Anode for lithium-free secondary battery and lithium-free secondary battery comprising same
The negative electrode with a copper-zinc intermetallic compound layer addresses lithium dendrite growth and stability issues in lithium-free secondary batteries, enhancing electrochemical and lifespan performance while simplifying manufacturing and enabling high-energy-density production.
Patent Information
- Application Number
- PCT/KR2024/006158
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-22
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-14
AI Technical Summary
Lithium-free secondary batteries face challenges with lithium dendrite growth and instability due to uneven lithium metal deposition, leading to short circuits and poor lifespan, and existing solutions for improving these issues are costly and complex, making mass production difficult.
A negative electrode for lithium-free secondary batteries is developed, featuring a conductive metal layer with a lithium electrodeposition inducing layer composed of a copper-zinc intermetallic compound, which reduces interface resistance and overvoltage, suppressing dendrite growth and enhancing electrochemical properties through a simplified manufacturing process.
The solution effectively improves the electrochemical and lifespan characteristics of lithium-free secondary batteries by promoting uniform lithium deposition, reducing resistance and overvoltage, and allowing for the production of thin, high-energy-density batteries with extended cycle life.
Smart Images

Figure KR2024006158_14112024_PF_FP_ABST
Abstract
Description
Anode for lithium-free secondary battery and lithium-free secondary battery containing the same
[0001] Cross-citation with related application(s)
[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0059728, filed May 9, 2023, and Korean Patent Application No. 10-2024-0053381, filed April 22, 2024, the entire contents of which are incorporated herein by reference.
[0003] The present invention relates to a negative electrode for a lithium-free secondary battery, a method for manufacturing the same, and a lithium-free secondary battery capable of improving the electrochemical characteristics and lifespan characteristics of the lithium-free secondary battery.
[0004] Lithium metal batteries utilize lithium metal (Li-metal) as the anode active material. Compared to conventional graphite or lithium alloy anodes, lithium metal batteries theoretically offer significantly higher energy density and capacity. Therefore, research and development are ongoing to apply these lithium metal batteries to batteries requiring high energy densities.
[0005] However, lithium metal batteries have disadvantages such as large volume changes in the negative electrode during the charge and discharge process, the growth of needle-like lithium metal layers (such as lithium dendrites), and the occurrence of side reactions between the lithium metal layers and the electrolyte due to the highly reactive nature of lithium metal, resulting in large irreversible capacity. As a result, lithium metal batteries have a high possibility of electrode short-circuiting and insufficient stability and lifespan characteristics, which have prevented their commercialization.
[0006] Recently, as an alternative to the lithium metal battery, research and interest in lithium-free secondary batteries (anode-free secondary batteries) that form the anode with the anode current collector itself without forming a separate lithium metal layer or other anode active material layer on the anode current collector have been growing. Such lithium-free secondary batteries can be defined as batteries that utilize lithium metal as an anode active material as lithium is deposited on the anode current collector during charging.
[0007] However, since existing lithium-free secondary batteries also utilize lithium metal as an anode active material, problems such as the growth of lithium dendrites due to uneven growth of lithium metal may still arise.
[0008] To overcome these technical limitations, technologies have been reported, such as fabricating a current collector with a lithium-philic material or increasing the surface area of the current collector to induce uniform deposition of lithium.
[0009] However, most processes used to fabricate current collectors containing these lithium-philic materials or three-dimensional current collectors with high surface areas suffer from long processing times or high costs, hindering mass production. Furthermore, these methods present additional challenges, such as the difficulty in fabricating thin current collectors, making it difficult to fully utilize the high energy density of lithium-free secondary batteries.
[0010] Accordingly, the present invention provides an anode for a lithium-free secondary battery and a method for manufacturing the same, which can improve the electrochemical characteristics and lifespan characteristics of a lithium-free secondary battery by suppressing the growth of lithium dendrites, etc., and can be manufactured through a simplified process and with a thin thickness.
[0011] In addition, the present invention provides a lithium-free secondary battery exhibiting improved electrochemical characteristics and lifespan characteristics, including the negative electrode.
[0012] According to one embodiment of the invention, there is provided a negative electrode for a lithium-free secondary battery, comprising: a conductive metal layer; and a lithium electrodeposition inducing layer formed on the conductive metal layer and including an intermetallic compound of copper and zinc.
[0013] In such a negative electrode, the lithium electrodeposition-inducing layer may include an intermetallic compound in which copper and zinc are combined in a weight ratio of 2:8 to 9.5:0.5. In a further embodiment, the lithium electrodeposition-inducing layer may include an intermetallic compound in which copper and zinc are combined in a weight ratio of 3:7 to 9:1 and include oxygen in an amount of 0.01 to 5 wt% based on the weight of the total intermetallic compound.
[0014] Additionally, in the above negative electrode, the lithium electrodeposition induction layer may have a thickness of 0.05 to 2 μm.
[0015] Meanwhile, according to another embodiment of the invention, a method for manufacturing the cathode of the above embodiment is provided, comprising the step of electrically depositing copper and zinc on a conductive metal layer using an electrolyte including a copper precursor, a zinc precursor, and pyrophosphate.
[0016] In this manufacturing method, the electrical deposition step can be performed by applying a voltage to an electrical deposition system including a working electrode including the conductive metal layer; a counter electrode including an alloy of copper and zinc; and the electrolyte.
[0017] In addition, the manufacturing method may further include a step of heat-treating the electrical deposit at a temperature of 200°C or higher under a vacuum or inert gas atmosphere after the electrical deposition step, and by performing this heat-treatment step, the chemical composition of the lithium electrodeposition-inducing layer may change, and the electrochemical characteristics of the negative electrode may be further improved.
[0018] Meanwhile, according to a further embodiment of the invention, a lithium-free secondary battery is provided, comprising: a positive electrode including a positive active material; a negative electrode according to one embodiment; and a separator or electrolyte layer interposed between the positive electrode and the negative electrode.
[0019] In these lithium-free secondary batteries, a lithium metal layer is deposited on the lithium electrodeposition induction layer of the negative electrode during the charging process, thereby acting as a negative electrode active material.
[0020] According to one embodiment of the invention, a cathode can be manufactured by a simple process of forming an intermetallic compound of copper and zinc by electrical deposition on a conductive metal layer.
[0021] It was confirmed that the interfacial resistance and overvoltage of the negative electrode can be significantly reduced during the lithium metal layer deposition process when the battery is charged by the formation of a lithium electrodeposition-inducing layer including such intermetallic compounds. Due to the reduction in resistance and overvoltage during the electrodeposition of the lithium metal layer, the growth of lithium dendrites and side reactions in the negative electrode of a lithium-free secondary battery can be suppressed, and the life characteristics of the lithium-free secondary battery can be improved. In addition, due to the reduction in resistance, etc., the electrochemical characteristics of the lithium-free secondary battery can be improved.
[0022] Accordingly, according to the present invention, not only can the negative electrode of a lithium-free secondary battery be manufactured in a thin form through a simplified process, but also the electrochemical characteristics and life characteristics of the lithium-free secondary battery can be improved.
[0023] FIG. 1 is a schematic diagram illustrating an example of an electrodeposition system used for manufacturing a cathode according to an embodiment of the invention.
[0024] Figures 2a to 2c are photographs of the cathode surfaces formed in Comparative Example 2 (Figure 2a), Example 1 (Figure 2b), and Example 2 (Figure 2c), each analyzed using an electron microscope.
[0025] Figure 3 is a photograph showing the change in film quality of the lithium electrodeposition induction layer before and after heat treatment, analyzed using an electron microscope, during the negative electrode manufacturing process of Example 5.
[0026] Figure 4 is a graph showing the results of overvoltage evaluation during lithium deposition for half cells including the negative electrodes of Comparative Example 1 and Example 2.
[0027] Figure 5 is a graph showing the results of evaluating the life characteristics of half cells including the cathodes of Comparative Examples 1 and 2 and Examples 1 and 2.
[0028] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless specifically stated otherwise.
[0029] The terms "about," "substantially," and the like used throughout this specification are used to mean at or near the numerical value when manufacturing and material tolerances inherent to the meanings stated are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that state precise or absolute values to aid understanding of this specification. The terms "step of doing" or "step of" used throughout this specification do not mean "step for doing."
[0030] In this specification, the term "combination of these" included in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including one or more selected from the group consisting of the components.
[0031] In addition, in the present specification, the term “lithium-free secondary battery” may refer to a secondary battery in which, in a state before charging and discharging, for example, in a state immediately after manufacturing, there is no separate negative electrode active material layer, such as a lithium metal layer, a lithium alloy layer, or other carbon or silicon-containing layer, on the negative electrode current collector (e.g., a negative electrode current collector including a conductive metal layer such as copper and a lithium electrodeposition induction layer). Accordingly, the “lithium-free secondary battery” may be defined as one that does not include a separate negative electrode active material layer (e.g., a lithium metal layer, etc.) on the negative electrode current collector in a state before charging and discharging. However, it should be understood that addition of a separate insulating layer or functional layer in addition to the negative electrode active material layer is not limited.
[0032] In addition, the term “lithium-free secondary battery” above cannot be interpreted as limiting the presence of a lithium-containing positive electrode active material or limiting the presence of a lithium metal layer or lithium-containing compound deposited on the negative electrode according to the charging and discharging operation.
[0033]
[0034] Hereinafter, based on the above definitions, implementation examples of the invention will be described in detail. However, these are presented as examples and are not intended to limit the invention. The invention is defined solely by the scope of the claims set forth below.
[0035]
[0036] According to one embodiment of the invention, a negative electrode for a lithium-free secondary battery may include a conductive metal layer; and a lithium electrodeposition inducing layer formed on the conductive metal layer and including an intermetallic compound in which copper and zinc are combined.
[0037] It was confirmed that the interfacial resistance and overvoltage of the negative electrode can be reduced by the formation of an intermetallic compound in which the copper and zinc are chemically bonded. This is believed to be due to the zinc component contained in the intermetallic compound. Due to this reduction in interfacial resistance and overvoltage, not only can the electrochemical characteristics of a lithium-free secondary battery be improved, but also the uniform electrodeposition of lithium metal can be induced, which can suppress the growth of lithium dendrites, etc., which can result in improved life characteristics of a lithium-free secondary battery.
[0038] In addition, the negative electrode forms an intermetallic compound of copper and zinc by electrical deposition, instead of simply forming a lithium-philic metal such as zinc on a conductive metal layer. During battery operation, the lithium-philic metal such as zinc may cause volume expansion by undergoing an alloying reaction with lithium, and such volume expansion may be a factor in reducing the lifespan characteristics of a lithium-free secondary battery. In contrast, the intermetallic compound can alleviate the volume expansion caused by the alloying reaction with lithium, thereby further improving the lifespan characteristics of a lithium-free secondary battery.
[0039] In addition, the negative electrode of the above embodiment can be manufactured through a simplified process of electrical deposition, and can be formed with a thin thickness that does not include a three-dimensional structure, etc. As a result, the high energy density of a lithium-free secondary battery can be fully utilized using the negative electrode.
[0040] Meanwhile, in the negative electrode for a lithium-free secondary battery according to the above-described embodiment, the conductive metal layer may have a thickness equivalent to that of a general negative electrode current collector, for example, a thickness of 3 to 500 μm, or 5 to 100 μm, or 7 to 50 μm.
[0041] In addition, the conductive metal layer can be formed using any metal that has been previously known to be usable as a negative electrode current collector, as a metal that has high conductivity while having relatively low reactivity and does not cause chemical changes in the battery.
[0042] Specific examples thereof include metals such as stainless steel, aluminum, nickel, titanium, or copper, or surfaces of copper, aluminum, or stainless steel that have been surface-treated with carbon, nickel, titanium, silver, etc. The conductive metal layer may be formed in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric. However, considering the excellent conductivity and light weight of the negative electrode current collector and the negative electrode, and the appropriate formation of the lithium electrodeposition induction layer, the conductive metal layer may include copper, and more specifically, the conductive metal layer may be made of a copper foil.
[0043] In the negative electrode of the above embodiment, a lithium electrodeposition inducing layer is formed on the conductive metal layer. This lithium electrodeposition inducing layer may include, for example, an intermetallic compound formed by electrical deposition on the conductive metal layer, which is a combination of copper and zinc.
[0044] More specifically, the intermetallic compound may be a compound in which copper and zinc are chemically bonded in a weight ratio of 2:8 to 9.5:0.5, or 3:7 to 9:1, or 3:7 to 6:4. In a specific embodiment, the intermetallic compound may be an intermetallic compound that does not include additional metal elements and substantially does not include oxygen.
[0045] If the content of copper contained in the intermetallic compound is excessively high, the interfacial resistance and overvoltage of the negative electrode increase, which may induce lithium dendrite growth and deteriorate the electrochemical characteristics and life characteristics of the lithium-free secondary battery. Conversely, if the content of zinc is excessively high, side reactions between the negative electrode and electrolyte, volume expansion of the negative electrode, etc. may increase, which may deteriorate the life characteristics of the lithium-free secondary battery.
[0046] As will be described in more detail below, the lithium electrodeposition-inducing layer including the intermetallic compound may be formed by electrical deposition and then additionally heat-treated. This heat treatment appears to cause some of the zinc component from the lithium electrodeposition-inducing layer to diffuse around the conductive metal layer and the like, and a trace amount of the zinc component to volatilize. As a result, the chemical composition of the lithium electrodeposition-inducing layer changes, while micro-defects are removed, allowing the lithium electrodeposition-inducing layer to become more uniform and dense.
[0047] In a specific example, the lithium electrodeposition induction layer after the heat treatment may include an intermetallic compound in which copper and zinc are chemically bonded in a weight ratio of 3:7 to 9:1, or 5:5 to 9:1, or 7:3 to 9:1, and includes oxygen in an amount of 5 wt% or less, or 0.01 to 5 wt%, or 0.1 to 3 wt% based on the weight of the total intermetallic compound.
[0048] As the negative electrode of one embodiment includes a lithium electrodeposition-inducing layer that is uniform and densified by the heat treatment, the interfacial resistance of the negative electrode can be further reduced, and the electrochemical characteristics or life characteristics of a lithium-free secondary battery can also be improved. This is presumably because the lithium electrodeposition-inducing layer after the heat treatment can induce more uniform lithium deposition, thereby further suppressing the formation of lithium dendrites, etc.
[0049] The above-described lithium electrodeposition induction layer can be formed on the conductive metal layer with a thickness of 0.05 to 2 μm, or 0.1 to 1 μm, or 0.1 to 0.5 μm. By forming the layer with such a thickness, the resistance and overvoltage of the lithium-free secondary battery can be effectively reduced, while reducing the decrease in the energy density of the battery due to an increase in the thickness of the negative electrode.
[0050] Meanwhile, according to another embodiment of the invention, a method for manufacturing an anode for a lithium-free secondary battery of the above-described embodiment is provided. The method for manufacturing such an anode may include a step of electrically depositing copper and zinc on a conductive metal layer using an electrolyte including a copper precursor, a zinc precursor, and pyrophosphate.
[0051] In this manufacturing method, the electrical deposition step can be performed by applying a voltage to an electrical deposition system including a working electrode including the conductive metal layer; a counter electrode including an alloy of copper and zinc; and the electrolyte. FIG. 1 illustrates an example of such an electrical deposition system, in which copper foil is used as the working electrode and a brass mesh (an alloy including copper and zinc in a weight ratio of 65:35) is used as the counter electrode.
[0052] In such an electrochemical deposition system, for example, when a voltage of 1.5 V or higher, or 1.5 V to 3.0 V, is applied and electrochemical deposition is performed for 1 to 30 minutes, or 5 to 20 minutes, or 7 to 15 minutes, copper and zinc ions move from the counter electrode to the working electrode, and an intermetallic compound in which copper and zinc are combined is deposited on the conductive metal layer, thereby forming the lithium electrodeposition-inducing layer. In particular, by controlling the electrochemical deposition time, the life characteristics of the secondary battery can be further improved.
[0053] At this time, the electrolyte may include a copper precursor, a zinc precursor, and a pyrophosphate. As the copper precursor and the zinc precursor, for example, a copper salt and a sulfate such as copper sulfate or zinc sulfate may be used. In addition, the pyrophosphate may be an additive that induces electrical deposition, and a metal pyrophosphate, for example, a pyrophosphate of an alkali (earth) metal such as K2P2O7, may be used.
[0054] Additionally, in a specific example, the electrolyte may be an aqueous solution containing a metal pyrophosphate at a concentration of 70 to 800 mM, or 80 to 300 mM, or 90 to 200 mM, a copper precursor at a concentration of 10 to 50 mM, or 20 to 40 mM, and a zinc precursor at a concentration of 10 to 50 mM, or 20 to 40 mM. In such an electrolyte, by controlling the concentration of the copper precursor and / or the zinc precursor, the chemical composition of the intermetallic compound of copper and zinc included in the lithium electrodeposition-inducing layer, for example, the bonding ratio of copper and zinc, can be controlled.
[0055] In addition, by controlling the concentration of the metal pyrophosphate in the electrolyte, the shape of the lithium electrodeposition-inducing layer can be controlled. For example, by controlling the concentration of the metal pyrophosphate to 80 to 300 mM, the lithium electrodeposition-inducing layer can be formed in the form of a thin film, so that the negative electrode of the lithium-free secondary battery can be formed to have a thinner and higher energy density and other electrochemical characteristics. In contrast, when the concentration of the metal pyrophosphate becomes excessively high or the applied voltage of the electrodeposition step becomes excessively high, the intermetallic compound included in the lithium electrodeposition-inducing layer is formed in a branched microstructure, which may be undesirable in terms of the life characteristics of the lithium-free secondary battery or the uniform electrodeposition of the lithium metal layer during charge and discharge.
[0056] Meanwhile, the manufacturing method of the other embodiment described above may further include, prior to the electrical deposition step, performing a surface treatment of the conductive metal layer with a sulfuric acid solution or the like to remove oxides on the surface of the conductive metal layer. This allows for a better formation of a lithium electrodeposition induction layer and further reduction of the resistance of the negative electrode of one embodiment.
[0057] In addition, the negative electrode manufacturing method of the other embodiment may further include, after the electrical deposition step, a step of heat-treating the electrical deposition material at a temperature of 200°C or higher, or from 200 to 600°C, or from 200 to 400°C, under a vacuum and / or inert gas atmosphere. As the heat treatment progresses, the chemical composition of the lithium electrodeposition-inducing layer changes, while micro-defects are removed, so that the lithium electrodeposition-inducing layer can become more uniform and dense, and a better lithium electrodeposition-inducing layer can be formed.
[0058] Meanwhile, according to a further embodiment of the invention, a lithium-free secondary battery comprising the negative electrode of the above-described embodiment is provided. Such a lithium-free secondary battery may include, for example, the negative electrode of the above-described embodiment; a positive electrode facing the negative electrode and comprising a positive electrode active material; and a separator or electrolyte layer interposed between the positive electrode and the negative electrode. In addition, the lithium-free secondary battery may further comprise, together with the separator, an electrolyte comprising a lithium salt and a non-aqueous organic solvent.
[0059] In such lithium-free secondary batteries, the negative electrode does not include a separate negative electrode active material layer before charging and discharging. However, as the lithium-free secondary battery is charged and discharged, lithium ions moved from the positive electrode may be deposited on the lithium electrodeposition inducing layer of the negative electrode, for example, a thin film of the intermetallic compound combining copper and zinc, thereby forming a lithium metal layer or a lithium alloy layer, and such a lithium metal layer or lithium alloy layer may function as a negative electrode active material.
[0060] In addition, a solid electrolyte interphase may be additionally formed on the lithium electrodeposition induction layer of the negative electrode by the reaction between lithium ions and electrolytes during initial charge and discharge. This solid electrolyte interphase may include, for example, lithium fluoride, and may suppress additional side reactions with the electrolyte.
[0061] Meanwhile, in the lithium-free secondary battery of the above additional embodiment, the positive electrode may include a positive electrode current collector and a positive electrode active material layer positioned on the positive electrode current collector.
[0062] These positive electrodes can be manufactured by mixing an active material and a binder, and in some cases, a conductive material, a filler, etc. in a solvent to prepare a positive electrode slurry composition, and applying the composition to a positive electrode current collector.
[0063] The positive electrode current collector may generally have a thickness of 3 to 500 μm. In addition, the positive electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. The current collector may also form fine unevenness on its surface to increase the adhesive strength of the positive electrode active material, and various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric are possible.
[0064] And, in the case of the above positive electrode active material, it may include a compound capable of reversible intercalation and deintercalation of lithium, specifically a lithium metal oxide containing one or more metals such as iron, cobalt, manganese, nickel, or aluminum and lithium.
[0065] Specifically, the lithium metal oxide is a lithium-manganese oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt oxide (e.g., LiCoO2, etc.), a lithium-nickel oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese oxide (e.g., LiNi 1-Y Mn Y O2 (here, 0 <Y<1), LiMn 2-Z Ni Z O4 (where 0<Z<2), etc.), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y1 Co Y1 O2 (here, 0 <Y1<1) 등), 리튬-망간-코발트계 산화물(예를 들면, LiCo 1-Y2 Mn Y2 O2 (here, 0 <Y2<1), LiMn 2-Z1 Co Z1 O4 (wherein, 0<Z1<2) etc.), lithium-nickel-manganese-cobalt oxides (e.g., Li(Ni p Co q Mn r )O2(wherein, 0<p<1, 0<q<1, 0<r<1, p+q+r=1) or Li(Ni p1 Co q1 Mn r1 )O4 (wherein, 0<p1<2, 0<q1<2, 0<r1<2, p1+q1+r1=2) etc.), lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r2 M s2 )O2 (wherein, M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r2 and s2 are atomic fractions of independent elements, respectively, 0<p2<1, 0<q2<1, 0<r2<1, 0<s2<1, p2+q2+r2+s2=1), etc.), or lithium iron phosphate (e.g., Li 1+a Fe 1-x M x (PO 4-b )X b(Here, M is at least one selected from Al, Mg, and Ti, X is at least one selected from F, S, and N, -0.5≤a≤+0.5, 0≤x≤0.5, 0≤b≤0.1), and any one or two or more compounds thereof may be included.
[0066] Among these, the positive electrode active material includes a lithium metal oxide including lithium and two or more metals selected from the group consisting of nickel, manganese, cobalt, and aluminum, and the lithium metal oxide may include nickel in an amount of 50 mol% or more, or 60 to 99 mol%, or 70 to 95 mol%, based on the total metal content excluding lithium. Such a lithium metal oxide may be represented by, for example, the following chemical formula 1:
[0067] [Chemical Formula 1]
[0068] Li x Ni a Co b M 1 c M 2 d O2
[0069] In the above chemical formula 1, the M 1 Mn and Al may be one or more selected from or a combination thereof, and M 2 may be at least one selected from the group consisting of Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S, and may be 0.90≤x≤1.1, or 0.95≤x≤1.08, or 1.0≤x≤1.08, and may be 0.50≤a<1.0, or 0.60≤a≤0.99, or 0.70≤a≤0.95. In addition, 0 <b≤0.3이고, 0<c≤0.3이고, 0≤d≤0.1일 수 있다.
[0070] By using a lithium metal oxide containing such a high nickel content as a positive electrode active material and combining it with an anode of one embodiment, the output and capacity characteristics, as well as the life characteristics, of a lithium-free secondary battery can be further improved.
[0071] The above-described positive electrode active material may be included in an amount of 60 to 99 wt%, or 70 to 99 wt%, or 80 to 98 wt% based on the total weight of the positive electrode active material layer.
[0072] Meanwhile, the conductive material included in the positive electrode active material layer is a component for further improving the conductivity of the positive electrode active material. The conductive material is not particularly limited as long as it has conductivity without causing chemical changes in the battery. For example, carbon powder such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive nanomaterials such as carbon nanofibers or carbon nanotubes; fluorinated carbon powder; conductive powder such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. can be used. Among these, the conductive material can further lower the resistance of a lithium-free secondary battery and improve output characteristics, etc. by including a conductive nanomaterial such as carbon nanotubes or carbon nanofibers.
[0073] Typically, the conductive material may be included in an amount of 1 to 20 wt%, or 1 to 15 wt%, or 1 to 10 wt% based on the total weight of the positive electrode active material layer.
[0074] The binder optionally included in the above-described positive electrode active material layer is a component that assists in the bonding of the positive electrode active material and the conductive material, and in the bonding to the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, nitrile rubber, styrene-butadiene rubber, or fluororubber, and a mixture or copolymer of two or more selected from these may also be used.
[0075] Typically, the binder may be included in an amount of 1 to 20 wt%, or 1 to 15 wt%, or 1 to 10 wt% based on the total weight of the positive electrode active material layer.
[0076] Additionally, a filler may be optionally added to the positive electrode as a component that suppresses its expansion. Such filler is not particularly limited as long as it can suppress the expansion of the electrode without causing chemical changes in the battery. Examples of fillers that can be used include olefin polymers such as polyethylene and polypropylene; fibrous materials such as glass fiber and carbon fiber; and the like.
[0077] The above-described positive electrode can be manufactured by dispersing and mixing the positive electrode active material, binder, and conductive agent in a dispersion medium (solvent) to make a slurry, applying the slurry on a metal current collector, and then drying and rolling. At this time, the dispersion medium may be NMP (N-methyl-2-pyrrolidone), DMF (Dimethyl formamide), DMSO (Dimethyl sulfoxide), ethanol, isopropanol, water, and mixtures thereof, but is not necessarily limited thereto.
[0078] Meanwhile, the lithium-free secondary battery of the other embodiment may further include an electrolyte including a non-aqueous organic solvent and a lithium salt.
[0079] The lithium salt included in the above electrolyte is used as a medium for transferring ions within a secondary battery. Lithium salt is, for example, Li as a cation. + Including, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO2 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - and SCN -It may include an anion selected from the group consisting of .
[0080] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (Lithium bis(fluorosulfonyl) imide, LiN(SO2F)2), LiBF2(C2O4), LiBETI (lithium bis(perfluoroethanesulfonyl) imide, LiN(SO2CF2CF3)2) and LiTFSI (lithium bis(trifluoromethanesulfonyl) imide, LiN(SO2CF3)2).
[0081] The concentration of the above lithium salt can be appropriately changed within a commonly usable range, and can be included in the electrolyte at a concentration of 0.4 M to 6 M, or a concentration of 0.5 M to 5 M.
[0082] In a more specific embodiment, the electrolyte may contain a lithium salt at a relatively low concentration of 0.4 M or more and less than 2 M, or 0.5 M to 1.5 M, but may also contain the lithium salt at a high concentration of 2 M to 6 M, or 2.5 M to 5.5 M. By using an electrolyte containing such a high concentration of lithium salt, the output characteristics of the secondary battery can be further improved.
[0083] Meanwhile, the type of non-aqueous organic solvent that can be included in the electrolyte is not particularly limited, and any organic solvent that has been previously known to be applicable to electrolytes of lithium ion batteries, etc., can be used. Examples of such organic solvents include at least one selected from the group consisting of carbonate solvents, ether solvents, nitrile solvents, phosphate solvents, and sulfone solvents. However, considering the stability of the lithium metal layer electrodeposited on the lithium electrodeposition induction layer, etc., it is preferable that the non-aqueous organic solvent include a carbonate solvent or an ether solvent.
[0084] More specifically, as the carbonate solvent, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, methyl propyl carbonate, ethyl methyl carbonate, ethyl propyl carbonate or methyl (2,2,2-trifluoroethyl) carbonate can be used, and as the phosphate solvent, trimethyl phosphate, triethyl phosphate or 2-(2,2,2-trifluoroethoxy)-1,3,2-dioxaphosphorane 2-oxide can be used.
[0085] In addition, as the ether solvent, dibutyl ether, tetraglyme, diglyme, dimethoxy ethane, or tetrahydrofuran derivatives such as 2-methyl tetrahydrofuran can be used, and as the nitrile solvent, succinonitrile, adiponitrile, sebaconitrile, acetonitrile, or propionitrile can be used. In addition, as the sulfone solvent, dimethyl sulfone, ethylmethyl sulfone, or sulforane can be used.
[0086] Meanwhile, the lithium-free secondary battery described above may further include a porous separator interposed between the positive electrode and the negative electrode.
[0087] These porous membranes can be made of olefin polymers such as polyethylene and polypropylene, glass fibers, etc. in the form of sheets, multi-membranes, microporous films, woven fabrics, and non-woven fabrics, but are not necessarily limited thereto. However, it may be preferable to use porous polyethylene or porous glass fiber non-woven fabric (glass filter) as the membrane, and it may be more preferable to use porous glass filter (glass fiber non-woven fabric) as the membrane. The membrane may be an insulating thin film having high ion permeability and mechanical strength, and the pore diameter of the membrane may generally be in the range of 0.01 to 10 ㎛, and the thickness may generally be in the range of 5 to 300 ㎛, but is not limited thereto.
[0088] In addition, in another example of the lithium-free secondary battery, the separator may be integrated with the electrolyte and interposed between the positive and negative electrodes in the form of an electrolyte layer or electrolyte film. In one example, the electrolyte layer or electrolyte film may be in the form of a polymer matrix containing the lithium salt and a non-aqueous organic solvent described above, or in the form of a solid electrolyte. In addition, a well-known polymer-based solid electrolyte, etc. may be used as the polymer matrix.
[0089] The lithium-free secondary battery of the above-described embodiment can be a semi-solid battery using a liquid electrolyte and a solid electrolyte in combination or an all-solid battery having a solid electrolyte layer, depending on whether the electrolyte layer is included and its shape, etc.
[0090] Meanwhile, the lithium-free secondary battery of the above-described other embodiment can be manufactured according to a conventional method in the art. For example, the electrode assembly including the positive electrode, negative electrode, and separator can be housed in a case, and manufactured by a method of injecting and impregnating the electrolyte described above, or the electrode assembly including the positive electrode, negative electrode, and electrolyte layer can be housed in a case, and manufactured.
[0091] These lithium-free secondary batteries can be applied to battery cells used as power sources for small devices, and are particularly suitable for use as unit cells in battery modules that serve as power sources for medium- to large-sized devices.
[0092]
[0093] Below, preferred embodiments of the invention, comparative examples to compare with them, and experimental examples for evaluating them are described. However, the following examples are merely preferred embodiments of the invention, and the present invention is not limited to the following examples.
[0094]
[0095] Comparative Examples 1 and 2, Examples 1 and 2: Preparation of a negative electrode for a lithium-free secondary battery
[0096] First, copper foil itself was used as the cathode of Comparative Example 1. In addition, the cathodes of Comparative Example 2 and Examples 1 and 2 were manufactured using the following method. An electrolyte for electrodeposition was manufactured by dissolving pyrophosphate (K2P2O7), copper sulfate, and zinc sulfate in DI water solvent at concentrations (mM) shown in Table 1 below.
[0097] Meanwhile, an electrodeposition system as shown in Fig. 1 was prepared. This electrodeposition system included a working electrode made of copper foil and a counter electrode made of brass mesh (an alloy mesh containing Cu:Zn=65:35 in a weight ratio), and each electrode was used after having its surface oxide removed by being previously immersed in a 1 M sulfuric acid aqueous solution for about 30 minutes.
[0098] The working electrode of acid-treated copper foil and the counter electrode of brass mesh were fixed to the electrodeposition jig and then connected to the (-) and (+) poles of the power source, respectively. The electrodeposition jig, to which both the working electrode and the counter electrode were connected, was placed vertically in a tank containing the above-described electrodeposition electrolyte, and the electrodeposition process was performed for 10 minutes under constant voltage (2.0 V) conditions, thereby forming a lithium electrodeposition-inducing layer including an intermetallic compound combining copper and zinc on the copper foil.
[0099] After the electrodeposition process, the copper foil on which the lithium electrodeposition induction layer was formed was separated from the electrodeposition jig and then washed with DI water to remove all electrolyte residues used in the electrodeposition process. Through the above process, negative electrodes for lithium-free secondary batteries of Comparative Example 2 and Examples 1 and 2 were manufactured, respectively.
[0100] Electrodeposition electrolyte concentration Electrodeposition applied voltage (V) Electrodeposition time (min) Intermetallic compound composition (wt%) Intermetallic compound composition formula K2P2O7 (mM) Copper sulfate (mM) Zinc sulfate (mM) Copper Zinc Comparative example 1---2.0101000CuExample 110040102.0107327Cu7Zn3Example 210010402.0102773Cu3Zn7Comparative example 21000502.0100100Zn
[0101] The cathode surfaces formed in Comparative Example 2, Examples 1 and 2 were analyzed using an electron microscope and are shown in Figures 2a to 2c, respectively. Through this, it was confirmed that the lithium electrodeposition-inducing layer including the intermetallic compound was formed well in Examples 1 and 2.
[0102]
[0103] Examples 3 to 5: Preparation of negative electrode for lithium-free secondary battery
[0104] The cathode sample manufactured in Example 2 was placed in a vacuum furnace (-0.1 MPa) and then heat-treated under an Ar gas atmosphere with a flow rate of 5 (SLPM) at each temperature listed in Table 2 below. The heat-treatment process time was set as TS (time to reach the target temperature listed in Table 2 below) = 1 hr, and Tm (maintenance time under the target temperature listed in Table 2 below) = 2 hr.
[0105] Through this additional heat treatment, the negative electrodes of Examples 3 to 5 were manufactured. The compositional changes of the intermetallic compounds included in the lithium electrodeposition induction layer in the negative electrodes of Examples 3 to 5 were confirmed and summarized in Table 2 below. In addition, the film quality changes of the lithium electrodeposition induction layer before and after the treatment in Example 5 were analyzed using an electron microscope and are shown in Fig. 3.
[0106] Heat treatment temperature (℃)Composition of intermetallic compound before heat treatment (wt%)Composition of intermetallic compound after heat treatment (wt%)Guri-Ria-Ria-Yu-San-OxygenExample 3200277375223Example 4250277381163Example 5300277388102
[0107] Referring to Table 2 and Figure 3 above, it was confirmed that the composition of the intermetallic compound included in the lithium electrodeposition induction layer changed through the heat treatment, and it was also confirmed that the micro-defects included in the lithium electrodeposition induction layer were removed and the film quality became more dense.
[0108]
[0109] Test Example 1: Overvoltage Evaluation
[0110] Half cells were manufactured using the negative electrodes of Comparative Example 1 and Example 2. These half cells included lithium foil as the negative electrode and counter electrode, and 75 μl of an electrolyte of 0.6 M LiBF4 + 0.6 M LiBF2(C2O4) in FEC / DEC (1:2 volume ratio). For these half cells, 0.5 mAh cm -2 Lithium with a capacity of 10μA·cm -2When electrodepositing, the lithium electrodeposition overvoltage applied to each negative electrode was evaluated, and the evaluation results are shown in Fig. 4. Referring to Fig. 4, it was confirmed that a lower lithium electrodeposition overvoltage was applied when lithium electrodeposition was performed using the negative electrode of Example 2. Through this, it was confirmed that uniform lithium deposition was induced on the lithium electrodeposition induction layer included in the negative electrode of the example.
[0111]
[0112] Test Example 2: Battery Life Characteristics Evaluation
[0113] In the same manner as in the above Test Example 2, half-cells including the negative electrodes of Comparative Examples 1 and 2 and Examples 1 and 2 were prepared. For these half-cells, 1 mAh·cm -2 @ 0.5mA·cm -2 A stable charge-discharge cycle was evaluated through a galvanic charge-discharge test while charging and discharging under the conditions of (0.5 C, cut-off voltage: 1 V). The results of each evaluation are shown in comparison in Fig. 5.
[0114] Referring to FIG. 5, it was confirmed that stable charging and discharging were performed over a longer cycle in the secondary battery including the negative electrode of the embodiment, and in particular, it was confirmed that stable charging and discharging were performed over the longest cycle in the secondary battery including the negative electrode of Example 2.
Claims
1. Conductive metal layer; and A negative electrode for a lithium-free secondary battery, comprising a lithium electrodeposition inducing layer formed on the conductive metal layer and including an intermetallic compound composed of copper and zinc.
2. A negative electrode for a lithium-free secondary battery, wherein the conductive metal layer comprises copper.
3. A negative electrode for a lithium-free secondary battery, wherein the lithium electrodeposition induction layer comprises an intermetallic compound in which copper:zinc are combined in a weight ratio of 2:8 to 9.5:0.
5.
4. In the first paragraph, the lithium electrodeposition induction layer is a negative electrode for a lithium-free secondary battery comprising an intermetallic compound in which copper and zinc are combined in a weight ratio of 3:7 to 9:1 and oxygen is contained in an amount of 0.01 to 5 wt% based on the weight of the entire intermetallic compound.
5. A negative electrode for a lithium-free secondary battery, wherein the lithium electrodeposition induction layer in the first paragraph has a thickness of 0.05 to 2 μm.
6. A method for manufacturing a negative electrode for a lithium-free secondary battery of claim 1, comprising a step of electrically depositing copper and zinc on a conductive metal layer using an electrolyte containing a copper precursor, a zinc precursor, and pyrophosphate.
7. A method for manufacturing a negative electrode for a lithium-free secondary battery, wherein the electrical deposition step is performed by applying voltage to an electrical deposition system including a working electrode including the conductive metal layer; a counter electrode including an alloy of copper and zinc; and the electrolyte.
8. A method for manufacturing a negative electrode for a lithium-free secondary battery, wherein the electrolyte is an aqueous solution containing a metal pyrophosphate at a concentration of 70 to 800 mM, a copper precursor at a concentration of 10 to 50 mM, and a zinc precursor at a concentration of 10 to 50 mM in the 6th paragraph.
9. A method for manufacturing a negative electrode for a lithium-free secondary battery, further comprising, after the electrical deposition step, a step of heat-treating the electrical deposition material at a temperature of 200°C or higher under a vacuum or inert gas atmosphere.
10. A cathode containing a cathode active material; The cathode of paragraph 1; and A lithium-free secondary battery comprising a separator or electrolyte layer interposed between the positive and negative electrodes.
11. A lithium-free secondary battery further comprising a lithium metal layer deposited on the lithium electrodeposition induction layer of the negative electrode by charging the lithium-free secondary battery in the 10th paragraph.
Citation Information
Patent Citations
Preparation method of negative current collector capable of improving cycling stability of metal lithium
CN114400331A
Porous three dimensional copper, tin, copper-tin, copper-tin-cobalt, and copper-tin-cobalt-titanium electrodes for batteries and ultra capacitors
KR1020110122177A
Unmanned mobile assistant robots for geospatial surveys
KR1020240036290A
Pogo pin
KR102659686B1
KR20220082710A