Power storage device and exterior material for power storage device

The use of a colored adhesive layer in the exterior material for all-solid-state batteries allows for precise removal of the sealant layer, enhancing cooling performance and preventing gas leakage by creating a clear color difference between coated and uncoated areas, addressing the challenges faced by conventional batteries.

WO2024242101A1PCT designated stage expired Publication Date: 2024-11-28RESONAC PACKAGING CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018665
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-21
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional all-solid-state batteries face challenges in forming accurate openings in the sealant layer for improved cooling performance and preventing gas leakage, such as hydrogen sulfide, due to the difficulty in determining the boundary between adhesive-coated and uncoated areas during the removal process.

Method used

The exterior material for all-solid-state batteries includes a base material layer, a metal foil layer, a gas barrier layer, and a sealant layer with a colored adhesive layer that creates a clear color difference between coated and uncoated areas, allowing for precise removal of the sealant layer to form openings, enhancing cooling performance and preventing gas leakage.

Benefits of technology

This solution enables the formation of highly accurate openings in the sealant layer, improving cooling performance and preventing gas leakage, thus addressing the limitations of conventional all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018665_28112024_PF_FP_ABST
    Figure JP2024018665_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an exterior material for a power storage device in which openings can be accurately formed in a sealant layer. The present invention relates to an exterior material 1 for a power storage device, the exterior material 1 including a substrate layer 11, a metal foil layer 12 laminated on the inner surface side of the substrate layer 11, a gas barrier layer 13 laminated on the inner surface side of the metal foil layer 12, and a sealant layer 15 laminated on the inner surface side of the gas barrier layer 13 via an adhesive layer 14. The sealant layer 15 is provided with a to-be-open part 2a. The adhesive layer 14 is provided with a non-adhesive-coated part 14b, which is provided corresponding to the to-be-open part 2a and in which no adhesive is present, and an adhesive-coated part 14a, which is provided in portions other than the to-be-open part and in which an adhesive is present. The adhesive in the adhesive-coated part 14a is composed of a colored adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Electricity storage device and exterior material for the same

[0001] The present invention relates to an electricity storage device such as an all-solid-state battery used as a high-power battery such as an in-vehicle battery, a battery for portable devices such as a mobile electronic device, or a battery for storing regenerative energy, and an exterior material for the electricity storage device.

[0002] All-solid-state batteries use solid electrolytes, so they do not leak or develop dendrites, and the separator is not damaged. Therefore, there are no concerns about fires caused by separator damage, and they are attracting a lot of attention from a safety perspective.

[0003] A typical all-solid-state battery is configured by sealing an all-solid-state battery body, such as an electrode active material and a solid electrolyte, inside an exterior material serving as a casing. As research into solid electrolytes advances in all-solid-state batteries, it has gradually become apparent that the performance required of the exterior material differs from that of exterior materials for batteries using conventional liquid electrolytes, and various exterior materials have been proposed to satisfy the performance requirements for all-solid-state batteries.

[0004] The exterior material for an all-solid-state battery has a basic structure including a metal foil layer and a heat-sealing layer (sealant layer) laminated on the inside of the metal foil layer, and the all-solid-state battery main body is encapsulated by heat-sealing the sealant layer.

[0005] For example, the all-solid-state battery packaging material disclosed in Patent Document 1 below has a protective film interposed between a metal foil layer and a sealant layer, and uses a sealant layer with high hydrogen sulfide gas permeability. Furthermore, the all-solid-state battery packaging material disclosed in Patent Document 2 uses a sealant layer with low hydrogen sulfide gas permeability. Furthermore, the all-solid-state battery packaging material disclosed in Patent Document 3 uses a gas-absorbing sealant layer. Furthermore, the all-solid-state battery packaging material disclosed in Patent Document 4 is configured by laminating a vapor-deposited film layer on the inner surface of a sealant layer.

[0006] However, the above-mentioned conventional all-solid-state batteries have a problem in that gases such as hydrogen sulfide gas generated by a reaction between the solid electrolyte and water may leak out.

[0007] On the other hand, all-solid-state batteries have a higher resistance and generate more heat than liquid electrolytes because electron (ion) exchange occurs in the solid electrolyte during charging and discharging. However, it is believed that the performance of all-solid-state batteries is not affected even in high-temperature environments, and currently, no consideration has been given to high-temperature countermeasures (cooling performance) including in the above-mentioned Patent Documents 1 to 4. However, as battery technology advances toward higher output and higher capacity, it is fully expected that improved cooling performance will also be required in all-solid-state batteries in the future.

[0008] Therefore, the applicant of the present application has proposed an all-solid-state battery that can prevent leakage of hydrogen sulfide gas and the like while ensuring sufficient cooling performance, as disclosed in Patent Document 5 below.

[0009] In this all-solid-state battery, the exterior material is constructed by sequentially laminating a metal foil layer, a gas barrier layer, and a sealant layer on the inner surface of a base layer, and an opening is formed in the sealant layer to expose the gas barrier layer to the inside. In this all-solid-state battery, the gas barrier layer prevents leakage of hydrogen sulfide gas and the like, while the opening improves cooling performance.

[0010] In this all-solid-state battery, an opening is formed by removing a part (a planned opening portion) of the sealant layer in the packaging sheet in which the sealant layer is laminated over the entire inner surface of the gas barrier layer.

[0011] Japanese Patent No. 6777276 Japanese Patent No. 6747636 JP 2020-187855 JP 2020-187835 WO 2023 / 022087

[0012] However, because the exterior material of an all-solid-state battery is composed of a film-like laminate (laminate sheet), it is difficult to accurately determine the boundary between the portion of the sealant layer to be removed (the intended opening portion) and the portion to be left, and this makes it difficult to properly remove the sealant layer corresponding to the opening, resulting in the problem of difficulty in forming an opening with excellent dimensional accuracy.

[0013] The above describes the issues with all-solid-state batteries, but similar issues may arise in other power storage devices.

[0014] The preferred embodiments of the present invention have been made in light of the above and / or other deficiencies in the related art, and provide significant improvements over existing methods and / or apparatus.

[0015] The present invention has been made in view of the above-mentioned problems, and aims to provide an electricity storage device and an exterior material for an electricity storage device that can reliably form an opening with excellent dimensional accuracy in a sealant layer.

[0016] Other objects and advantages of the present invention will be apparent from the following preferred embodiments.

[0017] In order to solve the above problems, the present invention comprises the following means.

[0018] [1] An electricity storage device comprising an electricity storage device main body and an exterior material for an electricity storage device that exteriors the electricity storage device main body, wherein the exterior material for an electricity storage device comprises a resin base layer, a metal foil layer laminated on the inner surface side of the base layer, a gas barrier layer laminated on the inner surface side of the metal foil layer, and a resin sealant layer laminated on the inner surface side of the gas barrier layer via an adhesive layer, wherein the sealant layer has an opening in a position corresponding to the electricity storage device main body, where no resin for the sealant layer is present, and the adhesive layer has an adhesive-uncoated portion that is provided in correspondence with the opening and where no adhesive is present, and an adhesive-coated portion that is provided in correspondence with portions other than the opening and where adhesive is present, and wherein the adhesive in the adhesive-coated portion is composed of a colored adhesive.

[0019] [2] The electricity storage device according to the preceding paragraph 1, further comprising: a case body provided with a storage section for storing the electricity storage device body; and a closing member attached to the case body in a state of closing an open portion of the storage section, wherein at least one of the case body and the closing member is made of the exterior material for an electricity storage device.

[0020] [3] An exterior packaging material for an electricity storage device used in the electricity storage device described in the preceding item 1 or 2, wherein the sealant layer contains a sealant layer resin and is provided with an intended opening portion that is to become the opening; the adhesive layer is provided with an adhesive-uncoated portion that is provided in correspondence with the intended opening portion and is free of adhesive, and an adhesive-coated portion that is provided in a portion other than the intended opening portion and is free of adhesive; and the adhesive in the adhesive-coated portion is made of a colored adhesive.

[0021] [4] The packaging material for an electricity storage device according to the preceding paragraph 3, wherein the colored adhesive contains a two-component curing adhesive and a colorant, and the colorant contains a pigment or a dye.

[0022] [5] The amount of the colored adhesive applied is 1 g / m 2 ~6g / m 2 5. The packaging material for an electricity storage device according to item 3 or 4, wherein the content of the colorant is 0.1 wt % to 10 wt %.

[0023] [6] The exterior material for an electricity storage device according to any one of items 3 to 5, wherein the exterior material is configured so that the relationship |La - Lb| ≧ 0.5 holds, where "La" is the L value of an adhesive-coated portion measured from the inner surface side of the sealant layer, and "Lb" is the L value of an adhesive-uncoated portion.

[0024] [7] An opening-equipped exterior material for an electricity storage device, formed by removing the sealant layer at the intended opening portion in the exterior material for an electricity storage device according to any one of items 3 to 6 above.

[0025] According to the electricity storage devices of inventions [1] and [2], in the adhesive layer between the heat-resistant gas barrier layer and the sealant layer in the exterior packaging material, an adhesive-uncoated portion where no adhesive is applied is formed at the opening, and an adhesive-coated portion where a colored adhesive is applied is formed in the portion other than the opening. Therefore, when forming an opening by removing a portion of the sealant layer, the position of the boundary between the adhesive-coated portion and the adhesive-uncoated portion can be accurately grasped from the color difference due to the presence or absence of the colored adhesive, and the sealant layer can be partially excised accurately along the boundary position, thereby forming an opening with high precision.

[0026] According to the packaging material for an electricity storage device of the invention [3], similarly to the above, openings can be formed in the sealant layer with high precision.

[0027] According to the packaging materials for an electricity storage device of the inventions [4] to [6], the adhesive-coated portion and the adhesive-uncoated portion can be more clearly distinguished, and the above-mentioned effects can be more reliably obtained.

[0028] According to the packaging material with an opening for an electricity storage device of the invention [7], similarly to the above, it is possible to form an opening with high precision in the sealant layer.

[0029] FIG. 1 is a schematic cross-sectional view showing an all-solid-state battery as an electricity storage device according to an embodiment of the present invention. FIG. 2 is a schematic cross-sectional view showing an enlarged view of a main portion of FIG. 1. FIG. 3 is an exploded perspective view showing a schematic all-solid-state battery according to an embodiment. FIG. 4 is a schematic cross-sectional view showing an exterior material for a case body in an all-solid-state battery according to an embodiment. FIG. 5 is a schematic inner view showing an exterior material according to an embodiment. FIG. 6 is a schematic cross-sectional view for explaining a method of forming an opening in an exterior material according to an embodiment. FIG. 7 is a schematic cross-sectional view showing a mold device for molding a case body using an exterior material with an opening according to an embodiment. FIG. 8 is a schematic cross-sectional view showing an all-solid-state battery according to a first modified example of the present invention. FIG. 9 is a schematic cross-sectional view showing an all-solid-state battery according to a second modified example of the present invention. FIG. 10 is a schematic cross-sectional view showing an all-solid-state battery according to a third modified example of the present invention. FIG. 11 is a schematic cross-sectional view showing an all-solid-state battery according to a fourth modified example of the present invention.

[0030] Fig. 1 is a schematic cross-sectional view showing an all-solid-state battery as an electricity storage device according to an embodiment of the present invention, Fig. 2 is a schematic cross-sectional view showing an enlarged view of a main part of Fig. 1, and Fig. 3 is an exploded perspective view showing a schematic view of the all-solid-state battery according to the embodiment. As shown in these figures, the all-solid-state battery according to this embodiment includes a case body 3 and a closing member 4 as a casing, and an all-solid-state battery body 5 housed and sealed in the casing.

[0031] 4 is a schematic cross-sectional view showing an exterior material 1 constituting the case body 3 of an all-solid-state battery according to an embodiment. As shown in the figure, the exterior material 1 includes a base material layer 11 disposed on the outermost side, a metal foil layer 12 laminated and bonded to the inner surface of the base material layer 11 via a first adhesive layer (not shown), a heat-resistant gas barrier layer 13 laminated and bonded to the inner surface of the metal foil layer 12 via a second adhesive layer (not shown), and a sealant layer 15 laminated and bonded to the inner surface of the heat-resistant gas barrier layer 13 via a third adhesive layer 14. In the present invention, when describing the positions of the layers constituting the exterior material 1 in terms of directions, the direction toward the base material layer 11 (upper side in FIG. 3 ) is referred to as the outside, and the direction toward the sealant layer 15 (lower side in FIG. 3 ) is referred to as the inside.

[0032] The exterior material 1 constituting the blocking member 4 also has the same structure as the exterior material 1 constituting the case body 3 described above.

[0033] The case body 3 is formed from a molded exterior material 1 and integrally includes a top wall 31, a side wall (circumferential side wall) 32 extending downward from the outer periphery of the top wall 31, and a flange 33 provided on the outer periphery of the lower end of the side wall 32. A storage section 35 is formed inside the top wall 31 and the side wall 32. The closing member 4 is formed from the sheet-like exterior material 1. The all-solid-state battery body 5 is housed in the storage section 35 of the case body 3, and the closing member 4 is arranged to close the open lower end of the storage section 35. The closing member 4 is arranged with its sealant layer 15 facing inward (upward), and the sealant layer 15 of the flange 33 of the case body 3 and the sealant layer 15 of the outer periphery of the closing member 4 are overlapped and face each other. The overlapped sealant layers 15 are joined together by thermal bonding (heat sealing) to form an all-solid-state battery in which the all-solid-state battery body 5 is housed in a sealed state within the casing (the case body 3 and the closing member 4).

[0034] Furthermore, the case body 3 of the all-solid-state battery has an opening 2 formed in a portion corresponding to the accommodation portion 35, where the resin constituting the sealant layer 15 and the adhesive constituting the adhesive layer 14 are not present. Furthermore, the closing member 4 also has an opening 2 formed in a portion corresponding to the accommodation portion 35, where the resin for the sealant layer and the adhesive for the adhesive layer are not present. Through the opening 2 in the case body 3 and the closing member 4, the heat-resistant gas barrier layer 13 of the exterior material 1 is exposed inside the accommodation portion 35 and is disposed so as to face the all-solid-state battery body 5.

[0035] Furthermore, in the all-solid-state battery of this embodiment, a tab lead (not shown) is provided for taking out electricity. One end (inner end) of this tab lead is adhesively fixed to the all-solid-state battery body 5, and the middle part is arranged so as to pass through the heat-sealed part between the flange 33 of the case body 3 and the outer peripheral edge part of the closing member 4, and the other end side is drawn out to the outside.

[0036] Each part of the all-solid-state battery of this embodiment will be described in detail below.

[0037] The base material layer 11 of the packaging material 1 is made of a heat-resistant resin film having a thickness of 5 μm to 50 μm. Suitable resins that can be used to make up this base material layer 11 include oriented polyamide film, oriented polyester (PET, PBT, PEN, etc.), and oriented polyolefin (PE, PP, etc.).

[0038] The metal foil layer 12 has a thickness set to 5 μm to 120 μm and has the function of blocking the penetration of oxygen and moisture from the surface (outer surface) side. Aluminum foil, SUS foil (stainless steel foil), copper foil, nickel foil, etc. can be suitably used as this metal foil layer 12. In this embodiment, the terms "aluminum," "copper," and "nickel" are used to mean alloys thereof.

[0039] Furthermore, if the metal foil layer 12 is subjected to a plating process or the like, the risk of pinholes occurring is reduced, and the function of blocking the penetration of oxygen and moisture can be further improved.

[0040] Furthermore, if the metal foil layer 12 is subjected to a chemical conversion treatment such as chromate treatment, the corrosion resistance is further improved, so that defects such as chipping can be more reliably prevented, and the adhesion to the resin can be improved, thereby further improving durability.

[0041] The sealant layer (heat-sealable resin layer) 15 has a thickness of 20 μm to 100 μm and is made of a film of heat-adhesive (heat-sealable) resin. Suitable resins for the sealant layer 15 include polyethylene (LLDPE, LDPE, HDPE), polyolefins such as polypropylene, cyclic polyolefins, olefin copolymers, acid-modified products thereof, and ionomers, such as non-oriented polypropylene (CPP, IPP).

[0042] Considering that electricity is extracted using a tab lead, that is, in consideration of sealing properties and adhesiveness with the tab lead, it is preferable to use a polypropylene-based resin (non-oriented polypropylene film (CPP, IPP)) as the sealant layer 15.

[0043] The heat-resistant gas barrier layer 13 is made of a heat-resistant and insulating resin film. Suitable resins for the heat-resistant gas barrier layer 13 include polyamides (such as 6-nylon, 66-nylon, and MXD nylon), polyesters (PET, PBT, and PEN), polyvinylidene chloride (PVDC), polyethylenes (LLDPE, LDPE, and HDPE), polyolefins such as polypropylene (CPP and OPP), olefin copolymers, acid-modified products thereof, and ionomers.

[0044] In this embodiment, the thickness of the heat-resistant gas barrier layer 13 is preferably set to 3 μm to 50 μm, and more preferably to 10 μm to 40 μm. That is, when the thickness of the heat-resistant gas barrier layer 13 is set within this range, the hydrogen sulfide gas and water vapor gas permeation suppression effect can be reliably obtained, and even if the sealant layer 15 melts and flows out due to thermal adhesion, the heat-resistant gas barrier layer 13 can reliably ensure insulation. In other words, if the heat-resistant gas barrier layer 13 is too thin, there is a risk that the gas permeation suppression effect and insulation property cannot be ensured, which is undesirable. Conversely, if the heat-resistant gas barrier layer 13 is too thick, not only will it be impossible to thin the packaging material 1, but the full effect of making the layer thicker than necessary will also be undesirable.

[0045] In this embodiment, it is preferable to use a resin film as the heat-resistant gas barrier layer 13. That is, the entire film serves as a barrier layer, and therefore, unlike a vapor-deposited film or the like, no barrier cracks occur, and the barrier properties can be improved.

[0046] Furthermore, a non-stretched film or a stretched film can be used as the resin film constituting the heat-resistant gas barrier layer 13, and it is particularly preferable to use a stretched film. That is, when a stretched film is used, the heat resistance, insulating properties, formability, and gas barrier properties can be further improved.

[0047] The heat-resistant gas barrier layer 13 of the present embodiment has good insulating properties, and maintains good insulating properties even after the all-solid-state battery body 5 is enclosed (sealed) with the case body 3 and the closing member 4 as the exterior material 1 of the present embodiment.

[0048] In this embodiment, the resin constituting the heat-resistant gas barrier layer 13 has a water vapor permeability of 50 (g / m) or less, as measured in accordance with JIS K7129-1 (humidity sensor method, 40°C, 90% Rh). 2 It is preferable to adjust the water vapor transmission rate to 50 (g / m 2 / day) or less, the gas permeation prevention effect of the heat-resistant gas barrier layer 13 can prevent the intrusion of moisture such as water vapor gas from the outside, thereby suppressing the generation of hydrogen sulfide gas due to a reaction between moisture and the solid electrolyte, and more reliably preventing the leakage of hydrogen sulfide gas and the like.

[0049] In this embodiment, it is preferable to use a resin having a thermal conductivity of 0.2 W / m·K or more as the resin constituting the heat-resistant gas barrier layer 13. That is, when this configuration is used, the heat conductivity of the heat-resistant gas barrier layer 13 can be sufficiently ensured, and the cooling performance of the all-solid-state battery body 5 can be further improved.

[0050] Furthermore, in this embodiment, it is preferable to use a resin constituting the heat-resistant gas barrier layer 13 that has a melting point 10°C or more higher than that of the resin constituting the sealant layer 15. In other words, if the heat-resistant gas barrier layer 13 has a high melting point, there will be no change in the thickness of the heat-resistant gas barrier layer 13 during heat sealing after the solid state battery is housed, and the water vapor permeation prevention function of the heat-resistant gas barrier layer 13 can be well maintained, making it possible to more reliably suppress the generation of hydrogen sulfide gas. In this embodiment, the melting point is measured as the melting peak temperature of DSC measured in accordance with JIS K7121-1987.

[0051] In this embodiment, two-component curing dry lamination adhesives such as polyurethane adhesives, acrylic adhesives, polyacrylate adhesives, modified polypropylene adhesives, polyester adhesives, polyamide adhesives, and epoxy adhesives can be suitably used for the first adhesive layer that bonds the base material layer 11 and the metal foil layer 12, the second adhesive layer that bonds the metal foil layer 12 and the heat-resistant gas barrier layer 13, and the third adhesive layer 14 that bonds the heat-resistant gas barrier layer 13 and the sealant layer 15. The thicknesses of these first to third adhesive layers are preferably set to 1 μm to 6 μm.

[0052] In this embodiment, the adhesive constituting the third adhesive layer 14 between the heat-resistant gas barrier layer 13 and the sealant layer 15 is a colored adhesive obtained by adding a coloring agent made of a pigment or dye to the above-mentioned adhesive. As a result, in the exterior material 1 before the opening 2 is formed, as will be described later, the adhesive-uncoated portion 14b (opening portion 2a) where no adhesive is present and the adhesive-coated portion 14a where the colored adhesive is present can be clearly distinguished by the color difference caused by the presence or absence of the colored adhesive.

[0053] Colored adhesives are the two-component curing adhesives described above that contain colorants. Colorants are generally classified into dyes that are soluble in solvents such as water and oil, and pigments that are not soluble in solvents such as water and oil.

[0054] Examples of dyes classified by chemical structure include azo dyes having an azo group (—N═N—) in the molecule, anthraquinone dyes having an anthraquinone skeleton in the molecule, and indigoid dyes such as indigo, thioindigo, and derivatives thereof.

[0055] Pigments are classified into inorganic and organic pigments. Inorganic pigments include various oxides, sulfides, and ferrocyanide compounds, such as white pigments (titanium oxide, zinc oxide, and zinc-containing calcined hydrotalcite), red pigments (iron oxide red), blue pigments (ferrocyanide Prussian blue), and black pigments (carbon black).

[0056] Furthermore, some pigments are not only used for coloring but also for special purposes. For example, aluminum oxide, which is a white pigment, is sometimes used as a moisture absorbent. When zinc-containing calcined hydrotalcite is added as a white pigment to an adhesive, it absorbs hydrogen sulfide gas generated when a sulfide all-solid-state battery reacts with moisture, suppressing the leakage of hydrogen sulfide gas to the outside of the battery, and it is also possible to absorb water vapor entering from outside the battery and suppress the generation of hydrogen sulfide gas.

[0057] On the other hand, organic pigments include azo pigments, phthalocyanine pigments, perylene pigments, quinacridone pigments, etc. Azo pigments are yellow to red coloring materials and are widely used for plastics, while phthalocyanine pigments are blue and green coloring materials and are used for plastics and inks.

[0058] In this embodiment, of the pigment and the dye, the pigment is more advantageous in terms of weather resistance, solvent resistance, and heat resistance, and it is even more preferable to use the pigment as the colorant.

[0059] In this embodiment, it is preferable to adjust the colorant content of the colored adhesive to 0.1 wt% to 10 wt%. That is, if this content is 0.1 wt% or more, the boundary between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b can be clearly seen when the exterior packaging material 1 is viewed from the inside, and the opening 2 can be formed with high precision. Note that even if the colorant content exceeds 10 wt%, there is no particular effect commensurate with that content and in some cases there is a risk of increased costs, so it is preferable to adjust it to 10 wt% or less.

[0060] Furthermore, the coating amount of the colored adhesive in the adhesive coating portion 14a of the third adhesive layer 14 is set to 1 g / m 2 ~6g / m 2 It is preferable to adjust the coating amount to 1 g / m. 2 In the above case, when the exterior packaging material 1 is viewed from the inside, the boundary between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b can be clearly seen, and the opening 2 can be formed with high precision. 2 Even if the amount exceeds 6 g / m, there is no particular effect commensurate with the amount applied, and in some cases there is a risk of increased costs. 2 It is preferable to adjust as follows:

[0061] In the present embodiment, the second adhesive layer that bonds the metal foil layer 12 and the heat-resistant gas barrier layer 13 can be formed by using an adhesive resin (a polyolefin-based resin such as polyolefin, carboxylic acid-modified polyolefin, or metal-modified polyolefin, a polyvinyl acetate-based resin, a (meth)acrylic resin, or an amino resin) instead of an adhesive, and laminating the adhesive resin and the resin that forms the heat-resistant gas barrier layer 13 onto the metal foil layer 12 by co-extruding them (extrusion lamination method), or by forming a laminate in which the adhesive resin and the heat-resistant gas barrier layer 13 are laminated in advance, and laminating this laminate on the metal foil layer 12 by thermal lamination, or by pouring a molten adhesive resin between the metal foil layer 12 and the heat-resistant gas barrier layer 13 while bonding the metal foil layer 12 and the heat-resistant gas barrier layer 13 together (sand lamination method).

[0062] In this embodiment, the opening 2 on the case body 3 side has its outer peripheral edge 21 provided on the flange 33 of the case body 3. Furthermore, the opening 2 on the closing member 4 side has its opening edge 21 formed to correspond to the opening edge 21 of the opening 2 of the case body 3.

[0063] In the present embodiment, the opening 2 formed in the case body 3 and the closing member 4 is not provided with the colored adhesive that constitutes the adhesive layer 14, and the heat-resistant gas barrier layer 13 is exposed (exposed) to the inside through the opening 2, and in a state where the all-solid-state battery is fabricated, the heat-resistant gas barrier layer 13 is disposed so as to face the upper surface, peripheral side surface, and lower surface of the all-solid-state battery body 5.

[0064] Next, a method for manufacturing the exterior material 1 in this embodiment will be described. Needless to say, in the present invention, the method for manufacturing the exterior material 1 is not limited (the same applies to the method for manufacturing the case body 3 and the method for manufacturing the all-solid-state battery, which will be described later).

[0065] In this embodiment, first, a laminate without a sealant layer is produced by, for example, a dry lamination method. That is, a resin film for the base layer 11 is bonded via an adhesive to the outer surface of a metal foil for the metal foil layer 12, which has been subjected to a surface treatment and a chemical conversion treatment as necessary, and a resin film for the heat-resistant gas barrier layer 13 is bonded via an adhesive to the inner surface of the metal foil, thereby producing a laminate without a sealant layer, in which the metal foil layer 12 and the heat-resistant gas barrier layer 13 are laminated on the inner surface side of the base layer 11.

[0066] It should be noted that when producing a laminate without a sealant layer, it is also possible to produce it by a method other than the dry lamination method, such as the extrusion lamination method, as described above. For example, the above laminate may be produced by extruding and laminating the resin composition for the base layer 11 and the resin composition for the heat-resistant gas barrier layer 13 onto the inner and outer surfaces of a metal foil, respectively.

[0067] Next, the adhesive (colored adhesive) that constitutes the adhesive layer 14 is applied to the inner surface of the above-mentioned sealant layer-free laminate (the inner surface of the heat-resistant gas barrier layer 13) using a gravure roll or the like. During this application, the adhesive is applied to the inner surface of the heat-resistant gas barrier layer 13, except for the portion where the opening 2 in the sealant layer 15 is to be formed (planned opening portion 2a), to form an adhesive-coated portion 14a, while the adhesive is not applied to the portion corresponding to the planned opening portion 2a, to form an adhesive-uncoated portion 14b.

[0068] Then, a resin film for a sealant layer is attached to the inner surface of the heat-resistant gas barrier layer 13 having the adhesive-uncoated portion 14b via the adhesive layer 14, and is then dried. The resin film for a sealant layer is also provided in the portion corresponding to the adhesive-uncoated portion 14b.

[0069] As shown in FIG. 5, the exterior material 1 obtained in this manner has the adhesive-coated portion 14a (shown by diagonal hatching in the same figure) colored with a colored adhesive, and therefore the color difference (difference in brightness, etc.) between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b (planned opening portion 2a) makes the boundary between the two portions 14a, 14b clear.

[0070] 6, the area between the adhesive-coated portion 14a and the intended opening portion 2a is cut away, and the intended opening portion 2a, which is the sealant layer 15 of the adhesive-uncoated portion 14b, is cut away to form the opening 2. This cutting method can be performed using a laser cutter, a roll blade, a punching blade (such as a Thomson blade or an etching blade), an ultrasonic cutter, or the like. Of these, it is preferable to use a laser cutter, which can perform processing with high precision.

[0071] In this embodiment, as shown in FIG. 5, the opening 2 can be formed by automatically cutting out the sealant layer 14 at the intended opening portion 2a using an opening position detection device and a laser cutting device 82.

[0072] That is, the opening position detection device 81 detects the boundary position between the adhesive coated portion 14a and the adhesive uncoated portion 14b, and is provided with, for example, a detection sensor that detects the amount of reflected light of light irradiated onto the subject from a light source, and detects the boundary position between the adhesive coated portion 14a and the adhesive uncoated portion 14b based on the difference in the amount of light, etc. 2 The opening position detecting device 82 is configured with a laser cutting device or the like, and based on position information from the opening position detecting device 81, cuts the boundary position between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b, i.e., the outer peripheral edge portion 21a of the intended opening portion 2a, and cuts away the sealant layer 15 of the intended opening portion 2a to form the opening 2. In this way, the opening 2 is automatically formed in the exterior packaging material 1, and an exterior packaging material with an opening is manufactured. Therefore, by using the opening position detecting device 81 and the laser cutting device 82, the opening 2 can be automatically formed in the exterior packaging material 1, and an exterior packaging material with an opening can be manufactured.

[0073] In the exterior packaging material 1 before the opening 2 of this embodiment is formed, when the L value, which is the lightness of the adhesive-coated portion 14a measured from the sealant layer 15 side (inner surface side), is "La" and the L value, which is the lightness of the adhesive-uncoated portion 14b, is "Lb," it is preferable to set the absolute value of ΔL (lightness difference), which is the absolute value of the difference between La and Lb, to 0.5 or more. In other words, it is preferable to configure it so that the relationship |La - Lb| = |ΔL| ≧ 0.5 holds.

[0074] In other words, when the above relational expression is satisfied, the brightness difference ΔL between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b is large, so the boundary position between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b can be properly captured, and a highly accurate opening 2 can be formed.

[0075] However, in the present invention, the color difference (boundary position) between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b may be detected by a color difference other than a difference in brightness, such as a difference in hue or a difference in saturation.

[0076] Next, we will explain how to mold the sheet-like exterior material with an opening obtained as described above to produce the case body 3. First, as shown in Figure 6, the sheet-like exterior material 1 for the case body before molding includes a planned top wall portion 31a that is the portion intended to become the top wall 31, a planned side wall portion 32a that is the portion intended to become the side wall 32, and a planned flange portion 33a that is the portion intended to become the flange 33.

[0077] In this embodiment, the outer peripheral edge 21a of the intended opening portion 2a is set within the range of the intended flange portion 33a.

[0078] 7 is a schematic cross-sectional view showing a mold device for molding the case body 3 using the opening-equipped exterior material 1. As shown in the figure, this mold device includes a die 6 as an upper mold, and a punch 7 and a blank holder 70 as a lower mold.

[0079] The die 6 has a molding recess 65 formed on the lower surface thereof for molding the housing portion 35 (top wall 31 and side wall 32 ) of the case body 3 .

[0080] The punch 7 is disposed in correspondence with the forming recess 65 of the die 6 , and the blank holder die 70 is disposed on the outer periphery of the punch 7 and faces the outer periphery of the lower surface of the die 6 .

[0081] The opening-equipped exterior material 1 serving as the molding material is then placed so that its planned sidewall portion 32a corresponds to the outer peripheral edge of the tip of the punch 7. In this state, the planned flange portion 33a of the exterior material 1 is sandwiched and supported by the outer periphery of the die 6 and the blank holder die 70, and the punch 7 is driven into the molding recess 65 of the die 6, thereby pressing the exterior material 1. This produces a case body molded body (molding material) having a housing portion 35 (top wall 31 and side wall 32) and a flange 33 outside the housing portion 35. The flange 33 of this molded body is then cut to a predetermined size, thereby producing the case body 3 of this embodiment. In this case body 3, the opening 2 is disposed over the entire area of ​​the housing portion 35, and the outer peripheral edge 21 of the opening 2 is disposed on the flange 33, as shown in FIGS. 1 to 3 .

[0082] 1 to 3 , in this embodiment, an all-solid-state battery is produced by packaging a solid-state battery body 5 using the case body 3 and the sheet-like closing member 4. That is, the all-solid-state battery body 5 is housed in the housing portion 35 of the case body 3, and the closing member 4 is arranged so as to close the housing portion 35 from below, and the sealant layer 15 of the flange 33 of the case body 3 and the sealant layer 15 of the outer peripheral edge of the closing member 4 are arranged so as to face each other and overlap. In this state, the flange 33 of the case body 3 and the outer peripheral edge of the closing member 4 are sandwiched between a pair of sealing dies and heated. As a result, the overlapping sealant layers 15 are heat-sealed and joined together, and an all-solid-state battery is produced in which the all-solid-state battery body 5 is housed in an airtight state within the case body 3 and the closing member 4.

[0083] According to the all-solid-state battery of the present embodiment having the above-described configuration, the heat-resistant gas barrier layer 13 is provided between the metal foil layer 12 and the sealant layer 15 in the case body 3 and the closing member 4, and the opening 2 is formed in the top wall 31 and the side wall 32 by removing a part of the sealant layer 15. Therefore, heat generated from the all-solid-state battery body 5 is efficiently transferred to the metal foil layer 12 via the opening 2 and the heat-resistant gas barrier layer 13 and dissipated without being blocked by the sealant layer 15, thereby ensuring sufficient heat dissipation and cooling properties.

[0084] In particular, in the present embodiment, the outer peripheral edge 21 of the opening 2 in the case body 3 is set to the flange 33 of the case body 3, so that a large opening 2 can be formed that corresponds to almost the entire area of ​​the all-solid-state battery body 5, and heat dissipation and cooling properties can be further improved.

[0085] Furthermore, in the adhesive layer 14 between the heat-resistant gas barrier layer 13 and the sealant layer 15 in the exterior material 1 of this embodiment, an adhesive-uncoated portion 14b where no adhesive is applied is formed in the planned opening portion 2a, and an adhesive-coated portion 14a is formed in the portions other than the planned opening portion 2a by applying a colored adhesive. Therefore, the boundary position between the adhesive-coated portion 14a and the adhesive-uncoated portion 14b can be accurately grasped from the color difference caused by the presence or absence of the colored adhesive, and the sealant layer 15 can be accurately cut along the boundary position (the outer peripheral edge portion 21a of the planned opening portion 2a) using a laser cutter or the like, and the opening 2 can be formed with high precision.

[0086] In particular, in this embodiment, when the brightness difference |La-Lb| between the adhesive-coated portion 15a and the adhesive-uncoated portion 15b is adjusted to 0.5 or more, the boundary position between the two portions 14a, 14b can be captured more accurately, and an opening 2 with even higher dimensional accuracy can be formed.

[0087] Furthermore, according to the all-solid-state battery of this embodiment, since the heat-resistant gas barrier layer 13 is disposed on the inner surface side of the metal foil layer 12, even if the solid electrolyte of the all-solid-state battery body 5 reacts with moisture in the outside air to generate hydrogen sulfide gas or the like, leakage of the gas can be reliably prevented by the heat-resistant gas barrier layer 13. Furthermore, the gas permeation prevention action of the heat-resistant gas barrier layer 13 can prevent the intrusion of moisture such as water vapor gas from the outside, and therefore the generation of hydrogen sulfide gas itself due to the reaction between the moisture and the solid electrolyte can also be suppressed, making it possible to more reliably prevent leakage of hydrogen sulfide gas or the like.

[0088] Furthermore, in the all-solid-state battery of this embodiment, in the portion where the opening 2 is formed, although the sealant layer 15 is not present between the all-solid-state battery body 5 and the metal foil layer 12, the heat-resistant gas barrier layer 13 having insulating properties is disposed therebetween, and therefore, the heat-resistant gas barrier layer 13 can reliably ensure insulation.

[0089] Furthermore, when cutting the exterior packaging material 1 with a laser cutter or the like to form the opening 2, laser damage may be formed in the outer peripheral edge 21 of the opening, which may result in defects such as cracks or pinholes. However, in this embodiment, the outer peripheral edge 21 of the opening is formed in the flange 33 of the case body 3, so that the adverse effects of the damaged area can be avoided. That is, the flange 33 of the molded body 3 is heat-sealed, and a resin reservoir formed by the heat sealing is formed in the damaged area (the outer peripheral edge 21 of the opening). Therefore, the damaged area can be covered and repaired by the resin reservoir, so that the adverse effects of the damaged area due to laser cutting can be reliably avoided.

[0090] Furthermore, in the all-solid-state battery of this embodiment, the sealant layer 15 is not formed in the portion of the exterior packaging material 1 that corresponds to the all-solid-state battery body 5, and therefore, the space for accommodating the all-solid-state battery body 5 can be made larger (thicker) accordingly. Therefore, in the all-solid-state battery of this embodiment, compared to conventional all-solid-state batteries, a larger-sized all-solid-state battery body 5 can be accommodated without changing the external dimensions of the case body 3, and therefore, high output and high capacity can be achieved while achieving a thinner design.

[0091] Furthermore, in the all-solid-state battery of this embodiment, the sealant layer 15 is provided on the flange 33 provided around the entire periphery of the case body 3, and therefore the sealant layer 15 provided around the entire periphery can reliably seal the entire periphery of the all-solid-state battery, ensuring good sealing performance.

[0092] In the all-solid-state battery of the above embodiment, the case where the opening 2 is formed in both the case body 3 and the closing member 4 has been described as an example, but the present invention is not limited to this. As shown in FIG. 8 , the opening 2 may be formed in the case body 3, and the opening 2 may not be formed in the closing member 4.

[0093] In addition, the all-solid-state battery of this embodiment shown in FIG. 1 is arranged so that the case body 3 is disposed on the upper side and the blocking member 4 is disposed on the lower side, but this is not limited thereto. In the present invention, the all-solid-state battery shown in FIG. 1 may be inverted, that is, the case body 3 which is a molded body is disposed on the lower side and the sheet-like blocking member 4 is disposed on the upper side.

[0094] In the above embodiment, the edge 21 of the opening 2 is set within the flange 33, but the present invention is not limited to this. For example, in the present invention, the edge 21 of the opening 2 may be set in the side wall 32 of the case body 3 as shown in Fig. 9, or the edge 21 of the opening 2 may be set in the top wall (bottom wall) 33 of the case body 3 as shown in Fig. 10. In other words, the shape and size of the opening 2 are not particularly limited in the present invention.

[0095] Furthermore, in the present invention, a molded body may be used as the blocking member 4. For example, as shown in Fig. 11 , a tray-shaped molded body having a shape obtained by inverting the case body 3 upside down may be used as the blocking member 4, and the casing of the all-solid-state battery may be formed by the case body 3 which is a molded body and the tray-shaped blocking member 4 which is also a molded body. In this case, by using a similar configuration for the blocking member 4 as the case body 3, the same effect can be obtained with the blocking member 4.

[0096] In the above embodiment, a case has been described in which an all-solid-state battery is used as the electricity storage device of the present invention, but the present invention is not limited to this, and can also be applied to electricity storage devices other than all-solid-state batteries.

[0097]

[0098] The abbreviations in Table 1 are as follows: TDI: toluene diisocyanate, TMP: trimethylolpropane, HDI: hexamethylene diisocyanate, HT: zinc-containing calcined hydrotalcite [(Mg / Zn) 0.8. Al 0.2 (OH) 2 ] 0.2 (CO 3) 0.2 CB: Carbon Black Example 1 As shown in Table 1, the inner structure of the sample (exterior material) was as follows: a 40 μm-thick aluminum foil (JIS H4160 A8021-O) was used as the metal foil layer; a 12 μm-thick matte PET (polyethylene terephthalate) film was laminated to the inner surface (erased side) as the heat-resistant gas barrier layer via a two-component curing polyester-urethane adhesive as the second adhesive layer. Furthermore, an 80 μm-thick CPP (non-oriented polypropylene) film was laminated to the inner surface of the heat-resistant gas barrier layer as the sealant layer using a colored adhesive as the third adhesive layer. The third adhesive layer was not applied to the intended opening area. The uncoated area (intended opening area) was a rectangle measuring 100 mm x 200 mm (see Figures 4 and 5).

[0099] The colored adhesive used as the third adhesive layer was an adhesive containing polyester polyol as the base resin and an adduct of TDI and TMP as the curing agent, to which 0.2 wt% of CB having a particle size of 0.4 μm was added as a colorant. The amount of the colored adhesive applied was 2 g / m. 2 is.

[0100] Although not shown in the table, the outer structure of the sample is such that a 25 μm thick stretched nylon film (ONY) is laminated to the outer surface (glossy surface) of the metal foil layer 12 via a two-component curing polyester-urethane adhesive (first adhesive layer) (the same applies to Examples 2 to 10 and Comparative Examples 1 and 2).

[0101] The laminated film thus obtained was laminated with each layer, and then cured at 40° C. for 5 days to prepare 50 sheets of samples (exterior packaging materials) of Example 1.

[0102] Examples 2 to 7 and Comparative Examples 1 and 2 Using the materials shown in Table 1, 50 samples (exterior materials) with uncoated adhesive portions were produced for each of Examples 2 to 7 and Comparative Examples 1 and 2 in the same manner as in Example 1 above.

[0103] In the samples of Comparative Examples 1 and 2, no colorant was added to the adhesive constituting the third adhesive layer.

[0104] <Evaluation of L value and detectability>

[0105]

[0106] As shown in Table 2, for 50 sheets of each sample from each of the above Examples and Comparative Examples, the L value (Lb) of the adhesive-uncoated area (area to be opened) and the L value (La) of the adhesive-coated area were measured from the inside using a Konica Minolta spectrophotometer (CM-2500c), and the average value of the lightness difference (|ΔL| = |La - Lb|) between the adhesive-uncoated area and the adhesive-coated area was calculated. The results are shown in Table 2.

[0107] In addition, for 50 samples of each of the above examples and comparative examples, an opening forming device consisting of an opening position detection device and a laser cutting device was used to remove the sealant layer from the intended opening area (area where adhesive was not applied).

[0108] The opening position detection device used was an MR101 scanning head manufactured by Nireco Corporation. This detection device uses an LED as a light source, and an SPD (silicon photodiode) receives the difference in the amount of light reflected from the colored adhesive-uncoated area and the colored adhesive-coated area, and detects the outer periphery of the colored adhesive-uncoated area (the area to be opened) based on a mechanism that outputs a voltage proportional to the amount of light.

[0109] The laser cutting equipment is CO 2 A laser cutting device was used, which cut and removed only the sealant layer (CPP film) on the colored adhesive-uncoated area based on the position information of the colored adhesive-uncoated area (planned opening area) in the center of each sample detected by the opening position detection device, to create an exposed area (opening) of the heat-resistant gas barrier layer (matte PET film) measuring 100 mm wide x 200 mm long.

[0110] In Table 2, with regard to the detectability of the adhesive-uncoated areas, "○" indicates that the outer peripheral position of the adhesive-uncoated areas could be accurately detected in all 50 samples, and openings could be formed with high precision; "△" indicates that the adhesive-uncoated areas could not be detected in only one location out of the 50 samples, and an opening could not be formed; and "×" indicates that the outer peripheral position of the adhesive-uncoated areas could not be sufficiently detected, and an opening could not be formed.

[0111] As is clear from Table 2, the samples of Examples 2 to 10 had large ΔL, the difference between the adhesive-uncoated area and the adhesive-coated area was clear, and the adhesive-uncoated area (the area to be opened) could be cut out with high precision. Note that although the ΔL of the sample of Example 1 was somewhat small, it was basically possible to detect the adhesive-uncoated area, and it is believed that an opening can be formed without any problems in practical use.

[0112] In contrast, the samples of Comparative Examples 1 and 2 had a small ΔL, making the difference between the adhesive-uncoated area and the adhesive-coated area unclear, and the opening position detection device was unable to accurately detect the outer periphery of the adhesive-uncoated area, making it impossible to cut out the intended opening area.

[0113] This application claims priority from Japanese Patent Application No. 2023-86465, filed on May 25, 2023, the disclosure of which is incorporated herein by reference in its entirety.

[0114] It should be understood that the terms and expressions used herein are used for the purpose of explanation and not for limiting interpretation, and do not exclude any equivalents of the features shown and described herein, but also allow various modifications within the claimed scope of the present invention.

[0115] The exterior packaging material for an electricity storage device of the present invention can be suitably used as a material for a battery case (casing) for accommodating an all-solid-state battery main body such as an all-solid-state battery.

[0116] 1: Exterior material 11: Base material layer 12: Metal foil layer 13: Heat-resistant gas barrier layer 14: Adhesive layer (third adhesive layer) 14a: Adhesive-coated portion 14b: Adhesive-uncoated portion 15: Sealant layer 2: Opening 2a: Pre-opening portion 3: Case body 35: Storage portion 4: Closing member 5: All-solid-state battery body La: L value of adhesive-coated portion Lb: L value of adhesive-uncoated portion

Claims

1. An electricity storage device comprising an electricity storage device main body and an exterior material for an electricity storage device that exteriors the electricity storage device main body, wherein the exterior material for an electricity storage device comprises a resin base layer, a metal foil layer laminated on the inner surface side of the base layer, a gas barrier layer laminated on the inner surface side of the metal foil layer, and a resin sealant layer laminated on the inner surface side of the gas barrier layer via an adhesive layer, wherein the sealant layer has an opening at a position corresponding to the electricity storage device main body, where no resin for the sealant layer is present, and wherein the adhesive layer has an adhesive-uncoated portion corresponding to the opening and where no adhesive is present, and an adhesive-coated portion corresponding to a portion other than the opening and where adhesive is present, and wherein the adhesive in the adhesive-coated portion is composed of a colored adhesive.

2. The energy storage device according to claim 1, comprising a case body having a storage section in which the energy storage device main body is housed, and a blocking member attached to the case body so as to block the open portion of the storage section, wherein at least one of the case body and the blocking member is made of the exterior material for the energy storage device.

3. An exterior material for an electricity storage device used in the electricity storage device described in claim 1 or 2, characterized in that the sealant layer has a sealant layer resin present and is provided with a planned opening portion that is to become the opening, the adhesive layer has an adhesive-uncoated portion that is provided in correspondence with the planned opening portion and where no adhesive is present, and an adhesive-coated portion that is provided in a portion other than the planned opening portion and where adhesive is present, and the adhesive in the adhesive-coated portion is composed of a colored adhesive.

4. The exterior material for an electricity storage device according to claim 3, wherein the colored adhesive comprises a two-component curing adhesive and a colorant, and the colorant comprises a pigment or a dye.

5. The coating amount of the colored adhesive is 1 g / m 2 ~6g / m 2 The packaging material for an electricity storage device according to claim 3 or 4, wherein the content of the colorant is 0.1 wt % to 10 wt %.

6. The exterior material for an electricity storage device according to any one of claims 3 to 5, wherein the L value of the adhesive-coated portion measured from the inner surface side of the sealant layer is "La" and the L value of the adhesive-uncoated portion is "Lb", so that the following relationship holds: |La-Lb|≧0.

5.

7. An opening-equipped exterior material for an electricity storage device according to any one of claims 3 to 6, which is formed by removing the sealant layer at the intended opening portion in the exterior material for an electricity storage device.

Citation Information

Patent Citations

  • Electrochemical device

    JP2015228365A

  • Outer packaging body for power storage device

    JP2016129091A

  • Method for working laminate material

    JP2018069418A

  • Exterior material for power storage device, manufacturing method thereof, and power storage device

    JP7060185B1

  • Outer package material for all-solid-state batteries, and all-solid-state battery

    WO2023017683A1