Coated positive electrode material, and preparation method therefor and use thereof
Through gas-phase coating technology, Li2SiO3/LiF and Si3N4 composite clad layer is formed on high-nickel ternary cathode material, which solves the problem of material deterioration caused by residual lithium and residual alkali, improves the cycle life and safety of lithium-ion batteries, and realizes the realization of the More even and stable coating effect.
Patent Information
- Application Number
- PCT/CN2023/092282
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-14
Smart Images

Figure PCTCN2023092282-FTAPPB-I100001
Abstract
Description
Coated positive electrode material and its preparation method and application Technical Field
[0001] The present disclosure belongs to the technical field of lithium-ion battery positive electrode materials, and particularly relates to a coated positive electrode material and a preparation method and application thereof. Background Art
[0002] With the pursuit of energy conservation and environmental protection, new energy vehicles have rapidly become a hot topic in the automotive market. Lithium-ion batteries, due to their high energy density, long cycle life, and environmental friendliness, have become a research hotspot in the new energy industry. The cathode material is the core of lithium-ion batteries and plays a decisive role in their energy density.
[0003] Nickel cobalt manganese oxide ternary positive electrode materials have the advantages of high specific capacity, high energy density, low price and environmental friendliness. The discharge capacity of high nickel ternary materials can reach more than 200mAh / g. However, since nickel ions are easily reduced and enter the lithium layer, serious ion mixing will occur, lithium is easily precipitated, and the extra lithium salt added during sintering will also remain on the surface of the material in the form of oxides.
[0004] Residual lithium is very sensitive to moisture and easily absorbs water and carbon dioxide in the air to generate lithium hydroxide and lithium carbonate, causing the material surface to deteriorate. Materials with excessive residual lithium can easily form a jelly-like slurry during the homogenization and coating process of battery production, resulting in uneven coating, which can easily lead to problems such as difficulty in electrode production and capacity decay. Furthermore, residual lithium has poor conductivity, which hinders the intercalation and deintercalation of lithium ions and causes polarization of the electrode. Residual alkali easily reacts with the electrolyte at high temperatures to generate gas, causing battery bloating and posing serious safety hazards. Therefore, high-nickel ternary positive electrode materials have more stringent requirements for storage conditions and subsequent processing conditions.
[0005] To address these issues, high-nickel materials are typically treated with water washing or surface coating to reduce residual alkali production. However, water washing consumes significant amounts of water and reacts with the high-nickel ternary cathode material, leading to lithium loss, structural damage, and ultimately reduced capacity. Solid-phase coatings, on the other hand, suffer from poor surface uniformity and are unable to completely isolate the material from H2O and CO2 in the air.
[0006] Chinese patent CN108807969A discloses a method for reducing residual alkali on the surface of layered positive electrode materials for lithium-ion batteries. This method involves water washing to reduce residual alkali on the surface, followed by alcohol washing to quickly remove residual surface moisture, and then sintering to stabilize the surface structure by adding nano-zirconia. This invention effectively reduces residual alkali on the surface of the positive electrode material. However, the material structure is destroyed after water washing, and despite the addition of nano-zirconia to stabilize the surface structure, significant lithium loss during the water washing process remains.
[0007] Summary of the Invention
[0008] The present disclosure aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present disclosure provides a coated positive electrode material and its preparation method and application.
[0009] According to one aspect of the present disclosure, a method for preparing a coated positive electrode material is proposed, comprising the following steps:
[0010] The positive electrode material is placed in a reaction device, silicon tetrafluoride gas is introduced first to heat the reaction, and then ammonia gas is introduced to heat the reaction. After the reaction is completed, the reaction is cooled to obtain the coated positive electrode material.
[0011] The present invention utilizes silicon tetrafluoride gas to react with residual alkaline components (Li2CO3 and LiOH) on the surface of the positive electrode material to form a Li2SiO3 / LiF composite coating layer on the surface of the positive electrode material, and then introduces ammonia gas to cause the residual silicon tetrafluoride gas in the reaction device to react with ammonia gas to generate silicon nitride, which is deposited on the surface of the positive electrode material after cooling. The reaction formula is as follows: SiF4+6LiOH==Li2SiO3+4LiF+3H2O; SiF4+2Li2CO3+2H2O==H4SiO4+4LiF+2CO2; 3SiF4+4NH3==Si3N4+12HF.
[0012] In some embodiments of the present disclosure, the positive electrode material is a high-nickel ternary positive electrode material or a lithium iron phosphate material.
[0013] In some embodiments of the present disclosure, the chemical formula of the high nickel ternary cathode material is LiNi x Co y Mn z O2, 0.7≤x≤0.9, 0.05≤y≤0.15, 0.05≤z≤0.15, and x+y+z=1.
[0014] In some embodiments of the present disclosure, the average particle size D50 of the positive electrode material is 2-15 μm.
[0015] In some embodiments of the present disclosure, the temperature of the silicon tetrafluoride gas heated during the reaction is 500-600°C.
[0016] In some embodiments of the present disclosure, the flow rate of the silicon tetrafluoride gas is 0.05-0.15 L / min.
[0017] In some embodiments of the present disclosure, the time for heating the reaction by introducing the silicon tetrafluoride gas is 2-4 hours.
[0018] In some embodiments of the present disclosure, the reaction device is a tubular furnace; and the filling volume ratio of the positive electrode material in the reaction device is 5%-15%.
[0019] In some embodiments of the present disclosure, after the cathode material is placed in a reaction device, a protective gas is introduced to expel oxygen, the temperature is raised to the reaction temperature at a rate of 2-10°C / min, and then the silicon tetrafluoride gas is introduced to react.
[0020] In some embodiments of the present disclosure, the temperature of the ammonia gas introduced for heating the reaction is 500-600°C.
[0021] In some embodiments of the present disclosure, the flow rate of the ammonia gas is 0.01-0.1 L / min.
[0022] In some embodiments of the present disclosure, the heating reaction time of the ammonia gas is 0.5-2 hours. The amount of the Si3N4 coating layer can be controlled by controlling the flow rate of the ammonia gas and the reaction time.
[0023] The present disclosure also provides a coated positive electrode material, which is prepared by the preparation method. The coated positive electrode material is coated with a Li2SiO3 / LiF composite coating layer and a Si3N4 coating layer in sequence from the inside to the outside.
[0024] In some embodiments of the present disclosure, the coating amount of the Si3N4 coating layer is 0.2%-1% of the mass of the positive electrode material.
[0025] The present disclosure also provides application of the coated positive electrode material in a lithium-ion battery.
[0026] The present disclosure has at least the following beneficial effects:
[0027] 1. The present invention uses a vapor-phase coating method to fully contact SiF4 with the surface of the positive electrode material. SiF4 does not damage the ternary material structure and reacts with the residual alkali components (Li2CO3 and LiOH), which can reduce the amount of residual alkali on the material surface without causing lithium loss, forming a conductive Li2SiO3 / LiF composite coating layer. After the residual alkali is completely reacted, NH3 is introduced to react with the remaining SiF4. The resulting Si3N4 is deposited on the surface of the positive electrode material, making the coating more uniform and complete, thereby improving the cycle life, cycle stability, and safety of the positive electrode material.
[0028] 2. Through gas-solid reaction, the damage to the structure of the positive electrode material and the loss of lithium caused by liquid immersion are avoided, and the problem of uneven solid phase grinding can be effectively avoided. The gas-solid contact makes the residual alkali removed more completely, and the obtained coating layer has high uniformity, which can avoid direct contact between the positive electrode material and the electrolyte. Si3N4 has the characteristics of high hardness, wear resistance, corrosion resistance, and high thermal stability. As a coating layer, it can effectively enhance the strength of the positive electrode material and stabilize the material structure.
[0029] 3. The Li2SiO3 / LiF composite coating is selectively generated at the residual alkali site. Si3N4 can increase the uniformity of the coating and enhance the protective effect of the coating. The Si3N4 coating is non-conductive, while the Li2SiO3 / LiF composite coating has lithium ion conductivity. The synergistic effect of the two can enhance the strength of the material without reducing the lithium ion conductivity of the material. DETAILED DESCRIPTION
[0030] The following will clearly and completely describe the concept and technical effects of the present disclosure in conjunction with embodiments to fully understand the purpose, features and effects of the present disclosure.
[0031] Example 1
[0032] This embodiment prepares a coated ternary cathode material, and the specific process is as follows:
[0033] (1) 1 kg of high nickel ternary positive electrode material LiNi with an average particle size D50 of 10 μm 0.8 Co 0.1 Mn 0.1 O2 powder is placed in a tube furnace;
[0034] (2) A protective gas was introduced into the tube furnace to completely expel oxygen, and the temperature was raised to 600°C at a rate of 10°C / min. Silicon tetrafluoride gas was then introduced at a flow rate of 0.15 L / min. The reaction time was 2 h, and the residual alkali was converted into a Li2SiO3 / LiF composite coating.
[0035] (3) Maintaining the temperature of step (2), ammonia gas was introduced into the tube furnace at a gas flow rate of 0.1 L / min and a reaction time of 0.5 h;
[0036] (4) After naturally cooling to room temperature, Si3N4 is deposited on the surface of the positive electrode material to form a uniform coating layer. The mass of the Si3N4 coating layer is 1% of the mass of the high-nickel ternary positive electrode material.
[0037] Example 2
[0038] This embodiment prepares a coated ternary cathode material, and the specific process is as follows:
[0039] (1) 1 kg of high nickel ternary positive electrode material LiNi with an average particle size D50 of 2.7 μm 0.7 Co 0.1 Mn 0.2 O2 powder is placed in a tube furnace;
[0040] (2) A protective gas was introduced into the tube furnace to completely expel oxygen, and the temperature was raised to 550°C at a rate of 5°C / min. Silicon tetrafluoride gas was then introduced at a flow rate of 0.1 L / min. The reaction time was 2.5 h, and the residual alkali was converted into a Li2SiO3 / LiF composite coating layer;
[0041] (3) Maintaining the temperature of step (2), ammonia gas was introduced into the tube furnace at a gas flow rate of 0.05 L / min and a reaction time of 0.5 h;
[0042] (4) After naturally cooling to room temperature, Si3N4 is deposited on the surface of the positive electrode material to form a uniform coating layer. The mass of the Si3N4 coating layer is 0.5% of the mass of the high-nickel ternary positive electrode material.
[0043] Example 3
[0044] This embodiment prepares a coated ternary cathode material, and the specific process is as follows:
[0045] (1) 1 kg of high nickel ternary positive electrode material LiNi with an average particle size D50 of 14.3 μm 0.9 Co 0.05 Mn 0.05 O2 powder is placed in a tube furnace;
[0046] (2) A protective gas was introduced into the tube furnace to completely expel oxygen, and the temperature was raised to 500°C at a rate of 2°C / min. Silicon tetrafluoride gas was then introduced at a flow rate of 0.05 L / min. The reaction time was 4 h, and the residual alkali was converted into a Li2SiO3 / LiF composite coating.
[0047] (3) Maintaining the temperature of step (2), ammonia gas was introduced into the tube furnace at a gas flow rate of 0.01 L / min and a reaction time of 2 h;
[0048] (4) After naturally cooling to room temperature, Si3N4 is deposited on the surface of the positive electrode material to form a uniform coating layer. The mass of the Si3N4 coating layer is 0.2% of the mass of the high-nickel ternary positive electrode material.
[0049] Comparative Example 1
[0050] This comparative example prepares a low residual alkali ternary positive electrode material. The difference from Example 1 is that the high nickel ternary material LiNi is directly removed by water washing. 0.8 Co 0.1Mn 0.1 The residual alkali on the surface of O2. The specific process is:
[0051] (1) 1 kg of high nickel ternary positive electrode material LiNi with an average particle size D50 of 10 μm 0.8 Co 0.1 Mn 0.1 Disperse O2 powder into 2kg of clean water, stir and wash for 10min at a stirring speed of 1000r / min and a washing temperature of 35℃;
[0052] (2) After washing, the ternary material is separated from the water by filtration and dried in vacuum at 100°C for 4 h to obtain the washed low residual alkali ternary positive electrode material.
[0053] Comparative Example 2
[0054] This embodiment prepares a coated ternary cathode material, and the specific process is as follows:
[0055] (1) 1 kg of high nickel ternary positive electrode material LiNi with an average particle size D50 of 10 μm 0.8 Co 0.1 Mn 0.1 O2 is mixed with 10g Al2O3 and ground;
[0056] (2) calcining in a tubular furnace at a temperature of 600°C for 5 hours;
[0057] (3) Cool to room temperature and grind to obtain Al2O3-coated LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0058] Comparative Example 3
[0059] This embodiment prepares a coated ternary cathode material. The difference from Example 1 is that no ammonia gas is introduced into the reaction. The specific process is as follows:
[0060] (1) 1 kg of high nickel ternary positive electrode material LiNi with an average particle size D50 of 10 μm 0.8 Co 0.1 Mn 0.1 O2 powder is placed in a tube furnace;
[0061] (2) A protective gas was introduced into the tube furnace to completely expel oxygen, and the temperature was raised to 600°C at a rate of 10°C / min. Silicon tetrafluoride gas was then introduced at a flow rate of 0.15 L / min, and the reaction time was 2 h.
[0062] (3) After cooling naturally to room temperature, LiNi containing Li2SiO3 / LiF composite coating layer is obtained 0.8 Co0.1 Mn 0.1 O2.
[0063] Test example
[0064] 1. The residual lithium of the high-nickel ternary positive electrode materials obtained in the examples and comparative examples was detected, and the results are shown in Table 1.
[0065] 2. To test the electrochemical properties of the high-nickel ternary positive electrode material, the materials prepared in the examples and comparative examples were made into positive electrode sheets: the high-nickel ternary material, binder PVDF, and conductive agent SP were dissolved in NMP at a mass ratio of 8:1:1, stirred to form a slurry, and the slurry was coated on aluminum foil, dried, and assembled into button batteries. Charge, discharge, and cycle tests were performed. The results are shown in Table 1.
[0066] Table 1 Residual lithium and electrochemical performance test of the embodiments and comparative examples
[0067] As can be seen from Table 1, the residual lithium content in Comparative Example 1 is similar to that in Example 1, but the discharge capacity and cycle performance are lower than those in Example 1. This is because Comparative Example 1 uses a water washing method to remove residual lithium, which damages the material structure to a certain extent after washing, resulting in a decrease in material capacity and cycle performance. The discharge capacity and cycle performance of Comparative Example 2 are also somewhat lower than those in Example 1. This is because Comparative Example 2 uses solid-phase coating, and the surface uniformity of the coating layer is poor, which cannot completely block the material from contact with H2O and CO2 in the air. Comparative Example 3 introduces silicon tetrafluoride gas to react with residual alkali, achieving a good effect in reducing residual alkali. However, due to the lack of silicon nitride coating, its electrochemical performance is still inferior to that of Example 1.
Claims
1. A method for preparing a coated positive electrode material, characterized in that: The following steps are involved: The positive electrode material is placed in a reaction device, silicon tetrafluoride gas is introduced first to heat the reaction, and then ammonia gas is introduced to heat the reaction. After the reaction is completed, the reaction is cooled to obtain the coated positive electrode material.
2. The preparation method according to claim 1, characterized in that: The positive electrode material is a high-nickel ternary positive electrode material or a lithium iron phosphate material.
3. The preparation method according to claim 2, characterized in that: The chemical formula of the high nickel ternary positive electrode material is LiNi x Co y Mn z O2, 0.7≤x≤0.9, 0.05≤y≤0.15, 0.05≤z≤0.15, and x+y+z=1.
4. The preparation method according to claim 1, characterized in that: The average particle size D50 of the positive electrode material is 2-15 μm.
5. The preparation method according to claim 1, characterized in that: The temperature of the silicon tetrafluoride gas heated to react is 500-600°C.
6. The preparation method according to claim 1, characterized in that: The flow rate of the silicon tetrafluoride gas is 0.05-0.15 L / min.
7. The preparation method according to claim 1, characterized in that: The time for heating the reaction by introducing the silicon tetrafluoride gas is 2-4 hours.
8. The preparation method according to claim 1, characterized in that: The reaction device is a tubular furnace; the filling volume ratio of the positive electrode material in the reaction device is 5%-15%.
9. The preparation method according to claim 1, characterized in that: After placing the positive electrode material in a reaction device, first introduce protective gas to expel oxygen, heat to the reaction temperature at a rate of 2-10° C. / min, and then introduce the silicon tetrafluoride gas to react.
10. The preparation method according to claim 1, characterized in that: The temperature of the ammonia gas for heating reaction is 500-600°C.
11. The preparation method according to claim 1, characterized in that: The flow rate of the ammonia gas is 0.01-0.1 L / min.
12. The preparation method according to claim 1, characterized in that: The time for heating the reaction by introducing the ammonia gas is 0.5-2h.
13. A coated positive electrode material, characterized in that: Prepared by the preparation method described in claims 1-12, the coated positive electrode material is coated with a Li2SiO3 / LiF composite coating layer and a Si3N4 coating layer in sequence from the inside to the outside.
14. The coated positive electrode material according to claim 13, characterized in that: The coating amount of the Si3N4 coating layer is 0.2%-1% of the mass of the positive electrode material.
15. Use of the coated positive electrode material according to claim 13 in a lithium ion battery.
Citation Information
Patent Citations
Method for preparing lithium silicate coated lithium ion battery ternary layered anode material
CN104505505A
Fluorine-containing lithium ion battery positive electrode material and preparation method thereof
CN107732199A
Composite material and preparation method thereof
CN111063866A
Nitride / graphitized carbon nanosheet coated ternary positive electrode material and preparation method thereof
CN114023936A
Positive electrode material and preparation method thereof
CN114864886A