Ceramic sheet, method for preparing same, and all-solid secondary battery comprising same
The introduction of a garnet-type oxide-based ceramic sheet with controlled lithium content and a specific manufacturing method addresses the safety concerns of conventional lithium secondary batteries by enhancing lithium ion conductivity and mechanical stability, leading to improved performance and safety in all-solid-state batteries.
Patent Information
- Application Number
- PCT/KR2024/006047
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-03
- Filing Date
- 2024-05-03
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional lithium secondary batteries pose safety risks due to their flammable liquid electrolytes, which can ignite when exposed to water, particularly in electric vehicles, necessitating the development of safer alternatives with improved performance.
A garnet-type oxide-based ceramic sheet with controlled lithium content and a manufacturing method involving primary and secondary sintering steps to produce a high lithium ion conductivity solid electrolyte for all-solid-state batteries, reducing impurity phase formation and enhancing atmospheric stability.
The garnet-type oxide-based ceramic sheet achieves high lithium ion conductivity and electronic conductivity, while maintaining mechanical stability and preventing reactions with moisture and carbon dioxide, thereby improving the safety and performance of all-solid-state batteries.
Smart Images

Figure KR2024006047_07112024_PF_FP_ABST
Abstract
Description
Ceramic sheet, method for manufacturing the same, and all-solid-state secondary battery comprising the same
[0001] The present disclosure relates to a ceramic sheet, a method for manufacturing the same, and an all-solid-state secondary battery including the same.
[0002] Lithium secondary batteries boast large electrochemical capacity, high operating potential, and excellent charge-discharge cycling characteristics. Demand for them continues to grow as an energy source for mobile devices, portable electronic devices, small home power storage devices, motorcycles, electric vehicles, and hybrid electric vehicles. As the applications of lithium secondary batteries expand, so too does the demand for improved safety and higher performance.
[0003] Conventional lithium secondary batteries use highly flammable liquid electrolytes, which can pose serious safety risks if a short circuit occurs. Furthermore, they are prone to ignition when exposed to water in the air. These safety concerns are becoming increasingly important in electric vehicles.
[0004] Recently, research into all-solid-state secondary batteries (SSDs) utilizing solid electrolytes made of non-flammable inorganic materials has been actively pursued to enhance safety. All-solid-state SSDs are attracting attention as next-generation secondary batteries due to their numerous advantages, including safety, high energy density, high output, long life, simplified manufacturing process, and the potential for larger / compacterized and lower-cost batteries.
[0005] The present disclosure seeks to provide a garnet-type oxide ceramic sheet having excellent atmospheric stability.
[0006] The present disclosure provides a method for manufacturing the above garnet-type oxide ceramic sheet.
[0007] Furthermore, the present disclosure seeks to provide an all-solid-state battery including a garnet-type oxide ceramic sheet.
[0008] The present disclosure provides a garnet-type oxide-based ceramic sheet, and according to one embodiment of the present disclosure, a garnet-type oxide-based ceramic sheet comprising a garnet-type oxide, wherein the garnet-type oxide-based ceramic sheet comprises a surface portion and a deep portion, an average lithium content of garnet-type oxide particles in the surface portion is higher than an average lithium content of garnet-type oxide particles in the deep portion, and a ratio of the average lithium content of the garnet-type oxide in the surface portion to the average lithium content of the garnet-type oxide in the surface portion is greater than 1 and less than 1.014.
[0009] The surface portion may be a region from one surface of the ceramic sheet to a thickness of 1 μm, and the deep portion may be a region from the thickness of 1 μm to the center of the thickness.
[0010] The average lithium content of the garnet-type oxide of the above surface layer may be less than 6.33 in the stoichiometric ratio of lithium based on the composition formula of the garnet-type oxide particles when oxygen is 12.
[0011] The above garnet-type oxide may include an LLZO-type oxide.
[0012] The above LLZO-based oxide may include a doping element.
[0013] The above LLZO-based oxide may include at least one type of doping element selected from the group consisting of Ga and Al at the Li site.
[0014] The above ceramic sheet can have a lithium ion conductivity of 1.3 mS / cm or more at 25°C.
[0015] The above ceramic sheet is 10Х10 -10 It can have an electronic conductivity of less than cm.
[0016] The above ceramic sheet has grain boundaries and may have an average grain size of 4 to 200 μm.
[0017] The above garnet-type oxide powder has an average particle size of 1 μm or less and may have two or more particle sizes.
[0018] The above garnet-type oxide powder is D 10 This is less than 1㎛, and D 50 This can be 1㎛ to 30㎛.
[0019] The present disclosure also provides, in one aspect, a method for producing a garnet-type oxide ceramic sheet, and according to one embodiment, the method includes a step of producing an oxide molded body by molding garnet-type oxide powder having an average particle size of 1 ㎛ or less and two or more particle sizes into a predetermined shape, and a step of sintering the oxide molded body to produce a sintered body, wherein the sintering includes a first sintering and a second sintering, and the first sintering temperature may be higher than the second sintering temperature.
[0020] The above first sintering temperature may be 1050 to 1400°C, and the above second sintering temperature may be 1000 to 1300°C.
[0021] The method of one embodiment according to the present disclosure may further include the step of calcining a precursor powder to produce calcined garnet-type oxide powder; and the step of pulverizing the calcined garnet-type oxide powder to provide garnet-type oxide powder having two or more particle sizes.
[0022] The above calcined garnet oxide powder is D 10 This is less than 1㎛, and D 50 This can be 1㎛ to 10㎛.
[0023] The above garnet-type oxide may include an LLZO-type oxide.
[0024] The present disclosure provides, in one aspect, an all-solid-state secondary battery, which may include, according to one embodiment, a cathode, an anode, and any one of the above-described garnet-type oxide ceramic sheets as a solid electrolyte.
[0025] The ceramic sheet including the garnet-type oxide according to the present disclosure has excellent atmospheric stability because the lithium concentration is controlled on the surface, thereby reducing the formation reaction of impurity phases due to moisture or carbon dioxide in the atmosphere.
[0026] An all-solid-state battery including a ceramic sheet containing a garnet-type oxide according to the present disclosure as an electrolyte sheet can suppress a decrease in ionic conductivity by reducing the amount of impurity phase generated between the electrode and the electrolyte sheet.
[0027] The solid electrolyte of the present disclosure can be widely applied in green technology fields such as electric vehicles, battery charging stations, and other battery-powered solar and wind power generation. Furthermore, the solid electrolyte of the present disclosure can be used in eco-friendly electric vehicles, hybrid vehicles, and other vehicles to prevent climate change by suppressing air pollution and greenhouse gas emissions.
[0028] Figure 1 is a schematic diagram showing the effect of particle size distribution characteristics on the densification of a sintered body, where (a) is the case where a single-sized powder is used, (b) is the case where a powder having a bimodal particle size distribution is used, and (c) is the case where a powder having a trimodal particle size distribution is used.
[0029] Figure 2 is a schematic diagram showing the crystal shape of a sintered body manufactured by one-step sintering at high temperature for a long time and the reaction that occurs when the sintered body is exposed to air. (a) shows the crystal shape (i) of the surface of the sintered body and the change (ii) of the surface according to the reaction, and (b) shows the crystal shape (i) of the cross-section of the sintered body and the change (ii) of the surface according to the reaction.
[0030] Figure 3 is a schematic diagram showing the crystal shape of a sintered body manufactured by two-step sintering, sintering at high temperature for a short time and sintering at low temperature for a long time, and the reaction that occurs when the sintered body is exposed to air. (a) shows the crystal shape (i) of the surface of the sintered body and the change (ii) of the surface according to the reaction, and (b) shows the crystal shape (i) of the cross-section of the sintered body and the change (ii) of the surface according to the reaction.
[0031] Fig. 4 (a) is a SEM image of the GLLZO powder manufactured in Reference Example 1, (b) is a SEM image of the GLLZO powder after the particle size of the GLLZO powder has been adjusted by ball milling, and (c) is a graph showing the particle size analysis results of the particle size-adjusted GLLZO powder of (b).
[0032] Figures 5 (a) to (c) are drawings showing the Rietveld fitting results according to XRD analysis of ceramic sheets manufactured in Reference Example 1, Reference Example 2, and Example 1, and (d) is a drawing showing the XRD analysis results of a GLLZO ceramic sheet.
[0033] Figure 6 is an SEM photograph of the surface of a ceramic sheet manufactured in Reference Example 1, Reference Example 2, and Example 1.
[0034] FIG. 7 is a diagram showing a two-probe AC impedance pattern of ceramic sheets manufactured in Reference Example 1, Reference Example 2, and Example 1.
[0035] FIG. 8 is a diagram showing the lithium ion conductivity of the ceramic sheets manufactured in Reference Example 1, Reference Example 2, and Example 1, along with known lithium ion conductivity values for LLZO including doping elements.
[0036] FIG. 9 is a diagram showing the resistance measured according to temperature and the ionic conductivity analyzed according to temperature for ceramic sheets manufactured in Reference Example 1, Reference Example 2, and Example 1.
[0037] Fig. 10 is a drawing showing the results of a DC polarization test performed on ceramic sheets manufactured in Reference Example 1, Reference Example 2, and Example 1.
[0038] Figure 11 is an image of the surface of a ceramic sheet (a) manufactured in Reference Example 1, Reference Example 2, and Example 1, a ceramic sheet (b) obtained by aging each of the ceramic sheets (a) in a desiccator, and a ceramic sheet (c) obtained by aging each of the ceramic sheets (a) in air, observed using a scanning electron microscope (SEM).
[0039] FIG. 12 is a diagram showing changes in the complex impedance spectrum and lithium ion conductivity at 25°C for each of Reference Example 1, Reference Example 2, and the ceramic sheets (a) to (c) of the examples.
[0040] FIG. 13 is a diagram showing the Li2CO3 / LLZO peak ratio for the ceramic sheets (a) to (c) of each of Reference Example 1, Reference Example 2, and Example 1.
[0041] Figure 14 is a graph showing the results of analyzing lithium strength by performing secondary ion mass spectrometry (SIMS) to confirm the difference in Li2CO3 production amount of ceramic sheets manufactured in Reference Example 1, Reference Example 2, and Example 1.
[0042] All-solid-state secondary batteries consist of a positive electrode, a solid electrolyte layer, and a negative electrode. The solid electrolyte in the solid electrolyte layer requires high ionic conductivity and low electronic conductivity. All-solid-state secondary batteries typically exhibit low interfacial compatibility between the solid electrolyte layer and the electrode, and low ionic conductivity.
[0043] For example, Li7La3Zr2O 12Garnet-type oxides such as (Li-La-Zr-O, LLZO) have attracted much attention as solid electrolytes for all-solid-state batteries due to their relatively excellent lithium ion conductivity (>0.1 mS / cm), wide electrochemical stability window (>4.5 V), and excellent stability toward Li metal anodes.
[0044] However, despite the high potential described above, the garnet-type oxide solid electrolyte is required to achieve a lithium ion conductivity (total conductivity (including grain + grain boundary components)) of 1 mS / cm or more at room temperature (25°C).
[0045] Lithium ion conductivity can be affected by factors such as sample density, crystal structure, sample stoichiometry, concentration of mobile lithium ions, lithium ion vacancies, and lithium ion mobility. At least pure LLZO, i.e., undoped LLZO, generally crystallizes in a tetragonal structure, resulting in low ionic conductivity. Furthermore, high ionic conductivity at 25°C is required.
[0046] The present disclosure provides a garnet-type oxide ceramic sheet having excellent atmospheric stability, a method for manufacturing the ceramic sheet, and an all-solid-state battery including the ceramic sheet as a solid electrolyte.
[0047] The method for manufacturing the garnet-type oxide ceramic sheet according to the present disclosure includes a step of manufacturing an oxide molded body by molding a garnet-type oxide powder into a predetermined shape and a step of sintering the molded body to manufacture a sintered body.
[0048] A method for manufacturing a garnet-type oxide ceramic sheet according to the present disclosure includes a step of manufacturing a molded body by molding garnet-type oxide powder into a predetermined shape.
[0049] The above garnet-type oxide powder is an ionic conductor having a garnet structure, for example, a cubic or orthorhombic crystal structure, and has the chemical formula Li7. - x La3Zr2 - x Ta x O 12 (wherein, 0≤x≤2) may be lithium lanthanum zirconium oxide (LLZO). Specifically, the garnet-type oxide powder may have a stoichiometric composition of, for example, Li7La3Zr2O 12 It can be a solid ionic conductor.
[0050] Lithium ion conductivity can be improved by introducing doping elements into oxide-based solid electrolytes. Specifically, other doping elements can be doped into the La, Zr, and Li sites.
[0051] For example, the garnet-type oxide powder may include a doping element at the Li site. By including a doping element at the lithium site of the garnet-type oxide powder, the lithium content can be reduced or the concentration of lithium vacancies can be increased, thereby stabilizing the crystal structure and improving ionic conductivity.
[0052] The above La and Zr sites may include doping elements. By doping the La and Zr sites with doping elements, crystallization can be performed in a cubic shape, thereby improving ionic conductivity.
[0053] The doping element of the Li site is not limited thereto, but may include, for example, one selected from the group consisting of Ga, Al, In, Sc, Fe, and Y, and may include two or more doping elements at the same time. More specifically, the doping element of the Li site may be at least one selected from the group consisting of Ga and Al. Accordingly, the garnet-type oxide powder including the doping element at the Li site has, for example, a chemical formula of Li 7-3x Ga x La3Zr2O 12 or Li 7-3x Al x La3Zr2O 12 (0 <x≤0.25)로 표시될 수 있다.
[0054] Meanwhile, garnet-type oxide powders such as LLZO can be rapidly decomposed in the air because Li2CO3 can be easily generated on the surface due to reactions with moisture (H2O) and carbon dioxide (CO2). The Li2CO3 is Li + Wow H + As a result of ion exchange, it can be mainly formed at the boundaries between particles in the sintered body, and secondary phases such as La2Zr2O7 can grow. Li2CO3 generated at such particle boundaries can cause an increase in impedance, which can significantly reduce the performance of the battery. The solid electrolyte can provide air stability by including a doping element at the Li site. For this purpose, the garnet-type oxide powder can include a doping element such as Mg or Ga.
[0055] The above garnet-type oxide powder may also include additional doping elements at the La and / or Zr sites.
[0056] By including a doping element in the La site, the crystal lattice of the garnet-type oxide powder can be stabilized. The doping element included in the La site is not limited thereto, but may be, for example, an alkaline earth metal, and specifically, may be any one selected from the group consisting of Ca, Sr, Ba, Ra, Be, and Mg, and may include two or more doping elements simultaneously.
[0057] In addition, the doping element included in the Zr site is not limited thereto, but may be at least one selected from the group consisting of Ta, Te, Nb, Sb, W, Mo, Cr, Y, V, and Ti, and may include two or more doping elements at the same time.
[0058] The above garnet-type oxide powder can be manufactured by a conventional method, and is not particularly limited thereto, and can be manufactured by a solid-state reaction method, a sol-gel method, or a co-precipitation method. For example, when manufacturing a garnet-type oxide powder by a solid-state reaction method, powders of raw materials containing components of the garnet-type oxide can be mixed, and the resulting mixed powder can be milled and then calcined to manufacture a garnet-type oxide powder.
[0059] More specifically, the mixed powder of the above raw materials can be obtained by mixing a lithium source such as lithium hydroxide or lithium carbonate, lanthanum oxide and zirconium oxide, and, if necessary, an oxide containing a doping element in a stoichiometric ratio.
[0060] The above lithium source may be input in excess, considering that lithium is lost in the subsequent sintering step, and may be selected as needed, but is not limited thereto. For example, the lithium source may be input in an amount exceeding 10 wt% additionally compared to the lithium source content to be input based on the stoichiometric ratio of the garnet-type oxide, for example, in an amount exceeding 10 wt% and 30 wt% or less, exceeding 10 wt% and 20 wt% or less, or exceeding 10 wt% and 15 wt% or less. Accordingly, the garnet-type oxide powder according to one embodiment may include lithium in an amount exceeding 10 at% of the stoichiometric ratio, for example, in an amount exceeding 10 at% and 30 at% or less, in an amount exceeding 10 at% and 20 at% or less, or in an amount exceeding 10 at% and 15 at% or less.
[0061] The method for manufacturing the above garnet-type oxide powder may include a step of grinding the mixture of raw materials. The grinding step may control the powder shape, particle size, and distribution of each raw material constituting the mixture of raw materials.
[0062] The above pulverization is not particularly limited, but can be performed, for example, by ball milling, and the ball milling can be performed by a dry or wet method. The ball milling is not limited thereto, but can be performed for 1 hour to 48 hours, more specifically for 5 hours or more and 30 hours or less, at 100 to 300 rpm, more specifically 150 to 250 rpm.
[0063] A step of calcining the mixture after the above-mentioned grinding may be included. The calcination can obtain the desired crystal phase and remove impurities. The calcination can be performed, but is not limited to, at a temperature range of 750 to 900°C for 3 to 12 hours. As a result, a garnet-type oxide powder according to one embodiment of the present disclosure can be obtained.
[0064] The above garnet-type oxide powder may have an average particle size of 1 μm or less, and may have a multi-modal particle size distribution such as bi-modal. The average particle diameter and particle size distribution can be analyzed using a commonly used particle size analyzer, for example, a particle size analyzer utilizing laser diffraction can be used. Specifically, the particle size analyzer utilizing laser diffraction is not particularly limited, but for example, a Malvern particle size analyzer or a Horiba particle size analyzer can be used.
[0065] The size of the garnet-type oxide powder can affect the densification of the sintered body. Therefore, in order to obtain a sintered body with high lithium ion conductivity, it may be required to have a high-quality microstructure at the grain and grain boundaries. When the garnet-type oxide powder has a small particle size and two or more particle sizes, specifically a bimodal distribution, a high-density ceramic sheet can be obtained by sintering.
[0066] The size of the garnet-type oxide powder can affect the densification of the sintered body. Therefore, to obtain a sintered body with high lithium ion conductivity, a high-quality microstructure at the grain and grain boundaries may be required. When the garnet-type oxide powder has a small particle size and a multimodal distribution, a high-density ceramic sheet can be obtained by sintering.
[0067] Fig. 1 is a schematic diagram showing the effect of particle size distribution characteristics on the densification of a sintered body. As can be seen from Fig. 1, when powder having a monomodal particle size distribution is used (a), the relative density is low due to gaps between particles, and when powder having two or more particle sizes is used (b), the gaps formed by the first powder having a large particle size are filled with a second powder having a smaller particle size, which can increase the apparent relative density of the sintered body.
[0068] For example, the garnet-type oxide powder may include a first powder having a particle size in the range of 0.1 μm to 1 μm and a second powder having a particle size in the range of 0.5 μm to 10 μm. Specifically, the garnet-type oxide powder may include a first powder having a particle size in the range of 0.2 μm to 0.7 μm and a second powder having a particle size in the range of 0.7 μm to 3 μm.
[0069] At this time, the first powder may be 50% to 80% of the volume of the total powder, and the second powder may be 20 to 50% of the volume of the total powder.
[0070] As another example, for example, the garnet-type oxide powder has Dv 10 1㎛ or less and Dv 50 It can have a bimodal particle size distribution of 1㎛ to 30㎛. More specifically, Dv 10 0.3㎛ to 1㎛ and Dv 50 It may be 1㎛ to 10㎛ or 1㎛ to 5㎛.
[0071] As another embodiment, the garnet-type oxide powder may have a trimodal particle size distribution, as shown in (c) of Fig. 1. When the garnet-type oxide powder has a trimodal particle size distribution, the gap between the first and second powders can be filled more densely with a third powder having a smaller particle size, and further, the gap can be filled more densely with the third powder, thereby further increasing the apparent relative density of the sintered body.
[0072] Although not limited thereto, the garnet oxide powder has a Dv 10 First powder less than 1㎛, Dv 50 Second powder of 1 to 3 μm and D v90 It may have a trimodal particle size distribution of the third powder of 1.5 to 30㎛, more specifically, Dv 10First powder of 0.3 to 1㎛, Dv 50 Second powder of 0.7 to 2.5㎛ and D v90 It can have a particle size distribution of the third powder of 1.5 to 20㎛, and also, Dv 10 First powder of 0.4 to 0.6㎛, Dv 50 First powder of 0.7 to 2㎛ and D v90 The first powder may have a particle size distribution of 1.5 to 15 μm.
[0073] In order to ensure that the garnet-type oxide powder obtained by the above calcination has a multimodal particle size distribution such as the above bimodal, a step of pulverizing the garnet-type oxide powder after calcination may be included as needed, thereby providing a garnet-type oxide powder having an average particle size of less than 1 µm.
[0074] The above-mentioned grinding is not particularly limited, but may be performed by ball milling as described above. The ball milling may be performed by a dry or wet method, and may be performed, for example, at 100 to 300 rpm for 48 to 100 hours. In addition, the balls used in the ball milling may have a diameter of 5 to 10 mm.
[0075] A step of manufacturing a garnet-type oxide-based molded body using a garnet-type oxide powder having a multimodal particle size distribution such as a bimodal particle size distribution as described above is included. The garnet-type oxide-based molded body is not particularly limited and may be, for example, in a sheet shape.
[0076] The specific thickness or size of the garnet-type oxide-based molded body can be adjusted according to the characteristics of the sintered body to be manufactured and is not particularly limited. For example, the thickness of the garnet-type oxide-based molded body may be 100 to 1000 μm.
[0077] A step of sintering the garnet-type oxide-based molded body manufactured above is included. The sintering is a step of densifying the garnet-type oxide-based molded body to manufacture a garnet-type oxide-based ceramic sheet, and the sintering can be performed by a two-step sintering method including a first sintering step and a second sintering step.
[0078] Specifically, the two-step sintering method includes a first sintering step performed at a first sintering temperature and a second sintering step performed at a second sintering temperature, and the first sintering temperature may be higher than the second sintering temperature.
[0079] More specifically, the first sintering step is performed at a relatively high temperature during the sintering process of the second sintering step, and can be performed specifically at a temperature range of 1050 to 1400°C, for example, 1050°C or higher and 1400°C or lower.
[0080] If the first sintering temperature of the first sintering step is too low, a sintered body having an excellent sintering degree may not be obtained, and if the first sintering temperature is too high, excessive particle growth may occur during sintering.
[0081] The above first sintering temperature may be specifically 1100°C or higher, more specifically 1150°C or higher, specifically 1350°C or lower, more specifically 1300°C or lower, or 1250°C or lower. By performing the first sintering step in the above temperature range, the sintered body can be densified without excessive grain growth. At this time, but not limited thereto, the first sintering can be performed to have a density of about 90% or higher and a relative density of 90% or higher.
[0082] The above first sintering step can be performed for a short period of time. By performing sintering at a high temperature for a short period of time as described above, excessive grain growth of the garnet-type oxide ceramic sheet can be suppressed. Specifically, the above first sintering step can be performed for 10 seconds to 1 hour, and more specifically, for 1 minute or more, 3 minutes or more, 5 minutes or more, 7 minutes or more, or 10 minutes or more, and for 1 hour or less, 50 minutes or less, 40 minutes or less, or 30 minutes or less.
[0083] The second sintering step is not particularly limited as long as it is performed at a temperature lower than the first sintering temperature of the first sintering step, but specifically, the second sintering temperature may be 1000 to 1300°C, for example, 1000°C or higher, 1050°C or higher, or 1100°C or higher, and 1300°C or lower, 1250°C or lower, 1200°C or lower, or 1150°C or lower.
[0084] The sintering temperature difference between the first sintering step and the second sintering step is not particularly limited, but may be, for example, 50 to 200°C, specifically 50 to 150°C, and more specifically 50 to 100°C. Since the eleventh sintering step and the second sintering step have a sintering temperature difference within the above-described range, excessive grain growth of the garnet-type oxide ceramic sheet can be prevented.
[0085] The second sintering step may be performed for a longer period of time than the first sintering step. Specifically, the second sintering step may be performed for 10 minutes to 24 hours, and more specifically, for 10 minutes or more, 15 minutes or more, 30 minutes or more, 1 hour or more, 1 hour and 30 minutes or more, 2 hours or more, 3 hours or more, or 4 hours or more, and for 24 hours or less, 20 hours or less, 18 hours or less, 15 hours or less, 12 hours or less, 10 hours or less, 8 hours or less, 6 hours or less, or 4 hours or less.
[0086] The above second sintering step is a process of maintaining sintering, and can suppress excessive particle growth by performing the first sintering step at a high temperature for a short time, and promote densification of the sintered body by performing the second sintering step at a lower temperature for a long time.
[0087] In this way, by performing a two-step sintering in which the first sintering step is performed at a relatively high temperature and the second sintering step is performed at a relatively low temperature, more specifically, by performing a two-step sintering in which the first sintering step is performed for a short time and the second sintering step is performed for a long time, thereby manufacturing a sintered body, the particles can be suppressed from melting during the sintering process and growing within the sintered body, thereby preventing coarsening of the particles. Accordingly, the densification between particles can be improved while maintaining the fine particle size within the ceramic sheet, thereby obtaining a ceramic sheet having a high relative density.
[0088] Furthermore, since sintering at high temperatures is not performed for a long period of time, the phenomenon of lithium within the ceramic sheet moving to the surface and volatilizing can be suppressed. Consequently, a ceramic sheet with a high lithium concentration on the surface and a low lithium concentration within can be obtained.
[0089] For example, in the case of long-term sintering at high temperatures, liquid sintering occurs due to melting of particles during the sintering process, and as shown in Fig. 2, the crystals of the sintered body become coarser, and during the sintering process, lithium inside moves to the surface and volatilizes, reducing the lithium content, and lithium can rise from the inside on the surface of the ceramic sheet, increasing the Li content. When such a ceramic sheet is exposed to the air, as shown in Fig. 2 (a), the Li increased on the surface of the ceramic sheet can easily react with moisture and carbon dioxide in the air, and as shown in Fig. 2 (b), Li2CO3 can be generated on the surface of the ceramic sheet. This generation of Li2CO3 can cause a decrease in ionic conductivity.
[0090] However, in ceramic sheets manufactured by two-step sintering, liquid sintering due to particle melting can be suppressed by sintering at high temperature for a short time and then at low temperature for a long time during the sintering process. As a result, as shown in Fig. 3, coarsening of the crystals in the sintered body can be suppressed, and an increase in the lithium content on the surface of the sintered body can be prevented.
[0091] By using oxide powders containing lithium in excess of the stoichiometric ratio, a sintered body manufactured by two-step sintering can maintain the fine size of oxide particles, and furthermore, the sintered body can be densified by oxide powders having two or more particle sizes, specifically, a bimodal particle size distribution. By maintaining and densifying the fine particle size, volatilization of lithium can be suppressed, and lithium in the oxide powder can be suppressed from reacting with moisture or carbon dioxide.
[0092] That is, even if the ceramic sheet is exposed to the air, the reaction of the GLLZO of the ceramic sheet with moisture and carbon dioxide in the air can be suppressed as shown in Fig. 3 (a), and as a result, the amount of impurity phases such as insulators Li2CO3 and La2Zr2O7 on the surface of the ceramic sheet can be reduced as shown in Fig. 3 (b). Accordingly, when a garnet-type oxide ceramic sheet is used as an electrolyte sheet of an all-solid-state battery, the interfacial compatibility between the electrode and the electrolyte layer can be improved, the ionic conductivity of the ceramic sheet can be maintained, the interfacial resistance can be reduced, and dendrite growth can be alleviated.
[0093] According to another embodiment, the garnet-type oxide ceramic sheet may include a surface portion and a deep portion, and the average lithium content of the garnet-type oxide particles present in the surface portion may be higher than the average lithium content of the garnet-type oxide particles present in the deep portion. Here, the garnet-type oxide may be as described above.
[0094] The above surface and deep portions can be determined based on the point where the lithium content differs by analyzing the lithium content according to thickness, and the lithium content can be analyzed, for example, through secondary ion mass spectrometry (SIMS).
[0095] Alternatively, the surface portion and the deep portion may be distinguished based on a depth of 1 μm in the thickness direction from the surface of the ceramic sheet.
[0096] At this time, the 1 / 2 point can be set as the thickness center based on the average thickness of the garnet-type oxide ceramic sheet, and the surface can be set as 0 ㎛, and the thickness from the surface toward the thickness center can be measured.
[0097] The ratio of the average lithium content of the garnet-type oxide of the surface layer to the average lithium content of the garnet-type oxide of the deep layer may be greater than 1 and less than 1.014, specifically greater than 1 and less than 1.01, or greater than 1 and less than 1.009. By having an average lithium content ratio in the above-described range, a ceramic sheet having better atmospheric stability and mechanical stability can be manufactured.
[0098] The average lithium content of the garnet-type oxide of the surface layer may be less than 6.33, specifically 6.32 or less, 6.31 or less, or 6.30 or less, based on the compositional formula of the garnet-type oxide particles when oxygen is 12. In addition, the average lithium content of the garnet-type oxide of the surface layer may be 6.25 or more, 6.27 or more, or 6.28 or more. As the garnet-type oxide particles of the surface layer have an average lithium content in the above-described range, the atmospheric stability may be further improved. Specifically, the average lithium content is such that the compositional formula of the garnet-type oxide particles is Li x Ga 0.25 La3Zr2O 12 If so, it means the value of X.
[0099] The average lithium content of the garnet-type oxide of the above-mentioned deep portion may be less than 6.30 in the stoichiometric ratio of lithium based on the composition formula of the garnet-type oxide particle when oxygen is 12, and may be specifically 6.28 or less, 6.25 or less, 6.24 or less, or 6.23 or less. In addition, the average lithium content of the garnet-type oxide of the above-mentioned deep portion may be 6.20 or more, 6.22 or more, or 6.23 or more.
[0100] The sintering in the step of sintering the garnet-type oxide-based molded body manufactured above is not limited thereto, but can be performed by a method selected from the group consisting of spark plasma sintering, rapid thermal annealing, flash lamp sintering, and laser sintering.
[0101] The sintering in the step of sintering the garnet-type oxide-based molded body manufactured above is not limited thereto, but can be performed by a method selected from the group consisting of spark plasma sintering, rapid thermal annealing, flash lamp sintering, and laser sintering.
[0102] As described above, the garnet-type oxide-based ceramic sheet provided in the present disclosure can have high ionic conductivity by suppressing the reaction with moisture and / or carbon dioxide in the atmosphere, thereby reducing the amount of impurities formed on the surface of the garnet-type oxide-based ceramic sheet, and specifically, can have high lithium ion conductivity of 1.3 mS / cm or more at 25°C.
[0103] In addition, the garnet-type oxide ceramic sheet of the present disclosure has a thickness of 10Х10 -10 It can have an electronic conductivity of less than cm.
[0104] In addition, the garnet-type oxide-based ceramic sheet according to the present disclosure can suppress excessive grain growth by being sintered at a relatively low temperature or for a short time, such as light sintering. As a result, the garnet-type oxide-based ceramic sheet can have grain boundaries and an average grain size of 4 to 200 μm. More specifically, the average grain size can be 4 μm or more, 5 μm or more, or 6 μm or more, and 200 μm or less, 100 μm or less, 50 μm or less, 30 μm or less, or 10 μm or less. By having such a fine grain size, atmospheric stability can be improved. In addition, the garnet-type oxide-based ceramic sheet according to the present disclosure can prevent excessive grain growth, thereby improving mechanical strength.
[0105] An all-solid-state secondary battery comprising a garnet-type oxide-based ceramic sheet according to the present disclosure is provided. Specifically, the all-solid-state secondary battery comprises a negative electrode, a positive electrode, and a solid electrolyte, wherein the solid electrolyte may be a garnet-type oxide-based ceramic sheet provided in the present disclosure.
[0106] The above positive electrode is not particularly limited, and may include a lithium-transition metal oxide such as lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), or lithium nickel oxide (LiNiO2) as a positive electrode active material, or a lithium-transition metal composite oxide in which some of these transition metals are replaced with other transition metals.
[0107] For example, the lithium-transition metal oxide may include nickel (Ni) and may further include at least one selected from the group consisting of cobalt (Co) and manganese (Mn). For example, the cathode active material may include an NCM-based cathode active material; a Mn-rich-based cathode active material; or an LLO (Li rich layered oxides, Over Lithiated Oxides, Over-lithiated layered oxide, OLO, LLOs)-based cathode active material. For example, the lithium-transition metal oxide may be at least one selected from the group consisting of the following chemical formulas 2 to 4.
[0108] [Chemical Formula 2]
[0109] Li a Ni b M 1-b O2
[0110] M may include at least one selected from the group consisting of Na, Mg, Ca, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Co, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, Ba and Zr, specifically may include Co, Mn or Al, more specifically may include Co and Mn, and optionally may further include Al. Furthermore, in the above chemical formula 2, a may be 0.9 or more and 1.2 or less, more specifically may be 0.95 or more and 1.08 or less, and b may be 0.5 or more, more specifically may be 0.6 or more, 0.8 or more, 0.9 or more or 0.98 or more.
[0111] [Chemical Formula 3]
[0112] pLi2MnO3ㆍ(1-p)LiqJO2
[0113] In the above chemical formula 3, J may include one or more elements selected from the group consisting of Mn, Ni, Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg and B, and 0 <p<1이고, 0.9≤q≤1.2일 수 있다.
[0114] [Chemical Formula 4]
[0115] Li 1+x M 1-x O2
[0116] In the above chemical formula 4, 0≤x≤0.4, and M is at least one of Na, Mg, Ca, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Ni, Mn, Co, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, Ba, and Zr. Specifically, in the above chemical formula 4, M may include Ni, Co, Mn, or Al, and more specifically, may include Ni, Co, and Mn, and optionally further include Al.
[0117] Additionally, the above-mentioned positive electrode active material may be a lithium iron phosphate (LFP)-based positive electrode active material, typically represented by the chemical formula LiFePO4.
[0118] In addition, the lithium-transition metal oxide may be a primary particle or a secondary particle. Specifically, the lithium-transition metal oxide may be in the form of a single particle, or may be a secondary particle formed by assembling or agglomerating a plurality of primary particles to form substantially a single particle. Here, the single particle form excludes, for example, a secondary particle formed by assembling or agglomerating a plurality of more than 10 primary particles (for example, more than 10) to form substantially a single particle, and may include a structure in which 2 to 10 single particles are attached or adhered to each other to form a substantially single body form (for example, a structure converted into a single particle). In some embodiments, the positive electrode active material may include both a secondary particle form and a single particle form.
[0119] The above negative electrode is not particularly limited, and the negative electrode active material may be a carbon-based active material such as artificial graphite or natural graphite, or silicon oxide (SiO). x ; 0 <x<2), Si-C 복합체, pure Si 등의 규소계 활물질, 리튬 메탈, 리튬-메탈 합금 등의 금속을 포함할 수 있다.
[0120] Meanwhile, the above-described all-solid-state lithium secondary battery may be a non-anode secondary battery. That is, it may be a battery including an anode that does not form a negative electrode active material layer on the negative electrode current collector during the battery assembly process, that is, an anode made of only the negative electrode current collector. When the non-anode lithium secondary battery is initially charged, the main positive electrode active material and the sacrificial positive electrode active material are delithiated, and lithium ions generated from the positive electrode active material are reduced on the negative electrode current collector to form a lithium metal layer or a lithium layer including a solid lithium layer.
[0121] The method for manufacturing the above-mentioned all-solid-state lithium secondary battery is not particularly limited, but the above-mentioned all-solid-state lithium secondary battery can be manufactured by applying a slurry containing a negative electrode or positive electrode active material on a current collector, then performing a drying and rolling process to manufacture a negative electrode or positive electrode, respectively, applying a slurry containing oxide particles or the like on the negative electrode or positive electrode, then drying the resulting oxide-based thin film sheet, and performing a photo-sintering process on the resulting oxide-based solid electrolyte sheet.
[0122] When the above-described all-solid-state lithium secondary battery includes the oxide-based solid electrolyte sheet described above, there is no risk of fire due to electrolyte leakage, and it can have excellent performance such as high energy density.
[0123] Hereinafter, the present disclosure will be described in more detail with reference to examples. However, the following examples are intended to illustrate specific examples of one implementation and are not intended to limit one implementation.
[0124] Reference Example 1
[0125] Preparation of GLLZO powder
[0126] Raw stoichiometric powders of Li2CO3 (Soekawa Chemicals, 99.9%), La2O3 (High Purity Chemicals, 99.9%), ZrO2 (Samchun Chemicals, 99.9%), and Ga2O3 (High Purity Chemicals, 99.9%) were used as starting reagents and mixed in a stoichiometric ratio. Li2CO3 was weighed in excess of 10% by weight to compensate for Li loss during sintering.
[0127] The above mixture was ball milled at 150 rpm for 24 hours using ZrO2 balls as a grinding medium in a Nalgene bottle containing isopropanol.
[0128] After removing the ZrO2 balls, the slurry was dried in an oven at 80°C for 3 hours. The dried powder was then calcined in air at 850°C for 6 hours to obtain Ga-doped Li 6.25 Ga 0.25 La3Zr2O 12 (GLLZO) was manufactured. The manufactured GLLZO powder was photographed by SEM and is shown in Fig. 4 (a).
[0129] The calcined GLLZO powder was ground by hand and ball milled at 150 rpm for 24 hours in a Nalgene bottle containing isopropanol using ZrO2 balls as a grinding medium to control particle size. The resulting slurry was dried at 80°C for 6 hours and the powder was ground by hand for 10 minutes. The obtained GLLZO powder was photographed by SEM and is shown in Fig. 4(b).
[0130] Furthermore, the particle size distribution of the above-mentioned particle size-controlled GLLZO powder was measured using a Malvern particle size analyzer. v10 , D v50 and D v90was measured, and the results are shown in (c) of Fig. 4.
[0131] Referring to (a) of the above Fig. 4, the calcined powder was a spherical particle with a size of about 10 μm, but by ball milling the calcined powder, the particle size could be adjusted to about 1 μm, as shown in (b) of Fig. 4. Furthermore, referring to (c) of Fig. 4, the particle size distribution of the GLLZO powder whose particle size was adjusted to about 1 μm by the ball milling was Dv(10) of 0.446 μm, Dv(50) of 0.737 μm, and D v90 With this 2.52㎛, we can confirm that it is a mixture of particles with two or more different sizes.
[0132] Manufacturing of ceramic sheets
[0133] The above-obtained GLLZO powder was cold pressed into pellets having a diameter of about 8 mm and a thickness of about 1 mm at 200 MPa using a cold isotactic press.
[0134] The cold-pressed pellets were sintered in air to produce ceramic sheets. At this time, the sintering conditions were as follows: first sintering at 1250°C for 10 minutes, followed by second sintering at 1150°C for 180 minutes to produce ceramic sheets.
[0135] XRD analysis was performed on the above-manufactured ceramic sheet, and the Rietveld fitting results for the XRD are shown in Fig. 5 (a). Furthermore, the characteristics and fitting reliability function values for the above-manufactured ceramic sheet were measured, and the results are shown in Table 1 below.
[0136] The above-mentioned manufactured ceramic sheet was photographed by SEM, and the photograph is shown in Fig. 6 (a).
[0137] Meanwhile, the crystal grain size and relative density of the manufactured ceramic sheet were measured, respectively, and the results are shown in Table 2. The crystal grain size was measured using the SEM image of the ceramic sheet using image J, and the relative density was calculated by dividing the measured density of the sample by the theoretical density. The measured density was obtained by measuring the mass and volume of the sample, and the theoretical density was obtained using the lattice constant of XRD.
[0138] Additionally, the two-probe AC impedance of the above-mentioned manufactured ceramic sheet was measured, and its pattern is shown in Fig. 7.
[0139] In addition, the ionic conductivity of the ceramic sheet manufactured above is shown in Fig. 8. At this time, for comparison, the known lithium ion conductivity value for LLZO including a doping element is also shown in Fig. 8.
[0140] In addition, the resistance according to temperature was measured for the ceramic sheet, and the ionic conductivity according to temperature was analyzed, and the results are shown in Fig. 9.
[0141] Furthermore, a DC polarization test was performed on the above-mentioned manufactured ceramic sheet, and the results are shown in Fig. 10.
[0142] Reference Example 2
[0143] A ceramic sheet (S2) was manufactured by the same method as in Reference Example 1, except that the first sintering temperature was 1200°C.
[0144] The ceramic sheet obtained above was analyzed using the same method as that performed in Reference Example 1, and the analysis results are shown in Table 1, Table 2, Fig. 5 (b), Fig. 6 (b), and Figs. 7 to 10, respectively.
[0145] Example 1
[0146] A ceramic sheet (S3) was manufactured by the same method as in Reference Example 1, except that the second sintering temperature was 1100°C.
[0147] The ceramic sheet obtained above was analyzed using the same method as that performed in Reference Example 1, and the analysis results are shown in Table 1, Table 2, (c) of Fig. 5, (c) of Fig. 6, and Figs. 7 to 10, respectively.
[0148] Evaluation 1. Lithium content analysis of ceramic sheets
[0149] The average lithium content in the deep region (the region from the surface to the center of the thickness from a depth of more than 1 ㎛) of the ceramic sheets of Reference Example 1, Reference Example 2, and Example 1 was analyzed through ICP elemental analysis. The average lithium contents in the surface region of the ceramic sheets of Reference Example 1, Reference Example 2, and Example 1 were 6.43, 6.33, and 6.30, respectively. Here, the average lithium content is the stoichiometric ratio of lithium based on the case where oxygen is 12 in the compositional formula of the garnet-type oxide particles. Specifically, the compositional formula of the garnet-type oxide particles in Reference Example 1, Reference Example 2, and Example 1 is Li x Ga 0.25 La3Zr2O 12 Therefore, the average lithium content refers to the X value.
[0150] In addition, the lithium strength change according to the thickness of the ceramic sheet analyzed by SIMS (Secondary ion mass spectrometry) for the ceramic sheets of Reference Example 1, Reference Example 2, and Example 1, and the lithium content of the deep portion were calculated from the increase in the lithium content of the surface portion (area from the surface to a thickness of 1 μm) compared to the deep portion, thereby analyzing the lithium content of the surface portion. Figure 14 shows the lithium content distribution from the surface portion to the deep portion of the ceramic sheet of Example 1.
[0151] The average lithium contents in the deep portions of the ceramic sheets of Reference Example 1, Reference Example 2, and Example 1 were 6.23, 6.24, and 6.25, respectively. Here, the average lithium contents are the same as described above.
[0152] That is, the ceramic sheets of Reference Example 1, Reference Example 2, and Example 1 all have a higher lithium content in the surface layer than in the deep layer, and the ratio of the average lithium content of the garnet-type oxide in the surface layer to the average lithium content of the garnet-type oxide in the deep layer is 1.008 in Example 1, while it can be confirmed that Reference Example 1 and Reference Example 2 are 1.032 and 1.014, respectively, which is 1.014 or more.
[0153] Evaluation 2. Crystal structure and grain morphology
[0154]
[0155] In the above Table 1, a is the length of one side of the cubic unit cell, and V is the volume of the unit cell. Rwp, Rp, and Rexp are the reliability values of the fitting, and it can be confirmed that the fitting results have sufficient reliability as the values of Rwp, Rp, and Rexp are approximately 10% or less. Li 1-O1 (Å)Х4 is the distance between lithium and oxygen atoms Х4, V Li1 -O (Å 3 ) is the volume, Li1-Li3(Å): the distance between lithium and lithium, <li3-o>(Å) is the distance between lithium and oxygen, V Li3-O (Å 3 ) is the volume, and these values are for the reliability index of the Rietveld refinement and each reliability coefficient value.
[0156] Reference Example 1 Reference Example 2 Example 1 Grain size (㎛) 400 ㎛ or more 200 ㎛ or more + about 4 ㎛ about 6 ㎛ Relative density (%) about 97 about 96 about 94 Li content Surface layer 6.4 36.3 36.30 Deep layer 6.2 36.2 36.25
[0157] Referring to Table 1 above, it was found that the ceramic sheets of Reference Example 1, Reference Example 2, and Example 1 had cubic crystals. Meanwhile, (a) to (c) of FIGS. 5 are drawings showing the Rietveld fitting results for XRD of the ceramic sheets obtained in Reference Example 1, Reference Example 2, and Example 1, and (d) of FIG. 5 is the XRD analysis result of the GLLZO ceramic sheet. Referring to (a) to (d) of FIGS. 5, it can be confirmed that the Rietveld fitting results for the XRD of the ceramic sheets obtained in Reference Example 1, Reference Example 2, and Example 1 are reliable. From this, it was found that the ceramic sheets manufactured in Reference Example 1, Reference Example 2, and Example 1 were all GLLZO.
[0158] FIG. 6 is an SEM photograph of the ceramic sheets of Reference Example 1, Reference Example 2, and Example 1. Referring to FIG. 6 (a), the ceramic sheet of Reference Example 1 exhibited a large grain size without distinct grain boundaries due to grain growth. In addition, referring to the results of analyzing the SEM image of the ceramic sheet in Table 2 using the Image J program, it can be seen that the manufactured ceramic sheet had a grain size of 400 μm or more, the grains were tightly bonded, and had a very high relative density of about 97%, thereby having a high-density microstructure. Furthermore, it can be confirmed that spherical pores partially existed on the surface, and although not intended to be bound by a particular theory, the pores may have been formed due to the loss of some lithium during the sintering process.
[0159] Referring to Fig. 6 (b), it was confirmed that the ceramic sheet of Reference Example 2 had coexistence of normal grains (NGG) and coarse grains (AGG) due to the growth of some grains. In addition, referring to Table 2 above, it was confirmed that the ceramic sheet manufactured in Reference Example 2 had a high-density microstructure by including coarse grains (AGG) having a grain size of 200 ㎛ or more and normal grains (NGG) having a grain size of about 4 ㎛, and having a relative density of about 96%. However, no spherical pores were observed on the surface.
[0160] Referring to Fig. 6 (C) and Table 2, it was confirmed that the ceramic sheet of Example 1, in which the ratio of the average lithium content of the garnet-type oxide in the surface layer to the average lithium content of the garnet-type oxide in the deep layer is greater than 1 and less than 1.014, and the lithium content of the surface layer is less than 6.33, had normal grains with a grain size of about 6 ㎛ observed in the entire ceramic sheet in a transgranular morphology without the formation of coarse grains (AGG) due to grain growth.
[0161] Meanwhile, referring to Table 2 above, it can be confirmed that the ceramic sheet of the reference example has an excellent relative density of about 94% and no spherical pores are observed on the surface, thus having a high-density microstructure.
[0162] Evaluation 3. Ionic Conductivity
[0163] FIG. 7 shows electrochemical impedance spectroscopy (EIS) measurements performed to investigate the effect of microstructure on lithium ion conductivity of ceramic sheets manufactured in Reference Examples 1, 2, and Example 1, showing the impedance spectra at 25°C and the enlarged high-frequency region for each ceramic sheet.
[0164] The spectrum shown in Fig. 7 shows a partially depressed semicircle at high frequencies and a strong increase in the imaginary impedance at low frequencies, which is due to Li at the electrode-electrolyte interface (electrode). + This may be due to the blocking of the pellet. The high frequency part is related to the total impedance of the pellet, i.e. the bulk contribution, and the bulk resistance (R bulk ) and electrode resistance (R el ) were estimated by fitting the impedance spectrum using the equivalent circuit based on the Bricklayer model.
[0165] Two parallel RQ circuits connected in series were used to fit the impedance data shown in Fig. 7, where Q is a constant phase factor C = (R 1- n Q) 1 / n , where n is a fitting parameter.
[0166] The above fitting clearly showed the bulk transport process of all samples, and therefore the total lithium ion conductivity (σ total ) is R of the following formula bulk can be estimated using .
[0167]
[0168] Here, t and A are the thickness and area of the ceramic sheet, respectively.
[0169] The lithium ion conductivities of the ceramic sheets manufactured in Reference Example 1, Immersion Example 2, and Example 1 were obtained along with the known lithium ion conductivity values for LLZO including doping elements, and are shown in FIG. 8. Referring to FIG. 8, it can be confirmed that the ion conductivities of the ceramic sheets manufactured in Reference Example 1, Immersion Example 2, and Example 1 are all excellent, at ~1.7, ~1.6, and ~1.3 mS / cm, respectively, at 25°C.
[0170] The resistance according to temperature was measured for the ceramic sheets of Reference Example 1, Immersion Example 2 and Example 1, and the ionic conductivity according to temperature was analyzed, and the Arrhenius plot is shown in Fig. 9. In Fig. 9, the activation energy (E a ) was extracted from the Arrhenius plot of Fig. 9 using the following equation.
[0171]
[0172] Here σ O and K B are the pre-exponential constant and the Boltzmann constant, respectively.
[0173] σ obtained for the ceramic sheets of Reference Example 1, Immersion Example 2 and Example 1 total The values are ~0.27, ~0.28, and ~0.29 eV, respectively, and it can be confirmed that they are consistent with the ionic conductivity and trend.
[0174] In addition, the electronic conductivity (σ) for lithium ion conductivity in the ceramic sheets of each of Reference Example 1, Reference Example 2 and Example 1 elec ) were performed to quantify the contribution of the ceramic sheets, and the results are shown in Fig. 10. Fig. 10 shows the current-time plot at a DC polarization of 250 mV at 25°C, showing that the current initially decreased over time but gradually reached a steady state (~14 to 60 pA) for all ceramic sheets.
[0175] Evaluation 4. Surface Evaluation Based on Air Exposure
[0176] Three ceramic sheets each of the above-mentioned Reference Example 1, Immersion Example 2, and Example 1 were prepared. Each of the prepared ceramic sheets (a), a ceramic sheet stored in a vacuum desiccator at 25°C for 9 months (b), and a ceramic sheet left in the air for 2 weeks (c) were prepared, respectively.
[0177] For each of the three types of ceramic sheets of each of the above-mentioned Reference Example 1, Immersion Example 2, and Example 1, the surface condition of each ceramic sheet was observed using a scanning electron microscope (SEM) to evaluate the formation of Li2CO3, and the SEM image according to the SEM observation is shown in Fig. 11.
[0178] Referring to Fig. 11, cracks occurred along grain boundaries on the surface of the sintered body, as shown in the ceramic sheet (b) after being stored in the desiccator of Reference Example 1 and the ceramic sheet (c) after being exposed to air. In addition, similar cracks occurred in the ceramic sheet (b) and the ceramic sheet (c) of Reference Example 2. However, no traces of cracks or breakage were found in the ceramic sheet (b) after being stored in the desiccator of Example 1 and the ceramic sheet (c) after being exposed to air.
[0179] In addition, the surface color of the ceramic sheets (b) and (c) of Reference Examples 1 and 2 changed from white to black. Although not intended to be bound by a specific theory, it is assumed that a mossy reaction layer was formed on the surface of the ceramic sheets (b) and (c) through a reaction with carbon dioxide. Such a mossy reaction layer may mean that a secondary phase was formed on the surface of the sintered body during storage in the air and in a desiccator, and the ceramic sheets of Reference Examples 1 and 2 may be spontaneously crushed, resulting in a decrease in lithium ion conductivity.
[0180] However, referring to Fig. 11, the ceramic sheet of Example 1 having smaller crystal grains showed no surface damage, no signs of deterioration or formation of impure layers, such as changes in surface color. Accordingly, it was confirmed that the structure was stably maintained without the occurrence of cracks.
[0181] In summary, it can be confirmed that the ceramic sheet of Example 1 does not easily develop cracks in the specimen even when exposed to air for a large amount or for a long time. Although not intended to be bound by a specific theory, the cracks are generated by applying stress to the specimen when the insulator Li2CO3 is generated, and ultimately, they can propagate along defects (grain boundaries, voids, etc.) in the specimen from the generated cracks, which can lead to complete destruction of the sample after a certain period of time. However, since the ceramic sheet of Example 1 does not easily develop cracks, the generation of an insulator phase is less, and the reaction of lithium with moisture or carbon dioxide on the surface is less.
[0182] Evaluation 5. Electrical Characteristics Evaluation According to Air Exposure
[0183] Electrochemical impedance analysis was performed on each of the three types of ceramic sheets of each of Reference Example 1, Reference Example 2 and Example 1 using a potentiostat (VMP-300, manufactured by BioLogic (France)) to measure the resistance component and ionic conductivity (σ total ) was calculated. The complex impedance spectrum and the change in lithium ion conductivity were measured at 25°C, and the results are shown in Fig. 12. The Nyquist plots for the results of the change in the complex impedance spectrum and lithium ion conductivity measured for each of the three types of ceramic sheets of each of Reference Example 1, Reference Example 2, and Example 1 are shown in A to C of Fig. 12.
[0184] Specifically, A of FIG. 12 is a ceramic sheet of Reference Example 1, B is a ceramic sheet of Reference Example 2, and C is a ceramic sheet of Example 1, which respectively show the complex impedance spectra for the ceramic sheets in the states (a), (b), and (c) described above. Meanwhile, D of FIG. 12 shows the results of measuring the change in lithium ion conductivity according to the ceramic sheets in the states (a), (b), and (c) for each of Reference Example 1, Reference Example 2, and Example 1.
[0185] Referring to A and B of FIG. 12, the total impedance of the ceramic sheet (b) after desiccator storage and the ceramic sheet (c) after exposure to the air increased compared to the ceramic sheet (a) of Reference Examples 1 and 2. However, it can be confirmed that the ceramic sheet (b) and the ceramic sheet (c) of Example 1 have impedance values that are not significantly different from the impedance value of the ceramic sheet (a).
[0186] Meanwhile, the lithium ion conductivity shown in D of Fig. 12 is determined by fitting the corresponding impedance spectrum to an equivalent RC circuit, and σ total It can be confirmed that the values are significantly reduced in the ceramic sheet (b) after desiccator storage and in the ceramic sheet (c) after air exposure compared to the ceramic sheet (a) of each of Reference Examples 1 and 2, and in particular, it can be seen that the conductivity of the ceramic sheet (c) directly exposed to air is reduced more rapidly compared to the ceramic sheet (b) aged in a desiccator.
[0187] Specifically, in the ceramic sheet of Reference Example 1, the ceramic sheet (c) aged in air has a σ of about 4 times (0.0002 mS / cm) higher than that of the ceramic sheet (a). total While the ceramic sheet aged in a desiccator (b) shows a decrease in σ of about 3 times (0.0079 mS / cm) total The degree of decrease was shown. Meanwhile, in the ceramic sheet of Reference Example 2, σ of the ceramic sheet (c) aged in air total The degree of decrease was about 3 times the value, and in the case of the ceramic sheet (b) stored in the desiccator, it was about 2 times σ total The degree of reduction was shown.
[0188] However, in the ceramic sheet of Example 1, the ionic conductivity of the ceramic sheet (c) aged in air was 1.1 mS / cm, and the ionic conductivity of the ceramic sheet (b) aged in a desiccator was 1.2 mS / cm, showing no significant change from the ionic conductivity of the ceramic sheet (a). Therefore, it can be confirmed that the ceramic sheet of Example 1 having an NGG microstructure has superior air stability compared to the ceramic sheets of Reference Examples 1 and 2 containing AGG.
[0189] Furthermore, without being bound by any particular theory, it is believed that the ceramic sheets of Reference Examples 1 and 2 containing larger sintered particles have lower fracture strength and fracture more easily when exposed to air, whereas the ceramic sheet of Example 1 having smaller grains may have higher fracture strength even when exposed to air due to the tightly bonded grain boundaries. Additionally, the hardness of Al-doped LLZO ceramic sheets decreases with increasing grain size, and a ceramic sheet having coarse grains may have lower mechanical strength than a ceramic sheet having fine grains.
[0190] Evaluation 6. Evaluation of surface Li2CO3 content
[0191] Figure 13 shows Raman Microscopy images of ceramic sheets (a) to (c) manufactured in each of Reference Example 1, Reference Example 2 and Example 1 at 200 to 1200 cm2 using NANOBASE. -1 Raman analysis was performed over a range of frequencies, and the results of the Raman analysis are shown in A to C, and the change in the peak intensity ratio of Li2CO3 / LLZO according to each ceramic sheet is shown.
[0192] As shown in Fig. 13, the Li2CO3 / LLZO peak ratios were approximately 4.5% and approximately 2% for the ceramic sheets (a) of Reference Examples 1 and 2, respectively. On the other hand, no peak corresponding to Li2CO3 was detected in the ceramic sheet (a) of Example 1. These results indicate that a large amount of Li2CO3 was formed on the surface of the sintered body having larger crystal grains.
[0193] In addition, the Li2CO3 / LLZO peak intensity ratio gradually increased in the order of ceramic sheet (b) and ceramic sheet (c) in all cases of Reference Example 1, Reference Example 2, and Example 1. However, the Li2CO3 / LLZO peak intensity ratio was significantly lower in the ceramic sheet of Example 1 than in Reference Examples 1 and 2. Therefore, in the ceramic sheets (b) and (c) of Reference Examples 1 and 2 including the AGG structure, Li2CO3 grew abnormally on the entire or partial surface, but in the ceramic sheets (b) and (c) of Example 1 having the NGG microstructure, less Li2CO3 was formed, and the amount generated also decreased over time.
[0194] That is, when Li2CO3 is formed on the surface of a ceramic sheet, lithium ion conductivity may decrease, and it can be seen that this occurs more easily in ceramic sheets containing coarse grains with weak mechanical strength. Therefore, compared to the ceramic sheets of Reference Examples 1 and 2, the ceramic sheet of Example 1 may have better air stability because the Li2CO3 phase is less formed on the surface.
Claims
1. A garnet-type oxide ceramic sheet including a garnet-type oxide, The above garnet-type oxide ceramic sheet includes a surface layer and a deep layer, The average lithium content of the garnet-type oxide particles in the surface layer is greater than the average lithium content of the garnet-type oxide particles in the deep layer, A garnet-type oxide ceramic sheet, wherein the ratio of the average lithium content of the garnet-type oxide in the surface layer to the average lithium content of the garnet-type oxide in the deep layer is greater than 1 and less than 1.
014.
2. A garnet-type oxide ceramic sheet in the first paragraph, wherein the surface portion is a region from one surface of the ceramic sheet to a thickness of 1 μm, and the deep portion is a region from the thickness of 1 μm to the center of the thickness.
3. In the first paragraph, a garnet-type oxide ceramic sheet having an average lithium content of the garnet-type oxide of the surface layer, wherein the stoichiometric ratio of lithium is less than 6.33 based on the composition formula of the garnet-type oxide particles when oxygen is 12.
4. A garnet-type oxide ceramic sheet according to claim 1, wherein the garnet-type oxide comprises an LLZO-type oxide.
5. In the fourth paragraph, the LLZO-based oxide is a garnet-type oxide-based ceramic sheet containing a doping element.
6. In the fifth paragraph, the LLZO-based oxide is a garnet-type oxide-based ceramic sheet comprising at least one type of doping element selected from the group consisting of Ga and Al at the Li site.
7. In the first paragraph, the ceramic sheet is a garnet-type oxide ceramic sheet having a lithium ion conductivity of 1.3 mS / cm or more at 25°C.
8. In the first paragraph, the ceramic sheet has a size of 10Х10 -10 A garnet-type oxide ceramic sheet having an electronic conductivity of less than cm.
9. In the first paragraph, the ceramic sheet is a garnet-type oxide ceramic sheet having grain boundaries and an average grain size of 4 to 200 μm.
10. A step of manufacturing an oxide molded body by molding garnet-type oxide powder having an average particle size of 1㎛ or less and two or more particle sizes into a predetermined shape; and It includes a step of sintering the above oxide molded body to manufacture a sintered body, A method for manufacturing a garnet-type oxide ceramic sheet, wherein the above sintering includes first sintering and second sintering, and the first sintering temperature is higher than the second sintering temperature.
11. A method for manufacturing a garnet-type oxide ceramic sheet in the 10th paragraph, wherein the first sintering temperature is 1050 to 1400°C, and the second sintering temperature is 1000 to 1300°C.
12. In paragraph 10, A step of producing calcined garnet-type oxide powder by calcining precursor powder; and A step of pulverizing the above calcined garnet-type oxide powder to provide garnet-type oxide powder having two or more particle sizes. A method for manufacturing a garnet-type oxide ceramic sheet, further comprising:
13. In the 12th paragraph, the calcined garnet-type oxide powder is D 10 This is less than 1㎛, and D 50 A method for manufacturing a ceramic sheet having a diameter of 1 μm to 30 μm.
14. A method for manufacturing a ceramic sheet according to any one of claims 10 to 13, wherein the garnet-type oxide includes an LLZO-type oxide.
15. Containing a cathode, anode and solid electrolyte, The above solid electrolyte is a ceramic sheet according to any one of claims 1 to 9. All-solid-state secondary battery.
Citation Information
Patent Citations
A dry preparation process for solid electrolytes
CN113880577B
Solid electrolyte, all-solid secondary battery, and manufacturing method thereof
JP2020140963A
System and method for controlling vehicle
KR1020230158841A
Galium- gadolinium dopped solid electrolyte material for all-solid-state lithium secondary battery and method for preparing the same
KR102200967B1
Method and system for predictive maintenance of probe station
KR102252740B1