Solar cell and preparation method therefor

By using a multi-layer structure of molybdenum oxide and tungsten oxide in undoped heterojunction solar cells, combined with hot wire chemical vapor deposition method and annealing treatment, the problems of low open circuit voltage and reduced filling factor are solved, and efficient space Cavit selective transmission and battery performance improvement.

WO2024234845A1PCT designated stage expired Publication Date: 2024-11-21TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/084896
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-03-29
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The open circuit voltage of undoped heterojunction solar cells is low, and increasing the hole-selective transport layer thickness to increase the voltage will reduce the filling factor.

Method used

The first hole-selective transport layer of molybdenum oxide is prepared on the silicon wafer, and a second hole-selective transport layer of tungsten oxide is provided thereon. The oxygen content and deposition rate are controlled by the hot wire chemical vapor deposition method to ensure oxidation The oxygen in tungsten can be transferred to molybdenum oxide, thereby increasing the oxygen content and work function of molybdenum oxide and avoiding increasing the thickness of the hole-selective transport layer.

Benefits of technology

The open circuit voltage of the solar cell is increased, the filling factor is maintained, and oxygen transfer and damage repair are promoted through annealing treatment, which enhances the thermal stability and hole selective transmission effect of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024084896_21112024_PF_FP_ABST
    Figure CN2024084896_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present invention is a preparation method for a solar cell. The preparation method comprises the following steps: providing a silicon wafer (10), and preparing an electron selective transport layer (20) on one surface of the silicon wafer (10); preparing a first hole selective transport layer (30) on the other surface of the silicon wafer (10), wherein the material of the first hole selective transport layer (30) is molybdenum oxide; and preparing a second hole selective transport layer (40) on the first hole selective transport layer (30), wherein the material of the second hole selective transport layer (40) is tungsten oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Solar cell and preparation method thereof

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 16, 2023, with application number 202310552107.6 and invention name “Solar Cell and Its Preparation Method”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present invention relates to the technical field of solar cells, and in particular to a solar cell and a preparation method thereof. Background Art

[0003] Undoped heterojunction solar cells can effectively mitigate the severe optical parasitic absorption losses and carrier recombination found in the amorphous silicon layer of traditional heterojunction solar cells, effectively increasing short-circuit current density. Undoped heterojunction solar cells primarily consist of a silicon wafer, a hole-selective transport layer, and a transparent conductive layer, positioned sequentially on top of the wafer. The hole-selective transport layer is made of a transition metal oxide.

[0004] The open-circuit voltage of undoped heterojunction solar cells is primarily determined by the work function and thickness of the transition metal oxide. The work function of the transition metal oxide is significantly affected by its oxygen content: a higher oxygen content indicates a higher work function, and vice versa. The transition metal oxide spontaneously undergoes a redox reaction with the silicon wafer, forming silicon oxide, which lowers the work function of the transition metal oxide and, consequently, reduces the transition metal oxide's selective transport of holes, resulting in a lower open-circuit voltage in undoped heterojunction solar cells. To achieve this selective hole transport, the thickness of the transition metal oxide must be increased, but this in turn reduces the fill factor of the undoped heterojunction solar cell.

[0005] Summary of the Invention

[0006] Based on this, it is necessary to provide a method for preparing a solar cell that can improve the open circuit voltage and fill factor.

[0007] In addition, it is necessary to provide a solar cell.

[0008] At least one embodiment of the present invention provides a method for preparing a solar cell, comprising the following steps:

[0009] Providing a silicon wafer, and preparing an electron selective transport layer on one surface of the silicon wafer;

[0010] Preparing a first hole selective transport layer on the other surface of the silicon wafer, wherein the material of the first hole selective transport layer is molybdenum oxide;

[0011] forming a second hole selective transport layer on the first hole selective transport layer, wherein the material of the second hole selective transport layer is tungsten oxide;

[0012] preparing a front electrode on the second hole selective transport layer; and

[0013] A back electrode is prepared on the electron selective transport layer.

[0014] In some embodiments, after preparing the back electrode, the preparation method further includes the following steps:

[0015] The first hole selective transport layer and the second hole selective transport layer are annealed.

[0016] In some embodiments, the preparation method includes at least one of the following (1) to (2):

[0017] (1) The annealing temperature is 120°C to 150°C;

[0018] (2) The annealing treatment time is 30 minutes to 60 minutes.

[0019] In some embodiments, the second hole selective transport layer is prepared by hot-wire chemical vapor deposition.

[0020] In some embodiments, the preparation method includes at least one of the following (3) to (7):

[0021] (3) In the hot wire chemical vapor deposition method, the oxygen content in the reaction atmosphere in the reaction chamber is ≤6.7%, and the oxygen content in the reaction atmosphere in the reaction chamber is ≥1.7%;

[0022] (4) In the hot filament chemical vapor deposition method, the distance between the filament and the first hole selective transport layer is 80 mm to 100 mm;

[0023] (5) In the hot filament chemical vapor deposition method, the current passing through the filament is 30A to 60A;

[0024] (6) In the hot wire chemical vapor deposition method, the deposition pressure of the second hole selective transport layer is 2 Pa to 6 Pa;

[0025] (7) In the hot wire chemical vapor deposition method, the deposition rate of the second hole selective transport layer is

[0026] In some embodiments, the first hole selective transport layer is prepared by thermal evaporation.

[0027] In some embodiments, in the thermal evaporation method, the deposition rate of the first hole selective transport layer is

[0028] In some embodiments, after preparing the second hole selective transport layer and before preparing the front electrode, the preparation method further includes the following steps:

[0029] A first transparent conductive layer is prepared on the second hole selective transport layer by using a magnetron sputtering method.

[0030] At least one embodiment of the present invention provides a solar cell prepared using the above-mentioned preparation method, comprising the silicon wafer, the first hole selective transport layer, the second hole selective transport layer and the front electrode stacked in sequence on one surface of the silicon wafer, and the electron selective transport layer and the back electrode stacked in sequence on the other surface of the silicon wafer.

[0031] In some embodiments, the solar cell further comprises a first transparent conductive layer between the second hole selective transport layer and the front electrode, and the difference between the work function of the second hole selective transport layer and the work function of the first transparent conductive layer is less than or equal to 0.5 eV.

[0032] The present invention forms a first hole-selective transport layer made of molybdenum oxide on the silicon wafer, and forms a second hole-selective transport layer made of tungsten oxide on the first hole-selective transport layer. Oxygen in the second hole-selective transport layer can be transferred to the first hole-selective transport layer, thereby increasing the oxygen content of the first hole-selective transport layer, restoring and improving the work function of the first hole-selective transport layer, ensuring the selective transport of holes by the first hole-selective transport layer, and thereby improving the open-circuit voltage of the solar cell. Furthermore, because the present invention does not require increasing the thickness of the existing hole-selective transport layer, it can avoid reducing the fill factor of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] FIG1 is a flow chart of the preparation of a solar cell provided by the present invention;

[0034] FIG2 is a schematic structural diagram of a solar cell provided by the present invention;

[0035] FIG3 is a SEM image of an undoped heterojunction solar cell prepared in Example 1 of the present invention;

[0036] FIG4 is a graph showing the relationship between short-circuit current and open-circuit voltage of the undoped heterojunction solar cells prepared in Example 1 and Comparative Examples 1 and 2 of the present invention;

[0037] FIG5 is a diagram of minority carrier lifetimes of the undoped heterojunction solar cells prepared in Example 1 of the present invention and Comparative Examples 1-2.

[0038] Figure numerals: 100 - solar cell; 10 - silicon wafer; 11 - first intrinsic hydrogenated amorphous silicon layer; 12 - second intrinsic hydrogenated amorphous silicon layer; 20 - electron selective transport layer; 30 - first hole selective transport layer; 40 - second hole selective transport layer; 50 - first transparent conductive layer; 60 - second transparent conductive layer; 70 - front electrode; 80 - back electrode. DETAILED DESCRIPTION

[0039] To facilitate understanding of the present invention, the present invention will be described more fully below with reference to the accompanying drawings. Preferred embodiments of the present invention are shown in the accompanying drawings. However, the present invention may be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the present disclosure.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention pertains. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0041] Referring to FIG. 1 and FIG. 2 , the present invention provides a method for preparing a solar cell, comprising the following steps:

[0042] Step S11 , please refer to FIG. 1 , and provide a silicon wafer 10 .

[0043] In one embodiment, the silicon wafer 10 may be an N-type silicon wafer. Specifically, the N-type silicon wafer may be a textured N-type silicon wafer.

[0044] Step S12 , forming a first intrinsic hydrogenated amorphous silicon layer 11 on one surface of the silicon wafer 10 and forming a second intrinsic hydrogenated amorphous silicon layer 12 on the other surface of the silicon wafer 10 .

[0045] Specifically, a plasma enhanced chemical vapor deposition (PECVD) device is used to form the first intrinsic hydrogenated amorphous silicon layer 11 on one surface of the silicon wafer 10 and the second intrinsic hydrogenated amorphous silicon layer 12 on the other surface of the silicon wafer 10 .

[0046] Step S13 : forming an electron selective transport layer 20 on the second intrinsic hydrogenated amorphous silicon layer 12 .

[0047] Step S14 : forming a first hole selective transport layer 30 on the first intrinsic hydrogenated amorphous silicon layer 11 .

[0048] In one embodiment, the material of the first hole selective transport layer 30 is molybdenum oxide (MoO x ). The first hole selective transport layer 30 has high transmittance, high conductivity and high work function.

[0049] In one embodiment, the thickness of the first hole selective transport layer 30 is 3 nm to 5 nm.

[0050] In one embodiment, the preparation method of the first hole selective transport layer 30 is a thermal evaporation method. In the thermal evaporation method, the deposition rate of the first hole selective transport layer 30 is The deposition temperature of the first hole selective transport layer 30 is room temperature.

[0051] Among them, when preparing the first hole selective transport layer 30, the first hole selective transport layer 30 will undergo an oxidation-reduction reaction with the first intrinsic hydrogenated amorphous silicon layer 11 to generate a silicon oxide layer (not shown in the figure), thereby reducing the oxygen content of the first hole selective transport layer 30, reducing the work function of the first hole selective transport layer 30, affecting the selective transport of holes by the first hole selective transport layer 30, and further affecting the open circuit voltage of the subsequently prepared solar cell.

[0052] Step S15 , forming a second hole selective transport layer 40 on the first hole selective transport layer 30 .

[0053] In one embodiment, the material of the second hole selective transport layer 40 is tungsten oxide (WO x ). The second hole selective transport layer 40 has a high transmittance, a high conductivity and a high work function.

[0054] The selection of molybdenum oxide as the material for the first hole-selective transport layer 30 and tungsten oxide as the material for the second hole-selective transport layer 40 is based on Gibbs free energy calculations. Because molybdenum has a stronger binding affinity with oxygen atoms than tungsten, molybdenum can remove oxygen atoms from tungsten when oxygen is insufficient. Therefore, the second hole-selective transport layer 40, made of tungsten oxide, is disposed above the first hole-selective transport layer 30, made of molybdenum oxide. It should be noted that oxygen is not introduced into the first hole-selective transport layer 30 because oxygen would undergo a redox reaction with the first intrinsic hydrogenated amorphous silicon layer 11, generating excess silicon oxide.

[0055] The materials of the first hole-selective transport layer 30 and the second hole-selective transport layer 40 should have similar atomic radii to facilitate delamination and prevent mixing of the elements of the first hole-selective transport layer 30 and the second hole-selective transport layer 40, which would otherwise reduce the hole-selective transport effects of the first hole-selective transport layer 30 and the second hole-selective transport layer 40. Molybdenum and tungsten are elements of the same main group and have similar atomic radii of 139 pm.

[0056] In one embodiment, the thickness of the second hole selective transport layer 40 is 3 nm to 5 nm.

[0057] In one embodiment, the second hole selective transport layer 40 is prepared by hot-wire chemical vapor deposition.

[0058] When the second hole selective transport layer 40 is prepared by hot-wire chemical vapor deposition, the growth state of the second hole selective transport layer 40 can be controlled by adjusting the oxygen content in the reaction atmosphere in the reaction chamber.

[0059] In one embodiment, in the hot wire chemical vapor deposition method, the oxygen content in the reaction atmosphere in the reaction chamber is ≤6.7%, and the oxygen content in the reaction atmosphere in the reaction chamber is ≥1.7%. When the oxygen content in the reaction atmosphere in the reaction chamber is greater than 6.7%, the reaction between tungsten and oxygen is too fast, and although the generated WO x The proportion is high, but due to WO x The boiling point is much lower than that of tungsten, the sublimation speed is too fast, and the film preparation process is difficult to control, resulting in poor film quality of the second hole selective transport layer 40; when the oxygen content in the reaction atmosphere in the reaction chamber is less than 1.7%, the generated WO x The x in here is too low and difficult to control precisely.

[0060] Among them, the dense tungsten oxide is not conducive to the transfer of oxygen atoms therein to the first hole selective transport layer 30. Oxygen and tungsten undergo redox reaction to generate tungsten oxide, which then sublimates. During this process, the surface temperature of the filament is extremely high, usually above 1500°C. At this time, more oxygen will react with WO x The combined tungsten oxide vapor is almost the same as WO3 and is slowly deposited on the surface of the first hole selective transport layer 30. This loose film structure is conducive to the transfer of oxygen during annealing and also avoids excessive mixing of tungsten atoms into the first hole selective transport layer 30.

[0061] In addition, when using hot wire chemical vapor deposition to prepare the second hole selective transport layer 40, the work function of the second hole selective transport layer 40 can also be controlled by adjusting the oxygen content in the reaction atmosphere in the reaction chamber to avoid mismatching between the work function of the second hole selective transport layer 40 and the work function of the subsequently prepared first transparent conductive layer, and at the same time, oxidation of the silicon wafer 10 can also be avoided.

[0062] When the second hole selective transport layer 40 is formed using hot-filament chemical vapor deposition, the deposition rate of the second hole selective transport layer 40 can be controlled by adjusting the distance between the filament and the first hole selective transport layer 30. The greater the distance between the filament and the first hole selective transport layer 30, the slower the deposition rate of the second hole selective transport layer 40; and the closer the distance between the filament and the first hole selective transport layer 30, the faster the deposition rate of the second hole selective transport layer 40.

[0063] In addition, when the second hole selective transport layer 40 is prepared by hot filament chemical vapor deposition, the oxygen content in the second hole selective transport layer 40 can be controlled by adjusting the distance between the filament and the first hole selective transport layer 30. Since the temperature of the filament is extremely high, that is, the temperature of the filament is usually above 1500°C, W will react with O to form WO. x It will sublime, and in the reaction chamber, WO x Steam will continue to react with O, increasing WO x The oxygen content in. Among them, when the distance between the filament and the first hole selective transport layer 30 is far, x is closer to 3. Theoretically, the farther the distance is, the slower the deposition rate of the second hole selective transport layer 40 is, and the higher the oxygen content. Since oxygen is always introduced into the reaction chamber and a vacuum atmosphere is maintained, when the distance between the filament and the first hole selective transport layer 30 is too far, the second hole selective transport layer 40 is difficult to deposit uniformly. After a lot of debugging, it was found that when the distance between the filament and the first hole selective transport layer 30 is 80mm~100mm, the prepared second hole selective transport layer 40 is better, that is, the film-forming effect of the second hole selective transport layer 40 is better. At this time WO x In the film, x is approximately equal to 2.9, the deposition rate is slow, and the film quality is very good.

[0064] Among them, the filament will emit light and heat when working. Because the reaction chamber is kept in vacuum, the heat transfer is relatively small. According to sensor monitoring, the surface temperature of the sample is 70℃~80℃, and the light emitted by the filament can play the role of light injection, which is beneficial to improve the performance of the subsequently prepared solar cells.

[0065] It should be noted that the process for preparing the second hole selective transport layer 40 should be relatively gentle, and the growth rate of the second hole selective transport layer 40 should be controlled as slow as possible. Too fast a growth rate or too intense a preparation method (such as magnetron sputtering) is not feasible. In one embodiment, in the hot wire chemical vapor deposition method, the deposition rate of the second hole selective transport layer 40 is

[0066] In one embodiment, in the hot-filament chemical vapor deposition method, the current passing through the filament is 30 A to 60 A. In one embodiment, in the hot-filament chemical vapor deposition method, the deposition pressure of the second hole selective transport layer 40 is 2 Pa to 6 Pa.

[0067] Step S16 : preparing a first transparent conductive layer 50 on the second hole selective transport layer 40 .

[0068] Specifically, the first transparent conductive layer 50 is formed on the second hole selective transport layer 40 by using a magnetron sputtering method.

[0069] In one embodiment, the material of the first transparent conductive layer 50 includes indium zinc oxide (IZO). The work function of the second hole selective transport layer 40 cannot be too high and the difference between the work function of the first transparent conductive layer 50 and the first transparent conductive layer 50 should be within 0.5 eV to avoid a potential barrier to hole transport.

[0070] The second hole selective transport layer 40 can be used to protect the first hole selective transport layer 30 to reduce damage to the first hole selective transport layer 30 when the first transparent conductive layer 50 is prepared by magnetron sputtering.

[0071] Step S17 : preparing a second transparent conductive layer 60 on the electron selective transport layer 20 .

[0072] In one embodiment, the material of the second transparent conductive layer 60 includes indium zinc oxide (IZO).

[0073] Step S18 : preparing a front electrode 70 on the first transparent conductive layer 50 .

[0074] Specifically, the front electrode 70 is prepared on the first transparent conductive layer 50 by screen printing.

[0075] In one embodiment, the front electrode 70 may be a metal electrode. Specifically, the front electrode 70 may be a silver electrode.

[0076] Step S19 : preparing a back electrode 80 on the second transparent conductive layer 60 .

[0077] Specifically, the back electrode 80 is prepared on the second transparent conductive layer 60 by screen printing.

[0078] In one embodiment, the back electrode 80 may also be a metal electrode. Specifically, the back electrode 80 may also be a silver electrode.

[0079] Step S20 , annealing the first hole selective transport layer 30 and the second hole selective transport layer 40 to obtain the solar cell 100 .

[0080] Specifically, the first hole selective transport layer 30 and the second hole selective transport layer 40 are annealed under vacuum conditions to obtain the solar cell 100 .

[0081] In one embodiment, the temperature of the annealing treatment is 120° C. to 150° C. In one embodiment, the time of the annealing treatment is 30 min to 60 min.

[0082] Annealing the first hole selective transport layer 30 and the second hole selective transport layer 40 has the following advantages:

[0083] (1) Annealing the first hole-selective transport layer 30 and the second hole-selective transport layer 40 can promote the transfer of oxygen from the second hole-selective transport layer 40 to the first hole-selective transport layer 30, thereby increasing the oxygen content of the first hole-selective transport layer 30, restoring and improving the work function of the first hole-selective transport layer 30, ensuring the selective transport of holes by the first hole-selective transport layer 30, and thereby improving the open-circuit voltage of the prepared solar cell 100. In addition, the prepared solar cell 100 also has good thermal stability.

[0084] (2) Annealing the first hole selective transport layer 30 and the second hole selective transport layer 40 can also repair the damage to the first hole selective transport layer 30 caused by magnetron sputtering in step 16. Since step 16 inevitably damages the first hole selective transport layer 30 when preparing the first transparent conductive layer 50 by magnetron sputtering, such damage further reduces the selective transport of holes by the first hole selective transport layer 30. Annealing the first hole selective transport layer 30 and the second hole selective transport layer 40 in step S19 repairs the damage to the first hole selective transport layer 30, thereby improving the selective transport of holes by the first hole selective transport layer 30, thereby improving the open circuit voltage of the prepared solar cell 100.

[0085] (3) Annealing the first hole selective transport layer 30 and the second hole selective transport layer 40 can also optimize the contact between the front electrode 70 and the first transparent conductive layer 50 .

[0086] In one embodiment, the solar cell 100 may be an undoped heterojunction solar cell. In another embodiment, the solar cell 100 may also be any solar cell having an intrinsic hydrogenated amorphous silicon layer.

[0087] The fabrication method provided by the present invention first forms the first hole-selective transport layer 30 on the first intrinsic hydrogenated amorphous silicon layer 11, then forms the second hole-selective transport layer 40 on the first hole-selective transport layer 30. The first and second hole-selective transport layers 30 and 40 are then annealed to promote the transfer of oxygen from the second hole-selective transport layer 40 to the first hole-selective transport layer 30. This increases the oxygen content of the first hole-selective transport layer 30, restores and improves the work function of the first hole-selective transport layer 30, ensures the selective transport of holes by the first hole-selective transport layer 30, and thereby improves the open-circuit voltage of the fabricated solar cell 100. Furthermore, because the present invention does not require increasing the thickness of the existing hole-selective transport layer, it can avoid reducing the fill factor of the solar cell 100.

[0088] Referring again to FIG. 2 , at least one embodiment of the present invention provides a solar cell 100 fabricated using the aforementioned fabrication method. The solar cell 100 includes a silicon wafer 10; a first intrinsic hydrogenated amorphous silicon layer 11, a first hole selective transport layer 30, a second hole selective transport layer 40, a first transparent conductive layer 50, and a front electrode 70 sequentially stacked on one surface of the silicon wafer 10; and a second intrinsic hydrogenated amorphous silicon layer 12, an electron selective transport layer 20, a second transparent conductive layer 60, and a back electrode 80 sequentially stacked on the other surface of the silicon wafer 10.

[0089] In one embodiment, the silicon wafer 10 may be an N-type silicon wafer. Specifically, the N-type silicon wafer may be a textured N-type silicon wafer.

[0090] In one embodiment, the material of the electron selective transport layer 20 includes metal fluoride. In one embodiment, the metal fluoride includes at least one of lithium fluoride (LiF), rubidium fluoride (RbF), sodium fluoride (NaF), and magnesium fluoride (MgF2).

[0091] In one embodiment, the material of the first hole selective transport layer 30 is molybdenum oxide (MoO x). The first hole selective transport layer 30 has high transmittance, high conductivity and high work function.

[0092] In one embodiment, the thickness of the first hole selective transport layer 30 is 3 nm to 5 nm.

[0093] In one embodiment, a silicon oxide layer (not shown) is further provided between the first intrinsic hydrogenated amorphous silicon layer 11 and the first hole selective transport layer 30. The silicon oxide layer is a byproduct generated by the reaction between the first intrinsic hydrogenated amorphous silicon layer 11 and the first hole selective transport layer 30.

[0094] In one embodiment, the material of the second hole selective transport layer 40 is tungsten oxide (WO x ). The second hole selective transport layer 40 has a high transmittance, a high conductivity and a high work function.

[0095] Among them, the selection of molybdenum oxide as the material of the first hole selective transport layer 30 and the selection of tungsten oxide as the material of the second hole selective transport layer 40 are calculated based on Gibbs free energy. Since the binding ability of molybdenum element with oxygen atoms is stronger than that of tungsten element with oxygen atoms, under the condition of insufficient oxygen, molybdenum element can take oxygen atoms from tungsten element. Therefore, the second hole selective transport layer 40 made of tungsten oxide is arranged above the first hole selective transport layer 30 made of molybdenum oxide.

[0096] The materials of the first hole-selective transport layer 30 and the second hole-selective transport layer 40 should have similar atomic radii to facilitate delamination and prevent mixing of the elements of the first hole-selective transport layer 30 and the second hole-selective transport layer 40, which would otherwise reduce the hole-selective transport effects of the first hole-selective transport layer 30 and the second hole-selective transport layer 40. Molybdenum and tungsten are elements of the same main group and have similar atomic radii of 139 pm.

[0097] In one embodiment, the thickness of the second hole selective transport layer 40 is 3 nm to 5 nm.

[0098] In one embodiment, the material of the first transparent conductive layer 50 includes indium zinc oxide (IZO). The work function of the second hole selective transport layer 40 cannot be too high and the difference between the work function of the first transparent conductive layer 50 and the first transparent conductive layer 50 should be within 0.5 eV to avoid a potential barrier to hole transport.

[0099] In one embodiment, the material of the second transparent conductive layer 60 includes indium zinc oxide (IZO).

[0100] In one embodiment, the front electrode 70 may be a metal electrode. Specifically, the front electrode 70 may be a silver electrode.

[0101] In one embodiment, the back electrode 80 may also be a metal electrode. Specifically, the back electrode 80 may also be a silver electrode.

[0102] In one embodiment, the solar cell 100 may be an undoped heterojunction solar cell. In another embodiment, the solar cell 100 may also be any solar cell having an intrinsic hydrogenated amorphous silicon layer.

[0103] The solar cell 100 provided by the present invention includes a first hole-selective transport layer 30 and a second hole-selective transport layer 40. The first hole-selective transport layer 30 is made of molybdenum oxide, and the second hole-selective transport layer 40 is made of tungsten oxide. Oxygen in the second hole-selective transport layer 40 can be transferred to the first hole-selective transport layer 30, thereby increasing the oxygen content of the first hole-selective transport layer 30, restoring and improving the work function of the first hole-selective transport layer 30, ensuring the selective transport of holes by the first hole-selective transport layer 30, and thereby improving the open-circuit voltage of the solar cell 100. Furthermore, because the present invention does not require increasing the thickness of the existing hole-selective transport layer, it can avoid reducing the fill factor of the solar cell 100.

[0104] The present invention is further described below with reference to specific examples and comparative examples.

[0105] Example 1

[0106] (1) A textured N-type silicon wafer is provided, and a plasma enhanced chemical vapor deposition device is used to prepare a first intrinsic hydrogenated amorphous silicon layer on one surface of the silicon wafer and a second intrinsic hydrogenated amorphous silicon layer on the other surface of the silicon wafer.

[0107] (2) An electron selective transport layer is prepared on the second intrinsic hydrogenated amorphous silicon layer.

[0108] (3) A first hole selective transport layer is deposited on the first intrinsic hydrogenated amorphous silicon layer using a thermal evaporation device. The material of the first hole selective transport layer is molybdenum oxide, and the deposition rate of the first hole selective transport layer is The deposition temperature of the first hole selective transport layer is room temperature.

[0109] (4) A second hole selective transport layer is deposited on the first hole selective transport layer using a hot wire chemical vapor deposition method. The material of the second hole selective transport layer is tungsten oxide. In the hot wire chemical vapor deposition method, the current passing through the filament is 48A, the distance between the filament and the second hole selective transport layer is 80mm, the deposition temperature of the second hole selective transport layer is 70°C, the deposition pressure of the second hole selective transport layer is 5Pa, and the deposition rate of the second hole selective transport layer is

[0110] (5) A first transparent conductive layer is prepared on the second hole selective transport layer by magnetron sputtering, wherein the material of the first transparent conductive layer is indium zinc oxide.

[0111] (6) Preparing a second transparent conductive layer on the electron selective transport layer, wherein the material of the second transparent conductive layer is indium zinc oxide.

[0112] (7) A front silver electrode is prepared on the first transparent conductive layer by screen printing.

[0113] (8) A back silver electrode is prepared on the second transparent conductive layer by screen printing.

[0114] (9) Annealing the first hole selective transport layer and the second hole selective transport layer under vacuum conditions to obtain an undoped heterojunction solar cell, wherein the annealing temperature is 120° C. and the annealing time is 30 minutes.

[0115] Comparative Example 1

[0116] (1) A textured N-type silicon wafer is provided, and a plasma enhanced chemical vapor deposition device is used to prepare a first intrinsic hydrogenated amorphous silicon layer on one surface of the silicon wafer and a second intrinsic hydrogenated amorphous silicon layer on the other surface of the silicon wafer.

[0117] (2) An electron selective transport layer is prepared on the second intrinsic hydrogenated amorphous silicon layer.

[0118] (3) A first hole selective transport layer is deposited on the first intrinsic hydrogenated amorphous silicon layer using a thermal evaporation device. The material of the first hole selective transport layer is molybdenum oxide, and the deposition rate of the first hole selective transport layer is The deposition temperature of the first hole selective transport layer is room temperature.

[0119] (4) A first transparent conductive layer is prepared on the first hole selective transport layer by magnetron sputtering, wherein the material of the first transparent conductive layer is indium zinc oxide.

[0120] (5) Preparing a second transparent conductive layer on the electron selective transport layer, wherein the material of the second transparent conductive layer is indium zinc oxide.

[0121] (6) A front silver electrode is prepared on the first transparent conductive layer by screen printing.

[0122] (7) A back silver electrode is prepared on the second transparent conductive layer by screen printing.

[0123] (8) Annealing the first hole selective transport layer under vacuum conditions to obtain an undoped heterojunction solar cell, wherein the annealing temperature is 120° C. and the annealing time is 30 minutes.

[0124] Comparative Example 2

[0125] (1) A textured N-type silicon wafer is provided, and a plasma enhanced chemical vapor deposition device is used to prepare a first intrinsic hydrogenated amorphous silicon layer on one surface of the silicon wafer and a second intrinsic hydrogenated amorphous silicon layer on the other surface of the silicon wafer.

[0126] (2) An electron selective transport layer is prepared on the second intrinsic hydrogenated amorphous silicon layer.

[0127] (3) A second hole selective transport layer is deposited on the first intrinsic hydrogenated amorphous silicon layer using a hot filament chemical vapor deposition method. The material of the second hole selective transport layer is tungsten oxide. In the hot filament chemical vapor deposition method, the current passing through the filament is 48A, the distance between the filament and the second hole selective transport layer is 80mm, the deposition temperature of the second hole selective transport layer is 70°C, the deposition pressure of the second hole selective transport layer is 5Pa, and the deposition rate of the second hole selective transport layer is

[0128] (4) A first transparent conductive layer is prepared on the second hole selective transport layer by magnetron sputtering, wherein the material of the first transparent conductive layer is indium zinc oxide.

[0129] (5) Preparing a second transparent conductive layer on the electron selective transport layer, wherein the material of the second transparent conductive layer is indium zinc oxide.

[0130] (6) A front silver electrode is prepared on the first transparent conductive layer by screen printing.

[0131] (7) A back silver electrode is prepared on the second transparent conductive layer by screen printing.

[0132] (8) Annealing the second hole selective transport layer under vacuum conditions to obtain an undoped heterojunction solar cell, wherein the annealing temperature is 120° C. and the annealing time is 30 minutes.

[0133] (1) The undoped heterojunction solar cell prepared in Example 1 was tested using a scanning electron microscope.

[0134] Please refer to FIG. 3 . As can be seen from FIG. 3 , the total thickness of the first hole selective transport layer and the second hole selective transport layer of the undoped heterojunction solar cell prepared in Example 1 is about 9 nm.

[0135] (2) The open circuit voltage, short circuit current, fill factor and conversion efficiency of the undoped heterojunction solar cells prepared in Example 1 and Comparative Examples 1-2 were tested respectively. The test results are shown in Table 1 below.

[0136] Table 1 Preparation conditions of Example 1 and Comparative Examples 1-2 and the open circuit voltage, short circuit current, fill factor and conversion efficiency of the prepared undoped heterojunction solar cells

[0137] Please refer to Figure 4. It can be seen from Figure 4 and Table 1 above that the open circuit voltage and fill factor of the undoped heterojunction solar cell prepared in Example 1 (using molybdenum oxide and tungsten oxide as the first hole selective transport layer and the second hole selective transport layer, respectively) are higher than those of the undoped heterojunction solar cell prepared in Comparative Example 1 (using molybdenum oxide as the first hole selective transport layer) and the undoped heterojunction solar cell prepared in Comparative Example 2 (using tungsten oxide as the second hole selective transport layer). This indicates that the oxygen in the tungsten oxide of the undoped heterojunction solar cell prepared in Example 1 can be transferred to the molybdenum oxide, thereby increasing the oxygen content in the molybdenum oxide that plays a role in hole selective transport, thereby increasing the work function of the molybdenum oxide and enhancing the carrier selective transport characteristics of the molybdenum oxide. In addition, because the transmittance of molybdenum oxide is lower than that of tungsten oxide, the short-circuit current of the undoped heterojunction solar cell prepared in Example 1 is lower than that of the undoped heterojunction solar cell prepared in Comparative Example 2 using tungsten oxide. However, due to the high electrical conductivity and high hole-selective transport properties of molybdenum oxide, the fill factor of the undoped heterojunction solar cell prepared in Example 1 is higher than that of the undoped heterojunction solar cell prepared in Comparative Example 2. As can be seen from Table 1 above, the undoped heterojunction solar cell prepared in Example 1 also has a higher conversion efficiency than the undoped heterojunction solar cells prepared in Comparative Examples 1 and 2.

[0138] (3) The minority carrier lifetimes in the undoped heterojunction solar cells prepared in Example 1 and Comparative Examples 1-2 were tested respectively.

[0139] Referring to Figure 5 , it can be seen that the minority carrier lifetime in the undoped heterojunction solar cell prepared in Example 1 is 1001.55 μs, while the minority carrier lifetime in the undoped heterojunction solar cell prepared in Comparative Example 1 is only 826.21 μs, and the minority carrier lifetime in the undoped heterojunction solar cell prepared in Comparative Example 2 is only 571.62 μs. This suggests that annealing facilitates the redox reaction between molybdenum oxide and the silicon wafer, generating silicon oxide that improves the passivation level of the silicon wafer. Furthermore, annealing also facilitates the transfer of oxygen from tungsten oxide to molybdenum oxide.

[0140] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0141] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.

Claims

1. A method for preparing a solar cell, comprising the following steps: Providing a silicon wafer, and preparing an electron selective transport layer on one surface of the silicon wafer; Preparing a first hole selective transport layer on the other surface of the silicon wafer, wherein the material of the first hole selective transport layer is molybdenum oxide; Preparing a second hole selective transport layer on the first hole selective transport layer, wherein the material of the second hole selective transport layer is tungsten oxide; preparing a front electrode on the second hole selective transport layer; and A back electrode is prepared on the electron selective transport layer.

2. The method for preparing a solar cell according to claim 1, wherein: After preparing the back electrode, the preparation method further comprises the following steps: The first hole selective transport layer and the second hole selective transport layer are annealed.

3. The method for preparing a solar cell according to claim 2, wherein: The temperature of the annealing treatment is 120°C to 150°C.

4. The annealing treatment time according to any one of claims 2 to 3 is 30 min to 60 min.

5. The method for preparing a solar cell according to any one of claims 1 to 4, wherein: The second hole selective transport layer is prepared by hot wire chemical vapor deposition.

6. The method for preparing a solar cell according to claim 5, wherein: In the hot wire chemical vapor deposition method, the content of oxygen in the reaction atmosphere in the reaction chamber is ≤6.7%, and the content of oxygen in the reaction atmosphere in the reaction chamber is ≥1.7%.

7. The method for preparing a solar cell according to any one of claims 5 to 6, wherein: In the hot-filament chemical vapor deposition method, the distance between the filament and the first hole selective transport layer is 80 mm to 100 mm.

8. The method for preparing a solar cell according to any one of claims 5 to 7, wherein: In the hot-filament chemical vapor deposition method, the current passing through the filament is 30A to 60A.

9. The method for preparing a solar cell according to any one of claims 5 to 8, wherein: In the hot wire chemical vapor deposition method, the deposition pressure of the second hole selective transport layer is 2Pa to 6Pa.

10. The method for preparing a solar cell according to any one of claims 5 to 9, wherein: In the hot wire chemical vapor deposition method, the deposition rate of the second hole selective transport layer is 11. The method for preparing a solar cell according to any one of claims 1 to 10, wherein: The first hole selective transport layer is prepared by thermal evaporation.

12. The method for preparing a solar cell according to claim 11, wherein: In the thermal evaporation method, the deposition rate of the first hole selective transport layer is 13. The method for preparing a solar cell according to any one of claims 1 to 12, wherein: After preparing the second hole selective transport layer and before preparing the front electrode, the preparation method further comprises the following steps: A first transparent conductive layer is prepared on the second hole selective transport layer by magnetron sputtering.

14. A solar cell prepared using the preparation method according to any one of claims 1 to 13, comprising the silicon wafer, the first hole selective transport layer, the second hole selective transport layer and the front electrode stacked in sequence on one surface of the silicon wafer, and the electron selective transport layer and the back electrode stacked in sequence on the other surface of the silicon wafer.

15. The solar cell according to claim 14, wherein: The solar cell further includes a first transparent conductive layer located between the second hole selective transport layer and the front electrode, and a difference between a work function of the second hole selective transport layer and a work function of the first transparent conductive layer is less than or equal to 0.5 eV.

Citation Information

Patent Citations

  • Inverted green light quantum dot film electroluminescence device

    CN105845840A

  • Novel double-sided undoped heterojunction solar cell and preparation method thereof

    CN113707735A

  • Solar cell and preparation method thereof

    CN116487465A

  • Organic light-emitting diode having buffer layer containing tungsten oxide and molybdenum oxide

    KR1020150113622A

  • Quantum dot light-emitting device, preparation method therefor, and display apparatus

    WO2023050287A1