Resin composition, method for producing resin composition, and injection-molded object
The resin composition for injection molded articles, using crushed waste bumpers and propylene-based polymers, addresses the need for enhanced material recycling by increasing coating visibility and design quality in polypropylene reuse, improving moldability and impact strength.
Patent Information
- Application Number
- PCT/JP2024/014335
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-04-09
- Publication Date
- 2024-11-21
AI Technical Summary
The increasing demand for material recycling of waste plastics, driven by environmental initiatives like the 'Plastic Resource Circulation Strategy,' requires innovative methods to reuse polypropylene molded articles effectively, particularly in producing injection molded articles with enhanced design and visibility of coated films.
A resin composition comprising crushed automobile-derived waste bumpers, paint film removal powder, and a propylene-based polymer, with specific mass ratios and melt-kneading processes, is developed to create injection molded articles that reuse polypropylene effectively, enhancing design and visibility of coatings.
The solution increases the visibility of coatings on the surface of injection molded articles while reusing polypropylene, achieving a relatively excellent design and improving the moldability and impact strength of the resulting products.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Resin composition, method for producing resin composition, and injection-molded article CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority from Japanese Patent Application No. 2023-80116, the disclosure of which is incorporated herein by reference.
[0002] The present disclosure relates to a resin composition, a method for producing the resin composition, and an injection-molded article comprising the resin composition.
[0003] Traditionally, the main method of recycling plastics has been thermal recycling, which involves recovering and reusing the heat generated when waste plastic is burned. However, in May 2019, the Ministry of the Environment formulated the "Plastic Resource Circulation Strategy," which clearly states that by 2035, 100% of used plastics will be effectively utilized through reduction and recycling. In this social climate, there is a growing demand for material recycling, which reuses waste plastics as raw materials for plastic products.
[0004] Polypropylene has good moldability and excellent rigidity, heat resistance, etc., and is therefore widely used in automobile parts (for example, exterior parts such as bumpers, and interior parts such as door trims and instrument panels), housings for household electrical appliances, etc. Therefore, polypropylene molded articles used in the market are collected and reused as raw materials for plastic products.
[0005] Meanwhile, polypropylene molded articles are also required to have excellent design properties. For example, Patent Document 1 discloses that a molded article made of a resin composition in which polypropylene resin and aluminum powder are mixed has a metallic appearance.
[0006] Japanese Patent Application Publication No. 2006-9034
[0007] The present disclosure has been made in consideration of the above circumstances, and aims to provide a resin composition that can increase the number of coating films visible from the outside while reusing polypropylene, thereby obtaining a molded article with relatively excellent design properties; a method for producing the resin composition; and an injection-molded article containing the resin composition.
[0008] The resin composition according to the present disclosure contains component (A): crushed material of scrap automobile bumpers containing 1% by mass or more and less than 30% by mass of xylene insolubles, component (B): paint peeling powder of scrap automobile bumpers containing 30% by mass or more and less than 50% by mass of xylene insolubles, and component (C): a propylene-based polymer, wherein the content of component (A) is 15% by mass or more and 35% by mass or less, the content of component (B) is 15% by mass or more and 35% by mass or less, and the content of component (C) is 30% by mass or more and 70% by mass or less, relative to the total mass of the resin composition.
[0009] A method for producing a resin composition according to the present disclosure includes a step of melt-kneading a mixture containing: component (A): crushed material of automobile-derived scrap bumpers containing 1% by mass or more and less than 30% by mass of xylene insolubles; component (B): paint peeling powder of automobile-derived scrap bumpers containing 30% by mass or more and less than 50% by mass of xylene insolubles; and component (C): a propylene-based polymer, without passing the mixture through a screen mesh, wherein the content of component (A) is 15% by mass or more and 35% by mass or less, the content of component (B) is 15% by mass or more and 35% by mass or less, and the content of component (C) is 30% by mass or more and 70% by mass or less, relative to the total mass of the mixture.
[0010] The injection-molded article according to the present disclosure contains the above-described resin composition.
[0011] Hereinafter, embodiments of the present disclosure will be described, but the present disclosure is not limited to the following embodiments.
[0012] [Resin Composition] The resin composition according to the present embodiment contains component (A): crushed material from scrap automobile bumpers containing 1% by mass or more and less than 30% by mass of xylene insolubles, component (B): peeled paint powder from scrap automobile bumpers containing 30% by mass or more and less than 50% by mass of xylene insolubles, and component (C): a propylene-based polymer. The resin composition preferably further contains component (D): an ethylene-α-olefin copolymer.
[0013] <Component (A)> The crushed material of scrap automobile bumpers, which is component (A), is obtained by crushing scrap automobile bumpers collected from the market or scrap automobile bumpers collected during a process that could not be made into a product due to poor paintwork, etc. Scrap automobile bumpers have a paint film.
[0014] Component (A) contains xylene insolubles in an amount of 1% by mass or more and less than 30% by mass, and preferably 1% by mass or more and 25% by mass or less, based on the total mass of component (A). The content of xylene insolubles can be calculated by weighing the residue obtained by Soxhlet extraction.
[0015] The crushed material of component (A) can have a maximum dimension of, for example, 20 mm or less.
[0016] Component (A) may contain a propylene polymer, which will be described below as component (C). The content of the propylene polymer is preferably 40% by mass or more, more preferably 50% by mass or more, based on the total mass of component (A). The content of the propylene polymer is preferably 99% by mass or less, more preferably 95% by mass or less, based on the total mass of component (A).
[0017] Component (A) may contain an ethylene-α-olefin copolymer, which will be described below as component (D). The content of the ethylene-α-olefin copolymer is preferably 1% by mass or more, more preferably 5% by mass or more, based on the total mass of component (A). Furthermore, the content of the ethylene-α-olefin copolymer is preferably 50% by mass or less, more preferably 30% by mass or less, based on the total mass of component (A).
[0018] Component (A) may contain a filler, which will be described later. The content of the filler is preferably 1% by mass or more, more preferably 5% by mass or more, based on the total mass of component (A). The content of the filler is preferably 50% by mass or less, more preferably 30% by mass or less, based on the total mass of component (A).
[0019] The content of component (A) is 15% by mass or more and 35% by mass or less, based on the total mass of the resin composition. The content of component (A) is preferably 20% by mass or more, and more preferably 25% by mass or more, based on the total mass of the resin composition. Furthermore, the content of component (A) is preferably 30% by mass or less, and more preferably 28% by mass or less, based on the total mass of the resin composition.
[0020] The melt flow rate (MFR) of component (A) is preferably 1 g / 10 min or more and 100 g / 10 min or less, more preferably 12 g / 10 min or more and 70 g / 10 min or less, and even more preferably 15 g / 10 min or more and 50 g / 10 min or less. From the viewpoint of improving the molding processability of the resulting resin composition, the MFR of component (A) is preferably 10 g / 10 min or more. From the viewpoint of improving the impact strength of the resulting molded article, the MFR of component (A) is preferably 100 g / 10 min or less. The MFR of component (A) is measured by Method A in accordance with the method specified in JIS K7210-1995, under conditions of a temperature of 230°C and a load of 2.16 kg.
[0021] Depending on the application, component (A) may contain additives such as neutralizing agents, antioxidants, ultraviolet absorbers, nucleating agents, lubricants, antistatic agents, antiblocking agents, colorants (inorganic pigments, organic pigments, pigment dispersants, etc.), etc. The process for recovering component (A) is not particularly limited, and known methods can be used.
[0022] <Component (B)> The paint film peeled powder from automobile-derived scrap bumpers, which is component (B), is obtained by peeling from automobile-derived scrap bumpers collected from the market or from automobile-derived scrap bumpers collected during a process that did not become a product due to poor painting, etc. The method for peeling component (B) is not particularly limited, and known methods can be used.
[0023] Component (B) contains 30% by mass or more and less than 50% by mass, and preferably 35% by mass or more and 45% by mass or less, of xylene insolubles relative to the total mass of component (B). The content of xylene insolubles can be calculated by weighing the residue obtained by Soxhlet extraction.
[0024] In one embodiment, component (B) contains titanium oxide. The content of titanium oxide is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, based on the total mass of component (B). Furthermore, the content of titanium oxide is preferably 5% by mass or less, more preferably 4.8% by mass or less, based on the total mass of component (B). In one embodiment, the content of titanium oxide is 0.05% by mass or more and 5% by mass or less, based on the total mass of component (B).
[0025] In one embodiment, component (B) contains metallic aluminum. The content of metallic aluminum is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, based on the total mass of component (B). Furthermore, the content of metallic aluminum is preferably 1 mass% or less, more preferably 0.8 mass% or less, based on the total mass of component (B). In one embodiment, the content of metallic aluminum is 0.01 mass% or more and 1 mass% or less, based on the total mass of component (B).
[0026] In one embodiment, component (B) contains talc. The talc content is preferably 5% by mass or more, more preferably 10% by mass or more, based on the total mass of component (B). Furthermore, the talc content is preferably 20% by mass or less, more preferably 15% by mass or less, based on the total mass of component (B). In one embodiment, the talc content is 5% by mass or more and 20% by mass or less, based on the total mass of component (B).
[0027] The content of component (B) is 15% by mass or more and 35% by mass or less, based on the total mass of the resin composition. The content of component (B) is preferably 20% by mass or more, and more preferably 25% by mass or more, based on the total mass of the resin composition. Furthermore, the content of component (B) is preferably 30% by mass or less, and more preferably 28% by mass or less, based on the total mass of the resin composition.
[0028] <Component (C)> The propylene-based polymer, which is component (C), is a polymer containing 50% by mass or more of monomer units derived from propylene. Examples of the propylene-based polymer include a propylene homopolymer, a random copolymer of propylene and a monomer other than propylene, and a heterophasic propylene polymer material. The resin composition according to this embodiment may contain only one type of propylene-based polymer, or may contain two or more types of propylene-based polymers.
[0029] From the viewpoint of improving the molding processability of the resin composition, the melt flow rate (MFR) of component (C) is preferably 0.1 g / 10 min or more, more preferably 1 g / 10 min or more and 300 g / 10 min or less, and even more preferably 5 g / 10 min or more and 300 g / 10 min or less. The MFR of component (C) is measured by Method A in accordance with the method specified in JIS K7210-1995, under conditions of a temperature of 230°C and a load of 2.16 kg.
[0030] The content of component (C) is 30% by mass or more and 70% by mass or less, based on the total mass of the resin composition. The content of component (C) is preferably 35% by mass or more, and more preferably 38% by mass or more, based on the total mass of the resin composition. Furthermore, the content of component (C) is preferably 60% by mass or less, and more preferably 50% by mass or less, based on the total mass of the resin composition.
[0031] (Propylene Homopolymer) From the viewpoint of improving the fluidity of the resin composition when melted and the toughness of a molded product, the propylene homopolymer has an intrinsic viscosity ([η]) of preferably 0.10 dL / g or more and 4.00 dL / g or less, more preferably 0.50 dL / g or more and 3.00 dL / g or less, and even more preferably 0.70 dL / g or more and 2.00 dL / g or less.
[0032] In this specification, the intrinsic viscosity (unit: dL / g) is a value measured at a temperature of 135°C using tetralin as a solvent by the following method.
[0033] Using an Ubbelohde viscometer, the reduced viscosity is measured at three concentrations: 0.1 g / dL, 0.2 g / dL, and 0.5 g / dL. The reduced viscosity is plotted against the concentration, and the intrinsic viscosity is calculated by extrapolation, extrapolating the concentration to zero. The method for calculating the intrinsic viscosity by extrapolation is described, for example, on page 491 of "Polymer Solutions, Polymer Experiments 11" (published by Kyoritsu Shuppan Co., Ltd. in 1982).
[0034] The propylene homopolymer can be produced, for example, by carrying out a polymerization step in which propylene is polymerized using a polymerization catalyst.
[0035] Examples of the polymerization catalyst include Ziegler catalysts; Ziegler-Natta catalysts; catalysts containing a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring and an alkylaluminoxane; catalysts containing a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex upon reaction with the transition metal compound, and an organoaluminum compound; and modified catalysts obtained by supporting a catalyst component (a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex, an organoaluminum compound, etc.) on inorganic particles (silica, clay mineral, etc.).
[0036] Examples of the polymerization catalyst include those described in JP-A-61-218606, JP-A-5-194685, JP-A-7-216017, JP-A-9-316147, JP-A-10-212319, JP-A-2004-182981, JP-A-2010-168545, and JP-A-2011-246699.
[0037] Furthermore, a polymer obtained by prepolymerizing propylene in the presence of the above polymerization catalyst can also be used as the polymerization catalyst.
[0038] Examples of polymerization methods include bulk polymerization, solution polymerization, and gas phase polymerization. Here, bulk polymerization refers to a method in which polymerization is carried out using an olefin that is liquid at the polymerization temperature as a medium. Solution polymerization refers to a method in which polymerization is carried out in an inert hydrocarbon solvent such as propane, butane, isobutane, pentane, hexane, heptane, or octane. Gas phase polymerization refers to a method in which gaseous monomers are used as a medium and the gaseous monomers are polymerized in the medium.
[0039] The polymerization method may be, for example, a batch method, a continuous method, or a combination thereof. The polymerization method may be a multi-stage method in which a plurality of polymerization reactors are connected in series.
[0040] From the viewpoint of industrial and economical excellence, the polymerization method is preferably a continuous gas phase polymerization method or a bulk-gas phase polymerization method in which bulk polymerization and gas phase polymerization are carried out continuously.
[0041] Various conditions in the polymerization step (polymerization conditions such as polymerization temperature, polymerization pressure, monomer concentration, catalyst input amount, and polymerization time) may be appropriately determined depending on the molecular structure of the target polymer.
[0042] In the method for producing a propylene homopolymer, other steps may be carried out before or after the polymerization step. For example, after the polymerization step, the polymer may be dried at a temperature equal to or lower than the melting point of the polymer, as necessary, in order to remove residual solvent contained in the polymer and ultralow molecular weight oligomers produced as by-products during production. Examples of drying methods include those described in JP-A-55-75410 and JP-A-2565753.
[0043] (Random copolymer of propylene and a monomer other than propylene) The random copolymer of propylene and a monomer other than propylene contains monomer units derived from propylene and monomer units derived from a monomer other than propylene. The random copolymer preferably contains 0.01% by mass or more and 20% by mass or less of the monomer units derived from a monomer other than propylene, based on the total mass of the copolymer.
[0044] Examples of monomers other than propylene include ethylene and α-olefins having 4 to 12 carbon atoms. In this specification, α-olefins are aliphatic unsaturated hydrocarbons having a carbon-carbon unsaturated double bond at the α-position. Examples of α-olefins having 4 to 12 carbon atoms include 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 4-methyl-1-pentene, and 4-methyl-1-hexene.
[0045] The monomer other than propylene is preferably at least one selected from the group consisting of ethylene and α-olefins having 4 to 10 carbon atoms, more preferably at least one selected from the group consisting of ethylene, 1-butene, 1-hexene, and 1-octene, and even more preferably at least one selected from the group consisting of ethylene and 1-butene.
[0046] Examples of random copolymers of propylene and a monomer other than propylene include propylene-ethylene random copolymers, propylene-1-butene random copolymers, propylene-1-hexene random copolymers, propylene-1-octene random copolymers, propylene-ethylene-1-butene random copolymers, propylene-ethylene-1-hexene random copolymers, and propylene-ethylene-1-octene random copolymers.
[0047] The random copolymer of propylene and a monomer other than propylene has an intrinsic viscosity ([η]) of preferably 0.10 dL / g or more and 4.00 dL / g or less, more preferably 0.50 dL / g or more and 3.00 dL / g or less, and even more preferably 0.70 dL / g or more and 2.00 dL / g or less, from the viewpoint of improving the fluidity of the propylene resin composition when melted.
[0048] A random copolymer of propylene and a monomer other than propylene can be produced, for example, by polymerizing propylene and a monomer other than propylene in accordance with the polymerization catalyst, polymerization method, polymerization system, and polymerization conditions that can be used in the production of the above-mentioned propylene homopolymer.
[0049] (Heterophagic Propylene Polymerization Material) The heterophasic propylene polymerization material is a mixture containing a polymer I containing 80% by mass or more of monomer units derived from propylene (where the total mass of the polymer I is taken as 100% by mass), and a polymer II containing monomer units derived from at least one α-olefin selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms and monomer units derived from propylene.
[0050] The heterophasic propylene polymer material can be produced, for example, by carrying out a first polymerization step of polymerizing polymer I and a second polymerization step of polymerizing polymer II. These polymerization steps can be carried out using the same polymerization catalyst, polymerization method, polymerization system, and polymerization conditions as those usable in the production of the above-mentioned propylene homopolymer.
[0051] The heterophasic propylene polymer material may be such that the sum of polymer I and polymer II contained in the heterophasic propylene polymer material is 100% by mass relative to the total mass of the heterophasic propylene polymer material.
[0052] As described above, polymer I contains 80% by mass or more of monomer units derived from propylene (where the total mass of polymer I is 100% by mass). Polymer I may be, for example, a propylene homopolymer, or may contain monomer units derived from a monomer other than propylene. When polymer I contains monomer units derived from a monomer other than propylene, the content of such units may be, for example, 0.01% by mass or more and less than 20% by mass relative to the total mass of polymer I.
[0053] Examples of the monomer other than propylene include ethylene and α-olefins having 4 or more carbon atoms. Examples of the α-olefins having 4 or more carbon atoms include 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 4-methyl-1-pentene, and 4-methyl-1-hexene.
[0054] The monomer other than propylene is preferably at least one selected from the group consisting of ethylene and α-olefins having 4 to 10 carbon atoms, more preferably at least one selected from the group consisting of ethylene, 1-butene, 1-hexene, and 1-octene, and even more preferably at least one selected from the group consisting of ethylene and 1-butene.
[0055] Examples of polymer I containing a monomer unit derived from a monomer other than propylene include a propylene-ethylene copolymer, a propylene-1-butene copolymer, a propylene-1-hexene copolymer, a propylene-1-octene copolymer, a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, and a propylene-ethylene-1-octene copolymer.
[0056] From the viewpoint of improving the dimensional stability of the molded article, polymer I is preferably a propylene homopolymer, a propylene-ethylene copolymer, a propylene-1-butene copolymer, or a propylene-ethylene-1-butene copolymer, and more preferably a propylene homopolymer.
[0057] The content of polymer I is preferably 50% by mass or more and 99% by mass or less, more preferably 60% by mass or more and 95% by mass or less, based on the total mass of the heterophasic propylene polymer material.
[0058] As described above, polymer II contains monomer units derived from at least one α-olefin selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms, and monomer units derived from propylene. Examples of α-olefins having 4 to 12 carbon atoms include 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 4-methyl-1-pentene, and 4-methyl-1-hexene.
[0059] Polymer II preferably contains 30% by mass or more of monomer units derived from at least one α-olefin selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms, and also contains monomer units derived from propylene (where the total mass of Polymer II is taken as 100% by mass).
[0060] In Polymer II, the content of monomer units derived from at least one α-olefin selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms may be 30% by mass or more and 70% by mass or less, or 35% by mass or more and 60% by mass or less (where the total mass of Polymer II is taken as 100% by mass).
[0061] In Polymer II, the at least one α-olefin selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms is preferably at least one selected from the group consisting of ethylene and α-olefins having 4 to 10 carbon atoms, more preferably at least one selected from the group consisting of ethylene, 1-butene, 1-hexene, 1-octene, and 1-decene, and even more preferably at least one selected from the group consisting of ethylene and 1-butene.
[0062] Examples of polymer II include propylene-ethylene copolymer, propylene-ethylene-1-butene copolymer, propylene-ethylene-1-hexene copolymer, propylene-ethylene-1-octene copolymer, propylene-ethylene-1-decene copolymer, propylene-1-butene copolymer, propylene-1-hexene copolymer, propylene-1-octene copolymer, propylene-1-decene copolymer, etc. Among these, polymer II is preferably a propylene-ethylene copolymer, a propylene-1-butene copolymer, or a propylene-ethylene-1-butene copolymer, and more preferably a propylene-ethylene copolymer.
[0063] The content of polymer II is preferably 1% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 40% by mass or less, based on the total mass of the heterophasic propylene polymer material.
[0064] In the heterophasic propylene polymerization material, the content of monomer units derived from at least one α-olefin selected from the group consisting of ethylene and α-olefins having 4 to 12 carbon atoms may be 0.3% by mass or more and 35% by mass or less, or 0.7% by mass or more and 24% by mass or less (where the total mass of the heterophasic propylene polymerization material is 100% by mass).
[0065] Examples of heterophasic propylene polymer materials include (propylene)-(propylene-ethylene) polymer materials, (propylene)-(propylene-ethylene-1-butene) polymer materials, (propylene)-(propylene-ethylene-1-hexene) polymer materials, (propylene)-(propylene-ethylene-1-octene) polymer materials, (propylene)-(propylene-1-butene) polymer materials, (propylene)-(propylene-1-hexene) polymer materials, (propylene)-(propylene-1-octene) polymer materials, and (propylene)-(propylene- (propylene-ethylene)-(propylene-ethylene) polymerization material, (propylene-ethylene)-(propylene-ethylene-1-butene) polymerization material, (propylene-ethylene)-(propylene-ethylene-1-hexene) polymerization material, (propylene-ethylene)-(propylene-ethylene-1-octene) polymerization material, (propylene-ethylene)-(propylene-ethylene-1-decene) polymerization material, (propylene-ethylene)-(propylene-1-butene) polymerization material, (propylene-ethylene)-(propylene-1-hexene) (propylene-ethylene)-(propylene-1-octene) polymerization material, (propylene-ethylene)-(propylene-1-decene) polymerization material, (propylene-1-butene)-(propylene-ethylene) polymerization material, (propylene-1-butene)-(propylene-ethylene-1-butene) polymerization material, (propylene-1-butene)-(propylene-ethylene-1-hexene) polymerization material, (propylene-1-butene)-(propylene-ethylene-1-octene) polymerization material, (propylene-1-butene)-(propylene-ethylene- (propylene-1-decene) polymerization material, (propylene-1-butene)-(propylene-1-butene) polymerization material, (propylene-1-butene)-(propylene-1-hexene) polymerization material, (propylene-1-butene)-(propylene-1-octene) polymerization material, (propylene-1-butene)-(propylene-1-decene) polymerization material, (propylene-1-hexene)-(propylene-1-hexene) polymerization material, (propylene-1-hexene)-(propylene-1-octene) polymerization material, (propylene-1-hexene)-(propylene-1-decene) polymerization material,Examples include (propylene-1-octene)-(propylene-1-octene) polymer materials, (propylene-1-octene)-(propylene-1-decene) polymer materials, etc.
[0066] Here, the expression "(propylene)-(propylene-ethylene) polymer material" means "a heterophasic propylene polymer material in which polymer I is a propylene homopolymer and polymer II is a propylene-ethylene copolymer." The same applies to other similar expressions.
[0067] The heterophasic propylene polymeric material is preferably a (propylene)-(propylene-ethylene) polymeric material, a (propylene)-(propylene-ethylene-1-butene) polymeric material, a (propylene-ethylene)-(propylene-ethylene) polymeric material, a (propylene-ethylene)-(propylene-ethylene-1-butene) polymeric material, or a (propylene-1-butene)-(propylene-1-butene) polymeric material, and more preferably a (propylene)-(propylene-ethylene) polymeric material.
[0068] The intrinsic viscosity number ([η]I) of Polymer I is preferably 0.10 dL / g or more and 4.00 dL / g or less, more preferably 0.50 dL / g or more and 3.00 dL / g or less, and even more preferably 0.70 dL / g or more and 2.00 dL / g or less.
[0069] The intrinsic viscosity number ([η]II) of Polymer II is preferably 1.00 dL / g or more and 10.00 dL / g or less, more preferably 2.00 dL / g or more and 10.00 dL / g or less, and even more preferably 2.00 dL / g or more and 9.00 dL / g or less.
[0070] The ratio ([η]II / [η]I) of the intrinsic viscosity number ([η]II) of Polymer II to the intrinsic viscosity number ([η]I) of Polymer I is preferably 1 or more and 20 or less, more preferably 1 or more and 10 or less.
[0071] The intrinsic viscosity number ([η]I) of polymer I can be measured, for example, by extracting polymer I from a reactor in which polymer I is polymerized and measuring the intrinsic viscosity number of the polymer.
[0072] The intrinsic viscosity number ([η]II) of polymer II can be calculated, for example, by the following formula (i) using the intrinsic viscosity number ([η]Total) of the heterophasic propylene polymerization material, the intrinsic viscosity number ([η]I) of polymer I, and the contents of polymer II and polymer I.
[0073] [η]II=([η]Total-[η]I×XI) / XII (i) [η]Total: intrinsic viscosity number (dL / g) of the heterophasic propylene polymerization material [η]I: intrinsic viscosity number (dL / g) of polymer I XI: ratio of the mass of polymer I to the total mass of the heterophasic propylene polymerization material (mass of polymer I / mass of heterophasic propylene polymerization material) XII: ratio of the mass of polymer II to the total mass of the heterophasic propylene polymerization material (mass of polymer II / mass of heterophasic propylene polymerization material)
[0074] Here, XI and XII can be determined from the material balance during polymerization.
[0075] XII may be calculated by measuring the heat of fusion of polymer I and the heat of fusion of the heterophasic propylene polymer material and using the following formula: XII=1-(ΔHf)T / (ΔHf)P, where (ΔHf)T: heat of fusion of heterophasic propylene polymer material (J / g), (ΔHf)P: heat of fusion of polymer I (J / g).
[0076] <Component (D)> The resin composition according to this embodiment may contain an ethylene-α-olefin copolymer as component (D). The ethylene-α-olefin copolymer may be an ethylene-α-olefin random copolymer. The ethylene-α-olefin copolymer refers to a copolymer containing monomer units derived from ethylene and monomer units derived from an α-olefin having 4 or more carbon atoms, and is substantially free of monomer units derived from propylene.
[0077] The ethylene-α-olefin copolymer that is component (D) may have a total content of monomer units derived from ethylene and monomer units derived from an α-olefin having 4 or more carbon atoms of 100% by mass relative to the total mass of the copolymer.
[0078] Examples of α-olefins having 4 or more carbon atoms include α-olefins having 4 to 12 carbon atoms. Examples of α-olefins having 4 to 12 carbon atoms include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene. The α-olefins having 4 to 12 carbon atoms are preferably 1-butene, 1-hexene, or 1-octene. The α-olefins having 4 to 12 carbon atoms may also be α-olefins having a cyclic structure, such as vinylcyclopropane and vinylcyclobutane.
[0079] Examples of the ethylene-α-olefin copolymer include an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, an ethylene-1-octene copolymer, an ethylene-1-decene copolymer, an ethylene-(3-methyl-1-butene) copolymer, and a copolymer of ethylene and an α-olefin having a cyclic structure.
[0080] In the ethylene-α-olefin copolymer, the content of monomer units derived from α-olefins having 4 or more carbon atoms is preferably 1% by mass or more and 49% by mass or less, more preferably 5% by mass or more and 49% by mass or less, and even more preferably 24% by mass or more and 49% by mass or less, based on the total mass of the ethylene-α-olefin copolymer.
[0081] The density of component (D) is preferably 0.85 g / cm from the viewpoint of improving the impact resistance of the molded article. 3 0.89g / cm or more 3 More preferably, it is 0.85 g / cm or less. 3 0.88g / cm or more 3 More preferably, it is 0.85 g / cm or less. 3 0.87g / cm or more 3 The following is the result.
[0082] The melt flow rate (MFR) of component (D) is preferably 0.1 g / 10 min or more and 80 g / 10 min or less. The MFR of the ethylene-α-olefin copolymer is measured by Method A in accordance with JIS K7210-1995, under conditions of a temperature of 190°C and a load of 2.16 kg.
[0083] The content of component (D) is preferably 5% by mass or more, more preferably 7% by mass or more, based on the total mass of the resin composition. The content of component (D) is preferably 15% by mass or less, more preferably 12% by mass or less, based on the total mass of the resin composition. In one embodiment, the content of component (D) is 5% by mass or more and 15% by mass or less, based on the total mass of the resin composition.
[0084] The ethylene-α-olefin copolymer, component (D), can be produced by polymerizing ethylene and an α-olefin having 4 or more carbon atoms using a polymerization catalyst.
[0085] Examples of the polymerization catalyst include homogeneous catalysts such as metallocene catalysts, and Ziegler-Natta catalysts.
[0086] Examples of homogeneous catalysts include catalysts containing a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring and an alkylaluminoxane; catalysts containing a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that reacts with the transition metal compound to form an ionic complex, and an organoaluminum compound; and modified catalysts in which a catalyst component (a compound of a transition metal of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex, an organoaluminum compound, etc.) is supported on inorganic particles (silica, clay mineral, etc.).
[0087] Examples of Ziegler-Natta catalysts include catalysts that combine a titanium-containing solid transition metal component with an organometallic component.
[0088] The ethylene-α-olefin copolymer may be a commercially available product. Examples of commercially available ethylene-α-olefin copolymers include ENGAGE (registered trademark) manufactured by Dow Chemical Japan, TAFMER (registered trademark) manufactured by Mitsui Chemicals, Inc., NEOZEX (registered trademark) and ULTOZEX (registered trademark) manufactured by Prime Polymer Co., Ltd., and EXCELLEN FX (registered trademark), SUMIKACENE (registered trademark), and ESPRENE SPO (registered trademark) manufactured by Sumitomo Chemical Co., Ltd.
[0089] <Filler> The resin composition according to this embodiment may contain a filler. Examples of the filler include inorganic fillers and organic fillers. The resin composition may contain only one type of filler, or may contain two or more types of fillers.
[0090] Examples of inorganic fillers include glass, silicate minerals, alumina, silica, silicon dioxide, titanium oxide, iron oxide, aluminum oxide, magnesium oxide, antimony oxide, barium ferrite, strontium ferrite, beryllium oxide, magnesium hydroxide, aluminum hydroxide, basic magnesium carbonate, calcium carbonate, magnesium carbonate, carbonate minerals, calcium sulfate, magnesium sulfate, basic magnesium sulfate, calcium sulfite, carbon black, and cadmium sulfide.
[0091] Examples of organic fillers include polyester, aromatic polyamide, cellulose, vinylon, and the like.
[0092] The shape of the filler may be plate-like, needle-like, or fibrous.
[0093] From the viewpoint of improving the rigidity, impact resistance and dimensional stability of the molded body, the filler is preferably an inorganic filler, more preferably talc, which is a plate-like silicate mineral.
[0094] <Resin Composition> The shape of the resin composition according to the present embodiment is not particularly limited, and may be, for example, a strand, a sheet, a plate, or a pellet. A pellet-shaped resin composition can be produced, for example, by forming a strand-shaped resin composition and then cutting it to an appropriate length.
[0095] From the viewpoint of improving the moldability of the resin composition and the production stability when producing a molded article, the shape of the resin composition before being molded into a molded article is preferably in the form of pellets having a length of about 1 to 50 mm.
[0096] The resin composition according to the present embodiment may contain other components in addition to those described above, such as a neutralizing agent, an antioxidant, an ultraviolet absorber, a nucleating agent, a lubricant, an antistatic agent, an antiblocking agent, a processing aid, an organic peroxide, a colorant (inorganic pigment, organic pigment, pigment dispersant, etc.), etc.
[0097] The melt flow rate (MFR) of the resin composition according to this embodiment is preferably 1 g / 10 min or more and 100 g / 10 min or less, more preferably 12 g / 10 min or more and 70 g / 10 min or less, and even more preferably 15 g / 10 min or more and 40 g / 10 min or less. From the viewpoint of improving molding processability, the MFR of the resin composition is preferably 10 g / 10 min or more. From the viewpoint of improving the impact strength of the resulting molded article, the MFR of the resin composition is preferably 100 g / 10 min or less. The MFR of the resin composition is measured by Method A in accordance with the method specified in JIS K7210-1995, under conditions of a temperature of 230°C and a load of 2.16 kg.
[0098] The density of the resin composition according to this embodiment is preferably 1.30 g / cm 3 More preferably, it is 1.20 g / cm or less. 3 More preferably, it is 1.10 g / cm or less. 3 The density of the resin composition is preferably 0.80 g / cm or less. 3 More preferably, 0.85 g / cm 3 More preferably, it is 0.90 g / cm 3 The density is measured by the water displacement method, which is Method A described in JIS K7112.
[0099] [Method for producing resin composition] A method for producing a resin composition according to this embodiment includes a step of melt-kneading a mixture containing: component (A): crushed material of automobile-derived scrap bumpers containing 1% by mass or more and less than 30% by mass of xylene insolubles; component (B): paint peeled powder of automobile-derived scrap bumpers containing 30% by mass or more and less than 50% by mass of xylene insolubles; and component (C): a propylene-based polymer, without passing the mixture through a screen mesh, wherein the content of component (A) is 15% by mass or more and 35% by mass or less, the content of component (B) is 15% by mass or more and 35% by mass or less, and the content of component (C) is 30% by mass or more and 70% by mass or less, relative to the total mass of the mixture.
[0100] The mixture contains the above-mentioned components (A), (B), and (C). The mixture may further contain the above-mentioned ethylene-α-olefin copolymer (component (D)), a filler, and other components.
[0101] In the melt-kneading step, the temperature during melt-kneading may be 180°C or higher, 180°C or higher and 300°C or lower, or 180°C or higher and 250°C or lower.
[0102] For melt kneading, a Banbury mixer, a single-screw extruder, a twin-screw co-rotating extruder, or the like can be used.
[0103] The order in which the raw material components contained in the mixture are kneaded is not particularly limited. For example, all of the components may be kneaded at once, or some of the components may be kneaded and then the resulting mixture may be kneaded with the other components.
[0104] [Injection Molded Article] The injection molded article according to this embodiment includes the resin composition described above. That is, the resin composition described above can be used as a material for forming the injection molded article by molding.
[0105] Injection-molded articles can be produced by injection molding. Examples of injection molding methods include general injection molding, injection foam molding, supercritical injection foam molding, ultra-high speed injection molding, injection compression molding, gas-assisted injection molding, sandwich molding, sandwich foam molding, and insert-outsert molding. The shape of the injection-molded article is not particularly limited.
[0106] The injection-molded article can be used, for example, for automotive materials, home appliance materials, containers, etc., and is preferably used for automotive interior and exterior applications. Examples of automotive interior and exterior parts include door trims, pillars, instrument panels, bumpers, etc.
[0107] The present disclosure includes the following aspects. [1] A resin composition comprising: component (A): crushed material from automobile-derived scrap bumpers containing 1% by mass or more and less than 30% by mass of xylene insolubles; component (B): paint peeling powder from automobile-derived scrap bumpers containing 30% by mass or more and less than 50% by mass of xylene insolubles; and component (C): a propylene-based polymer, wherein the content of component (A) is 15% by mass or more and 35% by mass or less, the content of component (B) is 15% by mass or more and 35% by mass or less, and the content of component (C) is 30% by mass or more and 70% by mass or less, relative to the total mass of the resin composition. [2] The resin composition according to [1], further comprising component (D): an ethylene-α-olefin copolymer, wherein the content of component (D) is 5% by mass or more and 15% by mass or less, relative to the total mass of the resin composition. [3] The resin composition according to [1] or [2], wherein component (B) contains titanium oxide, and the content of the titanium oxide is 0.05% by mass or more and 5% by mass or less, relative to the total mass of component (B). [4] The resin composition according to any one of [1] to [3], wherein component (B) contains metallic aluminum, and the content of the metallic aluminum is 0.01% by mass or more and 1% by mass or less, relative to the total mass of component (B). [5] The resin composition according to any one of [1] to [4], wherein component (B) contains talc, and the content of the talc is 5% by mass or more and 20% by mass or less, relative to the total mass of component (B). [6] A method for producing a resin composition, comprising: a step of melt-kneading a mixture containing, without passing through a screen mesh, component (A): crushed material from automobile-derived scrap bumpers containing 1% by mass or more and less than 30% by mass of xylene insolubles, component (B): paint peeling powder from automobile-derived scrap bumpers containing 30% by mass or more and less than 50% by mass of xylene insolubles, and component (C): a propylene-based polymer, wherein the content of component (A) is 15% by mass or more and 35% by mass or less, the content of component (B) is 15% by mass or more and 35% by mass or less, and the content of component (C) is 30% by mass or more and 70% by mass or less, relative to the total mass of the mixture. [7] An injection-molded article comprising the resin composition according to any one of [1] to [5].
[0108] It should be noted that the resin composition, the method for producing a resin composition, and the injection-molded article according to the present disclosure are not limited to the configurations of the above-described embodiments. Furthermore, the resin composition, the method for producing a resin composition, and the injection-molded article according to the present disclosure are not limited to the above-described effects. The resin composition, the method for producing a resin composition, and the injection-molded article according to the present disclosure can be modified in various ways without departing from the spirit of the present disclosure.
[0109] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to these examples.
[0110] <Raw Materials> The following raw materials were used in the examples and comparative examples.
[0111] Component (A): Shredded Automobile-Derived Bumper Scrap As component (A), the following (A-1) shredded automobile-derived painted bumper scrap collected from the market was prepared.
[0112] (A-1) Crushed paint-coated waste bumper material from recycled automobiles MFR (temperature 230°C, load 2.16 kg): 42 g / 10 min Amount of xylene insoluble matter: 23.2 mass%
[0113] Component (B): Paint film peeling powder from scrap automobile bumpers As component (B), the following paint film peeling powder from scrap automobile bumpers (B-1) to (B-4) collected from the market was prepared.
[0114] (B-1) Paint peeling powder from scrap bumpers from recycled automobiles Number of paint peeling processes: 2 Amount of xylene insoluble matter: 42.8% by mass
[0115] (B-2) Paint peeling powder from scrap bumpers from recycled automobiles Number of paint peeling processes: 3 Amount of xylene insoluble matter: 41.7% by mass
[0116] (B-3) Paint peeling powder from scrap bumpers from recycled automobiles Number of paint peeling processes: 4 Amount of xylene insoluble matter: 40.7% by mass
[0117] (B-4) Paint peeling powder from scrap bumpers from recycled automobiles Number of paint peeling processes: 6 Amount of xylene insoluble matter: 36.5% by mass
[0118] (Amount of Xylene Insolubles) 4 g of each of components (A) and (B) was weighed out and refluxed in boiling xylene for 5 hours using a cylindrical filter and a Soxhlet extraction tube. The Soxhlet extraction residue remaining in the cylindrical filter after refluxing was vacuum dried, and the resulting residue was weighed to determine the amount of xylene insolubles. The xylene insolubles of components (A) and (B) are believed to be mainly composed of the coating film and talc.
[0119] Component (C): Propylene-Based Polymers As component (C), the following propylene-based polymers (C-1) and (C-2) were prepared.
[0120] (C-1) Heterophagic propylene polymer material MFR (temperature 230°C, load 2.16 kg): 27 g / 10 min Propylene homopolymer (polymer I): 80 mass% Ethylene-propylene random copolymer (polymer II): 20 mass%
[0121] The mass ratio XII of polymer II to the total mass of the heterophasic propylene polymer material was calculated from the following formula using the heat of crystalline fusion of polymer I and the entire heterophasic propylene polymer material: XII = 1 - (ΔHf)T / (ΔHf)P, where (ΔHf)T is the heat of fusion of the entire heterophasic propylene polymer material (polymer I and polymer II) (unit: cal / g), and (ΔHf)P is the heat of fusion of polymer I (unit: cal / g).
[0122] (C-2) Ethylene-propylene-random copolymer MFR (temperature 230°C, load 2.16 kg): 25 g / 10 min Ethylene content: 2.5 mass%
[0123] Component (D): Ethylene-α-olefin Copolymer As component (D), the following ethylene-α-olefin random copolymer (D-1) was prepared.
[0124] (D-1) Ethylene-1-octene random copolymer MFR (temperature 190 ° C., load 2.16 kg): 1.0 g / 10 min Density: 0.858 g / cm 3
[0125] <Production of Resin Compositions> (Examples 1 to 9 and Comparative Examples 1 to 4) The compositions shown in Table 1 were melt-kneaded in a single-screw extruder V40-NSIII type (cylinder inner diameter 40.0 mm, screw outer diameter 39.5 mm, L / D = 28) manufactured by Tanabe Plastics Co., Ltd. under conditions of a cylinder temperature of 230°C, a screw rotation speed of 40 rpm, a discharge rate of 7 kg / hr, no screen mesh, and a cylindrical breaker plate (outer diameter: 55.0 mm, inner diameter: 40.0 mm, length: 20.0 mm), to obtain pellet-shaped resin compositions.
[0126] Comparative Example 5 Melt kneading was carried out in the same manner as above, but strands could not be drawn by foaming from the die head, and a pellet-shaped resin composition could not be obtained.
[0127] Comparative Example 6 The composition shown in Table 1 was melt-kneaded using a single-screw extruder V40-NSIII type (cylinder inner diameter 40.0 mm, screw outer diameter 39.5 mm, L / D = 28) manufactured by Tanabe Plastics Co., Ltd. under the conditions of a cylinder temperature of 230°C, a screw rotation speed of 40 rpm, a discharge rate of 7 kg / hr, a screen mesh of 100 mesh, and a cylindrical breaker plate (outer diameter: 55.0 mm, inner diameter: 40.0 mm, length: 20.0 mm). However, since the mesh was clogged, a pellet-shaped resin composition could not be obtained.
[0128] <Production of injection-molded articles for evaluating the number of coatings on the surface of molded articles> The resin compositions obtained in Examples 1 to 9 and Comparative Examples 1 to 4 were dried at 110°C for 2 hours and then injection-molded under the following conditions to produce flat-plate injection-molded articles having a length of 400 mm, a width of 100 mm, a thickness of 3.0 mm, a textured design surface with a satin-finish texture and a texture depth of 100 μm. Injection molding machine: SE180D manufactured by Sumitomo Heavy Industries, Ltd. (clamping force 180 tons, cylinder diameter 50 mm) Cylinder temperature: 240°C Mold temperature: 80°C Injection speed: 200 mm / sec Cooling time: 30 sec
[0129] <Evaluation of the number of coating films on the surface of the molded article> An image of the obtained flat-plate-shaped molded article was captured using an Epson GT-X900 scanner, and the number of coating films on the surface of the molded article was then measured using image analysis software from Mitani Shoji Co., Ltd. under the following analysis conditions: Software: WinROOF2015 Analysis area: 90 mm x 269 mm Image adjustment: Brightness -25, contrast +75, median filter 3*3 Binarization: Automatic binarization, discrimination and sorting method, threshold value 20 to 255
[0130]
[0131] As can be seen from the results in Table 1, the resin compositions of each example that satisfy all of the constituent requirements of the present disclosure can increase the number of coating films visible from the outside while reusing polypropylene, thereby producing injection-molded articles with relatively excellent design. Furthermore, as can be seen from a comparison between Examples 8 and 9 and Comparative Example 1, by including component (C) in the resin composition in addition to component (A) and component (B), the number of coating films visible from the outside can be increased.
Claims
1. A resin composition comprising: component (A): crushed material of automobile-derived scrap bumpers containing 1% by mass or more and less than 30% by mass of xylene insolubles; component (B): peeled paint powder of automobile-derived scrap bumpers containing 30% by mass or more and less than 50% by mass of xylene insolubles; and component (C): a propylene-based polymer, wherein the content of component (A) is 15% by mass or more and 35% by mass or less, the content of component (B) is 15% by mass or more and 35% by mass or less, and the content of component (C) is 30% by mass or more and 70% by mass or less, relative to the total mass of the resin composition.
2. The resin composition according to claim 1, further comprising component (D): an ethylene-α-olefin copolymer, and the content of said component (D) is 5% by mass or more and 15% by mass or less based on the total mass of the resin composition.
3. The resin composition according to claim 1, wherein the component (B) contains titanium oxide, and the content of the titanium oxide is 0.05 mass % or more and 5 mass % or less based on the total mass of the component (B).
4. The resin composition according to claim 1, wherein the component (B) contains metallic aluminum, and the content of the metallic aluminum is 0.01 mass % or more and 1 mass % or less based on the total mass of the component (B).
5. The resin composition according to claim 1, wherein the component (B) contains talc, and the content of the talc is 5 mass % or more and 20 mass % or less based on the total mass of the component (B).
6. A method for producing a resin composition, comprising: a step of melt-kneading a mixture containing: component (A): crushed material of automobile-derived scrap bumpers containing 1% by mass or more and less than 30% by mass of xylene insolubles; component (B): paint peeled powder of automobile-derived scrap bumpers containing 30% by mass or more and less than 50% by mass of xylene insolubles; and component (C): a propylene-based polymer, without passing the mixture through a screen mesh; wherein the content of component (A) is 15% by mass or more and 35% by mass or less, the content of component (B) is 15% by mass or more and 35% by mass or less, and the content of component (C) is 30% by mass or more and 70% by mass or less, relative to the total mass of the mixture.
7. An injection molded article comprising the resin composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Recycling of resin product
JP1996309750A
Method for recycling plastic
JP2001353721A
Method for producing recycled resin product and resin component for car
JP2004058481A
Resin composition used for vehicle interior by using crushed material of vehicle bumper mingled with insoluble substance as raw material and molded article of the same
JP2005139421A