Liquid crystal composition for radio wave control element, and radio wave control element

The liquid crystal composition with high dichroic dye content and metasurface structure enhances refractive index anisotropy and response speed in radio wave control elements, addressing limitations in existing technologies for directing high-frequency radio waves.

WO2024242035A1PCT designated stage expired Publication Date: 2024-11-28FUJIFILM CORP

Patent Information

Application Number
PCT/JP2024/018254
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing radio wave control elements using liquid crystal media face limitations in refractive index anisotropy and thickness, making it difficult to efficiently direct high-frequency radio waves, such as millimeter waves, due to insufficient absorption characteristics and slow response times.

Method used

A liquid crystal composition with a high content of dichroic dyes, specifically designed to exhibit a nematic phase over a wide temperature range, is used to create a radio wave control element with a metasurface structure, allowing for adjustable refractive index anisotropy and reduced thickness, enabling efficient directionality and faster response times for radio waves.

Benefits of technology

The composition achieves significant refractive index anisotropy and rapid switching of radio wave directionality, improving the ability to control and redirect high-frequency radio waves, while minimizing noise interference from visible and infrared light.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018254_28112024_PF_FP_ABST
    Figure JP2024018254_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a liquid crystal composition for a radio wave control element whereby it is possible to obtain a material having large refractive index anisotropy with respect to radio waves; and a radio wave control element. The liquid crystal composition for a radio wave control element according to the present invention contains at least one dichroic dye. The total content of the dichroic dye is 30 mass% or more relative to the total mass of the liquid crystal composition for a radio wave control element, and the integrated absorbance Q represented by formula (1) in the wavelength range of 350-1000 nm in the absorption spectrum of a chloroform solution of the liquid crystal composition for a radio wave control element is 10,000 L⋅g-1⋅cm-1 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Liquid crystal composition for radio wave control element, radio wave control element

[0001] The present invention relates to a liquid crystal composition for a radio wave control element and a radio wave control element.

[0002] Radio waves, such as the high-frequency radio waves (millimeter waves and terahertz waves) required for high-capacity wireless communication, tend to propagate in a straight line. Therefore, there is a need for radio wave control elements that can bend the direction of radio waves in any direction. However, for example, a conventional reflector reflects radio waves in a fixed direction, and the reflection direction is a specular reflection with the angle of incidence and the angle of emission being equal. This significantly limits the range in which the direction of radio waves can be changed, making it difficult to deliver radio waves to the desired destination.

[0003] Patent Document 1 discloses a radio wave control element using a liquid crystal medium, and discloses a predetermined pleochroic compound as the liquid crystal medium.

[0004] Patent No. 7101619

[0005] On the other hand, for radio wave control elements using a liquid crystal medium, there has been a demand for thinner devices and shorter operating times. To obtain a radio wave control element exhibiting such characteristics, a liquid crystal medium with a larger refractive index anisotropy (Δn) is required. The present inventors evaluated the properties of the liquid crystal medium described in Patent Document 1 and found that it did not satisfy current requirements and that further improvement was necessary.

[0006] In view of the above circumstances, an object of the present invention is to provide a liquid crystal composition for a radio wave control element, which can be used as a material having a large refractive index anisotropy with respect to radio waves. Another object of the present invention is to provide a radio wave control element.

[0007] As a result of extensive research into solving the above problems, the present inventors have found that the problems can be solved by the following configuration.

[0008] (1) A liquid crystal composition for a radio wave control element containing at least one dichroic dye, wherein the total content of the dichroic dyes is 30% by mass or more relative to the total mass of the liquid crystal composition for a radio wave control element, and the integrated absorbance Q, expressed by the following formula (1), in the wavelength range of 350 to 1000 nm in the absorption spectrum of a chloroform solution of the liquid crystal composition for a radio wave control element is 10,000 L g -1 ・cm -1 (2) A liquid crystal composition for a radio wave control element according to (1), comprising two or more dichroic dyes. (3) A liquid crystal composition for a radio wave control element according to (1) or (2), wherein the dichroic dye is a compound represented by formula (X) described below. (4) A liquid crystal composition for a radio wave control element according to any one of (1) to (3), which exhibits a nematic phase over the entire temperature range of 10 to 50°C. (5) A liquid crystal composition for a radio wave control element according to any one of (1) to (4), which exhibits a nematic phase at any temperature between 50 and 150°C, and exhibits a glassy state or a smectic phase at any temperature below 50°C. (6) A radio wave control element having, in this order: a first electrode; a liquid crystal composition layer composed of the liquid crystal composition for a radio wave control element according to any one of (1) to (5); and a second electrode. (7) The radio wave control element according to (6), which has a metasurface structure formed by arranging a plurality of microstructures, the microstructures constituting at least one of the first electrode and the second electrode. (8) The radio wave control element according to (6) or (7), which further has a temperature adjusting member for adjusting the temperature of the liquid crystal composition layer. (9) The radio wave control element according to any one of (6) to (8), which has a layer between the first electrode and the second electrode whose refractive index does not change with voltage, or which has a gap between one of the first electrode and the second electrode and the liquid crystal composition layer. (10) The radio wave control element according to any one of (6) to (9), which further has a light-shielding layer that blocks at least a portion of light in the wavelength range of 250 to 1000 nm.

[0009] According to the present invention, it is possible to provide a liquid crystal composition for a radio wave control element, which can be used as a material having large refractive index anisotropy for radio waves. Also, according to the present invention, it is possible to provide a radio wave control element.

[0010] FIG. 1 is a diagram showing an example of a use of a radio wave control element. FIG. 2 is a diagram showing an example of a metasurface structure used in a radio wave control element. FIG. 3 is a diagram explaining the mechanism by which the emission direction of radio waves is changed in a radio wave control element. FIG. 4 is a diagram conceptually showing an example of a radio wave control element. FIG. 5 is a diagram conceptually showing an example of a liquid crystal orientation pattern in a radio wave control element. FIG. 6 is a diagram conceptually showing the relationship between the applied voltage and the amount of phase delay of radio waves. FIG. 7 is a diagram conceptually showing another example of a radio wave control element. FIG. 8 is a diagram conceptually showing another example of a radio wave control element. FIG. 9 is a diagram conceptually showing another example of a radio wave control element.

[0011] The present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0012] In this specification, parallel and perpendicular do not mean parallel and perpendicular in the strict sense, but rather mean a range of parallel ±5° and a range of perpendicular ±5°, respectively.

[0013] In addition, in this specification, for each component, a substance corresponding to the component may be used alone or in combination of two or more. Here, when two or more substances for each component are used in combination, the content of the component refers to the total content of the substances used in combination, unless otherwise specified.

[0014] In this specification, the bonding direction of a divalent group (e.g., -CO-O-, etc.) is not limited unless otherwise specified. For example, when Y is -CO-O- in a compound represented by the formula "X-Y-Z," the compound may be either "X-O-CO-Z" or "X-CO-O-Z."

[0015] The liquid crystal composition for radio wave control elements of the present invention (hereinafter also simply referred to as "the composition") contains at least one dichroic dye, the total content of the dichroic dyes being 30% by mass or more relative to the total mass of the liquid crystal composition for radio wave control elements, and the integrated absorbance Q, expressed by the following formula (1), in the wavelength range of 350 to 1000 nm in the absorption spectrum of a chloroform solution of the liquid crystal composition for radio wave control elements is 10000 L g -1 ・cm -1 The integrated absorbance Q, which is a characteristic feature of the present composition, will be described in detail below, and then the components contained in the present composition will be described in detail.

[0016] The integrated absorbance Q of the chloroform solution of this composition in the wavelength range of 350 to 1000 nm in the absorption spectrum, expressed by the following formula (1), is 10,000 L g -1 ・cm -1 The cumulative absorbance Q is 10,000 L g or more. -1 ・cm -1 Due to the above, the present composition can become a material with large refractive index anisotropy for radio waves. More specifically, as described below, the refractive index anisotropy for radio waves can be increased by orienting the dichroic dye in the present composition. Note that radio waves refer to electromagnetic waves with a frequency of 0.007 to 0.3 THz, which have a strong tendency to propagate in a straight line due to their high frequency. The integrated absorbance Q is an index that represents the light absorption characteristics of the present composition in the wavelength range of 350 to 1000 nm, and a high value of this integrated absorbance Q indicates excellent absorption characteristics. The refractive index of a substance is known to be related to the light absorption characteristics, and the present inventors have found that by adjusting the integrated absorbance Q of the present composition within a predetermined range, the refractive index anisotropy for radio waves can be significantly increased. In particular, they have found that by improving the absorption characteristics in the wavelength range of 350 to 1000 nm, the refractive index in the radio wave region can be increased, resulting in increased refractive index anisotropy for radio waves.

[0017] In particular, the refractive index anisotropy of the material obtained using this composition is larger (hereinafter, simply referred to as "the effect of the present invention is superior"), and the integrated absorbance Q is 11,000 L g -1 ・cm-1 Preferably, 12,000 L g or more. -1 ・cm -1 More preferably, 13,000 L g -1 ・cm -1 More preferably, 15,000 L g -1 ・cm -1 The upper limit of the integrated absorbance Q is not particularly limited, but is preferably 50,000 L g -1 ・cm -1 In most cases, it is 40,000 L / g. -1 ・cm -1 More often, the following cases are 30,000 L / g -1 ・cm -1 The following cases are even more common:

[0018] The integrated absorbance Q is calculated by the following formula (1).

[0019]

[0020] In equation (1), Q is the integrated absorbance (L g -1 ・cm -1 ), and D represents the mass concentration (g·L) of the liquid crystal composition for radio wave control elements in a chloroform solution. -1 ), L represents the optical path length (cm) of the cell used to measure the absorption spectrum, and Abs(λ) represents the absorbance at wavelength λ (nm). The definite integral in formula (1) is obtained by numerically integrating the absorbance measured at 1 nm intervals over wavelengths from 350 to 1000 nm. A commercially available device can be used to measure the integrated absorbance Q, such as the UV-3100PC spectrophotometer manufactured by Shimadzu Corporation. The integrated absorbance Q is measured by filling a cell of a predetermined optical path length with a chloroform solution in which a predetermined amount of a liquid crystal composition for a radio wave control element has been dissolved.

[0021] <Dichroic Dye> A dichroic dye is a substance that exhibits dichroism, and dichroism refers to the property of having different absorbance depending on the polarization direction. The "dichroic dye" in the present invention preferably has a maximum absorption wavelength in the range of 350 to 1000 nm. As the dichroic dye, an optimal type of dichroic dye is appropriately selected so as to satisfy the range of the integrated absorbance Q described above. The dichroic dye may be used alone or in combination of two or more types. In particular, the present composition preferably contains two or more types of dichroic dyes. When the present composition contains two or more types of dichroic dyes, the present composition preferably contains two to four types of dichroic dyes, and more preferably contains two to three types of dichroic dyes.

[0022] The dichroic dye preferably exhibits liquid crystallinity. That is, a liquid crystalline dichroic dye is preferred. Here, "exhibiting liquid crystallinity" means that the compound has the property of exhibiting a liquid crystal phase (intermediate phase) between a crystalline phase (low temperature side) and an isotropic phase (high temperature side) when the temperature is changed. As a specific observation method, the optical anisotropy and fluidity derived from the liquid crystal phase can be confirmed by observing the compound under a polarizing microscope while heating or cooling it.

[0023] Among these, the compound represented by formula (X) is preferred as the dichroic dye in terms of the superior effect of the present invention.

[0024]

[0025] In formula (X), R 1 and R 2 each independently represents a linear or branched hydrocarbon group having 1 to 10 carbon atoms, and the hydrocarbon group may contain an oxygen atom, a nitrogen atom, or a sulfur atom. The hydrocarbon group has 1 to 10 carbon atoms, and from the viewpoint of achieving superior effects of the present invention, the number of carbon atoms is preferably 1 to 8, and more preferably 2 to 6. The hydrocarbon group is linear or branched, and is preferably linear. The hydrocarbon may be a saturated hydrocarbon group or an unsaturated hydrocarbon group.

[0026] The hydrocarbon group may contain an oxygen atom, a nitrogen atom, or a sulfur atom. The hydrocarbon group may contain a plurality of atoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms. For example, the hydrocarbon group may contain, between carbon atoms or at the terminal, -O-, -S-, -CO-, -CS-, -CO-O-, -CO-NR 10 -, -NR 10 -, or a combination thereof. 10 represents a hydrogen atom or an alkyl group. The hydrocarbon group may include, for example, —O—, —S—, —CO—, —CS—, —CO—O—, —CO—NR 10 -, -NR 10 -, or alkyl groups which may contain a combination of these groups are preferred.

[0027] R 1 and R 2 may be bonded to each other to form a ring. The ring formed may be an aliphatic ring or an aromatic ring.

[0028] A and B each independently represent a divalent aromatic ring group. Examples of the divalent aromatic ring group include a divalent aromatic hydrocarbon ring group or a divalent aromatic heterocyclic group. The divalent aromatic hydrocarbon ring group is a group formed by removing two hydrogen atoms from an aromatic hydrocarbon ring. The aromatic hydrocarbon ring may be a monocyclic ring or a condensed ring. Examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, an anthracene ring, a pyrene ring, a phenanthrene ring, and a fluorene ring. The divalent aromatic heterocyclic group is a group formed by removing two hydrogen atoms from an aromatic heterocycle. The aromatic heterocycle may be a monocyclic ring or a condensed ring.Examples of the aromatic heterocycle include a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a triazine ring (for example, a 1,2,3-triazine ring, a 1,2,4-triazine ring, and a 1,3,5-triazine ring), a tetrazine ring (for example, a 1,2,4,5-tetrazine ring), a quinoxaline ring, a pyrrole ring, a furan ring, a thiophene ring, an imidazole ring, an oxazole ring, a thiazole ring, a benzopyrrole ring, a benzofuran ring, a benzothiophene ring, a benzimidazole ring, a benzoxazole ring, a benzothiazole ring, a naphthopyrrole ring, a naphthofuran ring, a naphthothiophene ring, a naphthoimidazole ring, a naphthoxazole ring, a pyrroloimidazole ring (for example, a 5H-pyrrolo[1,2-a]imidazole ring), an imidazooxazole ring (for example, an imidazo[2,1-b]oxazole ring), a thienoyl group, a benzophenone ring, a benzophenone ring, a benzoisopropyl group ... Thiazole rings (for example, thieno[2,3-d]thiazole rings, etc.), benzothiadiazole rings, benzodithiophene rings (for example, benzo[1,2-b:4,5-b']dithiophene rings, etc.), thienothiophene rings (for example, thieno[3,2-b]thiophene rings, etc.), thiazolothiazole rings (for example, thiazolo[5,4-d]thiazole rings, naphthodithiophene rings (for example, naphtho[2,3-b: [6,7-b']dithiophene ring, naphtho[2,1-b:6,5-b']dithiophene ring, naphtho[1,2-b:5,6-b']dithiophene ring, and 1,8-dithiadicyclopenta[b,g]naphthalene ring, etc.), benzothienobenzothiophene ring, dithieno[3,2-b:2',3'-d]thiophene ring, and 3,4,7,8-tetrathiadicyclopenta[a,e]pentalene ring.

[0029] L represents a single bond, -CR=CR-, -C≡C-, -CR=N-, or -N=N-. Each R independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 6 carbon atoms.

[0030] n represents an integer of 1 to 3, and when n is 2 or 3, a plurality of As and Ls may be the same or different.

[0031] R 3represents a hydrogen atom or a substituent. The type of the substituent is not particularly limited, and examples thereof include a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), a hydrocarbon group (an alkyl group (including a cycloalkyl group, a bicycloalkyl group, and a tricycloalkyl group), an alkenyl group (including a cycloalkenyl group and a bicycloalkenyl group), an alkynyl group, and an aryl group), a heterocyclic group, a cyano group, an isothiocyanate group, a nitro group, an alkoxy group, an aryloxy group, a silyl group, a silyloxy group, a heterocyclic oxy group, an acyloxy group, a carbamoyloxy group, an alkoxycarbonyloxy group, an aryloxycarbonyl Examples of the substituent include an oxy group, a primary, secondary or tertiary amino group (including an anilino group), an alkylthio group, an arylthio group, a heterocyclic thio group, an alkyl or arylsulfinyl group, an alkyl or arylsulfonyl group, an acyl group, an aryloxycarbonyl group, an alkoxycarbonyl group, an aryl or heterocyclic azo group, an imido group, a phosphino group, a phosphinyl group, a phosphinyloxy group, a phosphinylamino group, a phosphono group, a carboxy group, a phosphoric acid group, a sulfonic acid group, a hydroxy group, a thiol group, an acylamino group, a carbamoyl group, a ureido group, a boronic acid group, and a combination thereof.Among these, the substituent is preferably an alkyl group, an alkoxy group, a cyano group, or an isothiocyanate group, which may contain an oxygen atom, a nitrogen atom, or a sulfur atom.The alkyl group may contain an oxygen atom, a nitrogen atom, or a sulfur atom. For example, the alkyl group and alkoxy group may have —O—, —S—, —CO—, —CS—, —CO—O—, or —CO—NR between carbon atoms or at the terminal. 10 -, -NR 10 -, or a combination thereof. 10 represents a hydrogen atom or an alkyl group. The alkyl group and alkoxy group are each selected from the group consisting of —O—, —S—, —CO—, —CS—, —CO—O—, and —CO—NR 10 -, -NR 10The number of carbon atoms in the alkyl group and alkoxy group is not particularly limited, and is preferably 1 to 30, more preferably 1 to 25, and even more preferably 3 to 25.

[0032] The dichroic dye used in the present invention is also preferably a compound represented by formula (Y).

[0033] R 11 -L 11 -A 11 -(Z 11 -B 11 ) m -L 12 -R 12 Formula (Y): In formula (Y), R 11 and R 12 are each independently —CH 2 - represents an alkyl group which may be substituted with -O- or -CO-O-, a cyano group, a halogen atom, -N=C=S, or -N=C=Se, provided that R 11 and R 12 At least one of R represents an alkyl group having an asymmetric carbon atom; 11 and R 12 The total number of asymmetric carbon atoms contained in L is 2 or more. 11 and L 12 each independently represents a single bond, —O—, —CO—, —CO—O—, —O—CO—O—, or —NR 13 - or -CH=CH-, and O may be substituted with S. 13 represents an alkyl group which may have a substituent. 11 and B 11 each independently represents an aromatic ring group which may have a substituent or an aliphatic ring group which may have a substituent. 11 and B 11 Examples of the aromatic ring group represented by the formula (X) include the same divalent aromatic hydrocarbon ring group or divalent aromatic heterocyclic group as those described for A and B in the formula (X), and B 11 If there are multiple B 11 may be the same or different. 11represents a single bond, —O—, —CO—, —CO—O—, —O—CO—O—, —CR Z =CR Z -, -C≡C-, -N=N-, -CR Z =CR Z -CR Z =CR Z -, -C≡C-C≡C-, -CR Z =CR Z -CO- or -CR Z =CR Z represents —CO—O—, O may be substituted with S, Z 11 If there are multiple Z 11 R may be the same or different. Z each independently represents a hydrogen atom or a fluorine atom, and m represents an integer of 1 to 4.

[0034] The dichroic dyes used in the present invention may include compounds described in "Dichroic Dyes for Liquid Crystal Displays" (A. V. Ivashchenko, CRC, 1994). Methine dyes such as cyanine, oxonol, and merocyanine may also be used.

[0035] The total content of the dichroic dyes in the composition is 30% by mass or more, based on the total mass of the composition. When the composition contains only one dichroic dye, the total content of the dichroic dyes refers to the content of that one dichroic dye relative to the total mass of the composition. When the composition contains two or more dichroic dyes, the total content of the dichroic dyes refers to the combined amount of those two or more dichroic dyes. As described below, a liquid crystal composition layer made of the composition may exhibit a large refractive index anisotropy with respect to radio waves. While the details of this are unclear, it is believed that increasing the total content of the dichroic dyes in the liquid crystal composition layer increases the interaction between the dichroic dyes, thereby increasing the degree of orientational order of the absorption axes due to the absorbing skeletons in the dichroic dyes. As a result, the absorption anisotropy of the dichroic dyes affects the increase in refractive index anisotropy at wavelengths longer than the absorption wavelength. In order to obtain a more excellent effect of the present invention, the total content of the dichroic dyes in the composition is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on the total mass of the composition. The upper limit is not particularly limited, but may be 100% by mass or less.

[0036] <Other Components> The composition may contain components other than the dichroic dye. Examples of such components include liquid crystal compounds. Liquid crystal compounds that may be used in combination with the dichroic dye are preferably liquid crystal compounds having a skeleton with a high Δn. Examples of skeletons with a high Δn include skeletons having multiple rings selected from aromatic hydrocarbon rings and aromatic heterocycles, and having triple bonds and / or double bonds as linking groups. Preferred linking groups are tolan, ditolan, vinylene, or butadiene, and multiple such linking groups may be present in a single molecule. Furthermore, the liquid crystal compound preferably has an electron-donating or electron-accepting substituent at its terminal. Examples of electron-donating substituents include alkoxy groups, thioalkoxy groups, and alkylamino groups. Examples of electron-accepting groups include cyano groups, nitro groups, isocyanate groups, isothiocyanate groups, cyanovinylene groups, and dicyanovinylene groups. These compounds do not necessarily need to be visible-transparent, and the Δn tends to increase as the absorption wavelength extends into the visible light region. The maximum absorption wavelength (λmax) of these compounds is preferably 320 nm or more, more preferably 350 nm or more, and even more preferably 380 nm or more. The present composition preferably does not substantially contain a solvent. The phrase "substantially does not contain a solvent" means that the solvent content is 5% by mass or less, preferably 1% by mass or less, based on the total mass of the present composition.

[0037] <Liquid Crystal Composition for Radio Wave Control Device> The present composition is a composition that exhibits liquid crystallinity. For example, when the present composition contains a liquid crystal dichroic dye, the present composition may exhibit liquid crystallinity. In particular, in terms of achieving superior effects of the present invention, the present composition preferably exhibits a nematic phase over the entire temperature range of 10 to 50°C. Furthermore, the present composition preferably exhibits a nematic phase at any temperature between 50 and 150°C, and exhibits a glassy state or smectic liquid crystallinity at any temperature below 50°C.

[0038] <Radio wave control element> The composition can be applied to a radio wave control element. The radio wave control element acts on radio waves. Examples of radio waves include radio waves with a frequency of 0.007 to 0.3 THz. Radio waves in this frequency band (RW) are also called high-frequency radio waves (centimeter waves, millimeter waves, terahertz waves), and are capable of high-capacity wireless communication while also having high linearity.

[0039] An example of a radio wave control element is a radio wave control element having, in this order, a first electrode, a liquid crystal composition layer made of the present composition, and a second electrode. In the radio wave control element, applying a voltage between the first and second electrodes controls the orientation state of the dichroic dye contained in the liquid crystal composition layer, thereby adjusting the refractive index anisotropy of the liquid crystal composition layer and thereby adjusting the propagation direction of radio waves. In a liquid crystal composition layer made of the present composition, the orientation state of the dichroic dye can be changed by voltage application. This characteristic is particularly likely to be exhibited when the dichroic dye exhibits liquid crystallinity. In a liquid crystal composition layer made of the present composition, a state exhibiting large refractive index anisotropy can be achieved by controlling the orientation state of the dichroic dye. Generally, the response speed of a radio wave control element depends on the film thickness of the liquid crystal composition layer. Because a liquid crystal composition layer made of the present composition can exhibit large refractive index anisotropy, the film thickness of the liquid crystal composition layer can be reduced, resulting in improved response speed. Therefore, the reflection direction of incident radio waves can be switched in a short time.

[0040] In addition, in a radio wave control element including a liquid crystal composition layer made of this composition, the integrated absorbance Q being equal to or greater than a predetermined value can also reduce noise in sensors using visible light or infrared light. More specifically, if the integrated absorbance Q is large, the visible light or infrared light that strikes the radio wave control element is absorbed by the liquid crystal composition layer, preventing it from becoming noise light and resulting in a radio wave control element that is less susceptible to noise. In other words, an electromagnetic wave control element can be realized that does not cause unnecessary reflection or scattering by the radio wave control element and is less susceptible to noise when detecting signals using a visible light or infrared light sensor shared with an antenna. Furthermore, from the perspective of decoration, this is desirable because it can make the electrodes used in the radio wave control element less visible.

[0041] Specific examples of radio wave control elements will be described below with reference to the drawings. A radio wave reflecting device 2 shown in FIG. 1 uses a radio wave control element 10A according to the technology of the present disclosure. The radio wave reflecting device 2 can reflect highly directional radio waves RW radiated from an antenna ANT located behind a building BL toward an area AR1 in front of the building BL, which is in the shadow of the antenna ANT. The radio wave reflecting device 2 can also change the reflection direction of the radio waves RW to different directions in multiple areas AR1 and AR2. For example, the area where many users are present may change depending on the time of day, such as when many wireless communication users are present in area AR1 during the daytime and in area AR2 during the nighttime. In such cases, the radio wave reflecting device 2 can change the area to which the radio waves RW are supplied by changing the reflection direction of the radio waves RW depending on the time of day.

[0042] As shown in FIG. 2 , the radio wave control element 10A has a metasurface structure 12 and is a reflective radio wave control element that reflects the propagation direction of radio waves RW in a desired direction. The metasurface structure 12 is a structure that uses metamaterials. Metamaterials are artificial materials that exhibit properties not found in natural materials, such as a negative refractive index for radio waves. The radio wave control element 10A is configured with a plurality of unit cells UC arranged two-dimensionally, and the two-dimensional plane formed by the arrangement of the plurality of unit cells UC serves as a reflection surface for the radio waves RW. Each unit cell UC includes a microstructure 14 as a metamaterial, and constitutes the smallest unit on the reflection surface that can actively change the phase of the radio waves RW. The microstructure 14 is made of metal, for example. The microstructure 14 is sized on the order of the wavelength of the incident radio waves RW or less and functions as a resonator that resonates through interaction with the incident radio waves RW. Electrically, the microstructure 14 can be considered equivalent to a resonant circuit, for example, a coil and a capacitor connected in series to resonate an alternating current. The phase of the incident radio wave RW changes due to the resonance action of the microstructure 14. Furthermore, by actively changing the resonance conditions of the microstructure 14 using various methods, it is also possible to control the amount of phase delay of the radio wave RW.

[0043] The radio wave control element 10A mainly acts on radio waves RW with a frequency of 0.007 to 0.3 THz. In the radio wave control element 10A, the metasurface structure 12 is configured to act on radio waves RW with a frequency of 0.007 to 0.3 THz. The wavelength of radio waves RW with a frequency of 0.007 to 0.3 THz is 0.07 to 3 mm, and the size of the microstructures 14 that make up the metasurface structure 12 is, for example, on the order of about half the wavelength. By making the size of the microstructures 14 equal to or less than the wavelength of the radio waves RW, the microstructures 14 resonate with the radio waves RW that pass through them and function as a phase modulation element that modulates the phase of the radio waves RW.

[0044] As shown in FIG. 3 by the incident direction IN and the outgoing direction OUT, the overall traveling direction of the radio wave RW can be considered as the normal direction to the line connecting the wavefronts of the multiple radio waves RW. In the radio wave control element 10A, for example, consider gradually increasing the phase delay of the radio wave RW incident on and reflected from each of the multiple unit cells UC arranged in a one-dimensional array from the right-hand unit cell UC to the left-hand unit cell UC. In this case, even if the line connecting the wavefronts of the individual incident radio waves RW is parallel to the reflecting surface, the line connecting the wavefronts of the individual radio waves RW reflected by each unit cell UC is inclined with respect to the reflecting surface. In other words, the outgoing direction OUT, which is the traveling direction of the radio wave RW emitted from the reflecting surface, changes by an angle θ with respect to the incident direction IN of the radio wave RW. In this way, the traveling direction of the radio wave RW can be controlled by performing phase modulation, i.e., controlling the phase delay, for each unit cell UC.

[0045] As a result, while a normal reflector can only change the direction of propagation of the radio wave RW in the direction of specular reflection, the radio wave reflecting device 2 can change the direction of propagation of the radio wave RW in a direction other than specular reflection by using the metasurface structure 12. In addition, by actively changing the amount of phase delay in each unit cell UC, it becomes possible to actively change the direction of propagation of the radio wave RW.

[0046] As an example, as conceptually shown in Figure 4, a radio wave control element 10A uses a liquid crystal composition layer 20 as an element that actively changes the resonance conditions of the microstructures 14 of the metasurface structure 12. The radio wave control element 10A has, from the bottom in the figure, a first electrode layer 26, a liquid crystal composition layer 20, and the metasurface structure 12, in this order. The liquid crystal composition layer 20 is provided on a support 24. Furthermore, the first electrode layer 26 is provided so as to entirely cover the surface of the support 24 opposite to the liquid crystal composition layer 20. The liquid crystal composition layer 20 contains a dichroic dye (liquid crystal dichroic dye LD) that exhibits liquid crystallinity.

[0047] Each unit cell UC is configured to include a microstructure 14, a liquid crystal composition layer 20, and a first electrode layer 26. Of these, the microstructure 14 is provided individually for each unit cell UC. The remaining components, the support 16, the liquid crystal composition layer 20, the support 24, and the first electrode layer 26, are not independent components for each unit cell UC, but are integrally formed in regions corresponding to a plurality of unit cells UC.

[0048] In the radio wave control element 10A, the first electrode layer 26 and the support 24, and the liquid crystal composition layer 20 and the support 16 are attached using an adhesive (pressure-sensitive adhesive or adhesive) as necessary. There are no limitations on the attachment method, and various known methods that are permeable to the radio waves that are the target of the radio wave control element 10A, such as a method that uses an OCA (Optical Clear Adhesive) that is permeable to the radio waves that are the target of the radio wave control element 10A, can be used.

[0049] As an example, the microstructure 14 is formed of a conductive material and doubles as an electrode that forms an electrode pair with the first electrode layer 26. Furthermore, a power supply 28 is connected to each microstructure 14 for applying a voltage between the microstructure 14 and the first electrode layer 26. This makes it possible to control the magnitude of the voltage applied to each unit cell UC. The first electrode layer 26 is a common electrode shared by each unit cell UC, and the microstructure 14 of each unit cell UC functions as an individual electrode. The first electrode layer 26 functioning as a common electrode is an example of a "first electrode" according to the technology of the present disclosure, and the individual electrode shared by the microstructure 14 is an example of a "second electrode." The microstructure 14 as the second electrode and the first electrode layer 26 as the first electrode are an example of an "electrode pair for applying a voltage."

[0050] The radio wave control element 10A is a reflective type, and the first electrode layer 26 also serves as a reflective layer that reflects the radio wave RW.

[0051] In the liquid crystal composition layer 20, the orientation state (hereinafter also referred to as the orientation pattern) of the liquid crystal dichroic dye changes upon application of a voltage. The alignment direction of the microstructures 14 of each unit cell UC is a direction (X direction or Y direction in the figure) perpendicular to the thickness direction of the liquid crystal composition layer 20 (Z direction in the figure). Here, the microstructures 14 and the first electrode layer 26 are disposed on both sides of the thickness direction of the liquid crystal composition layer 20. By supplying power from a power source 28, a voltage is applied between the microstructures 14 and the first electrode layer 26 of each unit cell UC. The application of the voltage generates an electric field in the thickness direction of the liquid crystal composition layer 20, changing the orientation state of the liquid crystal dichroic dye LD in each unit cell UC. Furthermore, the orientation state of the liquid crystal dichroic dye LD in each unit cell UC can be adjusted by adjusting the voltage applied to each unit cell UC.

[0052] As shown in Fig. 5, the liquid crystal dichroic dye LD has a cross section that is approximately elliptical with a major axis and a minor axis. As an example, when no voltage is applied between the microstructure 14 and the first electrode layer 26, which function as an electrode pair, no electric field is generated in the liquid crystal composition layer 20. In this state, as conceptually shown in the upper part of Fig. 5, the liquid crystal dichroic dye LD is oriented with its major axis aligned along the thickness direction of the liquid crystal composition layer 20. In the following description, this alignment state will also be referred to as "vertical alignment."

[0053] When a voltage is applied between the microstructures 14 and the first electrode layer 26 from this state, an electric field is generated in the liquid crystal composition layer 20, and the alignment state of the liquid crystal dichroic dye LD changes. Specifically, as conceptually shown in the lower part of Figure 5, the alignment state of the liquid crystal dichroic dye LD in the region corresponding to the microstructures 14 changes depending on the magnitude of the applied voltage, and the liquid crystal dichroic dye LD is tilted with respect to the thickness direction of the liquid crystal composition layer 20. The example shown in the lower part of Figure 5 shows a state in which the tilt angle of the liquid crystal dichroic dye LD is maximum. When the tilt angle is maximum, the liquid crystal dichroic dye LD is oriented so that its major axis is aligned in a direction perpendicular to the thickness direction of the liquid crystal composition layer 20. In the following description, the alignment state in which the tilt angle is maximum is also referred to as "horizontal alignment."

[0054] The refractive index of the liquid crystal composition layer 20 increases as the inclination of the liquid crystal dichroic dye LD increases, i.e., as the angle of the long axis of the liquid crystal dichroic dye LD approaches the principal surface direction of the liquid crystal composition layer 20 (the X or Y direction in FIG. 5 ). Conversely, the refractive index of the liquid crystal composition layer 20 decreases as the inclination of the liquid crystal dichroic dye LD decreases, i.e., as the angle of the long axis of the liquid crystal dichroic dye LD approaches the thickness direction of the liquid crystal composition layer 20 (the Z direction in FIG. 5 ). This change in the refractive index of the liquid crystal composition layer 20 of each unit cell UC changes the resonance condition of the microstructure 14, thereby changing the amount of phase delay of the incident radio wave RW. In this example, the amount of phase delay of the unit cell UC in the lower row of FIG. 5 is greater than that of the unit cell UC in the upper row of FIG. 5 .

[0055] That is, when the alignment state of the liquid crystal dichroic dye LD in the liquid crystal composition layer 20 located around the microstructures 14 of each unit cell UC changes, the refractive index of the liquid crystal composition layer 20 changes with respect to the radio wave RW transmitted through each unit cell UC. Because the refractive index and the dielectric constant are positively correlated, a change in the refractive index of the liquid crystal composition layer 20 changes the resonance conditions of the microstructures 14, which function as a resonator. The change in the resonance conditions of the microstructures 14 manifests as a change in the phase delay of the radio wave RW. Therefore, changing the refractive index of the liquid crystal composition layer 20 can change the phase delay of the radio wave RW. Furthermore, a change in the refractive index of the liquid crystal composition layer 20 itself also causes a change in the phase delay of the radio wave RW. Because the refractive index of the liquid crystal composition layer 20 of each unit cell UC changes depending on the voltage V applied to each unit cell UC, the relationship between the voltage V and the phase delay of the radio wave RW is, for example, as shown in FIG. 6 .

[0056] As shown in FIG. 3 , when a radio wave RW enters the radio wave control element 10A from the microstructure 14 side, the radio wave RW passes through the microstructure 14 and the liquid crystal composition layer 20 in this order. Furthermore, the radio wave RW is reflected by the first electrode layer 26, which also serves as a reflective layer, and again passes through the liquid crystal composition layer 20 and the microstructure 14 in this order before exiting the radio wave control element 10A. The radio wave RW is reflected along this incident / exit path. Along the incident / exit path, the radio wave RW passing through each unit cell UC undergoes phase modulation due to resonance by the microstructure 14 and phase modulation due to transmission through the liquid crystal composition layer 20. More specifically, in each unit cell UC, the resonance condition of the microstructure 14 is determined according to the refractive index of the liquid crystal composition layer 20, and phase modulation of the radio wave RW occurs due to resonance according to this condition. In addition, phase modulation of the radio wave RW also occurs according to the magnitude of the refractive index of the liquid crystal composition layer 20.

[0057] Based on the relationship shown in FIG. 6, the reflection direction of the radio wave RW reflected by the radio wave control element 10A is controlled by controlling the amount of phase delay of the radio wave RW for each unit cell UC through the applied voltage V.

[0058] 3, while a normal reflector can only change the direction of propagation of the radio wave RW in the direction of specular reflection, the radio wave control element 10A can change the direction of propagation of the radio wave RW in a direction other than specular reflection by using the metasurface structure 12. In addition, by actively changing the amount of phase delay in each unit cell UC, it is possible to actively change the direction of propagation of the radio wave RW.

[0059] Furthermore, various examples of controlling the direction of travel of the radio waves RW emitted from the radio wave control element 10A are possible other than controlling the reflected radio waves RW so that they travel in a straight line overall in one direction as in the example shown in Figure 3. For example, the radio waves RW emitted from the radio wave control element 10A may be made to converge toward a single focal point, or conversely, may be made to diverge. The direction of travel of the emitted radio waves RW can be controlled by adjusting the voltage applied to each unit cell UC, thereby adjusting the amount of phase delay of the radio waves RW for each unit cell UC.

[0060] For example, in the case of a plurality of unit cells UC arranged in one direction as shown in FIG. 3 , consider increasing the phase delay of the central unit cell UC and decreasing the phase delay toward both sides. In this case, connecting the wavefronts of the radio waves RW passing through each unit cell UC forms a V-shape, allowing the emitted radio waves RW to be focused. Conversely, consider decreasing the phase delay of the central unit cell UC and increasing the phase delay toward both sides. In this case, connecting the wavefronts of the radio waves RW passing through each unit cell UC forms a mountain-like shape (inverted V-shape), allowing the emitted radio waves RW to diverge. The degree of such focusing and divergence can also be adjusted by controlling the phase delay of the radio waves RW passing through each unit cell UC through adjusting the magnitude of the applied voltage.

[0061] Similar to known metasurface structures, the metasurface structure 12 is formed by two-dimensionally arranging microstructures 14, which are metamaterials, on a support 16. In the illustrated metasurface structure 12, as shown in Fig. 2, the microstructures 14 are two-dimensionally arranged at equal intervals in the X and Y directions, which are orthogonal to each other. In this metasurface structure 12, all of the microstructures 14 are, for example, the same.

[0062] There are no limitations on the support 16, and various known sheet-like materials can be used as long as they can support the microstructure 14 and can transmit radio waves RW of 0.007 to 0.3 THz, which are the frequency range targeted by the radio wave control element 10A. Examples of the support 16 include a metal substrate having an oxide insulating layer, such as a silicon substrate having silicon oxide, a support made of an oxide such as silicon oxide, a support made of a semiconductor such as germanium and chalcogenide glass, a polyacrylic resin film such as polymethyl methacrylate, a cellulose resin film such as cellulose triacetate, a cycloolefin polymer film (for example, a product under the trade name "Arton" manufactured by JSR Corporation, or a product under the trade name "Zeonor" manufactured by Zeon Corporation), a resin film such as a polyethylene terephthalate (PET) film, a polycarbonate film, and a polyvinyl chloride film, and a glass plate.

[0063] There is no limitation on the thickness of the support 16, as long as it can support the microstructure 14, has sufficient transparency to radio waves RW with a frequency of 0.007 to 0.3 THz, and has sufficient strength depending on the application of the radio wave control element 10A, etc. The thickness of the support 16 is set appropriately depending on the material from which the support 16 is made so as to satisfy these conditions.

[0064] In the radio wave control element 10A according to the technology of the present disclosure, the support 16 is not an essential component of the metasurface structure 12, and the support 16 may be omitted. For example, if possible, the metasurface structure 12 may be formed by arranging the microstructures 14 directly on the surface of the liquid crystal composition layer 20.

[0065] As described above, the metasurface structure 12 is composed of microstructures 14, which are metamaterials, spaced apart and arranged two-dimensionally on a plane, and more specifically, is composed of an arrangement of unit cells UC, each of which basically consists of one microstructure 14 and the space surrounding the microstructure 14.

[0066] In the radio wave control element 10A according to the technology of the present disclosure, the shape of the metasurface structure is basically the same as that of known metasurface structures. Therefore, various known metasurface structures can be used in the radio wave control element 10A according to the technology of the present disclosure. That is, the technology of the present disclosure does not limit the shape and material of the microstructures 14, the arrangement of the microstructures 14, or the pitch between the microstructures 14. Furthermore, the metasurface structure 12 may be designed using known methods depending on the wavelength of the radio wave RW to be controlled by the radio wave control element 10A and the desired reflection characteristics (e.g., the range of controllable reflection directions). For example, the amplitude and phase of the radio wave RW reflected by the microstructures 14 used may be calculated using commercially available simulation software, and the arrangement of the microstructures 14 may be set to achieve the desired distribution of phase modulation amounts. When a liquid crystal composition layer 20 is used as in this example, phase modulation occurs due to the refractive index and the interaction between the refractive index and the microstructures 14. The amount of phase modulation is determined by the resonance characteristics of the microstructures 14, which change depending on the refractive index.

[0067] The radio wave control element 10A according to the technology of the present disclosure is intended to control radio waves RW with a frequency of 0.007 to 0.3 THz. Therefore, the metasurface structure 12 has microstructures 14 selected so as to impart a desired phase difference to the radio waves RW with this frequency, and the arrangement of the microstructures is also set. Specifically, when radio waves RW with a frequency of 0.007 to 0.3 THz are to be controlled, the wavelength range of the radio waves RW is approximately 0.07 to 3 mm, so the size of the microstructures 14 is selected to be equal to or smaller than this wavelength range.

[0068] Although one unit cell UC basically has one microstructure 14, the technology of the present disclosure is not limited to this. That is, in the radio wave control element according to the technology of the present disclosure, one unit cell UC may have multiple microstructures 14 as necessary depending on the reflection characteristics, the size, material and shape of the microstructures 14, and the size of the unit cell UC. In this case, one unit cell UC may have different microstructures 14. However, because the unit cell UC is the smallest unit capable of actively changing the phase of the radio wave RW, even when one unit cell UC has multiple microstructures 14, the amount of phase modulation is determined for each unit cell UC.

[0069] Furthermore, there are no limitations on the material for forming the microstructure 14, and various materials used as microstructures in known metasurface structures can be used. Examples of materials for forming the microstructure 14 include metals and dielectrics. In the case of metals, copper, gold, and silver are preferred due to their low optical loss. In addition, composites consisting of metal particles and binders and oxide semiconductors can also be used as materials for forming the microstructure 14. On the other hand, in the case of dielectrics, silicon, titanium oxide, and germanium are preferred due to their high refractive index and the ability to increase the amount of phase modulation. Note that, as shown in FIG. 4 , when the microstructure 14 also serves as an electrode that forms an electrode pair with the first electrode layer 26, the microstructure 14 is formed from a conductor.

[0070] Similarly, the shape of the microstructure 14 is not limited, and various shapes used as microstructures in known metasurface structures can be used. Examples include a cross-shaped solid like a crossed rectangular parallelepiped, a rectangular parallelepiped, a cylindrical shape, a V-shaped solid like a rectangular parallelepiped connected at its ends as shown in JP 2018-046395 A, an approximately H-shaped solid like an H-beam, and an approximately C-shaped solid like a C-channel. As shown in JP 2018-046395 A, various shapes can be used for the V-shaped solid and the cross-shaped solid by adjusting the angle between the two rectangular parallelepipeds. Other shapes, such as those shown in Figure 5 of "Appl. Sci. 2018, 8(9), 1689; https: / / doi.org / 10.3390 / app8091689," can also be used.

[0071] In the metasurface structure 12, the microstructures 14 may be of the same type, or multiple types may be used in combination. Furthermore, the same microstructures 14 may be arranged in the same orientation in the XY plane, or in different orientations. Furthermore, microstructures 14 of the same orientation and those of different orientations may be mixed. However, in the radio wave control element 10A according to the technology of the present disclosure, it is preferable to use only one type of microstructure 14 and to arrange all of the microstructures 14 in the same orientation.

[0072] 3, the metasurface structure 12 preferably has identical microstructures 14, all of which have the same structure, arranged two-dimensionally at equal intervals in the mutually orthogonal X and Y directions. However, the technology of the present disclosure is not limited to this, and multiple types of microstructures may be used in combination as described above. Furthermore, the arrangement intervals and arrangement of the microstructures 14 may also differ in the plane direction of the support 16. However, considering the controllability of the reflection direction of radio waves RW when a voltage is applied to the liquid crystal composition layer 20, it is preferable that the metasurface structure 12 use all the same microstructures 14. Furthermore, it is more preferable that the microstructures 14 in the metasurface structure 12 are spaced at equal intervals, and even more preferably at equal intervals in both the orthogonal X and Y directions.

[0073] The liquid crystal composition layer 20 is a layer in which the liquid crystal dichroic dye LD is aligned in a predetermined state, and as described above, the alignment state of the liquid crystal dichroic dye LD changes when a voltage is applied.

[0074] In the liquid crystal composition layer 20 illustrated in Fig. 4, when no voltage is applied, the liquid crystal dichroic dye LD is vertically aligned. When a voltage is applied to the liquid crystal composition layer 20, the liquid crystal dichroic dye LD is aligned at an angle relative to the thickness direction in response to the applied voltage, and reaches a maximum horizontal alignment. In the radio wave control element 10A, the change in alignment of the liquid crystal dichroic dye LD is not limited to a change from vertical alignment to horizontal alignment or vice versa, but may be a change from a state tilted relative to the thickness direction to a horizontal or vertical alignment, a change from a horizontal or vertical alignment to a state tilted relative to the thickness direction, or a change at an angle from a state tilted relative to the thickness direction to a state tilted relative to the thickness direction.

[0075] The liquid crystal composition layer 20 may be formed, for example, on the surface of an alignment film described later by a known method. In the radio wave control element 10A, the liquid crystal composition layer 20 is formed on a support 24. The support 24 is basically the same as the support 16 described above.

[0076] Here, the support 24 on which the liquid crystal composition layer 20 is formed may further include an alignment film for orienting the liquid crystal dichroic dye LD in a predetermined state on the surface of the support 16 described above, which serves as the main body, on which the liquid crystal composition layer 20 is formed. Various known alignment films can be used. Examples include rubbed films made of organic compounds such as polymers, obliquely evaporated films of inorganic compounds, films with microgrooves, and films formed by accumulating LB (Langmuir-Blodgett) films made by the Langmuir-Blodgett method using organic compounds such as ω-tricosanoic acid, dioctadecylmethylammonium chloride, and methyl stearate. Furthermore, so-called photo-alignment films, which are formed by irradiating a photo-alignable material with polarized or unpolarized light, can also be used as the alignment film. These alignment films can be formed by known methods depending on the material used to form the main body.

[0077] The surface of the support 24 on which the liquid crystal composition layer 20 is formed, opposite to the liquid crystal composition layer 20, is entirely covered with a first electrode layer 26. The first electrode layer 26 is an electrode that changes the orientation of the liquid crystal dichroic dye LD in the liquid crystal composition layer 20, and also functions as a reflective layer that reflects radio waves RW with a frequency of 0.007 to 0.3 THz that are incident from the metasurface structure 12 side, as described above.

[0078] There are no limitations on the first electrode layer 26, and a sheet-like material made of various known materials can be used as long as it has sufficient conductivity and is capable of reflecting radio waves RW. Examples of the first electrode layer 26 include metal layers such as copper, aluminum, gold, and silver; inorganic conductive materials such as ITO (tin-doped indium oxide); organic conductive materials such as polythiophenes, typified by PEDOT (poly 3,4-ethylenedioxythiophene); and graphene. Inorganic conductive materials, organic conductive materials, and graphene are transparent to visible light but act as reflective layers for radio waves of the above frequencies.

[0079] There is no limitation on the thickness of the first electrode layer 26, and the thickness may be set appropriately depending on the material from which the first electrode layer 26 is made so that the target radio waves can be reflected with the required reflectivity.

[0080] As described above, the radio wave control element 10A according to the technology of the present disclosure is a reflective radio wave control element having a metasurface structure 12 and a liquid crystal composition layer 20. In the radio wave control element 10A, power is supplied to each microstructure 14 to change the alignment state of the liquid crystal dichroic dye LD in the corresponding region of the liquid crystal composition layer 20, thereby forming regions with different refractive indices for each unit cell UC, thereby reflecting the radio wave RW in a desired direction. Furthermore, by changing the power supplied to each microstructure 14, i.e., the voltage applied to the liquid crystal composition layer 20, the reflection direction of the incident radio wave RW can be switched.

[0081] In the radio wave control element 10A according to the technology of the present disclosure, the refractive index anisotropy Δn of the liquid crystal composition layer 20 with respect to radio waves is not limited, but is preferably large. Here, in the reflective radio wave control element 10A of this example, the refractive index anisotropy Δn of the liquid crystal composition layer 20 with respect to radio waves of 100 GHz is preferably 0.35 or more. By making the refractive index anisotropy Δn of the liquid crystal composition layer 20 with respect to radio waves of 100 GHz 0.35 or more, the liquid crystal composition layer 20 can be made thinner, which is preferable in that the reflection direction of the radio waves RW can be switched more quickly.

[0082] Furthermore, there is no limitation on the thickness of the liquid crystal composition layer 20, and a thickness that provides the necessary phase difference for the radio wave RW may be appropriately set depending on the material for forming the liquid crystal composition layer 20. As described above, in the radio wave control element 10A according to the technology of the present disclosure, the liquid crystal composition layer 20 is made of the present composition containing a predetermined amount of dichroic dye, and therefore the liquid crystal composition layer 20 can be made thin. In consideration of this point, the thickness of the liquid crystal composition layer 20 is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less. Setting the thickness of the liquid crystal composition layer 20 to 200 μm or less is preferable in that the reflection direction of the radio wave RW can be switched more quickly, for example.

[0083] Another example of a radio wave control element includes a temperature adjustment member that adjusts the temperature of the liquid crystal composition layer. In this embodiment, the orientation state of the dichroic dye in the liquid crystal composition layer can be fixed. This embodiment will be described in detail below. The radio wave control element 10B shown in FIG. 7 includes, from the bottom in the figure, a first electrode layer 26, a liquid crystal composition layer 20, and a metasurface structure 12, in this order. The liquid crystal composition layer 20 is provided on a support 24. Furthermore, the first electrode layer 26 is provided to completely cover the surface of the support 24 opposite the liquid crystal composition layer 20. Furthermore, a temperature adjustment member 30 is provided between the support 24 and the first electrode layer 26. The radio wave control element 10B shown in FIG. 7 has the same configuration as the radio wave control element 10A shown in FIG. 4, except for the temperature adjustment member 30. In the liquid crystal composition layer 20 shown in FIG. 7, when no voltage is applied, the liquid crystal dichroic dye LD is horizontally aligned, and as the applied voltage is increased, the liquid crystal dichroic dye LD is aligned in a direction that causes it to be vertically aligned.

[0084] The configuration of the temperature adjustment member 30 is not particularly limited as long as it is a member that adjusts the temperature of the liquid crystal composition layer 20. The location where the temperature adjustment member 30 is placed is also not limited as long as it can adjust the temperature of the liquid crystal composition layer 20. The temperature adjustment member 30 may also have a heating device that increases the temperature of the liquid crystal composition layer 20, a cooling device that decreases the temperature of the liquid crystal composition layer 20, or the like.

[0085] The procedure for fixing the alignment state of the liquid crystal dichroic dye LD in the liquid crystal composition layer 20 using the radio wave control element 10B is as follows. The liquid crystal dichroic dye LD contained in the liquid crystal composition layer 20 is a compound that exhibits liquid crystallinity when subjected to a heat treatment using the temperature adjustment member 30. Specifically, it is preferable to use the composition described above that exhibits a nematic phase at any temperature between 50 and 150°C and a glassy or smectic phase at any temperature below 50°C. First, in the radio wave control element 10B, the liquid crystal composition layer 20 is heated using the temperature adjustment member 30 to transition to a liquid crystal phase. Next, while maintaining the heat treatment, a voltage is applied between the first electrode layer 26 and the microstructure 14 to control the alignment direction of the liquid crystal dichroic dye LD. In this case, as shown in FIG. 8 , the voltages applied to the first unit cell UC1 and the second unit cell UC2 may be different to cause the alignment state of the liquid crystal dichroic dye LD to differ. Thereafter, when the heating and voltage application processes are stopped, the temperature drops below the transition temperature of the liquid crystal phase, and the alignment state of the liquid crystalline dichroic dye shown in Figure 8 is fixed. In other words, the aligned state of the liquid crystalline dichroic dye can be maintained even without applying a voltage.

[0086] Furthermore, in radio wave control elements, a state with higher alignment can be created depending on the type of dichroic dye used. For example, if a liquid crystal dichroic dye exhibits both a nematic phase and a higher-order liquid crystal phase such as a smectic phase, the higher-order liquid crystal phase can be fixed by rapidly cooling the radio wave control element. More specifically, the radio wave control element 10C shown in FIG. 9 has a configuration similar to that of the radio wave control element 10B shown in FIG. 7. However, in the radio wave control element 10C, the liquid crystal dichroic dye LD exhibits both a nematic phase and a smectic phase. Furthermore, in the liquid crystal composition layer 20 shown in FIG. 9, the liquid crystal dichroic dye LD is horizontally aligned when no voltage is applied, and as the applied voltage is increased, the liquid crystal dichroic dye LD is aligned in a direction toward vertical alignment. In such a radio wave control element 10C, the liquid crystal composition layer 20 is heated by a temperature adjustment member 30 as shown in FIG. 9 to align the liquid crystal dichroic dye LD and thereby develop a nematic phase. Note that Figure 9 corresponds to a mode in which no voltage is applied between the first electrode layer 26 and the microstructure 14, and the liquid crystal dichroic dye LD is horizontally aligned. As shown in Figure 9, although the liquid crystal dichroic dye LD is horizontally aligned, the degree of alignment of the nematic phase itself is not high, so the alignment direction of the liquid crystal dichroic dye LD is partially disturbed. Next, by stopping the heating treatment of the temperature adjustment member 30 and rapidly cooling the liquid crystal composition layer 20, the liquid crystal dichroic dye LD can be fixed in a state exhibiting a smectic phase. Specifically, as shown in Figure 10, the alignment of the liquid crystal dichroic dye LD is further improved. In other words, by performing the rapid cooling treatment, the liquid crystal dichroic dye can be fixed in a state with a higher degree of alignment.

[0087] Furthermore, the radio wave control element may have a layer between the first electrode and the second electrode whose refractive index does not change with voltage, or may have a gap between one of the first electrode and the second electrode and the liquid crystal composition layer. More specifically, the radio wave control element 10D shown in FIG. 11 has, from the bottom in the figure, a first electrode layer 26, a dielectric layer 32, a liquid crystal composition layer 20, and a metasurface structure 12, in this order. The radio wave control element 10D shown in FIG. 11 has the same configuration as the radio wave control element 10A shown in FIG. 4, except for the dielectric layer 32. In the liquid crystal composition layer 20 shown in FIG. 10, when no voltage is applied, the liquid crystal dichroic dye LD is horizontally aligned. As the applied voltage increases, the liquid crystal dichroic dye LD is aligned in a vertically aligned direction.

[0088] The dielectric layer 32 is a layer whose refractive index does not change with voltage. The material constituting the dielectric layer 32 is not particularly limited, as long as it has sufficient transparency to radio waves RW. Examples include semiconductors such as silicon, silicon oxide, germanium, and chalcogenide glass; polyacrylic resins such as polymethyl methacrylate; cellulose resins such as cellulose triacetate; resins such as cycloolefin polymers, polyethylene terephthalate (PET), polycarbonate, and polyvinyl chloride; and glass. The dielectric layer 32 may also be an alignment film for orienting the liquid crystal dichroic dye LD in a predetermined state. The thickness of the dielectric layer 32 is not particularly limited, but is preferably approximately the same as that of the liquid crystal composition layer 20. The difference between the thickness of the dielectric layer 32 and the thickness of the liquid crystal composition layer 20 is preferably 100 μm or less, more preferably 50 μm or less.

[0089] As in the radio wave control element 10D, by disposing a dielectric layer 32 between the first electrode layer 26 and the microstructures 14, the distance between the electrodes can be increased. This configuration reduces radio wave loss while maintaining the high response speed of the radio wave control element 10D. The location of the driving electrode that applies voltage to the liquid crystal composition layer is not particularly limited, and the electrode may be located between the first electrode layer 26 and the microstructures 14. Alternatively, an electrode may be provided between the dielectric layer 32 and the liquid crystal composition layer to efficiently apply voltage to the liquid crystal composition layer. In this case, a high-resistance electrode may be used to minimize the effect on radio waves. Furthermore, the electrodes may be positioned so as to sandwich the liquid crystal composition layer horizontally for driving with a transverse electric field. Furthermore, the dielectric constant of the material constituting the dielectric layer 32 with respect to the applied voltage is not particularly limited. When the liquid crystal composition layer and the dielectric layer are arranged in series between opposing planar electrodes, as in the case where the first electrode layer 26 and the microstructures 14 of the radio wave control element 10D are electrodes, a higher dielectric constant for the dielectric layer is preferred because it efficiently increases the electric field across the liquid crystal composition layer. In addition, when electrodes are positioned so as to sandwich the liquid crystal composition layer in the horizontal direction for driving by a transverse electric field, a low dielectric constant of the dielectric layer is preferable because the electric field of the liquid crystal composition layer can be efficiently increased. Furthermore, the dielectric layer may be patterned in the in-plane direction or the thickness direction, whereby the in-plane average effective value of the refractive index or the effective value distribution within the element can be adjusted, thereby adjusting the amount of radio wave control.

[0090] The radio wave control element may also have a light-shielding layer that blocks at least a portion of light in the wavelength range of 250 to 1000 nm. The position of the light-shielding layer in the radio wave control element is not particularly limited, but it is preferably located on the side of the liquid crystal composition layer where external light is incident. By having the light-shielding layer in the radio wave control element, light that can be absorbed by the dichroic dye can be prevented from reaching the dichroic dye, thereby suppressing decomposition of the dichroic dye.

[0091] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment details, and treatment procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.

[0092] <Dichroic Dyes> The following compounds 1-1 to 1-7 and 2-1 to 2-6 were prepared as dichroic dyes.

[0093]

[0094]

[0095]

[0096] As liquid crystal compounds used in the examples and comparative examples, the following Compound 3 and Liquid Crystal Compound A (Liquid Crystal A) (RDP-94990 manufactured by DIC Corporation) were prepared.

[0097]

[0098] Table 1 shows the integrated absorbance Q of the compounds 1-1 to 1-7, 2-1 to 2-6, 3, and liquid crystal A, which was measured in the same manner as the integrated absorbance Q of the present composition. The integrated absorbance Q of the compounds 1-1 to 1-7, 2-1 to 2-6, 3, and liquid crystal A was calculated by substituting D in the above formula (1) with the mass concentration (g L) of any of the compounds 1-1 to 1-7, 2-1 to 2-6, 3, and liquid crystal A in a chloroform solution. -1 ) and the integrated absorbance Q of the composition was measured in the same manner.

[0099]

[0100] Next, the above compounds 1-1 to 1-7, 2-1 to 2-6, and 3, and liquid crystal A were mixed to obtain the compositions shown in Table 2 below, to prepare compositions.

[0101] <Evaluation> (Liquid Crystallinity) The obtained compositions were heated and observed under a polarizing microscope equipped with a hot stage. Compositions in which the difference (TB-TA) between the transition temperature from the crystalline phase to the nematic phase (liquid crystal phase) and the transition temperature (TB) from the nematic phase (liquid crystal phase) to the isotropic phase was 50°C or more were rated A, those in which the difference (TB-TA) was less than 50°C were rated B, and those in which a liquid crystal phase was not expressed were rated C.

[0102] (Refractive index anisotropy (Δn)) The refractive index anisotropy Δn at radio waves of 100 GHz and 30 GHz was measured by the method disclosed in Applied Optics, Vol. 44, No. 7, p. 1150 (2005). The refractive index anisotropy Δn (100 GHz) was measured by filling a variable short-circuit waveguide with the above composition and aligning the dichroic dye in the composition. Radio waves of 100 GHz were input into the waveguide, and the amplitude ratio of the reflected wave to the incident wave was measured. Measurements were performed by changing the direction of the static magnetic field and the length of the short-circuit tube, and the refractive indices n e and n o were determined. The refractive index anisotropy (Δn (100 GHz)) was calculated from n e - n o. Δn (100 GHz)z was rated A when it was 0.4 or more, B when it was 0.35 or more but less than 0.4, and C when it was less than 0.35. Similarly, when the input radio wave was 30 GHz, the refractive index anisotropy Δn (30 GHz) was measured. A was assigned to samples with a Δn (30 GHz) of 0.4 or more, B to samples with a Δn (30 GHz) of 0.35 or more but less than 0.4, and C to samples with a Δn (30 GHz) less than 0.35.

[0103] In Table 2, the columns "First Component (%)", "Second Component (%)", and "Third Component (%)" indicate the type of each component used and the mass content (mass %) of each component relative to the total mass of the composition. In Table 2, "Integrated absorbance Q" is the measured value of the integrated absorbance Q described above. The compositions used in Examples 1 to 11 exhibited a nematic phase at any temperature between 50 and 150°C, and exhibited a glassy state or a smectic phase at any temperature below 50°C.

[0104]

[0105] As shown in Table 2, it was confirmed that the composition exhibited the desired effects.

[0106] 2 Radio wave reflecting device 10A, 10B, 10C, 10D Radio wave control element 12 Metasurface structure 14 Microstructure 16, 24 Support 20 Liquid crystal layer 26 First electrode layer 28 Power supply 30 Temperature adjustment member 32 Dielectric layer 34 Dielectric layer ANT Antenna AR1, AR2 Area BL Building LD Liquid crystal dichroic dye RW Radio wave UC Unit cell

Claims

1. A liquid crystal composition for radio wave control elements, comprising at least one dichroic dye, wherein the total content of the dichroic dye is 30% by mass or more based on the total mass of the liquid crystal composition for radio wave control elements, and the integrated absorbance Q in the wavelength range of 350 to 1000 nm in the absorption spectrum of a chloroform solution of the liquid crystal composition for radio wave control elements, expressed by formula (1), is 10,000 L g -1 ・cm -1 The liquid crystal composition for radio wave control element is as described above. In formula (1), Q is the integrated absorbance (L g -1 ・cm -1 ), and D is the mass concentration (g·L) of the liquid crystal composition for radio wave control element in a chloroform solution. -1 ), L represents the optical path length (cm) of the cell used in measuring the absorption spectrum, and Abs(λ) represents the absorbance at a wavelength λ (nm).

2. The liquid crystal composition for radio wave control element according to claim 1, which contains two or more kinds of said dichroic dyes.

3. The liquid crystal composition for radio wave control element according to claim 1, wherein the dichroic dye is a compound represented by formula (X). In formula (X), R 1 and R 2 R each independently represents a linear or branched hydrocarbon group having 1 to 10 carbon atoms, and the hydrocarbon group may contain an oxygen atom, a nitrogen atom, or a sulfur atom. 1 and R 2 may be bonded to each other to form a ring. A and B each independently represent a divalent aromatic ring group. L represents a single bond, -CR=CR-, -C≡C-, -CR=N-, or -N=N-. R each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 6 carbon atoms. n represents an integer of 1 to 3, and when n is 2 or 3, a plurality of As and Ls may be the same or different. R 3 represents a hydrogen atom or a substituent.

4. The liquid crystal composition for radio wave control elements according to claim 1, which exhibits a nematic phase over the entire range of 10 to 50°C.

5. The liquid crystal composition for radio wave control element according to claim 1, which exhibits a nematic phase at any temperature between 50 and 150°C, and exhibits a glass state or a smectic phase at any temperature below 50°C.

6. A radio wave control element comprising, in this order, a first electrode, a liquid crystal composition layer made of the liquid crystal composition for radio wave control elements according to any one of claims 1 to 5, and a second electrode.

7. A radio wave control element as described in claim 6, having a metasurface structure formed by arranging a plurality of microstructures, the microstructures constituting at least one of the first electrode and the second electrode.

8. The radio wave control element according to claim 6, further comprising a temperature adjusting member for adjusting the temperature of the liquid crystal composition layer.

9. A radio wave control element as described in claim 6, having a layer between the first electrode and the second electrode, the refractive index of which does not change with voltage, or having a gap between one of the first electrode and the second electrode and the liquid crystal composition layer.

10. The radio wave control element according to claim 6, further comprising a light-shielding layer for blocking at least a portion of light having a wavelength in the range of 250 to 1000 nm.

Citation Information

Patent Citations

  • Liquid crystal medium and high frequency device containing same

    JP2018501361A

  • Liquid crystal medium and high frequency component containing said liquid crystal medium

    JP2019512023A

  • Liquid crystal composition and liquid crystal element

    JP2023075037A

  • Liquid crystal composition and liquid crystal device

    JP2023121129A

  • Radio wave reflection device

    WO2023058399A1

Cited By

  • Liquid crystal composition for radio wave control element, radio wave control element, and compound

    WO2025204788A1

  • Liquid crystal composition for radio wave control element and radio wave control element