Negative electrode for lithium-free secondary battery, and lithium-free secondary battery comprising same

The introduction of a second metal oxide layer with a higher work function on the negative electrode of lithium-free secondary batteries addresses the issues of lithium dendrite growth and side reactions, improving stability and efficiency by reducing short circuits and capacity loss, resulting in improved battery performance.

WO2024232556A1PCT designated stage expired Publication Date: 2024-11-14LG ENERGY SOLUTION LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005055
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-04-16
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Lithium-free secondary batteries face issues with lithium dendrite growth and side reactions between the lithium metal layer and electrolyte, leading to reduced stability, efficiency, and lifespan due to the highly reactive nature of lithium metal, which results in potential short circuits and capacity loss.

Method used

A negative electrode with a conductive metal layer and a second metal oxide layer having a higher work function than the first metal, which suppresses side reactions between the lithium metal layer and the electrolyte during charging and discharging, thereby reducing the likelihood of short circuits and enhancing coulombic efficiency and lifespan.

Benefits of technology

The use of a negative electrode with a second metal oxide layer significantly reduces side reactions and improves the stability and lifespan of lithium-free secondary batteries by increasing the work function of the lithium metal layer, leading to enhanced capacity characteristics and reduced irreversible capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005055_14112024_PF_FP_ABST
    Figure KR2024005055_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to: a negative electrode for a lithium-free secondary battery, the negative electrode being capable of enhancing the efficiency and lifespan characteristics of the lithium-free secondary battery by suppressing side reactions between a lithium metal layer, deposited on the negative electrode, and an electrolyte during charging and discharging; and a lithium-free secondary battery comprising same.
Need to check novelty before this filing date? Find Prior Art

Description

Anode for lithium-free secondary battery and lithium-free secondary battery containing the same

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0059726, filed May 9, 2023, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to a negative electrode for a lithium-free secondary battery capable of improving the efficiency and lifespan characteristics of a lithium-free secondary battery, and a lithium-free secondary battery including the same.

[0004] Lithium metal batteries utilize lithium metal (Li-metal) as the anode active material. Compared to conventional graphite or lithium alloy anodes, lithium metal batteries theoretically offer significantly higher energy density and capacity. Therefore, research and development are ongoing to apply these lithium metal batteries to batteries requiring high energy densities.

[0005] However, lithium metal batteries have disadvantages such as large volume changes in the negative electrode during the charge and discharge process, the growth of needle-like lithium metal layers (such as lithium dendrites), and the occurrence of side reactions between the lithium metal layers and the electrolyte due to the highly reactive nature of lithium metal, resulting in large irreversible capacity. As a result, lithium metal batteries have a high possibility of electrode short-circuiting and insufficient stability and lifespan characteristics, which have prevented their commercialization.

[0006] Recently, as an alternative to the above lithium metal battery, research and interest in lithium-free secondary batteries (or non-anode secondary batteries) that form the anode with the anode collector itself without forming a separate lithium metal layer or other anode active material layer on the anode collector are growing.

[0007] These lithium-free secondary batteries can achieve higher energy density than lithium metal batteries, and the overall manufacturing process can be simplified as the formation of the lithium metal layer is omitted.

[0008] However, the lithium-free secondary battery also has problems due to the growth of lithium dendrites and side reactions between the lithium metal layer and the electrolyte, as a lithium metal layer is deposited on the negative electrode current collector during the charge and discharge process and acts as a type of negative electrode active material. In particular, due to the growth of the lithium dendrites, etc., the surface area in contact with the electrolyte further increases, so the side reactions between the lithium metal layer and the electrolyte may further increase.

[0009] Because of this, lithium-free secondary batteries still have the disadvantages of having electrical short-circuits, the loss of the lithium metal layer, and a large capacity loss, and significantly deteriorating the stability and lifespan characteristics of lithium-free secondary batteries.

[0010] To address these issues, methods have been proposed to suppress the growth of lithium dendrites, primarily through surface modification of the negative electrode current collector. However, even with these methods, it is difficult to fundamentally suppress side reactions between the lithium metal layer and the electrolyte, and there are limitations in improving the stability, efficiency, and lifespan of lithium-free secondary batteries.

[0011] Accordingly, the present invention provides a negative electrode for a lithium-free secondary battery that can improve the stability, efficiency, and lifespan characteristics of a lithium-free secondary battery by suppressing side reactions between a lithium metal layer deposited on the negative electrode during charging and discharging and an electrolyte.

[0012] The present invention also provides a lithium-free secondary battery including the negative electrode, which exhibits improved stability and lifespan characteristics.

[0013] Accordingly, the present invention comprises a conductive metal layer including a first metal; and

[0014] A negative electrode current collector including a second metal oxide layer formed on a conductive metal layer,

[0015] The second metal oxide provides a negative electrode for a lithium-free secondary battery having a work function greater than that of the first metal.

[0016] The present invention also comprises the cathode;

[0017] An anode facing the cathode;

[0018] An electrolyte comprising a lithium salt and a non-aqueous organic solvent; and

[0019] A lithium-free secondary battery including a separator between the positive and negative electrodes is provided.

[0020] Since the negative electrode for a lithium-free secondary battery of the present invention includes a metal oxide layer having a large work function, even if a lithium metal layer is deposited on the metal oxide layer and the lithium metal layer comes into contact with an electrolyte, side reactions between the lithium metal layer and the electrolyte can be greatly suppressed.

[0021] Accordingly, not only is the possibility of a short circuit due to a side reaction of the lithium metal layer and the electrolyte reduced, but the coulombic efficiency of the lithium-free secondary battery is increased and the irreversible capacity is reduced, thereby improving its life characteristics.

[0022] Therefore, the present invention can greatly contribute to the development of lithium-free secondary batteries as a next-generation secondary battery that exhibits improved stability and lifespan characteristics along with excellent capacity characteristics.

[0023] Figures 1a and 1b show images of the cathode cross-sections of Examples 1 and 2, respectively, analyzed using FIB-TEM (Focused Ion Beam Transmission Electron Microscopy).

[0024] Figure 2 shows the results of measuring the work function (eV) of the cathodes of Comparative Example 1 and Examples 1 and 2 by analyzing them using UPS (Ultraviolet Photoelectron Spectroscopy).

[0025] Figures 3a and 3b show the results of CV (Cyclic Voltammetry) tests performed on the cathodes of Examples 1 and 2, respectively.

[0026] Figures 4a and 4b show depth-dependent element profiles of the cathodes of Examples 1 and 2, which performed the above CV (Cyclic Voltammetry) test, respectively, analyzed by X-ray photoelectron spectroscopy (XPS).

[0027] Figure 5 shows the 1 mAh / cm on the cathode of Comparative Example 1, Examples 1 and 2. 2 After depositing lithium metal layers with a capacity of , the work function (eV) of each lithium metal layer was measured by analyzing it with UPS (Ultraviolet Photoelectron Spectroscopy). The results are shown.

[0028] Figure 6 shows the results of measuring the interface resistance through impedance analysis while electrodeposition of a lithium metal layer was performed under the application of current for half-cells including the negative electrodes of Comparative Example 1 and Examples 1 and 2.

[0029] Figure 7 shows the results of evaluating the initial coulombic efficiency at the first cycle charge and discharge for half-cells including the cathodes of Comparative Example 1 and Examples 1 and 2.

[0030] Figure 8 shows the results of evaluating the change in capacity per cycle while conducting a charge / discharge test on a full cell including the negative electrodes of Comparative Example 1 and Examples 1 and 2.

[0031] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless specifically stated otherwise.

[0032] The terms "about," "substantially," and the like used throughout this specification are used to mean at or near the numerical value when manufacturing and material tolerances inherent to the meanings stated are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that state precise or absolute values ​​to aid understanding of this specification. The terms "step of doing" or "step of" used throughout this specification do not mean "step for doing."

[0033] In this specification, the term "combination of these" included in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including one or more selected from the group consisting of the components.

[0034] In addition, in the present specification, the term “lithium-free secondary battery” may refer to a secondary battery in which, in a state before charging or discharging, for example, in a state immediately after manufacturing, there is no separate negative electrode active material layer, such as a lithium metal layer, a lithium alloy layer, or other carbon-containing layer, on the negative electrode collector, which includes a conductive metal layer including a first metal such as copper, and a second metal oxide layer having a higher work function. Accordingly, the “lithium-free secondary battery” may be defined as a battery in which the negative electrode is formed of the negative electrode collector in a state before charging or discharging, and does not include a separate negative electrode active material layer (e.g., a lithium metal layer, etc.) on the negative electrode collector. However, it should be understood that addition of a separate insulating layer or other functional thin film in addition to the negative electrode active material layer is not limited.

[0035] In addition, the term “lithium-free secondary battery” above cannot be interpreted as limiting the presence of a lithium-containing positive electrode active material or limiting the presence of a lithium metal layer or lithium-containing compound grown on a negative electrode current collector as a result of charge and discharge.

[0036]

[0037] Hereinafter, based on the above definitions, implementation examples of the invention will be described in detail. However, these are presented as examples and are not intended to limit the invention. The invention is defined solely by the scope of the claims set forth below.

[0038] According to one embodiment of the invention, a negative electrode for a lithium-free secondary battery is provided, comprising: a conductive metal layer including a first metal; and a negative electrode current collector including a second metal oxide layer formed on the conductive metal layer, wherein the second metal oxide has a work function greater than that of the first metal.

[0039] The above cathode is formed on a conductive metal layer including a first metal such as copper, and a second metal oxide layer having a work function greater than that of the first metal. At this time, the work function of the metal or metal oxide can be defined as the minimum thermodynamic energy (eV) required to remove one electron from the surface of the solid metal or metal oxide, and can be measured and calculated from the results of analyzing the solid material using UPS (Ultraviolet Photoelectron Spectroscopy).

[0040] In a lithium-free secondary battery including the negative electrode of the above embodiment, as charging and discharging proceed, a lithium metal layer is deposited on the second metal oxide layer. The second metal oxide may form a lithium metal oxide including an oxide of lithium and the second metal at the interface with the lithium metal layer, for example, through the reaction of the following reaction formula 1, and a lithium metal layer may be formed on the lithium metal oxide, or the lithium metal layer may include the lithium metal oxide.

[0041] [Reaction Formula 1]

[0042] MO3+ xLi + + xe - → Li x MO3(x ≤ 1.2)

[0043] As the lithium metal oxide and lithium metal layer at the interface are formed, the lithium metal layer deposited on the second metal oxide layer can have a relatively large work function, and in particular, it has been confirmed to have a significantly larger work function than an independently formed lithium metal foil or a lithium metal layer directly formed on a conductive metal layer including a first metal such as copper. This large work function means that a large amount of energy is required to remove electrons from the lithium metal layer, and due to this large work function, side reactions between the lithium metal layer formed on the second metal oxide layer and the electrolyte can be suppressed.

[0044] Therefore, by applying the negative electrode of one embodiment, not only is the possibility of a short circuit due to a side reaction of a lithium metal layer and an electrolyte in a lithium-free secondary battery reduced, but also the coulombic efficiency of the lithium-free secondary battery increases and the irreversible capacity decreases, thereby improving its life characteristics.

[0045] Meanwhile, in the negative electrode for a lithium-free secondary battery according to the above-described embodiment, the conductive metal layer may have a thickness equivalent to that of a general negative electrode current collector, for example, a thickness of 3 to 500 μm, or 5 to 100 μm, or 7 to 30 μm.

[0046] In addition, the first metal forming the conductive metal layer is a metal that has high conductivity while having relatively low reactivity and does not cause chemical changes in the battery, and can be formed using any metal that has been previously known to be usable as a negative electrode current collector.

[0047] Specific examples thereof include metals such as stainless steel, aluminum, nickel, titanium, or copper, or metals surface-treated with carbon, nickel, titanium, silver, etc. on the surface of copper, aluminum, or stainless steel. This conductive metal layer can be formed in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric. However, considering the excellent conductivity and light weight of the negative electrode current collector and the negative electrode, and the appropriate work function difference and low reactivity with the second metal oxide layer, the first metal may include copper (Cu), and more specifically, may be a copper foil.

[0048] Such a conductive metal layer comprising copper may have a work function of, for example, 4.53 to 5.10 eV, or 4.55 to 4.90 eV, or 4.55 to 4.65 eV.

[0049] In addition, a second metal oxide layer may be formed on at least one surface of the conductive metal layer. As described above, the second metal oxide forming the second metal oxide layer has a work function greater than that of the first metal of the conductive metal layer, thereby reducing side reactions between the lithium metal layer deposited on the negative electrode and the electrolyte during the charge and discharge process of the lithium-free secondary battery.

[0050] More specifically, the second metal oxide may have a work function of 5.5 eV or more, or 5.5 to 6.5 eV, or 5.9 to 6.4 eV, or 6.0 to 6.2 eV. Accordingly, the second metal oxide layer can be formed well on the conductive metal layer with a thin thickness, and side reactions between the lithium metal layer deposited on the negative electrode and the electrolyte can be effectively reduced.

[0051] In terms of the above-described appropriate work function range and effectively suppressing side reactions between the lithium metal layer and the electrolyte, the second metal oxide may include molybdenum oxide (e.g., MoO3) or tungsten oxide (e.g., WO3), and among these, by using tungsten oxide, side reactions between the lithium metal layer and the electrolyte in a lithium-free secondary battery can be further reduced, and the life characteristics of the secondary battery can be further improved.

[0052] The second metal oxide layer may have a thickness of, for example, 10 nm to 1 μm, or 10 to 500 nm, or 10 to 200 nm, in order to effectively suppress the side reaction while not impairing the excellent conductivity and lightness of the negative electrode current collector.

[0053] In addition, the method for forming the second metal oxide layer is not particularly limited, and may be formed by any method for coating a metal oxide on a metal layer. In a specific example, the second metal oxide layer may be formed by thermally evaporating the second metal oxide on the conductive metal layer, and such thermal evaporation may be formed to an appropriate deposition thickness by monitoring the deposition thickness and deposition rate of the second metal oxide in real time using a quartz crystal microbalance (QCM).

[0054] Meanwhile, according to another embodiment of the invention, a lithium-free secondary battery comprising the negative electrode of the above-described embodiment is provided. Such a lithium-free secondary battery may include, for example, the negative electrode of the above-described embodiment; a positive electrode facing the negative electrode; an electrolyte comprising a lithium salt and a non-aqueous organic solvent; and a separator between the positive electrode and the negative electrode.

[0055] In such lithium-free secondary batteries, the negative electrode does not include a separate negative electrode active material layer before charging and discharging. However, as the lithium-free secondary battery is charged and discharged, lithium ions moved from the positive electrode may be deposited on the second metal oxide layer of the negative electrode to form a lithium metal layer, and this lithium metal layer may function as a negative electrode active material.

[0056] During the electrodeposition of the lithium metal layer, a lithium metal oxide may be formed at the interface between the second metal oxide layer and the lithium metal layer by the reaction of the above-described reaction formula 1, and the lithium metal oxide may become a composite oxide of lithium and the second metal. In addition, during the continuous charging and discharging process of the lithium-free secondary battery, at least a portion of the lithium metal oxide may be separated into the second metal and lithium oxide (e.g., Li2O).

[0057] During the charge and discharge process, due to the large work function of the second metal oxide layer, the lithium metal layer deposited on the second metal oxide layer can have a relatively large work function, and for example, it has been confirmed to have a work function greater than that of an independently formed lithium metal foil or a lithium metal layer directly formed on a conductive metal layer such as copper. In a specific embodiment, for the lithium-free secondary battery of the other embodiment, for example, 0.5 mA / cm 2 Under a current of 1 mAh / cm 2When the lithium metal layer is deposited on the negative electrode with a capacity of , the lithium metal layer may have a work function of 2.8 eV or more, or 2.8 to 3.5 eV, or 2.81 to 3.30 eV.

[0058] Since the lithium metal layer has such a large work function, side reactions with the electrolyte can be suppressed during the charging and discharging process of the lithium-free secondary battery, and the stability and life characteristics of the lithium-free secondary battery can be further improved.

[0059] In addition, a solid electrolyte interphase may be additionally formed on the second metal oxide layer of the cathode by a reaction between lithium ions and the electrolyte during initial charge and discharge. This solid electrolyte interphase may include, for example, lithium fluoride, and may suppress additional side reactions with the electrolyte.

[0060] The formation of the above solid electrolyte interfacial film can be confirmed by performing a CV (Cyclic Voltammetry) test on the secondary battery of the other embodiment and analyzing the depth-dependent element profile of the negative electrode of the secondary battery using X-ray photoelectron spectroscopy (XPS). From the results of the formation of the solid electrolyte interfacial film on the second metal oxide layer, it can be confirmed that the second metal oxide layer does not simply act as a surface protective layer of the negative electrode current collector, but rather acts as an electrically active layer on which a lithium metal layer is deposited during charging and discharging.

[0061] Meanwhile, in the lithium-free secondary battery of the other embodiment, the positive electrode may include a positive electrode current collector and a positive electrode active material layer positioned on the positive electrode current collector.

[0062] These positive electrodes can be manufactured by mixing an active material and a binder, and in some cases, a conductive material, a filler, etc. in a solvent to prepare a positive electrode slurry composition, and applying the composition to a positive electrode current collector.

[0063] The positive electrode current collector may generally have a thickness of 3 to 500 μm. In addition, the positive electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. The current collector may also form fine unevenness on its surface to increase the adhesive strength of the positive electrode active material, and various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric are possible.

[0064] And, in the case of the above positive electrode active material, it may include a compound capable of reversible intercalation and deintercalation of lithium, specifically a lithium metal oxide containing one or more metals such as iron, cobalt, manganese, nickel, or aluminum and lithium.

[0065] Specifically, the lithium metal oxide is a lithium-manganese oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt oxide (e.g., LiCoO2, etc.), a lithium-nickel oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese oxide (e.g., LiNi 1-Y Mn Y O2 (here, 0 <Y<1), LiMn 2-Z Ni Z O4 (where 0<Z<2), etc.), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y1 Co Y1 O2 (here, 0 <Y1<1) 등), 리튬-망간-코발트계 산화물(예를 들면, LiCo 1-Y2 Mn Y2O2 (here, 0 <Y2<1), LiMn 2-Z1 Co Z1 O4 (wherein, 0<Z1<2) etc.), lithium-nickel-manganese-cobalt oxides (e.g., Li(Ni p Co q Mn r )O2(wherein, 0<p<1, 0<q<1, 0<r<1, p+q+r=1) or Li(Ni p1 Co q1 Mn r1 )O4 (wherein, 0<p1<2, 0<q1<2, 0<r1<2, p1+q1+r1=2) etc.), lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r2 M s2 )O2 (wherein, M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r2 and s2 are atomic fractions of independent elements, respectively, 0<p2<1, 0<q2<1, 0<r2<1, 0<s2<1, p2+q2+r2+s2=1), etc.), or lithium iron phosphate (e.g., Li 1+a Fe 1-x M x (PO 4-b )X b (Here, M is at least one selected from Al, Mg, and Ti, X is at least one selected from F, S, and N, -0.5≤a≤+0.5, 0≤x≤0.5, 0≤b≤0.1), and any one or two or more compounds thereof may be included.

[0066] Among these, the positive electrode active material includes a lithium metal oxide including lithium and two or more metals selected from the group consisting of nickel, manganese, cobalt, and aluminum, and the lithium metal oxide may include nickel in an amount of 50 mol% or more, or 60 to 99 mol%, or 70 to 95 mol%, based on the total metal content excluding lithium. Such a lithium metal oxide may be represented by, for example, the following chemical formula 1:

[0067] [Chemical Formula 1]

[0068] Li x Ni a Co b M 1 c M 2 d O2

[0069] In the above chemical formula 1, the M 1 Mn and Al may be one or more selected from or a combination thereof, and M 2 may be at least one selected from the group consisting of Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S, and may be 0.90≤x≤1.1, or 0.95≤x≤1.08, or 1.0≤x≤1.08, and may be 0.50≤a<1.0, or 0.60≤a≤0.99, or 0.70≤a≤0.95. In addition, 0 <b≤0.3이고, 0<c≤0.3이고, 0≤d≤0.1일 수 있다.

[0070] By using a lithium metal oxide containing such a high nickel content as a positive electrode active material and combining it with an anode of one embodiment, the output and capacity characteristics, as well as the life characteristics, of a lithium-free secondary battery can be further improved.

[0071] The above-described positive electrode active material may be included in an amount of 60 to 99 wt%, or 70 to 99 wt%, or 80 to 98 wt% based on the total weight of the positive electrode active material layer.

[0072] Meanwhile, the conductive material included in the positive electrode active material layer is a component for further improving the conductivity of the positive electrode active material. The conductive material is not particularly limited as long as it has conductivity without causing chemical changes in the battery. For example, carbon powder such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive nanomaterials such as carbon nanofibers or carbon nanotubes; fluorinated carbon powder; conductive powder such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. can be used. Among these, the conductive material can further lower the resistance of a lithium-free secondary battery and improve output characteristics, etc. by including a conductive nanomaterial such as carbon nanotubes or carbon nanofibers.

[0073] Typically, the conductive material may be included in an amount of 1 to 20 wt%, or 1 to 15 wt%, or 1 to 10 wt% based on the total weight of the positive electrode active material layer.

[0074] The binder optionally included in the above-described positive electrode active material layer is a component that assists in the bonding of the positive electrode active material and the conductive material, and in the bonding to the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, nitrile rubber, styrene-butadiene rubber, or fluororubber, and a mixture or copolymer of two or more selected from these may also be used.

[0075] Typically, the binder may be included in an amount of 1 to 20 wt%, or 1 to 15 wt%, or 1 to 10 wt% based on the total weight of the positive electrode active material layer.

[0076] Additionally, a filler may be optionally added to the positive electrode as a component that suppresses its expansion. Such filler is not particularly limited as long as it can suppress the expansion of the electrode without causing chemical changes in the battery. Examples of fillers that can be used include olefin polymers such as polyethylene and polypropylene; fibrous materials such as glass fiber and carbon fiber; and the like.

[0077] The above-described positive electrode can be manufactured by dispersing and mixing the positive electrode active material, binder, and conductive agent in a dispersion medium (solvent) to make a slurry, applying the slurry on a metal current collector, and then drying and rolling. At this time, the dispersion medium may be NMP (N-methyl-2-pyrrolidone), DMF (Dimethyl formamide), DMSO (Dimethyl sulfoxide), ethanol, isopropanol, water, and mixtures thereof, but is not necessarily limited thereto.

[0078] Meanwhile, the lithium-free secondary battery of the other embodiment further includes an electrolyte including a non-aqueous organic solvent and a lithium salt.

[0079] The lithium salt included in the above electrolyte is used as a medium for transferring ions within a secondary battery. Lithium salt is, for example, Li as a cation. + Including, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO2- , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - and SCN - It may include an anion selected from the group consisting of .

[0080] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10, LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (lithium bis(fluorosulfonyl) imide, LiN(SO2F)2), LiBETI (lithium bis(perfluoroethanesulfonyl) imide, LiN(SO2CF2CF3)2) and LiTFSI (lithium bis(trifluoromethanesulfonyl) imide, LiN(SO2CF3)2).

[0081] The concentration of the above lithium salt can be appropriately changed within a commonly usable range, and can be included in the electrolyte at a concentration of 0.5 M to 6 M, or a concentration of 1 M to 5 M.

[0082] In a more specific embodiment, the electrolyte may contain a lithium salt in a relatively low concentration of 0.5 M or more and less than 2 M, or 0.7 M to 1.5 M, but may also contain the lithium salt in a high concentration of 2 M to 6 M, or 2.5 M to 5.5 M. By using an electrolyte containing such a high-concentration lithium salt, the output characteristics of the secondary battery can be further improved. In addition, by using an electrolyte containing the high-concentration lithium salt, the growth of lithium dendrites and the like from the lithium metal layer deposited on the second metal oxide layer can be suppressed, so that the life characteristics of the lithium-free secondary battery can be further improved.

[0083] Meanwhile, the type of non-aqueous organic solvent that can be included in the electrolyte is not particularly limited, and any organic solvent that has been previously known to be applicable to electrolytes of lithium ion batteries, etc., can be used. Examples of such organic solvents include at least one selected from the group consisting of carbonate solvents, ether solvents, nitrile solvents, phosphate solvents, and sulfone solvents. However, considering the stability of the lithium metal layer deposited on the second metal oxide layer, etc., it is preferable that the non-aqueous organic solvent include an ether solvent.

[0084] More specifically, as the carbonate solvent, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, methyl propyl carbonate, ethyl methyl carbonate, ethyl propyl carbonate or methyl (2,2,2-trifluoroethyl) carbonate can be used, and as the phosphate solvent, trimethyl phosphate, triethyl phosphate or 2-(2,2,2-trifluoroethoxy)-1,3,2-dioxaphosphorane 2-oxide can be used.

[0085] In addition, as the ether solvent, dibutyl ether, tetraglyme, diglyme, dimethoxy ethane, or tetrahydrofuran derivatives such as 2-methyl tetrahydrofuran can be used, and as the nitrile solvent, succinonitrile, adiponitrile, sebaconitrile, acetonitrile, or propionitrile can be used. In addition, as the sulfone solvent, dimethyl sulfone, ethylmethyl sulfone, or sulforane can be used.

[0086] Meanwhile, the lithium-free secondary battery of the other embodiment described above may further include a porous separator interposed between the positive electrode and the negative electrode.

[0087] These porous membranes can be made of olefin polymers such as polyethylene and polypropylene, glass fibers, etc. in the form of sheets, multi-membranes, microporous films, woven fabrics, and non-woven fabrics, but are not necessarily limited thereto. However, it may be preferable to use porous polyethylene or porous glass fiber non-woven fabric (glass filter) as the membrane, and it may be more preferable to use porous glass filter (glass fiber non-woven fabric) as the membrane. The membrane may be an insulating thin film having high ion permeability and mechanical strength, and the pore diameter of the membrane may generally be in the range of 0.01 to 10 ㎛, and the thickness may generally be in the range of 5 to 300 ㎛, but is not limited thereto.

[0088] In addition, in another example of the lithium-free secondary battery, the separator may be integrated with the electrolyte and interposed between the positive and negative electrodes in the form of an electrolyte membrane or electrolyte film. In this case, the electrolyte membrane or electrolyte film may be in the form of a polymer matrix containing the lithium salt and a non-aqueous organic solvent described above, and a well-known polymer-based solid electrolyte or the like may be used as the polymer matrix. In this case, the lithium-free secondary battery of the other embodiment may be a semi-solid battery that uses a liquid electrolyte and a solid electrolyte in combination.

[0089] Meanwhile, the lithium-free secondary battery of the above-described other embodiment can be manufactured according to a conventional method in the art. For example, the electrode assembly including the positive electrode, negative electrode, and separator can be housed in a case and manufactured by injecting and impregnating the electrolyte described above.

[0090] These lithium-free secondary batteries can be applied to battery cells used as power sources for small devices, and are particularly suitable for use as unit cells in battery modules that serve as power sources for medium- to large-sized devices.

[0091]

[0092] Below, preferred embodiments of the invention, comparative examples to compare with them, and experimental examples for evaluating them are described. However, the following examples are merely preferred embodiments of the invention, and the present invention is not limited to the following examples.

[0093]

[0094] Comparative Example 1: Cathode for lithium-free secondary batteries

[0095] Copper foil itself having a thickness of 10㎛ was used as the negative electrode for the lithium-free secondary battery of Comparative Example 1.

[0096] The work function (eV) of the negative electrode of Comparative Example 1, i.e., the copper foil, was measured by UPS (Ultraviolet Photoelectron Spectroscopy) and the results are shown in Fig. 2. The negative electrode for a lithium-free secondary battery made of the copper foil of Comparative Example 1 was confirmed to have a work function of approximately 4.62 eV. The work function analysis was performed using X-ray photoelectron spectroscopy (Axis-Supra by Kratos) under irradiation of a He|X-ray source (hv=21.2 eV).

[0097]

[0098] Example 1: Preparation of a negative electrode for a lithium-free secondary battery

[0099] First, on a copper foil having a thickness of 10 μm, MoO3 was thermally deposited while monitoring the deposition thickness and deposition rate in real time using a quartz crystal microbalance (QCM), thereby forming a molybdenum oxide layer having a thickness of 20 nm. This was used as the negative electrode for the lithium-free secondary battery of Example 1.

[0100] The cross-section of the cathode of Example 1 above was analyzed using FIB-TEM (Focused Ion Beam Transmission Electron Microscopy), and the image is shown in Fig. 1a. From the analysis results, it was confirmed that a molybdenum oxide layer was formed on the copper foil.

[0101] In addition, the work function (eV) of the cathode of Example 1 was measured by analyzing it with UPS (Ultraviolet Photoelectron Spectroscopy) under the same conditions as Comparative Example 1, and the results are shown in Fig. 2. The molybdenum oxide layer of Example 1 was confirmed to have a work function of about 6.31 eV, which is greater than that of copper foil (about 4.62 eV).

[0102]

[0103] Example 2: Preparation of a negative electrode for a lithium-free secondary battery

[0104] First, on a copper foil having a thickness of 10 μm, WO3 was thermally deposited while monitoring the deposition thickness and deposition rate in real time using a quartz crystal microbalance (QCM) to form a 20 nm thick tungsten oxide layer. This was used as the negative electrode for the lithium-free secondary battery of Example 2.

[0105] The cross-section of the cathode of Example 2 above was analyzed using FIB-TEM (Focused Ion Beam Transmission Electron Microscopy), and the image is shown in Fig. 1b. From the analysis results, it was confirmed that a tungsten oxide layer was formed on the copper foil.

[0106] In addition, the work function (eV) of the cathode of Example 2 was measured by analyzing it with UPS (Ultraviolet Photoelectron Spectroscopy) under the same conditions as Comparative Example 1, and the results are shown in Fig. 2. It was confirmed that the tungsten oxide layer of Example 2 had a work function of about 6.07 eV, which is greater than that of copper foil (about 4.62 eV).

[0107]

[0108] Experimental Example 1: Confirmation of a Solid Interfacial Electrolyte Membrane

[0109] For the negative electrodes for lithium-free secondary batteries of Examples 1 and 2, a CV (Cyclic Voltammetry) test was performed under conditions of 3 V-0 V and 1 to 5 cycles, and the results of the CV test are shown in Figures 3a and 3b, respectively. From the results of the CV test, it was confirmed that as a potential was applied to the negative electrode, an electrochemical reaction occurred on the molybdenum oxide layer (Example 1) or the tungsten oxide layer (Example 2), and lithium deposition occurred.

[0110] In addition, the depth-dependent elemental profiles of the cathodes of Examples 1 and 2, for which the above-described CV (Cyclic Voltammetry) test was performed, were analyzed by X-ray photoelectron spectroscopy (XPS), and the analysis results are shown in Figs. 4a and 4b, respectively. From these analysis results, it was confirmed that a solid electrolyte interface film was formed on the molybdenum oxide layer (Example 1) or the tungsten oxide layer (Example 2).

[0111] From this, it was confirmed that the molybdenum oxide layer (Example 1) or the tungsten oxide layer (Example 2) in the negative electrode of Examples 1 and 2 acts as an electrically active layer on which a lithium metal layer is deposited during charging and discharging of a lithium-free secondary battery, rather than as a surface protective layer of the negative electrode current collector.

[0112]

[0113] Experimental Example 2: Work function measurement after electrodeposition of a lithium metal layer

[0114] A half-cell was manufactured using the cathode of the embodiment or comparative example as one electrode and a 150 μm lithium foil as the other electrode. This half-cell was manufactured to include a porous polypropylene separator interposed between the two electrodes and an electrolyte in which a lithium salt of LiFSI is dissolved in dimethoxyethane (DME) at a concentration of 4 M.

[0115] 0.5 mA / cm for the above half cell 2 1 mAh / cm under current application 2 While charging and discharging at a capacity of , a lithium metal layer was deposited on the negative electrode. After the lithium metal deposition, the half-cell was disassembled in a glove box filled with argon gas, and the work function of the negative electrode on which the lithium metal layer was deposited was measured.

[0116] The measurement of the above work function was performed by analyzing each cathode using UPS (Ultraviolet Photoelectron Spectroscopy) in the same manner as in the examples and comparative examples, and the results of the work function measurement are shown in Fig. 5.

[0117] Referring to Fig. 5, the work function of the lithium foil itself (Ref.) has a small value of 1.91 eV, and the lithium metal layer deposited on the negative electrode (copper foil) of Comparative Example 1 also has a relatively low work function of 2.77 eV, whereas the negative electrodes of Examples 1 and 2, in particular, the lithium metal layers deposited on the molybdenum oxide layer or the tungsten oxide layer, were confirmed to have high work functions of 2.81 eV and 3.20 eV, respectively. This is expected to be due to the presence of lithium metal oxide formed at the interface between the lithium metal layer and the molybdenum oxide layer or the tungsten oxide layer.

[0118] From this high work function, it was predicted that in a lithium-free secondary battery including the negative electrode of the embodiment, side reactions between the lithium metal layer deposited on the negative electrode and the electrolyte would be suppressed.

[0119]

[0120] Experimental Example 3: Measurement of corrosion resistance and interface resistance after electrodeposition of a lithium metal layer.

[0121] 0.25 mA / cm for each half-cell manufactured in the above experimental example 2 2 4 mAh / cm under current application 2 Impedance analysis was performed while a lithium metal layer was deposited on the negative electrode by charging and discharging at a capacity of . The impedance analysis was performed using a constant voltage EIS (Potentiostatic. EIS, PEIS) method under the conditions of a temperature of 25°C, a frequency of 0.1 to 1,000,000 Hz, and a voltage of 10 mV.

[0122] This impedance analysis was performed for approximately 24 hours, and the interface resistance was measured over time, and the measurement results are shown in Fig. 6.

[0123] Referring to Fig. 6, it was confirmed that the increase in interfacial resistance over time was very low in the half-cells including the negative electrodes of Examples 1 and 2 compared to Comparative Example 1. This interfacial resistance is resistance due to a film formed by the side reaction between the lithium metal layer and the electrolyte and the corrosion of the lithium metal layer, and it was confirmed that the side reaction between the lithium metal layer and the electrolyte and the corrosion of the lithium metal layer were greatly reduced in Examples 1 and 2 compared to Comparative Example 1.

[0124]

[0125] Experimental Example 4: Evaluation of the Initial Coulombic Efficiency of Half-Cells

[0126] For each half-cell manufactured in Experimental Example 2 using the cathodes of the examples and comparative examples, the coulombic efficiency per cycle was evaluated, and the evaluation results for the initial coulombic efficiency in the first cycle were compared and shown in Fig. 7.

[0127] Referring to Fig. 7, it was confirmed that the half-cell of the embodiment exhibited an initial Coulomb efficiency that was significantly improved compared to the comparative example.

[0128]

[0129] Experimental Example 5: Evaluation of the Initial Coulombic Efficiency of a Full Cell

[0130] First, LiNi is used as the positive electrode active material. 0.5 Co 0.2 Mn 0.3 O2 was used, carbon black was used as a conductive material, and PVDF polymer was used as a binder. The positive electrode active material: conductive material: binder were mixed in a weight ratio of 90:5:5 in an N-methylpyrrolidone solvent to prepare a slurry composition, which was then applied to an aluminum current collector, and dried and rolled in a vacuum oven at 110°C to prepare a positive electrode.

[0131] An electrode assembly was manufactured by interposing a porous polypropylene separator between the positive electrode and the negative electrode manufactured in the examples or comparative examples, and this was placed inside the case, and then an electrolyte in which a lithium salt of LiFSI was dissolved in dimethoxyethane (DME) at a concentration of 4 M was injected to manufacture a full cell of a lithium-free secondary battery (electrolyte / positive electrode ratio: 2.15 g / Ah).

[0132] For these lithium-free secondary batteries, charge and discharge tests were performed at 25°C in CC mode and by charging to 4.35 V at 0.2 C and discharging to 3.0 V at a constant current of 1.0 C. During the charge and discharge tests for 100 cycles, the capacity retention rate for each cycle was measured, and the measurement results are shown in Fig. 8.

[0133] Referring to Fig. 8, it was confirmed that Examples 1 and 2 exhibited superior cycle-by-cycle capacity retention and life characteristics compared to Comparative Example 1. This appears to be due to the suppression of side reactions between the lithium metal layer and the electrolyte in the Examples, thereby delaying capacity deterioration.

Claims

1. A conductive metal layer including a first metal; and A negative electrode current collector including a second metal oxide layer formed on a conductive metal layer, A negative electrode for a lithium-free secondary battery, wherein the second metal oxide has a work function greater than that of the first metal.

2. A negative electrode for a lithium-free secondary battery, wherein the first metal comprises copper (Cu) and the second metal oxide has a work function of 5.5 eV or more.

3. A negative electrode for a lithium-free secondary battery according to claim 1, wherein the second metal oxide comprises molybdenum oxide or tungsten oxide.

4. A negative electrode for a lithium-free secondary battery, wherein the second metal oxide layer has a thickness of 10 nm to 1 μm in the first paragraph.

5. A negative electrode for a lithium-free secondary battery, wherein the second metal oxide layer is formed by thermal evaporation of the second metal oxide on the conductive metal layer in the first paragraph.

6. The cathode of any one of paragraphs 1 to 5; An anode facing the cathode; An electrolyte comprising a lithium salt and a non-aqueous organic solvent; and A lithium-free secondary battery comprising a separator between the positive and negative electrodes.

7. A lithium-free secondary battery further comprising a lithium metal layer deposited on the second metal oxide layer of the negative electrode according to charging and discharging of the lithium-free secondary battery in accordance with paragraph 6.

8. In the 7th paragraph, the lithium metal layer is 1 mAh / cm 2 A lithium-free secondary battery having a work function of 2.8 eV or more when electrodeposited with a capacity of .

9. In the 7th paragraph, the lithium metal layer further includes a lithium metal oxide formed at the interface with the second metal oxide layer, The above lithium metal oxide is a lithium-free secondary battery comprising an oxide of lithium and a second metal.

10. A lithium-free secondary battery further comprising a solid electrolyte interphase formed on the second metal oxide layer of the negative electrode in the sixth paragraph.

11. In the 6th paragraph, the positive electrode comprises a lithium metal oxide including lithium and two or more metals selected from the group consisting of nickel, manganese, cobalt and aluminum, A lithium-free secondary battery wherein the lithium metal oxide contains nickel in an amount of 50 mol% or more based on the total metal content excluding lithium.

12. A lithium-free secondary battery according to claim 6, wherein the lithium salt is included in the electrolyte at a concentration of 0.5 M to 6 M.

13. A lithium-free secondary battery according to claim 6, wherein the non-aqueous organic solvent comprises at least one selected from the group consisting of carbonate solvents, ether solvents, nitrile solvents, phosphate solvents, and sulfone solvents.

Citation Information

Patent Citations

  • Secondary battery, negative electrode collector, electronic apparatus and electric vehicle

    JP2013164971A

  • Data visualization method and device

    KR1020230053384A

  • Gas turbine blade testing apparatus and method thereof

    KR1020240138633A

  • Artificial intelligence-based smart pass medical device system using mask detection and body temperature correction of visitors

    KR102310915B1

  • Method of diagnosing microsatellite instability using coefficient of variation of sequence length at microsatellite locus

    KR102717923B1