Quantum dot-containing composition, wavelength conversion member, and method for producing quantum dot-containing composition
The quantum dot-containing composition with a core-shell structure and siloxane bond surface coating addresses stability and dispersion issues, enhancing quantum yield and enabling stable display performance without barrier films, thus improving the efficiency and cost-effectiveness of quantum dot-based displays.
Patent Information
- Application Number
- PCT/JP2024/017800
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-28
AI Technical Summary
Current quantum dot-containing wavelength conversion materials for displays face challenges in stability, particularly in high temperature and high humidity environments, leading to reduced quantum yield and the need for barrier films that increase cost and thickness, while also facing issues with dispersion and patterning in color filters.
A quantum dot-containing composition with a core-shell type structure and a surface coating layer having siloxane bonds, incorporating reactive substituents like vinyl, acrylic, or methacryl groups, is developed, along with a method involving surface treatment with a ligand having a thiol group to form a ZnS shell and improve dispersibility and stability without using barrier films.
The solution enhances the stability and quantum yield of quantum dots, maintaining their characteristics and enabling reliable performance in displays without the need for barrier films, while also improving dispersibility and reducing material loss and complexity in the manufacturing process.
Smart Images

Figure JP2024017800_28112024_PF_FP_ABST
Abstract
Description
Quantum dot-containing composition, wavelength conversion member, and method for producing quantum dot-containing composition
[0001] The present invention relates to a quantum dot-containing composition, a wavelength conversion member, and a method for producing a quantum dot-containing composition.
[0002] In single-crystal semiconductor nanoparticles, when the crystal size is equal to or smaller than the Bohr radius of the exciton, a strong quantum confinement effect occurs, resulting in discrete energy levels. The energy levels depend on the crystal size, and the optical absorption and emission wavelengths can be adjusted by the crystal size.
[0003] Furthermore, the quantum confinement effect makes the light emission from exciton recombination in single-crystal semiconductor nanoparticles highly efficient, and because this light emission is essentially an emission line, if a uniform particle size distribution can be achieved, it will be possible to emit light with high brightness and narrow bandwidth, which has attracted attention. The phenomenon caused by the strong quantum confinement effect in such nanoparticles is called the quantum size effect, and semiconductor nanocrystals that utilize this property are being investigated as quantum dots (QDs) for wide application.
[0004] One application of quantum dots is being considered for use as phosphor materials for displays. If they can emit light with narrow bandwidth and high efficiency, it will be possible to express colors that could not be reproduced with existing technology, and so quantum dots are attracting attention as a next-generation display material.
[0005] One display in which quantum dots are currently being used is quantum dot liquid crystal displays, which are already being commercialized. Attempts are being made to convert the color of light irradiated from a white or blue LED backlight into green or red by passing it through a quantum dot-containing wavelength conversion material.
[0006] The surface of quantum dots is active, and the quantum yield gradually decreases due to moisture and oxygen in the atmosphere. Therefore, improving the stability of quantum dot-containing wavelength conversion materials is an essential item to consider.
[0007] Various studies have been conducted to stabilize wavelength conversion materials containing quantum dots. One example is gas barrier sealing. Stability has been improved by forming an inner layer in which quantum dots are dispersed in an amphiphilic polymer or a compatible polymer, and then dispersing them in another resin layer with low gas permeability.
[0008] Patent Document 1 discloses a method in which polymer beads are formed by dispersing QDs in a hydrophobic resin layer, and the polymer beads are surface-modified so that they can be dispersed in a hydrophilic polymer.
[0009] Hydrophilic polymers tend to have better gas barrier properties than hydrophobic polymers, so QDs are dispersed in these bilayer or multilayer structures. However, the gas barrier properties are insufficient for use in high-temperature, high-humidity environments such as those used in liquid crystal display units. Therefore, the QD film is sandwiched between gas barrier films to eliminate the effects of oxygen and water vapor.
[0010] Various studies have been conducted on the method of producing polymer beads. Patent Document 2 discloses a method in which QD-containing polymer beads are produced from polysiloxane having an amino group and a polymerizable functional group, and then a polymer having another polymerizable functional group is mixed with the resulting mixture, emulsified, and then cured.
[0011] This method can improve stability by increasing the concentration of QDs contained in the polymer beads by increasing the adhesion between the QDs and the polymer, which incorporates ligands that coordinate to the QD surface. However, this method still does not provide sufficient stability, so QDs are typically packaged by sandwiching them between barrier films.
[0012] US Patent No. 9708532 JP 2016-111292 A JP 2019-536653 A US Patent Application Publication No. 2019 / 0322926
[0013] However, using a barrier film not only increases costs, but also inevitably increases thickness. Currently, there is a demand for thinner LCD displays, which requires reducing the thickness of wavelength conversion materials, so improved stability without the need for a barrier film is required. Furthermore, when considering color filter applications, patterning is required, making it impractical to provide a protective layer such as a barrier film, and the stability of the quantum dots themselves is essential.
[0014] Patent Document 3 has been published as a study on improving heat resistance and moisture resistance without using a barrier film. In this method, a multilayer resin composition using the polymer bead structure of Patent Document 1 is further subjected to a silazane coating treatment, thereby improving stability. However, this method has the problem of a decrease in quantum yield when the silazane coating is photocured by irradiation with short ultraviolet light (170 nm).
[0015] Another attempt is disclosed in Patent Document 4. In this method, quantum dots are coordinated with ligands, reactive substituents such as vinyl groups or methacrylic groups are introduced into the ligands, and then a Si—H-containing silicone resin and a curing agent are mixed together, and the resulting mixture is spin-coated and heated to harden, producing a film with improved heat resistance and moisture resistance.
[0016] However, the Si-H-containing silicone resin used and quantum dots have low compatibility, and attempting to disperse them at high concentrations results in aggregation. Therefore, compatibility must be improved by ligand treatment, but if the balance between hydrophobic and hydrophilic groups changes when the ligand is coordinated, aggregation is likely to occur, resulting in a decrease in quantum yield.
[0017] Furthermore, when applying quantum dots to color filters, it is important to create a surface condition suitable for the patterning method. Currently, color filters are produced using a photolithography method in which a photosensitive resin composition containing a pigment is applied to a glass substrate, the solvent is dried, the composition is exposed to UV light through a mask, and the uncured portions are removed by alkaline development to form a color pattern. This process is repeated to form blue, red, and green patterns.
[0018] Photolithography has many problems, such as the uncured portions being wasted, resulting in a large amount of raw material loss, and the process being complicated and requiring expensive equipment. For this reason, inkjet methods have also been considered in recent years.
[0019] The inkjet method is cost-competitive because there is no loss of raw materials and it is possible to produce larger and larger-area prints without introducing expensive equipment. However, the technology to make fine nozzles is difficult, and as the nozzles get smaller, problems arise such as clogging and unstable ejection. Therefore, both photolithography, which has a proven track record, and cost-competitive inkjet printing are being considered for miniaturization.
[0020] However, the problem with both photolithography and inkjet printing is the creation of a resin composition containing quantum dots at high concentrations and high dispersions. Dispersing quantum dots at high concentrations can lead to problems such as slower curing and altered properties of the cured resin.
[0021] The present invention has been made to solve the above problems, and aims to provide a quantum dot-containing composition and a wavelength conversion member that can improve stability while maintaining the properties of quantum dots. Another aim of the present invention is to provide a method for producing a quantum dot-containing composition that can improve stability while maintaining the properties of quantum dots.
[0022] The present invention has been made to achieve the above-mentioned object, and provides a quantum dot-containing composition containing quantum dots that emit fluorescence when exposed to excitation light, the quantum dot-containing composition being a mixture of quantum dots and a polymerizable polymer composition, the quantum dots having a core-shell structure with an outermost shell made of ZnS, the surfaces of the quantum dots containing a surface coating layer having siloxane bonds, and the quantum dots having a fluorescence intensity of 1000 to 1200 cm by Fourier transform infrared spectroscopy. -1 The peak intensity present in the range of 2800 to 3000 cm -1 The present invention provides a quantum dot-containing composition, characterized in that the peak intensity is greater than that present in
[0023] Such a quantum dot-containing composition can improve the stability while maintaining the properties of the quantum dots.
[0024] In this case, the surface coating layer may have one or more reactive substituents selected from the group consisting of a vinyl group, an acrylic group, a methacrylic group, a hydroxyl group, a phenolic hydroxyl group, and an epoxy group.
[0025] This allows the introduction of a substituent group that can be polymerized with the polymerizable polymer into the surface coating layer, thereby improving the stability while maintaining the properties of the quantum dots.
[0026] In this case, the polymer contained in the polymerizable polymer composition may contain, as a substituent polymerizable with the reactive substituent, one or more of a vinyl group, an acrylic group, a methacrylic group, a hydroxyl group, a phenolic hydroxyl group, and an epoxy group.
[0027] This allows the reactive substituent to be polymerized with the polymer, and not only can it suppress poor curing during polymerization of the polymer, but it can also improve dispersibility.
[0028] The present invention also provides a wavelength conversion member that is a cured product of the quantum dot-containing composition described above.
[0029] Such a wavelength conversion member is a cured product of a quantum dot-containing composition that can improve stability while maintaining the properties of the quantum dots, and therefore the wavelength conversion member can also improve stability while maintaining the properties of the quantum dots.
[0030] Furthermore, the present invention provides a method for producing a quantum dot-containing composition containing quantum dots that emit fluorescence when exposed to excitation light, the method comprising: a surface treatment step of heating and mixing a solution in which quantum dots having ZnS formed on their outermost shells are dispersed, a ligand having a substituent capable of forming a siloxane bond and a thiol group, and a solution containing a zinc precursor and a sulfur precursor, to coordinate the ligand while forming additional ZnS on the outermost surface of the quantum dots; a surface coating layer formation step, after the surface treatment step, of reacting the substituent capable of forming a siloxane bond with a compound having a reactive substituent capable of forming a siloxane bond to form a surface coating layer having a siloxane bond; and a mixing step, after the surface coating layer formation step, of adding and mixing a polymerizable polymer composition containing the reactive substituent and a polymerizable substituent.
[0031] According to this manufacturing method, by reacting a ligand containing a substituent capable of forming a siloxane bond while forming a ZnS shell, a surface coating layer is formed to inactivate the quantum dots while suppressing a decrease in the luminescence efficiency of the quantum dots due to surface treatment, thereby improving stability. Furthermore, by arranging a substituent polymerizable with the polymerizable polymer composition, not only can poor curing during polymer polymerization be suppressed but also dispersibility can be improved.
[0032] As described above, the quantum dot-containing composition and wavelength conversion member of the present invention can improve the stability while maintaining the properties of the quantum dots. Furthermore, the method for producing the quantum dot-containing composition of the present invention can improve the stability while maintaining the properties of the quantum dots.
[0033] 1 shows a Fourier transform infrared spectroscopy (FT-IR) spectrum of the quantum dots of Example 1. 2 shows an FT-IR spectrum of the quantum dots of Comparative Example 1. 3 shows a flow diagram of a method for producing a quantum dot-containing composition of the present invention.
[0034] The present invention will be described in detail below, but the present invention is not limited thereto.
[0035] As described above, there has been a demand for a quantum dot-containing composition that can improve stability while maintaining the properties of the quantum dots.
[0036] As a result of intensive research into the above-mentioned problems, the present inventors have discovered a quantum dot-containing composition containing quantum dots that emit fluorescence when exposed to excitation light, the quantum dot-containing composition being a mixture of quantum dots and a polymerizable polymer composition, the quantum dots having a core-shell structure with an outermost shell made of ZnS, the surfaces of the quantum dots containing a surface coating layer having siloxane bonds, and the quantum dots having a wavelength of 1000 to 1200 cm by Fourier transform infrared spectroscopy. -1 The peak intensity present in the range of 2800 to 3000 cm -1 The present inventors have found that a quantum dot-containing composition characterized by a peak intensity greater than that present in the quantum dot-containing composition can improve the stability while maintaining the properties of the quantum dots, and have completed the present invention.
[0037] As described above, there has also been a demand for a wavelength conversion member that can improve stability while maintaining the properties of quantum dots.
[0038] As a result of extensive research into the above-mentioned problems, the inventors have discovered that a wavelength conversion member characterized by being a cured product of the quantum dot-containing composition described above can improve stability while maintaining the properties of quantum dots, and have thus completed the present invention.
[0039] Furthermore, as described above, there has been a need for a method for producing a quantum dot-containing composition that can improve stability while maintaining the properties of the quantum dots.
[0040] As a result of intensive research into the above-mentioned problems, the present inventors have found that a method for producing a quantum dot-containing composition containing quantum dots that emit fluorescence when exposed to excitation light, the method comprising: a surface treatment step of heating and mixing a solution in which quantum dots having ZnS formed on the outermost shell are dispersed, a ligand having a substituent capable of forming a siloxane bond and a thiol group, and a solution containing a zinc precursor and a sulfur precursor, to form additional ZnS on the outermost surface of the quantum dots while coordinating the ligand; a surface coating layer formation step of reacting the substituent capable of forming a siloxane bond with a compound having a reactive substituent capable of forming a siloxane bond to form a surface coating layer having a siloxane bond; and a mixing step of adding and mixing a polymerizable polymer composition containing the reactive substituent and a polymerizable substituent after the surface coating layer formation step, thereby improving the stability of the quantum dots while maintaining their properties, and have completed the present invention.
[0041] The present invention will be described in detail below, but is not limited thereto. The quantum dot-containing composition of the present invention is a composition containing quantum dots that emit fluorescence when exposed to excitation light, and a surface coating layer containing siloxane bonds formed on the surface of the quantum dots. More specifically, the quantum dot-containing composition is a mixture of quantum dots and a polymerizable polymer composition. It may also be a composite particle or a mixture thereof, in which a substituent capable of condensation polymerization with the polymerizable polymer composition is introduced into the surface coating layer.
[0042] (Quantum dots) The external shape of quantum dots in the present invention is not particularly limited, and any shape can be used. Quantum dots are mainly nanoparticles with a particle diameter of 10 nm or less, but they may also be nanowires, nanorods, nanotubes, nanocubes, etc., and any shape can be applied.
[0043] The quantum dots used in the present invention can be made of any suitable material, for example, a semiconductor material selected from the group consisting of II-VI group, III-V group, IV group, IV-VI group, I-III-VI group, II-IV-V group, mixed crystals or alloys thereof, or compounds having a perovskite structure, as long as they emit fluorescence when exposed to excitation light.
[0044] Specifically, ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, G aSb, InN, InP, InAs, InSb, Si, Ge, Sn, Pb, PbS, PbSe, PbTe, SnS, SnSe, SnTe, AgGaS 2 , AgInS 2 , AgGaSe 2 , AgInSe 2 , CuGaS 2 , CuGaSe 2 , CuInS 2 , ZnSiP 2 , ZnGeP 2 , CdSiP 2 , CdGeP 2 , CsPbCl 3 , CsPbBr 3 , CsPbI 3 , CsSnCl 3 , CsSnBr 3 , CsSnI 3 Examples include, but are not limited to, compounds containing:
[0045] The quantum dots used in the present invention have a core-shell structure. The shell material that can form the core-shell structure is not particularly limited as long as the outermost shell is ZnS, but a material that has a large band gap and low lattice mismatch with respect to the core material is preferred, and a material that has a smaller band gap than the ZnS of the outermost shell is also preferred, and any combination can be used depending on the core material and outermost shell material.
[0046] Specific shell materials include ZnO, ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, InSb, BeS, BeSe, BeTe, MgS, MgSe, MgTe, PbS, PbSe, PbTe, SnS, SnSe, SnTe, CuF, CuCl, CuBr, and CuI. The above materials may be selected as a single or multiple mixed crystals, but are not limited thereto.
[0047] There are various methods for producing quantum dots, such as a liquid phase method or a gas phase method, and the present invention is not particularly limited thereto. However, from the viewpoint of exhibiting high fluorescence emission efficiency, it is preferable to use semiconductor nanoparticles obtained by a hot soap method or a hot injection method, in which precursor species are reacted at high temperature in a non-polar solvent with a high boiling point. It is also preferable that organic ligands are coordinated to the surface of the quantum dots in order to impart dispersibility in the non-polar solvent and reduce surface defects.
[0048] From the viewpoint of dispersibility, the ligand preferably contains an aliphatic hydrocarbon. Examples of such ligands include oleic acid, stearic acid, palmitic acid, myristic acid, lauric acid, decanoic acid, octanoic acid, oleylamine, stearyl (octadecyl)amine, dodecyl (lauryl)amine, decylamine, octylamine, octadecanethiol, hexadecanethiol, tetradecanethiol, dodecanethiol, decanethiol, octanethiol, trioctylphosphine, trioctylphosphine oxide, triphenylphosphine, triphenylphosphine oxide, tributylphosphine, and tributylphosphine oxide. These may be used alone or in combination.
[0049] (Ligand having a thiol group) In addition to the above-mentioned ligand, it is desirable that the quantum dot of the present invention has a ligand having a substituent capable of forming a siloxane bond coordinated thereto. The ligand having a substituent capable of forming a siloxane bond preferably has a substituent that interacts with or is adsorbed to the quantum dot surface.
[0050] Substituents that interact or react with the quantum dot surface include amino groups, carboxy groups, mercapto groups, phosphine groups, phosphine oxide groups, sulfonyl groups, and quaternary ammonium salts. The outermost shell is made of ZnS, and among these, thiol groups are preferred from the viewpoint of coordination ability and reactivity.
[0051] The quantum dot-containing composition of the present invention also contains a surface coating layer having a siloxane bond. For example, the quantum dot surface is coated with a polymer such as polysiloxane. Therefore, it is desirable that the ligand having a substituent capable of coordinating to the quantum dot surface has a substituent capable of forming a siloxane bond.
[0052] Examples of the ligand having a substituent capable of forming a siloxane bond include compounds containing alkoxysilanes such as trimethoxysilyl, triethoxysilyl, dimethoxymethylsilyl, diethoxymethylsilyl, dimethylmethoxysilyl, and ethoxydimethylsilyl groups; compounds having a silazane bond; compounds having an Si—OH bond; compounds having an Si—X (X: halogen) bond; and carboxylic acids. However, it is preferable to use a ligand containing alkoxysilane, silazane, or Si—OH because the reaction can proceed under mild conditions that do not generate acid as a by-product of the reaction.
[0053] (Surface coating layer) The surface coating layer of the quantum dot-containing composition of the present invention has a siloxane bond. More specifically, it is desirable that the quantum dot surface is coated with a polymer using polysiloxane. Therefore, it is desirable to form a quantum dot surface polymer coating layer containing polysiloxane by reacting a substituent capable of forming a siloxane bond contained in a ligand having a thiol group capable of coordinating with the quantum dot with a compound having a reactive substituent capable of forming a siloxane bond.
[0054] The surface coating layer of the present invention preferably has at least one reactive substituent polymerizable with a polymer contained in the polymerizable polymer composition described below. The substituent polymerizable with the polymer is preferably contained in the surface coating layer by forming a covalent bond.
[0055] By forming a covalent bond, the substituent that can polymerize with the polymer is less likely to be detached during subsequent purification procedures, compared to when an aggregate is formed with the surface-coated quantum dots or when the substituent is contained so as to be coordinated to the surface of the quantum dots or the surface coating layer.
[0056] Furthermore, examples of reactive substituents that can polymerize with a polymer include vinyl groups, acrylic groups, methacrylic groups, hydroxyl groups, phenolic hydroxyl groups, epoxy groups, sulfonyl groups, carboxyl groups, and thiol groups. However, groups that are not too acidic and do not easily coordinate with quantum dots are preferred, as this ensures that aggregation can be suppressed. Specifically, vinyl groups, acrylic groups, methacrylic groups, hydroxyl groups, phenolic hydroxyl groups, and epoxy groups are preferred.
[0057] (FT-IR Spectrum) As shown in FIG. 1, the surface-coated quantum dots exhibited a peak intensity of 1000 to 1200 cm by FT-IR. -1 The peak intensity present in the range of 2800 to 3000 cm -1 The peak intensity is greater than that present in
[0058] As shown in Figure 2, 1000 to 1200 cm -1 The peak intensity present in the range of 2800 to 3000 cm -1 If the intensity is lower than the peak intensity present in the figure, the quantum dot characteristics such as the internal quantum efficiency may be reduced, and the stability may be poor.
[0059] (Polymerizable polymer composition) The quantum dot-containing composition of the present invention is a mixture of quantum dots and a polymerizable polymer composition. The polymerizable polymer composition comprises, for example, a polymer that is a base polymer and a polymerization initiator, and may also contain other ingredients such as an organic solvent, a polymerizable crosslinking agent, a photoacid generator, an antioxidant, and a light scattering agent.
[0060] Suitable polymers that can be used include polymers derived from acrylic acid, methacrylic acid, acrylic acid esters, and methacrylic acid esters, copolymers combining multiple polymers, polymers having glycidyl (meth)acrylate as a repeating unit, and polymers containing a siloxane skeleton, a urethane skeleton, a silphenylene skeleton, a norbornene skeleton, a fluorene skeleton, and an isocyanurate skeleton, and the polymer to be used may be selected appropriately depending on the application.
[0061] Examples thereof include acrylic resins, alkyd resins, melamine resins, epoxy resins, silicone resins, polyvinyl alcohol, polyvinylpyrrolidone, polyamides, polyamide-imides, polyimide precursors such as polyimides, and esterification products thereof, and reaction products of tetracarboxylic dianhydrides and diamines.
[0062] In addition, it is preferable that a polymerizable substituent capable of polymerizing with the reactive substituent is introduced into these polymers, and curing is possible by using them in combination with a polymerization initiator. Examples of radically polymerizable substituents include vinyl groups, acrylic groups, methacrylic groups, thiol groups, etc., and examples of cationically polymerizable substituents include hydroxyl groups, phenolic hydroxyl groups, epoxy groups, etc., and those containing one or more of any of these are preferred. Examples of other groups include glycidyl groups, oxetanyl groups, isocyanate groups, etc., and any of these can be suitably used. In addition, a carboxyl group may be introduced to impart alkaline developability.
[0063] The quantum dot-containing composition of the present invention also preferably contains a polymerization initiator. The polymerization initiator may be a thermal or photopolymerization initiator, either of which can be suitably used depending on the base polymer. Examples of photoradical polymerization initiators include those in the Irgacure (registered trademark) series commercially available from BASF, such as Irgacure 290, Irgacure 651, Irgacure 754, Irgacure 184, Irgacure 2959, Irgacure 907, Irgacure 369, Irgacure 379, Irgacure 819, and Irgacure 1173. Examples of the Darocure (registered trademark) series include TPO and Darocure 1173. Other known thermal radical polymerization initiators and photocationic polymerization initiators may also be included.
[0064] The content of the polymerization initiator is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, per 100 parts by mass of the polymer to be added.
[0065] The quantum dot-containing composition of the present invention may contain a solvent to improve its applicability. From the viewpoint of compatibility with quantum dots, organic solvents are preferred as the solvent, such as ketones, alkylene glycol ethers, alcohols, and aromatic compounds. From the ketone group, acetone, methyl ethyl ketone, cyclohexanone, etc., and from the alkylene glycol ether group, methyl cellosolve (ethylene glycol monomethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, ethylene glycol monopropyl ether, ethylene glycol monohexyl ether, ethylene glycol dimethyl ether, diethylene glycol ethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, and diethylene glycol methyl ether acetate are preferred. Suitable solvents that can be used include diethylene glycol ethyl ether acetate, diethylene glycol propyl ether acetate, diethylene glycol isopropyl ether acetate, diethylene glycol butyl ether acetate, diethylene glycol tert-butyl ether acetate, triethylene glycol methyl ether acetate, triethylene glycol ethyl ether acetate, triethylene glycol propyl ether acetate, triethylene glycol isopropyl ether acetate, triethylene glycol butyl ether acetate, and triethylene glycol tert-butyl ether acetate; methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butyl alcohol, and 3-methyl-3-methoxybutanol from the alcohol group; and benzene, toluene, and xylene from the aromatic solvent group.
[0066] Furthermore, the quantum dot-containing composition of the present invention may also contain a polymerizable crosslinking agent, a photoacid generator, an antioxidant, a light scattering agent, etc., and there are no particular limitations on these as long as they do not affect the coatability of the quantum dot-containing composition.
[0067] (Method for Producing Quantum Dot-Containing Composition) The quantum dot-containing composition of the present invention can be produced by the following method, exemplified in Fig. 3. First, quantum dots that have ZnS formed in the outermost shell and emit fluorescence when exposed to excitation light are produced, or if they have already been produced, the produced quantum dots are prepared and dispersed in a solution (S0 in Fig. 3). Examples of methods for producing quantum dots include the liquid phase method and gas phase method already mentioned.
[0068] Next, the solution in which the quantum dots are dispersed, a ligand having a thiol group and a substituent capable of forming a siloxane bond, and a solution containing a zinc precursor and a sulfur precursor are heated and mixed, and the ligand is coordinated while forming additional ZnS on the outermost surface of the quantum dots (S1 in Figure 3, surface treatment step).
[0069] The reason for coordinating the ligand while forming ZnS in this way is as follows. When coordinating a ligand having a substituent capable of forming a siloxane bond and a thiol group, quantum dots to which a ligand containing a long-chain hydrocarbon is coordinated are generally dispersed in a hydrophobic solvent, and then mixed with a ligand having a substituent capable of forming a siloxane bond and a thiol group that can be coordinated to the quantum dot surface to perform ligand exchange. The conditions for the ligand exchange reaction, such as the amount added, heating temperature, time, and light irradiation, are appropriately changed depending on the type of ligand. However, it has been found that this method results in a certain amount of decrease in quantum yield.
[0070] Therefore, by mixing a ligand into the zinc precursor and sulfur precursor solution when forming the ZnS shell, it is possible to introduce the ligand without reducing the quantum yield, and it is also possible to introduce more ligands than by ligand exchange.
[0071] Next, after the surface treatment step, a substituent capable of forming a siloxane bond is reacted with a compound having a reactive substituent capable of forming a siloxane bond to form a surface coating layer having a siloxane bond (S2 in FIG. 3, surface coating layer formation step).
[0072] Specifically, a reaction is carried out to form polysiloxane with quantum dots coordinated with thiols having substituents capable of forming siloxane bonds, which were introduced in the surface coating layer formation process, to form a surface coating layer containing siloxane bonds.
[0073] The sol-gel method is a common method for forming polysiloxane bonds, but because quantum dots are vulnerable to acidic conditions and moisture, a sol-gel method under basic conditions or a sol-gel method using a Lewis acid catalyst is preferred, and a non-hydrolytic sol-gel method using diphenylsilanediol, tetramethyldisiloxanediol, or the like, or a Lewis Acid Promoted Sol-Gel Reaction (LANHSG) using an alkoxysilane with a reactive substituent in the presence of a Lewis acid catalyst is even more preferred.
[0074] Furthermore, the surface coating layer of the present invention preferably has at least one substituent polymerizable with the polymer contained in the polymerizable polymer composition or a skeletal structure with a similar structure. The substituent polymerizable with the polymer or a compound with a similar skeletal structure is preferably contained in the surface coating layer by forming a covalent bond. There are no particular limitations on the method for forming the covalent bond. For example, a method in which a substituent capable of forming a siloxane bond is introduced into a substituent polymerizable with the polymer or a compound with a similar skeletal structure, and the resulting compound is added during the non-hydrolytic sol-gel reaction, thereby forming a covalent bond and incorporating the compound into the surface coating layer, or a method in which a substituent polymerizable with the polymer contained in the polymerizable polymer composition is introduced during the non-hydrolytic sol-gel reaction, and then the resulting compound is introduced into the surface coating layer by reacting with a polymer or a monomer, can be preferably used.
[0075] After the surface coating layer formation step, a polymerizable polymer composition containing a reactive substituent and a polymerizable substituent is added and mixed to obtain a quantum dot-containing composition (S3 in Figure 3, mixing step). Specifically, after forming the surface coating layer, unreacted materials are removed by purification, and the resulting mixture is mixed with the polymerizable polymer composition to produce a quantum dot-containing composition. Forming the surface coating layer improves compatibility with the polymerizable polymer composition, allowing the production of a quantum dot-containing composition in which the quantum dots are uniformly dispersed without aggregation.
[0076] (Wavelength conversion member having quantum dot-containing composition) The wavelength conversion member of the present invention is a resin composition that is a cured product of the quantum dot-containing composition produced by the above method. The form of the wavelength conversion member in the present invention is not particularly limited, but examples include a wavelength conversion film in which quantum dots are dispersed in a polymerizable polymer composition by processing into a sheet and then curing, and a wavelength conversion color filter patterned by inkjet or as a resist material.
[0077] The method for producing (manufacturing) the wavelength conversion member is not particularly limited. For example, the quantum dot-containing composition can be applied to a transparent film or substrate material such as PET or polyimide, cured, and laminated to obtain the wavelength conversion member.
[0078] The transparent film can be coated using a spraying method such as spray or inkjet, or by spin coating or bar coating.
[0079] The quantum dot-containing composition can be cured, for example, by heating a film coated with the quantum dot-containing composition at 60° C. for 2 hours, and then at 150° C. for 4 hours. Alternatively, the quantum dot-containing composition may be cured using a photopolymerization reaction, for example, using a UV LED irradiation device with a wavelength of 365 nm and an output of 4000 mW / cm. 2 The curing can be performed by irradiating the composition with light for 20 seconds, and the curing time is not particularly limited, but can be changed appropriately depending on the application.
[0080] Here, it is preferable that a substituent capable of polymerizing with the polymer in the quantum dot-containing composition is introduced into the surface coating layer, since this makes it possible to produce a wavelength conversion member that is highly reliable after curing and is free from aggregation and curing inhibition.
[0081] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to these. In these examples, core-shell quantum dots of InP / ZnSe / ZnS were used as the quantum dot material.
[0082] Example 1 (Quantum dot core synthesis process) 0.23 g (0.9 mmol) of palmitic acid, 0.088 g (0.3 mmol) of indium acetate, and 10 mL of 1-octadecene were added to a flask, heated to 100° C. under reduced pressure, and stirred to dissolve the raw materials while degassing for 1 hour.
[0083] Thereafter, nitrogen was purged into the flask, and 0.75 mL (0.15 mmol) of a solution prepared by mixing tristrimethylsilylphosphine with trioctylphosphine to adjust the concentration to 0.2 M was added, followed by heating to 300°C. The solution changed color from yellow to red, confirming the formation of core particles.
[0084] (Quantum dot shell layer synthesis step) Next, 2.85 g (4.5 mmol) of zinc stearate and 15 mL of 1-octadecene were added to another flask, and the mixture was heated at 100°C under reduced pressure and stirred. While dissolving, the mixture was degassed for 1 hour to prepare a 0.3 M zinc stearate octadecene solution. 3.0 mL (0.9 mmol) of this solution was added to the reaction solution after core synthesis, and the solution was cooled to 200°C.
[0085] Next, 0.474 g (6 mmol) of selenium and 4 mL of trioctylphosphine were added to another flask and dissolved by heating to 150°C to prepare a 1.5 M selenium trioctylphosphine solution. The reaction solution after the core synthesis step, which had been cooled to 200°C, was heated to 320°C over 30 minutes, while the selenium trioctylphosphine solution was added in 0.1 mL increments to a total of 0.6 mL (0.9 mmol), and the mixture was maintained at 320°C for 10 minutes and then cooled to room temperature. 0.44 g (2.2 mmol) of zinc acetate was added, and the mixture was dissolved by heating to 100°C under reduced pressure and stirring.
[0086] The flask was again purged with nitrogen and heated to 230°C, and 0.98 mL (4 mmol) of 1-dodecanethiol was added and maintained at this temperature for 1 hour. The resulting solution was cooled to room temperature to prepare a core-shell quantum dot-containing solution.
[0087] (Surface Treatment Step) (3-mercaptopropyl)triethoxysilane (Tokyo Chemical Industry Co., Ltd.) was used as a ligand having a substituent capable of forming a siloxane bond and a substituent capable of coordinating to the quantum dot surface. 0.45 g (2 mmol) of zinc bromide was dissolved in 2.4 mL of trioctylphosphine to prepare a zinc precursor solution.
[0088] Next, 0.064 g (2 mmol) of sulfur was dissolved in a mixed solution of 1.1 mL of 1-dodecanethiol and 1.1 mL of (3-mercaptopropyl)triethoxysilane to prepare a sulfur precursor solution. The core-shell quantum dot-containing solution obtained in the quantum dot shell layer synthesis step was heated to 210°C, and 1.25 mL of the zinc precursor solution and 1.3 mL of the sulfur precursor solution were added.
[0089] After the reaction was completed, ethanol was added to precipitate the reaction product, which was then centrifuged and the supernatant was removed.The same purification process was repeated, and the product was dispersed in toluene to produce a solution containing quantum dots coordinated with ligands having substituents capable of forming siloxane bonds.
[0090] (Surface coating layer formation process) Triethoxyvinylsilane (4.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution in which the quantum dots had been dispersed after the surface treatment process were added to a flask purged with nitrogen, and the mixture was heated and stirred for 24 hours at 65° C. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reaction product, the mixture was centrifuged, the supernatant was removed, and the product was dispersed in toluene.
[0091] (Fourier transform infrared spectroscopy) FT-IR measurement was carried out by dropping a dispersion liquid containing semiconductor nanoparticles (quantum dots) directly onto a detection section using a diamond ATR (Attenuated Total Reflection), thoroughly drying the dispersion, and then measuring the dispersion liquid at 400 to 4000 cm -1 The measurement was performed with 20 accumulations in the measurement range of 1000 to 1200 cm -1 The intensity of peak A present in the range of 2800 to 3000 cm -1It was confirmed that the intensity of peak B derived from the C—H bond present in the HCl solution was larger than that of peak B.
[0092] (Quantum dot-containing composition mixing step) The solution after the surface coating layer formation step dispersed in toluene and methacrylic modified silicone oil X-32-3817-3 (Shin-Etsu Chemical Co., Ltd.) were weighed and mixed so that the quantum dots were contained in a non-volatile content ratio of 20 wt %. After mixing, the solvent was removed using an evaporator to obtain a quantum dot-containing composition.
[0093] (Process for Producing Wavelength Conversion Member) A wavelength conversion member was produced using the obtained quantum dot-containing composition. The quantum dot-containing composition was degassed using a stirring degasser, poured onto a PET film, and formed into a thin film using a bar coater. Next, the formed thin film was irradiated with a UVLED irradiation device in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm. 2 The quantum dot-containing resin layer was photocured by irradiating it with light for 20 seconds, thereby producing a wavelength conversion member having a thickness of 50 μm.
[0094] (Measurement of Emission Wavelength, Emission Half Width, and Emission Efficiency) In the examples and comparative examples, the fluorescence emission characteristics of the quantum dots were evaluated by measuring the emission wavelength, fluorescence emission half width, and fluorescence emission efficiency (internal quantum efficiency) of the quantum dots at an excitation wavelength of 450 nm using a quantum efficiency measurement system (QE-2100) manufactured by Otsuka Electronics Co., Ltd.
[0095] (Reliability Test) The obtained wavelength conversion member was treated at 85° C. and 85% RH (relative humidity) for 250 hours, and the fluorescence emission efficiency of the treated wavelength conversion member was measured to evaluate its reliability.
[0096] Comparative Example 1 The same procedures as in Example 1 were carried out up to the quantum dot shell layer synthesis step, to obtain a solution in which quantum dots were dispersed.
[0097] (Surface Treatment Step) As a ligand having a substituent capable of forming a siloxane bond and a substituent capable of coordinating to the quantum dot surface, (3-mercaptopropyl)triethoxysilane (Tokyo Chemical Industry Co., Ltd.) (3.0 mmol) was added to the solution in which the quantum dots were dispersed, and the mixture was stirred for 24 hours. After the reaction was completed, ethanol was added to precipitate and purify the quantum dots in the same manner as in Example 1, and the quantum dots were then dispersed in toluene. In other words, unlike Example 1, no additional ZnS was formed in the surface treatment step.
[0098] (Surface coating layer formation process) Triethoxyvinylsilane (4.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution in which the quantum dots had been dispersed after the surface treatment process were added to a flask purged with nitrogen, and the mixture was heated and stirred for 24 hours at 65° C. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reaction product, the mixture was centrifuged, the supernatant was removed, and the product was dispersed in toluene.
[0099] (Fourier transform infrared spectroscopy) FT-IR measurement is carried out by dropping a dispersion liquid containing semiconductor nanoparticles (quantum dots) directly onto a detection section using a diamond ATR (Attenuated Total Reflection), drying it thoroughly, and then measuring the dispersion liquid at 400 to 4000 cm -1 The measurement was performed with 20 accumulations in the measurement range of 1000 to 1200 cm -1 The intensity of peak A present in the range of 2800 to 3000 cm -1 The intensity of peak B derived from the C—H bond present in the fluorine-containing compound was smaller than that of peak B.
[0100] (Quantum dot-containing composition mixing step) The solution after the surface coating layer formation step dispersed in toluene and methacrylic modified silicone oil X-32-3817-3 (Shin-Etsu Chemical Co., Ltd.) were weighed and mixed so that the quantum dots were contained in a non-volatile content ratio of 20 wt %. After mixing, the solvent was removed using an evaporator to obtain a quantum dot-containing composition.
[0101] (Process for Producing Wavelength Conversion Member) A wavelength conversion member was produced using the obtained quantum dot-containing composition. The quantum dot-containing composition was degassed using a stirring degasser, poured onto a PET film, and formed into a thin film using a bar coater. Next, the formed thin film was irradiated with a UVLED irradiation device in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm. 2 The quantum dot-containing resin layer was photocured by irradiating it with light of 1000 W for 20 seconds to prepare a wavelength conversion member having a thickness of 50 μm. Compared to Example 1, aggregates were observed in some cases, and the quantum yield was lower than that of Example 1.
[0102] Example 2 A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Example 1 up to the surface treatment step.
[0103] (Surface coating layer formation process) [(3-triethoxysilyl)propyl]succinic anhydride (Tokyo Chemical Industry Co., Ltd.) (4.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution in which the quantum dots had been dispersed after the surface treatment process were added to a flask that had been purged with nitrogen, and the mixture was heated and stirred for 24 hours at 65° C. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reaction product, which was then centrifuged, the supernatant was removed, and the product was dispersed in toluene.
[0104] (Quantum dot-containing composition mixing step) The solution after the surface coating layer formation step dispersed in toluene and acrylic resin RA-4101 (Negami Sangyo Co., Ltd.) were weighed out so that the quantum dots were contained in a nonvolatile content ratio of 20 wt%, and 5 parts by mass of photoradical generator Irgacure 1173 were added to 100 parts by mass of the acrylic resin nonvolatile content and mixed. After mixing, the toluene solvent was removed by distillation under reduced pressure to obtain a quantum dot-containing composition.
[0105] (Method for producing wavelength conversion member) A wavelength conversion member was produced using the obtained quantum dot-containing composition. The quantum dot-containing composition was vacuum degassed, and the quantum dot-containing composition with a solid content of 20% was poured into a PTFE-coated mold having a size of 20 cm x 10 cm and a thickness of 500 μm. The quantum dot-containing composition was heated on a hot plate at 120 ° C. for 1 hour to remove the solvent, thereby producing a quantum dot-containing resin layer. A portion of the layer was cut out and developed with a PGMEA solution to confirm that there was no remaining film.
[0106] Thereafter, the remaining quantum dot-containing resin layer was irradiated with a UV LED irradiator in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm 2 The coating was photocured by irradiating it with light of 100 .mu.m for 20 seconds to prepare a wavelength conversion member having a thickness of 100 .mu.m.
[0107] Comparative Example 2 A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Comparative Example 1 up to the surface treatment step, and a wavelength conversion member was prepared in the same manner as in Example 2 except for that.
[0108] Example 3 A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Examples 1 and 2 up to the surface treatment step.
[0109] (Surface coating layer formation process) Tris[3-(trimethoxysilyl)propyl]isocyanurate (1.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution in which the quantum dots had been dispersed after the surface treatment process were added to a flask that had been purged with nitrogen, and the mixture was heated and stirred for 24 hours at 65° C. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reaction product, the mixture was centrifuged, the supernatant was removed, and the product was dispersed in toluene.
[0110] (Quantum dot-containing composition mixing step) The solution after the surface coating layer formation step, in which an epoxy-containing silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., CAS No. 2253674-54-1) and toluene were dispersed, was weighed and mixed so that the quantum dots contained 20 wt% in terms of nonvolatile content. 2 parts by mass of photoacid generator CPI-310FG (manufactured by San-Apro) and 20 parts by mass of crosslinker THI-DE were weighed and mixed per 100 parts by mass of silicone resin nonvolatile content. After mixing, the toluene solvent was removed by distillation under reduced pressure to obtain a quantum dot-containing composition.
[0111] (Method for manufacturing wavelength conversion member) A wavelength conversion member was produced using the obtained quantum dot-containing composition. The quantum dot-containing composition was vacuum degassed, and the quantum dot-containing composition with a solid content of 20% was poured into a PTFE-coated mold having a size of 20 cm x 10 cm and a thickness of 500 μm. The quantum dot-containing composition was heated on a hot plate at 120 ° C. for 1 hour to remove the solvent, thereby producing a quantum dot-containing resin layer. A portion of the layer was cut out and developed with a PGMEA solution to confirm that there was no remaining film.
[0112] Thereafter, the remaining quantum dot-containing resin layer was irradiated with a UV LED irradiator in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm 2 The coating was photocured by irradiating it with light of 100 .mu.m for 20 seconds to prepare a wavelength conversion member having a thickness of 100 .mu.m.
[0113] Comparative Example 3 A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Comparative Example 1 up to the surface treatment step, and a wavelength conversion member was prepared in the same manner as in Example 3 except for that.
[0114] Example 4 A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Examples 1, 2 and 3 up to the surface treatment step.
[0115] (Surface coating layer formation process) Triethoxysilylpropyl methacrylate (4.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and a toluene solution in which the quantum dots after the surface treatment process were dispersed were added to a flask purged with nitrogen, and the mixture was heated and stirred for 24 hours at 65° C. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reactant, the mixture was centrifuged, the supernatant was removed, and the mixture was dispersed in toluene.
[0116] (Quantum dot-containing composition mixing step) A phenol-crosslinkable silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., CAS No. 916059-41-1) and the solution after the surface coating layer formation step, dispersed in toluene, were weighed and mixed so that the quantum dots contained 20 wt% in terms of nonvolatile content. 2 parts by mass of photoacid generator CPI-310FG (manufactured by San-Apro) and 20 parts by mass of crosslinker THI-DE were weighed and mixed per 100 parts by mass of silicone resin nonvolatile content. After mixing, the toluene solvent was removed by distillation under reduced pressure to obtain a quantum dot-containing composition.
[0117] (Method for producing wavelength conversion member) A wavelength conversion member was produced using the obtained quantum dot-containing composition. The quantum dot-containing composition was vacuum degassed, and the quantum dot-containing composition with a solid content of 20% was poured into a PTFE-coated mold having a size of 20 cm x 10 cm and a thickness of 500 μm. The quantum dot-containing composition was heated on a hot plate at 120 ° C. for 1 hour to remove the solvent, thereby producing a quantum dot-containing resin layer. A portion of the layer was cut out and developed with a PGMEA solution to confirm that there was no remaining film.
[0118] Thereafter, the remaining quantum dot-containing resin layer was irradiated with a UV LED irradiator in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm 2 The coating was photocured by irradiating it with light of 100 .mu.m for 20 seconds to prepare a wavelength conversion member having a thickness of 100 .mu.m.
[0119] Comparative Example 4 A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Comparative Example 1 up to the surface treatment step, and a wavelength conversion member was prepared in the same manner as in Example 4 except for the above.
[0120] The results of comparing Examples 1 to 4 with Comparative Examples 1 to 4 are shown in Table 1.
[0121]
[0122] The emission wavelength, fluorescence emission half-width, and internal quantum efficiency after quantum dot synthesis, after the surface treatment step, after the formation of the surface coating layer, after the mixing step (quantum dot-containing composition), and after curing of the quantum dot-containing composition (wavelength conversion member), the rate of decrease in internal quantum efficiency during reliability testing, and the presence or absence of aggregates in the wavelength conversion member are shown in Table 1. Table 1 also shows the results of FT-IR after the formation of the surface coating layer.
[0123] As can be seen from the results in Table 1, in all of the Examples, Peak A in the FT-IR after the formation of the surface coating layer was larger than Peak B, whereas in the Comparative Examples, Peak B was larger than Peak A, and the internal quantum efficiency was also inferior after the surface treatment step, after the formation of the surface coating layer, and after the preparation of the quantum dot-containing composition.
[0124] Furthermore, it can be seen that the internal quantum efficiency after fabrication of the wavelength conversion member in the comparative example is lower than that in the examples, and the emission wavelength is also significantly shifted to longer wavelengths, which is thought to be due to the formation of aggregates in the comparative example due to insufficient dispersion stability.
[0125] Furthermore, when the results of the reliability test (treated at 85°C and 85% RH for 250 hours) were compared between the Example and Comparative Example, the stability was comparable due to the formation of the surface coating layer, but the Comparative Example showed greater deterioration than the Example.
[0126] As described above, in the examples, in a reliability test at 85°C and 85% RH without a barrier film, the rate of decrease in internal quantum efficiency during 250 hours of treatment (rate of decrease in internal quantum efficiency after treatment) was able to be suppressed to within 10%, demonstrating that stabilization was possible.
[0127] As described above, it has been confirmed that the quantum dot-containing composition of the present invention exhibits high internal quantum efficiency and stability, and has good film quality after curing, and can be applied to quantum dot-containing resists and quantum dot-containing inkjet inks.
[0128] The present invention is not limited to the above-described embodiments, which are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that provides similar effects is included within the technical scope of the present invention.
Claims
1. A quantum dot-containing composition containing quantum dots that emit fluorescence when excited by excitation light, the quantum dot-containing composition being a mixture of quantum dots and a polymerizable polymer composition, the quantum dots having a core-shell structure with an outermost shell being ZnS, the quantum dot surfaces containing a surface coating layer having a siloxane bond, and the quantum dots having a fluorescence intensity of 1000 to 1200 cm by Fourier transform infrared spectroscopy. -1 The peak intensity present in the range of 2800 to 3000 cm -1 The quantum dot-containing composition is characterized in that the peak intensity is greater than that present in the 2. The quantum dot-containing composition according to claim 1, characterized in that the surface coating layer has one or more reactive substituents selected from the group consisting of vinyl groups, acrylic groups, methacrylic groups, hydroxyl groups, phenolic hydroxyl groups, and epoxy groups.
3. The quantum dot-containing composition according to claim 2, characterized in that the polymer contained in the polymerizable polymer composition contains one or more of the following substituents polymerizable with the reactive substituent: a vinyl group, an acrylic group, a methacrylic group, a hydroxyl group, a phenolic hydroxyl group, and an epoxy group.
4. A wavelength conversion member, comprising a cured product of the quantum dot-containing composition according to any one of claims 1 to 3.
5. A method for producing a quantum dot-containing composition containing quantum dots that emit fluorescence when excited by excitation light, comprising: a surface treatment step of heating and mixing a solution in which quantum dots having ZnS formed on their outermost shells are dispersed, a ligand having a substituent capable of forming a siloxane bond and a thiol group, and a solution containing a zinc precursor and a sulfur precursor, to form additional ZnS on the outermost surface of the quantum dots while coordinating the ligand; a surface coating layer formation step, after the surface treatment step, of reacting the substituent capable of forming a siloxane bond with a compound having a reactive substituent capable of forming a siloxane bond to form a surface coating layer having a siloxane bond; and a mixing step, after the surface coating layer formation step, of adding and mixing a polymerizable polymer composition containing the reactive substituent and a polymerizable substituent.
Citation Information
Patent Citations
Photosensitive resin composition, photosensitive resin coating, photosensitive dry film, pattern forming method, and light emitting element
JP2021089347A
Display device
JP2022027519A
Coated semiconductor nanoparticles and manufacturing method therefor
WO2021235152A1
Cited By
Quantum dot-containing composition, wavelength conversion member, and method for producing quantum dot-containing composition
WO2026216309A1