Porous glass with multi-directional communicating pores, and atomizing core and electronic atomizer

By designing a multi-directional communication hole structure in porous glass, the problems of uneven structure and poor connectivity of the existing porous glass are solved, the transmission speed of the atomized liquid matrix and the suction experience of electronic cigarettes are improved, and the atomized core is extended service life.

WO2024239802A1PCT designated stage expired Publication Date: 2024-11-28SMOORE INTERNATIONAL HOLDINGS LIMITED +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/085461
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-04-02
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The pore structure of existing pores and poor connectivity of porous glasses leads to slow transmission speed of the atomized liquid matrix, which easily leads to insufficient oil supply and carbon deposits, affecting the suction experience and aroma reduction of the electronic atomizer.

Method used

Porous glass with multi-directional communication holes is prepared by molding glass and fiber materials and pore-forming agent powder. The spherical holes are designed to communicate with at least 6 holes around it to improve porosity and connectivity, reduce the content of non-communication holes, and improve oil conduction. Performance and structural stability.

Benefits of technology

It improves the transmission speed of the atomized liquid matrix, reduces insufficient oil supply and carbon deposits, improves the taste and suction experience of the electronic cigarette, and extends the service life of the atomized core.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024085461_28112024_PF_FP_ABST
    Figure CN2024085461_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of porous materials, and particularly relates to porous glass with multi-directional communicating pores, and an atomizing core and an electronic atomizer. The porous glass with multi-directional communicating pores provided in the present application comprises a framework and multi-directional communicating pores, which are spherical pores and are each at least in communication with six pores surrounding same. In the present application, the structures of the communicating pores are defined, such that during transferring an atomizing liquid substrate such as e-liquid, the transfer speed is high, and the difference between transfer paths is small; and by means of multi-channel communication, the current problem of insufficient local supply of liquid or unbalanced supply of liquid to the atomizing core is reduced, such that local burning occurring during vaping is alleviated, thereby improving the taste and vaping experience of an electronic cigarette.
Need to check novelty before this filing date? Find Prior Art

Description

Porous glass with multi-directional connecting holes, atomizing core and electronic atomizer

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on May 19, 2023, with application number 202310575203.2 and invention name “A porous glass with multi-directional connecting holes, an atomizing core and an electronic atomizer”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application belongs to the technical field of porous materials, and specifically relates to a porous glass with multi-directional interconnected holes, an atomizing core, and an electronic atomizer. Background Art

[0004] An electronic vaporizer is a product that transforms a vaporized medium into vapor through atomization and other means for the user to inhale. The atomizer core is the core component of the electronic vaporizer and plays a crucial role in its performance, including taste and aerosol volume.

[0005] Most closed electronic atomizers use porous ceramics as the atomization core. Most of them use diatomaceous earth, silicon oxide, aluminum oxide, etc. as raw materials, add glass powder, pore-forming agents, etc., and produce porous ceramics by sintering the prepared particles. The use of porous ceramics as the atomization core has the characteristics of good uniformity, long life, delicate taste, and high degree of mechanization. However, the porous ceramic heating element has a certain proportion of semi-closed pores and fine pores, which easily cause the adsorption of low-viscosity components in the atomization medium, thereby affecting the suction taste and aroma restoration. At the same time, the microscopic surface of the porous ceramic heating element is rough and has low continuity, and it cannot be used with a thin film heating film.

[0006] Compared with porous ceramics, porous glass has the characteristics of smooth and continuous microstructure, low proportion of micro-nanopores, and is not easy to adsorb the atomized medium, which to a certain extent improves the taste and aroma restoration of electronic atomizers. However, the porous glass in the prior art has an uneven pore structure and poor pore connectivity, which makes the path length of the atomized liquid matrix (such as smoke oil) vary greatly. In particular, the presence of one-way connected open holes contained in the porous material hinders the transmission speed of the atomized liquid matrix (smoke oil), resulting in a large difference in the transmission speed of the atomized liquid matrix. In some areas where the transmission speed of the atomized liquid matrix is ​​slow, insufficient oil supply is easily generated during the atomization process, resulting in local coking and carbon deposits, which seriously affect the customer's smoking experience. At the same time, the cumulative effect of carbon deposits will also accelerate the failure of the atomizer core.

[0007] Summary of the Invention

[0008] Therefore, the technical problem to be solved by this application is to overcome the defects of the porous glass in the prior art, such as uneven pore structure, poor connectivity, and easy carbon deposition, thereby providing a porous glass, atomizing core and electronic atomizer with multi-directional connected holes.

[0009] To this end, this application provides the following technical solutions:

[0010] The present application provides a porous glass with multi-directional connected holes, comprising a skeleton and the multi-directional connected holes, wherein the multi-directional connected holes are spherical holes connected to at least six holes around them.

[0011] Optionally, the multi-directional connecting hole is connected to 6-12 holes around it;

[0012] Optionally, the multi-directional connecting hole is connected to 7-10 holes around it.

[0013] Optionally, the skeleton comprises a fiber skeleton serving as a scaffolding structure and a glass covering adhesive layer serving as an adhesive stabilization layer, and the total volume of the skeleton accounts for 25-35%;

[0014] Wherein, the glass covering adhesive layer includes glass powder and residual fiber particle components that have not formed a fiber skeleton.

[0015] Optionally, the fiber skeleton has a length of 75-150 microns and a diameter of 15-45 microns;

[0016] Optionally, in the porous glass having multi-directional interconnected pores, the weight percentage of the fiber skeleton is in the range of 12-45%;

[0017] Optionally, in the porous glass having multi-directional interconnected pores, the weight percentage of the glass-covered adhesive layer is in the range of 55-88%.

[0018] Optionally, the porosity of the porous glass is 65-75%;

[0019] Optionally, the porosity is 70-75%.

[0020] Optionally, the pore diameter of the multidirectional connecting pores is 70-80 microns, the average diameter of the pore throats of the connecting channels between the pores is 25-45 microns, and the pore throats are distributed in the 5-60 micron area, wherein more than 50% of the pore throats are distributed in the 20-45 micron area.

[0021] Optionally, the average diameter of the pore throats is 28-36 microns, the pore throats are distributed in the 10-55 micron region, and more than 90% of the pore throats are distributed in the 20-45 micron region.

[0022] Optionally, the average diameter of the pore throats is about 29-35 microns, the pore throats are distributed in the range of 12-50 microns, and the proportion of pore throats distributed in the range of 20-45 microns is greater than 95%;

[0023] Optionally, the pore throats are all distributed in the 20-45 micron region.

[0024] The present application also provides an atomizing core, which uses the above-mentioned porous glass with multi-directional connecting holes as a substrate, and a heating unit is provided on the substrate.

[0025] Optionally, during the atomization process, the temperature field deviation of the atomizer core is less than 10°C.

[0026] The present application also provides an electronic atomizer, comprising the above-mentioned atomization core.

[0027] Generally, for a rectangular flat-plate atomizer, such as 4×9 mm, or 7×3.5 mm, the porous glass substrate has a thickness of 1 to 3 mm, and optionally, a thickness of 1.2 to 2.5 mm.

[0028] Generally, based on the actual puffing process of people, during the test of electronic cigarette puffing, the electronic cigarette puffing time is set to 3s. For the porous matrix of the electronic cigarette atomization core, the smoke oil is transmitted from the oil inlet surface to the atomization surface through the porous matrix channel. When the time difference of passing through each oil supply channel is higher than 3s, there will be a local oil shortage. For a specific heating element, assuming that the transmission speed of a certain type of atomization medium such as smoke oil is V, the path difference caused by the 3s time difference is 3V. Therefore, for matrix materials of different thicknesses (L), the non-connected pore content allowed by each channel is approximately 3V / L.

[0029] For example, for a substrate with an oil conduction speed of 0.12 mm / s, if the thickness is 1.2 mm, the non-connected pore content allowed in each channel should be less than 30%, that is, the multi-directional connected pores account for at least 70%; when the thickness is 2 mm, the non-connected pore content allowed in each channel should be less than 18%, that is, the multi-directional connected pores account for at least 82%; when the thickness is 2.5 mm, the non-connected pore content allowed in each channel should be less than 14.4%, that is, the multi-directional connected pores account for at least 85.6%. Theoretically, the best embodiment is one in which the multi-directional connected pores account for 100%, which maximizes the uniformity of the heating element structure, and provides ideal structural stability and oil conduction performance.

[0030] Generally, for atomized liquid media such as smoke oil with a lower viscosity, the conduction speed thereof in the porous matrix is ​​faster, and accordingly, the proportion of its multi-directional connected pores can be reduced to a smaller value such as 65%.

[0031] The porous glass with multi-directional interconnected pores provided in the present application is prepared by molding glass and fiber materials and pore-forming agent powder.

[0032] Generally, for the five close-packing patterns of equal-diameter spheres: simple cubic close packing, with a coordination number of 6 and a packing density of 52.4%; orthorhombic close packing, with a coordination number of 8 and a packing density of 60.5%; tetragonal close packing, with a coordination number of 10 and a packing density of 69.8%; and face-centered cubic close packing and hexagonal close packing, with a coordination number of 12 and a packing density of 74.2%. To obtain a porous glass material with multidirectional interconnected pores, the pore-forming agent is added according to a designed volume ratio based on the close packing, i.e., the volume of the pore-forming agent accounts for 60-75% of the total material volume, and optionally, the volume of the pore-forming agent accounts for 70-75% of the total volume.

[0033] In this case, the glass powder acts as a bonding skeleton. Fine glass powder can be evenly dispersed throughout the system, making the porous glass pore distribution more uniform and well-connected after sintering. At the same time, fine glass powder can shorten the sintering time and reduce glass flow at high temperatures, thereby improving efficiency while increasing the uniformity of the overall material. The fiber component in this case acts as a skeleton support. For the preparation of porous materials with a pore size of 70-80 microns and a pore throat of 30-40 microns, a supporting fiber skeleton of 70-150 microns can be selected. Generally, small-sized fibers or ceramic particles do not affect the overall scaffolding structure. After sintering, small-sized fibers or ceramic particles are wrapped by the glass powder and aggregated at the fiber bonding point (the gap between the pore-forming agent) to form support endpoints.

[0034] The porous glass includes a skeleton and multi-directional interconnected pores, wherein the skeleton includes a fiber skeleton serving as a scaffolding structure and a glass covering adhesive layer serving as a bonding and stabilizing agent; the fiber skeleton has a length of 70-150 microns, a skeleton diameter of 15-45 microns, and a weight percentage range of 12-45%; the fiber skeleton material is a high-temperature resistant ceramic fiber material, including alumina, mullite, zirconia, etc., the fiber diameter is 10-40 microns, and the length is 10-150 microns, wherein the effective fiber length serving as the scaffolding structure is 70-150 microns; the glass covering adhesive layer includes glass material and fibers or ceramic powder that do not serve as a scaffolding structure, and the weight percentage range is 55-88%.

[0035] Optionally, the preparation method of the porous glass material generally includes the following steps: mixing glass powder, fiber components, and pore-forming agents to prepare a green body, performing debinding, and sintering.

[0036] Optionally, the fiber component has a diameter of 3-30 μm and a length of 20-500 μm;

[0037] Optionally, the fiber component has a diameter of 10-25 μm and a length of 20-150 μm.

[0038] Optionally, the aspect ratio of the fiber component is 1-10, and optionally, the aspect ratio of the fiber with a length of 50-150 μm is 2-5;

[0039] And / or, in the fiber component, fibers with a fiber length of more than 50 μm account for 25%, optionally, account for more than 40%; further optionally, account for 40-100%.

[0040] Based on the total mass of the glass powder and the fiber component, the glass powder accounts for 40-62%, and the fiber component accounts for 38-60%;

[0041] And / or, the amount of the pore former is 0.3-2.5 times the total mass of the glass powder and fiber components.

[0042] Select any one of the following processes: tape casting, injection molding, dry pressing, and gel casting to prepare the green body;

[0043] The above-mentioned processes for preparing green parts are all known in the art, and appropriate processing aids may be added depending on the selected process. Typically, and not limitingly, the injection molding process generally involves mixing the mixed materials with injection molding additives (such as paraffin wax, polyethylene, and dispersants) in an internal mixer at high temperature until uniform, followed by injection molding to produce a green part of a desired shape.

[0044] And / or, the debinding temperature is 200-800°C, and the debinding time is 5-50h; optionally, the debinding temperature is 200-350°C.

[0045] And / or, the sintering temperature is 900-1250° C. or 1180-1320° C., and the sintering time is 10-180 min.

[0046] Optionally, the method for preparing the porous glass satisfies at least one of the following (1)-(5):

[0047] (1) The softening temperature of the glass powder is 600-1200°C; the softening point of the selected fiber raw material is above the sintering temperature in the preparation method and can play a skeleton role;

[0048] (2) The particle size of the glass powder is less than 10 μm, and optionally, the particle size is less than 3000 mesh;

[0049] (3) The fiber component is at least one of silicon carbide fiber, silicon nitride fiber, aluminum silicate fiber, quartz fiber, mullite fiber, alumina fiber, hydroxyapatite fiber, and zirconium oxide fiber;

[0050] (4) The pore-forming agent material is one or a mixture of materials such as carbon powder, polystyrene, polymethyl methacrylate, polylactic acid, polyvinyl alcohol, polyethylene terephthalate, engineering plastics, starch, cellulose, sawdust, and graphite powder that can be decomposed, volatilized, or burned at high temperatures;

[0051] (5) The particle size of the pore former is 10-300 μm, and optionally, the average particle size of the pore former is 80 μm. A porous glass material with better connectivity can be obtained by adjusting the addition ratio of pore formers of different diameters.

[0052] In order to obtain porous glass with this special pore structure, the glass raw materials and fiber materials are pretreated as follows:

[0053] (1) The particle size of the glass powder raw material is less than 10 microns, and glass powder with a mesh size of less than 3000 can be used. In order to obtain glass powder with uniform particle size, commercially available glass powder can be milled in a high-energy planetary ball mill at a speed of 200-500 r / min using ethanol as a solvent for 3-5 hours, and then dried and sieved before use.

[0054] (2) The fiber can be a high-temperature resistant fiber such as mullite fiber, zirconia fiber or alumina fiber. In this case, mullite fiber can be selected, with a fiber diameter of 10-25 microns, a length of less than 100 microns, and a fiber aspect ratio of 1-10. Generally, commercially available 2-5 mm short-cut fibers are first crushed to less than 0.5 mm using a crusher, and then high-energy planetary ball milling is performed for 2-8 hours using ethanol as a solvent and stearic acid as a grinding aid at a ball milling speed of 100-400 r / min. Optionally, ball milling can be performed at 300 r / min for 6 hours. The ball-milled fibers are washed with ethanol, dried, and passed through a 100-mesh sieve to obtain the target fibers.

[0055] Optionally, the porous glass with multi-directional interconnected pores is prepared by injection molding, and the preparation method is as follows:

[0056] Glass, fiber, and pore-forming agent are mixed in a certain proportion and mixed in a three-dimensional mixer for 2 hours until uniform. The pore-forming agent is a spherical pore-forming agent with a particle size of 10-300 microns. Optionally, the pore-forming agent has a diameter of 80 microns or a diameter of 50 microns. The mixed material and injection molding additives (paraffin, polyethylene and dispersant) are mixed in a high-temperature mixer until uniform, and then prepared into a green body of a specified shape by injection molding. Heat to 200°C in 200 minutes, and then heat to 500°C at 0.5°C per minute, wherein a 2-hour insulation time is set at 240°C, 280°C, 300°C, and 350°C respectively, and then heat to 1180°C-1320°C at 5°C per minute, keep warm for 30 minutes, and cool naturally to room temperature. In general, a better debinding process can be obtained based on the thermogravimetric curve of the pore-forming agent.

[0057] Alternatively, the porous glass with multidirectional interconnected pores can be directly densely packed by hollow glass microspheres and then prepared by sintering. Generally, the particle size of the hollow glass microspheres selected is 50-120 microns, and optionally, the particle size of the hollow glass microspheres is 80-100 microns. Generally, the porous matrix can be prepared by gel casting, first heating the hollow glass microspheres to 80°C, then adding them to 80°C sol solution, stirring, degassing, injecting them into a mold with a pressure of 5MPa, waiting to be cooled into a gel blank, drying the blank at 50°C, and then sintering at 1000°C for 30 minutes, and obtaining a porous glass matrix after natural cooling.

[0058] Typically, but not limiting, the atomizer core provided in this application is based on a porous glass substrate, on which a heating unit is provided, wherein the heating unit is a heating wire, a heating mesh or a heating film. The heating wire or heating mesh needs to be embedded in the green body forming process, and then sintered together with the formed green body to obtain a porous glass atomizer core; when a heating film is used, a thick film resistive heating film can be printed on the porous glass substrate by screen printing or a thin film resistive heating film can be sprayed or magnetron sputtered, and the pattern of the heating film can be designed, and then the porous glass atomizer core can be obtained through a sintering step.

[0059] Typically, non-limitingly, a thick film resistive heating film is prepared by screen printing process. The main components of the thick film are nickel-based alloy, iron-based alloy, silver alloy, titanium alloy, aluminum alloy, stainless steel, etc., containing elements such as Fe, Cr, Ni, Ti, Pa, Pt, Al, Mo, Si, Ag, etc. The protruding thickness of the thick film is 11-100μm, the penetration thickness is 10-100μm, the line width is 250-450μm, the line spacing is 300μm-900μm, and the patterns used are S, M, Ω, etc. The sintering temperature of the heating film is 700-1200℃, and the sintering time is 0.5-3h.

[0060] Typically, but not limiting, thin film resistive heating films are prepared by spraying or magnetron sputtering. The main components of the film are nickel-based alloys, silver alloys, titanium alloys, aluminum alloys, stainless steel, etc., containing elements such as Fe, Cr, Ni, Ti, Pa, Pt, Al, Mo, Si, and Ag. The protruding thickness of the film is 0.5-5μm.

[0061] Specifically, the present application also provides a porous glass atomizing core prepared by sintering the printed film of the porous glass material, and its heating membrane is a porous heating membrane, wherein: the porous heating membrane includes a part higher than the surface of the porous substrate and a part infiltrated into the porous substrate, wherein the part higher than the surface of the porous substrate is a porous structure with a pore size of 5-30 microns, the pores are interconnected and connected with the pores of the substrate, the membrane is about 30-100 microns higher than the surface of the substrate, as shown in Figure 2, and the optional height is about 60-100 microns; the resistance of the heating film is 0.8-1.2 ohms.

[0062] The technical solution of this application has the following advantages:

[0063] The porous glass with multidirectional interconnected pores provided in this application comprises a framework and multidirectional interconnected pores, wherein the multidirectional interconnected pores are spherical and connected to at least six surrounding pores. By defining the interconnected pore structure, this application achieves fast transfer speeds and minimal differences in transfer paths during the delivery of atomized liquid matrices such as e-liquid. Multi-channel connectivity reduces the problem of insufficient or unbalanced localized oil supply to the atomizer core, improves localized coking during puffing, and enhances the taste and puffing experience of electronic cigarettes.

[0064] The porous glass with multi-directional connecting holes provided in the present application makes the connecting channel size between the holes more uniform by limiting the hole size, which can further avoid uneven liquid conduction speed and local overheating during the use of the atomizer core, and avoid the generation of local coking and carbon deposits. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the following will briefly introduce the drawings required for use in the specific implementation methods or the description of the prior art. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0066] FIG1 is a microscopic morphology of the green body obtained in Example 1 of the present application;

[0067] FIG2 is a microscopic morphology of the porous glass obtained in Example 1 of the present application, wherein a is the surface, and b and c are cross-sections;

[0068] FIG3 is a schematic diagram of the multi-directional interconnected pore structure of the porous glass obtained in Example 1 of the present application;

[0069] FIG4 is a diagram of the tobacco oil infiltration of the porous glass substrates obtained in Example 1 and Comparative Example 2 of the present application;

[0070] FIG5 is a macroscopic and microscopic morphology of the porous heating film in the test example of the present application;

[0071] FIG6 is a temperature field distribution and a temperature distribution diagram of Example 1 during the atomization process in the test example of the present application;

[0072] FIG7 is a comparison of carbon deposits in Example 1 of the present application (left) and a commercially available ceramic heating element (right);

[0073] FIG8 is a temperature field distribution and a temperature distribution diagram of Example 2 during the atomization process in the test example of the present application;

[0074] FIG9 is a temperature field distribution and a temperature distribution diagram of Comparative Example 1 during the atomization process in the test example of the present application;

[0075] FIG10 is a microscopic morphology of the green body obtained in Example 2 of the present application;

[0076] FIG11 is a schematic diagram showing the multi-directional interconnected pore structure of the porous glass obtained in Example 2 of the present application. DETAILED DESCRIPTION

[0077] The following examples are provided to further better understand the present application, but are not limited to the best implementation mode described herein, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the scope of protection of the present application.

[0078] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in this field can be used. If the manufacturer of the reagents or instruments is not specified, they are all commercially available conventional reagents.

[0079] Example 1

[0080] This embodiment provides a porous glass having multi-directional interconnected pores, and the preparation method thereof comprises the following steps:

[0081] Using ethanol as solvent, the glass powder was ball-milled in a planetary ball mill at a speed of 300 r / min for 3 hours, dried and sieved to obtain glass powder with a particle size of less than 5 microns; the crushed mullite chopped fibers were planetarily ball-milled in ethanol as solvent at a speed of 300 r / min for 6 hours with stearic acid as a grinding aid, washed with ethanol, dried and sieved with 100 mesh to obtain fiber raw materials. 13 volumes of glass powder (density 2.5 g / mL, the same below), 12 volumes of fiber (density 2.8 g / mL, the same below), and 75 volumes of PMMA (80 microns) pore-forming agent were mixed in a three-dimensional mixer for 2 hours. The mixed materials were added to an internal mixer, and 20% paraffin, 5% polyethylene, and 5% dispersing aid (dibutyl phthalate, the same below) were added. The mixture was mixed at 180°C for 2 hours and then prepared into a green body by an injection molding machine. The micromorphology is shown in Figure 1. It can be seen from the figure that in one plane, the pore-forming agent is closely stacked with the surrounding 6 pore-forming agents, and the pore-forming agent has a face-centered close-packed or hexagonal close-packed trend. The temperature was raised to 200°C over 200 minutes, then increased to 500°C at a rate of 0.5°C / min. Two-hour holding times were set at 240°C, 280°C, 300°C, and 350°C. The temperature was then raised to 1180°C at a rate of 5°C / min, held for 30 minutes, and naturally cooled to room temperature. This yielded a porous glass material with a fiber volume fraction of 48%. The micromorphology of the sintered porous glass matrix is ​​shown in Figures 2 and 3. As can be seen from the figures, the densely packed pore-forming agent leaves a porous structure after sintering. Within the same plane, the pores generated by the pore-forming agent are interconnected with approximately six surrounding pores. Mercury intrusion porosimetry revealed a porosity of 72.0%, with an average pore throat of 37.7 μm.

[0082] A porous glass substrate with a length of 9 mm, a width of 4 mm, and a height of 2.5 mm was prepared, and its oil conduction speed was tested at room temperature. The e-liquid with a viscosity of 230 cP was selected, and the substrate was placed vertically (height 9 mm). It took about 74.5 seconds for the e-liquid to rise 9 mm, and the oil conduction speed was 0.121 mm / s. Under the same conditions, the commercially available porous ceramic substrate (Feelm heating element, Shenzhen McWell Technology Co., Ltd.) took 100 seconds to raise the e-liquid by 9 mm, and the oil conduction speed was 0.09 mm / s. Compared with the commercially available ceramic heating element substrate, the oil conduction speed of the porous glass substrate was increased by about 34%. When tested with a thickness of 2.5 mm, the time difference from the presence of e-liquid on the atomizing surface to the e-liquid spreading all over the atomizing surface was 1 second, and the e-liquid immersion was shown in Figure 4a.

[0083] Example 2

[0084] The present embodiment provides a porous glass with multi-directional interconnected pores, which is different from Example 1 in that it is prepared with 9 volumes of glass powder, 11 volumes of fiber, and 30 volumes of PMMA (80 microns) pore formers. The porosity of the porous matrix tested by mercury intrusion is 60.5%, and the average pore throat is 27.5 microns. The microscopic morphology of the green body is shown in FIG10 . It can be seen from the figure that the pore former is approximately a tetragonal, orthogonal or simple cubic close-packed structure rather than a face-centered cubic or hexagonal close-packed structure. In the same plane, a single pore former is interconnected with the four surrounding pore formers. The microscopic morphology of the surface of the porous glass matrix is ​​shown in FIG11 , in which the matrix pores are interconnected with the five surrounding pores (in fact, the material is a three-dimensional structure, and there will also be interconnected pore structures on other surfaces).

[0085] The same test method as in Example 1 was used, with an oil guide speed of 0.114 mm / s and a thickness of 2.5 mm. The time difference from the presence of liquid on the atomizing surface to the complete spread of liquid on the entire atomizing surface was 1.5 s.

[0086] Comparative Example 1

[0087] This comparative example provides a porous glass substrate material, the preparation method of which comprises the following steps:

[0088] Glass powder was ball-milled in a planetary ball mill at 300 rpm for 3 hours using ethanol as a solvent, dried, and sieved to obtain glass powder with a particle size of 3-5 microns. The crushed mullite chopped fibers were ball-milled in ethanol at 300 rpm for 6 hours using stearic acid as a grinding aid. After washing with ethanol, they were dried and sieved through a 100-mesh sieve to obtain fiber raw material. 28 volumes of glass powder, 14 volumes of fiber, and 58 volumes of PMMA (80 micron) pore-forming agent were mixed in a three-dimensional mixer for 2 hours. The mixed materials were added to an internal mixer, where 20% paraffin wax, 5% polyethylene, and 5% dispersing agent were added. The mixture was then mixed at 180°C for 2 hours and then formed into green blanks using an injection molding machine. The temperature was raised to 200°C in 200 minutes, then raised to 500°C at a rate of 0.5°C per minute, with a holding time of 2 hours at 240°C, 280°C, 300°C, and 350°C respectively. The temperature was then raised to 1250°C at a rate of 5°C per minute, held for 30 minutes, and naturally cooled to room temperature to obtain a porous glass material with a fiber volume content of 33.3%.

[0089] A rectangular sample measuring 9 × 4 × 2.5 mm was prepared. Mercury intrusion testing revealed a porous matrix porosity of 57.9% and an average pore throat of 25 μm. Using the same testing method as in Example 1, the liquid transfer velocity was measured at 0.106 mm / s. At a thickness of 2.5 mm, the time difference from liquid depositing on the atomizing surface to complete liquid spread across the entire surface was 4 seconds. The matrix interconnected pores were calculated to be 82.4%. Liquid immersion is shown in Figure 4b.

[0090] Test Case

[0091] The atomizing core is prepared with the porous glass material prepared in the embodiment and the comparative example, and a porous nickel-based heating film slurry (the main element is Ni, containing a small amount of Fe, Cr, Co, W, Mo, Al, Ag, Ru, B, and elements) is used. The film is printed and sintered to obtain a porous heating film. The pore size of the porous heating film is 5-30 microns, the pores are interconnected, and the pores are connected to the substrate pores. It is about 70 microns higher than the substrate and has a penetration thickness of about 70 microns. The pattern is shown in Figure 5. The line width is about 350μm, the line spacing is about 550μm, the line is about 750μm away from the edge of the substrate, the sintering temperature is 1050℃, and the time is 30min to obtain a porous glass atomizing core. An infrared thermal imager was used to examine the atomization temperature of the porous glass atomizer core. Using fruit-flavored e-liquid and a 7.5W constant power board, the test followed a puffing schedule of 3s on and 27s off. During the atomization process, the porous glass atomizer core exhibited a uniform temperature distribution with no localized high-temperature spots. The atomization temperature of Example 1 was stably distributed between 230-240°C, as shown in Figure 6. The atomization temperature stability of Example 2 was slightly lower than that of Example 1, with its atomization temperature primarily distributed between 239°C and 256°C, as shown in Figure 8. The atomization temperature of Comparative Example 1 was unstable, ranging between 242-300°C, as shown in Figure 9.

[0092] The porous glass atomizer cores prepared in Examples 1 and 2 and Comparative Example 1 were tested for cigarette loading using fruit-flavored e-liquid at 7.5W. Compared to a commercially available ceramic heater (Feelm heater, Shenzhen McWell Technology Co., Ltd.), the porous glass atomizer core in Example 1 showed little carbon accumulation after puffing. As shown in Figure 7, after 400 puffs, the porous glass atomizer core (left image) showed a significant advantage over the ceramic heater (right image) in terms of carbon accumulation. The commercially available ceramic heater suffered from severe carbon accumulation after 400 puffs. The carbon accumulation in Example 2 was similar to that in Example 1, and the carbon accumulation in Comparative Example 1 was similar to that in the commercially available ceramic heater. Therefore, images are not shown here.

[0093] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will appreciate that other variations or modifications can be made based on the above description. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications derived therefrom remain within the scope of protection of this application.

Claims

1. A porous glass having multi-directional interconnected pores, characterized in that: It comprises a skeleton and multi-directional connecting holes, wherein the multi-directional connecting holes are spherical holes connected with at least six holes around them.

2. The porous glass having multi-directional interconnected pores according to claim 1, characterized in that: The multi-directional connecting hole is connected to 6-12 holes around it.

3. The porous glass having multi-directional interconnected pores according to claim 2, characterized in that: The multi-directional connecting hole is connected to 7-10 holes around it.

4. The porous glass having multi-directional interconnected pores according to claim 1, characterized in that: The skeleton comprises a fiber skeleton serving as a frame structure and a glass covering bonding layer serving as a bonding stabilization function, and the total volume of the skeleton accounts for 25-35%.

5. The porous glass having multi-directional interconnected pores according to claim 4, characterized in that: The fiber skeleton has a length of 75-150 microns and a diameter of 15-45 microns.

6. The porous glass having multi-directional interconnected pores according to claim 4, characterized in that: In the porous glass with multi-directional interconnected pores, the weight percentage of the fiber skeleton is in the range of 12-45%.

7. The porous glass having multi-directional interconnected pores according to claim 4, characterized in that: In the porous glass with multi-directional interconnected pores, the weight percentage of the glass-covered adhesive layer ranges from 55 to 88%.

8. The porous glass having multi-directional interconnected pores according to claim 1, characterized in that: The porosity of the porous glass is 65-75%.

9. The porous glass having multi-directional interconnected pores according to claim 8, characterized in that: The porosity is 70-75%.

10. The porous glass having multi-directional interconnected pores according to any one of claims 1 to 9, characterized in that: The pore diameter of the multi-directional connected pores is 70-80 microns, the average diameter of the pore throats of the connecting channels between the pores is 25-45 microns, and the pore throats are distributed in the 5-60 micron area, wherein more than 50% of the pore throats are distributed in the 20-45 micron area.

11. The porous glass having multi-directional interconnected pores according to claim 10, characterized in that: The average diameter of the pore throats is 28-36 microns, the pore throats are distributed in the 10-55 micron region, and more than 90% of the pore throats are distributed in the 20-45 micron region.

12. The porous glass material with uniform pore channels according to claim 11, characterized in that: The average diameter of the pore throats is about 29-35 microns, the pore throats are distributed in the 12-50 micron region, and the pore throats distributed in the 20-45 micron region account for more than 95%.

13. The porous glass material with uniform pore channels according to claim 12, characterized in that: The pore throats are distributed in the 20-45 μm region.

14. An atomizer core, characterized in that: The porous glass with multi-directional interconnected pores as claimed in any one of claims 1 to 13 is used as a substrate, and a heating unit is arranged on the substrate.

15. The atomizer core according to claim 14, characterized in that: During the atomization process, the temperature field deviation is less than 10°C.

16. An electronic atomizer, characterized in that: Comprising the atomizer core according to claim 14 or 15.

Citation Information

Patent Citations

  • Composition and porous ceramic atomization core containing continuous glass phase

    CN113149697A

  • Porous glass as well as preparation method and application thereof

    CN114804639A

  • Process for producing glass-ceramics

    KR1019920017967A