Sealing sheet and display
The sealing sheet with a resin composition layer and specific embeddability improvers addresses the challenges of embeddability and light resistance in micro LED displays, ensuring clear and durable performance by filling narrow spaces and resisting yellowing, thus improving micro LED display quality.
Patent Information
- Application Number
- PCT/JP2024/016323
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-21
AI Technical Summary
Existing sealing sheets for micro LED displays face challenges with embeddability and light resistance, as they struggle to fill the narrow spaces between micro-sized LED elements, leading to refracted light and reduced display clarity, and they yellow over time when exposed to sunlight, compromising image quality.
A sealing sheet with a resin composition layer containing a (meth)acrylic resin and an embeddability improver comprising a phosphorus-containing compound and a phenolic hydroxyl group-containing compound, which provides excellent embeddability, light resistance, adhesion to substrates, and zipping properties, ensuring clear and durable display performance.
The sealing sheet effectively fills the narrow spaces between micro LED elements, maintains display clarity, and resists yellowing, providing excellent embeddability, light resistance, and adhesion, thereby enhancing the manufacturing process and image quality of micro LED displays.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Encapsulating sheets and displays
[0001] The present disclosure relates to an encapsulating sheet, and more particularly to an encapsulating sheet including a resin composition layer for encapsulating a plurality of light-emitting elements used in various products such as electronic devices and displays, and a display having an encapsulating layer made of the resin composition layer.
[0002] In recent years, development of displays using various light-emitting elements has been actively pursued in order to further improve display performance. Specifically, various display specifications have been researched, such as backlit displays using liquid crystal or quantum dots, displays using self-emitting elements such as mini / micro LEDs and organic electroluminescence (EL), plasma displays, and electrophoretic displays, and a wide range of applications are being considered, from large display applications such as signage and televisions to small-sized applications such as tablets, personal computers, smartphones, and wearable devices. In particular, development of displays using LEDs is progressing at an increasing pace, and Patent Document 1 describes a thermosetting resin composition for encapsulating LED elements. Micro LED displays are attracting the most attention as a next-generation display technology.
[0003] Japanese Patent Application Laid-Open No. 2023-12051
[0004] Patent Document 1 describes a sheet-shaped resin composition for encapsulating optical semiconductor elements, which has excellent heat resistance. However, as LED elements have become increasingly miniaturized in recent years, the spacing between LED elements has become narrower, making it difficult for the sheet-shaped resin composition described in Patent Document 1 to fill the airspace (embedding) of micro-sized LED elements. If there is an airspace between the LED element and the encapsulating resin composition, light is refracted, resulting in a decrease in the clarity of the display. Furthermore, when displays are used outdoors, high light resistance is required. However, existing encapsulating sheets yellow over time when exposed to sunlight, causing the image displayed on the display to turn yellow. Therefore, an encapsulating sheet with excellent embedding and light resistance is needed to create displays that are clear and have minimal yellowing over time.
[0005] The present disclosure has been made in view of the above problems, and an object of the present disclosure is to provide an encapsulant sheet and a display having a resin composition layer that are excellent in embedding property and light resistance even when applied to a display using not only LED elements but also a plurality of various light-emitting elements such as organic EL as a light source. Another object of the present disclosure is to provide an encapsulant sheet that is excellent in adhesion to a substrate and zipping property from the viewpoint of simplifying the manufacturing process of a micro LED display.
[0006] As a result of intensive studies, the present inventors have found that the above-mentioned problems can be solved by the encapsulating sheet described below, and have completed the present inventions [1] to [8] below. [1]: An encapsulating sheet for encapsulating light-emitting elements used in a display using a plurality of light-emitting elements as a light source, the encapsulating sheet comprising a resin composition layer containing a resin (A) and an embeddability improver (B), the resin (A) having a glass transition temperature (Tg) of −30 to 40° C. and a weight average molecular weight (Mw) of 10,000 to 1,000,000, the embeddability improver (B) containing a phosphorus-containing compound (B1) and a phenolic hydroxyl group-containing compound (B2), and the resin composition layer having a thickness Ta of 1 to 100 μm. [2]: The encapsulating sheet according to [1], wherein the resin (A) is a (meth)acrylic resin (a), which is a copolymer having a structural unit derived from an acrylic acid alkyl ester (a1) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms and a structural unit derived from a methacrylic acid alkyl ester (a2) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms. [3]: The encapsulating sheet according to [2], wherein the (meth)acrylic resin (a) further contains a structural unit derived from (meth)acrylic acid (a3). [4]: The encapsulating sheet according to any one of [1] to [3], wherein the resin (A) is contained in an amount of 76 to 99.9% by mass relative to the total mass of the resin composition layer. [5]: The encapsulating sheet according to any one of [1] to [4], wherein the content of the embeddability improver (B) is 0.1 to 15% by mass relative to the total mass of the resin composition layer. [6]: The encapsulating sheet according to any one of [1] to [5], wherein a mass ratio B1:B2 of the phosphorus-containing compound (B1) to the phenolic hydroxyl group-containing compound (B2) in the embeddability improver (B) is 0.1:1 to 10:1. [7]: The encapsulating sheet according to any one of [1] to [6], wherein the resin composition layer has a loss tangent (tanδ40) at 40°C obtained by dynamic viscoelasticity measurement at a frequency of 10 Hz in a tensile mode of 0.8 to 2.0. [8]: A display having an encapsulating layer comprising the resin composition layer of the encapsulating sheet according to [7].
[0007] The present disclosure makes it possible to provide an encapsulating sheet that has excellent embeddability and light resistance even when applied to a display using a plurality of light-emitting elements as a light source. In addition to the above, the present disclosure also makes it possible to provide an encapsulating sheet that has excellent embeddability and light resistance, adhesion to a substrate, and zipping properties even when applied to a display using a micro LED element as a light source.
[0008] Fig. 1 is a schematic cross-sectional view showing an example of a layered structure of an encapsulating sheet. Fig. 2 is a schematic cross-sectional view showing another example of a layered structure of an encapsulating sheet. Fig. 3 is a schematic cross-sectional view showing another example of a layered structure of an encapsulating sheet. Fig. 4 is a schematic cross-sectional view showing a process of encapsulating light-emitting elements on a substrate having a plurality of light-emitting elements. Fig. 5 is a cross-sectional view showing an example of a test substrate simulating a substrate of a micro LED.
[0009] The present disclosure will be described in detail below. Note that the embodiment described below is an example of the present disclosure. The present disclosure is not limited to the following embodiment, and includes modifications implemented within the scope that does not change the gist of the present disclosure. In this specification, a numerical range specified using "to" includes the numerical values written before and after "to" as the lower and upper limit values of the range. (Meth)acrylic acid refers to acrylic acid and methacrylic acid. Furthermore, unless otherwise noted, the various components mentioned in this specification may each be used independently alone or in combination of two or more types.
[0010] In the present disclosure, when the weight average molecular weight (Mw) of the resin (A) is 10,000 or more and 1,000,000 or less, the glass transition temperature (Tg) of the resin (A) is -30°C to 40°C, the embeddability improver (B) contains a phosphorus-containing compound (B1) and a phenolic hydroxyl group-containing compound (B2), and the thickness Ta of the resin composition layer is 1 to 100 μm, light resistance and embeddability can be improved. Furthermore, adhesion and zipping resistance can also be improved. The inventor's speculations regarding the above effects are described in the following items.
[0011] [Configuration of Encapsulating Sheet] The encapsulating sheet of the present disclosure includes at least a resin composition layer. As shown in Fig. 1A, the encapsulating sheet can have a configuration in which a resin composition layer 2 and a release liner 4 are laminated. As shown in Fig. 1B, the encapsulating sheet may have a configuration in which the resin composition layer 2 is laminated with a substrate 3. The laminate structure of the resin composition layer and the substrate and / or the release liner is not particularly limited.
[0012] Examples of the release liner include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; plastic films such as polyolefin films such as polypropylene and polyethylene; and plastic sheets coated with a release agent such as silicone resin to provide a release layer. There are no particular restrictions on the thickness of the release liner, but it is generally about 10 to 200 μm.
[0013] The substrate is not particularly limited, but examples thereof include various optical films such as plastic films, antireflection (AR) films, polarizing plates, and retardation plates. Examples of the plastic films include polyvinyl chloride films, polyethylene films, polyethylene terephthalate (PET) films, polyurethane films, nylon films, polyolefin films, triacetyl cellulose films, and cycloolefin films. The thickness of the substrate is not particularly limited, but is preferably 10 to 2000 μm. Furthermore, the encapsulating sheet of the present disclosure preferably has a three-layer structure of substrate / resin composition layer / release liner.
[0014] As shown in FIG. 1C , the encapsulating sheet of the present disclosure particularly preferably has a three-layer structure of a first release liner 4a / resin composition layer 2 / second release liner 4b. The first and second release liners can be selected arbitrarily, and the same release liner may be used. From the viewpoint of handling, it is preferable that the first release liner be a light release liner and the second release liner be a heavy release liner. The thickness Tl of the light release liner is preferably in the range of 10 to 150 μm, and the thickness Th of the heavy release liner is preferably in the range of 25 to 200 μm, and it is preferable that the relationship Tl<Th is satisfied. Furthermore, when the encapsulating sheet is in a roll form, it is preferable that the light release liner be provided on the outer side of the roll. The release strength of the first and second release liners can be adjusted by a release treatment of the surface of each release liner that is attached to the resin composition layer. For example, it can be adjusted by the type of release agent, the amount of release agent applied, and the surface roughness of the release layer. To reduce the release strength, treatments such as increasing the surface roughness or the amount of release agent applied are effective, while to increase the release strength, the opposite can be done. When the three-layer structure shown in FIG. 1C is used, a preferred manufacturing method is to form a resin composition layer 2 on a second release liner 4b and then laminate the first release liner 4a thereon.
[0015] After or during the production of the encapsulating sheet, the encapsulating sheet is wound around a core into a roll to obtain an encapsulating sheet roll. The winding length can be designed depending on the application. From the viewpoint of increasing productivity, it is preferably 50 m or more, and more preferably 100 m or more. From the viewpoint of production yield, the winding length is preferably 10,000 m or less.
[0016] The encapsulating sheet of the present disclosure is preferably used to encapsulate light-emitting elements used in a display that uses multiple light-emitting elements as a light source. Examples of displays that use multiple light-emitting elements as a light source include displays that require high quality, such as organic EL display panels and micro LED display panels. The resin composition layer constituting the encapsulating sheet is preferably laminated in direct contact with an adherend. The adherend to be adhered is not particularly limited, but is preferably acrylic, urethane, polycarbonate, epoxy, polyimide, glass, paper, cloth, aluminum, ceramic, or polyethylene terephthalate. Furthermore, the adherend is more preferably a substrate having metal electrode portions or a substrate having multiple light-emitting element portions, such as a backlight module, LED, or organic EL. The substrate having multiple light-emitting element portions may further have a light-shielding layer between the light-emitting element portions.
[0017] The resin composition layer constituting the encapsulating sheet has high conformability to uneven surfaces, making it suitable for use in filling the spaces between multiple light-emitting elements. By filling the spaces between light-emitting elements with the resin composition layer, an encapsulating layer made of the resin composition layer is formed. The encapsulating layer functions to secure adjacent light-emitting elements and prevent them from falling off or becoming misaligned. In particular, since the resin composition layer of the encapsulating sheet of the present disclosure can conform to micro-sized light-emitting elements, micro-LEDs are more suitable as light-emitting elements, and it is more preferable to use the resin composition layer as an encapsulating layer for a micro-LED display panel. Micro-LEDs are tiny LED chips measuring 50 μm or less or 100 μm or less. By mounting multiple micro-LEDs (chips) on a substrate with wiring and circuits, a display using multiple light-emitting elements as a light source is formed. Micro-LEDs are formed from LED elements such as GaAs, GaP, AlGaInP, or InGaN, an encapsulating resin for encapsulating them, a package substrate, electrodes, etc., and operate at a temperature of 25 to 60°C. An example of a process for forming an encapsulating layer is described below with reference to FIG. 2.
[0018] Step (a): Step of placing encapsulating sheet As shown in an example in FIG. 2(a), the resin composition layer of the encapsulating sheet is placed on a substrate having a plurality of light-emitting elements so as to directly cover the light-emitting elements. When the encapsulating sheet has a first release liner and a second release liner, the first release liner is peeled off to expose the resin composition layer, and then the sheet is placed as described above. The second release liner may be peeled off immediately after placement, or may be peeled off after the pressing step described below. In this specification, the term "plurality of light-emitting elements" is not particularly limited as long as it refers to two or more light-emitting elements. In display applications, the number of light-emitting elements used is determined by the display size and the number of pixels. Furthermore, the light-emitting color of the light-emitting element is not particularly limited, and organic EL light-emitting elements and LED light-emitting elements can be used. Examples of colors that can be emitted include red, green, and blue. The size of the light-emitting element is a thickness of 100 μm or less and an area of 40,000 μm in plan view. 2 The thickness is preferably 50 μm or less and the area in plan view is 10,000 μm or less. 2 The following is more preferable: a thickness of 20 μm or less and an area in plan view of 2500 μm 2 The following are more preferred: The distance between light-emitting elements mounted on the substrate is, for example, 10 to 5000 μm. When a set of red, green, and blue light-emitting elements is mounted on the substrate as one pixel, the distance between pixels is, for example, 10 to 2000 μm, preferably 20 to 1800 μm, and more preferably 500 to 1500 μm. The distance between light-emitting elements in one pixel is, for example, 10 to 200 μm, preferably 10 to 100 μm, and more preferably 20 to 60 μm.
[0019] Step (b): Pressing Step As shown in FIG. 2(b), the resin composition layer is fluidized by pressing and filled around and between multiple light-emitting elements on the substrate. The resin composition layer filled around and between multiple light-emitting elements serves as a sealing layer. While the pressing method is not particularly limited, heat pressing and vacuum pressing are preferred. From the viewpoint of the filling property of the resin composition layer, the temperature during pressing is preferably 20 to 200°C, more preferably 30 to 150°C, even more preferably 40 to 130°C, and particularly preferably 60 to 110°C. To improve adhesion to the light-emitting elements and the adherend, further heat aging may be performed after pressing. The heating temperature is preferably 40 to 250°C, more preferably 80 to 220°C, and even more preferably 100 to 190°C. The heating time is preferably 30 to 300 minutes, more preferably 60 to 240 minutes, and even more preferably 90 to 180 minutes. By using the above heating temperature and heating time, residual stress in the resin composition layer can be removed and the adhesion surface can be smoothed. The heat aging may be carried out after the step (c) described below.
[0020] Step (c): Etching Step In step (c), etching is performed to remove or thin the sealing layer on the light-emitting element. Removing the sealing layer increases the brightness of the light-emitting element and ensures visibility during light emission. The thickness of the sealing layer after etching is preferably approximately the same as the thickness of the light-emitting element, as shown in FIG. 2(c-1), or less than the thickness of the light-emitting element, as shown in FIG. 2(c-2). It is not necessary to completely remove the sealing layer from the light-emitting element, as long as it is substantially removed, and some thin film may remain. Furthermore, if visibility can be ensured, step (c) may be omitted. The etching method is not particularly limited, but preferred examples include wet etching, such as chemical polishing using chemicals; physical polishing using an abrasive; laser etching; plasma etching using argon plasma or oxygen plasma; and dry etching, such as ion beam etching. To reduce surface irregularities, it is preferable to use a combination of wet etching and dry etching. Physical etching, such as plasma treatment, may also be used. Etching conditions include, for example, an anisotropic plasma device, CF 4 / O 2 / N2 Dry etching can be performed using a mixed gas of CF4 and CF5 under the conditions of an output of 1500 to 3000 W and a time of 180 to 600 seconds. 4 The gas supply rate is, for example, 50 to 100 sccm. 2 The gas supply rate is, for example, 500 to 1000 sccm, N 2 The gas supply rate may be set to, for example, 50 to 100 sccm.
[0021] As described above, the sealing layer can be formed from the resin composition layer through steps (a) to (c). Next, the components of the sealing sheet of the present disclosure will be described in detail while citing preferred examples.
[0022] [Resin Composition Layer] The resin composition layer contains a resin (A) and an embeddability improver (B), and preferably further contains a crosslinking agent, and may contain other components. In the present disclosure, the resin (A) is a substance that functions as a binder to bond and fix objects. Specific examples include the function of bonding and fixing a substrate having a light-emitting element or a plurality of light-emitting elements.
[0023] The loss tangent (tanδ40) at 40°C obtained by dynamic viscoelasticity measurement of the resin composition layer of the present disclosure is preferably 0.8 to 2.2, more preferably 1.0 to 2.0, and even more preferably 1.5 to 1.9. By setting the tanδ40 to 0.8 to 2.2, the diffusibility of the pressure applied to the resin composition layer during the pressing process is improved, resulting in improved embedding properties, adhesion to the adherend, and zipping properties. If the tanδ40 is lower than 0.8, the diffusibility of the resin composition layer during the pressing process is too high, making the resin composition layer prone to flow and thinning the edges of the sealing layer after the pressing process. If the tanδ40 is higher than 2.2, the diffusibility of the resin composition layer during the pressing process is too low, resulting in poor fluidity of the resin composition layer and the creation of an air space between the adherend and the sealing layer. The loss tangent (tanδ40) is the ratio of the loss modulus to the storage modulus obtained by dynamic viscoelasticity measurement in the tensile mode at a frequency of 10 Hz and -50 to 150°C. The tan δ40 can be adjusted by the type and composition of the resin (A). When the resin (A) contains the (meth)acrylic resin (a), the tan δ40 can be increased by increasing the content of the methacrylic acid alkyl ester (a2), and when a lower tan δ40 is desired, the same can be adjusted.
[0024] Furthermore, the peak top temperature (tanδ peak temperature) of the loss tangent (tanδ) obtained by dynamic viscoelasticity measurement of the resin composition layer of the present disclosure refers to the temperature at which the tanδ peak is maximum. When there are two or more peaks, it refers to the lowest peak temperature. The tanδ peak temperature is preferably between 0 and 60°C, more preferably between 15 and 55°C, and even more preferably between 35 and 45°C. By having a tanδ peak temperature of 0 to 60°C, the network structure of the molecular chains of the resin composition layer and the embeddability improver (B) can be stabilized after the heat aging process, and the residual stress of the resin can be sufficiently removed, thereby improving adhesion to the adherend. The tanδ peak temperature of the present disclosure can be adjusted by the type and composition of the resin (A), the type and amount of the crosslinking agent, the type and amount of the embeddability improver (B), and the amount of other components added. When the resin (A) contains a (meth)acrylic resin (a), the tan δ peak temperature can be increased by increasing the content of a monomer having a high homopolymer glass transition temperature (Tg); conversely, if a lower tan δ peak temperature is desired, the same can be adjusted. The glass transition temperature (Tg) of the homopolymer in this disclosure can be the value described in POLYMER HANDBOOK, 1999, FOURTH EDITION. Specific examples of monomers having a homopolymer glass transition temperature (Tg) of 0°C or higher include methyl acrylate, cyclohexyl acrylate, methyl methacrylate, and butyl methacrylate. Examples of monomers having a homopolymer glass transition temperature (Tg) of 0°C or lower include butyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, and 2-ethylhexyl methacrylate.
[0025] Furthermore, the peak top intensity (tan δ peak intensity) of the loss tangent (tan δ) obtained by dynamic viscoelasticity measurement of the resin composition layer of the present disclosure in the range of -50 to 80 °C refers to the value of the loss tangent (tan δ) when the tan δ peak is maximum. When there are two or more peaks, it refers to the top intensity of the peak at the lowest temperature. The tan δ peak intensity is preferably 0.8 to 2.2, more preferably 1.0 to 2.0, and even more preferably 1.5 to 1.9. By setting the tan δ peak intensity to 0.8 to 2.2, the resin composition layer is better able to absorb the pressure applied during the pressing process, forming a uniform encapsulating layer that conforms to the light-emitting element and improves embeddability. The tan δ peak intensity of the present disclosure can be adjusted by the type and composition of the resin (A). When the resin (A) contains a (meth)acrylic resin (a), the tan δ peak intensity can be lowered by increasing the content of the acrylic acid alkyl ester (a1). If a higher tan δ peak intensity is desired, the opposite can be achieved.
[0026] The dynamic viscoelasticity and loss tangent (tan δ) in the present disclosure were measured by the methods described in the Examples below. Note that when the resin composition layer contains a crosslinking agent, the crosslinking reaction due to heating is in an incomplete state at the time of measurement.
[0027] From the viewpoint of embeddability and zipping ability, the thickness Ta of the resin composition layer is 1 to 100 μm, preferably 3 to 50 μm, and more preferably 5 to 35 μm. By making the thickness Ta of the resin composition layer 1 μm or more, the stress generated when peeling off the release liner is efficiently dispersed, thereby exhibiting sufficient zipping ability. Furthermore, the pressure generated during the pressing process is diffused within the resin composition layer, thereby exhibiting sufficient embeddability. When the thickness Ta of the resin composition layer is 100 μm or less, the resin composition layer absorbs less pressure loss due to the pressure applied during the pressing process, allowing the resin composition layer to flow sufficiently, thereby exhibiting excellent embeddability. Furthermore, the stress applied to the resin composition layer when peeling off the release liner is less likely to be uneven, thereby exhibiting excellent zipping ability. When the thickness Ta of the resin composition layer is less than 1 μm, the pressure is not fully dispersed within the resin composition layer when the resin composition layer flows during the pressing process, which tends to cause unevenness, resulting in poor embeddability. Furthermore, the stress applied to the resin composition layer when the release liner is peeled off cannot be fully dispersed, resulting in poor zipping properties. If the thickness Ta of the resin composition layer is greater than 100 μm, the edges of the resin composition layer tend to flow when the resin composition layer flows during the pressing process, making the thickness of the resin composition layer non-uniform and causing a difference in applied pressure, resulting in poor embeddability. Furthermore, cohesive failure within the resin composition layer tends to occur, resulting in poor zipping properties. The resin composition layer may be in the form of a single layer or a laminate of two or more layers. The thickness Ta in the present disclosure was measured using the method described in the Examples below.
[0028] [Method for Forming Resin Composition Layer] The method for forming the resin composition layer is not particularly limited, but a suitable example is a method of forming a resin composition layer by coating a resin composition in which a solvent has been added to the components constituting the resin composition layer. The addition of the solvent is intended to adjust the viscosity level to a level suitable for coating. For coating, known coating machines and techniques such as a comma coater, die coater, roll coater, lip coater, reverse coater, gravure coater, bar coater, curtain coater, dip coating, spin coating, silk screen, and casting can be used. The solvent contained in the resin composition can be removed by a drying process after coating. In a preferred embodiment, the resin composition is applied to a support such as a release liner or substrate, and the coated film is then heated and dried using a hot air oven, infrared heater, or the like to form a resin composition layer on one side of the support. Furthermore, to increase the crosslink density of the resin composition layer, it is preferable to perform an aging treatment such as leaving the resin composition at rest under specific temperature conditions, or to irradiate it with UV light, for example.
[0029] [Resin Composition] The resin composition can be obtained by mixing a solvent, a resin (A), and an embeddability improver (B) while stirring. The optional solvent is used for the purpose of adjusting processing suitability, such as viscosity, when mixing the resin (A) and the embeddability improver (B). Therefore, any solvent compatible with the resin (A), such as an ester-based, ether ester-based, ether-based, alcohol-based, or aromatic solvent, can be used as appropriate. Specific examples of suitable solvents include acetone, 2-butanone, ethyl acetate, cyclohexanone, toluene, xylene, isopropyl alcohol, and N-methyl-2-pyrrolidone. A known stirring device can be used for stirring, and a disperser, mixer, shaker, homogenizer, or the like is preferred.
[0030] To obtain the resin composition, a two-stage or more manufacturing process may be employed, in which first, a mixture is prepared by mixing the embeddability improver (B) with the resin (A) and an optional solvent, and second, the resin (A), a crosslinking agent, and other components are added as necessary.
[0031] [Resin (A)] The resin (A) may be any of a thermosetting resin, a photocurable resin, and a thermoplastic resin, and may be used alone or in combination of two or more. From the viewpoint of embeddability, it is preferable to include at least one thermosetting resin. The thermosetting resin is a resin having multiple functional groups that can be used in a crosslinking reaction by heating, and may also have a self-crosslinkable functional group. The resin may also include a thermosetting monomer, but in this embodiment, from the viewpoint of coating film strength, it is preferable to use a thermosetting resin having a weight average molecular weight (Mw) of 10,000 or more.
[0032] Suitable examples of thermosetting resins include (meth)acrylic resin (a), maleic acid resin, polybutadiene resin, polyester resin, condensation polyester resin, addition polyester resin, melamine resin, urethane resin such as polyurethane resin or polyurethane urea resin, epoxy resin, polycarbonate resin, oxetane resin, phenoxy resin, polyimide resin, polyamideimide resin, alkyd resin, amino resin, polylactic acid resin, oxazoline resin, benzoxazine resin, silicone resin, fluororesin, etc. From the viewpoint of embeddability, it is preferable to contain at least one of (meth)acrylic resin (a), epoxy resin, urethane resin, polycarbonate resin, and polyamide resin. Furthermore, from the viewpoints of adhesion to the adherend and zipping properties, it is more preferable to contain (meth)acrylic resin (a). In addition, from the viewpoint of light resistance, it is particularly preferable to contain (meth)acrylic resin (a), which has high transparency and is resistant to oxidative degradation.
[0033] The functional group of the thermosetting resin may be appropriately selected depending on the combination with the crosslinking agent described below. Examples include hydroxyl groups, carboxyl groups, amino groups, epoxy groups, oxetanyl groups, oxazoline groups, oxazine groups, aziridine groups, thiol groups, isocyanate groups, blocked isocyanate groups, and silanol groups. From the viewpoint of compatibility with the embeddability improver (B), carboxyl groups, hydroxyl groups, and epoxy groups are preferred. When the thermosetting resin has a carboxyl group, the acid value of the thermosetting resin is preferably 1 to 50 mgKOH / g, more preferably 3 to 30 mgKOH / g, and even more preferably 5 to 20 mgKOH / g. By setting the acid value of the thermosetting resin to 1 mgKOH / g or more, the crosslink density with the crosslinking agent is optimized while maintaining good intermolecular forces with the adherend, improving light resistance, adhesion, and zipping properties. By setting the acid value of the thermosetting resin to 50 mgKOH / g or less, the intermolecular force with the substrate can be maintained well and the amount of carboxyl groups remaining after the crosslinking reaction, which promotes yellowing of the resin, can be appropriately controlled, thereby improving light resistance, adhesion, and zipping resistance. The acid value in this disclosure was measured by the method described in the Examples below.
[0034] In this disclosure, urethane resin is a general term for compounds containing two or more urethane bonds per molecule. Urethane resins can be obtained by reacting a polyisocyanate with a polyol. The polyisocyanate may be any polyisocyanate having two or more isocyanate groups per molecule. From the viewpoint of compatibility with the embeddability improver (B), a diisocyanate or triisocyanate is preferred, with a diisocyanate being more preferred. The diisocyanate may be appropriately selected from known aliphatic diisocyanates such as hexamethylene diisocyanate and known aromatic diisocyanates such as benzene-1,3-diisocyanate. Furthermore, an isocyanate-terminated prepolymer obtained by reacting a polyol with an excess amount of polyisocyanate may be used as an intermediate for the urethane resin. The polyol may be any polyol having two or more hydroxyl groups per molecule. From the viewpoint of compatibility with the embeddability improver (B), a diol or triol is preferred, with a diol being more preferred. The diol may be appropriately selected from known aliphatic diols such as ethylene glycol and known aromatic diols such as benzenediol. Prepolymers such as polyether polyols, polyester polyols, and polycarbonate polyols may also be used.
[0035] The urethane resin may be a polyurethane urea resin further having a urea bond. The polyurethane urea resin can be synthesized, for example, by reacting a urethane resin having an isocyanate group at the terminal with a polyamine. The polyamine may be any polyamine having two or more amino groups per molecule, and from the viewpoint of compatibility with the embeddability improver (B), a diamine or triamine is preferred, and a diamine is more preferred. The diamine can be appropriately selected from known aliphatic diamines such as ethylenediamine and known aromatic diamines such as phenylenediamine.
[0036] The photocurable resin may be any resin having one or more unsaturated bonds in one molecule that undergo a crosslinking reaction when exposed to light. Suitable examples of the photocurable resin include acrylic resin, maleic acid resin, polybutadiene resin, polyester resin, polyurethane resin, epoxy resin, oxetane resin, phenoxy resin, polyimide resin, polyamide resin, alkyd resin, amino resin, polylactic acid resin, oxazoline resin, benzoxazine resin, silicone resin, and fluororesin. The photocurable resin may also have a functional group that can be used for a crosslinking reaction when heated.
[0037] When the resin composition layer contains a photocurable resin, it preferably also contains an initiator. Examples of initiators that can be used include triazine-based photopolymerization initiators, borate-based photopolymerization initiators, carbazole-based photopolymerization initiators, acetophenone-based photopolymerization initiators, and oxime ester-based photopolymerization initiators. Among these, acetophenone-based photopolymerization initiators and oxime ester-based photopolymerization initiators are preferred because they cause less yellowing during the heat aging process. From the viewpoint of preventing yellowing, the initiator content is preferably 0.5 to 10% by mass, and more preferably 0.5 to 5% by mass, based on the total amount (100% by mass) of the resin composition layer.
[0038] Examples of thermoplastic resins include butyral resins, styrene-maleic acid copolymers, chlorinated polyethylene, chlorinated polypropylene, polyvinyl chloride, vinyl chloride-vinyl acetate copolymers, polyvinyl acetate, polyester resins, vinyl resins, alkyd resins, polystyrene resins, polyamide resins, rubber resins, cyclized rubber resins, celluloses, polyethylene (HDPE, LDPE), polybutadiene, and polyimide resins.
[0039] The weight-average molecular weight (Mw) of resin (A) is 10,000 to 1,000,000. From the viewpoint of light resistance and adhesion, a range of 25,000 to 300,000 is more preferable, and a range of 50,000 to 150,000 is even more preferable. By setting the weight-average molecular weight (Mw) to 10,000 or more, the molecular chain length is optimized, making it extremely easy to disentangle molecular chains during the heat aging process. This optimization allows for favorable conformability to the adherend, thereby improving adhesion. By setting the Mw to 1,000,000 or less, compatibility with the embeddability improver (B) is improved, preventing the effects of yellowing due to oxidative degradation caused by light exposure and improving light resistance. Furthermore, the ratio (Mw / Mn) of the number-average molecular weight (Mn) to the weight-average molecular weight (Mw), which indicates the degree of dispersion of resin (A), is preferably 1 to 5, more preferably 2 to 4.5, and even more preferably 2.5 to 4. By setting the Mw / Mn to 1 to 5, the flow rate when the resin is heated is made uniform within the resin, making it easier to control the fluidity of the resin and improving embeddability. Furthermore, the rate at which the resin wets the adherend is also made uniform, improving adhesion. The weight-average molecular weight (Mw) and number-average molecular weight (Mn) are values measured in terms of polystyrene using gel permeation chromatography (GPC). The weight-average molecular weight (Mw) and number-average molecular weight (Mn) in this disclosure were measured using the method described in the Examples below.
[0040] The glass transition temperature (Tg) of the resin (A) is -30°C to 40°C. From the viewpoints of light resistance, embeddability, and adhesion, -20°C to 30°C is more preferable, -10°C to 25°C is even more preferable, 0°C to 20°C is even more preferable, and 5°C to 15°C is particularly preferable. By setting the glass transition temperature (Tg) to -30°C or higher, the fluidity and wettability of the resin (A) in the pressing step can be made favorable, and embeddability and adhesion can be improved. Furthermore, in the heat aging step, a network structure of the resin (A) and the embeddability improver (B) is easily formed, improving light resistance. By setting the glass transition temperature (Tg) to 40°C or lower, when pressure is applied to the resin composition layer in the pressing step, the molecular motion of the resin (A) contained in the resin composition layer is activated, and entanglement of molecular chains becomes more likely to be loosened. When the molecular chain entanglements are loosened, the resin composition can deform to conform to uneven substrates, such as substrates and light-emitting elements, reducing the airspace between the light-emitting element and the resin composition layer, leading to improved embeddability. Furthermore, compatibility with the embeddability improver (B) is improved, preventing the effects of yellowing due to oxidative degradation caused by light and improving light resistance. Furthermore, during heat aging, the entanglement of the molecular chains in the resin composition layer and the coordination of the embeddability improver (B) are optimized, eliminating residual stress, smoothing the sealing layer and improving adhesion to the adherend. If the glass transition temperature (Tg) is lower than -30°C, the fluidity of the resin (A) becomes too high during the pressing process, resulting in an inconsistent thickness of the sealing layer and the resin at the edges of the sealing layer flowing and thinning, preventing the function of fixing the light-emitting element, resulting in poor adhesion and poor embeddability. Furthermore, during the heat aging process, it becomes difficult to form a network structure between the resin (A) and the embeddability improver (B), resulting in poor light resistance. If the glass transition temperature (Tg) is higher than 40° C., the fluidity of the resin (A) is low, making it difficult for the resin (A) to conform to the irregularities of the light-emitting element, resulting in poor embeddability. In addition, the wettability to the adherend is low, resulting in poor adhesion, and the compatibility between the embeddability improver (B) and the resin (A) becomes unstable, resulting in poor light resistance.
[0041] When the resin (A) contains a thermosetting resin or a photocurable resin, the glass transition temperature (Tg) of the resin (A) indicates the glass transition temperature (Tg) before heat curing or photocuring. The glass transition temperature (Tg) of the resin (A) in the present disclosure is measured by the method described in the examples below.
[0042] The content of resin (A) is preferably 76 to 99.9% by mass, more preferably 81 to 99% by mass, and even more preferably 86 to 95% by mass, based on the total amount (100% by mass) of the resin composition layer. When two or more types of resin (A) are contained, the content of each resin (A) is preferably 10% by mass or more, and the total content is preferably within the above-mentioned range. By setting the content of resin (A) to 76 to 99.9% by mass, light resistance, embeddability, adhesion, and zipping properties are improved. If the content of resin (A) is lower than 76% by mass, it is difficult to optimize the network structure of resin (A) and embeddability improver (B), resulting in poor light resistance. Furthermore, the embeddability improver (B) becomes less mobile during the pressing process, resulting in poor embeddability, and the intermolecular forces derived from resin (A) are weakened, resulting in poor adhesion and zipping properties.
[0043] [(Meth)acrylic resin (a)] In the present disclosure, the (meth)acrylic resin (a) is preferably an acrylic copolymer obtained by copolymerizing a (meth)acrylic acid ester monomer. A suitable example of the (meth)acrylic acid ester monomer is a (meth)acrylic acid alkyl ester monomer. When a crosslinked structure is formed, a (meth)acrylic copolymer obtained by copolymerizing a functional group-containing monomer and a (meth)acrylic acid ester monomer is preferred.
[0044] The (meth)acrylic acid alkyl ester monomer is a compound obtained by esterifying (meth)acrylic acid to introduce an alkyl group or a cycloalkyl group, and the alkyl group or cycloalkyl group may be any of a linear, branched, or cyclic saturated aliphatic hydrocarbon group. The saturated aliphatic hydrocarbon group is preferably a saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, and more preferably a saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, and (meth)acrylic acid. Examples of suitable acrylates include decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, 4-n-butylcyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. Among these, methyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate are particularly preferred from the viewpoint of compatibility with the embeddability improver (B).
[0045] The amount of the structural unit derived from the (meth)acrylic acid alkyl ester monomer relative to 100% by mass of the (meth)acrylic resin (a) is preferably 1 to 100% by mass, more preferably 20 to 99.9% by mass, and even more preferably 80 to 99.7% by mass.
[0046] The (meth)acrylic resin (a) preferably contains a functional group-containing monomer. Examples of the functional group-containing monomer include a carboxyl group-containing monomer, a hydroxyl group-containing monomer, an epoxy group-containing monomer, and an amino group-containing monomer. By containing the functional group-containing monomer, the cohesive strength of the resin (A) is improved, and a tough resin composition layer can be obtained.
[0047] Examples of carboxy group-containing monomers include (meth)acrylic acid, β-carboxyethyl (meth)acrylate, p-carboxybenzyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, citraconic acid, and isocrotonic acid. Among these, (meth)acrylic acid is particularly preferred from the viewpoint of adhesion.
[0048] Examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Among these, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are more preferred from the viewpoint of adhesion.
[0049] Examples of epoxy group-containing monomers include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 6-methyl-3,4-epoxycyclohexylmethyl (meth)acrylate.
[0050] Examples of amino group-containing monomers include (meth)acrylic acid monoalkylamino esters such as monomethylaminoethyl (meth)acrylate, monoethylaminoethyl (meth)acrylate, monomethylaminopropyl (meth)acrylate, and monoethylaminopropyl (meth)acrylate.
[0051] The total amount of structural units derived from functional group-containing monomers is preferably 0.1 to 20% by mass relative to 100% by mass of the (meth)acrylic resin (a). By adjusting the amount within this range, the cohesive strength can be adjusted by reaction with the crosslinking agent. The amount of structural units derived from carboxy group-containing monomers is preferably 0.1 to 10% by mass relative to 100% by mass of the (meth)acrylic resin (a). By adjusting the amount within this range, the adhesion to the adherend can be improved. Furthermore, the amount of structural units derived from hydroxyl group-containing monomers is preferably 0.1 to 10% by mass relative to 100% by mass of the (meth)acrylic resin (a). By adjusting the amount within this range, the adhesion to the adherend can be adjusted.
[0052] The (meth)acrylic resin (a) may contain structural units derived from other monomers copolymerizable with (meth)acrylic acid alkyl esters and functional group-containing monomers. Examples include monomers having an alkyleneoxy group and other vinyl monomers. Examples include methoxyethyl acrylate, methoxydiethylene glycol acrylate, vinyl acetate, vinyl crotonate, styrene, acrylonitrile, and acrylamide. The structural units derived from the other monomers preferably account for 0.1 to 20% by mass of 100% by mass of the (meth)acrylic copolymer.
[0053] A more preferred example of the (meth)acrylic resin (a) is a (meth)acrylic copolymer having one or more structural units derived from an acrylate alkyl ester (a1) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, and one or more structural units derived from a methacrylate alkyl ester (a2) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms. By including one or more structural units derived from an acrylate alkyl ester (a1) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, interaction with the adherend interface is more likely to occur in a short contact time, and gaps between the light-emitting element and the resin composition layer during embedding can be reduced, contributing to improved embeddability.
[0054] The (meth)acrylic resin (a) contains one or more structural units derived from a methacrylic acid alkyl ester (a2) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms, and therefore the (meth)acrylic resin (a) easily wets and spreads over the adherend interface over a long contact time, thereby reducing the gap between the light-emitting element and the resin composition layer during embedding and contributing to improved embeddability.
[0055] From the viewpoint of optimizing the interaction with the adherend interface in a short contact time and improving embeddability and adhesion, the alkyl acrylate ester (a1) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms is preferably an alkyl acrylate ester having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms, and more preferably an alkyl acrylate ester having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms. Furthermore, the saturated aliphatic hydrocarbon group of the alkyl acrylate ester (a1) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms is more preferably a linear or branched chain. From the viewpoint of improving embeddability and adhesion, the total mass of structural units derived from the acrylic acid alkyl ester (a1) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms is preferably 1 to 95 mass%, more preferably 5 to 70 mass%, and even more preferably 7 to 60 mass%, relative to 100 mass% of the (meth)acrylic resin (a).
[0056] From the viewpoint of optimizing wetting and spreading at the adherend interface over a long contact time and improving embeddability and adhesion, the methacrylic acid alkyl ester (a2) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms is preferably a methacrylic acid alkyl ester having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 4 carbon atoms. Furthermore, the saturated aliphatic hydrocarbon group of the methacrylic acid alkyl ester (a2) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms is more preferably linear or branched. From the viewpoint of improving embeddability and adhesion, the total mass of structural units derived from the methacrylic acid alkyl ester (a2) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms is preferably 1 to 95 mass%, more preferably 30 to 90 mass%, and even more preferably 35 to 85 mass%, relative to 100 mass% of the (meth)acrylic resin (a).
[0057] In the (meth)acrylic resin (a), the ratio of the total mass of structural units derived from the acrylic acid alkyl ester (a1) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms to the total mass of structural units derived from the methacrylic acid alkyl ester (a2) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms is preferably 1:0.4 to 1:20, more preferably 1:0.6 to 1:15, even more preferably 1:1 to 1:13, and particularly preferably 1:5 to 1:9. By adjusting the ratio to 1:0.4 to 1:20, light resistance is improved, intermolecular interactions within the (meth)acrylic resin (a) are optimized, and resin fluidity that provides good embeddability is achieved. Furthermore, the wettability of the (meth)acrylic resin (a) to the adherend is optimized, improving adhesion.
[0058] A more preferred example of the (meth)acrylic resin (a) is a (meth)acrylic copolymer containing, in addition to structural units derived from an acrylic acid alkyl ester (a1) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms and structural units derived from a methacrylic acid alkyl ester (a2) having a linear, branched, or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms, one or more structural units derived from (meth)acrylic acid (a3). The total mass of the structural units derived from (meth)acrylic acid (a3) is preferably 0.1 to 15 mass%, more preferably 0.3 to 10 mass%, and even more preferably 0.5 to 5 mass%, based on 100 mass% of the (meth)acrylic resin (a). A content of 0.1 to 15 mass% can enhance adhesion to the adherend through intermolecular interactions. Furthermore, from the viewpoint of enhancing adhesion to the adherend, it is more preferred that the (meth)acrylic acid (a3) is methacrylic acid.
[0059] A more preferred example of the functional group-containing monomer constituting the (meth)acrylic resin (a) is one in which the (meth)acrylic acid (a3) and the hydroxyl group-containing monomer are not simultaneously contained, which allows the cohesive strength of the (meth)acrylic resin (a) to be adjusted and the adhesion to be improved.
[0060] The (meth)acrylic resin (a) is obtained by polymerizing an acrylic monomer mixture. A polymerization initiator can be used during polymerization, if necessary. The content of the polymerization initiator is, for example, 0.01 to 10% by mass relative to 100% by mass of the monomer mixture. The polymerization method is not limited. For example, polymerization can be carried out by solution polymerization, bulk polymerization, emulsion polymerization, or suspension polymerization, with solution polymerization being particularly preferred due to ease of polymerization control. Examples of solvents used in solution polymerization include acetone, methyl acetate, ethyl acetate, toluene, xylene, anisole, methyl ethyl ketone, and cyclohexanone. The polymerization temperature can be, for example, 60 to 120°C, and the polymerization time can be approximately 2 to 12 hours.
[0061] The polymerization initiator is preferably a radical polymerization initiator. Suitable radical polymerization initiators include peroxides and azo compounds. Examples of azo compounds include 2,2'-azobisbutyronitriles such as 2,2'-azobisisobutyronitrile (AIBN) and 2,2'-azobis(2-methylbutyronitrile); 2,2'-azobisvaleronitriles such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile); 2,2'-azobispropionitriles such as 2,2'-azobis(2-hydroxymethylpropionitrile); and 1,1'-azobis-1-alkanenitriles such as 1,1'-azobis(cyclohexane-1-carbonitrile). Examples of peroxides include dialkyl peroxides such as di-t-butyl peroxide, dicumyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and 2,5-di(t-butylperoxy)hexyne-3; peroxy esters such as t-butyl peroxybenzoate, t-butyl peroxyacetate, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; ketone peroxides such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, and methylcyclohexanone peroxide; 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane; Examples of the peroxyketals include 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, and n-butyl-4,4-bis(t-butylperoxy)valerate; hydroperoxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, and 2,5-dimethylcyclohexane-2,5-dihydroperoxide; diacyl peroxides such as benzoyl peroxide, decanoyl peroxide, lauroyl peroxide, and 2,4-dichlorobenzoyl peroxide; and peroxydicarbonates such as bis(t-butylcyclohexyl)peroxydicarbonate.
[0062] [Embeddability Improver (B)] In the present embodiment, the embeddability improver (B) is a compound that improves the fluidity of the resin (A) and improves its embeddability between multiple light-emitting elements, and contains a phosphorus-containing compound (B1) and a phenolic hydroxyl group-containing compound (B2). The inclusion of both the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2) in the resin composition layer improves the embeddability. Additionally, they have the effect of improving light resistance, adhesion, and zipping resistance. The present inventors hypothesize the following mechanism. First, during the pressing process, the embeddability improver (B) moves freely enough to penetrate between the molecular chains of the resin (A), thereby severing the intermolecular interactions of the resin (A) and helping the resin (A) to uniformly loosen, thereby improving the fluidity and allowing the resin composition layer to deform to conform to the light-emitting elements. Thereafter, the phosphorus atom site of the phosphorus-containing compound (B1) weakly coordinates to the phenolic hydroxyl group site of the phenolic hydroxyl group-containing compound (B2) and penetrates into the molecular chain of the resin (A) having the weight-average molecular weight (Mw) specified in the present disclosure, forming a uniform network structure, suppressing further deformation of the resin composition layer and leading to improved embeddability. Furthermore, the intermolecular interactions of the resin (A) are suitably adjusted, resulting in good adhesion. Furthermore, the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2) have a radical trapping function, and the resin (A) and the embeddability improver (B) form a uniform network structure, thereby efficiently exhibiting the radical trapping function and improving light resistance. Furthermore, the intermolecular interactions between the adherend and the resin (A) are suitably adjusted, resulting in improved adhesion. Furthermore, the stress applied when peeling off the release liner is uniformly distributed, improving zipping properties.
[0063] The mass ratio B1:B2 of the phosphorus-containing compound (B1) to the phenolic hydroxyl group-containing compound (B2) in the embeddability improver (B) is preferably 0.1:1 to 10:1, more preferably 0.5:1 to 5:1, and even more preferably 1:1 to 3:1. By adjusting the mass ratio to 0.1:1 to 10:1, the molecular chains of the resin (A) and the embeddability improver (B) form a uniform network structure, improving embeddability. Furthermore, the radical trapping function of the embeddability improver (B) can be fully exerted, resulting in excellent light resistance. Furthermore, the coordination of the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2) is favorable, and the aggregation properties of the resin (A) are not inhibited, resulting in good zipping properties.
[0064] From the viewpoint of embeddability and adhesion, the content of the embeddability improver (B) is preferably 0.1 to 15 mass %, more preferably 0.3 to 10 mass %, and even more preferably 0.5 to 5 mass %, of the total amount (100 mass %) of the resin composition layer. By making it 0.1 to 15 mass %, embeddability, adhesion, light resistance, and zipping resistance are improved.
[0065] [Phosphorus-Containing Compound (B1)] The phosphorus-containing compound (B1) used in the present disclosure is not particularly limited as long as it contains phosphorus in the molecule, but is preferably one having a molecular weight of less than 10,000, more preferably 30 to 5,000, and even more preferably 30 to 2,000. Only one type of phosphorus-containing compound (B1) may be used, or two or more types may be used in combination. From the viewpoint of compatibility and embeddability, it is preferable to use one or more types of compounds that are solid at room temperature and one or more types of compounds that are liquid at room temperature in combination. Examples of the phosphorus-containing compound (B1) include tris(2-ethylhexyl)phosphite, tridecyl phosphite, trilauryl phosphite, tris(tridecyl)phosphite, tristearyl phosphite, phenyl isooctyl phosphite, phenyl isodecyl phosphite, phenyl di(tridecyl)phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl tridecyl phosphite, triphenyl phosphite, tricresyl phosphite, tris(nonylphenyl)phosphite, 4,4'isopropylidenediphenol alkyl phosphite, trisnonylphenyl phosphite, tris(dinonylphenyl)phosphite, tris(2,4-di-t-butylphenyl)phosphite, tris(biphenyl)phosphite, and bis(decyl)pentaerythritol diphosphite (also known as 3,9-bis( bis(tridecyl)pentaerythritol diphosphite (also known as 3,9-bis(tridecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), bis(tridecyl)pentaerythritol diphosphite (also known as 3,9-bis(tridecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), distearyl pentaerythritol diphosphite (also known as 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa -3,9-diphosphaspiro[5.5]undecane), di(nonylphenyl)pentaerythritol diphosphite (also known as 3,9-bis(nonylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), di(2,4-di-t-butylphenyl)pentaerythritol diphosphite (also known as 3,9-bis(2,4-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), di(2,6-di-t-butylphenyl)pentaerythritol diphosphite (also known as 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane), phenyl bisphenol A pentaerythritol diphosphite, tetratridecyl 4,4'-butylidenebis(3-methyl-6-t-butylphenol) diphosphite, hexatridecyl Suitable examples of suitable phosphate compounds include ethyl 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane triphosphite, 3,5-di-t-butyl-4-hydroxybenzyl phosphite diethyl ester, sodium bis(4-t-butylphenyl)phosphite, sodium 2,2-methylene-bis(4,6-di-t-butylphenyl)phosphite, 1,3-bis(diphenoxyphosphonyloxy)benzene, and ethyl bis(2,4-ditert-butyl-6-methylphenyl)phosphite. Other suitable phosphate compounds include oligomer-type compounds having a phosphite structure and a molecular weight of less than 10,000. In particular, compounds having a triphenyl phosphite skeleton, compounds having a trialkyl phosphite skeleton, compounds having a diphenyl monoalkyl phosphite skeleton, compounds having a monophenyl dialkyl phosphite skeleton, and compounds having a 2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane skeleton are preferred from the viewpoint of light resistance and embedding ability. The phenyl skeleton may contain a substituent such as t-butyl. More specifically, tris(2,4-di-t-butylphenyl)phosphite, tris(2-ethylhexyl)phosphite, bis(decyl)pentaerythritol diphosphite, bis(tridecyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, di(2,4-di-t-butylphenyl)pentaerythritol diphosphite, di(2,Di(2,6-di-t-butylphenyl)pentaerythritol diphosphite and phenyl bisphenol A pentaerythritol diphosphite are more preferred, and distearyl pentaerythritol diphosphite and di(2,6-di-t-butylphenyl)pentaerythritol diphosphite are even more preferred.
[0066] Specific examples of commercially available phosphorus-containing compounds (B1) include "ADEKA STAB PEP-8, PEP-36, C, TPP, HP-10, 135A, 1500, 2112, 2112RG, 3010, 1178, 4C, 24G, 2" manufactured by ADEKA Corporation, "IRGAFOS (registered trademark) 168, 168FF, 38, 126, P-EPQ, 12" manufactured by BASF Japan Ltd., "SUMILIZER (registered trademark) GP" manufactured by Sumitomo Chemical Co., Ltd., and "JP-360, JP-351, JP-3CP, JP-308E, JPE-308E, JP-310, JP-3" manufactured by Johoku Chemical Industry Co., Ltd. 12L, JP-333E, JPM-308, JPM-311, JPM-313, JPP-100, JA-805, JPH-1200, JPP-88, JPE-10, JPE-13R, JP-318E, JPP-2000PT, JP-650, JPH-3800, JC-356", Eiko Chemical Industries, Ltd. "Everaox (registered trademark) 168, 201, 202, 203, 204", Clariant Co., Ltd. "Hostanox (registered trademark) P-EPQ (registered trademark)", Fujifilm Wako Pure Chemical Industries, Ltd. "Ultranox (registered trademark) 626".
[0067] The content of the phosphorus-containing compound (B1) relative to the total amount (100% by mass) of the resin composition layer is preferably 0.05 to 10% by mass, more preferably 0.2 to 7% by mass, and even more preferably 0.4 to 6% by mass.
[0068] [Phenolic Hydroxyl Group-Containing Compound (B2)] The phenolic hydroxyl group-containing compound (B2) used in the present disclosure is a compound that contains a phenolic hydroxyl group in the molecule and does not contain phosphorus. The molecular weight is preferably less than 10,000, more preferably 94 to 5,000, and even more preferably 94 to 3,000. The phenolic hydroxyl group-containing compound (B2) may be used alone or in combination of two or more. Examples of the phenolic hydroxyl group-containing compound (B2) include 2,6-di-t-butylphenol, 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-4-ethylphenol, 2,6-di-t-butyl-4-s-butylphenol, 2,6-di-t-butyl-4-hydroxymethylphenol, pentaerythritol tetrakis[3-[3,5-di(tert-butyl)-4-hydroxyphenyl]propionate], thiodiethylenebis[ 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)-propionate, N,N'-(hexane-1,6-diyl)bis(3,5-di-tert-butyl-4-hydroxybenzenepropanamide), octyl 3-(4-hydroxy-3,5-diisopropylphenyl)propionate, 2,4-dimethyl-6-(1-methylpentadecyl)phenol 2,4,6-tris(4-hydroxy-3,5-di-tert-butylbenzyl)mesitylene, bis[[3,5-di(tert-butyl)-4-hydroxybenzyl]ethyl phosphonate]calcium, 2,4-bis(octylthiomethyl)-6-methylphenol, bis(3-tert-butyl-4-hydroxy-5-methylbenzenepropanoate)ethylenebis(oxyethylene), 1,6-hexanediol bis[3-(3,5-di-tert-butyl) tris[(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris[(3,5-di-tert-butyl-4-hydroxyphenyl)methyl]-1,3,5-triazinane-2,4,6-trione, 6-(4-hydroxy-3,5-di-tert-butylanilino)-2,4-bis(octylthio)-1,3,5-triazine, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 4,4',4''-(1-methylpropanyl-3-ylidene)tris(6-tert-butyl-m-cresol), 6,6'-di-tert-butyl-4,4'-butylidene-di-m-cresol, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene, and the like can be used. In particular, from the viewpoint of light resistance and embedding ability, phenolic hydroxyl group-containing compounds having a hindered skeleton in which two tert-butyl groups are bonded to the ortho-position of the phenolic hydroxyl group, or a semi-hindered skeleton in which one tert-butyl group is bonded to one of the ortho-positions of the phenolic hydroxyl group and one methyl group is bonded to the other, are preferred, and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene are more preferred.
[0069] Specific examples of commercially available products of the phenolic hydroxyl group-containing compound (B2) include "ADEKA STAB AO-20, AO-30, AO-40, AO-50, AO-50F, AO-50T, AO-60, AO-60G, AO-80, and AO-330" manufactured by ADEKA Corporation, and "KEMINOX" manufactured by Chemipro Chemicals. 9425, 179" manufactured by Sumitomo Chemical Co., Ltd. "SUMILIZER (registered trademark) GA-80, GM, GS, GA-80, MDP-S, WX-R, WX-RC, BBM-S" manufactured by BASF Japan Ltd. "IRGANOX (registered trademark) 1010, 1010FF, 1035, 1035FF, 1076, 1076FD, 1098, 1135, 1141, 1330, 1425WL, 1520L, 245, 245FF, 259, 3114, 565" manufactured by BASF Japan Ltd. "Yoshinox BB, 425" manufactured by Mitsubishi Chemical Corporation, and "Hostanox (registered trademark) O3, O310" manufactured by Clariant.
[0070] The content of the phenolic hydroxyl group-containing compound (B2) relative to the total amount (100% by mass) of the resin composition layer is preferably 0.04 to 5% by mass, more preferably 0.1 to 3.5% by mass, and even more preferably 0.2 to 3% by mass.
[0071] [Crosslinking Agent] The resin composition layer of the present disclosure may contain a crosslinking agent. In particular, when the resin (A) contains a thermosetting resin, it is preferable to use a crosslinking agent to promote the formation of a crosslinked structure. The crosslinking agents can be used alone or in combination of two or more. The crosslinking agent crosslinks with the reactive functional groups of the resin (A) during heat pressing or heat aging in the pressing process, thereby strengthening adhesion to an adherend such as a light-emitting element. Furthermore, the crosslinking agent can increase the cohesive strength of the resin composition layer, thereby improving zipping properties. The crosslinking agent has multiple functional groups reactive with the functional groups of the resin (A). Examples of crosslinking agents include known compounds such as silane coupling agents, epoxy compounds, acid anhydride group-containing compounds, imidazole compounds, isocyanate compounds, aziridine compounds, and amine compounds. From the viewpoint of adjusting the loss tangent (tan δ) of the resin composition layer, silane coupling agents, epoxy compounds, aziridine compounds, imidazole compounds, and isocyanate compounds are preferred, and epoxy compounds are more preferred.
[0072] The epoxy compound is a compound having two or more epoxy groups per molecule. Regarding the properties of the epoxy compound, using a liquid epoxy compound can lower the tan δ peak temperature of the resin composition layer, thereby enabling good adhesion between the light-emitting element and the resin composition layer. On the other hand, using a solid epoxy compound can increase the tan δ peak temperature of the resin composition layer, control the stickiness of the resin composition layer, and adjust the zipping properties. Examples of preferred epoxy compounds include glycidyl ether-type epoxy compounds, glycidyl amine-type epoxy compounds, glycidyl ester-type epoxy compounds, and cyclic aliphatic (alicyclic) epoxy compounds. Furthermore, from the viewpoint of light resistance, it is more preferred that the epoxy compound be a high-purity hydrogenated epoxy resin.
[0073] Examples of glycidyl ether epoxy compounds include cresol novolac epoxy compounds, tris(glycidyloxyphenyl)methane, and tetrakis(glycidyloxyphenyl)ethane. Examples of glycidylamine epoxy compounds include tetraglycidyldiaminodiphenylmethane and tetraglycidylmeta-xylylenediamine.
[0074] Examples of the glycidyl ester type epoxy compound include diglycidyl phthalate, diglycidyl hexahydrophthalate, and diglycidyl tetrahydrophthalate.
[0075] Examples of cyclic aliphatic (alicyclic) epoxy compounds include epoxycyclohexylmethyl-epoxycyclohexanecarboxylate, bis(epoxycyclohexyl)adipate, and the like.
[0076] Examples of the aziridine compound include trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, and 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane.
[0077] Imidazole compounds include 2-methylimidazole, 2-phenyl-4-methylimidazole, 2,4-dimethylimidazole, 2-phenylimidazole, imidazole, 2-undecylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]- Examples of imidazole compounds include ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. Further examples include compounds with improved storage stability, such as a type insoluble in a solvent obtained by reacting an imidazole compound with an epoxy resin, or a type in which an imidazole compound is encapsulated in microcapsules.
[0078] The isocyanate compound is an isocyanate having two or more isocyanate groups. Examples of the isocyanate compound include isocyanate monomers such as aromatic polyisocyanates, aliphatic polyisocyanates, araliphatic polyisocyanates, and alicyclic polyisocyanates, as well as biuret, nurate, and adduct forms thereof.
[0079] Examples of aromatic polyisocyanates include 1,3-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, 2,4,6-triisocyanate toluene, 1,3,5-triisocyanate benzene, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, and 4,4',4"-triphenylmethane triisocyanate.
[0080] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (also known as HDI), pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.
[0081] Examples of the aromatic aliphatic polyisocyanate include ω,ω'-diisocyanate-1,3-dimethylbenzene, ω,ω'-diisocyanate-1,4-dimethylbenzene, ω,ω'-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylxylylene diisocyanate, and 1,3-tetramethylxylylene diisocyanate.
[0082] Examples of alicyclic polyisocyanates include 3-isocyanatemethyl-3,5,5-trimethylcyclohexyl isocyanate (also known as IPDI, isophorone diisocyanate), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,4-bis(isocyanatemethyl)cyclohexane.
[0083] The biuret compound is a self-condensation product having a biuret bond formed by self-condensation of an isocyanate monomer, such as a biuret compound of hexamethylene diisocyanate.
[0084] The nurate derivative is a trimer of an isocyanate monomer, such as a trimer of hexamethylene diisocyanate, a trimer of isophorone diisocyanate, or a trimer of tolylene diisocyanate.
[0085] The adduct is a bifunctional or higher isocyanate compound obtained by reacting an isocyanate monomer with a bifunctional or higher low-molecular-weight active hydrogen-containing compound. Examples of the adduct include a compound obtained by reacting trimethylolpropane with hexamethylene diisocyanate, a compound obtained by reacting trimethylolpropane with tolylene diisocyanate, a compound obtained by reacting trimethylolpropane with xylylene diisocyanate, a compound obtained by reacting trimethylolpropane with isophorone diisocyanate, and a compound obtained by reacting 1,6-hexanediol with hexamethylene diisocyanate.
[0086] The isocyanate compound is preferably a trifunctional isocyanate compound from the viewpoint of forming a sufficient crosslinked structure. The isocyanate compound is more preferably an adduct or nurate, which is a reaction product of an isocyanate monomer and a trifunctional low-molecular-weight active hydrogen-containing compound. The isocyanate compound is preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a nurate of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, a nurate of tolylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, or a nurate of isophorone diisocyanate, and more preferably a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of tolylene diisocyanate, or a trimethylolpropane adduct of isophorone diisocyanate.
[0087] In the present disclosure, from the viewpoint of the coating film resistance to scratches, it is preferable to contain two or more types of crosslinking agents. From the viewpoint of adjusting the loss tangent (tan δ) of the resin composition layer, specific preferred examples include two or more types selected from a silane coupling agent, an epoxy compound, an aziridine compound, and an isocyanate compound, and more preferred examples include a combination of one or more of a silane coupling agent, an epoxy compound, an aziridine compound, and an isocyanate compound with an epoxy compound of a different type from the epoxy compound.
[0088] The content of the crosslinking agent (total content when two or more types are used in combination) is preferably 0.01 to 30% by mass, more preferably 0.05 to 20% by mass, and even more preferably 0.1 to 10% by mass, based on the total amount (100% by mass) of the resin composition layer. By setting the content within the above range (0.01 to 30% by mass), the compatibility, embeddability, and zipping properties of the embeddability improver (B) can be suitably adjusted.
[0089] [Other Components] The resin composition layer of the present disclosure may contain other components as long as the object of the present disclosure is not impaired. For example, inorganic fillers, colorants, dispersants, surface conditioning additives, curing accelerators, curing retarders, softeners, antistatic agents, lubricants, antiblocking agents, adhesion improvers, etc. may be added. From the viewpoint of controlling the film properties such as the diffusivity, reflectivity, light-blocking properties, and viscoelasticity of the resin composition layer, it is preferable to include inorganic fillers, dispersants, surface conditioning additives, curing accelerators, curing retarders, and adhesion improvers.
[0090] Examples of inorganic fillers include inorganic compounds that do not contain phosphorus, such as silica, alumina, magnesium hydroxide, barium sulfate, calcium carbonate, titanium oxide, zinc oxide, antimony trioxide, magnesium oxide, talc, kaolinite, mica, basic magnesium carbonate, sericite, montmorillonite, kaolinite, bentonite, boron nitride, aluminum nitride, and titanium nitride. Among these, from the viewpoint of coating film resistance to scratches, titanium oxide, titanium nitride, silica, talc, mica, kaolinite, or montmorillonite is preferred, and titanium oxide, titanium nitride, and silica are more preferred. In the present disclosure, from the viewpoint of coating film resistance, two or more types of inorganic fillers may be contained. Specifically, a preferred example is a combination of silica and one or more types selected from titanium oxide, titanium nitride, silica, talc, mica, kaolinite, and montmorillonite.
[0091] From the viewpoint of embeddability, the content of the inorganic filler (total content when two or more types are included) is preferably 0.01 to 10 mass %, and more preferably 0.1 to 5 mass %, based on the total amount (100 mass %) of the resin composition layer. By including 0.01 to 10 mass % of the inorganic filler, the effect of increasing the fluidity of the resin composition layer in the pressing step is easily exhibited, and embeddability is improved.
[0092] The average primary particle size (hereinafter referred to as particle size) of the inorganic filler is preferably 1 to 100 nm. By making the particle size 1 nm or more, it is easy to maintain the viscosity of the resin composition at a level suitable for coating. Furthermore, by making the particle size 100 nm or less, the coating film resistance is improved. The particle size of the inorganic filler can be determined from the average value of approximately 20 primary particles observed in an image magnified approximately 50,000 to 1,000,000 times using a transmission electron microscope (TEM).
[0093] The inorganic filler can also be dispersed in the resin (A) by mechanical crushing. It is preferable to use a dispersant for the dispersion treatment. In the present disclosure, the dispersant has the function of imparting repulsive forces between particles so that the particles divided through the dispersion treatment described above do not re-aggregate. Conventionally known compounds can be used as the dispersant, such as polymeric dispersants, pigment derivative dispersants, or compounds containing no phenolic hydroxyl groups or phosphorus among surfactants selected from cationic, anionic, or nonionic surfactants. The weight-average molecular weight (Mw) of these dispersants can be, for example, approximately 1,000 to 9,999.
[0094] Examples of surface conditioning additives include silicone-based, silicone acrylic, acrylic, fluorine-based, and acetylene glycol-based surfactants with a weight-average molecular weight (Mw) of 1,000 to 9,999, and compounds that do not contain phenolic hydroxyl groups or phosphorus. Among these, silicone-based and silicone acrylic surfactants are particularly preferred from the viewpoint of adhesion to the substrate. Preferred examples of silicone-based surface conditioning additives include modified polysiloxane compounds in which organic groups have been introduced into some of the methyl groups of polydimethylsiloxane. Examples of modifications include, but are not limited to, polyether-modification, methylstyrene-modification, alcohol-modification, alkyl-modification, aralkyl-modification, fatty acid ester-modification, epoxy-modification, amine-modification, amino-modification, and mercapto-modification. These modification methods can be used in combination. Among these, polyether-modified polysiloxane compounds and aralkyl-modified polysiloxane compounds are preferred in terms of compatibility, etc. As the silicone acrylic surface conditioning additive, for example, a siloxane-modified acrylic resin, which is a graft copolymer of an acrylic resin and a siloxane compound, is preferred from the viewpoint of compatibility, etc. From the viewpoint of coating suitability, the content of the surface conditioning additive is preferably 0.01 to 10% by mass, and more preferably 0.1 to 5% by mass, based on the total amount (100% by mass) of the resin composition layer.
[0095] The resin composition layer of the present disclosure preferably contains a curing accelerator to adjust the crosslinking rate, physical properties of the resin composition layer, etc. The curing accelerator is not particularly limited and can be selected appropriately. Specific examples of the curing accelerator include amine-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. These may be used alone or in combination of two or more. From the viewpoint of coating suitability, the content of the curing accelerator is preferably 0.01 to 10% by mass, and more preferably 0.1 to 5% by mass, based on the total amount (100% by mass) of the resin composition layer.
[0096] Examples of adhesion improvers include oligomers having a weight-average molecular weight (Mw) of 1,000 to 9,999 that do not contain phenolic hydroxyl groups or phosphorus. Examples include acrylic resins, urethane acrylic resins, rosin resins, terpene resins, alicyclic petroleum resins, and aromatic petroleum resins. The weight-average molecular weight (Mw) of the adhesion improver is more preferably 2,000 to 8,000, and even more preferably 3,000 to 5,000. From the viewpoints of adhesion to the adherend and zipping properties, the content of the adhesion improver is preferably 0.1 to 20% by mass, and more preferably 1 to 15% by mass, based on the total amount (100% by mass) of the resin composition layer.
[0097] Hereinafter, the present disclosure will be specifically described with reference to examples and comparative examples, but the present disclosure is not particularly limited to the examples. In the following description, "parts" and "%" represent "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0098] The values determined in this example were obtained by the following method. [Glass transition temperature (Tg) of resin (A)] A coating solution of resin (A) was applied to the release layer of a 75 μm thick second release liner (manufactured by Mitsui Chemicals Tohcello, Inc., SP-PET-O3) so that the dry thickness would be 25 μm. After drying for 3 minutes in a hot air oven at 100°C, the release layer side of a 50 μm thick first release liner (manufactured by Mitsui Chemicals Tohcello, Inc., SP-PET-O1) was laminated to the resin (A) side. The first and second release liners were then peeled off, and the Tg of the resulting resin (A) was measured using a differential scanning calorimeter (manufactured by TA Instruments, "Discovery DSC 2500"). Approximately 2 mg of the sample was placed in an aluminum pan, weighed, and set in a differential scanning calorimeter. Using an aluminum pan of the same type but without the sample as a reference, the pan was held at 100°C for 5 minutes and then rapidly cooled to -50°C using liquid nitrogen. Thereafter, the temperature was increased at a rate of 5°C / min, and the glass transition temperature (Tg) of the resin (A) was determined from the obtained DSC chart.
[0099] [Weight average molecular weight (Mw) and number average molecular weight (Mn)] The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured using a GPC "LC-GPC system" manufactured by Shimadzu Corporation, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were determined by conversion using polystyrene of known molecular weight as a standard substance. Apparatus name: LC-GPC system "Prominence" manufactured by Shimadzu Corporation Column: Four GMHXL columns manufactured by Tosoh Corporation and one HXL-H column manufactured by Tosoh Corporation were connected. Mobile phase solvent: tetrahydrofuran Flow rate: 1.0 mL / min Column temperature: 40°C
[0100] [Solid content] The mass of the aluminum cup (W0) was measured using a precision balance. Next, approximately 1 g of each sample was placed in the aluminum cup, and the mass of the sample in the aluminum cup (W1) was measured using a precision balance. The sample in the aluminum cup was heated in an oven at 150°C for 120 minutes, then removed from the oven and returned to room temperature. The residual mass (W2) of the sample in the aluminum cup after heating was measured using a precision balance. The solid content was then calculated using the formula (W2 - W0) / (W1 - W0) × 100 (%).
[0101] [Acid Value] Here, the "acid value" represents the acid value per 1 g of the solid content of the resin (A), and was determined by potentiometric titration in accordance with JIS K 0070.
[0102] [Resin (A)] [Production Example of (Meth)acrylic Resin (a) (R-1)] A reaction vessel (hereinafter simply referred to as "reaction vessel") equipped with a stirrer, thermometer, reflux condenser, dropping device, and nitrogen inlet tube was charged with 80 parts of ethyl acetate, 35 parts of methyl acrylate, 34.4 parts of 2-ethylhexyl acrylate, 30 parts of 2-ethylhexyl methacrylate, 0.3 parts of acrylic acid, 0.3 parts of hydroxybutyl acrylate, and 0.1 parts of 2,2'-azobisisobutyronitrile as an initiator, and the atmosphere inside the reaction vessel was replaced with nitrogen gas. Thereafter, the mixture was heated to 65°C while stirring under a nitrogen atmosphere to initiate the reaction. The reaction solution was then reacted at 65°C for 4 hours. After completion of the reaction, the reaction mixture was cooled and diluted with ethyl acetate to obtain a solution of (meth)acrylic resin (a) (R-1) having a weight average molecular weight (Mw): 20,000, a dispersity (Mw / Mn): 2, a glass transition temperature (Tg): −32° C., an acid value: 2 mgKOH / g, and a solids content: 25%.
[0103] [Production Examples of (Meth)acrylic Resins (a) (R-2 to R-12)] (Meth)acrylic resins (a) (R-2 to R-12) were produced in the same manner as in the production of (meth)acrylic resin (a) (R-1), except that the compositions and blending amounts (parts by mass) were changed to those shown in Table 1. Note that blank spaces indicate that no blending was performed, and the solid content was 25% in all cases.
[0104]
[0105] The abbreviations in the table are as follows: [Acrylic acid alkyl esters (a1)] MA: methyl acrylate (saturated aliphatic hydrocarbon group with 1 carbon atom) BA: n-butyl acrylate (saturated aliphatic hydrocarbon group with 4 carbon atoms) HA: hexyl acrylate (saturated aliphatic hydrocarbon group with 6 carbon atoms) CHA: cyclohexyl acrylate (saturated aliphatic hydrocarbon group with 6 carbon atoms) 2EHA: 2-ethylhexyl acrylate (saturated aliphatic hydrocarbon group with 8 carbon atoms) LA: lauryl acrylate (saturated aliphatic hydrocarbon group with 12 carbon atoms) [Methacrylic acid alkyl esters (a2)] MMA: methyl methacrylate (saturated aliphatic hydrocarbon group with 1 carbon atom) nBMA: n-butyl methacrylate (saturated aliphatic hydrocarbon group with 4 carbon atoms) 2EHMA: 2-ethylhexyl methacrylate (saturated aliphatic hydrocarbon group with 8 carbon atoms) [(Meth)acrylic acid (a3)] AA: acrylic acid MAA: methacrylic acid [Others] 4HBA: hydroxybutyl acrylate
[0106] [Production Example of Urethane Resin (R-13)] 166 parts of terephthalic acid, 146 parts of adipic acid, 212 parts of 3-methyl-1,5-pentanediol, and 25 parts of ethylene glycol were charged into a glass flask equipped with a stirrer, thermometer, reflux condenser, nitrogen inlet tube, and pressure reducing equipment, and the mixture was stirred while passing nitrogen gas through. The temperature was gradually raised under normal pressure, and the mixture was reacted at 200 to 230°C for approximately 8 hours to obtain a liquid with an acid value of 43 mgKOH / g. Next, 0.01 parts of tetra-n-butoxytitanium was charged, and after nitrogen substitution, the mixture was stirred at 180°C for 30 minutes in a sealed container. The mixture was then reacted at 230°C and 5 mmHg for 2 hours to obtain a polyester diol with an acid value of 1.1 mgKOH / g, a hydroxyl value of 114.2 mgKOH / g, a weight average molecular weight (Mw): 982, and a color of 10 (APHA method, the same applies below). Next, 734 parts of the polyester diol, 23.9 parts of dimethylolpropionic acid, 219 parts of toluene diisocyanate, and 242 parts of toluene were charged into a reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping device, and nitrogen inlet tube, and the mixture was allowed to react for 8 hours at 50°C under a nitrogen atmosphere. 1,200 parts of toluene was added to the mixture to obtain a solution of a urethane prepolymer having an isocyanate group at its terminal. The resulting prepolymer solution was then heated to 70°C, and while maintaining that temperature, a solution containing 20.0 parts of 1,3-diaminopropane, 3.1 parts of benzylamine, 600 parts of 2-propanol, and 961 parts of toluene was added dropwise over 1 hour. After completion of the dropwise addition, the mixture was allowed to react for an additional 6 hours at 70°C, thereby obtaining a solution of urethane resin (R-13) having a weight average molecular weight (Mw): 150,000, a dispersity (Mw / Mn): 4.5, a glass transition temperature (Tg): 18°C, an acid value: 10 mgKOH / g, and a solids content: 25%.
[0107] [Example 1] [Production Example of Resin Composition] As the resin (A), 374 parts of the solution of the aforementioned (meth)acrylic resin (a) (R-2) (93.5 parts of resin (A), 280.5 parts of solvent), as the embeddability improver (B), 1 part of ADK STAB PEP-36, which is a phosphorus-containing compound (B1), 0.5 parts of AO-80, which is a phenolic hydroxyl group-containing compound (B2), 5 parts of the epoxy-based crosslinking agent jER (registered trademark) YX8034 (manufactured by Mitsubishi Chemical Corporation), which is a crosslinking agent as other components, and 55 parts of 2-butanone as a solvent were sequentially added while stirring with a disper, and stirred until sufficiently uniform. Next, filtration was performed using a membrane filter with a pore size of 10 μm to remove coarse foreign matter that may cause coating unevenness, and a resin composition with a non-volatile content of 23% was obtained. The embeddability improver (B) and other components were expressed as solid content equivalents.
[0108] [Production Example of Encapsulating Sheet] The resin composition was applied onto the release layer of a 75 μm-thick second release liner (manufactured by Mitsui Chemicals Tohcello, Inc., SP-PET-O3) so that the thickness after drying would be 25 μm, and a resin composition layer was formed by drying for 3 minutes in a hot air oven at 100° C. Next, the release layer side of a 50 μm-thick first release liner (manufactured by Mitsui Chemicals Tohcello, Inc., SP-PET-O1) was attached to the exposed resin composition layer, and aging was performed at 0° C. for 7 days to obtain an encapsulating sheet of Example 1 in which the first release liner / resin composition layer / second release liner were laminated in this order.
[0109] [Thickness Tt of Encapsulating Sheet, Thickness Ta of Resin Composition Layer, Thickness Tl of First Release Liner, Thickness Th of Second Release Liner] Ten equally spaced positions were determined from one end to the other end in the width direction of an encapsulating sheet cut to a size of 10 cm x 10 cm, and the thicknesses of the ten positions were measured, and the average value was defined as the thickness Tt of the encapsulating sheet. Next, the first release liner was peeled from the encapsulating sheet, and the thicknesses of the peeled first release liner were measured at 10 positions corresponding to the same positions as above. The average value was defined as Tl. Thereafter, the second release liner was further peeled from the resin composition layer, and the thicknesses of the peeled second release liner were measured at 10 positions corresponding to the same positions as above. The average value was defined as Th. The thickness Ta of the resin composition layer was calculated using the following (Equation 1). The thickness was measured using an MH-15M (manufactured by Nikon Corporation). Ta = Tt - Tl - Th (Equation 1)
[0110] [Loss Tangent (tan δ) of Resin Composition Layer] In the above-described production example of the encapsulating sheet, an encapsulating sheet separately prepared so that the thickness after drying would be 50 μm was cut to a size of 0.5 cm × 2 cm, the first release liner and the second release liner were peeled off, and the resulting resin composition layer was measured for dynamic viscoelasticity using a dynamic viscoelasticity measuring device DVA-200 / L2 (manufactured by IT Measurement & Control Co., Ltd.) at a frequency of 10 Hz, a measurement temperature range of −50 to 150 ° C., a heating rate of 5 ° C. / min, and in tensile mode, and the loss tangent (tan δ) was plotted. From the obtained graph, the loss tangent at 40 ° C. (tan δ40), the peak top temperature of the loss tangent (tan δ) (tan δ peak temperature), and the peak top intensity of the loss tangent (tan δ) (tan δ peak intensity) were read.
[0111] [Evaluation Methods and Criteria] [Light Resistance] The encapsulating sheet was cut into 2 cm x 5 cm pieces, and a 1.1 mm thick glass plate (blue plate glass, manufactured by Kawamura Hisazo Shoten Co., Ltd.) was attached to the surface from which the first release liner had been peeled off, and the sheet was heat-pressed (100 ° C., 5 MPa, 5 minutes) for 5 minutes to bond the sheet to the resin composition layer. Furthermore, the second release liner of the encapsulating sheet was peeled off, and the test piece consisting of the glass plate and the resin composition layer was left standing for 120 minutes under 180 ° C. conditions, thereby adhering the glass plate and the resin composition layer to each other. Next, using a UV-visible spectrophotometer V-570 manufactured by JASCO Corporation, the spectral transmittance at 380 nm of the resin composition layer on the glass plate was measured, and the obtained value was taken as the initial transmittance. The resin composition layer on the glass plate was placed on a xenon weather meter XL75 manufactured by Suga Test Instruments Co., Ltd., and exposed for 300 hours under conditions of a black panel temperature of 50 ° C. and an irradiation dose of 100,000 Lux. After exposure, the spectral transmittance at 380 nm was measured in the same manner as the initial transmittance, and the obtained value was taken as the transmittance after exposure. The change in transmittance was calculated using the formula "|Initial transmittance - Transmittance after exposure| = Change in transmittance". The evaluation criteria were as follows, with A to C being rated as good. A: Change in transmittance less than 0.2 B: Change in transmittance 0.2 or more but less than 0.4 C: Change in transmittance 0.4 or more but less than 0.6 D: Change in transmittance 0.6 or more
[0112] [Embeddability] A glass substrate (size: 1 cm x 1 cm, recess width: 20 μm, protrusion height: 20 μm, protrusion width: 20 μm) was prepared with an uneven surface simulating the unevenness of a micro LED substrate. A schematic cross-sectional view of the test substrate is shown in FIG. 3 . The encapsulating sheet was cut to a size of 2 cm x 2 cm, and the first or second release liner was peeled off to expose the resin composition layer. The resin composition layer side was placed on the uneven surface of the glass substrate. The release liner on the opposite side was then peeled off, and a 50 μm-thick TPX (Opulent X-44B, manufactured by Mitsui Chemicals Tocello Inc.) and a 2.0 mm-thick PVC film (Celeb T, manufactured by Okamoto Corporation) were laminated in this order as cushioning materials, followed by cardboard to prevent sticking. Next, the test specimen was pressed against the substrate surface from above at 5 MPa and 100°C for 20 minutes, and the resin composition layer was filled into the unevenness of the glass substrate to form an encapsulating layer. After pressing, the cushioning material and cardboard were peeled off. The resin composition layer that protruded from the glass substrate of the obtained test piece was roughly removed using a cutter, and the resin composition layer remaining on the side surface of the glass substrate was further removed by sanding, exposing the side surface of the glass substrate and making it possible to observe the uneven portions of the glass substrate. Filling ability was evaluated by observing 20 recesses of the glass substrate at random using an electron microscope. In the recesses of the glass substrate, grooves were considered to be filled when the maximum gap between the resin composition layer and the glass substrate was 5 μm or less. The evaluation criteria were as follows, with A to C being considered good. A: Filled grooves in 18 or more places B: Filled grooves in 17 or less, 15 or more places C: Filled grooves in 14 or less, 12 or more places D: Filled grooves in 11 or less places
[0113] [Adhesion] The encapsulating sheet was cut into 2 cm x 8 cm pieces, and a glass plate (blue plate glass, manufactured by Kawamura Hisazo Shoten Co., Ltd.) having a thickness of 1.1 mm and a size of 2.5 cm x 10 cm was attached to the surface from which the first release liner had been peeled off, and the sheet was heat-pressed (100 ° C., 5 MPa, 5 minutes) for 5 minutes. Furthermore, the second release liner of the encapsulating sheet was peeled off, and the test piece consisting of the glass plate and the resin composition layer was left standing for 120 minutes under 180 ° C. conditions to adhere the glass plate and the resin composition layer to prepare a test piece consisting of the glass plate and the resin composition layer. In accordance with JIS K 5600-5-6 (cross-cut method), a right-angled grid pattern (25 squares) of 1 mm squares was created on the resin composition layer using a cross-cut guide and a cutter knife, and Nichiban Co., Ltd.'s adhesive tape "CT1835" was attached to the grid-cut portion and firmly adhered to the resin composition layer. Within 5 minutes of adhesion, the resin composition layer was peeled off at an angle close to 60° in 0.5 to 1.0 seconds. The state of the peeled resin composition layer was observed and adhesion was evaluated. The evaluation criteria were as follows, with A to C being rated as good. A: 0 squares completely peeled off, no partial peeling was observed at the edges of the incisions. B: 0 squares completely peeled off, partial peeling observed only at the edges of the incisions. C: 1 to 2 squares peeled off. D: 3 or more squares peeled off.
[0114] [Zipping Resistance] The encapsulating sheet was cut into a size of 2 cm x 8 cm, and a glass plate (blue plate glass, manufactured by Kawamura Hisazo Shoten Co., Ltd.) having a thickness of 1.1 mm and a size of 2.5 cm x 10 cm was attached to the surface from which the first release liner had been peeled off, and pressure-bonded by heat pressing (100°C, 5 MPa, 5 minutes). Three test pieces were prepared, and each was subjected to a heat aging treatment under the following three conditions: Condition (1) 60 minutes at 220°C, Condition (2) 120 minutes at 180°C, and Condition (3) 240 minutes at 120°C. After heat aging, the test piece was left to stand for at least 1 hour under conditions of 23°C and 50% relative humidity. Next, the second release liner was peeled off from the resin composition layer at a peel angle of 90° and a speed of 300 mm / min. The resin composition layer of the obtained test piece was observed for the presence or absence of zipping. The evaluation criteria were as follows, with A to C being considered good. A: No zipping was observed under any of the heat aging conditions. B: Zipping was observed under any one of the heat aging conditions. C: Zipping was observed under any two of the heat aging conditions. D: Zipping was observed under all of the heat aging conditions.
[0115] All of the above evaluations were rated on a four-point scale, with A being an outstanding rating, B being the next best rating, C being good rating, and D being unsuccessful in achieving the target performance. Note that performance ratings of all A to C correspond to the present disclosure.
[0116] [Examples 2 to 41], [Comparative Examples 1 to 7] Encapsulating sheets were produced in the same manner as in Example 1, except that the content and thickness Ta were changed as shown in Tables 2 to 5, and were evaluated in the same manner. Note that all other components were added at the same time. In Tables 2 to 5, the amounts of the resin (A), the embeddability improver (B), and other components are calculated as solid contents, and blank spaces indicate that no components were blended.
[0117] The abbreviations in the table are as follows: B1-1: Phosphorus-containing compound (ADK STAB PEP-36, manufactured by ADEKA Corporation, containing a 2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane skeleton, molecular weight 633) B1-2: Phosphorus-containing compound (ADK STAB HP-10, manufactured by ADEKA Corporation, containing a diphenyl monoalkyl phosphite skeleton, molecular weight 583) B1-3: Phosphorus-containing compound (ADK STAB 3010, manufactured by ADEKA Corporation, containing a trialkyl phosphite skeleton, molecular weight 503) B2-1: Phenolic hydroxyl group-containing compound (ADK STAB AO-80, manufactured by ADEKA Corporation, semi-hindered type, molecular weight 741) B2-2: Phenolic hydroxyl group-containing compound (ADK STAB AO-330, manufactured by ADEKA Corporation, hindered type, molecular weight 775) B2-3: phenolic hydroxyl group-containing compound (IRGANOX (registered trademark) 1010, manufactured by BASF Japan, hindered type, molecular weight 1,178) C-1: epoxy compound (jER (registered trademark) YX8034, manufactured by Mitsubishi Chemical Corporation) C-2: isocyanate compound (Cosmonate (registered trademark) T100, manufactured by Mitsui Fine Chemicals, Inc.) C-3: aziridine compound (ChemiTite (registered trademark) PZ-33, manufactured by Nippon Shokubai Co., Ltd.) C-4: silane coupling agent (KBE-403, manufactured by Shin-Etsu Silicones Co., Ltd.) F-1: silica (AEROSIL (registered trademark) R972, manufactured by Evonik Degussa)
[0118]
[0119]
[0120]
[0121]
[0122] In the present disclosure, in the case of an encapsulating sheet in which the glass transition temperature (Tg) of the resin (A) is outside the range of -30 to 40°C, it is found that there are problems with embeddability, as shown in Comparative Examples 1 and 2. Furthermore, in the case of an encapsulating sheet in which the thickness Ta of the resin composition layer is outside the range of 1 to 100 μm, there are problems with embeddability and zipping property, as shown in Comparative Examples 3 and 4. Furthermore, in the case where the embeddability improver (B) does not contain both the phosphorus-containing compound (B1) and the phenolic hydroxyl group-containing compound (B2), it is found that there are problems with light resistance, embeddability, and adhesion, as shown in Comparative Examples 5 to 7. As shown in Table 5, the encapsulating sheets of Comparative Examples 1 to 7 were unable to achieve a balanced high level of light resistance and embeddability. Furthermore, they were unable to achieve high levels of adhesion and zipping property. In contrast, according to Examples 1 to 41, the encapsulating sheets of the present disclosure exhibit excellent light resistance and excellent embeddability, as shown in Tables 2 to 5. Furthermore, since the encapsulating sheet of the present disclosure has excellent adhesion and zipping properties, it has been found that the encapsulating sheet of the present disclosure can be suitably used to encapsulate a plurality of light-emitting elements.
[0123] This application claims priority based on Japanese Patent Application No. 2023-079778, filed May 15, 2023, the disclosure of which is incorporated herein in its entirety.
[0124] DESCRIPTION OF SYMBOLS 1: Encapsulating sheet 2: Resin composition layer 3: Substrate 4: Release liner 4a: First release liner 4b: Second release liner 5: Light emitting element 6: Substrate 7: Glass substrate
Claims
1. An encapsulating sheet for encapsulating light-emitting elements used in a display using a plurality of light-emitting elements as a light source, the encapsulating sheet comprising a resin composition layer containing a resin (A) and an embeddability improver (B), the resin (A) having a glass transition temperature (Tg) of -30 to 40°C and a weight average molecular weight (Mw) of 10,000 to 1,000,000, the embeddability improver (B) containing a phosphorus-containing compound (B1) and a phenolic hydroxyl group-containing compound (B2), the resin composition layer having a loss tangent (tan δ40) at 40°C obtained by dynamic viscoelasticity measurement in a tensile mode at a frequency of 10 Hz of 0.8 to 2.0, and the resin composition layer having a thickness Ta of 1 to 100 μm.
2. The encapsulating sheet according to claim 1, wherein the resin (A) is a (meth)acrylic resin (a), which is a copolymer having a structural unit derived from an acrylic acid alkyl ester (a1) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 12 carbon atoms, and a structural unit derived from a methacrylic acid alkyl ester (a2) having a linear, branched or cyclic saturated aliphatic hydrocarbon group having 1 to 8 carbon atoms.
3. The encapsulating sheet according to claim 2, wherein the (meth)acrylic resin (a) further contains a structural unit derived from (meth)acrylic acid (a3).
4. The encapsulating sheet according to claim 1, wherein the resin (A) is contained in an amount of 76 to 99.9 mass% based on the total mass of the resin composition layer.
5. The encapsulating sheet according to claim 1, wherein the content of the embeddability improver (B) is 0.1 to 15 mass % based on the total mass of the resin composition layer.
6. The sealing sheet according to claim 1, wherein the mass ratio B1:B2 of the phosphorus-containing compound (B1) to the phenolic hydroxyl group-containing compound (B2) in the embeddability improver (B) is 0.1:1 to 10:
1.
7. A display having an encapsulating layer comprising a resin composition layer of the encapsulating sheet according to any one of claims 1 to 6.
Citation Information
Patent Citations
Resin composition for solar cell back face protective sheet
JP2014241383A
Curable resin composition, dry film, cured product, and electronic component
JP2022022562A
Photosensitive coloring composition, cured film using the same, color filter, optical filter, image display device, solid-state imaging device, and infrared sensor
JP7221348B1
Resin composition
WO2011111847A1
Flux-compatible epoxy-phenolic adhesive compositions for low gap underfill applications