Moisture-proof s-type hot aerosol fire extinguishing agent and preparation method therefor

The strontium nitrate is coated through the eutectic-coating process, which solves the problem of high hygroscopicity of S-type hot aerosol fire extinguishing agent, extends the service life and improves the fire extinguishing efficiency, and achieves a better modification effect.

WO2024229917A1PCT designated stage expired Publication Date: 2024-11-14HUBEI JIANDUN FIRE TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/098884
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2023-06-07
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Due to the strong hygroscopicity of strontium nitrate, the traditional S-type hot aerosol fire extinguishing agent has a short service life, high storage requirements and limited application range. The existing coating methods have problems such as large amounts of use and negative ignition performance.

Method used

Using eutectic-coating process, the oxidant and the coating agent are blended and dissolved in water. The oxidant and the coating agent are co-crystallized by volatilization of the alcohol solution, and then the reducing agent and binder are added to achieve the 2nd through the granulation process. Sub-coated to reduce the hygroscopicity of strontium nitrate.

Benefits of technology

It effectively reduces the hygroscopicity of strontium nitrate, extends the service life of the fire extinguishing agent, and improves production efficiency and fire extinguishing efficiency, and reduces the hygroscopicity to below 0.60%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023098884-FTAPPB-I100001
    Figure PCTCN2023098884-FTAPPB-I100001
Patent Text Reader

Abstract

Disclosed in the present invention are a moisture-proof S-type hot aerosol fire extinguishing agent and a preparation method therefor. By utilizing the dissolution properties of raw materials and using an "eutectic-coating" process, the method dissolves an oxidizing agent and a coating agent in water, then forms an eutectic oxidizing agent having a coating layer by using an anti-solvent method, coats the oxidizing agent in a targeted mode, then disperses a reducing agent into the oxidizing agent, and finally adds an adhesive therein for granulation and surface coating. A dual action of eutectic and coating forms the coating layer on the oxidizing agent, which hinders moisture absorption processes of the oxidizing agent and a hot aerosol fire extinguishing agent, and prepares the moisture-proof S-type hot aerosol fire extinguishing agent, thus reducing the storage requirements for hot aerosol fire extinguishing agents, prolonging the service life and expanding the use range.
Need to check novelty before this filing date? Find Prior Art

Description

A moisture-proof S-type hot aerosol fire extinguishing agent and preparation method Technical Field

[0001] The invention belongs to the technical field of aerosol fire extinguishing agents, and specifically provides a moisture-proof S-type hot aerosol fire extinguishing agent and a preparation method thereof. Background Art

[0002] Nitrates are a class of excellent oxidants. In traditional thermal aerosol fire extinguishing agent formulas, potassium nitrate is usually used as an oxidant to prepare K-type aerosol fire extinguishing agent. However, due to the large amount of corrosive substances produced after potassium nitrate is sprayed, its range of application is greatly limited. In order to solve this problem, strontium nitrate is currently used as the main oxidant, with potassium nitrate, potassium perchlorate, potassium chlorate, etc. as auxiliary oxidants. The thermal aerosol fire extinguishing agent prepared therefrom is classified as S-type, which significantly reduces corrosiveness and improves insulation, and is therefore widely used. However, the hygroscopicity of strontium nitrate is strong, and the S-type thermal aerosol fire extinguishing agent prepared therefrom has the problems of being easily hygroscopic, difficult to preserve, and having a short service life, which not only puts higher requirements on storage, but also limits its range of application.

[0003] To address this issue, coating S-type hot aerosol fire extinguishing agents is currently the primary approach. For example, Chinese patent CN107261379A describes coating the hot aerosol fire extinguishing agent with a stearic acid-acetone solution after mixing the raw materials, in an effort to reduce the hygroscopicity of strontium nitrate. The article "Discussion on the Hygroscopicity of Strontium Nitrate" describes coating strontium nitrate with materials such as nitrocellulose and fluororubber, which, to a certain extent, reduces its hygroscopicity.

[0004] However, when the coating agent is added in the later stage of the preparation of the hot aerosol fire extinguishing agent, the amount of coating agent used is relatively large, and its coating effect still has room for optimization; and when nitrocellulose and fluororubber are used to coat the S-type hot aerosol fire extinguishing agent, there is a certain negative impact on the ignition performance of the fire extinguishing agent, which reduces the fire extinguishing efficiency and has poor applicability.

[0005] Summary of the Invention

[0006] Based on the above technical problems, the present invention provides a method for preparing a moisture-proof S-type hot aerosol fire extinguishing agent, in which the oxidant is coated through a "eutectic-coating" process to reduce hygroscopicity and extend the service life of the hot aerosol fire extinguishing agent.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A moisture-proof S-type hot aerosol fire extinguishing agent is composed of 60-80 parts of an oxidizer, 10-33 parts of a reducing agent, 5-10 parts of an adhesive and 0.5-2 parts of a coating agent.

[0009] Preferably, the oxidant consists of strontium nitrate and eutectic oxide, and the mass ratio of strontium nitrate to eutectic oxide is 2-6:1.

[0010] Further preferably, the eutectic oxide is one or more of potassium perchlorate and potassium nitrate.

[0011] Preferably, the reducing agent is any one of activated carbon, guanidine nitrate, dicyandiamide, melamine or urea.

[0012] Preferably, the adhesive is any one of epoxy resin, phenolic resin, shellac or rubber.

[0013] Preferably, the coating agent is any one of sodium lauryl sulfate, stearic acid or fatty acid diethanolamide.

[0014] A method for preparing a moisture-proof S-type hot aerosol fire extinguishing agent comprises the following steps:

[0015] (1) dissolving the adhesive in anhydrous ethanol and mixing to obtain an adhesive solution;

[0016] (2) mixing the oxidant and the coating agent, dissolving them in water, and mixing them to obtain a mixed solution;

[0017] (3) adding anhydrous ethanol to the mixture and stirring thoroughly to crystallize;

[0018] (4) adding a reducing agent to the crystallized solution and stirring to form a slurry;

[0019] (5) adding the binder solution to the slurry and stirring to obtain a mixture;

[0020] (6) The mixture is sieved through a 20-mesh sieve to form granules, and dried at 40-60° C. to obtain an S-type hot aerosol fire extinguishing agent.

[0021] Preferably, the amount of anhydrous ethanol in step (1) is 2-5% of the weight of the S-type hot aerosol fire extinguishing agent.

[0022] Preferably, the mass ratio of water to oxidant in step (2) is 1:1-1.5.

[0023] Preferably, the mass ratio of the anhydrous ethanol to the oxidant in step (2) is 2:1.

[0024] The beneficial effects of the present invention are as follows: a "eutectic-coating" process is adopted, an oxidant and a coating agent are blended and then dissolved in water, and then an alcohol solution is added; as the alcohol volatilizes, the oxidant and the coating agent co-crystallize and precipitate, so that the coating agent is coated on the outside of the oxidant, so that the coating agent plays a good hydrophobic role, reduces the hygroscopicity of the oxidant, and has a targeted moisture-proof effect on the oxidant; then a reducing agent is added, and the remaining alcohol solution continues to dissolve the reducing agent and the binder, so as to promote dissolution and promote uniform mixing of the oxidant and the reducing agent; at the same time, the addition of the binder forms a secondary coating on the oxidant and the reducing agent in the subsequent granulation process, thereby strengthening the coating effect and further reducing the hygroscopicity of the oxidant such as strontium nitrate.

[0025] Strontium nitrate and other non-hygroscopic oxidants are dissolved in water and then form a eutectic under the action of alcohol. The addition of alcohol is not only a condition for the oxidant co-crystallization, but also helps the rapid evaporation of the solvent water, reducing the drying time and effectively improving production efficiency. DETAILED DESCRIPTION

[0026] The technical solutions of the present invention are further explained below with reference to specific embodiments. It is worth noting that the following embodiments are only preferred embodiments of the present invention and should not be construed as limiting the present invention. The scope of protection of the present invention shall be determined by the claims. Any modifications or substitutions made to the technical solutions of the present invention by those skilled in the art without creative effort shall fall within the scope of protection of the present invention.

[0027] Example 1

[0028] (1) Weigh 8 parts of epoxy resin and dissolve them in 4 parts of anhydrous ethanol, and mix them evenly to obtain an epoxy resin solution;

[0029] (2) Weigh 60 parts of strontium nitrate, 10 parts of potassium nitrate, and 0.5 parts of sodium lauryl sulfate, sieve through a 100-mesh sieve, and preliminarily mix them. Then, add 70 parts of deionized water, stir and dissolve, and obtain a mixed solution;

[0030] (3) adding 35 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0031] (4) adding 21.5 parts of activated carbon to the mixed solution after crystallization, stirring and mixing to obtain a slurry;

[0032] (5) Add the epoxy resin solution obtained in step (1) to the slurry, continue stirring and mixing, and finally granulate through a 20-mesh screen and dry at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0033] Example 2

[0034] (1) Weigh 8 parts of phenolic resin and dissolve them in 4 parts of anhydrous ethanol, and mix them evenly to obtain a phenolic resin solution;

[0035] (2) Weigh 60 parts of strontium nitrate, 15 parts of potassium perchlorate, and 0.5 parts of stearic acid, pass through a 100-mesh sieve, and preliminarily mix them. Then, add 75 parts of deionized water, stir and dissolve them to obtain a mixed solution;

[0036] (3) adding 37.5 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0037] (4) adding 16.5 parts of guanidine nitrate to the mixed solution after crystallization, stirring and mixing to obtain a slurry;

[0038] (5) adding the phenolic resin solution obtained in step (1) to the slurry, continuing to stir and mix, and finally granulating through a 20-mesh screen, and drying at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0039] Example 3

[0040] (1) Weigh 9 parts of shellac and dissolve them in 4 parts of anhydrous ethanol, and mix them evenly to obtain a shellac solution;

[0041] (2) Weigh 60 parts of strontium nitrate, 20 parts of potassium perchlorate, and 1 part of stearic acid, sieve through a 100-mesh sieve, and preliminarily mix them. Then, add 80 parts of deionized water and stir to dissolve them to obtain a mixed solution.

[0042] (3) adding 40 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0043] (4) adding 10 parts of melamine to the mixed solution after crystallization, stirring and mixing to obtain a slurry;

[0044] (5) adding the shellac solution obtained in step (1) to the slurry, continuing to stir and mix, and finally granulating through a 20-mesh screen, and drying at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0045] Example 4

[0046] (1) Weigh 6 parts of phenolic resin and dissolve them in 4 parts of anhydrous ethanol, and mix them evenly to obtain a phenolic resin solution;

[0047] (2) Weigh 60 parts of strontium nitrate, 10 parts of potassium perchlorate, and 1.5 parts of fatty acid glycol amide, sieve through a 100-mesh sieve, and preliminarily mix them. Then, add 70 parts of deionized water, stir and dissolve them to obtain a mixed solution;

[0048] (3) adding 35 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0049] (4) adding 22.5 parts of guanidine nitrate to the mixed solution after crystallization, stirring and mixing to obtain a slurry;

[0050] (5) adding the phenolic resin solution obtained in step (1) to the slurry, continuing to stir and mix, and finally granulating through a 20-mesh screen, and drying at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0051] Example 5

[0052] (1) Weigh 5 parts of rubber and dissolve them in 4 parts of anhydrous ethanol, and mix them evenly to obtain a phenolic resin solution;

[0053] (2) Weigh 50 parts of strontium nitrate, 5 parts of potassium perchlorate, 5 parts of potassium nitrate, and 2 parts of sodium lauryl sulfate, sieve through a 100-mesh sieve, and preliminarily mix them. Then, add 80 parts of deionized water, stir and dissolve, and obtain a mixed solution;

[0054] (3) adding 40 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0055] (4) adding 33 parts of urea to the mixed solution after crystallization, stirring and mixing to obtain a slurry;

[0056] (5) Add the rubber solution obtained in step (1) to the slurry, continue stirring and mixing, and finally granulate through a 20-mesh screen and dry at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0057] Example 6

[0058] (1) Weigh 8 parts of rubber and dissolve them in 4 parts of anhydrous ethanol, and mix them evenly to obtain a phenolic resin solution;

[0059] (2) Weigh 50 parts of strontium nitrate, 15 parts of potassium perchlorate, 5 parts of potassium nitrate, and 2 parts of sodium lauryl sulfate, sieve through a 100-mesh sieve, and preliminarily mix them. Then, add 70 parts of deionized water, stir and dissolve, and obtain a mixed solution;

[0060] (3) adding 35 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0061] (4) adding 20 parts of urea to the mixed solution after crystallization, stirring and mixing to obtain a slurry;

[0062] (5) Add the rubber solution obtained in step (1) to the slurry, continue stirring and mixing, and finally granulate through a 20-mesh screen and dry at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0063] Comparative Example 1

[0064] (1) Weigh 10 parts of shellac and dissolve it in 5 parts of anhydrous ethanol, and mix them evenly to obtain a shellac solution;

[0065] (2) 60 parts of strontium nitrate, 20 parts of potassium perchlorate, and 10 parts of melamine were weighed and preliminarily mixed through a 100-mesh sieve to obtain a mixture;

[0066] (3) pouring the shellac solution obtained in step (1) into the mixture obtained in step (2), and continuing to stir to mix uniformly;

[0067] (4) The mixture was granulated through a 20-mesh screen and dried at 50° C. until the volatile matter was less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0068] Comparative Example 2

[0069] (1) Weigh 10 parts of shellac and dissolve it in 5 parts of anhydrous ethanol, and mix them evenly to obtain a shellac solution;

[0070] (2) Weigh 60 parts of strontium nitrate and 20 parts of potassium perchlorate, sieve through a 100-mesh sieve for preliminary mixing, then add 80 parts of deionized water, stir and dissolve to obtain a mixed solution;

[0071] (3) adding 40 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0072] (4) adding 10 parts of melamine to the mixed solution after crystallization, stirring and mixing to obtain a slurry;

[0073] (5) Add the rubber solution obtained in step (1) to the slurry, continue stirring and mixing, and finally granulate through a 20-mesh screen and dry at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0074] Comparative Example 3

[0075] (1) 40 parts of strontium nitrate, 20 parts of potassium perchlorate, 10 parts of melamine and 10 parts of shellac were weighed and preliminarily mixed through a 100-mesh sieve to obtain a mixture;

[0076] (2) Weigh 20 parts of stearic acid and dissolve it in 70 parts of anhydrous ethanol to obtain a coating agent solution;

[0077] (3) adding the coating agent solution to the mixture obtained in step (1), stirring evenly, granulating through a 20-mesh sieve, and drying at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0078] Comparative Example 4

[0079] (1) Weigh 10 parts of shellac and dissolve it in 5 parts of anhydrous ethanol, and mix them evenly to obtain a shellac solution;

[0080] (2) 60 parts of strontium nitrate, 20 parts of potassium perchlorate, 9 parts of melamine and 1% of stearic acid were weighed and preliminarily mixed through a 100-mesh sieve to obtain a mixture;

[0081] (3) The shellac solution obtained in step (1) is then poured into the mixture obtained in step (2), stirred and mixed, and then granulated through a 20-mesh screen and dried at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0082] Comparative Example 5

[0083] (1) Weigh 5 parts of rubber and dissolve them in 4 parts of anhydrous ethanol, and mix them evenly to obtain a phenolic resin solution;

[0084] (2) Weigh 60 parts of strontium nitrate, 5 parts of potassium perchlorate, 5 parts of potassium nitrate, and 0.1 part of sodium lauryl sulfate, sieve through a 100-mesh sieve, and preliminarily mix them. Then, add 80 parts of deionized water, stir and dissolve to obtain a mixed solution;

[0085] (3) adding 40 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0086] (4) adding 24.9 parts of urea to the mixed solution after crystallization, stirring and mixing to obtain a slurry;

[0087] (5) Add the rubber solution obtained in step (1) to the slurry, continue stirring and mixing, and finally granulate through a 20-mesh screen and dry at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0088] Comparative Example 6

[0089] (1) Weigh 5 parts of rubber and dissolve them in 4 parts of anhydrous ethanol, and mix them evenly to obtain a phenolic resin solution;

[0090] (2) Weigh 60 parts of strontium nitrate, 5 parts of potassium perchlorate, 5 parts of potassium nitrate, and 3 parts of sodium lauryl sulfate, sieve through a 100-mesh sieve, and preliminarily mix them. Then, add 80 parts of deionized water, stir and dissolve to obtain a mixed solution;

[0091] (3) adding 40 parts of anhydrous ethanol to the mixed solution and stirring to crystallize;

[0092] (4) adding 22 parts of urea to the mixture after crystallization, stirring and mixing to obtain a slurry;

[0093] (5) Add the rubber solution obtained in step (1) to the slurry, continue stirring and mixing, and finally granulate through a 20-mesh screen and dry at 50° C. until the volatile matter is less than 1%, thereby obtaining an S-type hot aerosol fire extinguishing agent.

[0094] Result analysis:

[0095] The S-type hot aerosol fire extinguishing agents prepared in Examples 1-6 and Comparative Examples 1-6 were placed in an environment of 21° C. and 78% relative humidity for a hygroscopicity test. After 24 hours, the weight gain of the fire extinguishing agents was measured, and the moisture absorption rate was calculated and statistically analyzed.

[0096] The results show that compared with the S-type hot aerosol fire extinguishing agent prepared by the original process, eutectic process or single coating process used in the comparative example, the fire extinguishing concentration of the S-type hot aerosol fire extinguishing agent prepared by the "eutectic-coating" process of the present invention is basically unchanged, but the 24h moisture absorption rate is greatly reduced, reaching below 0.60%, indicating that the "eutectic-coating" method has a better modification effect than a single method.

Claims

1. A moisture-proof S-type hot aerosol fire extinguishing agent, characterized in that: It consists of 60-80 parts of oxidizing agent, 10-33 parts of reducing agent, 5-10 parts of adhesive and 0.5-2 parts of coating agent.

2. The moisture-proof S-type hot aerosol fire extinguishing agent according to claim 1, characterized in that: The oxidant consists of strontium nitrate and eutectic oxide, and the mass ratio of strontium nitrate to eutectic oxide is 2-6:

1.

3. A moisture-proof S-type hot aerosol fire extinguishing agent according to claim 2, characterized in that: The eutectic oxide is one or more of potassium perchlorate or potassium nitrate.

4. The moisture-proof S-type hot aerosol fire extinguishing agent according to claim 1, characterized in that: The reducing agent is any one of activated carbon, guanidine nitrate, dicyandiamide, melamine or urea.

5. The moisture-proof S-type hot aerosol fire extinguishing agent according to claim 1, characterized in that: The adhesive is any one of epoxy resin, phenolic resin, shellac or rubber.

6. The moisture-proof S-type hot aerosol fire extinguishing agent according to claim 1, characterized in that: The coating agent is any one of sodium dodecyl sulfate, stearic acid or fatty acid diethanolamide.

7. A method for preparing the moisture-proof S-type hot aerosol fire extinguishing agent according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) dissolving the adhesive in anhydrous ethanol and mixing well to obtain an adhesive solution; (2) mixing the oxidant and the coating agent, dissolving them in water, and mixing them evenly to obtain a mixed solution; (3) adding anhydrous ethanol to the mixed solution and stirring thoroughly to crystallize; (4) adding a reducing agent to the solution after crystallization, stirring and mixing to form a slurry; (5) adding the binder solution to the slurry and stirring to obtain a mixture; (6) The mixture is granulated through a 20-mesh sieve and dried at 40-60° C. to obtain an S-type thermal aerosol fire extinguishing agent.

8. The preparation method according to claim 7, characterized in that: The amount of anhydrous ethanol used in step (1) is 2-5% of the total mass of the S-type thermal aerosol fire extinguishing agent.

9. The preparation method according to claim 7, characterized in that: The mass ratio of water to oxidant in step (2) is 1:1-1.

5.

10. The preparation method according to claim 7, characterized in that: The mass ratio of the anhydrous ethanol to the oxidant in step (2) is 2:1.

Citation Information

Patent Citations

  • Compound cocrystallization preparation method for water-soluble condensed fire extinguishing aerosol fire extinguishing agent ingredients

    CN105641848A

  • Low-corrosion hot aerosol fire extinguishing agent

    CN107261379A

  • Fire extinguishing agent capable of extinguishing lithium battery fire and preparation method

    CN109999398A

  • Easily-demoulded high-insulation low-corrosion condensed aerosol fire extinguishing agent and preparation method thereof

    CN116510226A

  • Technology for reducing corrosiveness of aerosol extinguishing agent by in-site embedding aerosol particles