Battery cell, battery, and electric apparatus
By using gel polymer electrolytes in lithium-ion batteries and optimizing the electrode assembly structure, the problem of uneven distribution of electrolytes on the negative electrode sheet is solved, the cycling performance and space utilization of the battery are improved, and the battery life is extended.
Patent Information
- Application Number
- PCT/CN2024/076661
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2024-02-07
- Publication Date
- 2024-11-14
AI Technical Summary
Lithium-ion batteries have poor circulation performance in industrial production and applications, mainly because the electrolyte is easily extruded during the charging and discharging of the negative electrode sheet, resulting in reduced wetting and frequent lithium extraction, which affects battery life and capacity.
Gel polymer electrolyte is used to cure in situ between the positive electrode sheet and the negative electrode sheet, so as to alleviate the expansion pressure through the elasticity of the polymer matrix, maintain the uniform wetting of the electrolyte on the negative electrode sheet, and optimize the electrode assembly structure and electrolyte. Content to improve the circulation performance of the battery cell.
It effectively reduces the problem of uneven distribution of electrolyte on the negative electrode sheet, improves the cycling performance and space utilization of the battery, extends the battery life, and reduces the occurrence of lithium evolution.
Smart Images

Figure CN2024076661_14112024_PF_FP_ABST
Abstract
Description
Battery cells, batteries and electrical devices Technical Field
[0001] The present disclosure relates to the field of batteries, and in particular, to a battery cell, a battery, and an electrical device. Background Art
[0002] In recent years, the application of secondary batteries has become increasingly widespread. They are widely used in energy storage systems such as hydropower, thermal, wind, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. However, this increasing range of applications also poses severe challenges to the cycle performance of secondary batteries. Currently, lithium-ion batteries still face many challenges in industrial production and application.
[0003] Application Contents
[0004] In a first aspect of the present application, the present application proposes a battery cell, comprising: an electrode assembly, the electrode assembly comprising: a positive electrode sheet and a negative electrode sheet, the length of the negative electrode sheet in a first direction being a, the negative electrode sheet having a first end and a second end, the direction from the first end to the second end being the same as the first direction; a gel polymer electrolyte, the gel polymer electrolyte being at least located between the positive electrode sheet and the negative electrode sheet; wherein, when the capacity of the battery cell is less than or equal to 90% of the nominal capacity of the battery cell, there is an area of a on the negative electrode sheet. The first region, the distance between the point farthest from the first end in the first region and the first end is There is a second region on the negative electrode plate, the area of the second region is the same or substantially the same as that of the first region, and the distance between the point farthest from the second end in the second region and the second end is In the temperature range of 25°C-180°C, the heat loss of the negative electrode sheet in the first region is m, and the heat loss of the negative electrode sheet in the second region is n, with m / n being greater than or equal to 50%. Thus, by in-situ solidification between the positive and negative electrode sheets to form a gel polymer electrolyte with high elasticity, the pressure generated by the expansion of the negative electrode sheet can be effectively alleviated, and the electrolyte is not easily squeezed out of one side of the negative electrode sheet. The electrolyte has high wettability on the negative electrode sheet throughout the entire charge and discharge cycle. The electrolyte will vaporize and separate from the negative electrode sheet in the temperature range of 25°C-180°C. Therefore, by testing the heat loss of the negative electrode sheet in a specific region in the temperature range of 25°C-180°C, the electrolyte content in the corresponding region can be directly reflected. When the difference in heat loss between the upper and lower regions of the negative electrode sheet is small, the overall wettability of the negative electrode sheet is better, thereby resulting in better cycle performance of the battery cell.
[0005] According to an embodiment of the present application, the m / n ratio is greater than or equal to 70%. As a result, the difference in electrolyte content between the upper and lower ends of the negative electrode plate is small, the electrolyte has good wettability for the negative electrode plate, and the battery cell has excellent cycle performance.
[0006] According to an embodiment of the present application, a first angle is formed between the first direction and the second direction, and the first angle is 70°-90°. Thus, the battery cells can be placed close to or directly perpendicular to the ground, optimizing the arrangement of the battery cells and improving space utilization.
[0007] According to an embodiment of the present application, the first angle is 85°-90°. Thus, the battery cells can be placed closer to or directly perpendicular to the ground, optimizing the arrangement of the battery cells and improving space utilization.
[0008] According to an embodiment of the present application, the gel polymer electrolyte includes a polymer matrix, which is obtained by polymerizing polymer monomers. The polymer monomers include a first monomer and a second monomer, and the first monomer includes at least two cross-linking sites. Thus, the first monomer can not only trigger the polymerization reaction of the second monomer, but also cross-link multiple polymer chains formed by the polymerization of the second monomer, thereby improving the elasticity of the polymer matrix.
[0009] According to an embodiment of the present application, the cross-linking site includes at least one of a double bond, a triple bond, and a cyclic ether. Thus, the cross-linking effect of the first monomer is better, which can further improve the elasticity of the polymer matrix.
[0010] According to an embodiment of the present application, the first monomer includes at least one of an acrylic acid monomer and an acrylate monomer, thereby improving the cross-linking state of the polymer matrix.
[0011] According to an embodiment of the present application, the first monomer satisfies one or more of the following conditions: the acrylic monomer includes at least one of acrylic acid, methacrylic acid, methyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, isodecyl acrylate, isooctyl acrylate, lauryl acrylate, isobornyl acrylate, isobornyl methacrylate, and ethoxyethoxyethyl acrylate; the acrylic ester monomer includes cyanoacrylate, caprolactone acrylate, propylene glycol ... Acid ester, 2-phenoxyethyl acrylate, tetrahydrofuran acrylate, ethoxylated tetrahydrofuran acrylate, cyclotrimethylolpropane acrylate, 2-carboxyethyl acrylate, cyclohexyl acrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, propylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,4- Butanediol dimethacrylate, 1,3-butanediol diacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate, dipropylene glycol dimethacrylate, tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 2 (propoxy) neopentyl glycol diacrylate, ethylene glycol diacrylate oligomer, ethylene glycol dimethacrylate oligomer, propylene glycol diacrylate, propylene glycol dimethacrylate, propylene glycol diacrylate, propylene glycol dimethacrylate, propylene glycol diacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate, propylene glycol dimethacrylate At least one of glycol dimethacrylate oligomer, cyclohexyl acrylate oligomer, methoxy polyethylene glycol acrylate, ethoxylated trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, methoxyethylene glycol methacrylate oligomer, pentaerythritol triacrylate, propoxylated glycerol triacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, di(trimethylolpropane) tetraacrylate, pentaerythritol tetraacrylate, 4(ethoxy)pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate. This can further improve the crosslinking state of the polymer matrix and enhance the elasticity of the polymer matrix.
[0012] According to an embodiment of the present application, the second monomer includes at least one of a carbonate monomer, a sulfate monomer, a sulfonate monomer, a phosphate monomer, a carboxylate monomer, a sulfone monomer, an amide monomer, a nitrile monomer, and an ether monomer, thereby increasing the strength of the polymer matrix.
[0013] According to an embodiment of the present application, the second monomer meets one or more of the following conditions: the carbonate monomer includes at least one of vinylene carbonate, vinyl ethylene carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, and chloroethylene carbonate; the sulfate monomer includes at least one of vinyl vinyl sulfite, vinyl sulfite, 4-methyl vinyl sulfate, and 4-ethyl vinyl sulfate; the sulfonate monomer includes at least one of 1,3-propylene sultone, 1,3-propane sultone, 1,4-butane sultone, and methanedisulfonic acid methylene cycloester; the phosphate monomer includes dimethyl vinyl phosphate, diethyl vinyl phosphate, diethyl propylene phosphate, diethyl butylene phosphate, diethyl 1-butene-2-yl phosphonate, At least one of diethyl ethynyl phosphate, vinyl trifluoromethyl phosphate, vinyl-1-trifluoroethyl phosphate, diethyl fluorovinyl phosphate, and 1-trifluoropropenylethyl phosphate; the carboxylate monomer includes vinyl acetate; the sulfone monomer includes at least one of methyl vinyl sulfone, ethyl vinyl sulfone, sulfolene, sulfolane, and ethylene sulfoxide; the amide monomer includes acrylamide; the nitrile monomer includes at least one of acrylonitrile, succinonitrile, glutaronitrile, and adiponitrile; and the ether monomer includes at least one of 1,3-dioxolane, ethylene oxide, 1,2-propylene oxide, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, ethylene glycol dimethyl ether, ethylene glycol diglycidyl ether, and triethylene glycol divinyl ether. Thus, the strength of the polymer matrix can be further improved.
[0014] According to an embodiment of the present application, the mass of the electrolyte is c, the mass of the polymer matrix is b, and c / (c+b) is 60%-97%. As a result, the electrolyte content of the battery cell is high, which can further improve the cycle performance of the battery cell.
[0015] According to an embodiment of the present application, the ratio c / (c+b) is 80%-95%, thereby further improving the cycle performance of the battery cell.
[0016] According to an embodiment of the present application, the battery further includes a housing for encapsulating the electrode assembly and the gel polymer electrolyte. When the state of charge of the battery cell is less than 5%, the volume of the electrode assembly is V1, the volume of the battery housing is V2, and V1 / V2 is less than or equal to 92%. This improves the structural stability and operational reliability of the battery cell.
[0017] According to an embodiment of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. This can improve the energy density of the negative electrode plate.
[0018] According to an embodiment of the present application, the negative electrode active material meets one or more of the following conditions: the silicon-based material includes at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy; and the tin-based material includes at least one of elemental tin, tin oxide, and tin alloy. This can improve the energy density of the negative electrode.
[0019] In a second aspect of the present application, a battery is provided, comprising the aforementioned battery cell, which has all the features and advantages of the aforementioned battery cell and will not be further elaborated herein.
[0020] In a third aspect of the present application, an electrical device is provided, comprising the aforementioned battery cell and / or the aforementioned battery. Thus, the electrical device has all the features and advantages of the aforementioned battery cell and battery, which will not be elaborated upon here. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0022] FIG1 shows a schematic structural diagram of a battery cell according to an embodiment of the present application;
[0023] FIG2 shows a schematic structural diagram of a negative electrode sheet according to an embodiment of the present application;
[0024] FIG3 shows a schematic diagram of a battery cell according to an embodiment of the present application;
[0025] FIG4 is an exploded view of the battery cell according to an embodiment of the present application shown in FIG3 ;
[0026] FIG5 shows a schematic diagram of a battery module according to an embodiment of the present application;
[0027] FIG6 shows a schematic diagram of a battery pack according to one embodiment of the present application;
[0028] FIG7 is an exploded view of the battery pack shown in FIG6 according to an embodiment of the present application;
[0029] FIG8 shows a schematic diagram of an electrical device using a battery as a power source according to an embodiment of the present application.
[0030] Explanation of the accompanying drawings: battery pack 1, upper case 2, lower case 3, battery module 4, battery cell 5, positive electrode sheet 10, positive electrode current collector 11, positive electrode active material layer 12, negative electrode sheet 20, negative electrode current collector 21, negative electrode active material layer 22, separator 30, gel polymer electrolyte 40, shell 51, electrode assembly 52, top cover assembly 53, first end 201, second end 202, first region 203, second region 204. DETAILED DESCRIPTION
[0031] The following describes in detail embodiments of the present application. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application and are not to be construed as limiting the present application.
[0032] In the description of this application, it should be understood that the terms "length", "width", "thickness", "up", "down", "front", "back", "left", "right", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on this application.
[0033] In the description of this application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for example, and may be any technical feature connected by "and / or" in this application.
[0034] In the description of this application, “plurality” means two or more.
[0035] Unless otherwise specified, all technical and scientific terms used in this application have the same meanings as commonly understood by those skilled in the art to which this application belongs. All patents and publications referred to in this application are incorporated herein by reference in their entirety. The terms "comprising" or "including" are open-ended expressions, meaning that they include the contents specified in this application but do not exclude contents elsewhere.
[0036] In the description of this application, regardless of whether the word "about" or "approximately" is used, all numbers disclosed herein are approximate values. The value of each number may vary by less than 10% or by a reasonable difference considered by a person skilled in the art, such as 1%, 2%, 3%, 4% or 5%.
[0037] In the description of this application, when A and B are both numerical values, A and B being the same indicates that A and B are exactly the same, and A and B being substantially the same indicates that there is a difference of less than 10% between A and B or a reasonable difference considered by those skilled in the art, such as a difference of 1%, 2%, 3%, 4% or 5%.
[0038] In the present application, taking a metal battery using a liquid electrolyte as an example, when the battery cell 5 is charged, the metal active ions will be released from the positive electrode active material, migrate to the surface of the negative electrode plate 20 after diffusion through the electrolyte, and be embedded in the negative electrode active material; when the battery cell 5 is discharged, the metal active ions will be released from the negative electrode active material, and then migrate to the surface of the positive electrode plate 10 after diffusion through the electrolyte, and be embedded in the positive electrode active material. During the charge and discharge process, the negative electrode active material will expand in volume due to the embedding of the metal active ions, and shrink in volume due to the release of the metal active ions. As a result, the negative electrode active material will continue to change in volume during the charge and discharge cycle of the battery cell 5.
[0039] In some embodiments, taking a negative electrode active material that has a large volume expansion during the charge and discharge cycle, such as a silicon-based negative electrode active material, as an example, the volume of the negative electrode plate 20 containing the silicon-based negative electrode material is a minimum value c1 when the battery cell 5 is in a fully discharged state, and the volume of the negative electrode plate 20 containing the silicon-based negative electrode material reaches a maximum value c2 when the battery cell 5 is in a fully charged state. The volume change rate c2 / c1 of the negative electrode plate 20 containing the silicon-based negative electrode material during the charge and discharge cycle can reach more than 300%. The negative electrode plate 20 has a huge volume effect during the charge and discharge cycle. During the charging process of the battery cell 5, the expansion force inside the battery cell 5 increases as the volume of the negative electrode plate 20 increases, and the electrolyte inside the negative electrode plate 20 will gradually be squeezed out along one side of the negative electrode plate 20. For example, when the battery cell 5 is arranged perpendicular to the ground, during the charging process of the battery cell 5, the electrolyte inside the negative electrode plate 20 will gradually be squeezed out along the upper area of the negative electrode plate 20 and accumulated in the expansion space reserved inside the battery cell 5. During the discharge process of the battery cell 5, the squeezed-out electrolyte cannot flow back to the negative electrode plate 20 in time, resulting in reduced wettability of the electrolyte to the upper area of the negative electrode plate 20, and ultimately leading to lithium deposition. In the early stage of lithium deposition, the lithium crystal nucleus still maintains good contact with the negative electrode plate, and the deposited metallic lithium will further grow into lithium dendrites. In the subsequent cycle process, the top of the lithium dendrite is inactivated and becomes a lithium element that cannot participate in the charge and discharge cycle, thereby significantly affecting the cycle life and capacity of the battery cell.
[0040] Fully charged means the state of charge of the battery cell 5 is 100%. Of course, fully charged can also refer to the state of charge of the battery cell 5 at other values, for example, the state of charge is greater than 90%, and this application does not limit this. Fully discharged means the state of charge of the battery cell 5 is 0%. Of course, fully discharged can also refer to the state of charge of the battery cell 5 at other values, for example, the state of charge is less than 5%, and this application does not limit this.
[0041] The nominal capacity of a battery cell refers to the capacity of a fully charged battery cell at room temperature when discharged at a 1C rate, where the current corresponding to the 1C discharge rate is the current required to completely discharge the battery cell in 1 hour.
[0042] In the present application, by adopting a gel polymer electrolyte instead of a liquid electrolyte and utilizing the space-occupying effect of the polymer matrix in the gel polymer electrolyte, the problem of the electrolyte inside the battery cell being squeezed out when the internal pressure expands is effectively alleviated, thereby resulting in poor wettability of the negative electrode plate, and thus causing a significant decrease in the cycle performance of the battery cell.
[0043] In some embodiments, after the electrode assembly is installed in the battery cell housing, an electrolyte containing polymer monomers is injected into the battery cell, causing the interior of the battery cell 5 to be soaked with the electrolyte containing polymer monomers. External conditions, such as heat treatment, trigger a curing reaction of the polymer monomers to form a polymer matrix, thereby ensuring that the interior of the battery cell 5 is filled with a gel polymer electrolyte 40 composed of the polymer matrix and the electrolyte. Compared to liquid electrolytes, polymer matrices have higher elasticity and pressure-bearing capacity, and can rebound to their original state as much as possible after being subjected to pressure.
[0044] In the present application, a gel polymer electrolyte with high elasticity is formed by in-situ solidification between the positive electrode sheet and the negative electrode sheet, and a polymer matrix is used to partially replace the liquid electrolyte. Then, during the charge and discharge cycle of the battery cell 5, when the negative electrode sheet 20 expands, the polymer matrix can effectively relieve the pressure generated by the expansion of the negative electrode sheet 20, and the electrolyte is not easily squeezed out from the upper area of the negative electrode sheet 20. The electrolyte has a high wettability for the upper area of the negative electrode sheet 20 during the entire charge and discharge cycle, maintaining the ion path in the upper area of the negative electrode sheet 20, effectively inhibiting the growth of lithium dendrites on the surface of the negative electrode sheet 20, and effectively improving the cycle performance of the battery cell 5.
[0045] The battery cells disclosed in the embodiments of the present application can be used, but are not limited to, in electrical devices such as vehicles, ships, or aircraft. A power supply system comprising the battery cells and batteries disclosed in the present application can be used to form the electrical device.
[0046] The embodiments of the present application provide an electrical device that uses a battery cell and / or a battery as a power source. The electrical device may be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery-powered vehicle, an electric car, a ship, a spacecraft, etc. The electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, and the spacecraft may include an airplane, a rocket, a space shuttle, and a spacecraft.
[0047] It should be understood that the technical solutions described in the embodiments of the present application are not limited to the battery cells and electrical devices described above, but can also be applied to all batteries including battery cells and electrical devices using batteries. However, for the sake of simplicity, the following embodiments are explained using electric vehicles as an example.
[0048] In a first aspect of the present application, with reference to FIG1 and FIG2, the present application proposes a battery cell 5, comprising: an electrode assembly, the electrode assembly comprising: a positive electrode sheet 10 and a negative electrode sheet 20, the length of the negative electrode sheet 20 in the first direction being a, the negative electrode sheet 20 having a first end 201 and a second end 202, the direction from the first end 201 to the second end 202 being the same as the first direction; a gel polymer electrolyte 40, the gel polymer electrolyte 40 being located between the positive electrode sheet 10 and the negative electrode sheet 20; wherein, when the capacity of the battery cell 5 is less than or equal to 90% of the nominal capacity of the battery cell 5, there is an area of a on the negative electrode sheet 20 The first region 203, the distance between the point farthest from the first end 201 in the first region 203 and the first end 201 is There is a second region 204 on the negative electrode sheet 20. The area of the second region 204 is the same or substantially the same as the area of the first region 203. The distance between the point farthest from the second end 202 in the second region 204 and the second end 202 is Within the temperature range of 25°C to 180°C, the heat loss of the negative electrode plate 20 in the first region 203 is m, and the heat loss of the negative electrode plate 20 in the second region 204 is n, with m / n being greater than or equal to 50%. The use of the gel polymer electrolyte 40 can leverage the space-occupying effect of the polymer matrix in the gel polymer electrolyte to effectively alleviate the problem of electrolyte being squeezed out of the battery cell during internal pressure expansion, which in turn leads to poor wettability of the negative electrode plate. This effectively reduces lithium deposition on one side of the negative electrode plate 20 caused by poor electrolyte wettability during battery charge and discharge, thereby improving cycle performance.
[0049] In some embodiments, by in-situ curing between the positive and negative electrode sheets to form a highly elastic gel polymer electrolyte, the polymer matrix can effectively alleviate the pressure generated by the expansion of the negative electrode sheet 20, thereby preventing the electrolyte from being squeezed out of one side of the negative electrode sheet 20. The electrolyte maintains high wettability in the negative electrode sheet 20 throughout the entire charge-discharge cycle, as evidenced by high electrolyte content in both the first region 203 and the second region 204 of the negative electrode sheet 20. When the capacity of the battery cell 5 is less than or equal to 90% of the nominal capacity of the battery cell 5, i.e., when the battery cell 5 has undergone several charge-discharge cycles, the electrolyte content in the region of the negative electrode sheet 20 near the first end 201 and near the second end 202 is relatively small. Specifically, the electrolyte vaporizes and separates from the negative electrode sheet 20 within the temperature range of 25°C-180°C. Therefore, measuring the heat loss of a specific region of the negative electrode sheet 20 within the temperature range of 25°C-180°C can directly reflect the electrolyte content in that region.
[0050] As an example, when testing the heat loss of the negative electrode plate 20 in the temperature range of 25° C. to 180° C., the temperature of the negative electrode plate 20 can be gradually increased from 25° C. to 180° C. until the electrolyte is completely volatilized.
[0051] In the embodiment of the present application, the second direction may be parallel to the plane on which the battery cell 5 is placed. For example, the second direction may be parallel to the ground.
[0052] In some embodiments, a first angle exists between the first direction and the second direction. The first angle may be 70°-90°. Optionally, the first angle may be 85°-90°. The battery cells may be arranged close to or directly perpendicular to the ground to optimize the arrangement of the battery cells and improve space utilization. Specifically, when the angle between the first direction and the second direction is 90°, the battery cells are arranged perpendicular to the ground.
[0053] In the embodiment of the present application, the battery cell 5 may be a metal battery. In some embodiments, the battery cell 5 may be a sodium metal battery, a lithium metal battery, or the like.
[0054] In some embodiments, the electrode assembly is a wound structure formed by winding the positive electrode sheet 10 and the negative electrode sheet 20.
[0055] In some embodiments, the electrode assembly is a laminate structure.
[0056] As an example, a plurality of positive electrode sheets 10 and a plurality of negative electrode sheets 20 may be provided, and the plurality of positive electrode sheets 10 and the plurality of negative electrode sheets 20 may be alternately stacked.
[0057] As an example, a plurality of positive electrode sheets 10 may be provided, and the negative electrode sheet 20 may be folded to form a plurality of stacked folded segments, with one positive electrode sheet 10 being sandwiched between adjacent folded segments.
[0058] As an example, the positive electrode sheet 10 and the negative electrode sheet 20 are both folded to form a plurality of stacked folded segments.
[0059] In some embodiments, the separator 30 is disposed between the positive electrode sheet 10 and the negative electrode sheet 20 , mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0060] As an example, a plurality of separators 30 may be provided, each of which is disposed between any adjacent positive electrode sheets 10 or negative electrode sheets 20 .
[0061] As an example, the separator 30 may be provided continuously, and may be provided between any adjacent positive electrode sheets 10 or negative electrode sheets 20 by folding or winding.
[0062] In some embodiments, the shape of the electrode assembly can be cylindrical, flat, or polygonal.
[0063] In some embodiments, the electrode assembly is provided with tabs that can conduct current from the electrode assembly. The tabs include a positive tab and a negative tab.
[0064] In some embodiments, the positive electrode sheet 10 may include a positive electrode current collector 11 and a positive electrode active material layer 12 disposed on at least one side of the positive electrode current collector 11 .
[0065] As an example, the positive electrode current collector 11 has two surfaces facing each other in its thickness direction, and the positive electrode active material layer 12 is provided on either or both of the two facing surfaces of the positive electrode current collector 11 .
[0066] As an example, the positive electrode current collector 11 can be made of metal foil, foam metal or composite current collector. For example, as the metal foil, aluminum or stainless steel with silver surface treatment, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium, etc. can be used. The composite current collector can include a polymer material base and a metal layer. The foam metal can be foam nickel, foam copper, foam aluminum, foam alloy, or foam carbon, etc. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0067] In some embodiments, the negative electrode plate 20 may include a negative electrode current collector 21, and the negative electrode current collector 21 may be a metal foil, a foam metal, or a composite current collector. For example, as the metal foil, aluminum or stainless steel with a silver surface treatment, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel, or titanium, etc. may be used. The foam metal may be foam nickel, foam copper, foam aluminum, foam alloy, or foam carbon, etc. The composite current collector may include a polymer material base layer and a metal layer. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0068] In some embodiments, the negative electrode plate 20 may be a rolled metal foil or a surface coated inert layer of metal powder coated on a current collector.
[0069] In some embodiments, the negative electrode current collector 21 may be a composite current collector. For example, the composite current collector may include at least one of carbon cloth, carbon film, carbonaceous, porous current collector, alloyed modified current collector, lithium-philic modified current collector, and sodium-philic modified current collector.
[0070] In some embodiments, the negative electrode plate 20 may include a negative electrode current collector 21 and a negative electrode active material layer 22 arranged on at least one side surface of the negative electrode current collector 21. The negative electrode active material layer 22 may include a negative electrode active material. The negative electrode active material may be a material with a high gram capacity. For example, the negative electrode active material may include at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based material, tin-based material, and lithium titanate.
[0071] As an example, the silicon-based material may include at least one of elemental silicon, silicon oxide, silicon-carbon compound, silicon-nitrogen compound, and silicon alloy material; the tin-based material may include at least one of elemental tin, tin oxide, and tin alloy material.
[0072] The present application has no particular limitation on the type of the isolation membrane 30 , and any porous isolation membrane with good chemical stability and mechanical stability can be selected.
[0073] As an example, the primary material of the separator 30 may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, ceramic, and polyvinylidene fluoride. The separator 30 may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator 30 is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation. The separator 30 may be a separate component positioned between the positive electrode sheet 10 and the negative electrode sheet 20, or it may be attached to the surfaces of the positive and negative electrodes.
[0074] In some embodiments, when the capacity of the battery cell 5 is less than or equal to 90% of the nominal capacity of the battery cell 5, the battery cell has undergone multiple charge and discharge cycles, and the negative electrode plate 20 has correspondingly undergone multiple reciprocating volume expansion and volume contraction, and the electrolyte inside the battery cell 5 has been pressurized, squeezed out, and refluxed multiple times.
[0075] In some embodiments, the first direction can be parallel to a predetermined surface of the battery cell. For example, the first direction can be parallel to the larger surface of the battery cell. In this case, a first angle of 70°-90° exists between the first direction and the second direction. That is, the larger surface of the battery cell 5 can be at an angle of 70°-90° to the ground. For example, in a wound battery cell, the two surfaces with the larger side areas are referred to as the larger surfaces, and the other two surfaces are referred to as the narrow surfaces.
[0076] In some embodiments, the shape of the first region 203 is not particularly limited, as long as the distance between the farthest point in the first region from the first end 201 and the first end 201 is For example, the first area 203 may be in a circular, rectangular, or triangular shape. When the first area 203 is circular, there is only one point on the boundary of the first area 203 at a distance from the first end 201 of When the first area 203 is a rectangle or a triangle, there may be one or more points on the boundary of the first area 203 that are at a distance of
[0077] In some embodiments, the shape of the second region 204 is not particularly limited, as long as the distance between the point in the second region 204 farthest from the second end 202 and the second segment 202 is That is, for example, the second area 204 can be in a circular, rectangular or triangular shape. When the second area 204 is circular, there is only one point on the boundary of the second area 204 at a distance from the second end 202 of When the second area 204 is a rectangle or a triangle, there may be one or more points on the boundary of the second area 204 that are at a distance of In some embodiments, the first region 203 and the second region 204 have the same shape.
[0078] In some embodiments, the areas of the first region 203 and the second region 204 are the same or substantially the same. For example, when a is greater than 50 mm, the areas of the first region 203 and the second region 204 are Can be 19.625mm 2, so that a disc of predetermined diameter, such as a disc with a diameter of 5 mm, can be obtained at the corresponding position of the negative electrode plate 20 through a relatively simple stamping process, that is, the first area 203 and the second area 204 with a circular shape can be obtained.
[0079] As an example, a differential scanning calorimeter (DSC) sample preparation device can be used. Specifically, a disc with a diameter of 5 mm is obtained by a mechanical die punching method.
[0080] As an example, a thermogravimetric analyzer may be used. Specifically, a differential thermal-thermogravimetric analyzer may be used to measure the heat loss of the negative electrode sheet 20 in the first region 203 and the negative electrode sheet 20 in the second region 204 within a range of 25° C. to 180° C.
[0081] In some embodiments, m / n may be greater than or equal to 70%. A larger m / n value indicates a smaller difference in electrolyte content between the area of the negative electrode plate 20 near the first end 201 and the area near the second end 202. When the battery cell is placed perpendicular to the ground, the wettability of the upper and lower areas of the negative electrode plate 20 approaches uniformity.
[0082] As an example, m / n can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 96%, or 97%. It is understood that, due to the limitations of the battery cell's electrolyte filling coefficient, the electrolyte content of the negative electrode plate 20 in the first region 203 will be less than the electrolyte content of the negative electrode plate 20 in the second region 204, that is, m / n can be a value greater than or equal to 50% and less than 100%.
[0083] In some embodiments, the gel polymer electrolyte includes a polymer matrix obtained by polymerizing polymer monomers. The polymer monomers include a first monomer and a second monomer. The first monomer includes at least two cross-linking sites.
[0084] For example, a first monomer can act as a crosslinker, and a second monomer can polymerize to form a polymer chain. Because the first monomer contains at least two crosslinking sites, it can both initiate polymerization of the second monomer and crosslink multiple polymer chains formed by polymerization of the second monomer. In other words, the first monomer can be both a component of a polymer chain and a connecting structure connecting multiple polymer chains.
[0085] As an example, the first monomer may include two cross-linking sites. The first monomer with double cross-linking sites can effectively improve the cross-linking state of the polymer matrix, effectively improve the elasticity of the polymer matrix, and thereby make the gel polymer electrolyte more elastic when under pressure, further reducing the electrolyte in the negative electrode plate 20 from being squeezed out due to pressure.
[0086] In some embodiments, the cross-linking site may include at least one of a double bond, a triple bond, and a cyclic ether.
[0087] In some embodiments, the first monomer may include at least one of an acrylic monomer and an acrylate monomer.
[0088] As an example, the acrylic monomer may include at least one of acrylic acid, methacrylic acid, methyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, isodecyl acrylate, isooctyl acrylate, lauryl acrylate, isobornyl acrylate, isobornyl methacrylate, and ethoxyethoxyethyl acrylate.
[0089] As an example, the acrylate monomer may include cyanoacrylate, caprolactone acrylate, 2-phenoxyethyl acrylate, tetrahydrofuran acrylate, ethoxylated tetrahydrofuran acrylate, cyclotrimethylolpropane acrylate, 2-carboxyethyl acrylate, cyclohexyl acrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, propylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,3-butanediol diacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate. , dipropylene glycol dimethacrylate, tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 2 (propoxy) neopentyl glycol diacrylate, ethylene glycol diacrylate oligomer, ethylene glycol dimethacrylate oligomer, propylene glycol dimethacrylate oligomer, cyclohexyl acrylate oligomer, methoxy polyethylene glycol acrylate, ethoxylated trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, methoxyethylene glycol methacrylate oligomer, pentaerythritol triacrylate, propoxylated glycerol triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, di(trimethylolpropane) tetraacrylate, pentaerythritol tetraacrylate, 4(ethoxy)pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate.
[0090] As an example, an oligomer refers to a polymer having a number average molecular weight of less than 10,000, and the oligomer can be obtained by oligomerization.
[0091] In some embodiments, the second monomer may include at least one of carbonate monomers, sulfate monomers, sulfonate monomers, phosphate monomers, carboxylate monomers, sulfone monomers, amide monomers, nitrile monomers, and ether monomers.
[0092] In some embodiments, the carbonate monomers may include at least one of vinyl carbonate, vinyl ethylene carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, and chloroethylene carbonate; the sulfate monomers may include at least one of vinyl sulfite, vinyl sulfite, 4-methyl vinyl sulfate, and 4-ethyl vinyl sulfate; the sulfonate monomers may include at least one of 1,3-propylene sultone, 1,3-propane sultone, 1,4-butane sultone, and methanedisulfonic acid methylene cycloester; the phosphate monomers may include dimethyl vinyl phosphate, diethyl vinyl phosphate, diethyl propenyl phosphate, diethyl butenyl phosphate, diethyl 1-butene-2-yl phosphonate, diethyl ethynyl phosphate, and ethyl 1-butene-2-yl phosphonate. At least one of alkenyl trifluoromethyl phosphate, vinyl-1-trifluoroethyl phosphate, diethyl fluorovinyl phosphate, and 1-trifluoropropenyl ethyl phosphate; the carboxylate monomer may include vinyl acetate; the sulfone monomer may include at least one of methyl vinyl sulfone, ethyl vinyl sulfone, cyclobutane sulfone, cyclobutane sulfoxide; the amide monomer may include acrylamide; the nitrile monomer may include at least one of acrylonitrile, succinonitrile, glutaronitrile, and adiponitrile; the ether monomer may include at least one of 1,3-dioxolane, ethylene oxide, 1,2-propylene oxide, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, ethylene glycol dimethyl ether, ethylene glycol diglycidyl ether, and triethylene glycol divinyl ether.
[0093] In some embodiments, the mass of the electrolyte is c, the mass of the polymer matrix is b, and c / (c+b) may be 60%-97%. Alternatively, c / (c+b) may be 80%-95%.
[0094] The use of gel polymer electrolytes can effectively reduce the problem of uneven distribution of electrolyte on the negative electrode during the later use of battery cells. Using less electrolyte can achieve better cycle performance, increase the volume energy density of battery cells, and reduce the occurrence of lithium plating. Using more electrolyte can achieve better cycle performance and reduce the occurrence of lithium plating.
[0095] As an example, c / (c+b) can be 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96% or 97%.
[0096] In some embodiments, the electrolyte in the gel polymer electrolyte may include a solvent and an inorganic salt.
[0097] As an example, the solvent in the electrolyte may include at least one of ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone;
[0098] As an example, the inorganic salt in the electrolyte may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorophosphate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0099] In some embodiments, the battery further includes a shell, which is used to encapsulate the electrode assembly and the gel polymer electrolyte. When the state of charge of the battery cell is less than 5%, the volume of the electrode assembly is V1, the volume of the battery shell is V2, and V1 / V2 is less than or equal to 92%.
[0100] By making the volume of the housing larger than that of the electrode assembly, expansion space for the negative electrode sheet 20 can be reserved within the battery cell housing, reducing the risk of housing deformation and structural failure caused by negative electrode sheet expansion. By partially replacing the liquid electrolyte with a gel polymer electrolyte, the phenomenon of negative electrode sheet electrolyte being squeezed out under pressure and then accumulating in the reserved expansion space within the battery cell 5 can be effectively reduced.
[0101] As an example, when V1 / V2 is greater than 92%, the reserved expansion space in the battery cell shell is too small. During the charge and discharge process, the volume change of the negative electrode plate will be directly reflected at the battery cell level, and defects such as battery cell bulging are very likely to occur.
[0102] As an example, the housing of the battery cell 5 is used to encapsulate the electrode assembly and electrolyte components. The housing can be a steel housing, an aluminum housing, a plastic housing (such as polypropylene), a composite metal housing (such as a copper-aluminum composite housing), or an aluminum-plastic film.
[0103] As an example, gel polymer electrolytes have strong structural plasticity and are extremely unlikely to explode when encountering abnormal usage conditions such as overcharging, over-discharging, impact, crushing, and puncture. They can be used to manufacture batteries of various shapes.
[0104] As an example, the battery cells may be cylindrical, prismatic, soft-pack, or other shaped battery cells. Prismatic battery cells include square-shell, blade-shaped, and polygonal prismatic cells. Polygonal prismatic cells may be hexagonal, etc., and this application does not have any particular limitations.
[0105] In the second aspect of the present application, the present application proposes a battery comprising the aforementioned battery cell 5. Therefore, the battery has all the features and advantages of the aforementioned battery cell 5, which will not be described in detail here.
[0106] Typically, a battery includes a positive electrode sheet 10, a negative electrode sheet 20, an electrolyte, and a separator 30. The electrolyte may include the aforementioned gel polymer electrolyte 40. During the battery's charge and discharge process, active ions are intercalated and released back and forth between the positive electrode sheet 10 and the negative electrode sheet 20. The electrolyte acts as an ion conductor between the positive electrode sheet 10 and the negative electrode sheet 20. The separator 30 is disposed between the positive electrode sheet 10 and the negative electrode sheet 20, primarily to prevent a short circuit between the positive and negative electrodes while allowing ions to pass through.
[0107] As an example, the present application has no particular restrictions on the shape of the battery, which can be cylindrical, square or any other shape. For example, Figure 3 is a battery cell 5 of a square structure as an example. Specifically, with reference to Figure 4, the outer packaging of the battery cell 5 may include a shell 51 and a top cover assembly 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the top cover assembly 53 can be covered on the opening to close the receiving cavity.
[0108] As an example, the positive electrode sheet 10, the negative electrode sheet 20, and the separator 30 can be wound or laminated to form an electrode assembly 52. The electrode assembly 52 is encapsulated within a housing cavity, and the gel polymer electrolyte fills the interior space of the electrode assembly 52. The battery cell 5 can contain one or more electrode assemblies 52, and those skilled in the art can select the number based on specific practical needs.
[0109] As an example, batteries can be assembled into battery modules, and the number of batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module. Figure 5 is a battery module 4 as an example. Referring to Figure 5, in the battery module 4, a plurality of battery cells 5 can be arranged in sequence along the length direction of the battery module 4. Of course, they can also be arranged in any other manner. The plurality of battery cells 5 can further be fixed by fasteners. The battery module 4 can also include a shell having a accommodating space, and the plurality of battery cells 5 are accommodated in the accommodating space.
[0110] As an example, the above-mentioned battery modules can also be assembled into a battery pack. The number of battery modules contained in the battery pack can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery pack. Figures 6 and 7 are battery packs 1 as an example. Referring to Figures 6 and 7, the battery pack 1 may include a battery box and a plurality of battery modules 4 arranged in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can be covered on the lower box body 3 to form a closed space for accommodating the battery module 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0111] In a third aspect of the present application, an electrical device is provided, comprising the aforementioned battery cell 5 and / or the aforementioned battery. Thus, the electrical device has all the features and advantages of the aforementioned battery cell and battery, which will not be elaborated upon here.
[0112] Batteries, battery modules, or battery packs can be used as power sources for electrical devices or as energy storage units for electrical devices. Electrical devices may include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc. Electrical devices can select batteries, battery modules, or battery packs based on their usage requirements.
[0113] As an example, Figure 8 shows an example electrical device. This device is a pure electric vehicle, hybrid electric vehicle, or plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module can be used.
[0114] As an example, the power-consuming device may also be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and may use a battery as a power source.
[0115] The present invention will be described below by way of specific examples. It should be noted that the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. Where specific techniques or conditions are not specified in the examples, they are determined according to the techniques or conditions described in the literature in this area or according to the product specifications. Reagents or instruments not specified by manufacturer are all commercially available conventional products.
[0116] Example 1
[0117] Preparation of positive electrode:
[0118] The positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O2, conductive agent carbon black (SuperP), and binder polyvinylidene fluoride (PVDF) were mixed uniformly in a solvent N-methylpyrrolidone (NMP) at a mass ratio of 91.6:1.8:6.6 to prepare a positive electrode slurry. The prepared positive electrode slurry was coated on one surface of the aluminum foil current collector with a coating surface density of 17.66 mg / cm 2 After drying in an oven, the same weight of positive electrode slurry is coated on the other side of the current collector, and then dried and cold pressed to obtain the positive electrode sheet.
[0119] Preparation of negative electrode sheet:
[0120] The negative electrode active material graphite, conductive agent carbon black (SuperP), binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) were mixed in an appropriate amount of solvent deionized water at a mass ratio of 95.4:1.5:2.5:0.6 to form a uniform negative electrode slurry. The negative electrode slurry was evenly coated on one surface of the copper foil current collector with a coating surface density of 11.3 mg / cm 2 After drying in an oven, the same weight of positive electrode slurry is coated on the other side of the current collector, and then dried and cold pressed to obtain the negative electrode sheet.
[0121] Battery Assembly:
[0122] The separator, positive electrode sheet, and negative electrode sheet are placed in the order of positive electrode sheet, separator, negative electrode sheet, and separator. After the winding process, they are hot pressed at 80°C and 1MPa pressure. The size of the electrode assembly is 143*84*25mm (i.e. V1=300.3cm 3 ), and then assembled into a non-liquid-injected hard-shell dry cell through the ear welding, shell insertion, and top cover welding process, where the internal size of the hard shell is 145*88*26mm (i.e. V2=331.76cm 3 ), V1 / V2 is 90.51%;
[0123] Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 3:7 to obtain an organic solvent, and then lithium hexafluorophosphate (LiPF6) is dissolved in the above organic solvent to obtain electrolyte A, wherein the concentration of LiPF6 is 1 mol / L. Subsequently, electrolyte A: first monomer (ethylene glycol diacrylate oligomer, molecular weight 400): second monomer (ethylene ethylene carbonate): initiator (azobisisobutyronitrile) are configured into a gel electrolyte in a weight ratio of 10:10:79.8:0.2. 110g of the gel electrolyte is injected into the battery cell, and then the battery cell is evacuated to -20kPa and maintained for 10 minutes. After standing at room temperature for 24 hours, the battery cell is charged to 4.0V at a current of 3A at 45°C, and the battery cell is formed. Then, the battery cell is discharged to 2.8V at a current of 3A at room temperature to form a gel polymer electrolyte to obtain a battery.
[0124] Example 2
[0125] Example 2 is consistent with Example 1, except that the first monomer in Example 2 is triethylene glycol diacrylate.
[0126] Example 3
[0127] Example 3 is consistent with Example 1, except that the first monomer in Example 3 is ethoxylated trimethylolpropane triacrylate.
[0128] Example 4
[0129] Example 4 is consistent with Example 1, except that the first monomer in Example 4 is pentaerythritol tetraacrylate.
[0130] Example 5
[0131] Example 5 is consistent with Example 1, except that the second monomer in Example 5 is diethyl propylene phosphate.
[0132] Example 6
[0133] Example 6 is consistent with Example 1, except that the second monomer in Example 6 is triethylene glycol divinyl ether.
[0134] Example 7
[0135] Example 7 is consistent with Example 1, except that the second monomer in Example 7 is ethyl vinyl sulfone.
[0136] Comparative Example 1
[0137] Comparative Example 1 is consistent with Example 1, except that a liquid electrolyte is used in Comparative Example 1. Specifically, ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 3:7 to obtain an organic solvent, and lithium hexafluorophosphate (LIPF6) is dissolved in the organic solvent to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L. The electrolyte injection volume is 110 g.
[0138] Comparative Example 2
[0139] Comparative Example 2 is consistent with Comparative Example 1, except that the injection amount in Comparative Example 2 is 120 g.
[0140] The following tests were performed on the batteries in Examples 1-7 and Comparative Examples 1 and 2. The test results are shown in Table 1.
[0141] Cycle number at 90% capacity retention: Cycle the battery for one cycle at a rate of 0.33C of the designed capacity, measure the actual capacity C0, and calibrate it as the nominal capacity of the battery. Then, charge and discharge the battery at a rate of 1C, and record the capacity retention C0 of each cycle. n , when C n When / C0=90%, record the cycle number p, which is the cycle number corresponding to 90% capacity retention.
[0142] Cycle life test: The battery is cycled for one cycle at a rate of 0.33C of the designed capacity, and the actual capacity C0 is measured, which is calibrated as the nominal capacity of the battery. Then the charge and discharge cycle is performed at a rate of 1C, and the capacity of each cycle C0 is recorded. n , when C n When / C0=80%, record the number of cycles q, which is the cycle life of the battery.
[0143] Negative electrode heat loss test: When the battery is cycled to 90% capacity retention, the battery is in 0% SOC state, the battery is disassembled, the outermost negative electrode sheet of the electrode assembly is taken out, and small discs with a diameter of 5 mm are punched out in the first and second areas of the same sheet. The samples are loaded into the test sample table, and two identical devices (Netzsch synchronous thermal analyzer STA-STA449F3) are used to test the first and second areas respectively. The test process is: heating to 70°C at 5°C / min, keeping warm at 70°C for 30 minutes, and recording the mass loss m in the first area and the mass loss n in the second area during the whole process.
[0144] Table 1
[0145] In the description of this specification, reference to the terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.
[0146] In the description of this specification, the terms "first" and "second" are used for descriptive purposes only and are not to be construed as indicating or implying relative importance or implicitly indicating the number of the technical features indicated. Although the embodiments of the present application have been shown and described above, it is understood that the above embodiments are exemplary and are not to be construed as limiting the present application. Persons of ordinary skill in the art may make changes, modifications, substitutions, and variations to the above embodiments within the scope of the present application.
Claims
1. A battery cell, wherein: include: An electrode assembly, the electrode assembly comprising: a positive electrode sheet and a negative electrode sheet, the negative electrode sheet has a length a in a first direction, the negative electrode sheet has a first end and a second end, and a direction from the first end to the second end is the same as the first direction; A gel polymer electrolyte, wherein the gel polymer electrolyte is at least located between the positive electrode plate and the negative electrode plate; Wherein, when the capacity of the battery cell is less than or equal to 90% of the nominal capacity of the battery cell, there is an area less than or equal to A first region, wherein the distance between the point in the first region farthest from the first end and the first end is There is a second region on the negative electrode plate, the area of the second region is the same or substantially the same as the area of the first region, and the distance between the point in the second region farthest from the second end and the second end is In the temperature range of 25° C.-180° C., the heat loss of the negative electrode plate in the first region is m, the heat loss of the negative electrode plate in the second region is n, and m / n is greater than or equal to 50%.
2. The battery cell according to claim 1, wherein: The m / n is 70%-100%.
3. The battery cell according to claim 1 or 2, wherein: There is a first angle between the first direction and the second direction, and the first angle is 70°-90°.
4. The battery cell according to any one of claims 1 to 3, wherein: The gel polymer electrolyte comprises a polymer matrix and an electrolyte. The polymer matrix is obtained by polymerizing polymer monomers. The polymer monomers comprise a first monomer and a second monomer. The first monomer comprises at least two cross-linking sites.
5. The battery cell according to claim 4, wherein: The cross-linking site includes at least one of a double bond, a triple bond, and a cyclic ether.
6. The battery cell according to claim 4 or 5, wherein: The first monomer includes at least one of an acrylic monomer and an acrylate monomer.
7. The battery cell according to claim 6, wherein: The first monomer satisfies one or more of the following conditions: The acrylic monomers include acrylic acid, methacrylic acid, methyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, isodecyl acrylate, At least one of isooctyl acrylate, lauryl acrylate, isobornyl acrylate, isobornyl methacrylate, and ethoxyethoxyethyl acrylate; The acrylic ester monomers include cyanoacrylate, caprolactone acrylate, 2-phenoxyethyl acrylate, tetrahydrofuran acrylate, ethoxylated tetrahydrofuran acrylate, cyclotrimethylolpropane acrylate, 2-carboxyethyl acrylate, cyclohexyl acrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, propylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,3-butanediol diacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate, dimethacrylate, At least one of propylene glycol dimethacrylate, tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 2 (propoxylated) neopentyl glycol diacrylate, ethylene glycol diacrylate oligomer, ethylene glycol dimethacrylate oligomer, propylene glycol dimethacrylate oligomer, cyclohexyl acrylate oligomer, methoxy polyethylene glycol acrylate, ethoxylated trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, methoxyethylene glycol methacrylate oligomer, pentaerythritol triacrylate, propoxylated glycerol triacrylate, tri(2-hydroxyethyl)isocyanuric acid triacrylate, di(trimethylolpropane) tetraacrylate, pentaerythritol tetraacrylate, 4(ethoxy)pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.
8. The battery cell according to any one of claims 4 to 7, wherein: The second monomer includes at least one of carbonate monomers, sulfate monomers, sulfonate monomers, phosphate monomers, carboxylate monomers, sulfone monomers, amide monomers, nitrile monomers, and ether monomers.
9. The battery cell according to claim 8, wherein: The second monomer satisfies one or more of the following conditions: The carbonate monomer includes at least one of vinylene carbonate, vinyl ethylene carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, and chloroethylene carbonate; The sulfate monomer includes at least one of vinyl sulfite, vinyl sulfite, 4-methyl vinyl sulfate, and 4-ethyl vinyl sulfate; The sulfonate monomer includes at least one of 1,3-propylene sultone, 1,3-propane sultone, 1,4-butane sultone, and methanedisulfonic acid methylene cyclopentane; The phosphate monomer includes at least one of dimethyl vinyl phosphate, diethyl vinyl phosphate, diethyl propenyl phosphate, diethyl butenyl phosphate, diethyl 1-buten-2-yl phosphonate, diethyl ethynyl phosphate, vinyl trifluoromethyl phosphate, vinyl-1-trifluoroethyl phosphate, diethyl fluorovinyl phosphate, and 1-trifluoropropenylethyl phosphate; The carboxylate monomer includes vinyl acetate; The sulfone monomer includes at least one of methyl vinyl sulfone, ethyl vinyl sulfone, cyclobutene sulfone, cyclopentane sulfone, and ethylene sulfoxide; The amide monomer includes acrylamide; The nitrile monomer includes at least one of acrylonitrile, succinonitrile, glutaronitrile and adiponitrile; The ether monomer includes at least one of 1,3-dioxolane, ethylene oxide, 1,2-propylene oxide, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, ethylene glycol dimethyl ether, ethylene glycol diglycidyl ether, and triethylene glycol divinyl ether.
10. The battery cell according to any one of claims 4 to 9, wherein: The mass of the electrolyte is c, the mass of the polymer matrix is b, and c / (c+b) is 60%-97%.
11. The battery cell according to claim 10, wherein: The c / (c+b) is 80%-95%.
12. The battery cell according to any one of claims 1 to 11, wherein: It further includes a shell, which is used to encapsulate the electrode assembly and the gel polymer electrolyte. When the state of charge of the battery cell is less than 5%, the volume of the electrode assembly is V1, the volume of the battery shell is V2, and V1 / V2 is less than or equal to 92%.
13. The battery cell according to any one of claims 1 to 12, wherein: The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer located at least on one side of the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based material, tin-based material, and lithium titanate.
14. The battery cell according to claim 13, wherein: The negative electrode active material satisfies one or more of the following conditions: The silicon-based material includes at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy material; The tin-based material includes at least one of elemental tin, tin oxide, and tin alloy material.
15. A battery, wherein: A battery cell comprising the battery cell according to any one of claims 1 to 14.
16. An electrical device, wherein: Comprising the battery monomer according to any one of claims 1 to 14; and / or the battery according to claim 15.
Citation Information
Patent Citations
Composition for gel polymer electrolyte and lithium secondary battery comprising the same
CN104380516A
In-situ polymerization solid-state battery with multi-layer structure electrolyte and preparation method of in-situ polymerization solid-state battery
CN114335716A
Secondary battery and method for manufacturing the same
CN116014224A
Composition for gel polymer electrolyte, gel polymer electrolyte and electrochemical device
WO2015058480A1
Electrochemical device and manufacturing method thereof
WO2020171483A1