Star-shaped liquid styrene-butadiene rubber modified by means of grafting, and preparation method therefor and use thereof

Through the preparation of star-type grafted modified liquid styrene butadiene-styrene copolymerization segment and cellulose ether modified terpene resin segment, the adhesion and stability of liquid styrene butadiene-styrene rubber are solved by combining the butadiene-styrene copolymerization segment and cellulose ether modified terpene resin segment. The problem of insufficient results enables efficient adhesion and adhesion improvement, simplifying the process and reducing costs.

WO2024239554A1PCT designated stage expired Publication Date: 2024-11-28PETROCHINA CO LTD

Patent Information

Application Number
PCT/CN2023/130988
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2023-11-10
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing liquid styrene butadhesion rubber has poor adhesion, stability, viscosity and adhesion properties, complex process, difficult operation and high cost, easy to generate gels and cause environmental pollution.

Method used

The liquid styrene butadiene rubber is subjected to star-type graft modification by negative ion solution polymerization method. By combining the butadiene-styrene copolymerization segment and the cellulose ether-modified terpene resin segment, the branched high is formed by coupling agent. Polymers achieve short-range structural bonding of different polymer molecular chains to improve compatibility and adhesion.

Benefits of technology

It significantly improves the viscosity, adhesion and adhesion properties of liquid styrene butadiene rubber, simplifies the process flow, reduces costs, expands the scope of application, and improves environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023130988_28112024_PF_FP_ABST
    Figure CN2023130988_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the field of rubber preparation. Disclosed are star-shaped liquid styrene-butadiene rubber modified by means of grafting, and a preparation method therefor and the use thereof. The modified liquid styrene-butadiene rubber comprises a polymerization chain segment from a coupling agent, and a plurality of butadiene-styrene copolymerization chain segments and cellulose ether modified terpene resin chain segments, which are grafted onto the polymerization chain segment, wherein the coupling agent is selected from multi-vinyl aromatic hydrocarbon monomers. The modified liquid styrene-butadiene rubber achieves combination of polymers at a molecular structure level, and has good compatibility, stability and adhesiveness. The generated modified liquid styrene-butadiene rubber improves the viscosity, adhesive force and other properties of a copolymer system, and can be used as a high-grade adhesive and a coating, and the application range thereof is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Star-shaped grafted modified liquid styrene-butadiene rubber and its preparation method and application

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Chinese patent application No. 202310587657.1 filed on May 23, 2023, the contents of which are incorporated herein by reference. Technical Field

[0003] The invention relates to the field of rubber preparation, and in particular to a star-shaped grafted modified liquid styrene-butadiene rubber and a preparation method and application thereof. Background Art

[0004] Liquid rubber generally refers to a polymer with a number-average molecular weight of 2,000-15,000 g / mol. Its viscosity varies with the polymer's relative molecular weight and molecular configuration. Liquid rubber offers fluidity and a wide range of bulk viscosities, making it easy to process, enabling continuous and automated production, improving production efficiency, and reducing power consumption. Liquid rubber can be directly added to fillers and reinforcing agents to make rubber products, or it can be added to thermosetting resins and other polymers for modification. Liquid rubber containing functional groups, due to their active functional groups, facilitates chain extension and cross-linking to form solid vulcanized rubber, significantly improving physical properties. It can also react with a wide range of other groups to form novel materials with various structures. There are many types of liquid rubber, which can be categorized by the presence and location of functional groups into non-functional liquid rubber, random functional liquid rubber, and terminal functional liquid rubber. Among the many liquid rubber types, diene-based liquid rubbers, particularly butadiene-based ones, were studied as the "rubber of the future" in the late 20th century due to their widespread availability and low cost. Liquid nitrile rubber, liquid styrene butadiene rubber and liquid isoprene rubber have outstanding application advantages in their respective fields.

[0005] Liquid styrene-butadiene rubber (LSBR) is a low-molecular-weight copolymer made from butadiene and styrene using free radical emulsion or negative (anionic) polymerization. It has a molecular weight of 2,000-15,000 g / mol and is a light yellow or light brown, transparent, viscous liquid. LSBR exhibits excellent electrical insulation and physical properties, is insoluble in common organic solvents, and does not melt upon heating. LSBR exhibits good compatibility with certain general-purpose rubbers, allowing them to be blended and used simultaneously with fillers and oils. Because these mixed components are evenly dispersed and have good pouring fluidity, they can be injection molded into hard rubber products. It can also be used as a plasticizer for styrene-butadiene rubber, nitrile rubber, and chloroprene rubber, as well as in adhesives and sealants. It is also used in high-end coatings, expanding its application range.

[0006] Reports both domestically and internationally have explored the use of liquid rubber in various fields, including the modification of various polymers using liquid rubber, primarily in liquid nitrile rubber and liquid isoprene rubber, or through terminalization. The poor adhesion, stability, viscosity, and degree of branching of the prepared liquid rubbers, coupled with the need to improve the viscosity and adhesion of copolymer systems, present challenges in this field. Furthermore, these processes present complex processes, operational difficulties, long reaction cycles, high costs, and the tendency to gel, which can lead to environmental pollution.

[0007] Summary of the Invention

[0008] The purpose of the present invention is to overcome the problems of poor adhesion, stability, viscosity, adhesion performance and branching degree of liquid rubber in the prior art, and to provide a star-shaped grafted modified liquid styrene-butadiene rubber and its preparation method and application.

[0009] The inventors of the present invention have discovered through research that a common liquid styrene-butadiene rubber anion solution polymerization method can be used to modify liquid styrene-butadiene rubber, which is a simple and reliable method.

[0010] In order to achieve the above-mentioned object, the first aspect of the present invention provides a star-shaped grafted modified liquid styrene butadiene rubber, wherein the modified liquid styrene butadiene rubber includes a polymer segment from a coupling agent and a plurality of butadiene-styrene copolymer segments and cellulose ether-modified terpene resin segments grafted on the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.

[0011] A second aspect of the present invention provides a method for preparing a star-shaped grafted modified liquid styrene-butadiene rubber, wherein the preparation method comprises:

[0012] (1) in the presence of an initiator and a polar activator, copolymerizing butadiene and styrene to obtain an active butadiene-styrene copolymer segment;

[0013] (2) performing a coupling reaction on the active butadiene-styrene copolymer segment and a coupling agent to obtain an active chain;

[0014] (3) polymerizing the active chain with a modified terpene resin to obtain the star-shaped grafted modified liquid styrene-butadiene rubber.

[0015] The third aspect of the present invention provides a star-shaped grafted modified liquid styrene-butadiene rubber obtained by the preparation method.

[0016] The fourth aspect of the present invention provides an application of the star-shaped grafted modified liquid styrene-butadiene rubber in the field of rubber processing.

[0017] Through the above technical solution, the invention provides a modified liquid styrene-butadiene rubber. From the perspective of the structure of the polymer chain, it is a branched polymer with a star-shaped structure, that is, multiple molecular chains are grafted onto the polymer segment to form different segments as branches, and similarly connected molecular arms (such as polybutadiene styrene arms, modified terpene resin polymer arms) are called mixed arms. In the modified liquid styrene-butadiene rubber, the polymer segment formed by the coupling agent is equivalent to the polybutadiene-styrene rubber and the modified terpene resin as the core and chained together, realizing the combination of different polymer molecular chains at the short-range structural level of the polymer chain, and having good compatibility, stability and adhesion. The obtained modified liquid styrene-butadiene rubber improves the viscosity, adhesion and other properties of the copolymer system, and can be used to make high-end adhesives, plasticizers, and coatings, expanding the scope of application. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a schematic diagram of the molecular chain structure of star-shaped grafted modified liquid styrene-butadiene rubber.

[0019] Description of Reference Numerals

[0020] PSB-represents butadiene-styrene copolymer segment, PT-represents cellulose ether modified terpene resin segment. DETAILED DESCRIPTION

[0021] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0022] The first aspect of the present invention provides a star-shaped grafted modified liquid styrene butadiene rubber, wherein the modified liquid styrene butadiene rubber comprises a polymer segment from a coupling agent and a plurality of butadiene-styrene copolymer segments and cellulose ether-modified terpene resin segments grafted onto the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.

[0023] In the present invention, the modified liquid styrene-butadiene rubber provided is a branched polymer with a star-shaped structure from the perspective of the structure of the polymer chain, wherein the polymer segment formed by the coupling agent serves as the polymer core, and the multiple vinyl functional groups possessed by the coupling agent provide the polymer segment with multiple vinyl groups that can further graft other branches; the butadiene-styrene copolymer chain and the cellulose ether modified terpene resin chain can be bonded to the vinyl groups on the polymer segment through the carbon-carbon double bonds contained in each of them, forming a butadiene-styrene copolymer segment and a cellulose ether modified terpene resin segment grafted on the polymer segment, that is, multiple molecular chains are grafted on the polymer segment to form different segments as branches, which are similarly connected molecular arms (such as polybutadiene styrene arms, modified terpene resin polymer arms) and can be called mixed arms. In the modified liquid styrene-butadiene rubber, the polymer chain segments formed by the coupling agent are used as the core and chained together, thereby realizing the combination of different polymer molecular chains at the short-range structural level of the polymer chain, and having good compatibility, stability and adhesion.

[0024] In the present invention, the coupling agent is selected from polyvinyl aromatic monomers, which form polymer segments with multiple terminal molecular arms through self-polymerization, thereby forming polymers with a high degree of branching.

[0025] In some specific embodiments of the present invention, the modified liquid styrene-butadiene rubber comprises 20-80 wt% of the cellulose ether-modified terpene resin segment and 20-80 wt% of the butadiene-styrene copolymer segment, based on the combined weights of the butadiene-styrene copolymer segment and the cellulose ether-modified terpene resin segment. By limiting the modified liquid styrene-butadiene rubber to these limits, the combination of different polymer chains at the short-range structural level of the polymer chain is achieved, resulting in excellent compatibility, stability, and adhesion.

[0026] In some embodiments of the present invention, in the modified liquid styrene-butadiene rubber, the content of the cellulose ether-modified terpene resin segment can be selected from 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, or any value within a range consisting of any two of the above values, based on the sum of the weights of the butadiene-styrene copolymer segment and the cellulose ether-modified terpene resin segment. The content of the butadiene-styrene copolymer segment can be selected from 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, or any value within a range consisting of any two of the above values.

[0027] In some specific embodiments of the present invention, the butadiene-styrene copolymer segment comprises 50-90 wt% of butadiene structural units and 10-50 wt% of styrene structural units. By limiting the above-described contents in the modified liquid styrene-butadiene rubber, the different polymer chains are combined at the short-range structural level of the polymer chain, resulting in good compatibility, stability, and adhesion.

[0028] In some embodiments of the present invention, the content of the butadiene structural unit in the butadiene-styrene copolymer segment can be selected from 50 wt%, 60 wt%, 70 wt%, 80 wt%, 90 wt%, or any value within a range consisting of any two of the above values. The content of the styrene structural unit can be selected from 10 wt%, 20 wt%, 30 wt%, 40 wt%, 50 wt%, or any value within a range consisting of any two of the above values.

[0029] In some specific embodiments of the present invention, the cellulose ether-modified terpene resin segment comprises 10-40 wt% of the cellulose ether and 60-90 wt% of the terpene resin. By limiting the above content in the modified liquid styrene-butadiene rubber, the different polymer chains are combined at the short-range structural level of the polymer chain, resulting in excellent compatibility, stability, and adhesion. The higher the terpene resin content in the cellulose ether-modified terpene resin segment, the higher the average binding force of the star-grafted modified liquid styrene-butadiene rubber, and the better the wet-slip resistance, high-temperature flow resistance, and adhesion of the liquid styrene-butadiene rubber.

[0030] In some embodiments of the present invention, the cellulose ether content in the cellulose ether-modified terpene resin segment can be 10 wt%, 20 wt%, 30 wt%, 40 wt%, or any value within a range consisting of any two of the foregoing values. The terpene resin content can be 60 wt%, 70 wt%, 80 wt%, 90 wt%, or any value within a range consisting of any two of the foregoing values.

[0031] In some specific embodiments of the present invention, preferably, the coupling agent is selected from divinylbenzene.

[0032] In some specific embodiments of the present invention, in the modified liquid styrene-butadiene rubber, the amount of the coupling agent is relatively small, and the polymer segment formed by the coupling agent is used as the core. The core formed by the coupling agent is a macromolecular active species, and the macromolecular active species provides the polymer with multiple reactive active points that can further initiate polymerization of the reaction monomers, thereby initiating polymerization of the monomers to form polymer segments. The proportion of the polymer segment formed by the coupling agent itself is very small relative to the amount of the macromolecular polymer, and the content can be excluded from the polymer proportion. The amount of the coupling agent has been described in the text.

[0033] In the present invention, functionality refers to the number of active sites on a polymer chain that can chemically react to form new bonds. The more active sites formed, the more polymer segments can be formed by initiating monomer polymerization. The better the branching properties of the modified liquid styrene-butadiene rubber, the greater the functionality. By characterizing and analyzing the polymer segments, the amount of polymer segments formed by the coupling agent can be determined based on the polymer functionality.

[0034] In some specific embodiments of the present invention, the modified liquid styrene butadiene rubber has a number average molecular weight of 3,000-25,000 g / mol, a viscosity of 20-60 Pa·s at 25°C, and a functionality of 4-7. High viscosity indicates good adhesive properties of the liquid styrene butadiene rubber; high functionality indicates good branching properties of the modified liquid styrene butadiene rubber.

[0035] A second aspect of the present invention provides a method for preparing a star-shaped grafted modified liquid styrene-butadiene rubber, wherein the preparation method comprises:

[0036] (1) in the presence of an initiator and a polar activator, copolymerizing butadiene and styrene to obtain an active butadiene-styrene copolymer segment;

[0037] (2) performing a coupling reaction on the active butadiene-styrene copolymer segment and a coupling agent to obtain an active chain;

[0038] (3) polymerizing the active chain with a modified terpene resin to obtain the star-shaped grafted modified liquid styrene-butadiene rubber.

[0039] In some specific embodiments of the present invention, the preparation method of the modified terpene resin includes: mixing the terpene resin and a solvent, and then adding cellulose ether to obtain the modified terpene resin.

[0040] In some specific embodiments of the present invention, the cellulose ether is selected from one or more of sodium methyl cellulose, sodium hydroxypropyl methyl cellulose, and sodium carboxymethyl cellulose.

[0041] The invention utilizes a negative ion solution polymerization method to prepare the star-shaped grafted modified liquid styrene butadiene rubber, thereby modifying the liquid styrene butadiene rubber. The method is simple and reliable.

[0042] In the present invention, in step (1), butadiene, styrene monomer and initiator are sequentially added to a polymerization system, and after the first monomer addition is completed, a coupling agent is added to carry out a coupling reaction to obtain the star-shaped grafted modified liquid styrene-butadiene rubber. In step (3), a modified terpene resin is added and polymerized to obtain the star-shaped grafted modified liquid styrene-butadiene rubber.

[0043] In some specific embodiments of the present invention, the coupling reaction is a process in which the polymer segment formed by the coupling agent bonds with the butadiene-styrene copolymer chain via the carbon-carbon double bond contained therein and the vinyl group on the polymer segment to obtain the active chain.

[0044] In some specific embodiments of the present invention, the solvent is selected from one or more of pentane, hexane, octane, heptane, cyclohexane, benzene, toluene and ethylbenzene, preferably cyclohexane.

[0045] In some specific embodiments of the present invention, the polar activator is selected from one or more of diethylene glycol dimethyl ether, tetrahydrofuran, ethyl ether, ethyl methyl ether, anisole, diphenyl ether, ethylene glycol dimethyl ether, triethylamine, tetramethylethylenediamine, and hexamethylphosphonic triamide, preferably one or more of diethylene glycol dimethyl ether, tetrahydrofuran, and tetramethylethylenediamine. A polar organic compound is added as an activator to the polymerization system of the present invention to produce a polarization or solvation effect on the initiator, thereby reducing its degree of association and increasing the initiation reaction rate of an initiator such as n-butyl lithium. The activator can also adjust the reactivity ratio of butadiene and styrene, allowing the two to copolymerize randomly. At the same time, the polar activator can increase the 1,2-structure content in the butadiene unit.

[0046] In some specific embodiments of the present invention, the initiator is selected from one or more of n-butyllithium, sec-butyllithium, methylbutyllithium, phenylbutyllithium, naphthalenelithium, cyclohexyllithium and dodecyllithium, preferably selected from n-butyllithium and / or sec-butyllithium.

[0047] In some specific embodiments of the present invention, the coupling agent is selected from polyvinyl aromatic hydrocarbons, preferably divinylbenzene.

[0048] In some specific embodiments of the present invention, the copolymerization reaction temperature is 50-90° C., the copolymerization reaction pressure is 0.1-0.25 MPa, and the copolymerization reaction time is 20-80 min.

[0049] In some specific embodiments of the present invention, the coupling reaction temperature is 50-90° C., the coupling reaction pressure is 0.1-0.25 MPa, and the coupling reaction time is 60-90 min.

[0050] In some specific embodiments of the present invention, the polymerization reaction temperature is 50-90° C., the polymerization reaction pressure is 0.1-0.25 MPa, and the polymerization reaction time is 60-100 min.

[0051] In some specific embodiments of the present invention, after the reaction is complete, the obtained polymer solution is treated with water. The amount of water used is generally 100-300 times the amount of the initiator used, preferably 150-250 times.

[0052] In some specific embodiments of the present invention, 0.5%-1% of the polymer weight of an antioxidant can be added to the obtained star-shaped grafted modified liquid styrene butadiene rubber, and then high-performance star-shaped grafted modified liquid styrene butadiene rubber is obtained through washing, dehydration and drying.

[0053] In some specific embodiments of the present invention, the mixed monomer of butadiene and styrene is 20-80 parts by weight, wherein butadiene accounts for 60-90wt% of the mixed monomer amount, and styrene accounts for 10-40wt% of the mixed monomer amount; preferably, the mixed monomer of butadiene and styrene is 30-70 parts by weight, wherein the butadiene accounts for 70-90wt% of the mixed monomer amount, and the styrene accounts for 10-30wt% of the mixed monomer amount.

[0054] In some specific embodiments of the present invention, the modified terpene resin is present in an amount of 20-80 parts by weight, wherein the cellulose ether accounts for 10-40 wt% of the modified terpene resin, and the terpene resin accounts for 60-90 wt% of the modified terpene resin; preferably, the modified terpene resin is present in an amount of 30-70 parts by weight, wherein the cellulose ether accounts for 10-30 wt% of the modified terpene resin, and the terpene resin accounts for 70-90 wt% of the modified terpene resin;

[0055] In some specific embodiments of the present invention, the initiator is 0.02-0.2 parts by weight, preferably 0.025-0.1 parts by weight.

[0056] In some specific embodiments of the present invention, the molar ratio of the polar activator to the initiator is 0.1-30:1, preferably 0.1-20:1.

[0057] In some specific embodiments of the present invention, the molar ratio of the coupling agent to the initiator is 0.1-1.5:1, preferably 0.1-1:1.

[0058] In the present invention, the functionality is determined by gel permeation chromatography, and the composition and structure of the star-shaped grafted modified liquid styrene-butadiene rubber can be determined by nuclear magnetic resonance, infrared, GPC, elemental analysis, etc., or by preparing and feeding.

[0059] The third aspect of the present invention provides a star-shaped grafted modified liquid styrene-butadiene rubber obtained by the preparation method, which may have the aforementioned composition and structural characteristics, which will not be described in detail.

[0060] The fourth aspect of the present invention provides an application of the star-shaped grafted modified liquid styrene-butadiene rubber in the field of rubber processing.

[0061] The present invention will be described in detail below through examples.

[0062] Determination of molecular weight: A Viscoteck TDA 302 gel permeation chromatography (GPC) from Agilent Technologies, USA was used to analyze the molecular weight and distribution of the samples.

[0063] Determination of viscosity: Determine according to GJB 2050-1994 using a rotational viscometer and the cone-plate viscometer method.

[0064] Fourier Transform Infrared Spectroscopy (FTIR) Analysis: Analyzed using a Nicolet 560 FTIR instrument (USA) without purification and coated with potassium bromide. This method is used to determine the styrene and butadiene contents in modified liquid styrene-butadiene rubber.

[0065] Determination of peel strength: The average bonding strength was tested using a 5567 universal material testing machine from Instron, USA, in accordance with GB / T7124-2008.

[0066] In the following examples and comparative examples, where specific conditions are not specified, the experiments were conducted under conventional conditions or those recommended by the manufacturer. Reagents and instruments used, where the manufacturer is not specified, are commercially available conventional products. The composition and structure of the modified liquid styrene-butadiene rubber described in the following examples and comparative examples can be determined by nuclear magnetic resonance (NMR), infrared, GPC, elemental analysis, or by preparing and feeding the raw materials.

[0067] Example 1

[0068] 1) Preparation of modified terpene resin: In a reaction kettle, 4212 g of cyclohexane and 374 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 94 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the content of terpene resin in the obtained cellulose ether-modified terpene resin segment was 80 wt % and the content of cellulose ether was 20 wt %).

[0069] 2) In a 15 L stainless steel reactor with a jacket, the system was replaced three times with argon. 4212 g of cyclohexane, 234 g of butadiene, 234 g of styrene, and 44.93 g of tetrahydrofuran were added to the polymerization kettle, followed by 0.624 mol of n-butyl lithium. The temperature was raised to 50° C. and polymerization was carried out for 80 min. After complete conversion of the monomers, the temperature was raised to 80° C. (wherein, the content of butadiene structural units in the resulting butadiene-styrene copolymer segment was 50 wt % and the content of styrene structural units was 50 wt %). 0.249 mol of divinylbenzene was added and coupling was continued. After 60 min of reaction, a mixture of 468 g of the prepared modified terpene resin and 4212 g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60 min. After completion of the reaction, the coupled reaction mixture was treated with water, 100 g of water and 12 g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by wet method and dried to obtain high-performance star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 50wt%, and the content of the butadiene-styrene copolymer segment is 50wt%).

[0070] Example 2

[0071] 1) Preparation of modified terpene resin: In a reaction kettle, 4212 g of cyclohexane and 374 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 94 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the content of terpene resin in the obtained cellulose ether-modified terpene resin segment was 80 wt % and the content of cellulose ether was 20 wt %).

[0072] 2) In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 4212g of cyclohexane, 234g of butadiene, 234g of styrene, and 29.95g of tetrahydrofuran were added to the polymerization kettle, followed by 0.416mol of n-butyllithium. The temperature was raised to 50°C and polymerization was carried out for 80min. After complete conversion of the monomers, the temperature was raised to 80°C (wherein the content of butadiene structural units in the obtained butadiene-styrene copolymer segment was 50wt% and the content of styrene structural units was 50wt%). 0.167mol of divinylbenzene was added and coupling was continued. After 60min of reaction, a mixture of 468g of the prepared modified terpene resin and 4212g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60min. After completion of the reaction, the coupled reaction mixture was treated with water, 100g of water and 12g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by wet method and dried to obtain high-performance star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 50wt%, and the content of the butadiene-styrene copolymer segment is 50wt%).

[0073] Example 3

[0074] 1) Preparation of modified terpene resin: In a reaction kettle, 4212 g of cyclohexane and 327 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 141 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the content of terpene resin in the obtained cellulose ether-modified terpene resin segment was 70 wt % and the content of cellulose ether was 30 wt %).

[0075] 2) In a 15 L stainless steel reactor with a jacket, the system was replaced three times with argon. 4212 g of cyclohexane, 234 g of butadiene, 234 g of styrene, and 44.93 g of tetrahydrofuran were added to the polymerization kettle, followed by 0.936 mol of n-butyl lithium. The temperature was raised to 50° C. and polymerization was carried out for 80 min. After complete conversion of the monomers, the temperature was raised to 80° C. (wherein, the content of butadiene structural units in the resulting butadiene-styrene copolymer segment was 50 wt % and the content of styrene structural units was 50 wt %). 0.374 mol of divinylbenzene was added and coupling was continued. After 60 min of reaction, a mixture of 468 g of the prepared modified terpene resin and 4212 g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60 min. After completion of the reaction, the coupled reaction mixture was treated with water, 100 g of water and 12 g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by a wet method and dried to obtain a star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 50wt%, and the content of the butadiene-styrene copolymer segment is 50wt%).

[0076] Example 4

[0077] 1) Preparation of modified terpene resin: In a reaction kettle, 4212 g of cyclohexane and 327 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 141 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the content of terpene resin in the obtained cellulose ether-modified terpene resin segment was 70 wt % and the content of cellulose ether was 30 wt %).

[0078] 2) In a 15 L stainless steel reactor with a jacket, the system was replaced three times with argon. 4212 g of cyclohexane, 234 g of butadiene, 234 g of styrene, and 44.93 g of tetrahydrofuran were added to the polymerization kettle, followed by 0.624 mol of n-butyllithium. The temperature was raised to 50° C. and polymerization was carried out for 80 min. After complete conversion of the monomers, the temperature was raised to 80° C. (wherein, the content of butadiene structural units in the resulting butadiene-styrene copolymer segment was 50 wt % and the content of styrene structural units was 50 wt %). 0.249 mol of divinylbenzene was added and coupling was continued. After 60 min of reaction, a mixture of 468 g of the prepared modified terpene resin and 4212 g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60 min. After completion of the reaction, the coupled reaction mixture was treated with water, 100 g of water and 12 g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by a wet method and dried to obtain a star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 50wt%, and the content of the butadiene-styrene copolymer segment is 50wt%).

[0079] Example 5

[0080] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 197 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 84 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the terpene resin content in the obtained cellulose ether-modified terpene resin segment was 70 wt % and the cellulose ether content was 30 wt %).

[0081] 2) In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 5897g of cyclohexane, 468g of butadiene, 187g of styrene, and 37.73g of tetrahydrofuran were added to the polymerization kettle, followed by 0.524mol of n-butyllithium. The temperature was raised to 50°C and polymerization was carried out for 80min. After complete conversion of the monomers, the temperature was raised to 80°C (wherein the content of butadiene structural units in the obtained butadiene-styrene copolymer segment was 70wt% and the content of styrene structural units was 30wt%). 0.212mol of divinylbenzene was added and coupling was continued. After 60min of reaction, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60min. After completion of the reaction, the coupled reaction mixture was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).

[0082] Example 6

[0083] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 225 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 56 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the content of terpene resin in the obtained cellulose ether-modified terpene resin segment was 80 wt % and the content of cellulose ether was 20 wt %).

[0084] 2) In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 5897g of cyclohexane, 468g of butadiene, 187g of styrene, and 23.58g of tetrahydrofuran were added to the polymerization kettle, followed by 0.327mol of n-butyllithium. The temperature was raised to 50°C and polymerization was carried out for 80min. After complete conversion of the monomers, the temperature was raised to 80°C (wherein the content of butadiene structural units in the resulting butadiene-styrene copolymer segment was 70wt% and the content of styrene structural units was 30wt%). 0.131mol of divinylbenzene was added and coupling was continued. After 60min of reaction, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60min. After completion of the reaction, the coupled reaction mixture was treated with water, 100g of water and 12g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).

[0085] Example 7

[0086] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 225 g of terpene resin (accounting for 80 wt% of the modified terpene resin segment) were added, heated to 80° C., and stirred until completely dissolved. Then, 56 g of dissolved sodium methylcellulose (accounting for 20 wt% of the modified terpene resin segment) was added and stirred until uniformly mixed to obtain a modified terpene resin (wherein, the terpene resin content in the obtained cellulose ether-modified terpene resin segment was 80 wt% and the cellulose ether content was 20 wt%).

[0087] 2) In a 15 L stainless steel reactor with a jacket, the system was replaced three times with argon. 5897 g of cyclohexane, 557 g of butadiene, 98 g of styrene, and 37.73 g of tetrahydrofuran were added to the polymerization kettle, followed by 0.524 mol of n-butyllithium. The temperature was raised to 50° C. and polymerization was carried out for 80 min. After complete conversion of the monomers, the temperature was raised to 80° C. (wherein, the content of butadiene structural units in the resulting butadiene-styrene copolymer segment was 85 wt % and the content of styrene structural units was 15 wt %). 0.212 mol of divinylbenzene was added and coupling was continued. After 60 min of reaction, a mixture of 281 g (30 wt % of the total) of the prepared modified terpene resin and 2527 g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60 min. After completion of the reaction, the coupled reaction mixture was treated with water, 100 g of water and 12 g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).

[0088] Example 8

[0089] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 197 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 84 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the terpene resin content in the obtained cellulose ether-modified terpene resin segment was 70 wt % and the cellulose ether content was 30 wt %).

[0090] 2) In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 5897g of cyclohexane, 557g of butadiene, 98g of styrene, and 53.90g of tetrahydrofuran were added to the polymerization kettle, followed by 0.504mol of n-butyllithium. The temperature was raised to 50°C and polymerization was carried out for 80min. After complete conversion of the monomers, the temperature was raised to 80°C (wherein the content of butadiene structural units in the obtained butadiene-styrene copolymer segment was 85wt% and the content of styrene structural units was 15wt%). 0.301mol of divinylbenzene was added to continue coupling. After 60min of reaction, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60min. After completion of the reaction, the coupled reaction mixture was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).

[0091] Example 9

[0092] 1) Preparation of modified terpene resin: In a reaction kettle, 2611 g of cyclohexane and 211 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 70 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the content of terpene resin in the obtained cellulose ether-modified terpene resin segment was 75 wt % and the content of cellulose ether was 25 wt %).

[0093] 2) In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 5813g of cyclohexane, 478g of butadiene, 84g of styrene, and 37.73g of tetrahydrofuran were added to the polymerization kettle, followed by 0.281mol of n-butyllithium. The temperature was raised to 50°C and polymerization was carried out for 80min. After complete conversion of the monomers, the temperature was raised to 80°C (wherein the content of butadiene structural units in the obtained butadiene-styrene copolymer segment was 85wt% and the content of styrene structural units was 15wt%). 0.212mol of divinylbenzene was added and coupling was continued. After 60min of reaction, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60min. After completion of the reaction, the coupled reaction mixture was treated with water, 100g of water and 12g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).

[0094] Example 10

[0095] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 225 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 56 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the content of terpene resin in the obtained cellulose ether-modified terpene resin segment was 80 wt % and the content of cellulose ether was 20 wt %).

[0096] 2) In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 5897g of cyclohexane, 468g of butadiene, 187g of styrene, and 23.58g of tetrahydrofuran were added to the polymerization kettle, followed by 0.197mol of n-butyllithium. The temperature was raised to 50°C and polymerization was carried out for 80min. After complete conversion of the monomers, the temperature was raised to 80°C (wherein the content of butadiene structural units in the obtained butadiene-styrene copolymer segment was 70wt% and the content of styrene structural units was 30wt%). 0.197mol of divinylbenzene was added and coupling was continued. After 60min of reaction, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60min. After completion of the reaction, the coupled reaction mixture was treated with water, 100g of water and 12g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).

[0097] Example 11

[0098] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 225 g of terpene resin were added, heated to 80° C., and stirred until completely dissolved. Then, 56 g of dissolved sodium methyl cellulose was added and stirred to mix uniformly to obtain a modified terpene resin (wherein, the content of terpene resin in the obtained cellulose ether-modified terpene resin segment was 80 wt % and the content of cellulose ether was 20 wt %).

[0099] 2) In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. 5897g of cyclohexane, 468g of butadiene, 187g of styrene, and 23.58g of tetrahydrofuran were added to the polymerization kettle, followed by 0.143mol of n-butyllithium. The temperature was raised to 50°C and polymerization was carried out for 80min. After complete conversion of the monomers, the temperature was raised to 80°C (wherein the content of butadiene structural units in the resulting butadiene-styrene copolymer segment was 70wt% and the content of styrene structural units was 30wt%). 0.172mol of divinylbenzene was added and coupling was continued. After 60min of reaction, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization kettle and the reaction was continued for 60min. After completion of the reaction, the coupled reaction mixture was treated with water, 100g of water and 12g of antioxidant 1010 were added, and the mixture was stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).

[0100] Comparative Example 1

[0101] The method of Example 1 was followed, except that the terpene resin was not modified, that is, the styrene-butadiene rubber segment and the terpene resin were directly coupled and then coagulated.

[0102] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, the system is replaced three times with argon. 4212g of cyclohexane, 234g of butadiene (accounting for 50wt% of the mixed monomer amount), 234g of styrene (accounting for 50wt% of the mixed monomer amount), and 44.93g of tetrahydrofuran are added to the polymerization kettle, followed by 0.624mol of n-butyl lithium. The mixture is heated to 50°C and polymerized for 80min. After the monomers are fully converted, the temperature is raised to 80°C, 0.249mol of divinylbenzene is added, and coupling is continued. After the reaction is completed for 60min, a mixture of 468g of terpene resin (accounting for 50wt% of the total amount) and 4212g of cyclohexane is pressed into the polymerization kettle and the reaction is continued for 60min. After the reaction is completed, the coupled reaction mixture is treated with water, 100g of water and 12g of antioxidant 1010 are added, and stirred. The rubber solution is subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0103] Comparative Example 2

[0104] The method of Example 2 was followed, except that the terpene resin was not modified, that is, the styrene-butadiene rubber segment and the terpene resin were directly coupled and then coagulated.

[0105] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, the system is replaced three times with argon. 4212g of cyclohexane, 234g of butadiene (accounting for 50wt% of the mixed monomer amount), 234g of styrene (accounting for 50wt% of the mixed monomer amount), and 29.95g of tetrahydrofuran are added to the polymerization kettle, followed by 0.416mol of n-butyl lithium. The temperature is raised to 50°C and polymerization is carried out for 80 minutes. After the monomers are fully converted, the temperature is raised to 80°C, 0.167mol of divinylbenzene is added, and coupling is continued. After the reaction is completed for 60 minutes, a mixture of 468g of terpene resin (accounting for 50wt% of the total amount) and 4212g of cyclohexane is pressed into the polymerization kettle and the reaction is continued for 60 minutes. After the reaction is completed, the coupled reaction mixture is treated with water, 100g of water and 12g of antioxidant 1010 are added, and stirred. The rubber solution is subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0106] Comparative Example 3

[0107] The method of Example 3 was followed, except that the terpene resin was not modified, that is, the styrene-butadiene rubber segment and the terpene resin were directly coupled and then coagulated.

[0108] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, the system is replaced three times with argon. 4212g of cyclohexane, 234g of butadiene (accounting for 50wt% of the mixed monomer amount), 234g of styrene (accounting for 50wt% of the mixed monomer amount), and 44.93g of tetrahydrofuran are added to the polymerization kettle, followed by 0.936mol of n-butyl lithium. The temperature is raised to 50°C and polymerization is carried out for 80 minutes. After the monomers are fully converted, the temperature is raised to 80°C, 0.374mol of divinylbenzene is added, and coupling is continued. After the reaction is completed for 60 minutes, a mixture of 468g of terpene resin (accounting for 50wt% of the total amount) and 4212g of cyclohexane is pressed into the polymerization kettle and the reaction is continued for 60 minutes. After the reaction is completed, the coupled reaction mixture is treated with water, 100g of water and 12g of antioxidant 1010 are added, and stirred. The rubber solution is subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0109] Comparative Example 4

[0110] The method of Example 4 was followed, except that the terpene resin was not modified, that is, the styrene-butadiene rubber segment and the terpene resin were directly coupled and then coagulated.

[0111] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, the system is replaced three times with argon. 4212g of cyclohexane, 234g of butadiene (accounting for 50wt% of the mixed monomer amount), 234g of styrene (accounting for 50wt% of the mixed monomer amount), and 44.93g of tetrahydrofuran are added to the polymerization kettle, followed by 0.624mol of n-butyl lithium. The mixture is heated to 50°C and polymerized for 80min. After the monomers are fully converted, the temperature is raised to 80°C, 0.249mol of divinylbenzene is added, and coupling is continued. After the reaction is completed for 60min, a mixture of 468g of terpene resin (accounting for 50wt% of the total amount) and 4212g of cyclohexane is pressed into the polymerization kettle and the reaction is continued for 60min. After the reaction is completed, the coupled reaction mixture is treated with water, 100g of water and 12g of antioxidant 1010 are added, and the mixture is stirred. The rubber solution is subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0112] Comparative Example 5

[0113] The method of Example 5 was followed, except that no coupling agent was added for the coupling reaction. That is, after the polymerization reaction of butadiene and styrene was completed, the modified terpene resin was added and mixed.

[0114] The specific preparation steps are as follows: 1) Preparation of modified terpene resin: In a reaction kettle, add 2527 g of cyclohexane and 187 g of terpene resin (accounting for 70 wt% of the modified terpene resin segment), heat to 80°C, and stir until completely dissolved. Then, add 94 g of dissolved sodium methylcellulose (accounting for 30 wt% of the modified terpene resin segment) and stir to mix thoroughly to produce the modified terpene resin. 2) In a jacketed 15 L stainless steel reaction kettle, purge the system three times with argon. 5897g of cyclohexane, 468g of butadiene (70wt% of the total monomer mixture), 187g of styrene (30wt% of the total monomer mixture), and 37.73g of tetrahydrofuran were added to a polymerization kettle. 0.281mol of n-butyl lithium was then added. The temperature was raised to 50°C and polymerization was carried out for 80 minutes. After complete monomer conversion, the temperature was raised to 80°C and the reaction was continued for 60 minutes. A mixture of 281g of the prepared modified terpene resin (30wt% of the total amount) and 2527g of cyclohexane was then pressed into the polymerization kettle. After mixing for 20 minutes, 100g of water and 12g of antioxidant 1010 were added and stirred. The rubber solution was subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0115] Comparative Example 6

[0116] The method of Example 6 was followed, except that no coupling agent was added for the coupling reaction. That is, after the polymerization reaction of butadiene and styrene was completed, the modified terpene resin was added and mixed.

[0117] The specific preparation steps are as follows: 1) Preparation of modified terpene resin: In a reaction kettle, add 2527 g of cyclohexane and 234 g of terpene resin (80 wt% of the modified terpene resin segment), heat to 80°C, and stir until completely dissolved. Then, add 47 g of dissolved sodium methylcellulose (20 wt% of the modified terpene resin segment) and stir to mix thoroughly to produce the modified terpene resin. 2) In a jacketed 15 L stainless steel reaction kettle, purge the system three times with argon. 5897g of cyclohexane, 468g of butadiene (70wt% of the total monomer mixture), 187g of styrene (30wt% of the total monomer mixture), and 23.58g of tetrahydrofuran were added to a polymerization kettle, followed by 0.327mol of n-butyl lithium. The mixture was heated to 50°C and polymerized for 80 minutes. After complete monomer conversion, the temperature was raised to 80°C and the reaction was continued for 60 minutes. A mixture of 281g of the prepared modified terpene resin (30wt% of the total amount) and 2527g of cyclohexane was then pressed into the polymerization kettle. After mixing for 20 minutes, 100g of water and 12g of antioxidant 1010 were added and stirred. The rubber solution was subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0118] Comparative Example 7

[0119] The method of Example 7 was followed, except that the terpene resin was not modified. That is, the styrene-butadiene rubber segment and the terpene resin were directly coupled, and then dissolved sodium carboxymethyl cellulose was added and then coagulation was carried out.

[0120] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. To a polymerization kettle were added 5897 g of cyclohexane, 557 g of butadiene (85 wt % of the total monomer content), 98 g of styrene (15 wt % of the total monomer content), and 37.73 g of tetrahydrofuran. 0.524 mol of n-butyl lithium was then added, and the mixture was heated to 50° C. for 80 min. After complete monomer conversion, the mixture was heated to 80° C., 0.212 mol of divinylbenzene was added, and coupling was continued. After 60 min of reaction, a mixture of 225 g of terpene resin (21 wt % of the total content) and 1685 g of cyclohexane was added and pressed into the polymerization kettle. The reaction was continued for 60 min. A mixture of 56 g of dissolved sodium carboxymethyl cellulose (9 wt % of the total content) and 842 g of cyclohexane was then added. After mixing for 20 min, the coupled reaction mixture was treated with water, 100 g of water, and 12 g of antioxidant 1010 were added and stirred. The rubber solution was subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0121] Comparative Example 8

[0122] The method of Example 8 was followed, except that the terpene resin was not modified. That is, the styrene-butadiene rubber segment and the terpene resin were directly coupled, and then dissolved sodium carboxymethyl cellulose was added and then coagulation was carried out.

[0123] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, the system was replaced three times with argon. To a polymerization kettle were added 5897 g of cyclohexane, 557 g of butadiene (85 wt% of the total amount of the mixed monomers), 98 g of styrene (15 wt% of the total amount of the mixed monomers), and 53.90 g of tetrahydrofuran. 0.504 mol of n-butyl lithium was then added, the temperature was raised to 50° C., and polymerization was continued for 80 min. After complete conversion of the monomers, the temperature was raised to 80° C., 0.301 mol of divinylbenzene was added, and coupling was continued. After 60 min of reaction, a mixture of 197 g of terpene resin (21 wt% of the total amount) and 1685 g of cyclohexane was added and pressed into the polymerization kettle. The reaction was continued for 60 min. A mixture of 84 g of dissolved sodium carboxymethyl cellulose (9 wt% of the total amount) and 842 g of cyclohexane was added. After mixing for 20 min, the coupled reaction mixture was treated with water, 100 g of water, 12 g of antioxidant 1010 were added, and the mixture was stirred. The rubber solution was subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0124] Comparative Example 9

[0125] The method of Example 10 was followed, except that the terpene resin was not modified. That is, the styrene-butadiene rubber segment and the terpene resin were directly coupled, and then dissolved sodium carboxymethyl cellulose was added and then coagulation was carried out.

[0126] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, argon gas was introduced to replace the system three times. To a polymerization kettle were added 5897 g of cyclohexane, 468 g of butadiene (70 wt % of the total monomer content), 187 g of styrene (30 wt % of the total monomer content), and 23.58 g of tetrahydrofuran. 0.262 mol of n-butyl lithium was then added, the mixture was heated to 50° C., and polymerization was continued for 80 min. After complete monomer conversion, the mixture was heated to 80° C., 0.131 mol of divinylbenzene was added, and coupling was continued. After 60 min of reaction, a mixture of 225 g of terpene resin (24 wt % of the total content) and 2527 g of cyclohexane was added and pressed into the polymerization kettle. The reaction was continued for 60 min. A mixture of 56 g of dissolved sodium carboxymethyl cellulose (6 wt % of the total content) and 842 g of cyclohexane was added. After mixing for 20 min, the coupled reaction mixture was treated with water, 100 g of water, and 12 g of antioxidant 1010 were added, and the mixture was stirred. The rubber solution was subjected to wet coagulation and drying to obtain liquid styrene-butadiene rubber.

[0127] Relevant performance measurements were performed on the results of Examples 1-11 and Comparative Examples 1-9. The results are shown in Table 1, wherein the styrene content is based on the total modified liquid styrene-butadiene rubber.

[0128] Table 1

[0129] As can be seen from the results in Table 1, in the synthesis process of the star-shaped grafted modified liquid styrene butadiene rubber of the present invention, a secondary feeding method (dividing the feeding of butadiene-styrene copolymer segment monomers and the feeding of cellulose ether modified terpene resin segments) is adopted to synthesize the star-shaped grafted modified liquid styrene butadiene rubber having mixed arms (such as polybutadiene styrene arms and modified terpene resin polymer arms). Due to the presence of the mixed arms, the polybutadiene-styrene rubber and the modified terpene resin are chained together through the polymer segment core formed by the coupling agent, thereby realizing the combination of different polymer molecular chains at the short-range structural level of the polymer chain, promoting the coordinated optimization of various performance properties of the product, and enabling the modified rubber to have good compatibility, stability and adhesion.

[0130] Average bonding strength refers to the average value of the peel strength between the adhesive and the substrate during a peel test, typically expressed as stress per unit area. It can be used to compare the adhesive adhesion properties of the liquid styrene-butadiene rubber in Examples and Comparative Examples under different conditions. A comparison between Examples 1-10 and Comparative Examples 1-9 shows that the average bonding strength of the grafted modified rubber increases with increasing molecular weight and viscosity. The higher the functionality and degree of branching of the grafted modified rubber, the greater the average bonding strength.

[0131] As can be seen from Examples 1-11, as the polymer molecular weight increases, the polymer viscosity also gradually increases, and the average binding force of the modified rubber also gradually increases. As the functionality of the polymer increases, the average binding force of the modified rubber also gradually increases, and the adhesion performance of the grafted modified rubber is better. A comparison of the Examples and the corresponding Comparative Examples shows that the average binding force values ​​of the Examples are higher than those of the Comparative Examples, indicating that the adhesion performance of the Comparative Examples is not as good as the liquid styrene butadiene rubber samples in the Examples. The functionality of the liquid styrene butadiene rubber in the Examples is also higher. The higher the functionality, the greater the branching degree of the liquid styrene butadiene rubber and the greater the viscosity. The higher the viscosity, the better the adhesion performance of the liquid styrene butadiene rubber.

[0132] Comparison of Examples 1-4 and Comparative Examples 1-4 reveals that the viscosity and average bonding strength of the grafted modified rubber increased after modification of the terpene resin, indicating that the adhesion properties of the modified liquid styrene-butadiene rubber in the Examples are better than those in the Comparative Examples, demonstrating that the modified cellulose ether provides a good bonding effect. The cellulose ether-modified terpene resin segments affect the average bonding strength of the prepared rubber, and the rubber structure of the present invention exhibits excellent adhesion.

[0133] A comparison of Examples 5-6 and Comparative Example 5-6 reveals that after the coupling agent is added to couple the modified terpene resin, the modified liquid styrene-butadiene rubber forms mixed arms. Consequently, the viscosity, functionality, and average bonding strength of the star-shaped modified liquid styrene-butadiene rubber in Examples 5-6 are all greater than those in Comparative Example 5-6, indicating that the star-shaped modified liquid styrene-butadiene rubber in Examples 5-6 exhibits superior adhesion properties compared to the corresponding Comparative Example 5-6. Therefore, the coupling effect of the divinylbenzene coupling agent can link the polybutadiene-styrene rubber and the modified terpene resin together, promoting the synergistic optimization of various product properties and imparting excellent compatibility, stability, and adhesion to the modified rubber.

[0134] From the results in Table 1, it can be seen that when Example 1 is compared with Example 3, and when Example 2 is compared with Example 4, under the same content of styrene and butadiene, the content of terpene resin in the cellulose ether modified terpene resin segment increases, the average binding force of the modified rubber prepared therefrom increases, and the adhesion of the rubber is better.

[0135] Examples 1-11, using the star-shaped grafting modification of the present invention, exhibit high viscosity, a high degree of branching, and significantly improved adhesive compatibility. The greater the adhesion and viscosity, the better the adhesion of the liquid styrene-butadiene rubber. This demonstrates that the modified liquid styrene-butadiene rubber exhibits advantages such as wet-slip resistance, high-temperature flow resistance, and good adhesion, broadening its application range.

[0136] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.

Claims

1. A star-shaped grafted modified liquid styrene-butadiene rubber, It is characterized in that The modified liquid styrene butadiene rubber comprises a polymer segment from a coupling agent and a plurality of butadiene-styrene copolymer segments and a cellulose ether modified terpene resin segment grafted on the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.

2. The modified liquid styrene-butadiene rubber according to claim 1, It is characterized in that In the modified liquid styrene-butadiene rubber, based on the sum of the weights of the butadiene-styrene copolymer segment and the cellulose ether-modified terpene resin segment, the content of the cellulose ether-modified terpene resin segment is 20-80wt%, and the content of the butadiene-styrene copolymer segment is 20-80wt%; Preferably, in the butadiene-styrene copolymer segment, the content of the butadiene structural unit is 50-90wt%, and the content of the styrene structural unit is 10-50wt%; Preferably, in the cellulose ether-modified terpene resin segment, the content of the cellulose ether is 10-40wt%, and the content of the terpene resin is 60-90wt%; Preferably, the coupling agent is selected from divinylbenzene.

3. The modified liquid styrene-butadiene rubber according to claim 1 or 2, It is characterized in that The modified liquid styrene-butadiene rubber has a number average molecular weight of 3000-25000 g / mol, a viscosity of 20-60 Pa·S at 25° C., and a functionality of 4-7.

4. A method for preparing a star-shaped grafted modified liquid styrene-butadiene rubber, It is characterized in that The preparation method comprises: (1) in the presence of an initiator and a polar activator, copolymerizing butadiene and styrene to obtain an active butadiene-styrene copolymer segment; (2) subjecting the active butadiene-styrene copolymer segment to a coupling reaction with a coupling agent to obtain an active chain; (3) subjecting the active chain to polymerization reaction with a modified terpene resin to obtain the star-shaped grafted modified liquid styrene-butadiene rubber.

5. The preparation method according to claim 4, It is characterized in that The preparation method of the modified terpene resin comprises: mixing the terpene resin and a solvent, and then adding cellulose ether to obtain the modified terpene resin.

6. The preparation method according to claim 4 or 5, It is characterized in that The solvent is selected from one or more of pentane, hexane, octane, heptane, cyclohexane, benzene, toluene and ethylbenzene, preferably cyclohexane; Preferably, the polar activator is selected from diethylene glycol dimethyl ether, tetrahydrofuran, ethyl ether, ethyl methyl ether, anisole, One or more selected from diphenyl ether, ethylene glycol dimethyl ether, triethylamine, tetramethylethylenediamine and hexamethylphosphonic triamide, preferably one or more selected from diethylene glycol dimethyl ether, tetrahydrofuran and tetramethylethylenediamine; Preferably, the initiator is selected from one or more of n-butyllithium, sec-butyllithium, methylbutyllithium, phenylbutyllithium, naphthalenelithium, cyclohexyllithium and dodecyllithium, preferably selected from n-butyllithium and / or sec-butyllithium; Preferably, the coupling agent is selected from polyvinyl aromatic hydrocarbons, preferably from divinyl benzene.

7. The preparation method according to any one of claims 4 to 6, It is characterized in that The copolymerization reaction temperature is 50-90°C, the copolymerization reaction pressure is 0.1-0.25MPa, and the copolymerization reaction time is 20-80min; Preferably, the coupling reaction temperature is 50-90°C, the coupling reaction pressure is 0.1-0.25MPa, and the coupling reaction time is 60-90min; Preferably, the polymerization reaction temperature is 50-90° C., the polymerization reaction pressure is 0.1-0.25 MPa, and the polymerization reaction time is 60-100 min.

8. The preparation method according to any one of claims 4 to 7, It is characterized in that The mixed monomer of butadiene and styrene is 20-80 parts by weight, wherein butadiene accounts for 60-90wt% of the mixed monomer, and styrene accounts for 10-40wt% of the mixed monomer; preferably, the mixed monomer of butadiene and styrene is 30-70 parts by weight, wherein butadiene accounts for 70-90wt% of the mixed monomer, and styrene accounts for 10-30wt% of the mixed monomer; Preferably, the modified terpene resin is 20-80 parts by weight, wherein the cellulose ether accounts for 10-40wt% of the modified terpene resin, and the terpene resin accounts for 60-90wt% of the modified terpene resin; preferably, the modified terpene resin is 30-70 parts by weight, wherein the cellulose ether accounts for 10-30wt% of the modified terpene resin, and the terpene resin accounts for 70-90wt% of the modified terpene resin; Preferably, the initiator is 0.02-0.2 parts by weight, preferably 0.025-0.1 parts by weight; Preferably, the molar ratio of the polar activator to the initiator is 0.1-30:1, preferably 0.1-20:1; Preferably, the molar ratio of the coupling agent to the initiator is 0.1-1.5:1, preferably 0.1-1:

1.

9. The star-shaped grafted modified liquid styrene-butadiene rubber obtained by the preparation method described in any one of claims 4 to 8.

10. Use of the star-shaped grafted modified liquid styrene-butadiene rubber according to any one of claims 1 to 3 and 9 in the field of rubber processing.

Citation Information

Patent Citations

  • A ternary copolymer rubber with a star-shaped block structure, its preparation method and its application

    CN102295733A

  • Preparation method of star-shaped solution polymerized butadiene styrene rubber with wide molecular weight distribution

    CN102344529A

  • Preparation method of high-performance liquid styrene butadiene rubber

    CN103539949A

  • Hot-melt adhesive agent

    CN105229105A

  • Asymmetric star type styrene-butadiene rubber, and preparation method thereof and applications of asymmetric star type styrene-butadiene rubber as sole rubber material

    CN107501488A

Cited By

  • Cold-resistant and compression-resistant hydrogenated nitrile rubber for oil field and preparation method thereof

    CN119899338A