Thin-film capacitor for human tumor treatment and preparation method therefor, and tumor treatment electrode patch and tumor treatment system

By setting a conductive defect repair layer between the dielectric layer and the electrode layer, the air gap ionization problem caused by the surface defect of the thin film capacitor dielectric layer is solved, and the stability of the electrode and the safety of tumor treatment are improved.

WO2024240156A1PCT designated stage expired Publication Date: 2024-11-28CHENGDU ROUDIAN YUNKE SCI & TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/094554
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2024-05-21
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The surface defects of the dielectric layer of the film capacitor in the existing tumor electric field treatment lead to air gap ionization, resulting in electrode damage and poor treatment effect.

Method used

A conductive defect repair layer is provided between the dielectric layer and the electrode layer, which closely combines the dielectric layer and the electrode layer to avoid the formation of tiny voids and thus prevent the phenomenon of air gap ionization.

Benefits of technology

It effectively avoids air gap ionization, improves the stability of the electrode and the safety of tumor treatment, and ensures the reliability and treatment effect of the film capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024094554_28112024_PF_FP_ABST
    Figure CN2024094554_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A thin-film capacitor for human tumor treatment and a preparation method therefor, and a tumor treatment electrode patch and a tumor treatment system. The thin-film capacitor comprises: a first electrode layer and a second electrode layer; a dielectric layer, which is located between the first electrode layer and the second electrode layer; and a first defect repair layer, which is located between the second electrode layer and the dielectric layer, wherein the first defect repair layer has electrical conductivity, the face of the dielectric layer that faces the first defect repair layer is provided with microscopic pits, one face of the first defect repair layer is tightly bound to the microscopic pits on the surface of the dielectric layer, and the other face of the first defect repair layer is in direct or indirect electrical contact with the second electrode layer. By means of providing a first defect repair layer on the face of a dielectric layer that faces away from a first electrode layer, surface defects in the face of the dielectric layer that faces away from the first electrode layer are compensated for by the first defect repair layer, thereby preventing tiny voids from being generated between the dielectric layer and a corresponding electrode layer and preventing an induced air-gap ionization phenomenon.
Need to check novelty before this filing date? Find Prior Art

Description

Film capacitor for human tumor treatment and preparation method thereof, tumor treatment electrode patch, and tumor treatment system

[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 22, 2023, with application number 202310577976.4, entitled “Thin film capacitor for treating human tumors and its preparation method, tumor treatment electrode patch, tumor treatment system”, and the Chinese patent application filed with the Patent Office of China on April 26, 2024, with application number 202410513253.2, entitled “Thin film capacitor for treating human tumors and its preparation method, tumor treatment electrode patch, tumor treatment system”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the technical field of tumor treatment, and specifically to a film capacitor for treating human tumors and a preparation method thereof, a tumor treatment electrode patch, and a tumor treatment system. Background Art

[0003] Currently, there are many treatments for tumors. Common treatments include surgery, radiotherapy, chemotherapy, molecular targeted therapy, etc. However, common treatments all have corresponding disadvantages. For example, radiotherapy or chemotherapy will kill normal cells. For example, although surgery can cure early tumors, some patients are prone to damage due to surgical contraindications.

[0004] Using alternating electric fields to treat tumors is one of the most cutting-edge tumor treatments currently under development. Tumor electric field therapy applies an alternating electric field to the treatment area of ​​the human body, thereby affecting the aggregation of tumor microtubules and preventing spindle formation, thereby inhibiting the mitotic process of cancer cells and inducing apoptosis. Specifically, existing tumor electric field therapy primarily attaches electrode patches to opposite sides of the patient's treatment area, such as the patient's waist. Thin-film capacitors within the electrode patches block the current from flowing directly to the patient, while the electrode plates of the thin-film capacitors on opposite sides apply an alternating electric field to the patient's treatment area, thereby achieving the purpose of tumor treatment.

[0005] In the prior art, in order to ensure the therapeutic effect of tumor electric field therapy, it is usually necessary to make the film capacitor have a sufficiently large capacitance. Therefore, reducing the thickness of the dielectric layer is one of the main ways to increase the capacitance of the film capacitor.

[0006] Solve technical problems

[0007] However, the surface of the dielectric layer is usually uneven and has surface defects, which results in tiny gaps between the dielectric layer and the electrode layer. When voltage is applied between the two electrode layers, the thinner dielectric layer will undergo air gap ionization in the tiny gaps. The air gap ionization phenomenon will cause the ionized positive and negative ions to be transferred between different layers and move toward the negative and positive electrodes of the thin film capacitor respectively, generating discharge sparks at the moment of contact with the electrodes, causing electrode damage. Technical Solutions

[0008] The present application provides a thin film capacitor for human tumor treatment and its preparation method, tumor treatment electrode patch, and tumor treatment system, aiming to solve the technical problem of air gap ionization caused by surface defects in the dielectric layer of the current capacitor.

[0009] In a first aspect, the present application provides a film capacitor for treating human tumors, comprising:

[0010] a first electrode layer and a second electrode layer;

[0011] a dielectric layer, the dielectric layer being located between the first electrode layer and the second electrode layer;

[0012] a first defect repairing layer, the first defect repairing layer being located between the second electrode layer and the dielectric layer;

[0013] The first defect repairing layer is conductive, one side of the first defect repairing layer is tightly bonded to the dielectric layer, and the other side of the first defect repairing layer is in direct or indirect electrical contact with the second electrode layer.

[0014] In some embodiments, the second electrode layer is a finished metal sheet, and the tensile index of the second electrode layer is greater than the tensile index of the first defect repairing layer.

[0015] In some embodiments, the thickness of the second electrode layer is greater than the thickness of the first defect repairing layer.

[0016] In some embodiments, a surface of the dielectric layer facing away from the first electrode layer has a first roughness, and a surface of the first defect repairing layer facing away from the dielectric layer has a second roughness;

[0017] The second roughness is less than or equal to the first roughness.

[0018] In some embodiments, the first defect repair layer includes multiple sub-metal layers.

[0019] In some embodiments, the first defect repair layer is a metal layer.

[0020] In some embodiments, the first defect repair layer includes overlapping aluminum metal layers and zinc metal layers; or

[0021] The first defect repairing layer includes overlapping aluminum metal layers and gold metal layers; or

[0022] The first defect repairing layer includes an overlapping aluminum metal layer and a titanium metal layer.

[0023] In some embodiments, the first electrode layer is laminated to the dielectric layer.

[0024] In some embodiments, the thin film capacitor further includes a second defect repair layer, the second defect repair layer being located between the first electrode layer and the dielectric layer;

[0025] The second defect repairing layer is conductive, one side of the second defect repairing layer is tightly bonded to the surface of the dielectric layer, and the other side of the second defect repairing layer is directly or indirectly electrically contacted with the first electrode layer.

[0026] In some embodiments, the tensile index of the first electrode layer is greater than the tensile index of the second defect-repairing layer.

[0027] In some embodiments, a surface of the dielectric layer facing the first electrode layer has a third roughness, and a surface of the second defect repairing layer facing away from the dielectric layer has a fourth roughness;

[0028] The fourth roughness is less than or equal to the third roughness.

[0029] In some embodiments, the dielectric layer includes a first insulating layer and a second insulating layer that are tightly bonded to each other;

[0030] The first defect repairing layer is tightly bonded to a side of the second insulating layer facing away from the first insulating layer, and the insulating strength of the second insulating layer is greater than that of the first insulating layer.

[0031] In some embodiments, the thickness of the first defect repairing layer is 10 nm to 1000 nm, and the tolerance value of the first defect repairing layer is ±10% of the thickness value thereof.

[0032] In some embodiments, the first defect repair layer has a thickness of 10 nm to 800 nm.

[0033] In some embodiments, the first defect repair layer has a thickness of 50 nm to 450 nm.

[0034] In some embodiments, the total thickness of the sub-metal layers in the first defect repair layer having an electrical conductivity better than or equal to that of metallic aluminum is 10 nm to 400 nm;

[0035] In some embodiments, the total thickness of the sub-metal layers in the first defect repair layer having an electrical conductivity better than or equal to that of metallic aluminum is 50 nm to 400 nm;

[0036] In some embodiments, the thickness of the dielectric layer is 1 um to 100 um.

[0037] In some embodiments, the dielectric layer has a thickness of 1 um to 10 um.

[0038] In some embodiments, the thickness of the dielectric layer is 2 um to 8 um.

[0039] In some embodiments, the thin film capacitor further comprises a flexible substrate;

[0040] The first electrode layer is attached to the flexible substrate.

[0041] In a second aspect, the present application provides a method for preparing a thin film capacitor for treating human tumors, comprising:

[0042] providing a first electrode layer;

[0043] forming a dielectric layer on the first electrode layer;

[0044] forming a first defect repairing layer on a side of the dielectric layer facing away from the first electrode layer;

[0045] forming a second electrode layer on a side of the dielectric layer facing away from the first defect repairing layer;

[0046] The first defect repairing layer is conductive, one side of the first defect repairing layer is tightly combined with the surface of the dielectric layer, and the other side of the first defect repairing layer is directly or indirectly in electrical contact with the second electrode layer.

[0047] In some embodiments, a surface of the dielectric layer facing away from the first electrode layer has a first roughness, and a surface of the first defect repairing layer facing away from the dielectric layer has a second roughness;

[0048] The second roughness is less than or equal to the first roughness.

[0049] In a third aspect, the present application provides a tumor treatment electrode patch comprising the thin film capacitor as described in the first aspect.

[0050] In a fourth aspect, the present application provides a tumor treatment system, comprising the tumor treatment electrode patch as described in the third aspect. Beneficial effects

[0051] In the prior art, thin-film capacitors cannot be tightly bonded to the dielectric layer and the electrode layer due to morphological defects or unevenness on the surface of the dielectric layer, resulting in air gap ionization. The present application avoids the air gap ionization caused by the generation of tiny gaps between the dielectric layer and the corresponding electrode layer by providing a defect repair layer between the dielectric layer and the electrode layer. At the same time, the use of a conductive defect repair layer makes the electrical connection with the electrode layer more stable, which is beneficial to ensuring the safety of the thin-film capacitor in the tumor treatment electrode patch. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0053] FIG1 is a schematic structural diagram of a thin film capacitor provided in an embodiment of the present application;

[0054] FIG2 is another schematic diagram of the structure of a thin film capacitor provided in an embodiment of the present application;

[0055] FIG3 is another structural diagram of a thin film capacitor provided in an embodiment of the present application;

[0056] FIG4 is another structural diagram of a thin film capacitor provided in an embodiment of the present application;

[0057] FIG5 is another structural diagram of a thin film capacitor provided in an embodiment of the present application;

[0058] FIG6 is another structural diagram of a thin film capacitor provided in an embodiment of the present application;

[0059] FIG7 is another structural diagram of a thin film capacitor provided in an embodiment of the present application;

[0060] FIG8 is another structural diagram of a thin film capacitor provided in an embodiment of the present application;

[0061] FIG9 is another schematic structural diagram of a thin film capacitor provided in an embodiment of the present application;

[0062] FIG10 is a schematic flow chart of a method for preparing a thin film capacitor provided in an embodiment of the present application;

[0063] FIG11 is another schematic flow chart of a method for preparing a thin film capacitor provided in an embodiment of the present application;

[0064] FIG12 is a schematic diagram of measuring the bending angle of a thin film capacitor provided in an embodiment of the present application.

[0065] Among them, 10 is the first electrode layer, 20 is the dielectric layer, 21 is the first insulating layer, 22 is the second insulating layer, 201 is the first microscopic pit, 202 is the second microscopic pit, 30 is the first defect repair layer, 31 is the aluminum metal layer, 32 is the zinc metal layer, 301 is the sub-metal layer, 40 is the second electrode layer, 50 is the second defect repair layer, 60 is the flexible substrate, 70 is the flexible conductive layer, and 80 is the conductive attachment layer.

[0066] Implementation Methods of the Application

[0067] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without making creative efforts are within the scope of protection of this application.

[0068] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the said features. In the description of the present application, "multiple" means two or more, unless otherwise clearly and specifically defined.

[0069] In this application, the word "exemplary" is used to mean "serving as an example, illustration, or illustration." Any embodiment described in this application as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. The following description is given to enable any person skilled in the art to implement and use the present application. In the following description, details are listed for the purpose of explanation. It should be understood that one of ordinary skill in the art can recognize that the present application can be implemented without using these specific details. In other instances, well-known structures and processes are not elaborated in detail to avoid obscuring the description of the present application with unnecessary details. Therefore, the present application is not intended to be limited to the embodiments shown, but is consistent with the widest scope consistent with the principles and features disclosed in this application.

[0070] The embodiments of the present application provide a thin film capacitor for treating human tumors, a preparation method thereof, a tumor treatment electrode patch, and a tumor treatment system, which are described in detail below.

[0071] First, refer to FIG1 , which shows a schematic structural diagram of a thin film capacitor in an embodiment of the present application, wherein the thin film capacitor includes:

[0072] A first electrode layer 10 and a second electrode layer 40;

[0073] The dielectric layer 20 is located between the first electrode layer 10 and the second electrode layer 40;

[0074] A first defect repairing layer 30 , the first defect repairing layer 30 is located between the second electrode layer 40 and the dielectric layer 20 ;

[0075] The first defect repairing layer 30 is conductive, and one side of the first defect repairing layer 30 is tightly bonded to the surface of the dielectric layer 20 , while the other side of the first defect repairing layer 30 is in direct or indirect electrical contact with the second electrode layer 40 .

[0076] Specifically, the first electrode layer 10 and the second electrode layer 40 are made of a conductive material and constitute electrodes connected to the two ends of the thin film capacitor for connecting to an AC power source, so that an AC voltage signal can be supplied to the thin film capacitor through the first electrode layer 10. In some embodiments of the present application, the first electrode layer 10 and the second electrode layer 40 can be thin and flexible metal layers, such as copper foil, so that the first electrode layer 10 has good flexibility and is easy to bend, thereby allowing the thin film capacitor to bend as a whole and better conform to the surface of human skin.

[0077] In some embodiments of the present application, the thickness of the first electrode layer 10 is 0.005 mm to 1 mm. Preferably, the thickness of the first electrode layer 10 is 0.01 mm to 0.1 mm. More preferably, the thickness of the first electrode layer 10 is 0.01 mm to 0.05 mm. The thickness of the first electrode layer 10 falling within the above range can ensure the flexibility of the first electrode layer 10 while also preventing the first electrode layer 10 from being too thin and prone to cracking.

[0078] It is understandable that the first electrode layer 10 and the second electrode layer 40 may also be made of other metal materials or non-metallic conductive materials, such as metal silver foil or conductive graphite.

[0079] In some embodiments of the present application, the first electrode layer 10 may refer to a corresponding metal layer on a circuit board. For example, a portion of a copper foil area is exposed on the circuit board, and the dielectric layer 20 is formed within the copper foil area. The power interface of the circuit board can conveniently connect the two poles of the power supply. Preferably, the circuit board may be a flexible circuit board, such as a flexible printed circuit board made of a polyimide or polyester film substrate, to simplify the electrical connection structure of the film capacitor while making the film capacitor flexible and bendable.

[0080] In some embodiments of the present application, the second electrode layer 40 can be a thin and flexible metal layer, such as a 0.1 mm to 1 mm thick copper foil, so that the second electrode layer 40 is flexible and easy to bend, thereby allowing the film capacitor to bend as a whole and completely close to the human skin surface. It is understood that the second electrode layer 40 can also be made of other metal materials or non-metallic conductive materials, such as metal silver foil, conductive graphite, conductive hydrogel, or conductive silicone gel.

[0081] In some embodiments of the present application, the second electrode layer 40 of the thin film capacitor is closer to the surface of human skin, while the first electrode layer 10 of the thin film capacitor is away from the surface of human skin.

[0082] In some embodiments of the present application, for example, for embodiments in which the second electrode layer 40 is closer to the surface of human skin, the second electrode layer 40 is preferably a stainless steel metal layer or a titanium metal layer. When the tumor treatment electrode patch is attached to the surface of human skin, sweat exuded from the human skin or water vapor generated by the hydrogel attached to the surface of the thin film capacitor may penetrate into the interior of the thin film capacitor. The second electrode layer 40 is preferably set to a stainless steel metal layer or a titanium metal layer. On the one hand, it can prevent the second electrode layer 40 from corrosion, and on the other hand, it can also block water vapor from penetrating into the dielectric layer 20 inside the thin film capacitor, thereby avoiding the phenomenon of dielectric layer 20 of the thin film capacitor being broken down and damaged due to water vapor.

[0083] In some embodiments of the present application, the thickness of the second electrode layer 40 is 0.005 mm to 1 mm. Preferably, the thickness of the second electrode layer 40 is 0.01 mm to 0.1 mm. More preferably, the thickness of the second electrode layer 40 is 0.01 mm to 0.05 mm. The thickness of the second electrode layer 40 falling within the above range can ensure the flexibility of the second electrode layer 40 while also preventing the second electrode layer 40 from being too thin and prone to cracking.

[0084] The dielectric layer 20 is made of an insulating material and can prevent current from flowing through it, thereby preventing the current connected to the first electrode layer 10 of the thin-film capacitor from directly acting on the human body. In some embodiments of the present application, the dielectric layer 20 can be made of an organic or inorganic material, such as ceramic, glass, mica, polypropylene, polystyrene, or polyethylene terephthalate.

[0085] Preferably, the material of the dielectric layer 20 may include one or more of poly(VDF-TrFE-CTFE)(poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene)), poly(VDF-TrFE-CFE)(poly(vinylidene fluoride-trifluoroethylene-1-chlorofluoroethylene)), poly(VDF-TrFECFE-CTFE)(poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene-chlorofluoroethylene)), and poly(VDF-DB)(poly(vinylidene fluoride-diethylene glycol butyl ether)). Since the above materials have a relatively high dielectric constant, they help to increase the capacitance of the thin film capacitor when the thickness and area of ​​the dielectric layer 20 are constant, thereby better applying the tumor treatment alternating electric field to the patient's treatment site.

[0086] In some embodiments of the present application, the researchers conducted the following experiment 1 to investigate the effect of different dielectric layer thicknesses on the performance of thin film capacitors:

[0087] Experimental purpose: To verify the effect of different dielectric layer thickness values ​​on the performance of film capacitors used for human tumor treatment;

[0088] Experimental plan: Prepare a first electrode layer 10 of copper-gold-plated material and a second electrode layer 40 of conductive hydrogel. The defect repair layer 30 is a composite structure of a 100nm thick aluminum metal layer and a 100nm thick titanium metal layer. The defect repair layer 30 is located on the side of the dielectric layer facing the second electrode layer 40. The first electrode layer 10, dielectric layer 20, defect repair layer 30, and second electrode layer 40 all have an area of ​​3.14 square centimeters and are stacked in a vertical direction. Based on this, multiple thin film capacitor samples of the same size but with different thicknesses of the dielectric layer 20 (polyimide / PVDF-TrFE-CFE) were prepared and tested according to the following steps:

[0089] (1) Set the test environment temperature to 25°C;

[0090] (2) Turn on the KEYSIGHT E4980AL LCR digital source meter, set the test voltage to 1V, the test frequency to 200kHz, and the test mode to Cs-D (capacitance-loss) mode;

[0091] (3) One of the two test clamps of the digital source meter is electrically connected to the first electrode layer 10 and is in conduction, and the other is electrically connected to the test electrode attached to the side of the second electrode layer 40 away from the dielectric layer and is in conduction;

[0092] (4) The Cs value recorded is the capacitance value.

[0093] (5) After completing the above steps, prepare an RK2670YL withstand voltage tester and adjust the leakage current of the withstand voltage tester to 20mA leakage current range;

[0094] (6) Electrically connect the positive test terminal of the withstand voltage tester to the second electrode layer 40;

[0095] (7) Connect the negative electrode of the withstand voltage tester to the first electrode layer 10, start the switch of the withstand voltage tester, and slowly increase the voltage. When the leakage current exceeds 20mA, the instrument will alarm. The voltage value read at the time of the alarm is the withstand voltage value.

[0096] The experimental results obtained after testing are as follows:

[0097] From the above experimental data and experimental results, it can be seen that as the thickness of the dielectric layer continues to increase, the capacitance value of the film capacitor continues to decrease, while its withstand voltage strength gradually increases. Therefore, under the comprehensive consideration of ensuring both the capacitance value and the withstand voltage strength of the film capacitor, in some embodiments of the present application, the thickness of the dielectric layer 20 is 1um to 10um; preferably, the thickness of the dielectric layer 20 is 2um to 8um. Among them, the thickness of the dielectric layer 20 meets the above-mentioned dimensional requirements, which can make the film capacitor have a higher capacitance and also avoid the breakdown phenomenon of the film capacitor caused by the thin dielectric layer 20.

[0098] In some embodiments of the present application, the dielectric layer 20 can be formed on the first electrode layer 10 by spin coating, doctor blade coating, atomization, casting, or screen printing. In other embodiments of the present application, the dielectric layer 20 is indirectly or directly attached to the first electrode layer 10 by means of a finished film.

[0099] It should be noted that regardless of whether the dielectric layer 20 is formed on the first electrode layer 10 by solution preparation or finished film bonding, there are surface defects on the surface of the dielectric layer 20. Since the defect may be an uneven surface, microscopic pits or microscopic protrusions, a gap is caused between the dielectric layer and the electrode layer; for example, the side of the dielectric layer 20 facing the first defect repair layer 30 has microscopic pits. The surface defect refers to the uneven surface after the dielectric layer 20 (or the finished film of the dielectric layer 20) is formed.

[0100] One side of the first defect repair layer 30 is tightly bonded to the microscopic pits on the surface of the dielectric layer 20, and the other side is in direct or indirect electrical contact with the second electrode layer 40. Specifically, the first defect repair layer 30 is bonded to the side of the dielectric layer 20 facing away from the first electrode layer 10. One side of the first defect repair layer 30 can be tightly bonded to the microscopic pits on the surface of the dielectric layer 20, so that the first defect repair layer 30 can compensate for the surface defects of the dielectric layer 20 facing away from the first electrode layer 10, thereby avoiding the formation of tiny gaps between the dielectric layer 20 and the corresponding electrode layer (such as the second electrode layer 40) or between the dielectric layer 20 and the first defect repair layer 30 and the resulting air gap ionization phenomenon. In some embodiments of the present application, the first defect repair layer 30 is conductive to avoid increasing the thickness of the dielectric layer 20 of the thin film capacitor to ensure the capacitance of the thin film capacitor.

[0101] In some embodiments of the present application, the first defect repair layer 30 is a metal layer. In some embodiments of the present application, the material of the first defect repair layer 30 can be one or a combination of Al, Ti, Au, Ag, Zn, Cu, Pt, Cr, Fe, Sn, or Ni. For example, the first defect repair layer 30 sequentially includes a magnetron sputtered Al material layer, a Zn material layer, and an Ag material layer. In another example, the first defect repair layer 30 includes a magnetron sputtered Al material layer or an Au material layer. In some embodiments of the present application, the first defect repair layer 30 can be formed by spin coating or spray coating of a non-metallic conductive material such as graphite or conductive silicon.

[0102] In some embodiments of the present application, referring to FIG. 2 , FIG. 2 shows another structural schematic diagram of the thin film capacitor in the present application, wherein the first defect repair layer 30 includes a multi-layer sub-metal layer 301. The arrangement of the multi-layer sub-metal layer can, firstly, enable the sub-metal layer 301 away from the dielectric layer 20 to further protect the sub-metal layer 301 close to the dielectric layer, thereby ensuring its strength and service life. Secondly, when the sub-metal layer away from the dielectric layer adopts a metal material with more stable oxidation resistance (i.e., relatively more stable metal activity) relative to the sub-metal layer close to the dielectric layer, oxidation of the sub-metal layer 301 close to the dielectric layer can also be avoided. Finally, in the thin film capacitor of the present application, generally, the better the conductivity of the defect repair layer, the better the working performance of the thin film capacitor can be guaranteed (specifically, the smaller the energy loss during the operation of the thin film capacitor). Therefore, when a multi-layer sub-metal layer structure is adopted, while overcoming the problem that the sub-metal layer of the first defect repair layer close to the dielectric layer is easily oxidized and affects the working performance of the thin film capacitor (such as the situation where the electrical connectivity is affected after oxidation and it cannot work normally, etc.), a metal material with better conductivity can be selected to be set close to the dielectric layer, thereby ensuring that the overall conductivity of the defect repair layer in the thin film capacitor is better, so as to achieve the above-mentioned effect.

[0103] As an example, refer to Figure 3, which shows another structural schematic diagram of the thin film capacitor in the present application, wherein the first defect repair layer 30 includes overlapping aluminum metal layers 31 and zinc metal layers 32, and the aluminum metal layer 31 is located between the zinc metal layer 32 and the dielectric layer 20, that is, the aluminum metal layer 31 first covers the dielectric layer 20, and then the zinc metal layer 32 covers the aluminum metal layer 31. Since the aluminum metal layer 31 has good ductility and conductivity, the phenomenon of cracks in the aluminum metal layer 31 when the thin film capacitor is bent can be avoided as much as possible; at the same time, the zinc metal layer 32 has good ductility and stable chemical properties, which can avoid cracks in the zinc metal layer 32 and protect the aluminum metal layer 31 from oxidation failure.

[0104] In some embodiments of the present application, the first defect repair layer includes overlapping aluminum metal layers and gold (Au) metal layers, and the aluminum metal layer is located between the gold (Au) metal layer and the dielectric layer 20, so that the gold (Au) metal layer with more stable chemical properties protects the aluminum metal layer.

[0105] In some embodiments of the present application, the first defect repair layer includes an overlapping aluminum metal layer and a titanium metal layer, and the aluminum metal layer is protected by the titanium metal layer having stable chemical properties and high structural strength.

[0106] It can be understood that the first defect repair layer 30 can also include multiple layers of aluminum metal layers 31 and zinc metal layers 32 (or gold (Au) metal layers, titanium metal layers) arranged in an interlaced manner, that is, there is a zinc metal layer 32 between adjacent aluminum metal layers 31, and there is an aluminum metal layer 31 between adjacent zinc metal layers 32, so that the multiple layers of aluminum metal layers 31 and zinc metal layers 32 arranged in an interlaced manner serve as multiple sub-metal layers 301 and prevent the first defect repair layer 30 from crack transmission; alternatively, the first defect repair layer 30 can also include multiple layers of sub-metal layers of different materials (such as aluminum, silver, zinc, titanium and gold) or sub-metal layers of the same material (such as aluminum).

[0107] In some embodiments of the present application, the researchers conducted the following experiment 2 to investigate the effect of different thicknesses of the metal layer in the defect repair layer on the performance of the thin film capacitor:

[0108] Experimental purpose: Based on the performance impact of thin film capacitors used for human tumor treatment, verify that the total thickness of the sub-metal layer with conductivity better than or equal to that of metal aluminum is stable;

[0109] Experimental plan: Prepare a first electrode layer 10 made of gold-plated copper and a second electrode layer 40 made of conductive hydrogel. The dielectric layer 20 (polyimide / PVDF-TrFE-CFE) is 5 μm thick, and the defect repair layer 30 is located on the side of the dielectric layer 20 facing the second electrode layer 40. The first electrode layer 10, dielectric layer 20, defect repair layer 30, and second electrode layer 40 each have an area of ​​3.14 square centimeters and are stacked vertically. Based on this, multiple thin film capacitor samples of the same size were prepared, each with aluminum sub-metal layers of varying thickness in the defect repair layer 30. Tests were performed according to the following steps:

[0110] (1) Set the test environment temperature to 25°C;

[0111] (2) Turn on the KEYSIGHT E4980AL LCR digital source meter, set the test voltage to 1V, the test frequency to 200kHz, and the test mode to Cs-D (capacitance-loss) mode;

[0112] (3) One of the two test clamps of the digital source meter is electrically connected to the first electrode layer 10 and is turned on, and the other is electrically connected to the test electrode attached to the side of the second electrode layer 40 away from the dielectric layer and is turned on;

[0113] (4) The Cs value recorded is the capacitance value, and the D value is the dielectric loss tangent value;

[0114] (5) Based on the data obtained in step (4), determine the film formation condition of the sub-metal layer.

[0115] The experimental results are shown in Table A:

[0116] Table A. Sub-metal layer thicknesses that verify electrical conductivity is better than or equal to that of aluminum:

[0117] From the experimental data in Table A, it can be seen that when the thickness of the sub-metal layer is 1nm, its capacitance value and dielectric loss value cannot be read, so it is judged that the sub-metal layer has not formed a film, but because of its measurement observation that when the thickness of the defect repair layer reaches 10nm, the air gap ionization phenomenon is weak, which shows that it can also fill the tiny pits on the surface of the dielectric layer 20 to a certain extent, so the defect repair layer of this thickness can also improve the air gap ionization situation; comparing the three groups of experimental data of Experiment 2, Experiment 3 and Experiment 4, it can be seen that the capacitance values ​​of the thin film capacitors in Experiment 2, Experiment 3 and Experiment 4 are normal data, but the dielectric loss value of the thin film capacitor corresponding to Experiment 2 is much larger than that of Experiment 3 and Experiment 4, so it is judged that the sub-metal layer with a thickness of 10nm has not formed a good film; in summary, a sub-metal layer less than or equal to 10nm cannot form a stable film. Therefore, in some embodiments of the present application, the total thickness of the sub-metal layer with a conductivity better than or equal to that of metal aluminum in the first defect repair layer is selected to be greater than 10nm.

[0118] The second electrode layer and the defect repair layer of the film capacitor are stacked, and there is a possibility of air between the contact surfaces of the two, which has an adverse effect on the capacitance value, dielectric loss, etc. of the film capacitor. The researchers of this application have found through experiments that when the defect repair layer uses a sub-metal layer with a resistivity better than or equal to that of aluminum metal, it can effectively reduce the dielectric loss of the film capacitor and improve the overall performance of the film capacitor. Therefore, it can be known that the sub-metal layer with a resistivity better than or equal to that of aluminum metal is one of the important factors affecting the performance of the film capacitor. Therefore:

[0119] In some embodiments of the present application, the researchers conducted the following experiment 3 to investigate the effect of different thicknesses of the metal layer in the defect repair layer on the performance of the thin film capacitor:

[0120] Experimental purpose: To verify the effect of different total thickness values ​​of sub-metal layers with conductivity better than or equal to that of metallic aluminum on the performance of film capacitors used for human tumor treatment;

[0121] Experimental plan: Prepare a first electrode layer 10 made of gold-plated copper and a second electrode layer 40 made of conductive hydrogel. The dielectric layer 20 (polyimide / PVDF-TrFE-CFE) is 5 μm thick, and the defect repair layer 30 is located on the side of the dielectric layer 20 facing the second electrode layer 40. The first electrode layer 10, dielectric layer 20, defect repair layer 30, and second electrode layer 40 each have an area of ​​3.14 square centimeters and are stacked vertically. Based on this, multiple thin film capacitor samples of the same size with different sub-metal layer thicknesses are prepared, respectively, when the sub-metal layer is aluminum, and when the sub-metal layer is aluminum and titanium. The samples are then tested according to the following steps:

[0122] (1) Set the test environment temperature to 25°C;

[0123] (2) Turn on the KEYSIGHT E4980AL LCR digital source meter, set the test voltage to 1V, the test frequency to 200kHz, and the test mode to Cs-D (capacitance-loss) mode;

[0124] (3) One of the two test clamps of the digital source meter is electrically connected to the first electrode layer 10 and is turned on, and the other is electrically connected to the test electrode attached to the side of the second electrode layer 40 away from the dielectric layer and is turned on;

[0125] (4) The Cs value recorded is the capacitance value, and the D value is the dielectric loss tangent value;

[0126] (5) Remove the sample and bend it three times by hand (the bending angle is about 90°). Observe whether there are obvious creases on the film capacitor sample. If there are creases, it means that the film capacitor is brittle.

[0127] (6) If there is no crease on the film capacitor after bending in step (5), repeat steps (1) to (4) to compare whether the capacitance value of the film capacitor before and after bending has changed. If there is no change, it means that the film capacitor is not brittle; otherwise, it also means that the film capacitor is brittle.

[0128] The results of Examples 1 to 9 are shown in Table B.

[0129] Table B. Sub-metal layer thickness selection to verify electrical conductivity better than or equal to that of metallic aluminum:

[0130] Comparative Example

[0131] The comparative example of the thin film capacitor is basically the same as the thin film capacitor embodiments 1 to 9, except that the defect repair layer 30 is not provided in the comparative example of the thin film capacitor. The comparative example of the thin film capacitor obtained by testing is shown in Table C:

[0132] Table C. Film capacitor comparative experimental data:

[0133] It can be seen from Table B and Table C above that the air gap ionization of the thin film capacitors prepared using Examples 1 to 8 of this scheme is significantly weaker than that of the thin film capacitors in the comparative example, indicating that the present application significantly improves the air gap ionization phenomenon caused by the generation of tiny gaps between the dielectric layer and the corresponding electrode layer, while making the electrical connection with the electrode layer more stable.

[0134] At the same time, it can be seen from Table B that, under the condition of ensuring the film thickness of the titanium metal layer, as the total thickness of the sub-metal layer continues to increase, the dielectric loss of the thin film capacitor is generally reduced to a stable trend. However, when the total thickness of the first defect repair layer is too thick, the film capacitor will be bent and caused by brittle cracking. This shows that the total thickness of the first defect repair layer should not be too thick, otherwise it will easily cause the defect repair layer in the film capacitor to be bent and brittle cracking, thereby affecting the performance of the film capacitor. Of course, when the film capacitor is naturally not bent or the bending angle is small (the bending angle is not less than 135 degrees), as shown in Figure 12 (mark two reference points on the film capacitor, and then use a right angle to make the line between the two points tangent to the film capacitor, and read the scale value on the right angle, which is the bending angle), the thickness of the defect repair layer can reach thousands of nanometers. Based on the above performance data changes, in some embodiments of the present application, the total thickness of the sub-metal layer in the first defect repair layer whose electrical conductivity is better than or equal to that of metal aluminum is preferably 10nm-400nm. For example, for an embodiment in which the first defect repair layer includes overlapping aluminum metal layers and titanium metal layers, the total thickness of the aluminum metal layer is 10nm-400nm; for another example, for an embodiment in which the first defect repair layer includes overlapping aluminum metal layers and gold metal layers, the total thickness of the aluminum metal layer and the gold metal layer is preferably 10nm-400nm; for another example, for an embodiment in which the first defect repair layer includes overlapping gold metal layers and copper metal layers, the total thickness of the gold metal layer and the copper metal layer is preferably 10nm-400nm.

[0135] Preferably, the total thickness of the sub-metal layer in the first defect repair layer whose electrical conductivity is better than or equal to that of metal aluminum is 50nm-400nm. For example, for an embodiment in which the first defect repair layer includes overlapping aluminum metal layers and titanium metal layers, the total thickness of the aluminum metal layer is 50nm-400nm; for another example, for an embodiment in which the first defect repair layer includes overlapping aluminum metal layers and gold metal layers, the total thickness of the aluminum metal layer and the gold metal layer is 50nm-400nm; for another example, for an embodiment in which the first defect repair layer includes overlapping gold metal layers and copper metal layers, the total thickness of the gold metal layer and the copper metal layer is 50nm-400nm.

[0136] In some embodiments of the present application, the first defect repair layer 30 can be formed on the side of the dielectric layer 20 facing away from the first electrode layer 10 by magnetron sputtering. During the magnetron sputtering process, the target material (such as aluminum) is sputtered by ion bombardment to produce small-diameter target atoms or molecules that can be deposited and enter the tiny pits on the surface of the dielectric layer 20, thereby compensating for the surface defects (microscopic pits) of the dielectric layer 20, so that one side of the first defect repair layer 30 is tightly bonded to the microscopic pits on the surface of the dielectric layer 20. In some embodiments of the present application, the first defect repair layer 30 can also be formed on the side of the dielectric layer 20 facing away from the first electrode layer 10 by electron beam evaporation. During the electron beam evaporation process, accelerated electrons are used to bombard the coating material (such as zinc). The kinetic energy of the electrons is converted into heat energy to heat and evaporate the coating material, ultimately forming the first defect repair layer 30 on the surface of the dielectric layer 20.

[0137] In some embodiments of the present application, for example, for an embodiment in which the first defect repair layer 30 includes overlapping aluminum metal layers 31 and zinc metal layers 32, when preparing the first defect repair layer 30, the aluminum metal layer 31 can be first formed on the surface of the dielectric layer 20 by magnetron sputtering, and then the zinc metal layer 32 can be formed on the aluminum metal layer 31 by magnetron sputtering.

[0138] In some embodiments of the present application, when the first defect repair layer 30 is not bent or has a small bending angle (the bending angle is not less than 135°), the thickness of the first defect repair layer 30 is 10nm to 1000nm, and the tolerance value of the first defect repair layer is ±10% of its thickness value. Preferably, the thickness of the first defect repair layer 30 is 10nm to 800nm. More preferably, the thickness of the first defect repair layer 30 is 50nm to 450nm. The first defect repair layer 30 meeting the above-mentioned size range can have good flexibility, and at the same time, it can also prevent the first defect repair layer 30 from being prone to cracking due to bending due to being too thick or from being unable to completely cover the dielectric layer 20 due to being too thin.

[0139] In some embodiments of the present application, for example, the first defect repairing layer 30 includes an overlapping aluminum metal layer 31 and a zinc metal layer 32 , the thickness of the aluminum metal layer 31 is 10 nm to 1000 nm, and the thickness of the zinc metal layer 32 is 10 nm to 1000 nm.

[0140] It is understandable that the first defect repairing layer 30 can also be formed on the surface of the dielectric layer 20 by physical vapor deposition, for example, arc plasma plating, ion plating and molecular beam epitaxy, so as to compensate for the surface defects of the dielectric layer 20.

[0141] In an embodiment of the present application, the present application sets a first defect repair layer 30 between the dielectric layer 20 and the second electrode layer 40. Since one side of the first defect repair layer 30 is tightly combined with the microscopic pits on the surface of the dielectric layer 20, it also avoids the generation of tiny gaps between the dielectric layer 20 and the corresponding second electrode layer 40 and the resulting air gap ionization phenomenon, and ultimately prevents the electrode layer (for example, the second electrode layer 40) from being partially volatilized or vaporized and damaged due to air gap ionization. In addition, if the defect repair layer is not added, since air is easily present between the dielectric layer 20 and the second electrode layer 40, the overall capacitance will be reduced. Therefore, adding a defect repair layer can expel air to a certain extent, thereby ensuring good capacitance of the transducer.

[0142] In some embodiments of the present application, the second electrode layer 40 is a finished metal sheet, and the tensile index of the second electrode layer 40 is greater than the tensile index of the first defect repairing layer 30 .

[0143] It should be noted that the inventors discovered during the research process that during the thin film capacitor tumor treatment process, since the thin film capacitor needs to be close to human skin and will bend, wearing it for more than a certain period of time will produce sweat, etc. Therefore, the second electrode layer 40 close to the human skin side needs to have waterproof and anti-cracking functions to prevent sweat exuded from the human skin or water vapor generated by the hydrogel from penetrating into the interior of the thin film capacitor. The second electrode layer 40 is directly formed on the surface of the dielectric layer 20 by physical vapor deposition. Although the tiny gap between the second electrode layer 40 and the dielectric layer 20 can be eliminated, the deposited second electrode layer 40 is prone to cracking after the thin film capacitor is bent, thereby causing sweat exuded from the human skin or water vapor generated by the hydrogel to penetrate into the interior of the thin film capacitor.

[0144] In the above embodiment, since the second electrode layer 40 used in the thin film capacitor used for tumor treatment is a finished metal sheet, and the tensile index of the second electrode layer 40 is greater than the tensile index of the first defect repair layer 30, the second electrode layer 40 can be prevented from cracking when the thin film capacitor is bent, thereby preventing sweat exuded from human skin or water vapor generated by hydrogel from penetrating into the interior of the thin film capacitor. At the same time, there is no small gap between the first defect repair layer 30 and the dielectric layer 20, so air gap ionization will not occur, thereby ultimately providing a tumor treatment thin film capacitor that is waterproof and resistant to air gap ionization.

[0145] It should be noted that the tensile index refers to the tensile strength of the sample (the second electrode layer 40 or the first defect-repairing layer 30), which shows the maximum tensile strength the sample can withstand before breaking. In some embodiments of the present application, the tensile index of the second electrode layer 40 can be the maximum tensile strength it can withstand before breaking. In some embodiments of the present application, the tensile index of the first defect-repairing layer 30 can be the maximum tensile strength it can withstand before breaking.

[0146] In some embodiments of the present application, the thickness of the second electrode layer 40 is greater than the thickness of the first defect repair layer 30. The thicker second electrode layer 40 has a larger tensile index, which is beneficial to ensure that the tensile index of the second electrode layer 40 is greater than the tensile index of the first defect repair layer 30; at the same time, the thicker second electrode layer 40 has better physical protection performance, ensuring the stability of the electrical connection.

[0147] In some embodiments of the present application, referring to FIG4 , FIG4 shows another structural schematic diagram of a thin film capacitor in an embodiment of the present application, wherein the side of the dielectric layer 20 facing away from the first electrode layer 10 has a first roughness, and the side of the first defect repair layer 30 facing away from the dielectric layer 20 has a second roughness; wherein the second roughness is less than or equal to the first roughness.

[0148] Preferably, the second roughness is smaller than the first roughness. After the first defect repair layer 30 is formed on the dielectric layer 20, the first defect repair layer 30 is tightly bonded to the microscopic pits of the dielectric layer 20, and the larger pits corresponding to the first roughness of the dielectric layer 20 are partially filled, thereby reducing the plane height difference caused by the microscopic pits, so that the second roughness of the first defect repair layer 30 facing away from the dielectric layer 20 is smaller. After the second electrode layer 40 is bonded to the first defect repair layer 30, the tip discharge phenomenon between the second electrode layer 40 and the first defect repair layer 30 can be weakened. That is to say, by arranging the first defect repair layer 30 that is tightly bonded and has a smaller roughness on the dielectric layer, on the one hand, the air gap ionization phenomenon between the insulating material layer (dielectric layer 20) and the conductive material layer (first defect repair layer 30) is effectively prevented, and at the same time, the tip discharge phenomenon between the two conductive material layers (the second electrode layer 40 and the first defect repair layer 30) is alleviated.

[0149] It should be noted that the roughness (first roughness, second roughness, third roughness or fourth roughness) referred to in this application may refer to the arithmetic mean of the contour deviation of the object within the sampling length, or may refer to the sum of the average value of multiple (for example, 5) largest contour peak heights and the average value of multiple (for example, 5) largest contour valley depths within the sampling length of the object, or may refer to the distance between the contour peak top line and the contour valley bottom line within the sampling length of the object. When measuring the first roughness and the second roughness, the surface roughness of the first defect repair layer 30 can be measured using an atomic force microscope (AFM) or a scanning probe microscope (SPM), and then the surface roughness of the dielectric layer 20 can be measured after the first defect repair layer 30 is removed. For example, the first defect repair layer 30 can be removed by chemical corrosion, and then the surface roughness of the dielectric layer 20 can be measured using a scanning probe microscope; alternatively, the thin film capacitor can be cut open along a cutting plane perpendicular to the dielectric layer 20, and the cross-sectional view of the thin film capacitor can be magnified using an electron microscope, and finally the corresponding roughness can be calculated using the contour lines between the interfaces (for example, the interface between the dielectric layer 20 and the first defect repair layer 30 or the surface contour line of the first defect repair layer 30, etc.).

[0150] In some embodiments of the present application, referring to FIG. 4 , a surface of the dielectric layer 20 facing away from the first electrode layer 10 has a plurality of first microscopic pits 201 ; the first defect repairing layer 30 is tightly combined with the inner wall surface of the first microscopic pits 201 .

[0151] Specifically, the first microscopic pits 201 of the dielectric layer 20 are formed after the dielectric layer 20 is prepared. For example, after the dielectric layer 20 is prepared by an atomization method, the pit structure on the surface of the dielectric layer 20 corresponds to the first microscopic pits 201, so that the first microscopic pits 201 form surface defects of the dielectric layer 20 facing the second electrode layer 40, and the first defect repair layer 30 can be tightly combined with the inner wall surface of the first microscopic pits 201 to compensate for the surface defects of the dielectric layer 20. For example, when the first defect repair layer 30 is prepared by magnetron sputtering, more atoms or molecules generated by magnetron sputtering can enter and fill the first microscopic pits 201, so that the first microscopic pits 201 are partially filled, thereby reducing the height difference of the dielectric layer surface caused by the first microscopic pits 201.

[0152] In some embodiments of the present application, the first electrode layer 10 is laminated to the dielectric layer 20. In some embodiments of the present application, the dielectric layer 20 can be formed with the first electrode layer 10 as a substrate, for example, by forming the dielectric layer 20 on the first electrode layer 10 by atomization.

[0153] Furthermore, in some embodiments of the present application, referring to Figure 5, Figure 5 shows another structural schematic diagram of the thin film capacitor in the embodiment of the present application, wherein the thin film capacitor also includes a flexible conductive layer 70, and the flexible conductive layer 70 is located between the second electrode layer 40 and the first defect repair layer 30. At the same time, the two sides of the flexible conductive layer 70 are respectively adhered to the second electrode layer 40 and the first defect repair layer 30.

[0154] It should be noted that the flexible conductive layer 70 has conductivity and a certain elastic modulus, so that the flexible conductive layer 70 electrically connects the second electrode layer 40 with the first defect repair layer 30, ensuring the electrical connectivity between the second electrode layer 40 and the first defect repair layer 30. At the same time, the elastic modulus of the flexible conductive layer 70 can avoid the phenomenon of tiny gaps between the second electrode layer 40 and the first defect repair layer 30, and prevent the occurrence of tip ionization between the second electrode layer 40 and the first defect repair layer 30.

[0155] Preferably, the flexible conductive layer 70 may be conductive paper, so that the flexible conductive layer 70 has higher tensile and tearing strengths, thereby preventing the flexible conductive layer 70 from being torn when the film capacitor is bent against the surface of the human body.

[0156] In some embodiments of the present application, the flexible conductive layer 70 may also be an indium tin oxide (ITO) film, conductive rubber, or conductive silicone.

[0157] In some embodiments of the present application, the thickness of the flexible conductive layer 70 is 0.001 mm to 1 mm. Preferably, the thickness of the flexible conductive layer 70 is 0.01 mm to 0.8 mm. More preferably, the thickness of the flexible conductive layer 70 is 0.1 mm to 0.6 mm. Specifically, the thickness of the flexible conductive layer 70 meeting the above dimensions can avoid the phenomenon of the flexible conductive layer 70 being too thick and thus causing its flexibility to be reduced, and can also prevent the flexible conductive layer 70 from being too thin and thus causing its cracking.

[0158] It can be understood that the flexible conductive layer 70 can also be formed by stacking at least two of conductive paper, conductive rubber and conductive silicone. For example, conductive paper and conductive rubber are stacked to form the flexible conductive layer 70. The conductive paper ensures the tensile strength of the flexible conductive layer 70, while the conductive rubber ensures the elasticity of the flexible conductive layer 70.

[0159] In some embodiments of the present application, referring to FIG6 , another schematic structural diagram of a thin film capacitor according to an embodiment of the present application is shown. The thin film capacitor further includes a conductive attachment layer 80 attached to the second electrode layer 40. The conductive attachment layer 80 is flexible and adhesive, so as to facilitate adhesion to the surface of human skin and minimize contact damage caused by mismatch between the thin film capacitor and soft tissue. For example, the conductive attachment layer 80 may be a conductive hydrogel or a conductive silicone gel.

[0160] Furthermore, in some embodiments of the present application, such as embodiments in which the dielectric layer 20 is a finished film, since both sides of the finished film of the dielectric layer 20 have surface defects, referring to FIG7 , FIG7 shows another structural schematic diagram of a thin film capacitor in an embodiment of the present application, wherein the thin film capacitor further includes a second defect repair layer 50, and the second defect repair layer 50 is located between the first electrode layer 10 and the dielectric layer 20. The second defect repair layer 50 is conductive, and the surface of the dielectric layer 20 facing the second defect repair layer 50 has microscopic pits. One side of the second defect repair layer 50 is tightly bonded to the microscopic pits on the surface of the dielectric layer 20, and the other side is in direct or indirect electrical contact with the first electrode layer 10.

[0161] Similarly, since a second defect repair layer 50 is provided on the side of the dielectric layer 20 facing the first electrode layer 10, the second defect repair layer 50 is used to compensate for the surface defects of the side of the dielectric layer 20 facing the first electrode layer 10, thereby avoiding the generation of tiny gaps between the dielectric layer 20 and the first electrode layer 10 and the resulting air gap ionization phenomenon, which is beneficial to ensuring the safety of the thin film capacitor in the tumor treatment electrode patch.

[0162] In some embodiments of the present application, the finished film of the dielectric layer 20 can be used as a substrate, and a first defect repair layer 30 can be formed on one side of the finished film of the dielectric layer 20 by magnetron sputtering, and then a second defect repair layer 50 can be formed on the other side of the finished film of the dielectric layer 20.

[0163] In some embodiments of the present application, the finished film of the dielectric layer 20 may be used as a substrate, and then the first defect repair layer 30 and the second defect repair layer 50 may be simultaneously formed (eg, by magnetron sputtering) on ​​both sides of the finished film of the dielectric layer 20 .

[0164] In some embodiments of the present application, the second defect repair layer 50 is a metal layer. In some embodiments of the present application, the material of the second defect repair layer 50 can be one or a combination of Al, Ti, Au, Ag, Zn, Cu, Pt, Cr, Fe, Sn, or Ni. For example, the second defect repair layer 50 sequentially includes a magnetron sputtered Al material layer, a Zn material layer, and an Ag material layer. In another example, the second defect repair layer 50 includes a magnetron sputtered Al material layer or an Au material layer. In some embodiments of the present application, the second defect repair layer 50 can be formed by spin coating or spray coating of a non-metallic conductive material such as graphite or conductive silicon.

[0165] In some embodiments of the present application, refer to Figure 8, which shows another structural schematic diagram of a thin film capacitor in an embodiment of the present application, wherein the second defect repair layer 50 includes multiple metal layers, such as multiple aluminum metal layers or multiple zinc metal layers. The zinc metal layer separated from the dielectric layer 20 can protect the aluminum metal layer close to the dielectric layer, thereby avoiding the phenomenon of oxidation failure of the aluminum metal layer close to the dielectric layer. As an example, the second defect repair layer 50 includes overlapping aluminum metal layers and zinc metal layers; as another example, the second defect repair layer 50 includes overlapping aluminum metal layers and gold (Au) metal layers. As another example, the second defect repair layer 50 includes overlapping aluminum metal layers and titanium (Ti) metal layers.

[0166] It is understandable that the second defect repairing layer 50 may also include multiple layers of aluminum metal layers and zinc metal layers arranged in an alternating manner, that is, there is a zinc metal layer between adjacent aluminum metal layers, and there is an aluminum metal layer between adjacent zinc metal layers.

[0167] In some embodiments of the present application, the second defect repair layer 50 can be formed on the side of the dielectric layer 20 facing the first electrode layer 10 by magnetron sputtering. During the magnetron sputtering process, the target material (e.g., aluminum) is sputtered by ion bombardment to produce target atoms or molecules with small diameters that can be deposited and enter the tiny pits (microscopic pits) on the surface of the dielectric layer 20. This allows one side of the second defect repair layer 50 to be tightly bonded to the microscopic pits on the surface of the dielectric layer 20, thereby compensating for the surface defects of the dielectric layer 20. In some embodiments of the present application, the second defect repair layer 50 can also be formed on the side of the dielectric layer 20 facing the first electrode layer 10 by electron beam evaporation. During the electron beam evaporation process, accelerated electrons are used to bombard the coating material (e.g., zinc). The kinetic energy of the electrons is converted into heat energy, causing the coating material to evaporate by heating, ultimately forming the second defect repair layer 50 on the surface of the dielectric layer 20.

[0168] In some embodiments of the present application, for example, for an embodiment in which the second defect repair layer 50 includes overlapping aluminum metal layers 31 and zinc metal layers 32, when preparing the second defect repair layer 50, an aluminum metal layer can be first formed on the surface of the dielectric layer 20 by magnetron sputtering, and then a zinc metal layer can be formed on the aluminum metal layer by magnetron sputtering.

[0169] In some embodiments of the present application, the second defect repair layer 50 has a thickness of 10 nm to 1000 nm. Preferably, the first defect repair layer 30 has a thickness of 10 nm to 800 nm. More preferably, the second defect repair layer 50 has a thickness of 50 nm to 450 nm. The second defect repair layer 50 meeting the above size range can provide good flexibility while also preventing the second defect repair layer 50 from cracking due to excessive thickness or from failing to fully cover the dielectric layer 20 due to excessive thinness.

[0170] In some embodiments of the present application, for example, the second defect repairing layer 50 includes an overlapping aluminum metal layer 31 and a zinc metal layer 32 , the thickness of the aluminum metal layer 31 is 10 nm to 1000 nm, and the thickness of the zinc metal layer 32 is 10 nm to 1000 nm.

[0171] In some embodiments of the present application, the first electrode layer 10 is a finished metal sheet, and the tensile index of the first electrode layer 10 is greater than the tensile index of the second defect-repairing layer 50. In the present application, the first electrode layer 10 has a greater tensile index, which helps ensure that the tensile index of the first electrode layer 10 is greater than the tensile index of the second defect-repairing layer 50.

[0172] In some embodiments of the present application, referring to FIG8 , the surface of the dielectric layer 20 facing the first electrode layer 10 has a third roughness, and the surface of the second defect repair layer 50 facing away from the dielectric layer 20 has a fourth roughness, and the fourth roughness is less than or equal to the third roughness.

[0173] Specifically, after the second defect repair layer 50 is formed on the dielectric layer 20, since the second defect repair layer 50 is tightly combined with the microscopic pits of the dielectric layer 20, the larger pits corresponding to the third roughness of the dielectric layer 20 are partially compensated, reducing the plane height difference caused by the microscopic pits, making the fourth roughness of the second defect repair layer 50 facing away from the dielectric layer 20 smaller. After the first electrode layer 10 and the second defect repair layer 50 are bonded, the tip discharge phenomenon between the first electrode layer 10 and the second defect repair layer 50 can be weakened.

[0174] It should be noted that when measuring the third roughness and the fourth roughness, the surface roughness of the second defect repair layer 50 can be measured first using an atomic force microscope (AFM) or a scanning probe microscope (SPM), and then the surface roughness of the dielectric layer 20 can be measured after the second defect repair layer 50 is removed. For example, the first defect repair layer 30 is removed by chemical corrosion, and then the surface roughness of the dielectric layer 20 is measured using a scanning probe microscope; alternatively, the thin film capacitor can be cut open through a cutting plane perpendicular to the dielectric layer 20, and the cross-sectional view of the thin film capacitor can be magnified by an electron microscope, and the corresponding roughness can be calculated through the contour lines between the interfaces (for example, the interface between the dielectric layer 20 and the second defect repair layer 50 or the surface contour line of the second defect repair layer 50, etc.).

[0175] In some embodiments of the present application, referring to FIG8 , a surface of the dielectric layer 20 facing the first electrode layer 10 has a plurality of second microscopic pits 202, and the second defect repairing layer 50 is tightly bonded to the inner wall surfaces of the second microscopic pits 202 to compensate for the surface defects of the dielectric layer 20. The second microscopic protrusions 501 of the second defect repairing layer 50 can be formed during the preparation process of the second defect repairing layer 50. For example, when the second defect repairing layer 50 is prepared by magnetron sputtering, the atoms or molecules generated by the magnetron sputtering enter and fill the second microscopic pits 202, thereby generating the second defect repairing layer 50 tightly bonded to the inner wall surfaces of the second microscopic pits 202, thereby eliminating the tiny interlayer gaps between the dielectric layer 20 and the second defect repairing layer 50.

[0176] In some embodiments of the present application, the thin film capacitor further includes a flexible substrate 60, and the first electrode layer 10 is attached to the flexible substrate 60. Preferably, the flexible substrate 60 is an insulating polyimide film, so that the thin film capacitor is flexible and bendable.

[0177] In some embodiments of the present application, refer to Figure 9, which shows another structural schematic diagram of the thin film capacitor in an embodiment of the present application, wherein the dielectric layer includes a first insulating layer 21 and a second insulating layer 22 that are tightly bonded to each other, and the first defect repair layer is tightly bonded to the side of the second insulating layer 22 facing away from the first insulating layer 21, and the insulation strength of the second insulating layer 22 is greater than the insulation strength of the first insulating layer 21.

[0178] In the above embodiment, by arranging the second insulating layer 22 between the first insulating layer 21 and the first defect repair layer 30, since the first insulating layer 21 and the second insulating layer 22 are tightly bonded to each other, and the insulation strength of the second insulating layer 22 is greater than the insulation strength of the first insulating layer 21, on the one hand, the phenomenon of a small gap between the first insulating layer 21 and the second insulating layer 22 can be avoided, and on the other hand, the anti-breakdown performance of the dielectric layer 20 of the thin-film capacitor can be effectively enhanced, which is beneficial to ensure the safety of the tumor treatment transducer in the tumor treatment electrode patch.

[0179] Exemplarily, the material of the first insulating layer 21 may include one or more of poly(VDF-TrFE-CTFE)(poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene)), poly(VDF-TrFE-CFE)(poly(vinylidene fluoride-trifluoroethylene-1-chlorofluoroethylene)), poly(VDF-TrFECFE-CTFE)(poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene-chlorofluoroethylene)), and poly(VDF-DB)(poly(vinylidene fluoride-diethylene glycol butyl ether)).

[0180] In some embodiments of the present application, the thickness of the first insulating layer 21 is 1 μm to 100 μm. In some embodiments of the present application, the thickness of the first insulating layer 21 is 1 μm to 10 μm. Preferably, the thickness of the first insulating layer 21 is 2 μm to 8 μm. The thickness of the first insulating layer 21 meeting the aforementioned dimensional requirements can ensure that the tumor treatment transducer has a high capacitance while also preventing breakdown of the tumor treatment transducer due to an excessively thin first insulating layer 21.

[0181] In some embodiments of the present application, the first insulating layer 21 can be formed on the first electrode layer 10 by spin coating, doctor blade coating, atomization, casting, or screen printing. In other embodiments of the present application, the first insulating layer 21 is directly attached to the first electrode layer 10 in the form of a finished film.

[0182] The material of the second insulating layer 22 is at least one of a non-conductive oxide, a nitride, a carbide and an insulating high molecular polymer, such as: wherein the oxide is selected from at least one of silicon dioxide, zirconium oxide, aluminum oxide, etc., wherein the nitride is selected from one of silicon nitride, boron nitride, aluminum nitride, etc., wherein the carbide is selected from chromium carbide, etc. In addition, when the insulating layer material is an insulating high molecular polymer, it can be selected from at least one of siloxane polymer, silazane polymer, polymethyl methacrylate (PMMA), polyimide (PI), polyethylene (PE), polyethylene terephthalate (PET), polyphenylene sulfide (PPS), polyurethane (PU), fluorinated ethylene propylene copolymer (FEP), fusible polytetrafluoroethylene (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), polyetheretherketone (PEEK), polysilazane, polycarbonate, silicone resin, fluoride material and rubber, etc.

[0183] In some embodiments of the present application, the thickness of the second insulating layer 22 is 1 nm to 1000 nm. Preferably, the thickness of the second insulating layer 22 is 5 nm to 800 nm. More preferably, the thickness of the second insulating layer 22 is 10 nm to 300 nm. The thickness of the second insulating layer 22 satisfies the aforementioned dimensional relationship. This can, on the one hand, prevent the second insulating layer 22 from being too thick, which in some cases increases its brittleness and causes cracking when the tumor treatment transducer is bent. On the other hand, it can also prevent the phenomenon of a significant reduction in the capacitance of the tumor treatment transducer due to an excessively thick second insulating layer 22.

[0184] In some embodiments of the present application, the second insulating layer 22 can be formed on the first insulating layer 21 by magnetron sputtering. During the magnetron sputtering process, target atoms or molecules with small diameters generated by ion bombardment of the target material (e.g., silicon dioxide) can be deposited and enter into tiny pits on the surface of the first insulating layer 21, so that the second insulating layer 22 is tightly bonded to the first insulating layer 21. In some embodiments of the present application, the second insulating layer 22 can also be formed on the first insulating layer 21 by electron beam evaporation. During the electron beam evaporation process, accelerated electrons are used to bombard the coating material (e.g., silicon dioxide). The kinetic energy of the electrons is converted into thermal energy, causing the coating material to evaporate by heating, ultimately forming the second insulating layer 22 on the surface of the first insulating layer 21.

[0185] In some embodiments of the present application, the second insulating layer 22 can be formed on the first insulating layer 21 by spin coating an organic solution. For example, a solution containing polydimethylsiloxane soluble insulating material is formed on the first insulating layer 21 by spin coating. Since the solution is subjected to centrifugal force during the spin coating process, the solution can enter the tiny pits on the surface of the first insulating layer 21. After the solution solidifies, the second insulating layer 22 tightly bonded to the first insulating layer 21 can be obtained.

[0186] It is understandable that the second insulating layer 22 can also be formed on the surface of the first insulating layer 21 by physical vapor deposition, such as arc plasma plating, ion plating and molecular beam epitaxy, so as to fill the microscopic pits on the surface of the first insulating layer 21.

[0187] Furthermore, in order to better implement the thin film capacitor in the embodiment of the present application, based on the thin film capacitor, the present application also provides a method for preparing the thin film capacitor. Referring to FIG10 , FIG10 shows a flow chart of the method for preparing the thin film capacitor in the embodiment of the present application, wherein the method for preparing the thin film capacitor includes:

[0188] Step S901, providing a first electrode layer 10;

[0189] In some embodiments of the present application, the first electrode layer 10 may refer to a corresponding metal layer on a circuit board. For example, a portion of a copper foil area is exposed on the circuit board, and the dielectric layer 20 is formed (for example, by atomization) within the copper foil area, while the power interface of the circuit board can be conveniently electrically connected to a power source. In some embodiments of the present application, such as embodiments in which the dielectric layer 20 is a finished film, a second defect repair layer 50 may be provided between the dielectric layer 20 and the first electrode layer 10 to compensate for defects on the side of the dielectric layer 20 facing the first electrode layer 10.

[0190] Step S902 , forming a dielectric layer 20 on the first electrode layer 10 ;

[0191] Preferably, the material of the dielectric layer 20 may include one or more of poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene), poly(vinylidene fluoride-trifluoroethylene-1-chlorofluoroethylene), poly(vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene-chlorofluoroethylene) or poly(VDF-DB) (poly(vinylidene fluoride-diethylene glycol butyl ether)). Since the above materials have a relatively high dielectric constant, they help to increase the capacitance of the film capacitor when the thickness and area of ​​the dielectric layer 20 are constant, thereby achieving the purpose of better applying the tumor treatment alternating electric field to the patient's treatment site.

[0192] In step S903, a first defect repair layer 30 is formed on the side of the dielectric layer 20 facing away from the first electrode layer 10; wherein the first defect repair layer is conductive, and the side of the dielectric layer facing the first defect repair layer has microscopic pits, one side of the first defect repair layer is tightly combined with the microscopic pits on the surface of the dielectric layer, and the other side is directly or indirectly electrically contacted with the second electrode layer.

[0193] In some embodiments of the present application, the first defect repair layer 30 is a metal layer. In some embodiments of the present application, the material of the first defect repair layer 30 can be one or a combination of Al, Ti, Au, Ag, Zn, Cu, Pt, Cr, Fe, Sn or Ni. In some embodiments of the present application, the first defect repair layer 30 includes multiple sub-metal layers 301. The first defect repair layer 30 with multiple sub-metal layers 301 can prevent such cracks from being transmitted between the sub-metal layers 301, thereby avoiding the occurrence of penetrating cracks in the first defect repair layer 30 as much as possible. In some embodiments of the present application, the first defect repair layer 30 includes overlapping aluminum metal layers 31 and zinc metal layers 32.

[0194] In some embodiments of the present application, the first defect repair layer 30 can be formed on the side of the dielectric layer 20 facing away from the first electrode layer 10 by magnetron sputtering. In some embodiments of the present application, the first defect repair layer 30 can also be formed on the side of the dielectric layer 20 facing away from the first electrode layer 10 by electron beam evaporation. In some embodiments of the present application, for example, in an embodiment in which the first defect repair layer 30 includes overlapping aluminum metal layers 31 and zinc metal layers 32, when preparing the first defect repair layer 30, the aluminum metal layer 31 can be first formed on the surface of the dielectric layer 20 by magnetron sputtering, and then the zinc metal layer 32 can be formed on the aluminum metal layer 31 by magnetron sputtering.

[0195] In step S904 , a second electrode layer 40 is formed on a surface of the first defect repairing layer 30 facing away from the dielectric layer 20 .

[0196] In some embodiments of the present application, the second electrode layer 40 of the thin film capacitor is closer to the surface of human skin, while the first electrode layer 10 of the thin film capacitor is farther away from the surface of human skin. In some embodiments of the present application, for example, in embodiments where the second electrode layer 40 is closer to the surface of human skin, the second electrode layer 40 is preferably a stainless steel metal layer or a titanium metal layer with a thickness of 0.005 mm to 0.1 mm. This not only prevents corrosion of the second electrode layer 40, but also blocks sweat from penetrating into the dielectric layer 20 inside the thin film capacitor, thereby preventing the dielectric layer 20 of the thin film capacitor from being broken down by human sweat.

[0197] The thin film capacitor prepared by the thin film capacitor preparation method of the present application has a first defect repair layer 30 set on the side of the dielectric layer 20 away from the first electrode layer 10. The first defect repair layer 30 can be used to compensate for the surface defects of the side of the dielectric layer 20 away from the first electrode layer 10, thereby avoiding the generation of tiny gaps between the dielectric layer 20 and the corresponding electrode layer and the resulting air gap ionization phenomenon, which is beneficial to ensuring the safety of the thin film capacitor in the tumor treatment electrode patch.

[0198] In some embodiments of the present application, referring to FIG11 , FIG11 shows another flow chart of a method for preparing a thin film capacitor in an embodiment of the present application, wherein the method for preparing a thin film capacitor includes:

[0199] Step S1001, providing a circuit board, wherein the circuit board has a flexible substrate 60 and a first electrode layer 10;

[0200] Step S1002, forming a dielectric layer 20 on the first electrode layer 10;

[0201] Step S1003 , forming a first defect repairing layer 30 on a side of the dielectric layer 20 away from the first electrode layer 10 ; wherein the first defect repairing layer 30 is used to compensate for surface defects on the side of the dielectric layer 20 away from the first electrode layer 10 ;

[0202] Step S1004 , forming a flexible conductive layer 70 on a side of the first defect repairing layer 30 facing away from the dielectric layer 20 ;

[0203] Step S1005 , forming a second electrode layer 40 on a side of the flexible conductive layer 70 facing away from the first defect repairing layer 30 ;

[0204] Step S1006 , forming a conductive attachment layer 80 on the second electrode layer 40 .

[0205] It should be noted that the flexible conductive layer 70 has electrical conductivity and a low elastic modulus, enabling it to electrically connect the second electrode layer 40 to the first defect-repairing layer 30, ensuring electrical connectivity between the second electrode layer 40 and the first defect-repairing layer 30. Furthermore, the conductive attachment layer 80 is flexible and adhesive, allowing it to adhere to the surface of human skin and minimize contact damage caused by mismatch between the thin-film capacitor and soft tissue. For example, the flexible conductive layer 70 can be one or more of conductive paper, polyimide, or polyester film, and the conductive attachment layer 80 can be conductive hydrogel or conductive silicone gel.

[0206] Furthermore, to better implement the thin film capacitors in the embodiments of this application, the present application also provides a tumor treatment electrode patch based on the thin film capacitors. The tumor treatment electrode patch includes a thin film capacitor as described in any of the above embodiments. Because the tumor treatment electrode patch in the embodiments of this application is provided with the thin film capacitors in the above embodiments, it has all the beneficial effects of the above film capacitors, and will not be further described here.

[0207] Furthermore, to better implement the tumor treatment electrode patch of the embodiments of this application, the present application also provides a tumor treatment system based on the tumor treatment electrode patch, which includes the tumor treatment electrode patch of any of the above embodiments. Because the tumor treatment system of the embodiments of this application is equipped with the film capacitor of the above embodiments, it has all the beneficial effects of the film capacitor, and will not be further described here.

[0208] In the above embodiments, the description of each embodiment has its own focus. For parts that are not described in detail in a certain embodiment, please refer to the detailed description of other embodiments above and will not be repeated here.

[0209] The basic concepts have been described above. It will be apparent to those skilled in the art that the detailed disclosure above is merely illustrative and does not limit the present application. Although not explicitly stated herein, those skilled in the art may make various modifications, improvements, and amendments to the present application. Such modifications, improvements, and amendments are suggested in the present application and remain within the spirit and scope of the exemplary embodiments of the present application.

[0210] At the same time, this application uses specific terms to describe the embodiments of this application. For example, "one embodiment," "an embodiment," and / or "some embodiments" refer to a certain feature, structure, or characteristic related to at least one embodiment of this application. Therefore, it should be emphasized and noted that "one embodiment," "an embodiment," or "an alternative embodiment" mentioned twice or multiple times in different locations in this specification does not necessarily refer to the same embodiment. In addition, certain features, structures, or characteristics in one or more embodiments of this application may be appropriately combined.

[0211] Similarly, it should be noted that, in order to simplify the presentation of this application and thus facilitate understanding of one or more embodiments of the invention, the foregoing descriptions of the embodiments of this application sometimes combine multiple features into a single embodiment, figure, or description thereof. However, this disclosure method does not mean that the subject matter of this application requires more features than those recited in the claims. In fact, an embodiment may have fewer features than all of the features of a single embodiment disclosed above.

[0212] In some embodiments, numbers are used to describe the quantity of components and attributes. It should be understood that such numbers used in the description of the embodiments are modified by the modifiers "about", "approximately" or "substantially" in some examples. Unless otherwise stated, "about", "approximately" or "substantially" indicate that the numbers are allowed to vary by ±20%. Accordingly, in some embodiments, the numerical parameters used in the description and claims are approximate values, which may change according to the required features of individual embodiments. In some embodiments, the numerical parameters should take into account the specified significant digits and adopt the general method of retaining digits. Although the numerical domains and parameters used to confirm the breadth of their range in some embodiments of the present application are approximate values, in specific embodiments, the settings of such numerical values ​​are as accurate as possible within the feasible range.

[0213] Each patent, patent application, patent application publication, and other materials, such as articles, books, specifications, publications, and documents, cited in this application is hereby incorporated by reference in its entirety, except for any application history that is inconsistent with or conflicts with this application, and excluding any document (currently or subsequently appended to this application) that limits the broadest scope of the claims of this application. It should be noted that if the descriptions, definitions, and / or terminology used in the accompanying materials are inconsistent with or conflict with the content of this application, the descriptions, definitions, and / or terminology used in this application will control.

[0214] The above is a detailed introduction to a thin film capacitor for human tumor treatment and its preparation method, tumor treatment electrode patch, and tumor treatment system provided in the embodiments of the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A film capacitor for human tumor treatment, wherein: include: a first electrode layer and a second electrode layer; a dielectric layer, the dielectric layer being located between the first electrode layer and the second electrode layer; a first defect repairing layer, wherein the first defect repairing layer is located between the second electrode layer and the dielectric layer; The first defect repairing layer is conductive, one side of the first defect repairing layer is tightly combined with the dielectric layer, and the other side of the first defect repairing layer is directly or indirectly in electrical contact with the second electrode layer.

2. The film capacitor according to claim 1, wherein: The tensile index of the second electrode layer is greater than the tensile index of the first defect repairing layer.

3. The film capacitor according to claim 2, wherein: The thickness of the second electrode layer is greater than the thickness of the first defect repairing layer.

4. The film capacitor according to claim 1, wherein: A side of the dielectric layer facing away from the first electrode layer has a first roughness, and a side of the first defect repairing layer facing away from the dielectric layer has a second roughness; Wherein, the second roughness is less than or equal to the first roughness.

5. The film capacitor according to claim 1, wherein: The first defect repairing layer is a metal layer.

6. The film capacitor according to claim 1, wherein: The first defect repairing layer includes multiple sub-metal layers.

7. The film capacitor according to claim 6, wherein: The first defect repairing layer includes an overlapping aluminum metal layer and a zinc metal layer; or The first defect repairing layer includes an overlapping aluminum metal layer and a gold metal layer; or The first defect repairing layer includes an overlapping aluminum metal layer and a titanium metal layer.

8. The film capacitor according to claim 1, wherein: Also comprising a second defect repairing layer, the second defect repairing layer is located between the first electrode layer and the dielectric layer; The second defect repairing layer is conductive, one side of the second defect repairing layer is tightly bonded to the surface of the dielectric layer, and the other side of the second defect repairing layer is directly or indirectly electrically contacted with the first electrode layer.

9. The film capacitor according to claim 8, wherein: The tensile index of the first electrode layer is greater than the tensile index of the second defect repairing layer.

10. The film capacitor according to claim 1, wherein: The dielectric layer includes a first insulating layer and a second insulating layer that are closely combined with each other; The first defect repairing layer is tightly bonded to a side of the second insulating layer facing away from the first insulating layer, and the insulating strength of the second insulating layer is greater than the insulating strength of the first insulating layer.

11. The film capacitor according to claim 1, wherein: The thickness of the first defect repairing layer is 10 nm to 1000 nm; and the tolerance value of the first defect repairing layer is ±10% of the thickness value thereof.

12. The film capacitor according to claim 1, wherein: The thickness of the first defect repairing layer is 10 nm to 800 nm.

13. The film capacitor according to claim 1, wherein: The thickness of the first defect repairing layer is 50 nm to 450 nm.

14. The film capacitor according to claim 1, wherein: The thickness of the dielectric layer is 1um to 100um; preferably, the thickness of the dielectric layer is 1um to 10um; preferably, the thickness of the dielectric layer is 2um to 8um.

15. The film capacitor according to claim 6, wherein: The total thickness of the sub-metal layer in the first defect repairing layer having an electrical conductivity better than or equal to that of metal aluminum is 10 nm to 400 nm; Preferably, the total thickness of the sub-metal layers in the first defect repairing layer whose electrical conductivity is better than or equal to that of metal aluminum is 50 nm-400 nm.

16. A method for preparing a film capacitor for treating human tumors, wherein: include: Providing a first electrode layer; forming a dielectric layer on the first electrode layer; forming a first defect repairing layer on a side of the dielectric layer away from the first electrode layer; forming a second electrode layer on a side of the dielectric layer away from the first defect repairing layer; The first defect repairing layer is conductive, one side of the first defect repairing layer is tightly bonded to the surface of the dielectric layer, and the other side of the first defect repairing layer is directly or indirectly electrically contacted with the second electrode layer.

17. A tumor treatment electrode patch, wherein: Comprising the film capacitor according to any one of claims 1 to 15.

18. A tumor treatment system, wherein: Comprising the tumor treatment electrode patch as described in claim 17.

Citation Information

Patent Citations

  • Thin-film capacitor

    CN110767450A

  • Formation of embedded capacitor polar plate sing thin dielectric

    CN1374666A

  • Film capacitors with improved dielectric properties

    CN1967751A

  • Thin film capacitor

    US20190096588A1

  • Thin film capacitor, circuit board incorporating the same, and thin film capacitor manufacturing method

    US20210257164A1