A" while the second layer may have as its specific chemical element an element called "B".In this case the first transition zone is characterized by a composition called “AB”.
[0026] The first transition zone is therefore judiciously chosen and adjusted according to the desired nature of the first layer and the second layer.
[0027] Preferably, the first transition zone is not a metal oxide layer. In other words, it is preferred that the first specific element and the second specific element are not oxygen.
[0028] According to the invention, the first specific chemical element is preferably nitrogen and the second specific chemical element is preferably a metal, it being understood that the first layer is made of a metal nitride and the second layer is made of a metal oxide or a metal oxynitride.
[0029] Typically, the first, electrically conductive layer is chosen to have an electrical resistivity of less than 10 -3 Q.cm, for example between 10 -6 Q.cm and 10 -3 Q.cm, while the second layer, electrically insulating, is chosen so as to have an electrical resistivity greater than 10 5 Q.cm, for example between 10 5 Q.cm and 10 18 Q.cm. This first layer can be used as a first electrode while this second layer can be used as a dielectric layer in a MIM type capacitance.
[0030] For example, the first layer may be titanium nitride, molybdenum nitride, tungsten nitride, tantalum nitride or niobium nitride or a mixture thereof and the second layer may be silicon, aluminum, hafnium, zirconium, tantalum, lanthanum or titanium oxide, or a mixture thereof. The second layer may also be silicon oxynitride. In this case, the first transition zone is advantageously aluminum nitride, tantalum nitride, hafnium nitride, niobium nitride, titanium carbonitride or tantalum carbonitride.
[0031] According to the invention, the first transition zone has a thickness preferably between 0.1 nm and 3 nm and, even better, equal to 0.5 nm.
[0032] It is specified that, in the above and below, the expressions "from ... to ..." and "between ... and ..." are equivalent and are intended to mean that the limits are included.
[0033] By presenting a very low thickness, the first transition zone can easily be integrated into the construction and preparation of micro- and nano-structures such as MIM-type capacitances.
[0034] Furthermore, the stack may further comprise a third electrically conductive layer (also called second electrode), the second layer being arranged between the first layer and the third layer. The stack therefore relates, in this case, to a MIM type capacitance.
[0035] According to an alternative embodiment, the third layer may be in contact with the second layer.
[0036] According to another embodiment, the structure comprises a second transition zone between the second layer and the third layer. In this case, the second transition zone is in contact with the second layer and the third layer. In other words, no other material is present between the second layer and the second transition zone or between the third layer and the second transition zone.
[0037] According to this other embodiment, the third layer comprises a third specific chemical element. The second transition zone then comprises the second specific chemical element and the third specific chemical element but is free of oxygen. The third specific chemical element may be the same as or different from the first specific chemical element. Preferably, the third specific chemical element is identical to the first specific chemical element.
[0038] The second transition zone thus ensures continuity between the second layer and the third layer. One of the properties of the second transition zone is linked to its physicochemical affinity with the second layer and with the third layer, this second transition zone being in contact with these layers. The composition of this second transition zone is characterized by a mixture comprising at least the second specific chemical element - which the second layer comprises - and at least the third specific chemical element - which the third layer comprises. For example, for a second layer having as its specific chemical element an element called "B" and a third layer having as its specific chemical element an element called "A'", then the second transition zone is characterized by a composition called "BA'".
[0039] The second transition zone is therefore judiciously chosen and adjusted according to the desired nature of the second layer and the third layer.
[0040] Preferably, the second transition zone is not a metal oxide layer. In other words, it is preferred that the third specific element and the second specific element are not oxygen.
[0041] As mentioned previously, the third specific chemical element is preferably identical to the first specific chemical element. Thus the third specific chemical element may be nitrogen, provided that the third layer is a metal nitride.
[0042] The third layer is also chosen to have an electrical resistivity of less than 10 -3 Q.cm, for example between 10 -6 Q.cm and 10 -3Q.cm. This third layer can be used as a second electrode in a MIM type capacitance.
[0043] This third layer may be identical or different from the first layer, preferably identical and may thus be made of titanium nitride, molybdenum nitride, tungsten nitride, tantalum nitride or niobium nitride or a mixture thereof.
[0044] In this case, the second transition zone is advantageously made of aluminum nitride, tantalum nitride, hafnium nitride, niobium nitride, titanium carbonitride or tantalum carbonitride. Preferably, the structure comprises one of the stacks as described in the following Table I:
[0045] Table I The stacks described above may further comprise a second transition zone and then a third layer. Preferably, the second transition zone is identical to the first transition zone. The third layer is preferably identical to the first layer.
[0046] The second transition zone has a thickness preferably between 0.1 nm and 3 nm and, more preferably, equal to 0.5 nm.
[0047] As for the first transition zone, this second transition zone, by having an extremely small thickness, can easily be integrated into the construction and preparation of micro- and nano-structures, such as MIM-type capacitances. Furthermore, in accordance with the invention, the substrate of the structure can have a flat surface - i.e. in two dimensions - or a microstructured surface - i.e. in three dimensions. It is specified that, in the foregoing and the following, the term "microstructured surface" means a surface comprising pores or vias, for example of an elongated shape, which makes it possible in particular to increase the specific surface area of the substrate - i.e. the surface area of the substrate intended to be covered by the stack comprising the first layer, the second layer and possibly the third layer - compared to a flat surface.
[0048] Thus, a microstructured surface can have a more or less important aspect ratio, this aspect ratio corresponding to the ratio of the longitudinal dimension to the transverse dimension of the pores or vias. Also, the higher the aspect ratio, the greater the specific surface area of the substrate. For example, an aspect ratio greater than 20 can be considered.
[0049] The substrate may also include microelectronic components.
[0050] The substrate may be silicon, metal nitride or a metal oxide material such as alumina, or any other suitable material.
[0051] The structure as previously described may be prepared by a method which comprises at least the following successive steps: a) deposition, preferably by ALD, of one of the first layer or the second layer on the substrate; b) deposition, preferably by ALD, of the other of the first layer or the second layer; the method being characterized in that it comprises a sub-step of forming the first transition zone at the end of step a) or at the beginning of step b).
[0052] It is possible to deposit the first layer then the second layer, or vice versa. Preferably, steps a) and b) are carried out using the vacuum ALD deposition technique (from a few mTorr to a few Torr; i.e. between approximately 0.1 Pa and a few hundred Pa, for example 300 Pa), which makes it possible to obtain very conformable layers of very high purity and very low thickness.
[0053] The ALD depositions of step a) and step b) can be carried out at a temperature between 200°C and 450°C, for example at 400°C for step a) and 330°C for step b). The sequence of steps a) and b) is typically carried out without breaking the vacuum, which in particular makes it possible to avoid the formation of oxide interface layers between the first layer and the second layer.
[0054] The formation of the first transition zone is characterized in that it is carried out in a single step either with the deposition of one of the first layer or the second layer - in the case where it is carried out at the end of step a) - or with the deposition of the other of the first layer or the second layer - in the case where it is carried out at the beginning of step b) - thus making it possible to control the composition and the thickness of the different layers and of the first transition zone of the structure.
[0055] By "single step" is meant that the formation of the first transition zone takes place under the same temperature and pressure conditions as the deposition of the first layer or the deposition of the second layer.
[0056] The fact that the formation of the first transition zone can be judiciously adapted either at the end of step a) or at the beginning of step b) makes it possible to prepare several structures in parallel.
[0057] It is recalled that the principle of ALD deposition lies in introducing at least two reactive species, called "precursors", into an ALD chamber, then circulating them alternately on the surface of a material.
[0058] The choice of precursors ultimately depends on the desired nature of the layer to be deposited or the transition zone to be formed.
[0059] In the context of the invention, the sub-step of forming the first transition zone can be carried out by ALD by introducing and circulating alternately a first pair of precursors to form the first transition zone, characterized in that one of the precursors of the first pair of precursors comprises the first specific chemical element and the other precursor of this first pair comprises the second specific chemical element.
[0060] According to a first particular embodiment of the invention, the first deposited layer is made of titanium nitride (TiN) using, for example, as precursors titanium tetrachloride (TiC), tetrakis(dimethylamino)titanium (TDMAT) or tetrakis(diethylamino)titanium (TDEAT), all being coupled with ammonia. According to this first particular embodiment, a second layer of alumina (AI2O3) can be deposited, for example, using as precursor trimethylaluminum (TMA) coupled with water vapor, in which case the first transition zone can advantageously be made of aluminum nitride (AIN), using, for example, as first pair of precursors TMA coupled with ammonia.
[0061] Still according to this first particular embodiment, the second deposited layer can also be in a mixture comprising aluminum oxide and titanium oxide (AI2O3, TiO2) using, for example, as precursors TMA coupled with water for KAI2O3 and TiCk coupled with water for TiO2 Or the second layer can be in a mixture comprising aluminum oxide and zirconium oxide (AI2O3, ZrO2) using, for example, as precursors TMA coupled with water for KAI2O3 and zirconium tetrachloride (ZrCU) coupled with water for ZrO2, in which case the first transition zone can advantageously be in AIN using, for example, as first pair of precursors TMA coupled with an ammonia plasma.
[0062] Still according to this first particular embodiment, the second deposited layer may be made of hafnium oxide (HfO2) using, for example, as precursor hafnium tetrachloride (HfCU) coupled with water or the second layer may be made of HfZnO using, for example, as precursors HfC and diethyl zinc (DEZ) coupled with water, in which case the first transition zone may advantageously be made of hafnium nitride (HfN) using, for example, as first pair of precursors HfCk coupled with an ammonia plasma or coupled with an H2N2 plasma.
[0063] Still according to this first particular embodiment, a second layer of titanium oxide (Tit^) can be deposited, for example, using TiC or TDMAT as precursors, these two precursors being coupled with water, in which case the first transition zone can advantageously be made of titanium carbonitride (TiCN), using, for example, as the first pair of precursors TDMAT coupled with an ammonia plasma or else coupled with an H2N2 plasma. According to a second particular embodiment of the invention, the first deposited layer is made of tantalum nitride (TaN) using, for example, as precursors tris(diethylam-ido)(tert-butylimido) tantalum (TBTDET) coupled with ammonia.
[0064] According to this second particular embodiment, the second deposited layer may be made of tantalum oxide (Ta2Os) using, for example, as precursors TBTDET coupled with an O2 plasma, in which case the first transition zone may advantageously be made of tantalum carbonitride (TaCN) using, for example, as the first pair of precursors TBTDET coupled with an ammonia plasma or else coupled with an H2N2 plasma.
[0065] Finally, according to a third particular embodiment of the invention, the first deposited layer is made of tungsten nitride (WN) using, for example, as precursors tungsten pentachloride or tungsten hexachloride coupled with ammonia.
[0066] According to this third particular embodiment, the second deposited layer may be made of AI2O3 using, for example, as precursors TMA coupled with water vapor, in which case the first transition zone may advantageously be made of AIN using, for example, as the first pair of precursors TMA coupled with ammonia.
[0067] According to the invention, steps a) and b) can also be carried out successively by ALD in the same ALD chamber, using different precursors during steps a) and b). In this case, the formation of the first transition zone is carried out only when changing the precursors used in step b) to deposit the other of the first layer or the second layer. This makes it possible in particular to avoid a step of changing the ALD chamber between steps a) and b) and also makes it possible to avoid the use of particular precursors for the formation of the first transition zone.
[0068] The introduction and alternating circulation of each of the precursors are followed by a time, called waiting time, before purging them. The waiting time represents the residence time of the precursors on the surface of the substrate or, where appropriate, on the surface of the underlying layer. It is directly proportional to the value of the aspect ratio of the substrate. The waiting time allows the precursors to diffuse and react optimally, particularly in complex structures including, for example, a microstructured surface with a high aspect ratio.
[0069] Typically, the wait time can be set between 15 seconds and 100 seconds, preferably set at 30 seconds.
[0070] Purging is generally carried out for a period ranging from 5 seconds to 40 seconds, to eliminate excess precursors and any unwanted by-products obtained during a reaction between the precursors.
[0071] The introduction and alternating circulation may be repeated a number of times until a desired thickness is obtained. For example, in the context of the invention, the thickness of the first layer and the thickness of the second layer are typically controlled between 1 nm and 50 nm (for example equal to 10 nm for the first layer and equal to 19 nm for the second layer), while the thickness of the first transition zone is typically controlled between 0.1 nm and 3 nm and, preferably, equal to 0.5 nm, by adjusting the number of repetitions of introduction and circulation of each of the precursors.
[0072] According to a particular embodiment of the invention, the method may further comprise a step c) during which the third layer is deposited, preferably by ALD, on the second layer, the method being characterized in that it comprises a sub-step of forming the second transition zone at the end of step b) or at the start of step c), it being understood that, in this case, the first layer is deposited during step a) and the second layer is deposited during step b).
[0073] This embodiment is particularly advantageous in the context of the preparation of MIM type capacitances for example.
[0074] The ALD deposition of step c) can be carried out at a temperature between 200°C and 450°C, for example at a temperature equal to 400°C. The sequence of steps b) and c) is also carried out without breaking the vacuum, for the same reasons as explained previously.
[0075] The formation of the second transition zone is characterized in that it is carried out in a single step either with the deposition of the second layer - in the case where it is carried out at the end of step b) - or with the deposition of the third layer - in the case where it is carried out at the beginning of step c) - thus making it possible to control the composition and thickness of the different layers and of the second transition zone of the structure.
[0076] By "single step" is meant that the formation of the second transition zone takes place under the same temperature and pressure conditions as the deposition of the second layer or the deposition of the third layer.
[0077] The fact of being able to judiciously adapt the formation of the second transition zone either at the end of step b) or at the beginning of step c) makes it possible to prepare several structures in parallel and, in particular, in this case to prepare several MIM type capacitances in parallel.
[0078] According to the invention, the sub-step of forming the second transition zone can be carried out by ALD by introducing and circulating alternately a second pair of precursors for the formation of the second transition zone, characterized in that one of the precursors of the second pair of precursors comprises the second specific chemical element and the other precursor of this second pair comprises the third specific chemical element.
[0079] Again, the choice of precursors depends on the desired nature of the second layer, the third layer and the second transition zone.
[0080] A person skilled in the art knows perfectly how to adapt the choice of precursors according to the nature of the layers to be deposited and the transition zones to be formed.
[0081] According to the invention, steps a), b) and c) can also be carried out successively by ALD in the same ALD chamber, using different precursors during steps a) and b) and during steps b) and c). In this case, the formation of the first transition zone is carried out only when changing the precursors used in step b) to deposit the second layer and the formation of the second transition zone is carried out only when changing the precursors used in step c) to deposit the third layer. This makes it possible in particular to avoid a step of changing the ALD chamber between steps a) and b) and between steps b) and c) and also makes it possible to avoid the use of particular precursors for the formation of the first transition zone and for the formation of the second transition zone.
[0082] It should be noted that the first layer, the second layer and / or the third layer may be structured, and thus present particular patterns, according to the conventional techniques of the prior art, for example by engraving.
[0083] Alternatively to ALD deposition, steps a), b) and c) and the sub-steps of forming the first transition zone and the second transition zone can also be implemented by a plasma-assisted ALD process (also called PEALD for “Plasma Enhanced Atomic Layer Deposition”), by a spatial ALD process (also called SALD for “Spatial Atomic Layer Deposition”) or by an atmospheric pressure ALD process.
[0084] Other alternatives can be implemented, in particular for the deposition of the first electrode and / or the deposition of the second electrode, such as deposition techniques adapted to thin layers, such as physical vapor deposition (or PVD for “Physical Vapor Deposition”) or even chemical vapor deposition (or CVD for “Chemical Vapor Deposition”).
[0085] The person skilled in the art knows perfectly well how to choose the most suitable deposition process, in particular depending on the surface of the substrate used (flat or microstructured).
[0086] The invention is particularly advantageous for preparing MIM structures formed from ultrathin layers.
[0087] However, the invention can be implemented for structures having layers with thicknesses of up to 100 nm.
[0088] Other characteristics and advantages of the invention will emerge from the additional description which follows.
[0089] It goes without saying that this additional description is given only as an illustration of the subject of the invention and should in no case be interpreted as a limitation of this subject. BRIEF DESCRIPTION OF THE FIGURES
[0090] Figure 1 shows a substrate 10 having a planar surface covered by a first electrode 20.
[0091] Figure 2 represents a structure comprising the substrate 10 whose surface is covered by a stack comprising the first electrode 20 and an assembly 300 formed successively by a first transition zone, a dielectric layer and a second transition zone (for reasons of readability, the detail of the assembly 300 is not shown in this figure).
[0092] Figure 3 represents the detail of the assembly 300 formed successively by the first transition zone 2030, the dielectric layer 30 and the second transition zone 3040.
[0093] Figure 4 represents a MIM type SI structure, obtained according to a particular embodiment of the invention, comprising the substrate 10 whose surface is covered by a stack successively comprising the first electrode 20, the assembly 300 and a second electrode 40 (for reasons of readability, the detail of the assembly 300 is not shown in this figure).
[0094] Figure 5 represents (left part) a structure S2 of MIM type, obtained according to another particular embodiment of the invention, comprising the substrate 10 whose surface is covered by a stack successively comprising an assembly 200, an assembly 301 and the second electrode 40; the detail of the assembly 200, formed successively by the first electrode 20 and by the first transition zone 2030 and the detail of the assembly 301, formed successively by the dielectric layer 30 and by the second transition zone 3040, are represented on the right part of this figure.
[0095] Figure 6 represents (left part) a structure S3 of MIM type, obtained according to another particular embodiment of the invention, comprising the substrate 10 whose surface is covered by a stack successively comprising the first electrode 20, an assembly 302 and an assembly 400; the detail of the assembly 302, formed successively by the first transition zone 2030 and by the dielectric layer 30 and the detail of the assembly 400, formed successively by the second transition zone 3040 and by the second electrode 40, are represented on the right part of this figure.
[0096] Figure 7 represents (left part) a structure S4 of MIM type, obtained according to another particular embodiment of the invention, comprising the substrate 10 whose surface is covered by a stack successively comprising the assembly 200, the dielectric layer 30 and the assembly 400; the detail of the assembly 200, formed by the first electrode 20 and by the first transition zone 2030 and the detail of the assembly 400, formed by the second transition zone 3040 and by the second electrode 40, are represented on the right part of this figure.
[0097] Figure 8 represents a MIM type structure, obtained according to another particular embodiment of the invention, comprising a substrate 100 whose surface is microstructured and is covered by a stack successively comprising the first electrode 20, the assembly 300 and the second electrode 40 (for reasons of readability, the detail of the assembly 300 is not shown in this figure).
[0098] It should be noted that the figures described above are schematic representations whose relative dimensions and proportions of the substrates 10 and 100, of the first electrode 20, of the first transition zone 2030, of the dielectric layer 30, of the second transition zone 3040 and of the second electrode 40 are not representative of those likely to be presented in a real situation, for reasons of readability.
[0099] DETAILED PRESENTATION OF SPECIFIC EMBODIMENTS EXAMPLE 1: PREPARATION OF A FIRST STRUCTURE SI
[0100] 1.1- Deposition of the first layer of electrically conductive nature:
[0101] A substrate 10 is placed in a first vacuum ALD chamber dedicated to the deposition of layers of an electrically conductive nature, called electrical layers or electrodes.
[0102] The substrate 10 is made of silicon with silicon oxide electrical insulation. It has a flat surface (Figure 1).
[0103] ALD deposition is carried out at a temperature equal to 400°C by carrying out
[0104] 200 times the following step cycle: - TiC injection for an injection time equal to 2 seconds;
[0105] - circulation of the TiCk on the surface of the substrate 10, respecting a waiting time equal to 30 seconds;
[0106] - purge excess TiC for 40 seconds; then
[0107] - injection of ammonia (NH3);
[0108] - circulation of NH3 on the surface of the substrate 10;
[0109] - purge of excess NH3 as well as any by-products obtained during a reaction between TiCU and NH3.
[0110] The injection time, waiting time and purge time of NH3 are the same as those applied for TiCk.
[0111] Thus, the first TiN electrode 20, with a thickness of 10 nm, is deposited over the entire surface of the substrate 10, as illustrated in FIG. 1.
[0112] 1.2- Formation of the first transition zone, deposition of the second layer of electrical insulating nature and formation of the second transition zone:
[0113] The assembly formed by the substrate 10 and the first TiN electrode 20, obtained in point 1.1 above, is moved to a second vacuum ALD chamber, at 330°C, this time dedicated to the deposition of layers of an insulating electrical nature, called dielectric layers.
[0114] The movement is carried out without passage to air - that is to say that the assembly remains under vacuum - which makes it possible to avoid the formation of an additional oxide interface layer on the surface of the TiN electrode 20.
[0115] 1.2.1 - Formation of the first transition zone
[0116] The first transition zone is formed by ALD deposition by alternately introducing and circulating TMA and NH3 on the surface of the electrode 20.
[0117] TMA is introduced for 1 second and then purged for 5 seconds, while NH3 is introduced for 5 seconds and then purged for 10 seconds, along with any by-products obtained from a reaction between TMA and NH3. The alternating introduction and circulation of TMA and NH3 are repeated 35 times, respecting the injection and purge times mentioned above, while respecting a waiting time of 30 seconds.
[0118] Thus, the first transition zone 2030 in AIN is formed over the entire surface of the first electrode 20 and has a thickness of 0.5 nm.
[0119] 1.2.2 - Deposition of the dielectric layer
[0120] While remaining in the second ALD chamber, the second electrically insulating layer 30, called the dielectric layer, is then deposited by ALD.
[0121] Here, TMA and water vapor are introduced and circulate, alternately, on the surface of the first transition zone 2030 obtained above.
[0122] The TMA and water vapor are each introduced for 0.1 seconds, then, after each introduction, a purge is carried out for 5 seconds after observing a waiting time of 30 seconds.
[0123] The alternating introduction and circulation of TMA and water vapor are repeated 200 times, allowing the dielectric layer 30 in AI2O3 with a thickness of 19 nm to be obtained, over the entire surface of the first transition zone 2030.
[0124] 1.2.3 - Formation of the second transition zone
[0125] Finally, the second transition zone 3040 is formed on the surface of the dielectric layer 30 in the second ALD chamber.
[0126] The formation of the second transition zone 3040 is implemented according to the same methods as those described in point 1.2.1 above.
[0127] The second transition zone 3040 in AIN, with a thickness of 0.5 nm, is thus formed over the entire surface of the dielectric layer 30.
[0128] A structure which thus comprises a stack successively comprising the first electrode 20 and an assembly 300, formed successively by the first transition zone 2030, the dielectric layer 30 and the second transition zone 3040, is obtained and is represented in FIG. 2.
[0129] For readability reasons, the detail of the assembly 300 is not shown in Figure 2 but is shown in Figure 3.
[0130] 1.3- Deposition of the third layer of electrically conductive nature: The structure obtained in point 1.2 above is moved to a third ALD vacuum chamber, dedicated to electrode deposition.
[0131] The movement of the second ALD chamber to the third ALD chamber is, here too, carried out without passage of air, to avoid any formation of an oxide interface layer on the surface of the assembly 300.
[0132] The second TiN electrode 40 is deposited on the surface of the assembly 300 by implementing the same cycle of steps as that described in point 1.1.
[0133] The second electrode 40 thus deposited has a thickness of 10 nm.
[0134] A MIM-type SI structure is then obtained and is represented in Figure 4.
[0135] EXAMPLE 2: PREPARATION OF A SECOND S2 STRUCTURE
[0136] A second MIM-type structure S2 is prepared according to another particular embodiment of the invention.
[0137] The preparation of the second structure S2 comprises the following successive steps and sub-steps: a) i) deposition of the first electrode 20 in TiN; ii) formation of the first transition zone 2030 in AIN; b) i) deposition of the dielectric layer 30 in AI2O3; ii) formation of the second transition zone 3040 in AIN; c) deposition of the second electrode 40 in TiN.
[0138] The above steps and sub-steps are all implemented according to the same methods as those described in example 1, except that the first transition zone is, here, formed at the end of step a) - corresponding to the deposition of the first electrode 20 - that is to say that it is formed in the first vacuum ALD chamber, dedicated to electrode depositions, at a temperature of 400°C.
[0139] A MIM-type structure S2 is thus obtained and represented in Figure 5 (left part). This structure comprises a substrate 10 covered by a stack successively comprising:
[0140] - an assembly 200 which successively comprises the first electrode 20 in
[0141] TiN and the first transition zone 2030 in AIN; - an assembly 301 which successively comprises the dielectric layer 30 in AI2O3 and the second transition zone 3040 in AIN; then the second electrode 40 in TiN.
[0142] The detail of this stacking is shown in Figure 5 (right part).
[0143] EXAMPLE 3: PREPARATION OF A THIRD S3 STRUCTURE
[0144] A third MIM-type structure S3 is prepared according to another particular embodiment of the invention.
[0145] The preparation of the third structure S3 comprises the following successive steps and sub-steps: a) deposition of the first electrode 20 in TiN; b) i) formation of the first transition zone 2030 in AIN; ii) deposition of the dielectric layer 30 in AI2O3; c) i) formation of the second transition zone 3040 in AIN; ii) deposition of the second electrode 40 in TiN.
[0146] The above steps and sub-steps are all implemented according to the same methods as those described in example 1, except that the second transition zone is, here, formed at the start of step c) - corresponding to the deposition of the second electrode 40 - that is to say that it is formed in the third vacuum ALD chamber, dedicated to electrode depositions, at a temperature of 400°C.
[0147] A MIM-type S3 structure is thus obtained and represented in Figure 6 (left part). This structure comprises a substrate 10 covered by a stack successively comprising:
[0148] - the first electrode 20 in TiN;
[0149] - an assembly 302 which successively comprises the first transition zone 2030 in AIN and the dielectric layer 30 in AI2O3; then
[0150] - a set 400 which successively includes the second transition zone
[0151] 3040 in AIN and the second electrode 40 in TiN.
[0152] The detail of this stacking is shown in Figure 6 (right part). EXAMPLE 4: PREPARATION OF A FOURTH S4 STRUCTURE
[0153] A fourth MIM-type structure S4 is prepared according to another particular embodiment of the invention.
[0154] The preparation of the fourth structure S4 comprises the following successive steps and sub-steps: a) i) deposition of the first electrode 20 in TiN; ii) formation of the first transition zone 2030 in AIN; b) deposition of the dielectric layer 30 in AI2O3; c) i) formation of the second transition zone 3040 in AIN; ii) deposition of the second electrode 40 in TiN.
[0155] The above steps and sub-steps are all implemented according to the same methods as those described in example 1, with the exception however that the first transition zone 2030 is formed at the end of step a) - corresponding to the deposition of the first electrode 20 - and that the second transition zone 3040 is, for its part, formed at the start of step c) - corresponding to the deposition of the second electrode 40.
[0156] In other words, the first transition zone 2030 is formed in the first ALD chamber and the second transition zone is formed in the third ALD chamber, i.e., the first transition zone 2030 and the second transition zone 3040 are both formed in vacuum ALD chambers, dedicated to electrode deposition, at a temperature of 400°C.
[0157] A MIM-type S4 structure is thus obtained and represented in Figure 7 (left part). This structure comprises a substrate 10 covered by a stack successively comprising:
[0158] - the assembly 200 which successively comprises the first electrode 20 in TiN and the first transition zone 2030 in AIN;
[0159] - the dielectric layer 30 in AI2O3; then
[0160] - the assembly 400 which successively comprises the second transition zone 3040 in AIN and the second electrode 40 in TiN.
[0161] The detail of this stack is shown in Figure 7 (right part). In the previous examples, the substrate is a substrate having a flat surface. However, as shown in Figure 8, the method for preparing a structure such as a MIM type capacitance could be applied to a substrate 100 having a microstructured surface. The different elements (first electrode 20, assembly 300 and second electrode 40) are then successively deposited on the substrate 100.
Claims
Claims 1. Structure comprising a substrate (10, 100) covered by a stack comprising a first layer (20) and a second layer (30), the first layer (20) being electrically conductive and comprising a first specific chemical element, the second layer (30) being a dielectric layer or an electrically insulating layer, the second layer (30) comprising a second specific chemical element, characterized in that the structure comprises a first transition zone (2030) between the first layer (20) and the second layer (30) and in that the first transition zone (2030) comprises the first specific chemical element and the second specific chemical element and also characterized in that the first specific chemical element is nitrogen and the second specific chemical element is a metal,the first layer (20) being made of a metal nitride and the second layer (30) being made of a metal oxide or a metal oxynitride and in that the first transition zone (2030) is in contact with the first layer (20) and the second layer (30), has a thickness of between 0.1 nm and 3 nm and is free of oxygen., 2. Structure according to claim 1, in which the first layer (20) is made of a titanium nitride, molybdenum nitride, tungsten nitride, tantalum nitride or niobium nitride or a mixture thereof and the second layer (30) is made of an oxide of silicon, aluminum, hafnium, zirconium, tantalum, lanthanum or titanium, a mixture thereof or a silicon oxynitride.
3. Structure according to claim 2, in which the first transition zone (2030) is made of aluminum nitride, tantalum nitride, hafnium nitride, niobium nitride, titanium carbonitride or tantalum carbonitride.
4. Structure according to any one of claims 1 to 3, in which the first transition zone (2030) has a thickness equal to 0.5 nm.
5. Structure according to any one of claims 1 to 4, in which the stack comprises a third electrically conductive layer (40), the second layer (30) being arranged between the first layer (20) and the third layer (40).
6. Structure according to claim 5, wherein the third layer (40) comprises a third specific chemical element, the structure being characterized in that it comprises a second transition zone (3040) between the second layer (30) and the third layer (40), in that this second transition zone (3040) comprises the second specific chemical element and the third specific chemical element, the third specific chemical element preferably being identical to the first specific chemical element and also characterized in that the second transition zone (3040) is in contact with the second layer (30) and the third layer (40) and is free of oxygen.
7. Structure according to any one of claims 1 to 6, in which the substrate (10, 100) has a microstructured surface.
8. A method of preparing a structure as defined according to any one of claims 1 to 7, comprising at least the following successive steps: a) deposition, preferably by ALD, of one of the first layer (20) or the second layer (30) on the substrate (10, 100); b) deposition, preferably by ALD, of the other of the first layer (20) or the second layer (30); the method being characterized in that it comprises a sub-step of forming the first transition zone (2030) at the end of step a) or at the beginning of step b).
9. Method according to claim 8, characterized in that the sub-step of forming the first transition zone (2030) is carried out by ALD by introducing and by circulating alternately a first pair of precursors to form the first transition zone (2030), characterized in that one of the precursors of the first pair of precursors comprises the first specific chemical element and the other precursor of this first pair comprises the second specific chemical element.
10. Method according to claim 8, in which steps a) and b) are successively carried out by ALD in the same ALD chamber, using different precursors during steps a) and b) and in which the formation of the first transition zone (2030) is carried out only when changing the precursors used in step b) to deposit the other of the first layer (20) or the second layer (30).
11. Method according to any one of claims 8 to 10, characterized in that the first layer (20) is deposited during step a) and the second layer (30) is deposited during step b), the method further comprising a step c) during which the third layer (40) is deposited, preferably by ALD, on the second layer (30), the method comprising a sub-step of forming the second transition zone (3040) at the end of step b) or at the start of step c).
12. Method according to claim 11, in which the sub-step of forming the second transition zone (3040) is carried out by ALD by introducing and circulating alternately a second pair of precursors for the formation of the second transition zone (3040), characterized in that one of the precursors of the second pair of precursors comprises the second specific chemical element and the other precursor of this second pair comprises the third specific chemical element.
13. Method according to claim 11, in which steps a), b) and c) are successively carried out by ALD in the same ALD chamber, using different precursors during steps a) and b) and during steps b) and c) and in which the formation of the first transition zone (2030) is carried out only during the changing the precursors used in step b) to deposit the second layer (30) and the formation of the second transition zone (3040) is carried out only when changing the precursors used in step c) to deposit the third layer (40).
Citation Information
Patent Citations
Integrated energy storage component
EP3570307A1
Electrode for a metal-insulator-metal structure, capacitor of metal-insulator-metal type, and method for fabricating one such electrode and one such capacitor
US10319806B2
Semiconductor device and its manufacturing method
JP2004039728A
In-situ formation of metal insulator metal capacitors cross reference to related applications
US20060151852A1
Interfacial materials for use in semiconductor structures and related methods