Lithium secondary battery having high specific capacity
By controlling the elemental sulfur content ratio in lithium-sulfur batteries, the battery's specific capacity and energy density are enhanced, addressing the issue of polysulfide dissolution and achieving high performance levels.
Patent Information
- Application Number
- PCT/KR2023/015467
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-06
- Filing Date
- 2023-10-06
- Publication Date
- 2024-11-07
AI Technical Summary
Lithium-sulfur batteries face a significant reduction in specific capacity and efficiency due to the dissolution of lithium polysulfide in the electrolyte, leading to shuttle reactions and battery deterioration, which limits their performance below theoretical capacity levels.
A lithium-sulfur battery design with a sulfur-carbon composite positive electrode and controlled elemental sulfur content ratio in the electrolyte and electrode, where the content ratio of elemental sulfur in the electrolyte solution to the positive electrode is maintained at 15% or less, enhancing the battery's specific capacity and energy density.
This configuration allows for a specific capacity of 1,000 mAh/g or more and energy density of 300 Wh/kg or more, closely approaching theoretical limits and improving overall battery performance.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Lithium secondary batteries with high specific capacity
[0001] The present invention relates to a lithium secondary battery, and particularly to a lithium-sulfur battery having a high specific capacity.
[0002] This application claims priority to Korean Patent Application No. 10-2023-0057999, filed May 3, 2023, and Korean Patent Application No. 10-2023-0133558, filed October 6, 2023, both of which are incorporated herein by reference.
[0003] As the scope of application of lithium secondary batteries expands beyond portable electronic devices to include electric vehicles (EVs) and electric storage systems (ESS), the demand for lithium secondary batteries with high capacity, high energy density, and long lifespan is increasing.
[0004] Among various lithium secondary batteries, the lithium-sulfur battery is a battery system that uses a sulfur-based material containing a sulfur-sulfur bond as a positive electrode active material, and lithium metal, a carbon-based material in which lithium ions can be inserted / deinserted, or silicon or tin that forms an alloy with lithium as a negative electrode active material.
[0005] Sulfur, the main material of the cathode active material in lithium-sulfur batteries, has the advantages of being a low atomic weight, abundant in resources, easy to supply, inexpensive, non-toxic, and environmentally friendly material.
[0006] In addition, lithium-sulfur batteries have a conversion reaction between lithium ions and sulfur (S8+16Li) at the cathode. + +16e - -> The theoretical specific capacity from 8Li2S reaches 1,675 mAh / g, and when lithium metal is used as the negative electrode, it shows a theoretical energy density of 2,600 Wh / kg. This is a very high figure compared to the theoretical energy density of other battery systems currently being studied (Ni-MH battery: 450 Wh / kg, Li-FeS battery: 480 Wh / kg, Li-MnO2 battery: 1,000 Wh / kg, Na-S battery: 800 Wh / kg) and lithium ion batteries (250 Wh / kg), and therefore, it is attracting attention as a high-capacity, eco-friendly, and low-cost lithium secondary battery among the secondary batteries being developed so far.
[0007] When a lithium-sulfur battery is discharged, sulfur accepts electrons at the positive electrode and a reduction reaction occurs, and lithium polysulfide (Li2S) is formed at the positive electrode. x , x=1~8) are generated, and some of them are easily dissolved in the electrolyte, causing side reactions within the battery, accelerating the deterioration of the battery, and causing a shuttle reaction during the charging process, which significantly reduces the charge / discharge efficiency. As a result, lithium-sulfur batteries currently under development are showing specific capacities that are far below the theoretical specific capacities.
[0008] Therefore, there is a need to develop a lithium-sulfur battery with a high specific capacity at the theoretical specific capacity level.
[0009] The present invention aims to solve the above-described problems and provide a lithium-sulfur battery having a high specific capacity at the theoretical specific capacity level.
[0010] In addition, the present invention seeks to provide a lithium-sulfur battery with high energy density.
[0011] To achieve the above purpose,
[0012] According to one aspect of the present invention, lithium-sulfur batteries of the following embodiments are provided.
[0013] A lithium-sulfur battery according to the first embodiment,
[0014] A lithium sulfur battery comprising a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, comprising:
[0015] The content ratio of sulfur element (S) according to the following formula 1 (R) SL ) is less than 15%.
[0016] [Formula 1]
[0017] R SL (%) = W SE / W SP X 100
[0018] In the above equation 1,
[0019] W SE is the weight of elemental sulfur (S) among the sulfur compounds present in the electrolyte,
[0020] W SP is the weight of elemental sulfur (S) among the sulfur compounds present in the above anode.
[0021] According to the second embodiment, in the first embodiment,
[0022] In the above equation 1, W SE and W SP may represent values measured at a discharge state of 1.7 V to 1.9 V, respectively.
[0023] According to the third embodiment, in the first embodiment or the second embodiment,
[0024] The sulfur compounds present in the above electrolyte are inorganic sulfur (S8), lithium polysulfide (Li2S) x , 1 ≤ x ≤ 8) or a mixture thereof.
[0025] According to the fourth embodiment, in any one of the first to third embodiments,
[0026] The sulfur compound present in the above anode may include inorganic sulfur (S8).
[0027] According to the fifth embodiment, in any one of the first to fourth embodiments,
[0028] Above W SE It may be 15 wt% or less based on the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery.
[0029] According to the sixth embodiment, in any one of the first to fifth embodiments,
[0030] Above W SP It may be 65 wt% or more based on the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery.
[0031] According to the seventh embodiment, in any one of the first to sixth embodiments,
[0032] Above W SP It may be 75.5 wt% or more based on the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery.
[0033] According to the eighth embodiment, in any one of the first to seventh embodiments,
[0034] The above lithium-sulfur battery may satisfy the following equation 2.
[0035] [Formula 2]
[0036] W' SP > 1.2 XW' SE + 56.86
[0037] In the above equation 2,
[0038] W' SEis the weight % of elemental sulfur (S) among the sulfur compounds present in the electrolyte, based on the total weight of elemental sulfur (S) among the sulfur compounds contained in the lithium-sulfur battery.
[0039] W' SP is the weight percentage of elemental sulfur (S) among the sulfur compounds present in the positive electrode, based on the total weight of elemental sulfur (S) among the sulfur compounds contained in the lithium-sulfur battery.
[0040] According to the ninth embodiment, in any one of the first to eighth embodiments,
[0041] The above lithium-sulfur battery may satisfy the following equation 3.
[0042] [Formula 3]
[0043] 10.667 XR S / C - 10.633 > R SL
[0044] In the above equation 3,
[0045] The above R SL is the content ratio of sulfur element (S) according to the above formula 1,
[0046] The above R S / C is the weight ratio of sulfur (S) and carbon (C) in the above sulfur-carbon complex.
[0047] According to the tenth embodiment, in any one of the first to ninth embodiments,
[0048] The above sulfur-carbon complex may have a sulfur / carbon weight ratio (S / C weight ratio) of 2.5 g / g or less.
[0049] According to the eleventh embodiment, in any one of the first to tenth embodiments,
[0050] The positive electrode comprises a current collector and a positive electrode active material layer including the sulfur-carbon complex,
[0051] The weight of the sulfur-carbon complex may be 80 wt% or more based on the total weight of the positive electrode active material layer.
[0052] According to the 12th embodiment, in any one of the 1st to 11th embodiments,
[0053] The weight ratio of sulfur in the electrolyte and the sulfur-carbon complex (El / S weight ratio) may be 3.5 g / g or less.
[0054] According to the 13th embodiment, in any one of the first to twelfth embodiments,
[0055] The above electrolyte may include an acyclic ether, a cyclic ether, or a mixture thereof.
[0056] According to the 14th embodiment, in any one of the first to 13th embodiments,
[0057] The above electrolyte may include a mixture of the acyclic ether and the cyclic ether, and the volume ratio of the acyclic ether and the cyclic ether may be 5:95 to 95:5 (v / v).
[0058] According to the 15th embodiment, in any one of the 1st to 14th embodiments,
[0059] It may have a specific capacity of 60% or more compared to the theoretical specific capacity calculated from the total content of sulfur compounds contained in the lithium-sulfur battery.
[0060] According to the 16th embodiment, in any one of the first to fifteenth embodiments,
[0061] The above sulfur compound may include inorganic sulfur (S8), lithium (poly)sulfide (Li2Sx, 1 ≤ x ≤ 8), or a mixture of two or more thereof.
[0062] According to the 17th embodiment, in any one of the first to sixteenth embodiments,
[0063] The specific capacity of the above lithium-sulfur battery may be 1,000 mAh / g or more.
[0064] According to the 18th embodiment, in any one of the first to seventeenth embodiments,
[0065] The energy density of the above lithium-sulfur battery may be 300 Wh / kg or more.
[0066] According to the 19th embodiment, in any one of the 1st to 18th embodiments,
[0067] The above lithium-sulfur battery may be a coin-type battery, a pouch-type battery, or a cylindrical battery.
[0068]
[0069] According to another aspect of the present invention, a method for evaluating the specific capacity of a lithium-sulfur battery of the following embodiments is provided.
[0070] A method for evaluating the specific capacity of a lithium-sulfur battery according to the 20th embodiment,
[0071] A method for evaluating the specific capacity of a lithium-sulfur battery comprising a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte comprising a sulfur-carbon complex,
[0072] At least one of the above cathode and the above electrolyte comprises a sulfur compound,
[0073] The content ratio of sulfur element (S) according to the following formula 1 (R) SL ) includes a step of determining a lithium-sulfur battery having a specific capacity of 15% or less as a high-specific-capacity battery.
[0074] [Formula 1]
[0075] R SL (%) = W SE / W SP X 100
[0076] In the above equation 1,
[0077] W SE is the weight of elemental sulfur (S) among the sulfur compounds present in the electrolyte,
[0078] W SP is the weight of elemental sulfur (S) among the sulfur compounds present in the above anode.
[0079] According to the 21st embodiment, in the 20th embodiment,
[0080] The high capacity battery may be a battery having a specific capacity of 1,000 mAh / g or more.
[0081] According to one aspect, the lithium-sulfur battery of the present invention has an advantage of being able to have a specific capacity at the level of theoretical specific capacity.
[0082] In particular, the lithium-sulfur battery of the present invention can have a specific capacity of 1,000 mAh / g or more.
[0083] According to one aspect, the lithium-sulfur battery of the present invention has the advantage of having a high energy density.
[0084] In particular, the lithium-sulfur battery of the present invention can have an energy density of 300 Wh / kg or more.
[0085] Hereinafter, the present invention will be described in more detail.
[0086] Throughout this specification, whenever a part is said to "include," "comprise," "have," or "have" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise stated.
[0087] In addition, the terms "about", "substantially", etc. used throughout this specification are used in the sense of numerical values or near numerical values when manufacturing and material tolerances inherent to the meanings stated are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that mention exact or absolute values to aid understanding of this specification.
[0088] Throughout this specification, references to 'A and / or B' mean 'A or B or both.'
[0089] The term "composite" used in this specification refers to a material in which two or more materials are combined to form physically and chemically different phases and exhibit more effective functions.
[0090] The term "(poly)sulfide" as used herein means "(poly)sulfide ion (S x 2- , 1≤ x ≤8)" and "lithium (poly)sulfide (Li2S x or Li2S x - , 1≤ x ≤8)" is a concept that includes all of them.
[0091] In this specification, the term "polysulfide" means "polysulfide ion (S x 2- , 1< x ≤8)" and "lithium polysulfide (Li2S x or Li2S x - , 1< x ≤8)" is a concept that includes all of them.
[0092] The unit used in this specification is "mAh / g s " is intended to indicate capacity per weight of sulfur (S) unless otherwise specified, and may be used interchangeably with other expressions such as mAh / g(s), mAh / gs, etc.
[0093] The unit "mg" used in this specification s / cm2 " is intended to represent the weight of sulfur (S) per unit area, unless otherwise stated, mg(s) / cm 2 , may be used interchangeably with other expressions such as mAh / gs.
[0094] Lithium-sulfur batteries have a problem in that lithium polysulfide, which is formed by the reduction reaction of sulfur (S8) at the positive electrode during charging and discharging, is eluted from the positive electrode into the electrolyte, and as a result, the capacity of the battery does not represent the theoretical capacity.
[0095] According to one aspect of the present invention, a lithium-sulfur battery having a high capacity, specifically a high specific capacity, is provided.
[0096]
[0097] A lithium-sulfur battery according to one aspect of the present invention comprises a positive electrode comprising a sulfur-carbon composite, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.
[0098] In one embodiment of the present invention, specifically, the lithium-sulfur battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, including the sulfur-carbon complex; the electrolyte; and a case in which the electrode assembly is housed.
[0099] At this time, the lithium-sulfur battery has a content ratio (R) of sulfur element (S) according to the following formula 1 SL ) is less than 15%.
[0100] [Formula 1]
[0101] R SL (%) = W SE / W SP X 100
[0102] In the above equation 1,
[0103] W SE is the weight of elemental sulfur (S) among the sulfur compounds present in the electrolyte,
[0104] W SPis the weight of elemental sulfur (S) among the sulfur compounds present in the above anode.
[0105]
[0106] As described above, lithium-sulfur batteries contain inorganic sulfur (S8) as a positive electrode active material. Within the lithium-sulfur battery, lithium (poly)sulfide is formed through a reduction reaction at the positive electrode during discharge. If the formed lithium (poly)sulfide is dissolved by the electrolyte and eluted from the positive electrode into the electrolyte phase, the amount of lithium (poly)sulfide oxidized at the positive electrode during charging of the lithium-sulfur battery decreases, which may ultimately result in a decrease in the capacity of the lithium-sulfur battery.
[0107] The inventors of the present invention have found that R according to the above-described formula 1 SL It was found that lithium-sulfur batteries with a value of 15% or less can exhibit high capacity. That is, when the active material present in the electrolyte compared to the active material present in the positive electrode of a lithium-sulfur battery is maintained below a certain standard, there is a favorable effect in realizing high capacity, and in order to quantify this, the weight ratio of sulfur element (S) among the sulfur compounds present in the positive electrode (W SP ) The weight ratio of sulfur element (S) among sulfur compounds present in the electrolyte (W SE ) as the above R SL was newly defined.
[0108] With reference to this mechanism, in the present specification, a substance containing elemental sulfur (S) derived from the positive electrode active material of the lithium-sulfur battery is collectively referred to as a "sulfur-based compound." The sulfur-based compound may include, for example, all sulfur-containing compounds that can be formed through a reduction reaction of inorganic sulfur (S8) or an oxidation reaction of lithium sulfide (Li2S), and more specifically, inorganic sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤ 8), disulfide compounds, and carbon-sulfur polymers ((C2S y ) n, y = 2.5 to 50, n ≥ 2), or two or more of these.
[0109] In one embodiment of the present invention, for the convenience of description, the lithium sulfide (Li2S) may be described as being included in lithium (poly)sulfide (Li2Sx, x=1), and at this time, the lithium (poly)sulfide may be expressed by the chemical formula of Li2Sx, 1 ≤ x ≤ 8. Accordingly, in one embodiment of the present invention, the sulfur-based compound may include, for example, inorganic sulfur (S8), lithium (poly)sulfide (Li2Sx, 1 ≤ x ≤ 8), or two or more thereof.
[0110] According to one aspect of the present invention, a new ratio of the amount of elemental sulfur (S) present in an electrolyte to the amount of elemental sulfur (S) present in a cathode of a lithium-sulfur battery capable of exhibiting a high specific capacity is proposed.
[0111] Specifically, according to one aspect of the present invention, the content ratio (R) of sulfur element (S) according to the above formula 1 SL ) is provided, a lithium-sulfur battery having a charge / discharge ratio of 15% or less.
[0112] The above R SL represents the ratio of the weight of elemental sulfur (S) among sulfur compounds present in the electrolyte to the weight of elemental sulfur (S) among sulfur compounds present in the positive electrode of a lithium-sulfur battery. Specifically, R according to the following formula 1 SL A lithium-sulfur battery is provided that achieves high capacity by controlling the charge / discharge ratio to less than 15%.
[0113] [Formula 1]
[0114] R SL (%) = W SE / W SP X 100
[0115] In the above equation 1,
[0116] W SE is the weight of elemental sulfur (S) among the sulfur compounds present in the electrolyte,
[0117] W SP is the weight of elemental sulfur (S) among the sulfur compounds present in the above anode.
[0118]
[0119] In one embodiment of the present invention, a lithium-sulfur battery having a high specific capacity has the R regardless of the charge / discharge state. SL It may be less than 15%. However, since it is desirable to control the rate at which lithium (poly)sulfide formed at the positive electrode when the lithium-sulfur battery is discharged is dissolved into the electrolyte and lost from the positive electrode, the R SL may represent less than 15% in the discharged state of a lithium-sulfur battery.
[0120] In another embodiment of the present invention, the lithium-sulfur battery having the high specific capacity comprises the R SL It may represent 14% or less, 13% or less, or 12% or less. The above R SL The lower limit is not particularly limited, as the smaller the R, the higher the capacity of the lithium-sulfur battery. For example, the above R SL may represent a value of 0.5% or more, 1% or more, 3% or more, 5% or more, 7% or more, or 10% or more within a range satisfying the above-described range. In another example, the R SL may be 0.5% to 15%, 1% to 14%, 2% to 13%, 3% to 12%, 4% to 12.5% or 5% to 12%, but the present invention is not limited thereto.
[0121] Next, the above R SL We will explain the measurement method.
[0122] In one embodiment of the present invention, the R SL can be measured when the lithium-sulfur battery is discharged to 1.7 V to 1.9 V, for example, to 1.8 V.
[0123] Specifically, the above R SL The discharge state of a lithium-sulfur battery, for example, a lithium-sulfur battery discharged to 1.7 V to 1.9 V, specifically 1.8 V, can be measured by disassembling the battery and measuring the ratio of the weight of sulfur (S) derived from the sulfur-based compound present in the electrolyte to the weight of sulfur (S) derived from the sulfur-based compound present on the positive electrode.
[0124] In the above formula 1, the weight of elemental sulfur (S) present in the sulfur compound present in the electrolyte is 'W SE ', and the weight of sulfur element (S) present in the sulfur compound present in the above anode is 'W SP ' is said.
[0125] In one embodiment of the present invention, the W SE and W SP Each of these can be measured by disassembling a lithium-sulfur battery in a discharged state, for example, a state discharged to 1.7 V to 1.9 V, specifically to 1.8 V, as described above.
[0126] In one embodiment of the present invention, the sulfur compound present in the electrolyte of the lithium-sulfur battery may be derived from being eluted from the positive electrode during operation of the lithium-sulfur battery, and such sulfur compound may be, for example, inorganic sulfur (S8), lithium (poly)sulfide (Li2S). x , 1 ≤ x ≤ 8) or a mixture thereof. Preferably, the sulfur compound present in the electrolyte is a material that can be dissolved by the electrolyte of the lithium-sulfur battery, such as lithium polysulfide (Li2S). x , 1 < x ≤8) can be included.
[0127] In one embodiment of the present invention, the W SE Inorganic sulfur (S8), lithium (poly)sulfide (Li2S) present in the above electrolyte x, 1 ≤ x ≤ 8) or a mixture thereof. Preferably, the W SE is lithium polysulfide (Li2S) present in the above electrolyte. x , 1 < x ≤ 8) may be the total weight. More preferably, the W SE is lithium polysulfide (Li2S) present in the above electrolyte. x , 2 < x ≤8) total weight, more preferably lithium polysulfide (Li2S x , 3 ≤ x ≤ 4) can be the total weight.
[0128] Above W SE The content of elemental sulfur (S) in the sulfur compound dissolved in the electrolyte of a lithium-sulfur battery can be measured according to a known method, or can be measured according to a newly developed method, and the measurement method is not particularly limited.
[0129] According to one embodiment of the present invention, the W SE can be measured by the following methods.
[0130] First, the lithium-sulfur battery to be measured is disassembled to separate the positive electrode / separator / negative electrode, and the separated positive electrode / separator / negative electrode is placed in a container containing a predetermined mass of solvent, respectively, to extract the sulfur-based compound. At this time, the extraction of the sulfur-based compound may be preferably performed for, for example, 20 minutes or more, specifically 20 minutes. After extraction, the solution may be stored in a glove box. Accordingly, the extraction solvents of the positive electrode, separator, and negative electrode may be stored separately or combined, and preferably may be stored separately from each other. The remaining positive electrode, separator, and negative electrode are stored in the glove box. The glove box may be filled with an inert gas, for example, nitrogen or argon gas.
[0131] In one embodiment of the present invention, the extraction solvent may be, for example, dimethoxyethane, a derivatizing reagent is added thereto, vortexing is performed, and then the extracts from each electrode are added thereto, followed by voltammetry and analysis using HPLC. Generally, the derivatized lithium (poly)sulfide (LiPS) is short chain LiPS (Me2S 3~4 ) and / or long-chain LiPS (Me2S 5~8 ) can exist. The data analyzed using HPLC are separated into derivatized LiPS and inorganic sulfur (S8), and quantitative analysis is performed using a calibration curve for each concentration of short-chain LiPS and inorganic sulfur with a standard. For long-chain LiPS, a sample obtained through preparative work is quantitatively analyzed, and the concentration of the original solution is calculated using the dilution ratio.
[0132] At this time, an appropriate extraction solvent can be used for each sulfur compound to be extracted, or a solvent identical in composition to the non-aqueous solvent in the electrolyte can be used. Once the extraction is complete, each solvent is obtained and analyzed to measure the amount of sulfur compounds present in the electrolyte, and by adding these amounts, the weight of elemental sulfur (S) in the electrolyte is calculated.
[0133] As described later, at this time, the positive electrode is dried at room temperature for more than 1 hour, for example, 1 hour, after extraction, and then scraped from the collector, and the weight of sulfur element present in the positive electrode (W) is determined through elemental analysis. SP ) can be calculated.
[0134] The method for extracting a sulfur compound from the separated electrolyte may use, for example, liquid chromatography, but the extraction method is not limited thereto.
[0135] In one embodiment of the present invention, the sulfur compound present in the positive electrode of the lithium-sulfur battery may be a material that is added during the manufacture of the lithium-sulfur battery or formed through an oxidation-reduction reaction during the operation of the lithium-sulfur battery, and the sulfur compound is particularly inorganic sulfur (S8), lithium (poly)sulfide (Li2S). x , 1 ≤ x ≤ 8) or mixtures thereof.
[0136] Specifically, as described below, the above W SP Since the sulfur compound present in the positive electrode is measured by disassembling the lithium sulfur battery after discharging, the sulfur compound present in the positive electrode may include a sulfur compound present in the discharged state of the lithium sulfur battery. Specifically, the sulfur compound present in the positive electrode is lithium (poly)sulfide (Li2S x , 1 ≤ x ≤ 8), specifically lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x < 3), or a mixture thereof. More specifically, the sulfur-based compound present in the positive electrode may include lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤ 2), or a mixture thereof. Even more specifically, the sulfur-based compound present in the positive electrode may include lithium sulfide (Li2S), lithium polysulfide (Li2S2), or a mixture thereof.
[0137] In one embodiment of the present invention, the W SP Inorganic sulfur (S8), lithium (poly)sulfide (Li2S) present in the above anode x , 1 ≤ x ≤ 8) or a mixture thereof. Preferably, the W SP may be the total weight of lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤ 2) or a mixture thereof present in the positive electrode. More preferably, the W SPmay be the total weight of lithium sulfide (Li2S), lithium polysulfide (Li2S2) or a mixture thereof present in the above positive electrode.
[0138] Above W SP The content of elemental sulfur (S) among sulfur compounds present in the positive electrode of a lithium-sulfur battery can be measured according to a known method, or can be measured according to a newly developed method, and the measurement method is not particularly limited.
[0139] In one embodiment of the present invention, the W SP The positive electrode after the above decomposition / drying can be obtained by scraping it from the current collector and performing elemental analysis on the powder. In one embodiment of the present invention, analysis can be performed using a sample in which multiple electrodes are scraped from the current collector to remove sample non-uniformity. For example, the sample is analyzed by an elemental analyzer that introduces a pyrolysis method, and a component corresponding to inorganic sulfur (S8) can be analyzed through the analysis method. The method for analyzing the content of the inorganic sulfur (S8) is not particularly limited to specific means and methods, as long as it is a method of analyzing by excluding components that form compounds with sulfur (S) other than inorganic sulfur (S8) present in the positive electrode. At this time, the analysis method must be able to analyze the content of elemental sulfur (S) for all components other than sulfur (S), and is based on the weight% content of elemental sulfur (S) that forms a mass balance with all analyzed components.
[0140] In one embodiment of the present invention, the W SP is the above W SE As described above in the measurement method, the lithium-sulfur battery to be measured is disassembled to separate the positive electrode / separator / negative electrode, the sulfur compound present in the electrolyte is extracted from the separated positive electrode, and then the active material layer on the current collector is scraped off from the current collector, and the powder is subjected to elemental analysis to be measured.
[0141] Therefore, in one embodiment, the weight of sulfur present at the anode (W SP ) can represent the weight of unextracted sulfur (S) using a solvent that extracts sulfur compounds to measure the weight of sulfur in the electrolyte as described above. That is, the weight of sulfur present in the anode (W SP ) may mean a sulfur compound that is not extracted from a solvent for more than 20 minutes, preferably within 20 minutes. After more than 1 hour, preferably after 1 hour, the current collector is completely scraped from the dried positive electrode to obtain sulfur (S) that can be included in the mixture from the positive electrode, and the weight of the mixture containing the sulfur (S) thus obtained is measured, and an elemental analysis is performed to obtain the weight (W) of sulfur present in the positive electrode. SP ) is obtained. Therefore, in one embodiment, the weight of sulfur present in the anode (W SP ) can be based on lithium-sulfur batteries.
[0142] In another embodiment, the sulfur (S) content in the negative electrode can be measured through elemental analysis. Accordingly, by disassembling a lithium-sulfur battery and measuring the weight (W) of sulfur present in the electrolyte SE ) As described above for the method of measuring the weight of sulfur in the negative electrode, after extracting a solvent-extractable sulfur compound from the negative electrode, drying the negative electrode, the weight of sulfur present in the negative electrode can be measured through elemental analysis. The weight of sulfur present in the negative electrode can be about 0, preferably 0, during or immediately after manufacturing a lithium-sulfur battery.
[0143] In another embodiment, the sulfur (S) content in the separator may be about 0, preferably 0, as measured by elemental analysis. To measure the sulfur (S) content in the separator, a lithium-sulfur battery may be first disassembled, and then a sulfur-based compound may be extracted with a solvent for measuring the weight of sulfur in the electrolyte as described above. Then, the separator may be dried, and the sulfur (S) content present in the separator may be measured. In a lithium-sulfur battery, the separator does not chemically react with sulfur (S), particularly sulfur-based compounds, particularly sulfur-based compounds derived from the sulfur-carbon complex of the positive electrode, so that sulfur (S) may not be chemically bound. In addition, sulfur-based compounds that may be present on the separator and / or within the pores of the separator may be completely removed when extracted with a solvent according to the method for measuring elemental sulfur present in the electrolyte as described above.
[0144] In one embodiment of the present invention, elemental analysis may be performed using, for example, ion chromatography (IC) analysis, inductively coupled plasma optical emission spectrometry (ICP-OES) analysis, elemental analyzer (EA) analysis, ONH analysis, etc., but the elemental analysis method is not limited thereto.
[0145] In one embodiment of the present invention, the content of the sulfur compound present in the electrolyte of the lithium-sulfur battery may be measured according to the method described in, for example, Korean Patent Application No. 2021-0188588, but the present invention is not limited thereto.
[0146] In one embodiment of the present invention, the content of the sulfur compound present in the positive electrode of the lithium-sulfur battery may be measured according to the method described in, for example, Korean Patent Application No. 2021-0173961, but the present invention is not limited thereto.
[0147] In one embodiment of the present invention, W measured as above SE and WSP Using the value of R above SL can be derived.
[0148] In one embodiment of the present invention, the W SE and W SP Each value is measured in weight units, converted to the same weight, and then expressed as a ratio R SL can be derived.
[0149] In one embodiment of the present invention, the W SE and W SP Each value may have a different range depending on the size of the lithium-sulfur battery, the amount of sulfur loaded in the cathode, etc.
[0150] However, the above W SE and W SP Each value can be expressed as a weight % based on the weight of total elemental sulfur (S) among the total sulfur compounds contained in the lithium-sulfur battery. Alternatively, it can be expressed as a weight % based on the weight of total elemental sulfur (S) derived from the sulfur compounds introduced as a positive electrode active material during the manufacture of the lithium-sulfur battery. This is referred to as W' in this specification. SE and W' SP You could say that.
[0151] That is, depending on the measurement method, the above W' SE and W' SP The content ratio of sulfur element (S) (R') according to the following equation 1-2 using the value SL ) can be measured. However, in the following equation 1-2, W' SE and W' SP Since the 'value of total sulfur element (S) among total sulfur compounds contained in lithium-sulfur battery', which serves as the standard for the weight %, is the same, R' according to Equation 1-2 SL The value is R according to Equation 1 SL It is self-evident that it has the same value as the value.
[0152] [Formula 1-2]
[0153] R' SL(%) = W' SE / W' SP X 100
[0154] In the above equation 1-2,
[0155] W' SE is the weight % of elemental sulfur (S) among the sulfur compounds present in the electrolyte, based on the weight of elemental sulfur (S) among the sulfur compounds present in the lithium-sulfur battery,
[0156] W' SP is the weight % of elemental sulfur (S) among the sulfur compounds present in the positive electrode, based on the weight of elemental sulfur (S) among the sulfur compounds present in the lithium-sulfur battery.
[0157] In one embodiment of the present invention, the sulfur element among the sulfur compounds present in the lithium-sulfur battery in Equation 1-2 can be measured by calculating the content of the total sulfur element (S) among the sulfur compounds introduced as a positive electrode active material in the manufacturing step of the lithium-sulfur battery.
[0158] In another embodiment of the present invention, when the content of the sulfur compound introduced as a positive electrode active material in the manufacturing step of the lithium-sulfur battery is not known, the lithium-sulfur battery is decomposed and inorganic sulfur (S8) and lithium (poly)sulfide (Li2S) are extracted according to the method described above. x , 1≤x≤8) can be measured by measuring the content of each and calculating the content of total sulfur element (S) calculated from them.
[0159] In one embodiment of the present invention, the W' SE may be 15 wt% or less based on the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery. For example, the W' SEThe amount of sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery may be, but is not limited to, 0.1 wt% to 15 wt%, 1 wt% to 15 wt%, 1 wt% to 10 wt%, 2 wt% to 9.5 wt%, 3 wt% to 9.5 wt%, 5 wt% to 9.5 wt%, or 7 wt% to 9 wt%, based on the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery.
[0160] In one embodiment of the present invention, the W' SP may be 65 wt% or more based on the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery. In another embodiment of the present invention, the W' SP may be 75 wt% or more, or 75.5 wt% or more, based on the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery. For example, the W SP The total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery may be, but is not limited to, 65 wt% to 99 wt%, 70 wt% to 98 wt%, 75 wt% to 95 wt%, 75 wt% to 90 wt%, 75 wt% to 85 wt%, 75 wt% to 80 wt%, or 75.5 wt% to 80 wt%, based on the weight of the total sulfur element (S).
[0161] In one embodiment of the present invention, the W' SE and the above W' SP may have a value satisfying the following equation 2.
[0162] [Formula 2]
[0163] W' SP > 1.2 XW' SE + 56.86
[0164] In the above equation 2,
[0165] W' SEis the weight % of elemental sulfur (S) among the sulfur compounds present in the electrolyte, based on the total weight of elemental sulfur (S) among the sulfur compounds contained in the lithium-sulfur battery.
[0166] W' SP is the weight percentage of elemental sulfur (S) among the sulfur compounds present in the positive electrode, based on the total weight of elemental sulfur (S) among the sulfur compounds contained in the lithium-sulfur battery.
[0167] In one embodiment of the present invention, when the lithium-sulfur battery satisfies the above formula 2, the lithium-sulfur battery may exhibit further improved effects in terms of specific capacity and energy density, but the present invention is not limited thereto.
[0168] In one embodiment of the present invention, the W' SE and W' SP Each of the above W SE and W SP As described above with respect to the measurement method, it can be measured based on a lithium-sulfur battery in a discharged state. For example, it can be measured by disassembling a lithium-sulfur battery discharged to 1.7 V to 1.9 V, for example, 1.8 V.
[0169] In one embodiment of the present invention, as described above, the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery may refer to the weight of sulfur element (S) contained in the positive electrode, negative electrode, electrolyte, and separator components of the lithium-sulfur battery.
[0170] In one embodiment of the present invention, the weight of total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery can be measured by separating each of the positive electrode, negative electrode, electrolyte, and separator contained in the lithium-sulfur battery, extracting the sulfur compound present in each of the positive electrode, negative electrode, electrolyte, and separator, measuring the content of sulfur element present in the extracted sulfur compound, and adding up the measured contents.
[0171] In another embodiment of the present invention, the total sulfur element (S) contained in the lithium-sulfur battery may preferably be derived from a sulfur-based compound used as a positive electrode active material during the manufacture of the lithium-sulfur battery. Accordingly, the weight of the total sulfur element (S) present in the sulfur-based compound contained in the lithium-sulfur battery may be consistent with the content of sulfur element (S) in the sulfur-based compound added to the positive electrode during or immediately after the manufacture of the lithium-sulfur battery.
[0172] In one embodiment of the present invention, the weight of the total sulfur element (S) contained in the lithium-sulfur battery may represent the sum of the contents of inorganic sulfur (S8) present in each of the positive electrode, negative electrode, electrolyte, and separator included in the lithium-sulfur battery and sulfur element (S) contained in lithium (poly)sulfide (Li2Sx, 1 ≤ x ≤ 8).
[0173] In one embodiment of the present invention, the weight of total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery may represent the weight of sulfur element (S) calculated from the content of inorganic sulfur (S8) added as a positive electrode active material during the manufacture of the lithium-sulfur battery.
[0174] In one embodiment of the present invention, the R SL It may be measured immediately after the manufacture of the lithium-sulfur battery, but it may also be measured based on a battery that has deteriorated after one or more charge / discharge cycles, and R according to the above formula 1 SL Since lithium-sulfur batteries with a value of 15% or less can exhibit excellent effects in terms of specific capacity and / or energy density, there is no particular limitation on the measurement period.
[0175] As described above, the above W SE and W SPis derived from the sulfur-based material introduced as a positive electrode active material during the manufacture of a lithium-sulfur battery. For example, it is derived from a sulfur-carbon complex within the positive electrode. Specifically, it is not derived from a sulfur-based salt introduced as a lithium salt or other additive to the electrolyte during the manufacture of the lithium-sulfur battery. More specifically, according to the above-described measuring method, the content of sulfur element derived from the sulfur-based material derived from the positive electrode, rather than the content of sulfur element derived from the sulfur-based salt contained in the lithium salt or other additive, can be measured.
[0176] More specifically, the above sulfur-based salts represent, for example, CF3SO3, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (C2F5SO2)2NLi, (SO2F)2NLi, (CF3SO2)3CLi, and especially (CF3SO2)2NLi (LiTFSI), which are sulfur-based materials (inorganic sulfur (S8), lithium polysulfide (Li2S)) described above. x , 1≤x≤8) etc.) should be distinguished from.
[0177]
[0178] Next, each component of the lithium-sulfur battery will be described in detail.
[0179] anode
[0180] In one embodiment of the present invention, the positive electrode may include a positive electrode current collector and a positive electrode active material layer applied to one or both surfaces of the positive electrode current collector.
[0181] The above-mentioned positive electrode current collector supports the positive electrode active material and is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, palladium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, silver, etc., aluminum-cadmium alloy, etc. can be used.
[0182] The above positive electrode current collector can form fine irregularities on its surface to strengthen the bonding strength with the positive electrode active material, and can be used in various forms such as a film, sheet, foil, mesh, net, porous body, foam, and non-woven fabric.
[0183] The above positive electrode active material layer includes a positive electrode active material and may further include a conductive material, a binder, and additives.
[0184] In one embodiment of the present invention, the positive electrode active material comprises a sulfur-carbon complex.
[0185] In one embodiment of the present invention, the sulfur-carbon composite may include a porous carbon material; and a sulfur-based compound supported on at least one of the inside of the pores of the porous carbon material and the outer surface of the porous carbon material. In the case of sulfur acting as the positive electrode active material, since it does not have electrical conductivity alone, it is used in a composite with a conductive material such as a carbon material, and a porous carbon material may be used to support sulfur. In addition, the sulfur-based compound is added as the positive electrode active material, and for example, inorganic sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤ 8), a disulfide compound, a carbon-sulfur polymer ((C2S) y ) n , y = 2.5 to 50, n ≥ 2), or two or more of these. Preferably, the sulfur compound may be inorganic sulfur (S8).
[0186] In one embodiment of the present invention, the porous carbon material is used to support a sulfur-based compound as a positive electrode active material, and to provide a framework in which the sulfur-based compound can be uniformly and stably fixed, while improving the conductivity of the positive electrode. Any porous carbon material can be used without particular limitation in its type.
[0187] The above porous carbon material can generally be manufactured by carbonizing precursors of various carbon materials. The porous carbon material includes pores that are not regular therein, and the average diameter of the pores ranges from 1 to 200 nm, and the porosity can range from 10 to 90 volume% of the total volume of the porous carbon material. If the average diameter of the pores is less than the above range, the pore size is only at the molecular level, making sulfur impregnation impossible. Conversely, if it exceeds the above range, the mechanical strength of the porous carbon material is weakened, making it undesirable for application to the electrode manufacturing process.
[0188] In one embodiment of the present invention, the 'average pore diameter' can be measured according to a method known in the art for measuring the pore diameter of a porous material, and the measuring method is not particularly limited. For example, the pore diameter can be measured according to a scanning electron microscope (SEM), a field emission electron microscope (laser diffraction method), a laser diffraction method, or the BET (Brunauer-Emmett-Teller) method. The measurement using the laser diffraction method can be, for example, using a commercially available laser diffraction particle size measuring device (for example, Microtrac MT 3000). In addition, the measurement according to the BET method can be, for example, using an analyzer of the BELSORP series of BEL Japan, but is not limited thereto.
[0189] In one embodiment of the present invention, the 'porosity' refers to the ratio of the volume occupied by pores to the total volume of a structure, and uses % as its unit, and can be used interchangeably with terms such as porosity and porosity. In the present invention, the measurement of the porosity is not particularly limited, and according to one embodiment of the present invention, for example, it can be measured according to the BET method using nitrogen gas or the mercury penetration method (Hg porosimeter) and ASTM D2873.
[0190] The shape of the above porous carbon material may be spherical, rod-shaped, needle-shaped, plate-shaped, tubular or bulk-shaped, and can be used without limitation as long as it is a shape commonly used in lithium-sulfur batteries.
[0191] The porous carbon material may be any material commonly used in the art that has a porous structure or a high specific surface area. For example, the porous carbon material may be at least one selected from the group consisting of graphite; graphene; carbon black such as Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and summer black; carbon nanotubes (CNTs) such as single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs); carbon fibers such as graphite nanofibers (GNFs), carbon nanofibers (CNFs), and activated carbon fibers (ACFs); and graphite and activated carbon such as natural graphite, artificial graphite, and expanded graphite, but is not limited thereto. Preferably, the porous carbon material may be a carbon nanotube.
[0192] In one embodiment of the present invention, the porous carbon material may include, for example, carbon nanotubes (CNTs).
[0193] In one embodiment of the present invention, the sulfur-carbon complex may have a sulfur / carbon weight ratio (S / C weight ratio) of, for example, 5 g / g or less, and more specifically, 2.5 g / g or less. For example, the sulfur-carbon complex may have a sulfur / carbon weight ratio of 2.4 g / g. When the S / C ratio of the sulfur-carbon complex is within the above-described range, it may be preferable in terms of securing the electron transfer ability (conductivity) and electrochemical specific surface area of the sulfur-carbon complex, and for example, it may be preferable in suppressing the elution of sulfur from the anode by increasing the usable surface area of the sulfur-carbon complex, but the present invention is not limited thereto.
[0194] In one embodiment of the present invention, the S / C ratio can be calculated from the weight (g) of sulfur and the weight (g) of carbon present in the sulfur-carbon complex. Alternatively, it can be calculated from the weight (wt%) of sulfur and the weight (wt%) of carbon based on the total weight of the sulfur-carbon complex. As such, the S / C ratio can be a unitless value.
[0195] In one embodiment of the present invention, the S / C weight ratio may have a value of, for example, 0.5 to 2.5, 1.0 to 2.50, 1.5 to 2.45, 2.0 to 2.45, or 2.35 to 2.45. For example, the S / C ratio may be calculated from the weight ratio of the inorganic sulfur (S8) to the weight ratio of the porous carbon material. For example, the S / C ratio may be calculated from the weight ratio of S8 / CNT.
[0196] The method for manufacturing the above sulfur-carbon composite is not particularly limited in the present invention, and any method commonly used in the art may be used. For example, a method may be used in which the sulfur and porous carbon material are simply mixed and then heat-treated to form a composite.
[0197] In addition to the composition described above, the positive electrode active material may further include one or more selected from among a transition metal element, a group ⅢA element, a group ⅣA element, a sulfur compound of these elements, and an alloy of these elements and sulfur.
[0198] The above transition metal elements include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Os, Ir, Pt, Au or Hg, etc., the above group 13 elements include Al, Ga, In, Ti, etc., and the above group 14 elements may include Ge, Sn, Pb, etc.
[0199] In one embodiment of the present invention, the S / C ratio of the sulfur-carbon complex is SL In relation to the value, it may satisfy the following equation 3.
[0200] [Formula 3]
[0201] 10.667 XR S / C - 10.633 > R SL
[0202] In the above equation 3,
[0203] The above R SL is the content ratio of sulfur element (S) according to the above formula 1,
[0204] The above R S / C is the weight ratio of sulfur (S) and carbon (C) in the above sulfur-carbon complex.
[0205] The inventors of the present invention have confirmed that when a lithium-sulfur battery satisfies the above formula 3, the specific capacity and / or energy density can be significantly improved.
[0206] In one embodiment of the present invention, the sulfur-carbon composite may be at least 50 wt% based on the total weight of the positive electrode. Specifically, when the positive electrode may include a current collector and a positive electrode active material layer formed on the current collector, and the sulfur-carbon composite is included in the positive electrode active material layer, the sulfur-carbon composite may be at least 80 wt%, at least 90 wt%, or at least 95 wt% based on the total weight of the positive electrode active material layer. Specifically, the sulfur-carbon composite may be included in an amount of 80 wt% to 100 wt%, more specifically 85 wt% to 99 wt%, 90 wt% to 100 wt%, 90 wt% to 99 wt%, 95 wt% to 98 wt%, or 95 wt% to 97 wt%, or 96 wt% based on the total weight of the positive electrode active material layer. If the content of the above sulfur-carbon complex is below the above range, the relative content of auxiliary materials such as conductive material and binder increases and the content of the sulfur-carbon complex decreases, making it difficult to implement a high-capacity, high-energy-density battery. Conversely, if it exceeds the above range, the content of the conductive material or binder described below is relatively insufficient, causing a problem in that the physical properties of the electrode deteriorate.
[0207] In one embodiment of the present invention, the loading amount of the positive electrode is, for example, 1.67 mg s / cm 2 Above, specifically 1.67 to 2.92 mg s / cm 2 , more specifically 1.67 to 2.08 mg s / cm 2 The above loading amount can be calculated from the content of the active material in the positive electrode and the content of sulfur (S) in the active material.
[0208] In one embodiment of the present invention, when the loading amount of the positive electrode is converted into capacity, for example, the loading amount is 2.0 mAh / cm 2 Above, specifically 2.0 mAh / cm2 3.5 mAh / cm 2 , more specifically 2.0 mAh / cm 2 2.5 mAh / cm 2 However, the present invention is not limited thereto.
[0209] The above conductive material is a material that electrically connects the electrolyte and the positive electrode active material and serves as a path for electrons to move from the current collector to the positive electrode active material. Any conductive material that is physically distinct from the carbon contained in the sulfur-carbon complex and is a component of the electrode can be used without limitation.
[0210] In one embodiment of the present invention, the conductive material may be, for example, carbon black such as Super-P, Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, carbon black; carbon derivatives such as carbon nanotubes or fullerene; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorocarbon, aluminum, and nickel powder; or conductive polymers such as polyaniline, polythiophene, polyacetylene, and polypyrrole, which may be used alone or in combination.
[0211] In one embodiment of the present invention, the content of the conductive material may be 0 to 10 wt%, for example, 1 to 10 wt%, based on the total weight of the positive electrode active material. If the content of the conductive material is less than the above range, electron transfer between the positive electrode active material and the current collector is not easy, resulting in a decrease in voltage and capacity. Conversely, if the content exceeds the above range, the proportion of the positive electrode active material may relatively decrease, thereby reducing the total energy (charge) of the battery. Therefore, it is preferable to determine an appropriate content within the above-described range.
[0212] In one embodiment of the present invention, the binder maintains the positive electrode active material on the positive electrode current collector and organically connects the positive electrode active materials to further increase the bonding strength between them, and any binder known in the art can be used.
[0213] For example, the binder may be a fluororesin binder including polyvinylidene fluoride (PVdF), a polyvinylidene fluoride polymer including at least one vinylidene fluoride as a repeating unit, polytetrafluoroethylene (PTFE), or a mixture of two or more thereof; a rubber binder including styrene butadiene rubber (SBR), acrylonitrile-butidiene rubber, or styrene-isoprene rubber; an acrylic binder; a cellulose binder including carboxyl methyl cellulose (CMC), starch, hydroxy propyl cellulose, or regenerated cellulose; a polyalcohol binder; a polyolefin binder including polyethylene and polypropylene; a polyimide binder; a polyester binder; a silane binder; a polyacrylic acid binder; And a mixture or copolymer of one or more selected from the group consisting of polyacrylonitrile-based binders may be used. In one embodiment of the present invention, the binder may include, for example, polyacrylate (PAA).
[0214] In one embodiment of the present invention, the content of the binder may be 1 to 10 wt% based on the total weight of the positive electrode active material layer. If the content of the binder is less than the above range, the physical properties of the positive electrode may deteriorate, causing the positive electrode active material and conductive material to fall off. If the content of the binder is more than the above range, the ratio of the positive electrode active material and conductive material in the positive electrode may relatively decrease, resulting in a decrease in battery capacity. Therefore, it is preferable to determine an appropriate content within the above-described range.
[0215] In the present invention, the method for manufacturing the positive electrode for the lithium secondary battery is not particularly limited, and various methods known to those skilled in the art or modified methods thereof can be used.
[0216] For example, the positive electrode for the lithium secondary battery may be manufactured by forming the positive electrode active material layer by preparing a positive electrode slurry composition including the composition described above and then applying the same to at least one surface of the positive electrode current collector.
[0217] The above positive electrode slurry composition includes the positive electrode active material described above, and may further include a binder, a conductive material, and a solvent.
[0218] The above solvent is one that can uniformly disperse the positive electrode active material. Water is most preferably an aqueous solvent, and the water may be distilled or deionized water. However, this is not necessarily limited to this, and if necessary, a lower alcohol that is easily mixed with water may be used. Examples of the lower alcohol include methanol, ethanol, propanol, isopropanol, and butanol, and preferably, these can be mixed with water and used.
[0219] The content of the above solvent may be contained at a level that has a concentration that can facilitate coating, and the specific content varies depending on the application method and device.
[0220] The above-mentioned positive electrode slurry composition may additionally contain, as necessary, substances commonly used in the relevant technical field for purposes such as improving its function. Examples thereof include viscosity modifiers, fluidizing agents, and fillers.
[0221] The method for applying the positive electrode slurry composition is not particularly limited in the present invention, and examples thereof include methods such as doctor blade, die casting, comma coating, and screen printing. In addition, the positive electrode slurry may be applied onto the positive electrode current collector by molding it on a separate substrate and then pressing or lamination.
[0222] After the above application, a drying process for solvent removal can be performed. The drying process is performed at a temperature and time that can sufficiently remove the solvent, and the conditions may vary depending on the type of solvent and are therefore not particularly limited to the present invention. Examples include drying using warm air, hot air, low-humidity air, vacuum drying, and drying using irradiation with (far) infrared rays and electron beams. The drying speed is usually adjusted to remove the solvent as quickly as possible within a speed range that does not cause cracks in the positive electrode active material layer due to stress concentration or cause the positive electrode active material layer to peel off from the positive electrode current collector.
[0223] Additionally, the density of the positive electrode active material within the positive electrode can be increased by pressing the entire body after drying. Pressing methods include mold pressing and roll pressing.
[0224] The porosity of the positive electrode manufactured by the composition and manufacturing method described above, specifically, the positive electrode active material layer, may be 50 to 80% by volume, specifically, 60 to 75% by volume. If the porosity of the positive electrode is less than 50% by volume, the filling degree of the positive electrode slurry composition including the positive electrode active material, the conductive agent, and the binder becomes excessively high, so that sufficient electrolyte capable of exhibiting ionic and / or electrical conductivity cannot be maintained between the positive electrode active materials, which may result in a deterioration in the output characteristics or cycle characteristics of the battery, and a serious problem of a decrease in overvoltage and discharge capacity of the battery. On the other hand, if the porosity of the positive electrode exceeds 80% by volume and has excessively high porosity, there is a problem in that the physical and electrical connection with the current collector is lowered, resulting in a decrease in adhesive strength and difficulty in reaction. In addition, the increased porosity may be filled with electrolyte, which may result in a problem in that the energy density of the battery may be lowered, and therefore, the porosity is appropriately controlled within the above range.
[0225]
[0226] cathode
[0227] The negative electrode may include a negative electrode current collector and a negative electrode active material layer applied to one or both surfaces of the negative electrode current collector. Alternatively, the negative electrode may be a lithium metal plate or a lithium foil.
[0228] The above negative electrode current collector is for supporting the negative electrode active material layer, as described in the positive electrode current collector.
[0229] The above-mentioned negative electrode active material layer may include a conductive material, a binder, etc. in addition to the negative electrode active material. In this case, the conductive material and the binder follow the above-mentioned.
[0230] The above negative active material is lithium (Li +) can be reversibly intercalated or deintercalated, a material that can react with lithium ions to form a reversibly lithium-containing compound, or a lithium metal or a lithium alloy.
[0231] The above lithium ion (Li + ) can be reversibly inserted or de-inserted, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The lithium ion (Li + ) can be, for example, tin oxide, titanium nitrate or silicon. The lithium alloy can be, for example, an alloy of lithium (Li) and a metal selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al) and tin (Sn).
[0232] Preferably, the negative active material may be lithium metal, and specifically, may be in the form of a lithium metal thin film or lithium metal powder.
[0233]
[0234] membrane
[0235] The separator separates or insulates the positive and negative electrodes from each other and enables lithium ion transport between the positive and negative electrodes. It may be made of a porous non-conductive or insulating material, and can be used without special restrictions as long as it is commonly used as a separator in a lithium secondary battery. The separator may be an independent member such as a film, or may be a coating layer added to the positive and / or negative electrodes.
[0236] It is preferable that the above separator have low resistance to ion movement of the electrolyte and excellent moisture absorption capacity for the electrolyte.
[0237] In one embodiment of the present invention, the separator may include a porous substrate, and any porous substrate typically used in secondary batteries may be used as the porous substrate, and a porous polymer film may be used alone or in a laminated manner. For example, a nonwoven fabric or a polyolefin porous film made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used, but is not limited thereto.
[0238] The material of the porous substrate is not particularly limited in the present invention, and any porous substrate commonly used in electrochemical devices can be used. For example, the porous substrate may be a polyolefin such as polyethylene, polypropylene, etc., a polyester such as polyethyleneterephthalate, polybutyleneterephthalate, polyamide, polyacetal, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenyleneoxide, polyphenylenesulfide, polyethylenenaphthalate, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, cellulose, nylon, It may include at least one material selected from the group consisting of poly(p-phenylene benzobisoxazole) and polyarylate.
[0239] In one embodiment of the present invention, the thickness of the porous substrate is not particularly limited, but may be 1 to 100 μm, preferably 5 to 50 μm. The thickness range of the porous substrate is not limited to the above-mentioned range, but if the thickness is excessively thinner than the above-mentioned lower limit, the mechanical properties may deteriorate, and the separator may be easily damaged during battery use.
[0240] In one embodiment of the present invention, the average diameter and porosity of the pores present in the porous substrate are not particularly limited, but may be 0.001 to 50 ㎛ and 10 to 95 volume%, respectively.
[0241] In one embodiment of the present invention, the separator may further include a porous coating layer formed on at least one surface of the porous substrate and including inorganic particles and a binder.
[0242] In one embodiment of the present invention, the inorganic particles and binder included in the porous coating layer may be used without particular limitation as long as they are commonly used in the porous coating layer of a separation membrane, and the manufacturing method thereof is also not particularly limited.
[0243]
[0244] electrolyte
[0245] The above electrolyte comprises a non-aqueous solvent as a medium through which ions involved in the electrochemical reaction of a lithium-sulfur battery can move and a lithium salt as an electrolyte.
[0246] The above electrolyte is not particularly limited as long as it has a composition that can be used in a lithium secondary battery, specifically a lithium-sulfur battery.
[0247] In one embodiment of the present invention, the non-aqueous solvent may be used without particular limitation as long as it is of a type that can be used in a lithium-sulfur battery, and for example, ether solvents, esters, amides, linear carbonates, and cyclic carbonates may be used.
[0248] In one embodiment of the present invention, the ester may be, for example, one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, or a mixture of two or more thereof, but is not limited thereto.
[0249] In one embodiment of the present invention, the linear carbonate may be, for example, one selected from the group consisting of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethylmethyl carbonate, methylpropyl carbonate, and ethylpropyl carbonate, or a mixture of two or more thereof, but is not limited thereto.
[0250] In one embodiment of the present invention, the cyclic carbonate is, for example, one selected from the group consisting of ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and halogenides thereof, or a mixture of two or more thereof. Examples of the halogenides thereof include, but are not limited to, fluoroethylene carbonate.
[0251] In one embodiment of the present invention, the non-aqueous solvent may include an ether solvent.
[0252] In one embodiment of the present invention, the ether solvent may be included in an amount of 60% by volume or more, for example, 60% by volume to 100% by volume, 70% by volume to 100% by volume, 80% by volume to 100% by volume, 85% by volume to 100% by volume, 90% by volume to 100% by volume, or 95% by volume to 100% by volume, based on the total volume of the non-aqueous solvent. When the amount of the ether solvent is in the above-described range based on the total volume of the non-aqueous solvent, an advantageous effect may be exhibited in terms of the solubility of the electrolyte composition such as a lithium salt, but the present invention is not limited thereto.
[0253] In one embodiment of the present invention, the ether solvent may include an acyclic ether, a cyclic ether, or a mixture thereof.
[0254] In one embodiment of the present invention, the acyclic ether may include at least one selected from the group consisting of, for example, dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, diisobutyl ether, ethyl methyl ether, ethylpropyl ether, ethyl tertbutyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, dimethoxypropane, diethylene glycol, diethylene glycol diethyl ether, triethylene glycol, tetraethylene glycol, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol dimethylene ether, butylene glycol ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, diethylene glycol butyl methyl ether, diethylene glycol tertbutyl ethyl ether, and ethylene glycol ethyl methyl ether. Preferably, it may include at least one selected from the group consisting of dimethoxyethane, diethoxyethane, diethylene glycol, triethylene glycol and tetraethylene glycol, and more preferably, it may include dimethoxyethane.
[0255] In one embodiment of the present invention, the cyclic ether is, for example, 2-methylfuran, 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, 2,5-dimethoxytetrahydrofuran, 2-ethoxytetrahydrofuran, 2-methyl-1,3-dioxolane, 2-vinyl-1,3-dioxolane, 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, 2-ethyl-2-methyl-1,3-dioxolane, tetrahydropyran, 1,4-dioxane, It may include at least one selected from the group consisting of 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, 1,4-dimethoxybenzene, and isosorbide dimethyl ether. Preferably, it may include at least one selected from the group consisting of 2-methylfuran, 1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, and 2,5-dimethyltetrahydrofuran, and more preferably, it may include 2-methylfuran.
[0256] In one embodiment of the present invention, the non-aqueous solvent may include, for example, dimethoxyethane (DME), ethylene glycol, propylene glycol, or a mixture of two or more thereof.
[0257] In one embodiment of the present invention, the non-aqueous solvent may include a mixture of an acyclic ether and a cyclic ether.
[0258] In one embodiment of the present invention, the non-aqueous solvent may include dimethoxyethane (DME) and 2-methylfuran (2-MeF).
[0259] In one embodiment of the present invention, the volume ratio of the acyclic ether and the cyclic ether may be 5:95 to 95:5 (v / v), specifically 95:5 to 50:50, more specifically 90:10 to 70:30, 85:15 to 75:25, or 80:20. In the present invention, the volume ratio corresponds to the ratio of "volume % of acyclic ether": "volume % of cyclic ether" in the ether solvent.
[0260] In one embodiment of the present invention, the non-aqueous solvent may not contain a carbonate solvent in terms of the solubility of the electrolyte. Alternatively, the non-aqueous solvent may contain a very small amount of a carbonate solvent such that the carbonate solvent does not affect the solubility of the lithium salt. For example, when the non-aqueous solvent contains the carbonate solvent, the content of the carbonate solvent may be 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, or 0 wt% (i.e., not contained at all) based on the total weight of the electrolyte for a lithium secondary battery.
[0261] In one embodiment of the present invention, the lithium salt may be used without particular limitation as long as it can be used as an electrolyte of a lithium secondary battery. The lithium salt may be, for example, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (C2F5SO2)2NLi, (SO2F)2NLi, (CF3SO2)3CLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate, lithium imide, or two or more thereof.
[0262] In one embodiment of the present invention, the concentration of the lithium salt may be appropriately determined in consideration of ionic conductivity, solubility, etc., and may be, for example, 0.1 to 4 M, preferably 0.25 to 2 M, 0.5 to 2 M, 0.5 to 1.5 M, or 0.5 to 1.0 M. When the concentration of the lithium salt is in the above-described range, it is advantageous to secure ionic conductivity suitable for battery operation, or to exhibit an advantageous effect in terms of improving the mobility of lithium ions and suppressing the decomposition reaction of the lithium salt itself by exhibiting an appropriate viscosity of the electrolyte, but the present invention is not limited thereto.
[0263] In one embodiment of the present invention, the electrolyte may further include a nitrogen compound in addition to a lithium salt to improve the electrical conductivity of the electrolyte and extend the life of the lithium-sulfur battery. Specifically, the nitrogen compound may, for example, inhibit the reduction reaction of polysulfides occurring during the charge / discharge process of the lithium-sulfur battery, thereby preventing irreversible depletion of polysulfides, thereby improving the performance of the lithium-sulfur battery, although its efficacy is not limited thereto.
[0264] In one embodiment of the present invention, the nitrogen compound may be used without particular limitation as long as it forms a stable film on a lithium metal electrode, which is a negative electrode of a lithium secondary battery, specifically a lithium-sulfur battery, and exhibits an effect of improving charge / discharge efficiency. For example, the nitrogen compound may be a nitric acid compound, a nitrite compound, or a mixture thereof.
[0265] In one embodiment of the present invention, the nitrogen compound is, for example, an inorganic nitric or nitrous compound such as lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), barium nitrate (Ba(NO3)2), ammonium nitrate (NH4NO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), cesium nitrite (CsNO2), ammonium nitrite (NH4NO2); an organic nitric or nitrous compound such as methyl nitrate, dialkyl imidazolium nitrate, guanidine nitrate, imidazolium nitrate, pyridinium nitrate, ethyl nitrite, propyl nitrite, butyl nitrite, pentyl nitrite, and octyl nitrite; It may be selected from the group consisting of organic nitro compounds such as nitromethane, nitropropane, nitrobutane, nitrobenzene, dinitrobenzene, nitropyridine, dinitropyridine, nitrotoluene, dinitrotoluene, and combinations thereof, and preferably may include lithium nitrate.
[0266] In one embodiment of the present invention, the nitrogen compound may be included in an amount of, for example, 1 wt% to 10 wt%, 2 wt% to 10 wt%, or 3 wt% to 10 wt%, specifically 3 wt% to 8 wt%, 3 wt% to 6 wt%, or 3 wt% to 5 wt%, based on the total weight of the electrolyte for a lithium secondary battery, but is not limited thereto. When the nitrogen compound is included in the above-described amount, it may exhibit a more advantageous effect in terms of improving the electrical conductivity of the electrolyte by the nitrogen compound and suppressing the reduction of polysulfide when used in a lithium-sulfur battery, but the present invention is not limited thereto.
[0267]
[0268] In one embodiment of the present invention, the lithium-sulfur battery may exhibit various energy densities depending on the ratio of the electrolyte and the positive electrode active material. However, in terms of the energy density of the lithium-sulfur battery, a smaller ratio of the electrolyte and the positive electrode active material may exhibit a more advantageous effect, and for example, the weight ratio of sulfur in the electrolyte and the sulfur-carbon complex (El / S weight ratio) may be 3.5 g / g or less.
[0269] In one embodiment of the present invention, the lithium-sulfur battery can be manufactured so that the El / S ratio is, for example, 3 g / g or less, or 2.9 g or less.
[0270] According to one embodiment of the present invention, the lithium-sulfur battery having the above-described configuration may have a specific capacity of 60% or more, specifically 65% or more, 70% or more, or 75% or more, of a theoretical specific capacity calculated from the total content of sulfur-based compounds contained in the lithium-sulfur battery. More specifically, the lithium-sulfur battery may have a specific capacity of 80% or more, further 90% or more, of a theoretical specific capacity calculated from the total content of sulfur-based compounds contained in the lithium-sulfur battery.
[0271] In one embodiment of the present invention, the sulfur specific capacity of the lithium-sulfur battery may be, for example, 1,000 mAh / g or more. For example, the sulfur specific capacity of the lithium-sulfur battery may be 1,050 mAh / g or more, 1,080 mAh / g or more, specifically, 1,000 mAh / g to 1,675 mAh / g, 1,000 mAh / g to 1,300 mAh / g, 1,050 mAh / g to 1,250 mAh / g, or 1,080 mAh / g to 1,150 mAh / g.
[0272] In one embodiment of the present invention, the energy density of the lithium-sulfur battery may be, for example, 300 Wh / kg or more. For example, the energy density of the lithium-sulfur battery may be 300 Wh / kg to 2,600 Wh / kg, 300 Wh / kg to 1,600 Wh / kg, 300 Wh / kg to 1,000 Wh / kg, 300 Wh / kg to 800 Wh / kg, 300 Wh / kg to 450 Wh / kg, or 330 Wh / kg to 400 Wh / kg.
[0273] In one embodiment of the present invention, the specific capacity and energy density of the lithium-sulfur battery may be measured according to a known method for measuring the specific capacity and energy density of a lithium-sulfur battery, and there is no particular limitation on the measurement method.
[0274] In one embodiment of the present invention, the specific capacity and energy density of the lithium-sulfur battery may be measured by discharging at a 0.5 C rate and charging at a 0.3 C rate in the range of 1.8 V to 2.5 V at a room temperature of, for example, 23°C.
[0275] In one embodiment of the present invention, the lithium-sulfur battery may have various shapes, for example, a coin shape, a pouch shape, or a cylindrical shape, but is not limited thereto.
[0276] According to another aspect of the present invention, a method for evaluating the specific capacity of a lithium-sulfur battery using the above formula 1 is provided.
[0277] The above evaluation method is the content ratio (R) of sulfur element (S) according to the above formula 1 SL ) includes a step of determining a lithium-sulfur battery having a specific capacity of 15% or less as a high-specific-capacity battery.
[0278] In one embodiment of the present invention, the high capacity battery may be, for example, a battery having a capacity of 1,000 mAh / g or more.
[0279]
[0280] Hereinafter, preferred examples are presented to help understand the present invention, but the following examples are only illustrative of the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of the present invention, and it is also natural that such changes and modifications fall within the scope of the appended patent claims.
[0281]
[0282] [Manufacturing of lithium-sulfur batteries]
[0283] Example 1
[0284] A sulfur-carbon composite (S / C weight ratio = 2.45) was prepared by mixing inorganic sulfur (S8) and carbon nanotubes (CNT) as positive electrode active materials, and a positive electrode slurry composition was prepared by mixing 96 wt% of the prepared sulfur-carbon composite and 4 wt% of polyacrylate (PAA) as a binder. The positive electrode slurry composition was applied to an aluminum current collector and then dried to prepare a positive electrode. The loading of the prepared positive electrode was 2.08 mg(s) / cm 2( 2.5 mAh / cm 2 ) was.
[0285] Lithium metal with a thickness of 60 μm was used as the cathode.
[0286] An electrode assembly was prepared by positioning the positive and negative electrodes so that they face each other and interposing a polyethylene separator having a thickness of 16 ㎛ and a porosity of 46 vol% between them.
[0287] The prepared electrode assembly was stored in a pouch-type case, and an electrolyte solution containing 0.75 M lithium salt (LiTFSI) and 3 wt% lithium nitrate (LiNO3) dissolved in a solvent mixed with dimethoxyethane (DME):2-methylfuran (2-MeF) in a volume ratio of 8:2 was injected to produce a lithium-sulfur battery so that the El / S ratio was 2.9 g / g.
[0288]
[0289] Comparative Example 1
[0290] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that the S / C weight ratio was 2.9 when manufacturing the sulfur-carbon composite.
[0291]
[0292] Comparative Example 2
[0293] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that the S / C weight ratio was 2.6 when manufacturing the sulfur-carbon composite.
[0294]
[0295] [Measurement of R(SL) and battery performance evaluation]
[0296] The lithium-sulfur batteries of Example 1, Comparative Example 1, and Comparative Example 2 manufactured above were each charged once at room temperature (23°C) at a 0.3 C rate in the range of 1.8 V to 2.5 V, and then discharged once at a 0.5 C rate to 1.8 V. The battery capacity (capacity, mAh) and energy (energy, Wh) at this time were measured, and then the specific capacity (mAh / g) and energy density (Wh / kg) of the batteries were evaluated by dividing by each battery capacity. The results are shown in Table 1 below.
[0297] Next, the lithium-sulfur battery discharged to 1.8 V was disassembled and R was calculated according to Equation 1 below. SL was measured.
[0298] [Formula 1]
[0299] R SL(%) = W SE / W SP X 100
[0300] In the above formula 1,
[0301] W SE is the weight of elemental sulfur (S) among the sulfur compounds present in the electrolyte,
[0302] W SP is the weight of elemental sulfur (S) among the sulfur compounds present in the above anode.
[0303]
[0304] W SE For measurement, the disassembled battery was placed in an extraction solvent (DME) and extracted for 48 hours. After removing the battery from the extract, methyl trifluoromethanesulfonate (CF3SO3CH3) was added to the extract to perform methyl derivatization. The methyl derivatized components were separated by liquid chromatography (LC) analysis under the following conditions, and then fractionated according to the fractionation range.
[0305] [LC / UV analysis conditions]
[0306] Column: CAPCELLPAL C18 column (inner diameter 4.6 mm, length 50 mm, particle size 3 ㎛, OSAKA SODA)
[0307] Mobile phase: H2O / methanol mixed solvent, gradient elution (0 min: H2O / methanol 75 / 25 (v / v), 10 min: H2O / methanol=0 / 100 (v / v), 20 min: H2O / methanol=0 / 100 (v / v)
[0308] Flow rate: 0.7 ml / min
[0309] Column temperature: 40 ℃
[0310] Injection volume: 10 μl
[0311] Detection wavelength: 254 nm
[0312] Afterwards, using the concentration-specific standard products manufactured in Korean Patent Application No. 2021-0188588, the peak area of each methyl derivatized component appearing in the chromatogram obtained by LC / UV analysis was measured to calculate the content of lithium polysulfide present in the extract by component, and then these were added to obtain W SE The value was measured.
[0313] W SP For measurement, the above W SE After extraction for measurement, the separated positive electrode was dried at room temperature, and the content of elemental sulfur (S) in the positive electrode was measured according to the method described in Korean Patent Application No. 2021-0173961. Specifically, the positive electrode active material layer was scraped and collected, placed in a Sn capsule, and placed in an EA device (Flash 2100, Thermo) and combusted at 990°C to generate gas. The generated gas was separated using a GC column, and the content of elemental sulfur (S) was measured. At this time, BBOT (2,5-Bis(5-tert-butyl-benzoxazol-2-yl)thiophene) was used as a standard material for quantitative analysis.
[0314] Table 1 below shows the W' measured above based on the total weight of elemental sulfur (S) derived from the content of inorganic sulfur (S8) used in manufacturing the sulfur-carbon composite used in each battery. SE and W' SP Each weight ratio is represented, and from this, R' according to Equation 1-2 SL Calculate the value, R' SL The value is R according to Equation 1 SL Since the values are the same, Table 1 below shows R SL The value was recorded.
[0315] [Formula 1-2]
[0316] R' SL (%) = W' SE / W' SP X 100
[0317] In the above equation 1-2,
[0318] W' SE is the weight % of elemental sulfur (S) among the sulfur compounds present in the electrolyte, based on the weight of elemental sulfur (S) among the sulfur compounds present in the lithium-sulfur battery,
[0319] W' SP is the weight % of elemental sulfur (S) among the sulfur compounds present in the positive electrode, based on the weight of elemental sulfur (S) among the sulfur compounds present in the lithium-sulfur battery.
[0320] Also, W' measured above SE and W' SP Using the values, whether the following equations 2 and 3 are satisfied is evaluated, and whether T(true) / F(fail) is evaluated, and this is shown together in Table 1 below.
[0321] [Formula 2]
[0322] W' SP > 1.2 XW' SE + 56.86
[0323] [Formula 3]
[0324] 10.667 XR S / C - 10.633 > R SL
[0325] S / C ratioW SE (mg)W SP (mg)W' SE (wt%)W' SP (wt%)R SL (%)Whether equation 2 is satisfiedWhether equation 3 is satisfiedCapacity (mAh / g)Energy density (Wh / kg)Example 12.4282379.176.811.9TT1,089349Comparative example 12.94723215.275.120.3FF979312Comparative example 22.63822112.271.517.1FF875278
[0326] As confirmed in Table 1 above, the R of the lithium-sulfur battery discharged to 1.8 V SLExample 1, in which the ratio was 15% or less, had a lower S / C ratio than Comparative Examples 1 and 2, showing a specific capacity of 1,000 mAh / g or more and an excellent energy density. However, when Comparative Examples 1 and 2 are compared, Comparative Example 1 has a lower specific capacity and energy density than Comparative Example 2 despite the high S / C ratio of Comparative Example 1. Therefore, R SL It was confirmed that a high-capacity lithium-sulfur battery can be identified through the value.
[0327] When discharged to 1.8 V, it is difficult for the sulfur reduction reaction to occur any more, so the maximum capacity that the battery can express has been expressed, and R SL The value is at its lowest. Therefore, for the implementation of lithium-sulfur batteries with high capacity and high energy density, R SL We were able to confirm that this should be controlled to less than 15%.
Claims
1. A lithium-sulfur battery comprising a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, comprising a sulfur-carbon complex. At least one of the above cathode and the above electrolyte comprises a sulfur compound, The content ratio of sulfur element (S) according to the following formula 1 (R) SL ) Lithium-sulfur batteries with less than 15%: [Formula 1] R SL (%) = W SE / W SP X 100 In the above equation 1, W SE is the weight of elemental sulfur (S) among the sulfur compounds present in the electrolyte, W SP is the weight of elemental sulfur (S) among the sulfur compounds present in the above anode.
2. In claim 1, In the above equation 1, W SE and W SP A lithium-sulfur battery showing values measured at a discharge state of 1.7 V to 1.9 V, respectively.
3. In claim 1, The sulfur compounds present in the above electrolyte are inorganic sulfur (S8), lithium (poly)sulfide (Li2S). x , 1 ≤ x ≤ 8) or a mixture thereof.
4. In claim 1, The sulfur compounds present in the above anode are inorganic sulfur (S8), lithium (poly)sulfide (Li2S). x , 1 ≤ x ≤ 8) or a mixture thereof.
5. In claim 1, Above W SE A lithium-sulfur battery having a total sulfur element (S) content of 15 wt% or less based on the weight of the sulfur compound contained in the lithium-sulfur battery.
6. In claim 1, Above W SP A lithium-sulfur battery having a sulfur compound contained in the lithium-sulfur battery in an amount of 65 wt% or more based on the weight of the total sulfur element (S) present in the sulfur compound contained in the lithium-sulfur battery.
7. In claim 6, Above W SP A lithium-sulfur battery having a total sulfur element (S) content of 75.5 wt% or more based on the weight of the sulfur compound contained in the lithium-sulfur battery.
8. In claim 1, A lithium-sulfur battery satisfying the following equation 2: [Formula 2] W' SP > 1.2 X W' SE + 56.86 In the above equation 2, W' SE is the weight % of elemental sulfur (S) among the sulfur compounds present in the electrolyte, based on the total weight of elemental sulfur (S) among the sulfur compounds contained in the lithium-sulfur battery. W' SP is the weight percentage of elemental sulfur (S) among the sulfur compounds present in the positive electrode, based on the total weight of elemental sulfur (S) among the sulfur compounds contained in the lithium-sulfur battery.
9. In claim 1, A lithium-sulfur battery satisfying the following equation 3: [Formula 3] 10.667 X R S / C - 10.633 > R SL In the above equation 3, The above R SL is the content ratio of sulfur element (S) according to the above formula 1, The above R S / C is the weight ratio of sulfur (S) and carbon (C) in the above sulfur-carbon complex.
10. In claim 1, The above sulfur-carbon complex is a lithium-sulfur battery having a sulfur / carbon weight ratio (S / C weight ratio) of 2.5 g / g or less.
11. In claim 1, The positive electrode comprises a current collector and a positive electrode active material layer including the sulfur-carbon complex, A lithium-sulfur battery in which the weight of the sulfur-carbon composite is 80 wt% or more based on the total weight of the positive electrode active material layer.
12. In claim 1, A lithium-sulfur battery having an El / S weight ratio of sulfur in the electrolyte and the sulfur-carbon complex of 3.5 g / g or less.
13. In claim 1, A lithium-sulfur battery wherein the electrolyte comprises an acyclic ether, a cyclic ether, or a mixture thereof.
14. In claim 13, The above electrolyte comprises a mixture of the above non-cyclic ether and the above cyclic ether, A lithium-sulfur battery wherein the volume ratio of the acyclic ether and the cyclic ether is 5:95 to 95:5 (v / v).
15. In claim 1, A lithium-sulfur battery having a specific capacity of 60% or more of the theoretical specific capacity calculated from the total content of sulfur compounds contained in the lithium-sulfur battery.
16. In claim 15, A lithium-sulfur battery comprising the sulfur compound, inorganic sulfur (S8), lithium (poly)sulfide (Li2Sx, 1 ≤ x ≤ 8), or a mixture of two or more thereof.
17. In claim 1, A lithium-sulfur battery having a specific capacity of 1,000 mAh / g or more.
18. In claim 1, A lithium-sulfur battery having an energy density of 300 Wh / kg or more.
19. In claim 1, The above lithium-sulfur battery is a lithium-sulfur battery that is a coin-type battery, a pouch-type battery, or a cylindrical battery.
20. A method for evaluating the specific capacity of a lithium-sulfur battery comprising a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte comprising a sulfur-carbon complex, At least one of the above cathode and the above electrolyte comprises a sulfur compound, The content ratio of sulfur element (S) according to the following formula 1 (R) SL ) An evaluation method including a step of determining a lithium-sulfur battery having a specific capacity of 15% or less as a high specific capacity battery: [Formula 1] R SL (%) = W SE / W SP X 100 In the above equation 1, W SE is the weight of elemental sulfur (S) among the sulfur compounds present in the electrolyte, W SP is the weight of elemental sulfur (S) among the sulfur compounds present in the above anode.
21. In claim 20, An evaluation method in which the above high capacity battery is a battery having a specific capacity of 1,000 mAh / g or more.
Citation Information
Patent Citations
High capacity lithium-sulfur batteries
KR1020020011562A
Electronic device for processing memory request using memory address space extension and method for operating thereof
KR1020240029502A
KR20210088025A