Method for metal anodizing

The metal anodizing method addresses corrosion issues in alloy metals by using multiple cleaning and anodizing steps with acid solutions to form a thick oxide film, enhancing corrosion resistance and appearance while reducing costs and process time.

WO2024237495A1PCT designated stage expired Publication Date: 2024-11-21SAMSUNG ELECTRONICS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005082
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-14
Filing Date
2024-04-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Alloy metals used in appliances and automobiles face corrosion issues due to thin naturally formed oxide films, which can be easily removed, and surface impurities during anodizing processes lead to defects and reduced corrosion resistance.

Method used

A metal anodizing method involving multiple surface cleaning steps with acid solutions, including nitric acid and hydrofluoric acid, and anodizing steps with varying voltages in sulfuric acid solutions, minimizes impurities and surface defects, forming a thick oxide film for improved corrosion resistance without the need for alkaline pretreatment.

Benefits of technology

The method results in a final product with enhanced corrosion resistance, improved appearance, and reduced surface defects, while minimizing production costs and process time, achieving superior durability and aesthetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005082_21112024_PF_FP_ABST
    Figure KR2024005082_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A method for metal anodizing, according to one aspect of the disclosed invention, comprises: a step of preparing a metal casting; a step of performing, in a solution containing two or more acids, first surface cleaning on the casting; a step of performing, in a solution containing at least one acid and a catalyst, second surface cleaning on the casting that has been subjected to the first surface cleaning step; a first anodizing step of applying a voltage of 25-35 V to the casting that has been subjected to the second surface cleaning; and a second anodizing step of applying a voltage that is higher than the voltage applied in the first anodizing, wherein the first anodizing and the second anodizing are continuously performed in the same acidic solution containing 18-25 wt% of sulfuric acid.
Need to check novelty before this filing date? Find Prior Art

Description

Metal anodizing method

[0001] The present disclosure relates to a method for anodizing metal.

[0002] Alloy metals such as aluminum, magnesium, titanium, and zinc are widely used as substitutes for steel in interior and exterior materials for home appliances, electronic devices, and automobiles.

[0003] These alloy metals exhibit improved corrosion resistance compared to iron because they react with the atmosphere to form a thin film on their surface. However, this film, which forms naturally, is very thin and can easily be removed in the environment in which the alloy metal is used, potentially causing corrosion. Therefore, a method has been proposed to enhance corrosion resistance through metal anodizing, which artificially forms a sufficiently thick oxide film on the surface of the alloy metal.

[0004] Impurities remaining on the metal surface during the anodizing process can negatively impact anodizing efficiency and quality. Therefore, metal anodizing processes require precise process conditions to remove surface impurities and form a high-quality film.

[0005] One aspect of the present disclosure is to provide a method of metal anodizing that minimizes impurities on a metal surface.

[0006] One aspect of the present disclosure is to provide a method of anodizing metal having improved appearance by eliminating surface stains in the final product.

[0007] One aspect of the present disclosure is to provide a method of metal anodizing that minimizes the occurrence of surface defects (cracks) in the use environment of the final product.

[0008] One aspect of the present disclosure is to provide a method of anodizing a metal, wherein the final product has improved corrosion resistance.

[0009] One aspect of the present disclosure is to provide a metal anodizing method that increases productivity by minimizing the anodizing process steps.

[0010] The technical problems to be achieved in this document are not limited to the technical problems mentioned above, and other technical problems not mentioned can be clearly understood by a person having ordinary skill in the technical field to which the present disclosure belongs from the description below.

[0011] A metal anodizing method according to the invention comprises the steps of: preparing a metal casting; performing a first surface cleaning of the casting in a solution containing two or more acids; performing a second surface cleaning of the casting subjected to the first surface cleaning step in a solution containing at least one acid and a catalyst; a first anodizing step of applying a voltage of 25 to 35 V to the casting subjected to the second surface cleaning; and a second anodizing step of applying a higher voltage than the applied voltage of the first anodizing, wherein the first anodizing and the second anodizing are performed sequentially in the same acidic solution containing 18 to 25 wt% sulfuric acid.

[0012] A metal anodizing method according to the invention comprises the steps of preparing a metal casting, performing surface cleaning of the casting in a solution containing 70 to 90 wt% of a nitric acid solution and the remainder of a hydrofluoric acid solution, a first anodizing step of applying a voltage of 25 to 35 V to the surface-cleaned casting, and a second anodizing step of applying a voltage higher than the voltage applied in the first anodizing, wherein the first anodizing and the second anodizing are performed continuously in the same acidic solution containing 18 to 25 wt% of sulfuric acid, and the temperature is maintained at 0 to 5° C.

[0013] According to the present disclosure, since a pretreatment process with an alkaline solution prior to the first anodizing step is not included, the manufacturing process can be minimized, thereby reducing production costs. Furthermore, since the pretreatment process with an alkaline solution is omitted, a neutralization or desmutting process can be omitted.

[0014] The effects that can be obtained from the present disclosure are not limited to the effects mentioned above, and other effects that are not mentioned can be clearly understood by a person having ordinary skill in the art to which the present disclosure belongs from the description below.

[0015] Figure 1a is a photograph of the appearance of Comparative Example 1 after preprocessing.

[0016] Figure 1b is a photograph of the appearance of Example 1 after surface treatment.

[0017] Figure 2a is a photograph of the appearance of Comparative Example 1 that has undergone an anodizing process according to the prior art.

[0018] Figure 2b is a photograph of the appearance of Example 1 that has undergone an anodizing process according to the present disclosure.

[0019] Figure 3 is an SEM image of Comparative Example 1 that underwent 2 cycles of salt spray testing.

[0020] Figure 4a is a photograph of the appearance of Comparative Example 1 that underwent two cycles of a corrosion resistance evaluation test.

[0021] Figure 4b is a photograph of the appearance of Example 1 after undergoing 8 cycles of a corrosion resistance evaluation test.

[0022] It should be understood that the various embodiments of the present disclosure and the terminology used therein are not intended to limit the technical features described in the present disclosure to specific embodiments, but rather to encompass various modifications, equivalents, or substitutes of the embodiments.

[0023] In connection with the description of the drawings, similar reference numerals may be used for similar or related components.

[0024] The singular form of a noun corresponding to an item may include one or more of said items, unless the relevant context clearly indicates otherwise.

[0025] In this disclosure, each of the phrases "A or B", "at least one of A and B", "at least one of A or B", "A, B, or C", "at least one of A, B, and C", and "at least one of A, B, or C" may include any one of the items listed together in the corresponding phrase, or all possible combinations thereof.

[0026] The term “and / or” includes any combination of a plurality of related described elements or any one of a plurality of related described elements.

[0027] Terms such as "first," "second," or "first" or "second" may be used simply to distinguish one component from another and do not qualify the components in any other respect (e.g., importance or order).

[0028] In addition, terms such as 'front', 'rear', 'top', 'bottom', 'side', 'left', 'right', 'upper', and 'lower' used in the present disclosure are defined based on the drawings, and the shape and position of each component are not limited by these terms.

[0029] The terms “include” or “have” are intended to specify the presence of a feature, number, step, operation, component, part or combination thereof described in the present disclosure, but do not preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts or combinations thereof.

[0030] When a component is said to be “connected,” “coupled,” “supported,” or “in contact with” another component, this includes not only cases where the components are directly connected, coupled, supported, or in contact, but also cases where the components are indirectly connected, coupled, supported, or in contact through a third component.

[0031] When we say that a component is “on” another component, this includes not only cases where the component is in contact with the other component, but also cases where there is another component between the two components.

[0032] Unless otherwise specifically stated in this disclosure, % is based on weight and wt% means weight%.

[0033] The metal anodizing process includes a pretreatment process, an anodizing process, and a post-treatment process. A typical metal anodizing process performs a pretreatment process including a degreasing-etching-desmuting process to remove residual impurities on the metal surface and improve the corrosion resistance of the final product. After the pretreatment process, an anodizing process cycle of anodizing and etching is repeated several times to form an oxide film.

[0034] However, the final product manufactured using the general metal anodizing method had the problem of easily corroding in the product use environment and having stains on the surface, which reduced the aesthetics.

[0035] The inventors of the present disclosure analyzed the corroded and normal areas of final products manufactured using conventional metal anodizing methods to develop a metal anodizing method that minimizes surface staining. As a result, they discovered that staining was caused by inorganic impurities, including approximately 6 to 8 wt% silicon, remaining on the film surface even after pretreatment using conventional metal anodizing methods. Furthermore, they discovered that these remaining inorganic impurities were transferred to the film during the anodizing process, increasing the frequency of surface defects and accelerating corrosion.

[0036] In view of this, a metal anodizing method according to one aspect of the present disclosure can provide a metal having improved corrosion resistance while minimizing surface stains by minimizing inorganic impurities including residual silicon, including first and second surface cleaning steps and first and second anodizing steps.

[0037] Below, the metal anodizing method is described in detail.

[0038] Steps to prepare a metal casting

[0039] A metal anodizing method according to one aspect of the present disclosure can prepare a metal casting by processing a metal that is a raw material for performing anodizing.

[0040] The step of preparing the metal casting may include the step of die casting the metal to form the product, followed by the step of shot blasting.

[0041] In the metal die-casting process, the target raw materials may be aluminum alloys, magnesium alloys, titanium alloys, zinc alloys, or nickel alloys. Examples include aluminum alloys, ALDC Type 6, and ALDC Type 12.

[0042] The shot blasting step may be a step in which stainless steel balls are sprayed at high pressure to completely blast the surface to remove foreign substances and burrs. The diameter of the stainless steel balls used in shot blasting is not particularly limited, but may be 0.35 mm in diameter, for example.

[0043] High temperature degreasing step

[0044] A method for anodizing metal according to one aspect of the present disclosure may include a step of preparing a metal casting, followed by a step of high-temperature degreasing the manufactured metal casting.

[0045] The high-temperature degreasing step is a step to remove organic impurities present on the surface, and the high-temperature degreasing process can be performed by immersing the metal casting in a degreasing solution at 50 to 70°C for more than 1 minute.

[0046] The degreasing solution may contain a sulfuric acid solution. For example, the degreasing solution may contain 4 to 6 wt% sulfuric acid. If the sulfuric acid concentration in the degreasing solution is lower than 4 wt%, the degreasing power may be insufficient, preventing surface impurities from being sufficiently removed. If the sulfuric acid concentration exceeds 6 wt%, excessive reaction between the sulfuric acid and the metal may occur, resulting in surface defects or erosion.

[0047] In addition to the sulfuric acid solution, the degreasing solution may further contain a degreasing agent. The degreasing agent may be an acid degreasing agent that allows the concentration of the degreasing solution to be below pH 7.0, an alkaline degreasing agent that allows the pH to be above pH 7.0, or a neutral degreasing agent. The degreasing agent may be suitably applied depending on the characteristics of the metal casting. For example, the degreasing solution may be a solution containing 4 to 6 wt% sulfuric acid and 8 to 12 wt% neutral degreasing agent.

[0048] Surface cleaning stage

[0049] A metal anodizing method according to one aspect of the present disclosure may include a surface cleaning step following a high-temperature degreasing step. The surface cleaning step may include a first surface cleaning step and a second surface cleaning step.

[0050] The first surface cleaning step is a step performed to remove inorganic impurities such as silicon, copper, zinc, and manganese from the surface of the metal casting, and can be performed by immersing the metal casting in a solution containing two or more acids.

[0051] The solution in which the first surface cleaning step is performed may contain nitric acid and hydrofluoric acid. Nitric acid and hydrofluoric acid can effectively dissolve and remove impurities in metals and non-ferrous metals, including silicon. For example, the solution in which the first surface cleaning step is performed may contain 70 to 90 wt% nitric acid and the remainder hydrofluoric acid.

[0052] The temperature at which the first surface cleaning step is performed may be 25 to 35°C, and the time for performing the step may be 60 to 120 seconds. Since the efficiency of nitric acid and hydrofluoric acid increases when external heat energy is applied, the first surface cleaning step may be performed within the corresponding temperature range.

[0053] The second surface cleaning step is a step performed to remove fine inorganic impurities that were not removed in the first surface cleaning step, and can be performed by immersing in a solution containing at least one acid and a catalyst.

[0054] The solution in which the second surface cleaning is performed may contain sulfuric acid. Because sulfuric acid generates a large amount of hydrogen and oxygen gases through chemical reactions, it may be more effective in removing fine inorganic impurities than nitric acid or hydrofluoric acid. For example, the solution in which the second surface cleaning is performed may contain 15 to 25 wt% sulfuric acid. To accelerate the reaction, it may further contain 3 to 7 wt% hydrogen peroxide as a catalyst.

[0055] The temperature at which the second surface cleaning step is performed may be lower than that of the first surface cleaning solution, and the time for performing the step may be 60 to 120 seconds. Since sulfuric acid is more reactive than nitric acid and hydrofluoric acid, the temperature at which the second surface cleaning step is performed may be lower than that of the first surface cleaning step. For example, the temperature may be room temperature (23 to 27°C).

[0056] The metal subjected to the first and second surface cleaning steps (hereinafter, "surface cleaning steps") may contain inorganic impurities in an amount of 1 wt% or less. Since the metal casting subjected to the surface cleaning step has inorganic impurities completely removed, flow marks due to inorganic impurities may not form on the surface. Accordingly, a final product with improved appearance can be provided.

[0057] Inorganic impurities remaining after the surface cleaning step can transfer to the oxide film formed by the anodizing process in the final product, causing corrosion. Since the final product manufactured according to the present disclosure has residual inorganic impurities of 1 wt% or less, corrosion caused by inorganic impurities can be minimized.

[0058] The surface cleaning step according to the present disclosure does not include a pretreatment step using an alkaline solution. Since separate etching and desmut processes are not performed, the manufacturing process is minimized, thereby reducing production costs. For example, since the pretreatment step using an alkaline solution is omitted, the neutralization or desmut process can be omitted, and the wastewater treatment process for alkaline solutions such as caustic soda used in the etching process or acidic solutions such as nitric acid and sulfuric acid used in the desmut process can be omitted.

[0059] Anodizing step

[0060] A metal anodizing method according to one aspect of the present disclosure may include an anodizing step following a surface cleaning step. The anodizing step may include a first anodizing step and a second anodizing step.

[0061] The first anodizing step is a step for forming an oxide film that serves as a seed layer, and can be performed by applying a voltage of 25 to 35 V to the casting that has undergone the surface cleaning step. If the applied voltage is less than 25 V, the applied voltage is insufficient to sufficiently form the oxide film. If the applied voltage exceeds 35 V, internal stress may increase during the first anodizing process, which may cause surface defects.

[0062] The second anodizing step is a step of forming an oxide film on the seed layer, and can be performed by applying a voltage higher than the voltage applied for the first anodizing to the casting that has undergone the first anodizing. For example, the voltage applied for the second anodizing step can be 40 to 50 V. If the voltage applied for the second anodizing is less than 40 V, the process time may increase excessively, which may reduce productivity, or the oxide film may not be sufficiently formed, which may reduce the durability of the oxide film. If the voltage applied exceeds 50 V, burring may occur during the second anodizing process, which may result in defective products, thereby increasing the defect rate of the final product.

[0063] The first anodizing step may be performed for 60 to 180 seconds, and the second anodizing step may be performed for 1800 seconds or more. Preferably, the first anodizing step may be performed for 60 to 120 seconds, and the second anodizing step may be performed for 1800 to 5400 seconds, and more preferably, the second anodizing step may be performed for 1800 to 2900 seconds.

[0064] If the first anodizing step is performed for more than 180 seconds, the seed layer may be formed to be excessively thick, and if the second anodizing step is performed for less than 1800 seconds, the oxide film may not be sufficiently formed. When anodizing is performed for the above-mentioned time, the thickness of the oxide film may be 20 to 40 μm.

[0065] The first anodizing step and the second anodizing step can be performed at 0 to 5°C. Since the temperatures of the first anodizing step and the second anodizing step do not differ, the process steps can be minimized. Since the first anodizing step and the second anodizing step are performed at relatively low temperatures, there is an advantage in that the occurrence of surface defects due to thermal energy is reduced.

[0066] In addition, when anodizing is performed in the above temperature range, a film can be uniformly formed even under an environment of an applied voltage of 25 V or higher. For example, if the first anodizing step and the second anodizing step are performed at a temperature exceeding 5°C, the film may not be uniformly formed, resulting in a significant deterioration in the hardness and wear resistance of the final product.

[0067] The first anodizing step and the second anodizing step may be performed in a solution containing 18 to 25 wt% of sulfuric acid, and preferably in a solution containing 18 to 22 wt% of sulfuric acid. If the sulfuric acid concentration of the solution in which the first anodizing step and the second anodizing step are performed is less than 18 wt%, the process time may be excessively increased, and an oxide film having a thickness of 20 μm or more may not be formed. If the sulfuric acid concentration exceeds 25 wt%, the oxide film may not be uniformly formed during the process, which may cause surface defects, and corrosion resistance may be reduced, which may easily cause corrosion.

[0068] The first and second anodizing steps are performed sequentially in the same sulfuric acid solution. Since the first and second anodizing steps are performed in the same solution with only different applied voltages, no separate etching or rinsing steps are required between the steps. This shortens the overall process time and reduces production costs.

[0069] Furthermore, since the oxide film formed in the second anodizing step is formed on the seed layer formed in the first anodizing step, the oxide film has a high density and thus can form an oxide film with excellent durability. Accordingly, even without a separate high-temperature sealing step as a post-processing step, a sufficient sealing effect can be achieved with only low-temperature sealing.

[0070] Coloring stage

[0071] A metal anodizing method according to one aspect of the present disclosure may include a coloring step following the anodizing step. The coloring step is a step of imparting a color to the final product and may be performed using a typical coloring process. For example, the coloring step may be performed by immersing the final product in a solution containing 1 wt% of the colorant to be imparted to the final product at room temperature for 10 minutes.

[0072] Low-temperature sealing treatment stage

[0073] A metal anodizing method according to one aspect of the present disclosure may include a low-temperature sealing step subsequent to the anodizing step.

[0074] The low-temperature sealing step is performed to seal the pores formed on the film surface and minimize residual pores. This step can be performed at a low temperature of 30 to 40°C. By performing the sealing step at a low temperature, surface defects that occur as the temperature increases during the process can be prevented. Furthermore, since the sealing process does not require high temperatures (over 60°C), there is the advantage of not requiring separate equipment to maintain the high-temperature process.

[0075] The low-temperature sealing step can be performed by immersing the casting in a solution containing a nickel-based substance for at least 20 minutes. The nickel-based substance is not particularly limited, but the sealing process can be performed most efficiently when it is nickel fluoride. For example, the process can be performed by immersing the casting in a sealing solution containing 0.4 to 0.6 wt% nickel fluoride for 20 minutes.

[0076] A metal anodizing method according to one aspect of the present disclosure may include a conventional post-treatment process following the low-temperature sealing step.

[0077] For example, a silicon organic film coating can be performed on the film to further improve durability.

[0078] For example, the casting can be dried for more than 30 minutes at a temperature range of 70 to 80°C to remove surface moisture and stabilize it.

[0079] Hereinafter, examples and comparative examples are described in detail with reference to the drawings.

[0080] Manufacturing Example 1

[0081] After die-casting aluminum of ALDC1 standard, shot blasting was performed using a 0.35 mm stainless steel ball to prepare an aluminum alloy specimen.

[0082] Comparative Example 1

[0083] A 10 wt% citric acid aqueous solution was prepared. While maintaining the aqueous solution at 45°C, the aluminum alloy specimen of Preparation Example 1 was degreased in the aqueous solution for 3 minutes and 30 seconds, and then washed.

[0084] Next, the degreased specimen was placed in a 10 wt% sodium hydroxide aqueous solution, etched at 45°C for 2 minutes, and then washed. The etched specimen was placed in a 35 wt% nitric acid aqueous solution, desmutted at approximately 20°C for 2 minutes, and then washed to produce a surface-treated specimen.

[0085] Example 1

[0086] An aqueous solution containing 5 wt% sulfuric acid and 10 wt% neutral degreasing agent was prepared. While maintaining the aqueous solution at 65°C, the aluminum alloy specimen of Preparation Example 1 was immersed in the aqueous solution for 3 minutes to perform a high-temperature degreasing process.

[0087] Next, an aqueous solution containing 80 wt% nitric acid and 20 wt% hydrofluoric acid was prepared. While maintaining the aqueous solution at 30°C, the specimens subjected to the high-temperature degreasing process were immersed in the aqueous solution for 90 seconds to perform the first surface cleaning process. Subsequently, an aqueous solution containing 15 wt% sulfuric acid and 5 wt% hydrogen peroxide was prepared while maintaining the temperature at 25°C. The specimens subjected to the first surface cleaning process were immersed in the aqueous solution for 90 seconds to perform the second surface cleaning process, thereby producing pretreated specimens.

[0088] Fig. 1a is a photograph of the appearance of Comparative Example 1 after pretreatment, and Fig. 1b is a photograph of the appearance of Example 1 after surface treatment.

[0089] In the case of the aluminum specimen of Comparative Example 1 manufactured according to the conventional technique, surface stains were observed, resulting in a deterioration in aesthetics. On the other hand, in the case of the aluminum specimen of Example 1 manufactured according to the surface treatment method according to the disclosed embodiment, surface stains were not observed, resulting in an improved appearance compared to the conventional Comparative Example 1.

[0090]

[0091] For Comparative Example 1, which performed a pretreatment process, and Example 1, which performed a surface treatment, an anodizing process was performed.

[0092] Comparative Example 1

[0093] For Comparative Example 1, which performed a pretreatment process, a first anodizing step and a first etching step, a second anodizing step and a second etching step, and a third anodizing step and a second etching step were performed.

[0094] The first anodizing step is performed by placing Comparative Example 1 after the pretreatment process into the first electrolyte. The first electrolyte contains a 20 wt% sulfuric acid aqueous solution, and the temperature is maintained at 17°C. The first anodizing step is applied with a voltage of 30 V and is performed for 15 minutes. Thereafter, the first etching step is performed.

[0095] The second anodizing step is performed by placing the first etched specimen in a second electrolyte. The second electrolyte contains a 30 wt% sulfuric acid aqueous solution. The temperature, applied voltage, and anodizing time are the same as those in the first anodizing step. Subsequently, the second etching step is performed.

[0096] The third anodizing step is performed by placing the second etched specimen in a third electrolyte. The third electrolyte contains a 40 wt% sulfuric acid aqueous solution. The temperature, applied voltage, and anodizing time are the same as in the first anodizing step. After the third etching step, the specimen is manufactured through washing and drying steps.

[0097] Example 1

[0098] For Example 1, in which a surface treatment process was performed, the first anodizing and second anodizing processes were performed.

[0099] The first and second anodizing were performed in the same sulfuric acid aqueous solution, which was a 20 wt% sulfuric acid aqueous solution. After performing the surface treatment process, Example 1 was placed in the 20 wt% sulfuric acid aqueous solution, and the temperature was maintained at 3°C.

[0100] Next, a first anodizing process was performed by applying an applied voltage of 30 V for 2 minutes to Example 1. Subsequently, a second anodizing process was performed for 48 minutes by changing only the applied voltage to 45 V without a separate etching process. The thickness of the film formed after the second anodizing was 30 μm.

[0101] Next, a coloring process was performed by immersing 1 wt% of a color dye at room temperature for 10 minutes, and then a low-temperature sealing process was performed by maintaining a solution containing 0.5 wt% of nickel fluoride at 30°C for 20 minutes. Afterwards, coating was performed using a silicon organic film coating agent from Korea Chemical Co., Ltd., to further improve durability, and then a specimen was manufactured by drying at 75°C for 30 minutes.

[0102] FIG. 2a is a photograph of the appearance of Comparative Example 1 that has undergone an anodizing process according to a conventional technique, and FIG. 2b is a photograph of the appearance of Example 1 that has undergone an anodizing process according to the present disclosure.

[0103] In Comparative Example 1, the stains observed after the pretreatment process still existed even after the anodizing process, indicating that the specimen was unsuitable for product application. In Example 1, a clean appearance was formed without surface stains after the surface treatment and anodizing processes. This indicates that the specimen can exhibit an excellent appearance without any defects due to discoloration or stains in a consumer use environment.

[0104]

[0105] Next, in order to evaluate the corrosion resistance of the specimen, a corrosion resistance evaluation test was performed on Comparative Example 1 and Example 1.

[0106] The corrosion resistance evaluation test was performed by performing a neutral salt spray-leaving process as one cycle, and a total of 8 cycles were performed for each specimen. The appearance of white rust on the specimen surface was observed at the end of each cycle. The neutral salt spray process was performed by preparing a 5% sodium chloride solution as a spray solution and spraying the spray solution on the specimen for 8 hours in a chamber maintained at 35°C. Afterwards, the specimen was left in a chamber maintained at the same temperature for 16 hours.

[0107] Afterwards, SEM (Scanning Electron Microscope) images of the white rust portion of the specimen where white rust occurred were obtained. The SEM images were taken at 500x magnification for the white rust portion, and the results are shown in Fig. 3.

[0108] Figure 3 is an SEM image of Comparative Example 1 that underwent 2 cycles of salt spray testing.

[0109] Fig. 4a is a photograph of the appearance of Comparative Example 1 that underwent 2 cycles of a corrosion resistance evaluation test, and Fig. 4b is a photograph of the appearance of Example 1 that underwent 8 cycles of a corrosion resistance evaluation test.

[0110] Referring to Fig. 3, it can be seen that in Comparative Example 1, surface defects (cracks) occurred on the specimen, resulting in reduced corrosion resistance. Accordingly, as shown in Fig. 4a, when the corrosion resistance evaluation test was repeated for two cycles, severe white rust occurred on the specimen surface.

[0111] On the other hand, in the case of Example 1, as shown in Fig. 4b, no white rust occurred on the surface of the specimen even when the corrosion resistance evaluation test was repeated 8 cycles. Accordingly, it can be seen that the corrosion resistance of Example 1, which performed anodizing according to the present disclosure, is significantly superior to that of Comparative Example 1.

[0112] In the above, only the disclosed embodiments are disclosed with reference to the attached drawings, but in addition to the above examples, a person having ordinary knowledge in the technical field to which the disclosure of this document belongs can make various changes and implementations without departing from the gist of the technical idea of ​​the disclosure described in the claims below.

[0113] A metal anodizing method according to the invention may include the steps of: preparing a metal casting; performing a first surface cleaning of the casting in a solution containing two or more acids; performing a second surface cleaning of the casting subjected to the first surface cleaning step in a solution containing at least one acid and a catalyst; a first anodizing step of applying a voltage of 25 to 35 V to the casting subjected to the second surface cleaning; and a second anodizing step of applying a higher voltage than the applied voltage of the first anodizing. In addition, the first anodizing and the second anodizing are performed in a solution containing 18 to 25 wt% sulfuric acid, and the first and second anodizing processes are performed continuously in the same acidic solution.

[0114] According to the present disclosure, since the first and second surface cleaning steps are performed, the silicon component on the surface is removed to a level of less than 1 wt%, thereby providing a product having an excellent appearance without surface stains.

[0115] According to the present disclosure, by performing a first anodizing process at a low voltage to form a seed layer and then performing a second anodizing process at a high voltage to form a film, internal stress can be minimized and the formation of surface defects can be prevented. In addition, since the first and second anodizing processes are performed continuously, a separate process such as an etching process is not required between each anodizing step. In addition, since the first and second anodizing processes are performed in the same acidic solution, only the applied voltage is changed without separating each anodizing process into a separate process, so the process efficiency is increased and productivity is improved.

[0116] The first surface cleaning is performed in a solution containing nitric acid and hydrofluoric acid, and can be performed at a temperature of 25 to 35°C for 60 to 120 seconds. According to the present disclosure, since the first surface cleaning solution contains nitric acid and hydrofluoric acid, inorganic impurities of metals and non-ferrous metals, including silicon, can be effectively removed. In addition, since it is performed at a temperature of 25 to 35°C, external heat energy can be applied to the nitric acid and hydrofluoric acid, thereby increasing the efficiency of the first surface cleaning.

[0117] The solution in which the first surface cleaning is performed may contain 70 to 90 wt% of nitric acid and the remainder of hydrofluoric acid.

[0118] The second surface cleaning is performed in a solution containing sulfuric acid, and can be performed for 60 to 120 seconds at a temperature lower than the temperature at which the first surface cleaning is performed. In addition, the second surface cleaning can be performed at 23 to 27°C. According to the present disclosure, since the second surface cleaning solution contains sulfuric acid, a large amount of hydrogen and oxygen gases are generated, and fine inorganic impurities remaining on the surface can be removed through a chemical reaction. In addition, since the temperature at which the second surface cleaning is performed is lower than the temperature at which the first surface cleaning is performed, the reactivity of sulfuric acid can be controlled.

[0119] The solution in which the second surface cleaning is performed may contain 15 to 25 wt% of sulfuric acid, 3 to 7 wt% of hydrogen peroxide, and the remainder of the solvent.

[0120] The first anodizing and the second anodizing can be performed at 0 to 5°C. According to the present disclosure, since the first and second anodizing processes are performed at low temperatures, the occurrence of surface defects is reduced, and a final product with improved hardness and wear resistance can be provided.

[0121] The first anodizing may be performed for 60 to 180 seconds, and the second anodizing may be performed for 1800 seconds or more. In addition, the thickness of the film formed after the second anodizing may be 20 to 40 μm. According to the present disclosure, by controlling the performance times of the first anodizing and the second anodizing as described above to form a film with a thickness of 20 to 40 μm, it is possible to provide a final product with excellent corrosion resistance while reducing the production cost.

[0122] The applied voltage of the second anodizing may be 40 to 50 V. According to the present disclosure, the productivity of the final product can be improved by quickly forming a film while minimizing defective products due to burring.

[0123] The metal anodizing method according to the invention may further include at least one of a step of high-temperature degreasing the casting at 50 to 70°C before the step of performing the first surface cleaning, or a step of low-temperature sealing the casting at 30 to 40°C after the step of performing the second anodizing.

[0124] According to the present disclosure, since a high-temperature degreasing step is included prior to the first surface cleaning step, organic impurities on the metal surface can be effectively removed. In addition, since a sealing process is performed at a low temperature after the second anodizing step, surface defects (cracks) that occur due to an increase in temperature during the sealing process can be prevented. In addition, since the sealing process is performed at a low temperature, an additional pressure device for the sealing process is not required, and since a post-sealing process performed at a high temperature after the low-temperature sealing process is not required, the manufacturing process can be minimized and production costs can be reduced.

[0125] The above high temperature degreasing step can be performed in a solution containing 4 to 6 wt% sulfuric acid and 8 to 12 wt% of a neutral degreasing agent.

[0126] The above low-temperature sealing step may be performed for 20 minutes or more in a solution containing a nickel-based material, and the nickel-based material may include nickel fluoride. According to the present disclosure, since the low-temperature sealing process is performed using a nickel-based material, pores can be effectively sealed, thereby minimizing pores on the film surface. Furthermore, according to the present disclosure, since nickel fluoride is used, the sealing effect can be significantly superior to conventional sealing processes using nickel acetate or distilled water.

[0127] A metal anodizing method according to the invention comprises the steps of: preparing a metal casting; performing surface cleaning of the casting in a solution containing 70 to 90 wt% of a nitric acid solution and the remainder of a hydrofluoric acid solution; a first anodizing step of applying a voltage of 25 to 35 V to the surface-cleaned casting; and a second anodizing step of applying a voltage higher than the voltage applied in the first anodizing, wherein the first anodizing and the second anodizing are performed continuously in the same acidic solution containing 18 to 25 wt% of sulfuric acid, and the temperature of the acidic solution is maintained at 0 to 5° C.

[0128] According to the present disclosure, the surface cleaning process is performed in a solution containing 70 to 90 wt% nitric acid and a remainder of hydrofluoric acid, so that inorganic impurities of metals and non-ferrous metals including silicon can be effectively removed.

[0129] According to the present disclosure, by performing a first anodizing process at a low voltage to form a seed layer and then performing a second anodizing process at a high voltage to form a film, internal stress can be minimized and the formation of surface defects can be prevented. In addition, since the first and second anodizing processes are performed continuously, a separate process such as an etching process is not required between each anodizing step. In addition, since the first and second anodizing processes are performed in the same acidic solution, only the applied voltage is changed without separating each anodizing process into a separate process, so the process efficiency is increased and productivity is improved.

[0130] According to the present disclosure, since the first and second anodizing performance temperatures are maintained at 0 to 5°C, the occurrence of surface defects is reduced, and a final product with improved hardness and wear resistance can be provided.

[0131] The applied voltage of the second anodizing may be 40 to 50 V. According to the present disclosure, the productivity of the final product can be improved by quickly forming a film while minimizing defective products due to burring.

[0132] The first anodizing may be performed for 60 to 180 seconds, and the second anodizing may be performed for 1800 seconds or more. In addition, the thickness of the film layer formed after the second anodizing may be 20 to 40 μm. According to the present disclosure, by controlling the performance times of the first anodizing and the second anodizing as described above to form a film having a thickness of 20 to 40 μm, it is possible to provide a final product having excellent corrosion resistance while reducing the production cost.

[0133] The metal anodizing method according to the invention may further include a step of performing a low-temperature sealing treatment by immersing the casting on which the second anodizing was performed in a 0.3 to 0.7 wt% nickel fluoride solution at a temperature of 30 to 40°C. According to the invention, since the low-temperature sealing treatment step is further included, surface defects that occur as the temperature increases during the sealing treatment process can be prevented, and since a post-sealing treatment process performed at a high temperature is not required, the manufacturing process can be minimized and the production cost can be reduced. In addition, since nickel fluoride is used as the sealing treatment solution, pores on the surface of the film can be effectively sealed, thereby minimizing pores on the surface of the film.

[0134] A metal anodizing method according to the invention is characterized in that it does not include a pretreatment step with an alkaline solution prior to the first anodizing.

Claims

1. Step of preparing a metal casting; A step of performing a first surface cleaning of the casting in a solution containing two or more acids; A step of performing a second surface cleaning on a casting that has undergone the first surface cleaning step in a solution containing at least one acid and a catalyst; A first anodizing step of applying a voltage of 25 to 35 V to the casting on which the second surface cleaning has been performed; and A second anodizing step for applying a voltage higher than the voltage applied to the first anodizing step is included; A metal anodizing method, wherein the first anodizing and the second anodizing are performed sequentially in the same acidic solution containing 18 to 25 wt% sulfuric acid.

2. In paragraph 1, A metal anodizing method, wherein the first surface cleaning is performed in a solution containing nitric acid and hydrofluoric acid, and is performed at a temperature of 25 to 35°C for 60 to 120 seconds.

3. In paragraph 1, A metal anodizing method, wherein the solution in which the first surface cleaning is performed contains 70 to 90 wt% of nitric acid and the remainder is hydrofluoric acid.

4. In paragraph 1, A metal anodizing method, wherein the second surface cleaning is performed in a solution containing sulfuric acid and is performed for 60 to 120 seconds at a temperature lower than the temperature at which the first surface cleaning is performed.

5. In paragraph 1, A metal anodizing method, wherein the solution in which the second surface cleaning is performed contains 15 to 25 wt% of sulfuric acid, 3 to 7 wt% of hydrogen peroxide, and a remainder of a solvent.

6. In paragraph 4, A metal anodizing method, wherein the second surface cleaning is performed at 23 to 27°C.

7. In paragraph 1, A metal anodizing method, wherein the first anodizing and the second anodizing are performed at 0 to 5°C.

8. In paragraph 1, The above first anodizing is performed for 60 to 180 seconds, A metal anodizing method, wherein the second anodizing is performed for 1800 seconds or longer.

9. In paragraph 1, A metal anodizing method, wherein the applied voltage of the second anodizing is 40 to 50 V.

10. In paragraph 1, A metal anodizing method, wherein the thickness of the film formed after the second anodizing is 20 to 40 ㎛.

11. In paragraph 1, Before the step of performing the first surface cleaning, a step of high-temperature degreasing of the casting at 50 to 70°C; and A metal anodizing method further comprising at least one of the steps of performing a low-temperature sealing treatment at 30 to 40° C. after the step of performing the second anodizing.

12. In paragraph 11, A metal anodizing method, wherein the high-temperature degreasing step is performed in a solution containing 4 to 6 wt% sulfuric acid and 8 to 12 wt% of a neutral degreasing agent.

13. In paragraph 11, A metal anodizing method, wherein the step of performing the above low-temperature sealing treatment is performed for 20 minutes or more in a solution containing a nickel-based material.

14. In paragraph 13, A metal anodizing method, wherein the nickel-based material comprises nickel fluoride.

15. Step of preparing a metal casting; A step of surface cleaning the above casting in a solution containing 70 to 90 wt% of nitric acid and the remainder of hydrofluoric acid; A first anodizing step of applying a voltage of 25 to 35 V to the casting that has undergone the surface cleaning; and A second anodizing step for applying a voltage higher than the voltage applied to the first anodizing step is included; A metal anodizing method, wherein the first anodizing and the second anodizing are performed continuously in the same acidic solution containing 18 to 25 wt% sulfuric acid, and the temperature is maintained at 0 to 5°C.

Citation Information

Patent Citations

  • Method for electrolytically coloring aluminum

    JP1998102289A

  • Method for producing corrosion-resistant aluminum-silicon alloy castings, such corrosion-resistant aluminum-silicon alloy castings and their uses - Patents.com

    JP2022520217A

  • (method for electroless nikel plating of aluminum connector using telecommuniction

    KR101260260B1

  • Anodizing Aluminum and Alloys Thereof

    KR1020170092209A

  • Mask apparatus for skin care

    KR102355064B1