Perovskite solar cell and method for producing same

The introduction of a three-layer electron transport buffer layer in perovskite solar cells addresses charge recombination and growth issues, enhancing performance and stability by preventing hole movement and improving electron transfer, thereby increasing the fill factor and stability of the solar cells.

WO2024232720A1PCT designated stage expired Publication Date: 2024-11-14HANWHA SOLUTIONS CORP

Patent Information

Application Number
PCT/KR2024/006358
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-05-10
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Perovskite solar cells face performance reduction and instability due to charge recombination at the electron transport layer interface and non-uniform growth of ultra-thin films, which affects reproducibility and stability.

Method used

A three-layer electron transport buffer layer is introduced between the perovskite light absorption layer and the electron transport layer, comprising a passivation buffer layer, a carbon-based electron transport layer, and a hole blocking buffer layer, to prevent hole movement and enhance selective electron transfer.

Benefits of technology

This configuration improves the fill factor and performance of perovskite solar cells by reducing shunts and increasing shunt resistance, while ensuring stability and uniformity of the thin film interface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006358_14112024_PF_FP_ABST
    Figure KR2024006358_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a perovskite solar cell in which an electron transport buffer layer having a three-layer structure is introduced between a perovskite light-absorption layer and an electron transport layer, and a method for producing same. The electron transport buffer layer having a three-layer structure has a structure in which a passivation buffer layer, a carbon-based electron transport layer, and a hole blocking buffer layer are sequentially laminated, and prevents the movement of holes to the electron transport layer and improves the selective transport of electrons, thereby minimizing performance degradation of the perovskite solar cell and ensuring stability.
Need to check novelty before this filing date? Find Prior Art

Description

Perovskite solar cell and method for manufacturing the same

[0001] The present invention relates to a perovskite solar cell in which a three-layer electron transport buffer layer is introduced between a perovskite light-absorbing layer and an electron transport layer, and a method for manufacturing the same.

[0002]

[0003] To address the depletion of fossil fuels and the global environmental problems caused by their use, research is actively being conducted on renewable and clean alternative energy sources such as solar energy, wind power, and hydropower.

[0004] Among these, interest in solar cells, which directly convert sunlight into electrical energy, is growing significantly. Here, a solar cell refers to a cell that generates current and voltage by utilizing the photovoltaic effect, which generates electrons and holes by absorbing light energy from sunlight.

[0005] Currently, it is possible to manufacture np diode-type silicon (Si) single crystal-based solar cells with a light energy conversion efficiency of over 20%, and these are actually being used for solar power generation. There are also solar cells using compound semiconductors such as gallium arsenide (GaAs) with even better conversion efficiencies. However, these inorganic semiconductor-based solar cells require highly purified materials to achieve high efficiency, so a lot of energy is consumed in refining the raw materials. In addition, expensive processing equipment is required in the process of forming single crystals or thin films using the raw materials, which limits the cost of lowering the manufacturing cost of solar cells, and this has been an obstacle to large-scale utilization.

[0006] Accordingly, in order to manufacture solar cells at low cost, it is necessary to drastically reduce the cost of materials or manufacturing processes used as core components of solar cells, and research is being conducted on perovskite solar cells that can be manufactured using low-cost materials and processes as an alternative to inorganic semiconductor-based solar cells.

[0007] Recently, perovskite solar cells using (NH3CH3)PbX3 (X=I, Br, Cl), a halogen compound with a perovskite structure, as a photoactive agent have been developed, and research is being conducted toward commercialization. The general structural formula of the perovskite structure is the ABX3 structure, where anions are located in the X position, large cations are located in the A position, and small cations are located in the B position.

[0008] Meanwhile, perovskite solar cells are being developed in the structure of PIN perovskite single solar cells or two-terminal perovskite / silicon tandem solar cells. In the case of two-terminal perovskite / silicon tandem solar cells, a recombination layer is formed on glass and a lower silicon solar cell, and then the upper perovskite solar cell layers, which are a hole transport layer, a perovskite light-absorbing layer, an electron transport layer, and a transparent electrode, are sequentially formed to manufacture a two-terminal perovskite / silicon tandem solar cell. At this time, electrons and holes separated from the perovskite light-absorbing layer are transferred to the electron transport layer and the hole transport layer, respectively.

[0009] Holes separated from the perovskite light-absorbing layer are not only transported to the underlying hole transport layer, but also to the upper electron transport layer. However, due to energy level mismatch, charge recombination occurs at the electron transport layer interface, potentially reducing solar cell performance.

[0010] In addition, when forming an electron transport layer, there is a problem that it is difficult to form a uniform ultra-thin film because the atomic layer does not grow uniformly in the initial nuclear growth stage, which not only reduces the performance of the solar cell, but also reduces the reproducibility and stability of the solar cell due to the instability of the thin film formation caused by the decrease in interface uniformity.

[0011]

[0012] The present invention has been devised to overcome the above-described problem, and provides a perovskite solar cell and a method for manufacturing the same, which introduces a three-layer electron transport buffer layer between a perovskite light-absorbing layer and an electron transport layer to prevent movement of holes to the electron transport layer, improve selective transport of electrons, and thereby minimize performance degradation of the perovskite solar cell and secure stability.

[0013]

[0014] In order to solve the above-described problem, the perovskite solar cell of the present invention includes a laminate in which a hole transport layer, a perovskite light-absorbing layer, an electron transport layer, a transparent electrode, and a metal electrode are sequentially laminated, and an electron transport buffer layer may be formed between the perovskite light-absorbing layer and the electron transport layer.

[0015] As a preferred embodiment of the present invention, the electron transfer buffer layer may include at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2).

[0016] As a preferred embodiment of the present invention, the electron transport buffer layer may have a structure in which a passivation buffer layer, a carbon-based electron transport layer, and a hole blocking buffer layer are sequentially laminated.

[0017] As a preferred embodiment of the present invention, the passivation buffer layer may be laminated on one surface of the perovskite light-absorbing layer, and the hole-blocking buffer layer may be laminated on one surface of the electron transport layer.

[0018] As a preferred embodiment of the present invention, the passivation buffer layer may include at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2).

[0019] As a preferred embodiment of the present invention, the hole blocking buffer layer may include at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2).

[0020] As a preferred embodiment of the present invention, the carbon-based electron transport layer may include a fullerene series organic material.

[0021] As a preferred embodiment of the present invention, the fullerene-based organic material is C 60 , C 70 , may include one or more selected from PC60BM and PC70BM.

[0022] As a preferred embodiment of the present invention, the carbon-based electron transport layer and the passivation buffer layer may have a thickness ratio of 1:0.01 to 0.2.

[0023] As a preferred embodiment of the present invention, the carbon-based electron transport layer and the hole blocking buffer layer may have a thickness ratio of 1:0.01 to 0.2.

[0024] As a preferred embodiment of the present invention, the passivation buffer layer may have an average thickness of 0.5 to 5 nm.

[0025] As a preferred embodiment of the present invention, the hole blocking buffer layer may have an average thickness of 0.5 to 5 nm.

[0026] As a preferred embodiment of the present invention, the carbon-based electron transport layer may have an average thickness of 3 to 30 nm.

[0027] As a preferred embodiment of the present invention, the electron transport layer and the electron transport buffer layer may have a thickness ratio of 1:1.1 to 2.4.

[0028] As a preferred embodiment of the present invention, the electron transport layer may have an average thickness of 3 to 30 nm.

[0029] As a preferred embodiment of the present invention, the perovskite solar cell of the present invention may be a pin structure type perovskite solar cell, a nip inverse structure type perovskite solar cell, a tandem type perovskite solar cell, or a tandem type silicon / perovskite heterojunction solar cell.

[0030] Meanwhile, the method for manufacturing a perovskite solar cell of the present invention includes a first step of forming a perovskite light-absorbing layer on a hole transport layer, a second step of forming an electron transport buffer layer on the perovskite light-absorbing layer through a deposition process or a solution process, and a third step of sequentially forming an electron transport layer, a transparent electrode, and a metal electrode on the electron transport buffer layer, wherein the electron transport buffer layer may include at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2).

[0031] As a preferred embodiment of the present invention, the second step may include a step 2-1 of forming a passivation buffer layer on top of a perovskite light-absorbing layer through a deposition process or a solution process, a step 2-2 of forming a carbon-based electron transport layer on top of the passivation buffer layer through a deposition process or a solution process, and a step 2-3 of forming a hole-blocking buffer layer on top of the carbon-based electron transport layer through a deposition process or a solution process.

[0032] Furthermore, the tandem silicon / perovskite heterojunction solar cell of the present invention is a heterojunction solar cell in which a solar cell, a transparent conductive layer, a hole transport layer, a perovskite light-absorbing layer, an electron transport buffer layer, an electron transport layer, a transparent electrode, and a metal electrode are sequentially laminated, and the electron transport buffer layer may include at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2).

[0033] In a preferred embodiment of the present invention, the solar cell may be a polycrystalline silicon solar cell, a crystalline silicon solar cell, a perovskite solar cell, a gallium arsenide (GaAs) solar cell, a cadmium telluride (CdTe) solar cell, a CIGS (CuInGaSe) solar cell, a CZTS (Cu2ZnSnS4) solar cell, an organic solar cell, a fuel-sensitized solar cell, or a group 3-5 compound solar cell.

[0034]

[0035] The perovskite solar cell of the present invention can improve the performance of the solar cell by introducing a three-layer electron transport buffer layer between the perovskite light-absorbing layer and the electron transport layer, thereby forming a physical barrier to impart physical passivation characteristics, improving hole blocking characteristics to reduce the occurrence of shunts in the solar cell, and increasing the fill factor (FF) by increasing the shunt resistance.

[0036]

[0037] FIG. 1 is a cross-sectional view illustrating an electron transfer buffer layer according to a preferred embodiment of the present invention.

[0038] Figure 2 is a graph showing the current density according to the applied voltage for each of the tandem silicon / perovskite heterojunction solar cells manufactured in Examples 1 to 3.

[0039]

[0040] Hereinafter, the present invention will be described in more detail.

[0041] In conventional perovskite solar cells, holes separated from the perovskite light-absorbing layer do not simply travel to the lower hole transport layer, but also to the upper electron transport layer. This energy level mismatch causes charge recombination at the electron transport layer interface, potentially reducing solar cell performance.

[0042] In addition, when forming an electron transport layer, there is a problem that it is difficult to form a uniform ultra-thin film because the atomic layer does not grow uniformly in the initial nuclear growth stage, which not only reduces the performance of the solar cell, but also reduces the reproducibility and stability of the solar cell due to the instability of the thin film formation caused by the decrease in interface uniformity.

[0043] Accordingly, the present invention relates to a perovskite solar cell in which a three-layer electron transport buffer layer is introduced between a perovskite light-absorbing layer and an electron transport layer to prevent movement of holes to the electron transport layer, improve selective transport of electrons, and thereby minimize a decrease in performance of the perovskite solar cell and secure stability.

[0044] The perovskite solar cell of the present invention may be a pin structure type perovskite solar cell, a nip inverse structure type perovskite solar cell, a tandem perovskite solar cell, or a tandem silicon / perovskite heterojunction solar cell, and preferably may be a tandem silicon / perovskite heterojunction solar cell, and may be a solar cell including a laminate in which a hole transport layer (HTL, or hole transport layer), a perovskite light-absorbing layer, an electron transport layer (ETL), a transparent electrode, and a metal electrode are sequentially laminated.

[0045] Additionally, the perovskite solar cell of the present invention may have an electron transport buffer layer formed between the perovskite light-absorbing layer and the electron transport layer.

[0046] For example, in a preferred embodiment, when the perovskite solar cell of the present invention is a tandem silicon / perovskite heterojunction solar cell, it may be a heterojunction solar cell in which a solar cell, a transparent conductive layer, a hole transport layer, a perovskite light-absorbing layer, an electron transport buffer layer, an electron transport layer, a transparent electrode, and a metal electrode are sequentially laminated.

[0047]

[0048] The solar cell may be a polycrystalline silicon solar cell, a crystalline silicon solar cell, a perovskite solar cell, a gallium arsenide (GaAs) solar cell, a cadmium telluride (CdTe) solar cell, a CIGS (CuInGaSe) solar cell, a CZTS (Cu2ZnSnS4) solar cell, an organic solar cell, a fuel-sensitized solar cell, or a group III-V compound solar cell.

[0049] In addition, there is no separate limitation on the thickness of the solar cell, but it may preferably have a thickness of 140 to 250 μm, more preferably 160 to 200 μm.

[0050]

[0051] The transparent conductive layer is a layer that induces recombination of electrons and holes generated in a solar cell and a perovskite light-absorbing layer to be described later, and may be a transparent thin film on which ITO (Indium Tin Oxide), FTO (Fluorine doped Tin Oxide), ATO (Sb2O3 doped Tin Oxide), GTO (Gallium doped Tin Oxide), ZTO (tin doped zinc oxide), ZTO:Ga (gallium doped ZTO), IGZO (Indium gallium zinc oxide), IZO (Indium doped zinc oxide), or AZO (Aluminum doped zinc oxide) is deposited.

[0052] In addition, as an example of forming a transparent conductive layer, when using a silicon solar cell doped with n- or p-type impurities as a solar cell, the silicon solar cell doped with n- or p-type impurities is treated with hydrofluoric acid to remove the SiOx oxide film, and then the remaining hydrofluoric acid is removed using ultrapure water. Then, a transparent conductive layer can be formed on the top of the silicon solar cell from which the oxide film has been removed through a sputtering process.

[0053] In addition, the thickness of the transparent conductive layer is not particularly limited, but may preferably have a thickness of 5 nm to 50 nm, more preferably 15 nm to 25 nm.

[0054]

[0055] The hole transport layer (HTL) is a layer that transports holes formed in the perovskite light-absorbing layer described below while simultaneously blocking the movement of electrons, and may include an inorganic and / or organic hole transport material.

[0056] At this time, the inorganic hole transport material may include at least one selected from nickel oxide (NiOx), CuSCN, CuCrO2, CuI, MoO, and V2O5.

[0057] In addition, organic hole transport materials include carbazole derivatives, polyarylalkane derivatives, phenylenediamine derivatives, arylamine derivatives, amino-substituted chalcone derivatives, styrylanthracene derivatives, fluorene derivatives, hydrazone derivatives, stilbene derivatives, silazane derivatives, aromatic tertiary amine compounds, styrylamine compounds, aromatic dimethylidine compounds, porphyrin compounds, phthalocyanine compounds, polythiophene derivatives, polypyrrole derivatives, polyparaphenylenevinylene derivatives, pentacene, coumarin 6 (coumarin 6, 3-(2-benzothiazolyl)-7-(diethylamino)coumarin), ZnPC (zinc phthalocyanine), CuPC (copper phthalocyanine), TiOPC (titanium oxide phthalocyanine), Spiro-MeOTAD(2,2',7,7'-tetrakis(N,Np-dimethoxyphenylamino)-9,9'-spirobifluorene), F16CuPC(copper(II) 1,2,3,4,8,9,10,11,15,16,17,18,22,23,24,25-hexadecafluoro-29H,31H-phthalocyanine), SubPc (boron subphthalocyanine chloride) and N3(cis-di(thiocyanato)-bis(2,2'-bipyridyl-4,4'-dicarboxylic acid)-ruthenium(II), P3HT(poly[3-hexylthiophene]), MDMO-PPV(poly[2-methoxy-5-(3',7'-dimethyloctyloxyl)]-1,4-phenylene vinylene), MEH-PPV(poly[2-methoxy-5-(2''-ethylhexyloxy)-p-phenylene vinylene]), P3OT(poly(3-octyl thiophene)), POT(poly(octyl thiophene)), P3DT(poly(3-decyl thiophene)),P3DDT(poly(3-dodecyl thiophene), PPV(poly(p-phenylene vinylene)), TFB(poly(9,9'-dioctylfluorene-co-N-(4-butylphenyl)diphenyl amine), 폴리아닐린(Polyaniline), Spiro-MeOTAD([2,22′,7,77′-tetrkis (N,N-di-pmethoxyphenyl amine)-9,9,9′-spirobi fluorine]), PCPDTBT(Poly[2,1,3-benzothiadiazole-4,7-diyl[4,4-bis(2-ethylhexyl-4H-cyclopenta [2,1-b:3,4-b']dithiophene-2,6-diyl]], Si-PCPDTBT(poly[(4,4′-bis(2-ethylhexyl)dithieno[3,2-b:2′,3′-d]silole)-2,6-diyl-alt-(2,1,3-benzothiadiazole)-4,7-diyl]), PBDTTPD(poly((4,8-diethylhexyloxyl), PFDTBT(poly[2,7-(9-(2-ethylhexyl)-9-hexyl-fluorene)-alt-5,5-(4', 7, -di-2-thienyl-2',1', 3'-benzothiadiazole)]), PFO-DBT(poly[2,7-.9,9-(dioctyl-fluorene)-alt-5,5-(4',7'-di-2-.thienyl-2', 1', 3'-benzothiadiazole)]), PSiFDTBT(poly[(2,7-dioctylsilafluorene)-2,7-diyl-alt-(4,7-bis(2-thienyl)-2,1,3-benzothiadiazole)-5,5′-diyl]), PCDTBT(Poly [[9-(1-octylnonyl)-9H-carbazole-2,7-diyl] -2,5-thiophenediyl-2,1,3-benzothiadiazole-4,7-diyl-2,5-thiophenediyl]), PFB(poly(9,It may include at least one selected from among 9′-dioctylfluorene-co-bis(N,N′-(4,butylphenyl))bis(N,N′-phenyl-1,4-phenylene)diamine), F8BT(poly(9,9′-dioctylfluorene-cobenzothiadiazole), PEDOT (poly(3,4-ethylenedioxythiophene)), PEDOT:PSS poly(3,4-ethylenedioxythiophene) poly(styrenesulfonate), PTAA (poly(triarylamine)), 2-PACz, MeO-2PACz, Br-2PACz, Me-4PACz, MeO-4PACz and 6-PACz.

[0058] In addition, methods for forming a hole transport layer include a coating method and a vacuum deposition method, and methods for applying the hole transport layer include a gravure coating method, a bar coating method, a printing method, a spray method, a spin coating method, a dip method, and a die coat method.

[0059] In addition, the thickness of the hole transport layer is not particularly limited, but may preferably have a thickness of 5 nm to 40 nm, more preferably 10 nm to 30 nm.

[0060]

[0061] The perovskite light-absorbing layer may include a general perovskite material applied to a light-absorbing layer of a solar cell, and as a preferred example, may include a perovskite material represented by the following chemical formula 1.

[0062] [Chemical Formula 1]

[0063] CMX3

[0064] In the above chemical formula 1, C is a monovalent cation, which may include amine, ammonium, a group 1 metal, a group 2 metal, and / or other cations or cation-like compounds, preferably formamidinium (FA), methylammonium (MA), FAMA, CsFAMA, CsFA or N(R)4. + (Here, R may be the same or different groups, and R may be a straight-chain alkyl group having 1 to 5 carbon atoms, a branched alkyl group having 3 to 5 carbon atoms, a phenyl group, an alkylphenyl group, an alkoxyphenyl group, or an alkyl halide.)

[0065] In addition, M in chemical formula 1 is a divalent cation and may include one or two selected from Fe, Co, Ni, Cu, Sn, Pb, Bi, Ge, Ti, Eu, and Zr.

[0066] In addition, X in chemical formula 1 is a monovalent anion and may include one or more halide elements and / or Group 16 anions selected from F, Cl, Br and I, and a preferred example is I x Br 3-x (0 ≤ x ≤ 3) may be.

[0067] And, as a preferred embodiment of chemical formula 1, FAPbI x Br 3-x (0 ≤ x ≤ 3), MAPbI x Br 3-x (0 ≤ x ≤ 3), CSFAPbI x Br 3-x (0 ≤ x ≤ 3), CSMAFAPbI x Br 3-x (0 ≤ x ≤ 3), CH3NH3PbX3 (X= Cl, Br, I, BrI2, or Br2I), CH3NH3SnX3 (X= Cl, Br, or I), CH(=NH)NH3PbX3 (X= Cl, Br, I, BrI2, or Br2I), or CH(=NH)NH3SnX3 (X= Cl, Br, or I).

[0068] Meanwhile, in the perovskite solar cell of the present invention, the perovskite light-absorbing layer may be a single layer composed of the same perovskite material, or may be a multilayer structure in which multiple layers composed of different perovskite materials are laminated, and may include a heterogeneous perovskite material other than the one type of perovskite material having a pillar shape such as a columnar shape, a plate shape, a needle shape, a wire shape, or a rod shape inside the light-absorbing layer composed of one type of perovskite material.

[0069] In addition, methods for forming a perovskite light-absorbing layer include a coating method and a vacuum deposition method, and methods for applying the layer include a gravure coating method, a bar coating method, a printing method, a spray method, a spin coating method, a dip method, an inkjet coating method, and a die coat method.

[0070]

[0071] Referring to Fig. 1, the electron transfer buffer layer (10) can be formed on top of the perovskite light-absorbing layer through a deposition process or a solution process.

[0072] At this time, deposition can be performed using a typical deposition process used in the art, and preferably, a vacuum deposition process can be performed. Additionally, the solution process can be performed using a spin coating process.

[0073] In addition, the electron transfer buffer layer (10) may include at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2), and preferably may include lithium fluoride (LiF).

[0074] Specifically, the electron transport buffer layer (10) may have a structure in which a passivation buffer layer (3), a carbon-based electron transport layer (2), and a hole blocking buffer layer (1) are sequentially laminated. In this case, the passivation buffer layer (3) may be laminated on one surface of the perovskite light-absorbing layer, and the hole blocking buffer layer (1) may be laminated on one surface of the electron transport layer.

[0075] The passivation buffer layer (3) is a layer included in the perovskite solar cell of the present invention and serves as a passivation layer, and may include at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2), and preferably may include lithium fluoride (LiF).

[0076] In addition, the passivation buffer layer (3) may have an average thickness of 0.5 to 5 nm, preferably an average thickness of 0.5 to 1.5 nm. If the average thickness is less than 0.5 nm, there may be a problem of energy mismatch due to loss of passivation characteristics, and if it exceeds 5 nm, there may be a problem of loss of charge transfer capability due to insulation characteristics.

[0077] The carbon-based electron transport layer (2) may include a fullerene-based organic material. In this case, the fullerene-based organic material is C 60 , C 70 , may include at least one selected from PC60BM and PC70BM, preferably C 60 second May include.

[0078] In addition, the carbon-based electron transport layer (2) may have an average thickness of 3 to 30 nm, preferably an average thickness of 5 to 20 nm, and more preferably an average thickness of 11 to 15 nm. If the average thickness is less than 3 nm, there may be a problem of reduced charge transfer capability due to failure to form uniformly on the rough surface of the perovskite light-absorbing layer, and if it exceeds 30 nm, there may be a problem of reduced characteristics of the solar cell due to absorption of light that should be absorbed by the perovskite light-absorbing layer, thereby hindering the light-receiving characteristics of the perovskite light-absorbing layer.

[0079] The hole blocking buffer layer (1) is a layer that is included in the perovskite solar cell of the present invention and plays a hole blocking role, and may include at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2), and preferably may include lithium fluoride (LiF).

[0080] In addition, the hole blocking buffer layer (1) may have an average thickness of 0.5 to 5 nm, preferably an average thickness of 0.5 to 1.5 nm. If the average thickness is less than 0.5 nm, it may hinder improvement of energy matching, and it may hinder uniform growth of atomic layers in the initial nucleation stage during formation of the electron transport layer, making it difficult to form a uniform ultra-thin film. If it exceeds 5 nm, there may be a problem of reduced charge transfer characteristics due to insulating characteristics.

[0081] Meanwhile, the carbon-based electron transport layer (2) and the passivation buffer layer (3) may have a thickness ratio of 1:0.01 to 0.2, preferably 1:0.05 to 0.08.

[0082] Additionally, the carbon-based electron transport layer (2) and the hole blocking buffer layer (1) may have a thickness ratio of 1:0.01 to 0.2, preferably 1:0.05 to 0.08.

[0083]

[0084] The electron transporting layer (ETL) is a layer that transports electrons formed in the perovskite light-absorbing layer while simultaneously blocking the movement of holes, and may include at least one selected from tin oxide (SnOx), nickel oxide (NiOx), tin oxide (SnO2), titanium dioxide (TiO2), zinc oxide (ZnO), barium tin oxide (BaSnO3), niobium hydroxide (NbOH), and niobium pentoxide (Nb2O5).

[0085] In addition, methods for forming the electron transport layer include a coating method, an ALD deposition method, and / or a vacuum deposition method, and methods for applying the electron transport layer include a gravure coating method, a bar coating method, a printing method, a spray method, a spin coating method, a dip method, and a die coat method.

[0086] In addition, the thickness of the electron transport layer is not particularly limited, but may preferably have an average thickness of 3 to 30 nm, more preferably 3 to 15 nm, and even more preferably 10 to 13 nm. At this time, the electron transport layer and the electron transport buffer layer may have a thickness ratio of 1:1.1 to 2.4, and preferably 1:1.36 to 2.04.

[0087]

[0088] A transparent electrode can be formed on top of the electron transport layer through a deposition process. The deposition process can be performed using a typical deposition process used in the art, and preferably, a sputtering process can be used.

[0089] In addition, the transparent electrode may be a transparent thin film on which ITO (Indium Tin Oxide), FTO (Fluorine doped Tin Oxide), ATO (Sb2O3 doped Tin Oxide), GTO (Gallium doped Tin Oxide), ZTO (tin doped zinc oxide), ZTO:Ga (gallium doped ZTO), IGZO (Indium gallium zinc oxide), IZO (Indium doped zinc oxide), or AZO (Aluminum doped zinc oxide) is deposited.

[0090] In addition, the thickness of the transparent electrode has no separate limitation, but may preferably have a thickness of 50 to 200 nm, more preferably 60 to 140 nm.

[0091]

[0092] A metal electrode can be formed by patterning a metal material on top of a transparent electrode. Specifically, the patterning process is largely composed of deposition, exposure (lithography), and etching. A metal electrode can be formed on top of a transparent electrode by spreading a metal material in the form of a thin film on one surface of a substrate, printing a pattern by exposure, and then removing unnecessary portions. In addition, the patterning process can also be performed through a screen printing method using a metal paste containing a metal material.

[0093] At this time, the metal material may include at least one selected from Pt, Au, Ni, Cu, Ag, In, Ru, Pd, Rh, Ir, Os, C, and a conductive polymer.

[0094] Additionally, there is no separate limitation on the thickness of the metal electrode, but it may preferably have a thickness of 50 nm to 2.5 μm.

[0095]

[0096] Meanwhile, the method for manufacturing a perovskite solar cell of the present invention may include a first step of forming a perovskite light-absorbing layer on top of a hole transport layer, a second step of forming an electron transport buffer layer on top of the perovskite light-absorbing layer through a deposition process or a solution process, and a third step of sequentially forming an electron transport layer, a transparent electrode, and a metal electrode on top of the electron transport buffer layer.

[0097] At this time, the electron transport buffer layer may have a structure in which a passivation buffer layer (3), a carbon-based electron transport layer (2), and a hole blocking buffer layer (1) are sequentially laminated.

[0098] Specifically, the second step of the method for manufacturing a perovskite solar cell of the present invention may include a step 2-1 of forming a passivation buffer layer on top of a perovskite light-absorbing layer through a deposition process or a solution process, a step 2-2 of forming a carbon-based electron transport layer on top of the passivation buffer layer through a deposition process or a solution process, and a step 2-3 of forming a hole-blocking buffer layer on top of the carbon-based electron transport layer through a deposition process or a solution process.

[0099] More specifically, the passivation buffer layer can be formed through a vacuum deposition process, the carbon-based electron transport layer can be formed through a vacuum deposition process, and the hole blocking buffer layer can be formed through a vacuum deposition process.

[0100]

[0101] Hereinafter, the present invention will be described in more detail through examples, but the following examples do not limit the scope of the present invention, and should be interpreted as helping to understand the present invention.

[0102]

[0103] Example 1: Fabrication of a tandem silicon / perovskite heterojunction solar cell

[0104] (1) A silicon solar cell (thickness: 180 ㎛) doped with n or p type impurities was prepared, and the SiOx oxide film was removed by hydrofluoric acid treatment. Then, the remaining hydrofluoric acid was removed using ultrapure water. A 20 nm thick transparent conductive layer (ITO) was formed on the top of the silicon solar cell from which the oxide film was removed through a sputtering process.

[0105] (2) Next, a 20 nm thick hole transport layer (NiOx) was formed on top of the transparent conductive layer through sputter vacuum deposition.

[0106] (3) Next, a yellow light-absorbing layer solution dissolved in dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) was formed on top of the hole transport layer by spin coating, and a perovskite light-absorbing layer (CSFAPbI) having a perovskite crystal structure with a thickness of 300 nm was formed by heat-treating at 125°C for 20 minutes. x Br 3-X (0 ≤ x ≤ 3)) was formed.

[0107] (4) Next, lithium fluoride (LiF) was deposited on top of the perovskite light-absorbing layer through a vacuum deposition process to form a passivation buffer layer with an average thickness of 1 nm.

[0108] (5) Next, C is deposited on top of the passivation buffer layer through a vacuum deposition process. 60 Fullerene (C 60 A carbon-based electron transport layer with an average thickness of 15 nm was formed by depositing fullerene.

[0109] (6) Next, lithium fluoride (LiF) was deposited on top of the carbon-based electron transport layer through a vacuum deposition process to form a hole blocking buffer layer with an average thickness of 1 nm.

[0110] (7) Next, an electron transport layer (SnO2) with an average thickness of 10 nm was formed on top of the hole blocking buffer layer through an ALD (atomic layer deposition) deposition process.

[0111] (8) Next, a 75 nm thick transparent electrode (ITO) was formed on top of the electron transport layer through a sputtering process.

[0112] (9) Finally, 1×10 silver (Ag) is added to the top of the transparent electrode. -7 A tandem silicon / perovskite heterojunction solar cell was fabricated in the form of a silicon solar cell, a transparent conductive layer, a hole transport layer, a perovskite light-absorbing layer, a passivation buffer layer, a carbon-based electron transport layer, a hole blocking buffer layer, an electron transport layer, a transparent electrode, and a metal electrode sequentially stacked by depositing the metal electrode to a thickness of 100 nm at a pressure of 10 torr.

[0113]

[0114] Example 2: Fabrication of a tandem silicon / perovskite heterojunction solar cell

[0115] (1) A silicon solar cell (thickness: 180 ㎛) doped with n or p type impurities was prepared, and the SiOx oxide film was removed by hydrofluoric acid treatment. Then, the remaining hydrofluoric acid was removed using ultrapure water. A 20 nm thick transparent conductive layer (ITO) was formed on the top of the silicon solar cell from which the oxide film was removed through a sputtering process.

[0116] (2) Next, a 20 nm thick hole transport layer (NiOx) was formed on top of the transparent conductive layer through sputter vacuum deposition.

[0117] (3) Next, a yellow light-absorbing layer solution dissolved in dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) was formed on top of the hole transport layer by spin coating, and a perovskite light-absorbing layer (CSFAPbI) having a perovskite crystal structure with a thickness of 300 nm was formed by heat-treating at 125°C for 20 minutes. x Br 3-X (0 ≤ x ≤ 3)) was formed.

[0118] (4) Next, lithium fluoride (LiF) was deposited on top of the perovskite light-absorbing layer through a vacuum deposition process to form a passivation buffer layer with an average thickness of 1 nm.

[0119] (5) Next, C is deposited on top of the passivation buffer layer through a vacuum deposition process. 60 Fullerene (C 60 A carbon-based electron transport layer with an average thickness of 15 nm was formed by depositing fullerene.

[0120] (6) Next, an electron transport layer (SnO2) with an average thickness of 10 nm was formed on top of the carbon-based electron transport layer through an ALD (atomic layer deposition) deposition process.

[0121] (7) Next, a 75 nm thick transparent electrode (ITO) was formed on top of the electron transport layer through a sputtering process.

[0122] (8) Finally, 1×10 silver (Ag) is added to the top of the transparent electrode. -7 A tandem silicon / perovskite heterojunction solar cell was fabricated in the form of a silicon solar cell, a transparent conductive layer, a hole transport layer, a perovskite light-absorbing layer, a passivation buffer layer, a carbon-based electron transport layer, an electron transport layer, a transparent electrode, and a metal electrode sequentially stacked by depositing the metal electrode to a thickness of 100 nm at a pressure of 10 torr.

[0123]

[0124] Example 3: Fabrication of a tandem silicon / perovskite heterojunction solar cell

[0125] (1) A silicon solar cell (thickness: 180 ㎛) doped with n or p type impurities was prepared, and the SiOx oxide film was removed by hydrofluoric acid treatment. Then, the remaining hydrofluoric acid was removed using ultrapure water. A 20 nm thick transparent conductive layer (ITO) was formed on the top of the silicon solar cell from which the oxide film was removed through a sputtering process.

[0126] (2) Next, a 20 nm thick hole transport layer (NiOx) was formed on top of the transparent conductive layer through sputter vacuum deposition.

[0127] (3) Next, a yellow light-absorbing layer solution dissolved in dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) was formed on top of the hole transport layer by spin coating, and a perovskite light-absorbing layer (CSFAPbI) having a perovskite crystal structure with a thickness of 300 nm was formed by heat-treating at 100°C for 20 minutes. x Br 3-X (0 ≤ x ≤ 3)) was formed.

[0128] (4) Next, a passivation buffer layer with an average thickness of 10 nm was formed by coating PCBM on top of the perovskite light-absorbing layer through a solution process.

[0129] (5) Next, C is deposited on top of the passivation buffer layer through a vacuum deposition process. 60 Fullerene (C 60 A carbon-based electron transport layer with an average thickness of 15 nm was formed by depositing fullerene.

[0130] (6) Next, an electron transport layer (SnO2) with an average thickness of 10 nm was formed on top of the hole blocking buffer layer through an ALD (atomic layer deposition) deposition process.

[0131] (7) Next, a 75 nm thick transparent electrode (ITO) was formed on top of the electron transport layer through a sputtering process.

[0132] (8) Finally, 1×10 silver (Ag) is added to the top of the transparent electrode. -7 A tandem silicon / perovskite heterojunction solar cell was fabricated in the form of a silicon solar cell, a transparent conductive layer, a hole transport layer, a perovskite light-absorbing layer, a passivation buffer layer, a carbon-based electron transport layer, a hole blocking buffer layer, an electron transport layer, a transparent electrode, and a metal electrode sequentially stacked by depositing the metal electrode to a thickness of 100 nm at a pressure of 10 torr.

[0133]

[0134] Experimental Example 1: Measuring Solar Cell Performance

[0135] Figure 2 is a graph showing the current density according to the applied voltage for each of the tandem silicon / perovskite heterojunction solar cells manufactured in Examples 1 to 3, measured using an LED Lamp-based JV measurement method.

[0136] As can be confirmed through the left graph of Fig. 2, the tandem silicon / perovskite heterojunction solar cell manufactured in Example 1, which has a structure in which a passivation buffer layer, a carbon-based electron transport layer, a hole blocking buffer layer, and an electron transport layer are sequentially laminated, physically blocks holes moving to the electron transport layer, thereby enhancing the hole blocking characteristic, and only electrons are selectively transported, thereby minimizing charge recombination at the interface, thereby suppressing shunt and inducing an improvement in fill factor. In addition, it was confirmed that the hole blocking buffer layer in the form of an ultra-thin film enables the formation of a dense thin film, thereby suppressing molecules that cause charge loss and facilitating charge capture, thereby increasing the short-circuit current density.

[0137] In addition, as can be confirmed through the right graph of Fig. 2, it was confirmed that the tandem silicon / perovskite heterojunction solar cell manufactured in Example 1 using lithium fluoride (LiF) as a passivation buffer layer improved energy matching, thereby improving the open circuit voltage, and improved the short-circuit current density by inducing only the passivation effect, compared to the tandem silicon / perovskite heterojunction solar cell manufactured in Example 3 using PCBM as a passivation buffer layer.

[0138] In addition, for each of the tandem silicon / perovskite heterojunction solar cells manufactured in Examples 1 to 3, the efficiency was measured using a solar simulation device and a JV Keithley device, and the initial JV curve was used, and the results are shown in Table 1 below.

[0139]

[0140] As can be seen in Table 1 above, it was confirmed that the tandem silicon / perovskite heterojunction solar cell manufactured in Example 1 had the best open circuit voltage, short-circuit current density, fill factor, and power conversion efficiency values.

[0141]

[0142] Experimental Example 2: Analysis of Surface Chemical Properties of the Electron Transport Layer

[0143] The surface chemical properties of the electron transport layer of each of the tandem silicon / perovskite heterojunction solar cells manufactured in Examples 1 and 2 were analyzed using XPS photoelectron spectroscopy, and are shown in Table 2 below.

[0144]

[0145] As can be seen in Table 2 above, the tandem silicon / perovskite heterojunction solar cell manufactured in Example 1 had a decreased work function (WF) and an increased valence band maximum (VBM) compared to the tandem silicon / perovskite heterojunction solar cell manufactured in Example 2, confirming its advantage in charge transfer. In addition, the tandem silicon / perovskite heterojunction solar cell manufactured in Example 1 had an increased O / Sn ratio and a decreased N / Sn ratio compared to the tandem silicon / perovskite heterojunction solar cell manufactured in Example 2, confirming that a film with fewer surface defects in the electron transport layer and a stoichiometrically stable film was formed.

[0146]

[0147] In conclusion, it was confirmed that the tandem silicon / perovskite heterojunction solar cell manufactured in Example 1 was capable of increasing the open circuit voltage through energy agreement matching and increasing the short-circuit current density and fill factor through enhanced surface properties.

[0148]

[0149] The above illustrates and describes specific embodiments. However, the invention is not limited to the aforementioned embodiments, and those skilled in the art will readily appreciate that various modifications and implementations can be made without departing from the spirit and scope of the invention as set forth in the claims below.

Claims

1. A laminate comprising a hole transport layer, a perovskite light-absorbing layer, an electron transport layer, a transparent electrode, and a metal electrode sequentially laminated, An electron transport buffer layer is formed between the perovskite light absorbing layer and the electron transport layer, A perovskite solar cell characterized in that the electron transfer buffer layer comprises at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2).

2. In paragraph 1, The above electron transport buffer layer has a structure in which a passivation buffer layer, a carbon-based electron transport layer, and a hole blocking buffer layer are sequentially laminated. A perovskite solar cell characterized in that the passivation buffer layer is laminated on one surface of the perovskite light-absorbing layer, and the hole blocking buffer layer is laminated on one surface of the electron transport layer.

3. In paragraph 2, Each of the above passivation buffer layer and the hole blocking buffer layer includes at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2). A perovskite solar cell characterized in that the carbon-based electron transport layer comprises a fullerene series organic material.

4. In paragraph 3, The above fullerene series organic material is C 60 , C 70 A perovskite solar cell characterized by comprising at least one selected from among PC60BM and PC70BM.

5. In paragraph 2, The above carbon-based electron transport layer and passivation buffer layer have a thickness ratio of 1:0.01 to 0.2, A perovskite solar cell characterized in that the carbon-based electron transport layer and hole blocking buffer layer have a thickness ratio of 1:0.01 to 0.

2.

6. In paragraph 2, Each of the above passivation buffer layer and hole blocking buffer layer has an average thickness of 0.5 to 5 nm, A perovskite solar cell characterized in that the carbon-based electron transport layer has an average thickness of 3 to 30 nm.

7. In paragraph 1, A perovskite solar cell characterized in that the electron transport layer and the electron transport buffer layer have a thickness ratio of 1:1.1 to 2.

4.

8. In paragraph 1, A perovskite solar cell characterized in that the electron transport layer has an average thickness of 3 to 30 nm.

9. In any one of the clauses 1 to 8 selected, A perovskite solar cell characterized in that the above perovskite solar cell is a pin structure type perovskite solar cell, a nip inverse structure type perovskite solar cell, a tandem type perovskite solar cell, or a tandem type silicon / perovskite heterojunction solar cell.

10. The first step is to form a perovskite light-absorbing layer on top of the hole transport layer; A second step of forming an electron transfer buffer layer on top of the perovskite light-absorbing layer through a deposition process or a solution process; and A third step of sequentially forming an electron transport layer, a transparent electrode, and a metal electrode on top of the electron transport buffer layer; A method for manufacturing a perovskite solar cell, characterized in that the electron transfer buffer layer comprises at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2).

11. In paragraph 10, the second step Step 2-1 of forming a passivation buffer layer on top of the perovskite light-absorbing layer through a deposition process or solution process; Step 2-2 of forming a carbon-based electron transport layer on top of the passivation buffer layer through a deposition process or a solution process; and Step 2-3 of forming a hole blocking buffer layer on top of the carbon-based electron transport layer through a deposition process or solution process; A method for manufacturing a perovskite solar cell, characterized in that it includes:

12. A heterojunction solar cell in which a solar cell, a transparent conductive layer, a hole transport layer, a perovskite light-absorbing layer, an electron transport buffer layer, an electron transport layer, a transparent electrode, and a metal electrode are sequentially laminated, A tandem silicon / perovskite heterojunction solar cell characterized in that the electron transfer buffer layer comprises at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2).

13. In paragraph 12, The above electron transport buffer layer has a structure in which a passivation buffer layer, a carbon-based electron transport layer, and a hole blocking buffer layer are sequentially laminated. A tandem silicon / perovskite heterojunction solar cell, characterized in that the passivation buffer layer is laminated on one surface of the perovskite light-absorbing layer, and the hole blocking buffer layer is laminated on one surface of the electron transport layer.

14. In paragraph 13, Each of the above passivation buffer layer and the hole blocking buffer layer includes at least one selected from lithium fluoride (LiF), magnesium fluoride (MgF2), cesium fluoride (CsF), sodium fluoride (NaF), potassium fluoride (KF), aluminum fluoride (AlF3), aluminum oxide (Al2O3), and calcium fluoride (CaF2). A tandem silicon / perovskite heterojunction solar cell characterized in that the carbon-based electron transport layer comprises a fullerene series organic material.

15. In paragraph 12, A tandem silicon / perovskite heterojunction solar cell characterized in that the solar cell is a polycrystalline silicon solar cell, a crystalline silicon solar cell, a perovskite solar cell, a gallium arsenide (GaAs) solar cell, a cadmium telluride (CdTe) solar cell, a CIGS (CuInGaSe) solar cell, a CZTS (Cu2ZnSnS4) solar cell, an organic solar cell, a fuel-sensitized solar cell, or a group 3-5 compound solar cell.

Citation Information

Patent Citations

  • Solar cell passivation structure and preparation method

    CN115881832A

  • Passivating barrier layers in contact with perovskites for solar cells

    JP2019521531A

  • Perovskite compound and light conversion element using the same

    JP7213557B2

  • Bird nest prevention system using luminous element driven by induction electromotive force

    KR1020200092809A

  • Lathe-type computer system

    KR102205036B1

Cited By

  • Perovskite battery based on composite interface modification engineering and preparation method thereof

    CN121419459A

  • Perovskite solar cell based on composite interface modification engineering and preparation method thereof