Stabilized high efficiency perovskite minimodules and methods of making and uses thereof
Incorporating lead chelating molecules into the hole transport layer of perovskite solar cells addresses stability and efficiency issues by enhancing the interaction with perovskite films, resulting in improved power conversion efficiency and stability.
Patent Information
- Application Number
- PCT/US2024/030735
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-28
AI Technical Summary
Perovskite solar cells face challenges in stability and efficiency due to degradation under stimuli like moisture, oxygen, heat, and light, with limited efficiency in p-i-n structure modules attributed to non-uniformity and defects at the hole transport layer interface.
Incorporating lead chelating molecules, such as bathocuproine, into the hole transport layer to form a multilayer perovskite composite, which enhances the interaction with perovskite films, reducing defects and improving crystallinity and stability through strong chelation with lead ions, thereby stabilizing the perovskite solar cells.
The solution significantly improves the power conversion efficiency, reproducibility, and long-term stability of perovskite solar cells and minimodules by reducing amorphous regions and non-radiative recombination, achieving higher Voc and FF, and maintaining efficiency under light soaking conditions.
Smart Images

Figure US2024030735_28112024_PF_FP_ABST
Abstract
Description
STABILIZED HIGH EFFICIENCY PEROVSKITE MINIMODULES AND METHODSOF MAKING AND USES THEREOFCROSS REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of priority to U.S. Provisional Application No.63 / 504,081, filed May 24, 2023, which is herein incorporated by reference in its entirety.FIELD
[0002] The presently disclosed subject matter relates generally to perovskite precursor solutions, perovskite films prepared from the precursor solutions, and solar cells comprising the perovskite films.GOVERNMENT SUPPORT
[0003] This invention was made with government support under Grant No. DE-EE0009520 awarded by the Department of Energy. The government has certain rights in the invention.BACKGROUND
[0004] Recent advances have focused on improving the stability and efficiency of solar cells. For example, bifacial silicon solar modules offer improved energy yield by harvesting reflected and diffuse sunlight from the rear side of the solar cell. Perovskite solar cells (PSCs) have also attracted attention due to their excellent optical and electronic properties and low production cost (Q. Dong et al. Science, 2015, 347, 967-970; H. Tan et al. Science, 2017, 355, 722-726; M. A. Green etal. Nat Photonics, 2014, 8, 506-514; J.-P. Correa-Baena etal. Science, 2017, 358, 739- 744). Indeed, the certified power conversion efficiency (PCE) of PSCs (25.2 %) has surpassed those of mainstream thin-film photovoltaic technologies (NREL’s Best Research-Cell Efficiency Chart, accessed on September 16, 2020). However, the stability of these PSCs is becoming increasingly important for their commercialization. Current efficient PSCs typically suffer from poor long-term operational stability due to the degradation of perovskite materials under stimuli, including moisture, oxygen, heat, and light irradiation (B. Chen et al. Chemical Society Reviews, 2019, 48, 3842-3867; C. C. Boyd et al. Chemical Reviews, 2019, 119, 3418-3451; T. Leijtens et al. Advanced Energy Materials, 2015, 5). However, there are few examples of efficient and stableperovskite cells, and their associated efficiencies are far behind their silicon counterparts. The perovskite module efficiency is limited by the low efficiency of p-i-n structure perovskites solar cells, the structure most perovskite PV modules adopt due to its superior stability and manufacturability, and the large efficiency loss upon transferring the small cells to modules, mainly induced by the non-uniformity of perovskites or charge transport layers. As such, what is needed in the art are strategies for enhancing the efficiency and stability of perovskite solar cells, specifically by controlling the interface between the hole transport layer and the perovskite film. The subject matter described herein addresses this unmet need.BRIEF SUMMARY
[0005] In one aspect, the presently disclosed subject matter is directed to a perovskite solar cell, comprising a multilayer perovskite composite comprising: i. a hole-transport layer comprising a hole transport material and lead chelating molecules (LCMs), and ii. a polycrystalline perovskite film disposed on top of the hole transport layer wherein the perovskite film comprises a composition of Formula (I):ABX3 (I) wherein A is a cation selected from the group consisting of methylammonium (MA), dimethylammonium (DMA), tetramethylammonium (TMA), formamidinium (FA), cesium (Cs), rubidium (Rb), potassium (K), sodium (NA), butylammonium (BAH), phenyl ethyl ammonium (PEA), phenylammonium (PHA), guanidinium (GU), and a combination thereof;B is at least one divalent metal; andX is at least one halide.
[0006] In another aspect, the presently disclosed subject matter is directed to methods of preparing the multilayer perovskite composite comprising: i. disposing a precursor solution comprising the hole transport layer material, the lead chelating molecules, and a solvent onto a substrate using a fast-coating process to form a hole transport film; andii. disposing a precursor perovskite solution comprising the perovskite material of Formula I and a solvent onto the hole transport film using a fast-coating process to form a perovskite film disposed on the hole transport film.
[0007] In another aspect, the presently disclosed subject matter is directed to a perovskite solar cell comprising: one or more transparent conductive oxide layers; one or more conductive electrode layers; one or more electron transport layers; and an active layer comprising the multilayer perovskite composite described herein.BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figures 1A-1 J. Chelation of lead ions by BCP. (A) Illustration for the Chelation of the LCMs (in hole transport layer) with Pb2+ions at the bottom perovskite films; (B) Photographs of BCP solution (in 2-ME, ~0.1 mg / mL), FAPbb solution (in 2-ME / DMSO, IM) and the mixture of the BCP solution and FAPbb solution (v:v = 1 : 1 mixture); (C) XRD pattern of the precipitation that form in the mixture of BCP and FAPbb solution. The inset shows the photographs of the dried precipitation before and after annealing; (D) and (E) FTIR of the BCP and FAPbb powder and the dried powder from BCP / FAPbb mixture. (F) XPS spectra of Pb 4f from the perovskite films with and without spun BCP on the top surface. Density functional theory (DFT) modeling of the interaction of (G) BCP and Pbb termination, (H) DMSO and Pbb termination, (I) BCP and FAI termination, and (J) DMSO and FAI termination
[0009] Figure 2. The chemical structure of some lead chelation molecules (LCMs) studied in this work: Bathocuproine (BCP), p-Toluenesulfonic anhydride (TSA), L-Ascorbic acid (VC), meso-2, 3 -Dimercaptosuccinic acid (MDSA) and Ethylenediaminetetraacetic acid (EDTA).
[0010] Figure 3. Schematic diagram of the chelation effect of LCMs and Pb2+. BCP can provide two coordination bonds for Pb2+. TSA, VC and MDSA can provide up to four coordination bonds with Pb2+. EDTA can provide six coordination bonds with Pb2+. The most likely chelation sites formed by two neighboring coordination bonds: BCP chelates Pb2+via Pb-N bonds, TSA chelates Pb2+via Pb-0 bonds (two possible chelation sites), VC chelates MDSA with Pb2+via Pb- O (four possible chelation sites), MDSA via Pb-0 and Pb-S (four possible chelation sites) to chelate Pb2+. EDTA chelates to Pb2+via Pb-N and Pb-0 (one chelation site).
[0011] Figure 4. Photographs ofFAPbb solution in 2-ME (left) and the mixture of FAPbl3 and TSA solution in 2-ME (right). When the FAPbh solution and TSA solution were mixed, a slight turbidity appeared in the mixed solution, an indication for the relative low solubility of the chelation product in 2-ME.
[0012] Figure 5. The XRD pattern of the precipitation formed in the mixture of BCP and FAPbh solution (scan range of 6-42°).
[0013] Figure 6. XRD pattern of the crystalized BCP powder, Pbb powder and the dried precipitation powder that form in the mixture of BCP and Pbh solution (in 2-ME). The inset shows the photographs of BCP, Pbh and the dried precipitation (100 °C for 10 min).
[0014] Figure 7. FTIR of the LCM solutions (in 2-ME) and the mixture of LCMs (dissolved in 2-ME) and FAPbh solution. The chelation of TSA, VC, MDSA, EDTA and FAPbh is reflected by the peak position shifts of S=O stretch, C=O stretch, C=O stretch and C-N stretch, respectively.
[0015] Figures 8A-8B (A) Steady-state PL and (B) TRPL decay of a perovskite sample with a structure of Glass / PTAA / perovskite / PTAA. The PL intensity and recombination lifetime mainly reflect the difference in defects on the top and bottom surfaces of the perovskite.
[0016] Figures 9A-9K. Functionality of BCP in reducing defects in perovskites. (A) and (D) Measurement geometry; (B) - (C) Steady state PL and TRPL decay of control and target perovskite fdms; (E) - (F) Steady state PL and TRPL decay of perovskite samples with and without BCP coated on top surface; (G) - (H) Fluorescence lifetime mapping (FLIM) of perovskite layers on PTAA with and without BCP; (I) Structure of Pb-Pb dimer on the Pbh-terminatcd (100) surface. (J) Structure of BCP binding to Pb-Pb dimer on the surface; (K) Calculated DOS of Pbh- termination without and with BCP binding; The dashed vertical lines indicate the valence band maximum (VBM) and conduction and minimum (CBM).
[0017] Figures 10A-10B. (A) Structure of DMSO binding to Pb-Pb dimer on the Pbh- terminated (100) surface; (B) Calculated DOS showing no elimination of gaps states with DMSO binding to the surface. The dashed vertical lines indicate the valence band maximum (VBM) and conduction and minimum (CBM).
[0018] Figures 11A-11B. (A) J-V curves and (B) Statistics JV parameters of the perovskite solar cells without (pure PTAA) or with different chelation molecules (collected from 5-10 devices for each condition). The working area of small devices is 0.08 cm2. There is no PEACI surfacepassivation on the top of perovskite solar cells. These data were collected from the devices without pre-light soaking, while optimal JV parameters are typically collected from devices that have undergone 2-4 days of light stability testing.
[0019] Figure 12. Accelerated efficiency evaluation of small devices without (pure PTAA) or with different chelation molecules under white LED light (~200 mW cm'2, 59-65 °C, 30-65% RH, Voc conditions). Detailed information of the light source can be found in Fig. 19A (LS2). The light intensity was calibrated with a standard reference Si solar cell. The working area of small devices is 0.08 cm2. All the devices were fabricated without PEACI surface passivation.
[0020] Figure 13. The chemical structure of molecules with similar structure to BCP, including bathophenanthroline (BPhen) and 1 , 10-phenanthroline (OPhen)
[0021] Figures 14A-14B. (A) J-V curves of the solar cells without and with 2% BCP, 2% BPhen and 2% OPhen in the PTAA layer. (B) Statistics parameters of J-V curves. The data were collected from 15-20 small devices for each group. The active area of all the small devices was defined by the overlap of Cu electrode and ITO electrode (0.4 cm x 0.2 cm). All the devices were fabricated with PEACI surface processing.
[0022] Figures 15A-15H. Influence of BCP on perovskite crystallization. (A) t-DOS of perovskite solar cells prepared on PTAA with and without BCP; (B) Change of trap band II trap density in the perovskite devices induced by BCP. SEM images of the bottom side of the perovskite films peeled off from ITO / glass substrates: (C)-(D) control films; (E)-(F) target films. (C) and (E) are fresh films, (D) and (F) are lOOOh aged films; The scale bars are all 2 pm; (G) GIXRD patterns of control and target perovskite films measured from bottom side; (H)1H-NMR. of DMSO residual in the control and target perovskite films.
[0023] Figures 16A-16B. Defect distribution inside the devices measured from CLo to PTAA side by DLCP for the control and target devices at the defect trapping ranges of (A) Trap band I and (B) Trap band II.
[0024] Figure 17. 'H-\MR of the control and target samples.
[0025] Figures 18A-18I. Perovskite device performance based on different HTLs. (A) Schematical structure of the perovskite solar cells. (B) J-V curves of the p-i-n structure small devices without and with BCP in PTAA HTLs. The active area of small devices is 0.08 cm2(C) Statistics device performance parameters of the small devices based on PTAA with 0-10 wt% BCP in PTAA; (D) Light soaking stability of the control and targe small devices under illumination oflight source LS2 with intensity of -100 mW cm'2, the data were collected from 18-20 devices for each group. (E) Photograph of an encapsulated minimodule. (F) J-V curves of the control and target minimodules with 8 subcells connected in series. Each subcell is 6 mm wide and 55 mm long; (G) Certification of stabilized PV performance for a minimodule by NREL using Asymptotic Pmax Scan protocol. The aperture area of this module is 26.9 cm2; (H) The calculated aperture efficiency of minimodules with different subcells width based on small cell efficiency of 24.1% (orange solid line) and 24.6% (green solid line); The maximum attenable efficiencies for a subcell width of 6 mm are 21.1% and 21.8%, respectively. (I) Light-soaking stability of the control and target minimodules under light source LS2, the efficiency data were collected from 5-6 minimodules (aperture area of -26.4 cm2) for each group.
[0026] Figures 19A-19B. (A) Photographs of different light sources (LSI, LS2, LS3) for light-soaking stability study. (B) Light spectrum of the corresponding light sources.
[0027] Figure 20. Photographs of the calibrated reference solar cell and meter (Model 91150V-KG5). This reference solar cell is made of 2 cm * 2 cm monocrystalline silicon with a KG5 IR-absorbing window. The output value of the reference cell should be calibrated to be between 0.995-1.005, corresponding to a light intensity of -100 mW cm'2.More details could be found at the website of Newport (https: / / www.newport.eom / f / calibrated-reference-cell).
[0028] Figures 21A-21C (A) Transmittance of 450 nm long pass UV filter. (B) Light spectrum of light source LS3 without long pass UV filter. (C) Light soaking stability of devices with and without long pass filter. The light intensity was calibrated to be -100 mW cm'2. The devices were tested at Voc conditions under 53-61 °C without any additional cooling and ambient humidity (30-65% RH). The data were collected from 5-10 devices for each condition. The working area of small devices is 0.08 cm2. There is no PEACI surface passivation on the top of perovskite solar cells.
[0029] Figure 22. Light-soaking stability of devices measured under different light sources in Fig. 19A The devices were tested under Voc conditions with cell temperatures of 45- 50 °C and ambient humidity of 30-65% RH. The data were collected from 5-10 devices for each condition. The working area of small devices is 0.08 cm2. The light intensity of the light sources was all calibrated to -100 mW cm'2using the method described in Fig.16. All the devices were fabricated without PEACI surface passivation.
[0030] Figures 23A-23B. J -V curves of the (A) control and (B) target small devices illuminated under light source LS2 for different durations. All devices were fabricated with PEACI surface processing. The working area of small devices is 0.08 cm2. The light intensity was calibrated to -100 mW cm'2. The devices were tested under Voc conditions with cell temperatures of 55-61 °C and ambient humidity (30-65% RH). No additional temperature control was applied
[0031] Figure 24. Light-soaking stability of devices measured under maximum power point (MPP) and open-circuit (Voc) condition. The light source for the MPPT and Voc condition testing is LS3 and LS2 in Fig. 19A, respectively. The devices at Voc conditions were tested under 55-61 °C and ambient humidity (30-65% RH). The devices at MPPT were tested under 58-65 °C and ambient humidity (30-65% RH). The data were collected from 5-10 devices for each condition. The working area of small devices is 0.08 cm2. All the devices were fabricated without PEACI surface passivation. LS3 was used as the light source of MPPT testing.
[0032] Figures 25A-25B. Defined working area of (A) small devices and (B) minimodules. The active area of small devices is defined by the overlapping of metal electrode Cu and pre-etched ITO. For the commonly small devices, the active area is 0.08 cm2. The aperture area of the minimodule is defined by a rectangle enclosed by straight black tape on four sides and can be calculated simply by multiplying the width (W) and length (L) of the rectangle. The black tape used here as a photomask needs to be thick enough to completely block the incident light and absorb scattered light, rather than reflecting light. The aperture area for the certified samples was also determined by this method and was precisely measured under a microscope by the NREL PV group.
[0033] Figures 26A-26B. (A) Microscopy images of laser-scribed Pl, P2, and P3 on the minimodules and (B) the corresponding height-scanning distance curve collected from the profiler. Those 5 lines were collected from different positions along the direction perpendicular to P1 / P2 / P3. The average width of the non-working area of each subcells is 320 pm.
[0034] Figure 27. Pre- Asymptotic IV measured by NREL PV Cell & Module Performance Group on the submodule with the certification of the stabilized IV performance in Fig. 27. This minimodule has an aperture area of 26.9 cm2defined by the photomask and measured by NREL.
[0035] Figure 28. Certification of stabilized photovoltaic (PV) performance of the submodule measured by NREL PV Cell & Module Performance Group. The device performance was measured using the NREL Asymptotic Pmax Scan protocol. According to the protocol, thedevices are held at 11 voltage points within the Vmax region until a constant current is reached. Their criterion is that the devices are only biased to the next voltage point when the current change is less than 0.1% per minute. A polynomial fit was applied to this set of stabilized current-voltage points to extract the steady-state Pmax.
[0036] Figures 29A-29B. Modeling of the variation of (A) current density of subcells and (B) fill factor of minimodules with different subcells width.
[0037] Figures 30A-30B. J -V curves of the (A) control and (B) target minimodules illuminated under light source LS2 for different durations. The aperture area of the minimodules was 26.4 cm2. The minimodule light soaking stability was also evaluated in ambient condition (30- 65% RH) with light intensity of -100 mW cm'2. The minimodule temperature was measured to be 56-62 °C and was kept constant during the testing process. No additional temperature control was applied.DETAILED DESCRIPTION
[0038] The subject matter described herein relates to hole transport layers that contain one or more lead chelating molecules, multilayer perovskite composites comprising the hole transport layers, methods for preparing the multilayer perovskite composites, and use of the multilayer perovskite composites in photovoltaic (PV) devices, such as perovskite solar cells.
[0039] The presently disclosed subj ect matter will now be described more fully hereinafter. However, many modifications and other embodiments of the presently disclosed subject matter set forth herein will come to mind to one skilled in the art to which the presently disclosed subject matter pertains having the benefit of the teachings presented herein. Therefore, it is to be understood that the presently disclosed subject matter is not to be limited to the specific embodiments disclosed and that modifications and other embodiments are intended to be included within the scope of the appended claims. In other words, the subj ect matter described herein covers all alternatives, modifications, and equivalents. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in this field. All publications, patent applications, patents, and other references mentioned herein are incorporated by reference in their entirety. In the event that one or more of the incorporated literature, patents, and similar materials differs from or contradicts this application,including but not limited to defined terms, term usage, described techniques, or the like, this application controls.I. Overview
[0040] With nearly one decade of global efforts, the power conversion efficiency (PCE) of small area n-i-p structure single-junction perovskite solar cells has reached the parity of monocrystalline silicon solar cells (1-4), however, the perovskite module efficiency is still much lower than the state-of-the art silicon modules (5-8). The perovskite module efficiency is limited by the low efficiency of p-i-n structure perovskites solar cells, the structure most perovskite PV modules adopt due to its superior stability and manufacturability, and the large efficiency loss upon transferring the small cells to modules, mainly induced by the non-uniformity of perovskites or charge transport layers. Several strategies, such as improving the crystallization process and passivating surface defects, have been applied to further improve the p-i-n structure device efficiency (9-13). For example, a recent study reported a certified stabilized efficiency of 24.05% for small area p-i-n structure devices using surface treatment to enhance charge extraction (14). In contrast to top surfaces, the perovskite-hole transport layer interface has received much less attention. It was recently found that nonradiative recombination of interface carriers due to defects at buried interfaces may limit the efficiency of p-i-n structure perovskite solar cells (15). A notable smaller photoluminescence (PL) quantum yield was observed for perovskites near hole transport layers (HTLs) (16).
[0041] In contrast to top surfaces, the bottom interface of perovskite- HTL is much more difficult to control. Some defect passivation species were attempted to be mixed with HTLs (17- 20), while many passivation molecules may be washed away during the perovskite coating because of their high solubility in perovskite precursor solvents, such as 2-methoxyethanol (2-ME), dimethylformamide (DMF), and dimethyl sulfoxide (DMSO). The other challenge comes from the top-to-down crystallization process of perovskite during solution coating process (21). The evaporation of initially trapped DMSO may generate amorphous region and tens-nanometer-size voids at the bottom of perovskite films during film formation process (6). Although the initially formed voids could be eliminated by introduce solid-state carbohydrazide to partially replace DMSO in perovskite precursor solutions, new voids were found to form at the bottom interfaces along grain boundaries during long-term device operation, indicating the presence of nonnegligible amorphous perovskite in perovskite films even after annealing (22). The amorphous regions close to the bottom interface have been also observed by high resolution tunneling electron microscopy studies (23, 24). The non-uniform distribution of the amorphous regions, caused by the non-uniform evaporation of DMSO, may cause non-uniform device performance and thus strongly impact the module efficiency and reproducibility, which is not reflected by champion small cell efficiency. Perovskite modules need to be fabricated to evaluate the impact of them.
[0042] The subject matter disclosed herein describes a method to effectively reduce the amorphous region at the bottom of perovskite films by embedding lead chelation molecules, including a broadly applied electron transport material of bathocuproine (BCP), into HTLs. BCP competes with DMSO to interact with lead ions by the strong chelation with lead ions, which reduces the DMSO residue and thus amorphous region in perovskites close to the HTLs. BCP also passivates perovskites and significantly improves the efficiency, reproducibility, and stability of the perovskite cells and minimodules.II. Definitions
[0043] As used herein, “and / or” refers to and encompasses any and all possible combinations of one or more of the associated listed items, as well as the lack of combinations when interpreted in the alternative (“or”).
[0044] As used herein, the term “about,” when referring to a measurable value such as an amount of a compound or agent of the current subject matter, dose, time, temperature, and the like, is meant to encompass variations of ±20%, ±10%, ±5%, ±1%, ±0.5%, or even ±0.1% of the specified amount.
[0045] As used herein, conditional language used herein, such as, among others, “can,” “could,” “might,” “may,” “e.g.,” and the like, unless specifically stated otherwise or otherwise understood within the context as used, is generally intended to convey that certain embodiments include, while other embodiments do not include, certain features, elements and / or steps. Thus, such conditional language is not generally intended to imply that features, elements and / or steps are in any way required for one or more embodiments or that one or more embodiments necessarily include logic for deciding, with or without author input or prompting, whether these features, elements and / or steps are included or are to be performed in any particular embodiment. The terms “comprising,” “including,” “having,” and the like are synonymous and are used inclusively, in anopen-ended fashion, and do not exclude additional elements, features, acts, operations, and so forth. Also, the term “or” is used in its inclusive sense (and not in its exclusive sense) so that when used, for example, to connect a list of elements, the term “or” means one, some, or all of the elements in the list.
[0046] As used herein, “PSC” refers to perovskite solar cell.
[0047] As used herein, “PCE” refers to power conversion efficiency. The terms “power conversion efficiency,” “PCE,” “photovoltaic efficiency”, and “solar cell efficiency,” may be used interchangeably and refer to the ratio of energy output from the photovoltaic device to the energy input to the photovoltaic device. The energy output is in the form of electrical energy and energy input is in the form of electromagnetic radiation (e.g., sunlight). Unless otherwise indicated, the photovoltaic efficiency refers to terrestrial photovoltaic efficiency, corresponding to AMI.5 conditions, where AM is Air Mass. PCE may be measured by one or more techniques conventionally known to one of ordinary skill in the art.
[0048] As used herein, the terms “incident light” or “incident photons” refer to light or photons that fall on the surface of a material. Incident light can be from natural lighting, like the sun, or from an artificial light source. Incident light can also be light that reflects off another surface, such as a reflector, on to the surface of the material of interest.
[0049] As used herein, “photoactive device” refers to (i) a device capable of and configured to convert electromagnetic radiation (e.g., X-ray, infrared, ultraviolet, and / or visible light) to electrical energy and / or converting electrical energy to electromagnetic radiation. A photoactive device may be configured to both convert light to electrical energy (e.g., as a solar cell) and convert electrical energy to light (e.g., via electroluminescence), for example depending on the direction of electrical current in the device (e.g., depending on whether electrical power is withdrawn from or supplied to the device). Exemplary photoactive devices include, but are not limited to, a photovoltaic cell (also referred to as a solar cell), a photodiode, and a light emitting diode (LED). In certain embodiments, a photoactive device can also refer to a device configured to change its optical, physical, and / or electrical properties with change in its exposure to electromagnetic radiation and / or a device configured to change its optical properties in response to a change in input of electrical energy. Exemplary photoactive devices can also include, but are not limited to, a photoresistor, phototransistor, photomultiplier, photoelectric cell, and an electrochromic cell.
[0050] As used herein, “active layer” refers to a photoactive layer in a device, such as a solar cell, and / or it may include a photoactive material. Furthermore, it should be noted that the use of the term “active layer” is in no way meant to restrict or otherwise define, explicitly or implicitly, the properties of any other layer in the device.
[0051] As used herein, the term “defect” refers to a defective site in a crystal lattice where the local crystal structure does not correspond to the crystal structure of the bulk material. Nonlimiting examples of defective sites include point defects, line defects, and planar defects. Point defects include vacancy defects (the absence of an ion), interstitial defects (the interstitial inclusion of an additional ion), Frenkel defects (a closely located pair of defects consisting of an interstitial defect and a vacancy defect) and the presence of an impurity ion. Planar defects include grain boundaries and stacking faults.
[0052] As used herein, the term “p-i-n perovskite structure” or “p-i-n planar structure” refers to perovskite solar cells wherein the solar cell is illuminated through the hole transport layer (HTL) side. Alternately, the term “n-i-p perovskite structure” refers to perovskite solar cells wherein the solar cell is illuminated through the electron transport layer (ETL) side.
[0053] As used herein, the term “fill factor” or “FF” refers to a measure of the efficiency of a PV device as determined by the short-circuit current (Jsc) and open-circuit voltage (Voc).
[0054] As used herein, the term “valence band” refers to the range of highest energy electronic states where electrons are normally present at absolute zero. The electrons in the valence band are held in place until acted upon by an external source, such as thermal or light energy.
[0055] As used herein, the term “conduction band” refers to the range of lowest energy electronic states that are vacant at absolute zero. Electrons in the conduction band can move freely to conduct electric current.
[0056] As used herein, the term “hole” refers to an empty state left behind by an electron that acquired sufficient energy to jump into the conduction band of a conductor or semiconductor material. The presence of holes in a valence band allows the electrons therein some degree of freedom and conductivity. As such, both electrons and electron holes serve as charge carriers in a semiconductor material.
[0057] As used herein, the term “grain” refers to a small region of crystalline or polycrystalline material having a specific and continuous crystal lattice orientation. Each grain represents a small single crystal.
[0058] As used herein, the term “multilayer” refers to a composite material comprises two or more distinct layers.
[0059] As used herein, the term “ 1 sun illumination” refers light intensity of approximately 100 mW cm'2.III. Multilayer Perovskite Composite
[0060] In one aspect, the subject matter described herein is directed to a multilayer perovskite composite comprising: i. a hole-transport layer comprising a hole transport material and lead chelating molecules (LCMs), and ii. a polycrystalline perovskite film disposed on top of the hole transport layer wherein the perovskite film comprises a composition of Formula (I):ABX3(I) wherein A is a cation selected from the group consisting of methylammonium (MA), dimethylammonium (DMA), tetramethylammonium (TMA), formamidinium (FA), cesium (Cs), rubidium (Rb), potassium (K), sodium (NA), butylammonium (BAH), phenylethylammonium (PEA), phenyl ammonium (PHA), guanidinium (GU), and a combination thereof;B is at least one divalent metal; andX is at least one halide.A. Compositions of Formula I
[0061] Described herein are perovskite films comprising compositions of Formula (I) which are disposed on the hole transport layer:ABX3(I).
[0062] In certain embodiments of the perovskite film, A may comprise an ammonium, an organic cation of the general formula [NR4]+where the R groups can be the same or different groups. Suitable R groups include, but are not limited to: methyl, ethyl, propyl, butyl, pentyl group or isomer thereof; any alkane, alkene, or alkyne CxHy, where x=l-20, y=l-42, cyclic, branched or straight-chain; alkyl halides, CxHyXz, x=l-20, y=0-42, z=l-42, X=F, Cl, Br, or I; any aromatic group (e.g., phenyl, alkylphenyl, alkoxyphenyl, pyridine, naphthalene); cyclic complexes where at least one nitrogen is contained within the ring (e g., pyridine, pyrrole, pyrrolidine, piperidine,tetrahydroquinoline); any sulfur-containing group (e.g., sulfoxide, thiol, alkyl sulfide); any nitrogen-containing group (nitroxide, amine); any phosphorous containing group (phosphate); any boron-containing group (e.g., boronic acid); any organic acid (e.g., acetic acid, propanoic acid); and ester or amide derivatives thereof; any amino acid (e.g., glycine, cysteine, proline, glutamic acid, arginine, serine, histidine, 5-ammoniumvaleric acid) including alpha, beta, gamma, and greater derivatives; any silicon containing group (e.g., siloxane); and any alkoxy or group, -OCxHy, where x=0-20, y=l-42. In certain embodiments, A is methylammonium (MA), (CH3NH3 ). In certain embodiments, A is methylammonium. In certain embodiments, A is dimethylammonium (DMA), ((CHB)2NH2+). In certain embodiments, A is tetramethylammonium (TMA), ((CHB)4N+). In certain embodiments, A is butylammonium, which may be represented by (CHB(CH2)3NH3+) for n-butylammonium, by ((CHs)3CNH3+) for t-butylammonium, or by (CH3)2CHCH2NH3+) for iso-butylammonium. In certain embodiments, A is phenylethylammonium (PEA+), which may be represented by C6Hs(CH2)2NH3+or by C6HsCH(CH3)NH3+. In certain embodiments, A comprises phenylammonium, C6H5NH3 . In certain embodiments, A is an ammonium cation selected from the group consisting of methylammonium (MA), tetramethylammonium (TMA), butylammonium (BAH), phenethylammonium (PEA), and phenylammonium (PHA), or a combination thereof.
[0063] In certain embodiments of the perovskite film, A may comprise a formamidinium, an organic cation of the general formula [R2NCHNR2]+where the R groups can be the same or different groups. Suitable R groups include, but are not limited to: hydrogen, methyl, ethyl, propyl, butyl, pentyl or an isomer thereof; any alkane, alkene, or alkyne CxHy, where x=l-20, y=l-42, cyclic, branched or straight-chain; alkyl halides, CxHyXz, x=l-20, y=0-42, z=l-42, X=F, Cl, Br, or I; any aromatic group (e.g., phenyl, alkylphenyl, alkoxyphenyl, pyridine, naphthalene); cyclic complexes where at least one nitrogen is contained within the ring (e.g., imidazole, benzimidazole, dihydropyrimidine, (azolidinylidenemethyl) pyrrolidine, triazole); any sulfur-containing group (e.g., sulfoxide, thiol, alkyl sulfide); any nitrogen-containing group (nitroxide, amine); any phosphorous containing group (phosphate); any boron-containing group (e.g., boronic acid); any organic acid (acetic acid, propanoic acid) and ester or amide derivatives thereof; any amino acid (e.g., glycine, cysteine, proline, glutamic acid, arginine, serine, histidine, 5-ammoniumvaleric acid) including alpha, beta, gamma, and greater derivatives; any silicon containing group (e.g., siloxane); and any alkoxy or group, -OCxHy, where x=0-20, y=l-42. In certain embodiments A is a formamidinium ion represented by (H2N=CH-NH2+).
[0064] In certain embodiments of the perovskite film, A may comprise a guanidinium, an organic cation of the general formula [(R2N)2C=NR.2]+where the R groups can be the same or different groups. Suitable R groups include, but are not limited to: hydrogen, methyl, ethyl, propyl, butyl, pentyl group or isomer thereof; any alkane, alkene, or alkyne CxHy, where x=l-20, y=l-42, cyclic, branched or straight-chain; alkyl halides, CxHyXz, x=l-20, y=0-42, z=l-42, X=F, Cl, Br, or I; any aromatic group (e.g., phenyl, alkylphenyl, alkoxyphenyl, pyridine, naphthalene); cyclic complexes where at least one nitrogen is contained within the ring (e.g., octahydropyrimido[ 1 ,2-a]pyrimidine, pyrimidof 1 ,2-a]pyrimidine, hexahydroimidazof 1 ,2-a] imidazole, hexahydropyrimidin-2-imine); any sulfur-containing group (e.g., sulfoxide, thiol, alkyl sulfide); any nitrogen-containing group (nitroxide, amine); any phosphorous containing group (phosphate); any boron-containing group (e.g., boronic acid); any organic acid (acetic acid, propanoic acid) and ester or amide derivatives thereof; any amino acid (e.g., glycine, cysteine, proline, glutamic acid, arginine, serine, histidine, 5-ammoniumvaleric acid) including alpha, beta, gamma, and greater derivatives; any silicon containing group (e.g., siloxane); and any alkoxy or group, -OCxHy, where x=0-20, y=l-42. In certain embodiments, A is a guanidinium ion of the type (H2N=C-(NH2)2+).
[0065] In certain embodiments of the perovskite film, A may comprise an alkali metal cation, such as Li+, Na+, K+, Rb+, or Cs+.
[0066] In certain embodiments of the perovskite film, A is a cation selected from the group consisting of methylammonium (MA), tetramethylammonium (TMA), formamidinium (FA), caesium (Cs), rubidium (Rb), potassium (K), sodium (Na), butylammonium (BAH), phenethylammonium (PEA), phenylammonium (PHA), and guanidinium (GU), or a combination thereof.
[0067] In certain embodiments of the perovskite film, A comprises XcY(i-c) wherein X and Y are a combination of two cations selected from the group consisting of methylammonium (MA), tetra-methylammonium (TMA), formamidinium (FA), caesium (Cs), rubidium (Rb), potassium (K), sodium (Na), butylammonium (BA), phenethylammonium (PEA), phenylammonium (PA), and guanidinium (GA). In certain embodiments of the perovskite film, A comprises a combination of two cations wherein “c” is the molar ratio of X:Y and is between 0.01 and 1.0. In certain embodiments of the perovskite film, A comprises FA and another cation selected from the group above. In certain embodiments, A comprises FA and Cs. In certain embodiments of the perovskitefilm, c is 0.01 , 0.02, 0.03, 0.04, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.41 , 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, or 1. In certain embodiments of the perovskite film, c is between 0.01 and 0.05, 0.01 and 0.03, 0.01 and 0.15, 0.02 and 0.10, 0.01 and 0.5, 0.01 and 0.75, 0.3 and 0.6, 0.2 and 0.7, 0.1 and 0.8, 0.3 and 0.5, 0.4 and 0.9, or 0.4 and 0.6.
[0068] In certain embodiments of the perovskite film, A is selected from the group consisting of Cs, FA, and MA, or a combination thereof. In certain embodiments, A is a combination of FA and Cs.
[0069] In certain embodiments, the perovskite crystal structure composition may be doped (e.g., by partial substitution of the cation A and / or the metal B) with a doping element, which may be, for example, an alkali metal (e.g., Li+, Na+, K+, Rb+, or Cs+), an alkaline earth metal (e.g., Mg+2, Ca+2, Sr+2, Ba+2) or other divalent metal, such as provided below for B, but different from B (e.g., Sn+2, Pb2+, Zn+2, Cd+2, Ge+2, Ni+2, Pt+2, Pd+2, Hg+2, Si+2, Ti+2), or a Group 15 element, such as Sb, Bi, As, or P, or other metals, such as silver, copper, gallium, indium, thallium, molybdenum, or gold, typically in an amount of up to or less than about 1, 5, 10, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 99, or 100 mol % of A or B. A may comprise a mixture of cations. B may comprise a mixture of cations.
[0070] The variable B comprises at least one divalent (B+2) metal atom. The divalent metal (B) can be, for example, one or more divalent elements from Group 14 of the Periodic Table (e.g., divalent lead, tin, or germanium), one or more divalent transition metal elements from Groups 3- 12 of the Periodic Table (e g., divalent titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, palladium, platinum, and cadmium), and / or one or more divalent alkaline earth elements (e.g., divalent magnesium, calcium, strontium, and barium). In certain embodiments, the at least one divalent metal is selected from the group consisting of lead, tin, cadmium, germanium, zinc, nickel, platinum, palladium, mercury, titanium, silicon, and a combination thereof. In certain embodiments, B is lead.
[0071] In certain embodiments of the perovskite film, B comprises DgE(i-g), wherein D and E are a combination of one or more divalent elements from Group 14 of the Periodic Table (e.g., divalent lead, tin, or germanium), one or more divalent transition metal elements from Groups 3- 12 of the Periodic Table (e g., divalent titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, palladium, platinum, and cadmium), and / or one or more divalent alkalineearth elements (e.g., divalent magnesium, calcium, strontium, and barium). Tn certain embodiments of the perovskite film, B comprises a combination of two cations wherein “g” is the molar ratio of D:E and is between 0.01 and 1.0. In certain embodiments of the perovskite film, g is 0.01, 0.02, 0.03, 0.04, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, or 1. In certain embodiments of the perovskite film, g is between 0.01 and 0.05, 0.01 and 0.03, 0.01 and 0.15, 0.02 and 0.10, 0.01 and 0.5, 0.01 and 0.75, 0.3 and 0.6, 0.2 and 0.7, 0.1 and 0.8, 0.3 and 0.5, 0.4 and 0.9, or 0.4 and 0.6. In certain embodiments, the at least one divalent metal is selected from the group consisting of lead, tin, cadmium, germanium, zinc, nickel, platinum, palladium, mercury, titanium, silicon, and a combination thereof. In certain embodiments of the perovskite film, B comprises Pb and another cation selected from the group above. In certain embodiments, B comprises Pb and Sn.
[0072] The variable X is independently selected from one or a combination of halide atoms, wherein the halide atom (X) may be, for example, fluoride (F ), chloride (Cl ), bromide (BE), and / or iodide (I-). In certain embodiments, the at least one halide is selected from the group consisting of I, Br, and a combination thereof. In certain embodiments, X is selected from the group consisting of SCN’, BFF, F‘, Cl’, Br , T, and a combination thereof.
[0073] In certain embodiments, the crystalline perovskite composition of Formula (I) is selected from the group consisting of cesium formamidinium lead bromo iodide (Cso2FAo 8Pb(Ii-xBrx)3 wherein x is about 0 to 0.5; methylammonium formamidinium lead iodide (MAxFAi-xPbla) wherein x is about 0 to 1; and cesium dimethylammonium formamidinium lead iodide (CsxDMAyFA(i-x-y)Pbl3) wherein x is about 0 to 0.4 and y is about 0 to 0.3.
[0074] In certain embodiments, the crystalline perovskite composition of Formula (I) is selected from the group consisting of cesium lead iodide (CsPbb), methylammonium tin iodide (CFbNFbSnb), cesium tin iodide (CsSnb), methylammonium lead iodide (CEbNFbPbb), cesium lead bromide (CsPbBn), methylammonium tin bromide (CFbNJFSnBrs), cesium tin bromide (CsSnBn), methylammonium lead bromide, (CFbNFbPbBn), formamidinium tin bromide (CHNFENFESnBn), formamidinium lead bromide (CHNFhNtbPbBn), formamidinium tin iodide (CHNFFNFESnlo), formamidinium lead iodide (CHNFFNFEPbb), cesium formamidinium lead iodide (Cso.1FAo.9Pbb), cesium formamidinium methylammonium lead iodide (Cso.o5FAo.7oMAo.25Pbl3), cesium formamidinium lead tin iodide (Cso.2FAo.sPbo 5Sno.5I3), cesiumformamidinium lead iodide bromide (Cso 2FAo sPb(Io 6Bro 4)3), and cesium methylammonium lead iodide bromide (Cso.iMAo.9Pb(Io.9Bro.i)3). In certain embodiments, the crystalline perovskite composition of Formula (I) is selected from the group consisting of CsPbks, MAPbh, FAPbh, MA0.7FA0.3PBI3, Cso.iFAo.9Pbl3, Cso.o5FAo.7oMAo 25Pbl3, and Cso.2FAo.sPbo.5Sno.5I3. In a preferred embodiment, the crystalline perovskite composition of Formula (I) is methylammonium formamidinium lead iodide (MA0.7FA0.3PBI3,). In another preferred embodiment, the crystalline perovskite composition of Formula (I) is cesium formamidinium lead iodide (Cso.iFAo. PbLs).
[0075] In embodiments, the subject matter described herein is directed to polycrystalline perovskite films characterized by a chemical formula comprising at least two chemical species, A and B, each independently selected from the group consisting of Pb, Cs, Sn, Sb, Fe, Ge, Mn, Mo, Ta, Ag, Na, K, Ru, Bi, Cs, Mg, Ti, Mn, Mg, V, Ni, Cu, Cd, Hg, Ga, In, formamidinium (“FA”), methylammonium (“MA”), ethylammonium, propyl ammonium, butylammonium, amylammonium, hexylammonium, heptylammonium, octylammonium, oleylammonium, formamidinium, dodecylammonium, phenylethylammonium, benzylammonium, ethylenediammonium, tetramethyl ammonium, tetraethylammonium, tetrabutylammonium, hexadecyl trimethyl ammonium, and ethanediammonium, and at least one chemical species, X, selected from the group consisting of I, Br, Cl, F, COO, BF3, and SCN. In certain embodiments, the chemical formula of the polycrystalline perovskite film is selected from the group consisting of ABX3, A2BX4, A2BB Xe, A3B2X9, and A2BXe, wherein B and B’ can each independently be monovalent, divalent, trivalent, or tetravalent metal cations selected from the list consisting of Pb, Cs, Sn, Sb, Fe, Ge, Mn, Mo, Ta, Ag, Na, K, Ru, Bi, Cs, Mg, Ti, Mn, Mg, V, Ni, Cu, Cd, Hg, Ga, and In, or a combination thereof. In certain embodiments, the polycrystalline perovskite film comprises a double perovskite, for example, Cs2AgBiXe. In certain embodiments, the polycrystalline perovskite film comprises a low dimensional perovskite, for example, PEA2PbX4.B. Compositions of Hole-transport layer
[0076] Described herein are charge transport materials that act as hole transport layer materials. In certain embodiments, the hole transport layer on which the perovskite film is disposed comprises at least one of poly(3,4-ethylene dioxithiophene) (PEDOT) doped with poly(styrene sulfon icacid) (PSS), Spiro-OMeTAD, pm-spiro-OMeTAD, po-spiro-OMeTAD, dopants in spiro- OMeTAD, 4,4'-biskptrichlorosilylpropylphenyl)pheny laminoThiphenyl (TPD-Si2), poly(3- hexyl-2,5-thienylene vinylene) (P3HTV), C60, carbon, carbon nanotube, graphene quantum dot,graphene oxide, copper phthalocyanine (CuPc), Polythiophene, poly(3,4- (Ihydroxymethyl)ethylenedioxythiophene (PHMEDOT), n-dodecylbenzenesulfonic acid / hydrochloric acid doped poly(aniline) nanotubes (a-PANIN)s, poly(styrene sulfonic acid)- graft-poly(aniline) (PSSA-g-PANI), poly(9. 9-dioctylfluorene)-co-N-(4-(l-methylpropyl)phenyl) diphenylamine (PFT), 4,4'-bis(p- trichlorosilylpropylphenyl) phenylaminobiphenyl (TSPP), 5,5'- bis(p-trichlorosilylpropylphenyl) phenylamino-2,20 bithiophene (TSPT), N- propyltri ethoxy silane, 3,3,3-trifluo ropropyltri chlorosilane or 3 -aminopropyltri ethoxy silane, Poly(bis(4-phenyl)(2,4,6-trimethylphenyl)amine) (PTAA), (Poly[[(2,4-dimethylphenyl)imino]- l,4-phenylene(9,9-dioctyl-9H-fluorene-2,7-diyl)-l,4phenylene], (PF8-TAA)), (Poly [[(2,4- dimethylphenyl)imino]-l,4-phenylene (6,12-dihydro-6,6,12,12tetraoctylindeno[l,2-b]fluorene- 2,8-diyl)-l,4-phenylene]) (PIF8-TAA), poly[[4,8-bis[(2-ethylhexyl)oxy]benzo[l,2-b:4,5- b]dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophenediyl]] (PTB7), poly [N-90-heptadecanyl-2,7-carbazol e-alt-5, 5-(40,70-di-2-thienyl-20, 10, 30-benzothiadiazole)] (PCDTBT), Poly[2,5-bis(2-decyldodecyl)pyrrolo[3,4-c]pyrrole-l,4(2H,5H)-dione-(E)-l,2- di(2,20-bithiophen-5-yl) ethene] (PDPPDBTE), 4,8-dithien-2-yl-benzo[l,2- d ;4,5- d ']bistriazole- alt -benzofl, 2- b :4,5b'] di thiophenes (pBBTa-BDTs), pBBTa-BDTl, pBBTa-BDT2 polymers, poly(3 -hexylthiophene) (P3HT), poly(4,4’-bis(N-carbazolyl)-l,l’-biphenyl) (PPN), triarylamine (TAA) and / or thiophene moieties, Paracyclophane, Triptycene, and Bimesitylene, Thiophene and Furan-based hole transport materials, Dendrimer-like and star-type hole transport materials, VO, VOX, MoC, WO, ReO, NiOx, AgOx, CuO, Cu2O, V2O5, Cui, CuS, CuInS2, colloidal quantum dots, lead sulphide (PbS), CuSCN, Cu2ZnSnS4, Au nanoparticles and their derivatives. Thiophene derivatives, Triptycene derivatives, Triazine derivatives, Porphyrin derivatives, Tri phenyl amine derivatives, Tetrathiafulvalene derivatives, Carbazole derivatives and Phthalocyanine derivatives. As used herein, when a material is referred to a “derivate” or as “derivatives,” such as Triphenylamine derivatives, the material contains Triphenylamine in its backbone structure. In certain embodiments, the hole transport layer between the perovskite fdm and the transparent conductive layer is Poly(bis(4-phenyl)(2,4,6-trimethylphenyl)amine) (PTAA).
[0077] In embodiments described herein, the hole transport layer further comprises one or more lead chelating molecules. In certain embodiments, the lead chelating molecules are selected from the group consisting of bathocuproine, dimercaptosuccinic acid, L-Ascorbic acid, alpha lipoic acid, ethylenediaminetetraacetic acid, 2,3-dimercaptopropanesulfonic acid, thiaminetetrahydrofuryl disulfide, p-toluenesulfonic anhydride, and penicillamine, or synthetic derivatives thereof. In certain embodiments, the lead chelating molecules are selected from the group consisting of bathocuproine, dimercaptosuccinic acid, L-Ascorbic acid, and p-toluenesulfonic anhydride, or synthetic derivates thereof.
[0078] In preferred embodiments, the hole transport layer comprises lead chelating molecules that are bathocuproine or synthetic derivatives thereof. In certain embodiments, the lead chelating molecules are synthetic derivatives of bathocuproine such as, but not limited to, bathophenanthroline (BPhen) or 1 , 10-phenanthroline (OPhen). In certain embodiments, the lead chelating molecules are bathocuproine. In certain embodiments, the hole transport material is PTAA and the lead chelating molecules are bathocuproine.
[0079] In certain embodiments, the lead chelating molecules comprise about 0.1 to 90 wt. % of the hole transport layer. In certain embodiments, the lead chelating molecules comprise about 1 to 40 wt. % of the hole transport layer. In certain embodiments, the lead chelating molecules comprise about 1.5 to 15 wt. % of the hole transport layer. In certain embodiments, the lead chelating molecules comprise about 4 to 14 wt. % of the hole transport layer. In certain embodiments, the lead chelating molecules comprise about 5 to 13 wt. % of the hole transport layer. In certain embodiments, the lead chelating molecules comprise 6 to 12 wt. % of the hole transport layer. In certain embodiments, the lead chelating molecules comprise about 7 to 11 wt. % of the hole transport layer. In certain embodiments, the lead chelating molecules comprise about 5 to 10% of the hole transport layer. In certain embodiments, the lead chelating molecules comprise about 8 to 10 wt. % of the hole transport layer. In embodiments described herein, the lead chelating molecules comprise about 1, about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9, about 10, about 11, about 12, about 13, about 14, or about 15 wt. % of the hole transport layer. In embodiments described herein, the lead chelating molecules comprise about 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.5, 0.6, 0.7, 0.8, or about 0.9 wt. % of the hole transport layer. In certain embodiments, the lead chelating molecules comprise about 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, or about 90 wt. % of hole transport layer.IV. Methods for preparing the multilayer perovskite composite
[0080] In one aspect, the subject matter described herein is directed a method of preparing the multilayer perovskite composite, comprising:i. disposing a precursor solution comprising the hole transport layer material, the lead chelating molecules, and a solvent onto a substrate using a fast-coating process to form a hole transport fdm; and ii. disposing a precursor perovskite solution comprising the perovskite material of Formula I and a solvent onto the hole transport film using a fast-coating process to form a perovskite film disposed on the hole transport film.
[0081] In certain embodiments, the fast-coating process is selected from the group consisting of spin coating, blade coating, slot die coating, shear coating, gravure coating, brush coating, syringe coating, and screen printing.
[0082] In certain embodiments of the above method, the fast-coating process is spin coating. In certain embodiments, a device is used in the fast-coating process for contacting the precursor solution onto the substrate. The spin coating process is a four-step process: deposition, spin up, spin off, and evaporation. In the first step, the precursor solution is deposited on a turntable followed by the spin up and spin off steps in sequence while the evaporation stage occurs throughout the process. High spinning speeds result in the thinning of the applied precursor solution on the turntable. The rapid rotation facilitates uniform evaporation of the high volatile components and solvent. In certain embodiments, the spin coating process proceeds at rotation speeds between 1000 and 600 rpm.
[0083] In certain embodiments of the above method, the fast-coating process is blade coating. In certain embodiments, a device is used in the fast-coating process for contacting the precursor solution onto the substrate. In the blade coating process, a “blade coater” may be used. As used herein, “blade coater” is synonymous with “doctor blade.” In certain embodiments, doctor blade coating techniques are used to facilitate formation of the perovskite film during the fabrication process.
[0084] Utilizing a fast coating process is advantageous because of increased scalability for perovskite device roll-to-roll production, simplicity, and cost effectiveness. Furthermore, fast coating processes also provide advantages due to high-throughput deposition, high material usage, and application onto flexible substrates. In particular, perovskite films and devices fabricated using a fast coating process, such as blade coating, can have advantageously long carrier diffusion lengths (e.g., up to 3 pm thick) due to the dramatically higher carrier mobility in the blade-coatedfilms. Such doctor-blade deposition can be utilized for large area perovskite cells fabricated with high volume roll-to-roll production.
[0085] In certain embodiments, the method for producing a polycrystalline perovskite film using the fast coating process can take place at a temperature between about 25 °C to about 250 °C. In certain embodiments, the process takes place at about room temperature (about 25 °C).
[0086] In certain embodiments of the fast coating process, the substrate is moving and the device is stationary. In certain embodiments, the device is a doctor blade. In certain aspects, the substrate is moving at a rate of about 2 mm / s relative to the device. In certain aspects, the substrate is moving at a rate of about 20 mm / s relative to the device. In certain aspects, the substrate is moving at a rate of about 40 mm / s relative to the device. In certain aspects, the substrate is moving at a rate of about 99 mm / s relative to the device. In certain aspects, the substrate is stationary and the device moves relative to the substrate. In certain aspects, the device is moving at a rate of about 2 mm / s relative to the substrate. In certain aspects, the device is moving at a rate of about 20 mm / s relative to the substrate. In certain aspects, the device is moving at a rate of about 40 mm / s relative to the substrate. In certain aspects, the device is moving at a rate of about 99 mm / s relative to the substrate.
[0087] In certain embodiments, the fast coating process described herein takes place at about 2 to about 15,000 mm / s. In certain embodiments, the fast coating process described herein takes place at about 2 to about 10,000 mm / s. In certain embodiments, the fast coating process described herein takes place at about 2 to about 99 mm / s. In certain embodiments, the fast coating process takes place at least or at about 2 mm / s, 15 mm / s, 20 mm / s, 40 mm / s, 60 mm / s, 80 mm / s, 99 mm / s, 150 mm / s, 275 mm / s, 500 mm / s, 700 mm / s, 800 mm / s, 900 mm / s, 1000 mm / s, 2000 mm / s, 3000 mm / s, 4000 mm / s, 5000 mm / s, 6000 mm / s, 7000 mm / s, 8000 mm / s, 9000 mm / s, or about 10,000 mm / s.
[0088] In certain embodiments, the distance between the devices used in the fast coating process for contacting the precursor perovskite solution onto the substrate is between about 10 pm and 1 cm. In certain embodiments, the distance between the device and the substrate is between about 150 and about 350 pm. In certain embodiments, the distance between the device and the substrate is between about 200 and about 300 pm. In certain embodiments, the distance between the device and the substrate is about 200 pm, 225 pm, about 250 pm, about 275 pm, or about 300pm. In a preferred embodiment, the distance between the device and the substrate is about 100 pm.
[0089] In certain embodiments, the methods described herein to produce polycrystalline perovskite fdms further comprise knife-assisted drying. Knife drying comprises applying a high velocity, low pressure gas to the precursor perovskite solution to form a perovskite film on the substrate. An advantage of knife drying in the polycrystalline perovskite film production process is that it helps produce uniform and smooth films. As used herein, an “air knife,” “N2 knife,” or “air doctor” may be used to describe the device that performs knife-assisted drying in the perovskite film production process. The knife may have a gas manifold with a plurality of nozzles that direct a high velocity stream of air or other gas at the perovskite ink on the substrate. The gas used in the knife-assisted drying process may be air, nitrogen, argon, helium, oxygen, neon, hydrogen, and a combination thereof.
[0090] In certain embodiments, the knife-assisted drying takes place at a temperature of about 25 °C to about 250 °C. In certain embodiments, the knife-assisted drying takes place at room temperature (about 25°C). In certain embodiments, the knife-assisted drying takes place at a temperature of about 50 °C to about 100 °C.
[0091] In certain embodiments, the knife-assisted drying takes place at a pressure in a range of about 0 to 500 psi. In certain embodiments, the knife-assisted drying takes place at a pressure in a range of about 5 to 400 psi, about 20 to 300 psi, about 50 to 200 psi, about 100 to 150 psi, about 5 to 25 psi, about 5 to 20 psi, about 10 to 20 psi, about 10 to 19 psi, about 12 to 18 psi, about 12-16 psi, or about 13-16 psi. In certain embodiments, the knife-assisted drying takes place at about 14 psi, about 15, psi, about 16 psi, at about 17 psi, at about 18 psi, or at about 19 psi.
[0092] In certain embodiments, the knife is angled against the device used in the fast coating process and the substrate to create a unidirectional air flow over the as-coated film for enhanced blowing uniformity. In certain embodiments, the knife is angled 0°, 5°, 10°, 15°, 20°, 25°, 30°, 35°, 40°, 45°, 50°, 55°, 60°, 65°, 70°, 75°, 80°, 90°, 100°, 120°, 150°, 155°, 170°, or 180° against the device or the substrate.
[0093] In certain embodiments, after fast coating, the film created from the precursor perovskite solution (while on the substrate) may undergo annealing. The film is annealed at a temperature of at least or above 30 °C. In certain embodiments, annealing employs a temperatureof about, at least, above, up to, or less than 40° C., 50° C., 60° C., 70° C , 80° C., 90° C., 100° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., 180° C., 190° C., or 200° C., or a temperature within a range bounded by any two of the foregoing values. In various embodiments, annealing may take place in a range of, for example, 30-200° C, 50-150° C, 30-180° C, 30-150° C, 30-140° C, 30-130° C, 30-120° C, 30-110° C, or 30-100° C. In a preferred embodiment, the annealing temperature is 70 °C.
[0094] Annealing may take place for a period of time, for example, in a range of about 0 seconds to 400 minutes, about 5 seconds to 30 seconds, about 5 minutes to about 10 minutes, about 10 minutes to 20 minutes, or about 20 minutes to 30 minutes. Annealing can take place for a period of time, for example, of at least 5 seconds, 10 seconds, 20 seconds, 30 seconds, 1, minute, 5 minutes, 10 minutes, 20 minutes, 30 minutes, 60 minutes, 90 minutes, 120 minutes, 180 minutes, 240 minutes, or 360 minutes.
[0095] In certain embodiments of the above method, the resultant perovskite film has a thickness of about 300 nm to about 2000 nm. In certain embodiments, the perovskite film has a thickness of about 300 nm to about 1000 nm, about 300 nm to about 500 nm, about 400 nm to about 800 nm, about 500 nm to about 1500 nm, about 600 nm to about 1800 nm, about 300 nm to about 900 nm, about 1000 nm to about 1500 nm, about 1000 nm to about 2000 nm, about 400 nm to about 1100 nm, about 1200 nm to about 1500 nm, about 1300 nm to about 1800 nm, about 300 nm to about 400 nm, about 400 nm to about 500 nm, about 500 nm to about 600 nm, about 600 nm to about 700 nm, about 700 nm to about 800 nm, about 800 nm to about 900 nm, about 900 nm to about 1000 nm, about 1000 nm to about 1100 nm, about 1100 nm to about 1200 nm, about 1200 nm to about 1300 nm, about 1300 nm to about 1400 nm, about 1400 nm to about 1500 nm, about 1500 nm to about 1600 nm, about 1600 nm to about 1700 nm, about 1700 nm to about 1800 nm, about 1800 nm to about 1900 nm, or about 1900 nm to about 2000 nm.
[0096] In certain embodiments of the above method, the perovskite precursor solutions comprise a composition of Formula I as described above and a solvent. In certain embodiments of the precursor perovskite solution, the solvent is selected from the group consisting of dimethyl sulfoxide, dimethylformamide, dichloromethane, tetrahydrofuran, ' / -butyrolactone, 2- methoxyethanol, N,N'-Dimethylpropyleneurea, N-methyl-2-pyrrol-idone, and acetonitrile, or a combination thereof. In certain embodiments, the solvent is selected from one or more of dimethyl sulfoxide, dimethylformamide, 2-methoxyethanol (2-ME), acetonitrile, methanol, propanol,butanol, tetrahydrofuran, pyridine, alkylpyridine, pyrrolidine, chlorobenzene, di chlorobenzene, di chloromethane, l-methoxypropan-2-ol, 2 -m ethoxy- 1 -methylethyl acetate, 2-butoxy ethanol, 2- butoxy ethyl acetate, 2-(propyloxy)ethanol, ethyl 3 -ethoxy propionate, glycol ethers, di methyl acetamide, acetone, N,N'-Dimethylpropyleneurea, and chloroform. In certain embodiments, the solvent is a mixed solvent. In certain embodiments, the mixed solvent comprises dimethyl sulfoxide (DMSO) and dimethylformamide (DMF). In certain embodiments, the ratio of DMSO:DMF is 1 :3.V. Devices
[0097] The multilayer perovskite composites comprising lead chelating molecules as described herein are useful in a variety of photoactive and photovoltaic applications. The multilayer perovskite composites can be integrated into, for example, photoluminescent devices, photoelectrochemical devices, thermoelectric devices, and photocatalytic devices. Some nonlimiting examples in which the multilayer perovskite composites comprising lead chelating molecules can be applied include solar cells, solar panels, solar modules, light-emitting diodes, lasers, photodetectors, x-ray detectors, batteries, hybrid PV batteries, field effect transistors, memristors, or synapses. The multilayer perovskite composites comprising lead chelating molecules described herein are useful in various solar cell structures, including, but not limited to, n-i-p structured standard solar cells, n-i-p structured perovskite solar cells, p-i-n structured standard solar cells, p-i-n structured perovskite solar cells, bifacial solar cells, bifacial allperovskite tandem solar cells, tandem solar cells, solar cells comprising low bandgap perovskites, and organic solar cells.
[0098] In certain embodiments, the subject matter disclosed herein is directed to a solar cell, comprising: one or more transparent conductive oxide layers; one or more conductive electrode layers; one or more electron transport layers; and an active layer comprising the multilayer perovskite composite described herein.
[0099] In certain embodiments of the above solar cell, the solar cell comprises: a transparent conductive oxide layer; an active layer comprising the multilayer perovskite composite described hereinan electron transport layer; an optional buffer layer; and a conductive electrode layer.
[0100] In certain embodiments of the above solar cell, the hole transport layer of the multilayer perovskite composite is disposed on the first transparent conductive oxide layer; the perovskite film of the multilayer perovskite composite is disposed on the hole transport layer of the multilayer perovskite composite; the electron transport layer is disposed on the perovskite film; the buffer layer, if present, is disposed on the electron transport layer; and the conductive electrode layer is disposed on the buffer layer.
[0101] In certain embodiments of the above solar cell, the transparent conductive oxide layer is ITO; the hole transport layer of the multilayer perovskite composite is PTAA with bathocuproine as lead chelating molecules; the electron transport layer is Ceo; and the conductive electrode layer is copper.
[0102] In embodiments of the above solar cell, the solar cell exhibits a Power Conversion Efficiency (PCE) between about 18% to 26%. In certain embodiments, the solar cell exhibits a PCE of about 22%. In certain embodiments, the solar cell exhibits a PCE of about 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, or 26%.
[0103] In embodiments of the above solar cell, the solar cell is stable. As used herein, the term “stable” refers to the solar cell’s ability to continue functioning at high efficiency (>85%) continuously for an extended period of time. In certain embodiments, the solar cell retains at least 90% of its PCE for between about 2000 to 7000 hours of continuous 1 sun illumination at real operational conditions (56-62 °C). In certain embodiments, the solar cell retains at least 90% of its PCE for between about 3000 hours of continuous 1 sun illumination. In certain embodiments, the solar cell retains at least 95% of its PCE for about 2000 hours of continuous 1 sun illumination.EXAMPLESMaterials and MethodsI. Materials
[0104] Materials: All the solvents were purchased from Sigma-Aldrich with purity of 99.9% (HPLC), including 2-methoxyethanol (2 -ME), dimethyl sulfoxide (DMSO), toluene (TL), isopropyl alcohol (IP A). PbI2 (99.999%) was purchased from Advanced Election Technology Co., Ltd. FAH2PO3 was synthesized in our lab according to our previous publication. Formamidinium iodide (FAI), formamidinium chloride (FAC1), guanidinium iodide (GAI), phenylammonium chloride (PEACI) and phenyl ammonium tetrafluoroborate (PEABF4) were purchased from GreatCell Solar. C60 was purchased from Nano-C Inc. All other solid chemicals were purchased from Sigma-Aldrich, including PTAA (average Mn 7,000-10,000), CsI (99.999%), L-a- phosphatidylcholine (LP, 99%), ZnC12 (99.999%), carbohydrazide (CBH, 98%), p- Toluenesulfonic anhydride (TSA) L-Ascorbic acid (VC, 99%), meso-2,3-Dimercaptosuccinic acid (MDSA, 98%), Ethylenedi aminetetraacetic acid (EDTA, 99.99%), bathocuproine (BCP, 96%), bathophenanthroline (BPhen, 97%) and 1 , 10-phenanthroline (OPhen, 99%).II. Methods
[0105] Device fabrication
[0106] The pre-patterned ITO glass substrates (15 Q sq’1) were cleaned by acetone in an ultrasonic machine. Before using, all the substrates were treated by UV-ozone for 15 min. The PTAA layer and perovskite layer were prepared by blade-coating at room temperature inside a fume hood. PTAA solution with a concentration of 2.2 mg mL’1(in toluene) was first blade-coated onto ITO glass substrates at a speed of 20 mm s'1and a coating gap of 150 pm. For the BCP and TSA based devices, they were dissolved in PTAA solution (2.2 mg mL1) with the mass ratio of 2%, respectively, then blade-coated onto ITO substrate with the same method of the pure PTAA. For the VC, MDSA, and EDTA based devices, they were dissolved in 2-ME (0.2 mg mL’1), respectively, then blade-coated onto the pure PTAA layer. The 1.1 M FAo.gCso.iPbE was prepared by directly mixing FAPbb (in 2-ME), CsPbE (in DMSO) and other additives (in 2-ME) and diluting with 2-ME solvent prior to blade coating. 0.23% v / v FAH2PO3, 2.3 mgmL-1FAC1, 0.25 mg mL’1PEABF4, 12.36 mg mL’1GAPbb, 0.18 mg mL’1LP, 0.57 mg mL’1CsI, 0.74 mg mL’1ZnC12 and 0.18 mg mL’1CBH were added into the precursor solutions as additives. These additives are used to achieve high-efficiency and stable devices by optimizing the perovskite crystallization process and passivate the surface and grain boundaries of perovskites. 1Subsequently, the precursor solution was blade-coated onto the PTAA-covered ITO glass substrates with a gap of 300 pm at a coating speed of 20 mm s'1. The wet perovskite films were then transferred onto hot plate and annealed at 150 °C for 4 min in air. The thickness of the final perovskite films is 800-900 nm.
[0107] The as-prepared FAo.9Cso.iPbl3 perovskite films were then surface processed with1 mg ml1PEACI (in IP A) solution by blade-coating method. This PEACI surface processing was used to obtain higher Voc and better light-soaking stability. To quickly check the effect of different LCMs on the light-soaking stability of the device, none of the samples fabricated for the accelerated stability test had PEACI surface processing. The coating speed and gap is 20 mm s'1and 150 pm, respectively. Before the thermal evaporation of electron transport layer, the surface processed perovskite films also need to be annealed at 100 °C for 3 min to remove the solvent residual. The solar cells were completed by thermally evaporating C60 (30 nm, 0.15 A s'1), BCP (6 nm, 0.1 A s'1), and 150 nm copper (1 A s'1). 100 nm MgF2 layer was evaporated onto the glass side of ITO substrates as an anti-reflection layer. The active area of solar cells is 8 mm2 (4 mm x2 mm determined by a metal shadow mask).
[0108] The minimodules were fabricated on pre-patterned large ITO glass substrates with Pl width of 30 pm followed by the same procedure as the small solar cells. The laser scribing was performed twice with a Keyence laser marker (MD-U1000C, 355 nm). The width of each subcell is 6 mm, while the final P2 and P3 widths were measured to be -110 and -75 pm, respectively. The total width of the non-working area was measured to be -320 pm, giving a GFF of 94.7%. A polydimethylsiloxane (PDMS) layer was attached to the front side of the perovskite solar cells as an anti -refl ection coating.
[0109] The GFF of minimodules was calculated from the height-scanning distance curves measured by a Brucker Dektak XT Profiler.
[0110] Sample characterization
[0111] XRD: Regular XRD and GIXRD measurements were both carried out with a Rigaku SmartLab diffractometer using Cu Ka radiation (). = 1.5418 A), and the height of films was calibrated before each measurement. The precipitation was collected from the bottom of BCP / FAPbb or BCP / Pbb mixture solution by a filter membrane and dried in a vacuum oven at room temperature to obtain the light-yellow powder. Then, the powder was annealed at 100 °C for 10 min to observe the changes on the powder. The crystalized BCP was formed by dropping theBCP solution (in 2-ME) onto a piece of glass and drying at 80 °C for 30 min to slowly remove the solvent.[001121 FTIR: FTIR spectra were acquired with a PerkinEImer Spectrum Two FT-IR spectrometer. After LCMs (in 2-ME) were mixed with FAPbli solution (in 2-ME), the peak positions of several characteristic peaks shifted due to the chelation of LCM and Pb2+. TSA chelates with FAPbE by the Pb-0 bonds. The O atoms in TSA were bonded to S atoms, so the TSA»Pb2+chelation makes the electron cloud in S=O bonds shift towards Pb2+. Compared to the TSA solution, the TSA-FAPbE mixture solution has peak shift from -1382 cm'1to -1373cm'1, corresponding to the signal of S=O stretching in TSA molecular. For the VC-FAPbb mixture solution, the peak position of C=O stretching in VC had peak shift from -1738 cm'1(VC only solution) to -1725 cm1. For the MDSA-FAPbE mixture solution, the peak position of C=O stretching in MDSA had peak shift from -1739 cm'1(MDSA only solution) to -1724 cm'1. For the EDTA-FAPbl3 mixture solution, the peak position of C-N stretching in MDSA had peak shift from -1739 cm'1(EDTA only solution) to -1726 cm'1.
[0113] XPS characterization: XPS characterization was performed on Kratos Axis Ultra DLD X-ray Photoelectron Spectrometer by using a monochromatized Al Ka source (hv = 1486.6 eV).
[0114] Photocurrent measurement: The J-V characteristics of solar cells and minimodules were performed using a Xenon-lamp based solar simulator (Oriel Sol3A, Class AAA Solar Simulator) and the output light intensity was calibrated to 100 mW cm'2by a silicon reference cell (Newport 9115OV-KG5). All devices were measured using a Keithley 2400 source meter with a backward scan rate of 0.1 V s'1in air at room temperature. There was no preconditioning before measurement. No temperature controlling was used for J-V curve measurement. The cell temperature was 35-40 °C when the device’s efficiency was measured under the solar simulator, so the efficiency would be higher if the device is cooled to 25 °C.
[0115] Stability measurement: There are three light sources that have been used for the light soaking stability test: LSI, LS2 and LS3. LSI is a Xenon light source (BenQ, B09813LFNK) with a 400 nm long-pass filter, LS2 is a white LED array with UV LEDs added (Lightimetunnel, HYG08-60>< 10W-W), and LS3 is a UV-filtered light emitting plasma (Gavita Pro 270e LEP US) light source with 450 nm long-pass filter. LSI has a radiation light wavelength of 390-680 nm and has a very good light intensity uniformity with variation less than 5% over a large area of 12 cm x10 cm. So, it is used for light soaking stability study for minimodules with an area of upto 100 cm2. LS2 is uniform light intensity over an area of 18 cm * 12 cm. LS2 has radiation light at 390 - 820 nm and is used for the light-soaking stability study of small area cells and the minimodules with an area of less than 200 cm2. LS3 has a much broader spectrum of 440 - 1060 nm and has a light intensity uniformity with variation less than 5% over a smaller area of 5 cm x 5 cm. It is used for light soaking stability study of small area cells. For light soaking stability, the devices were exposed to different light sources.
[0116] After light soaking for different durations, the devices were taken to solar simulator for efficiency measurement, after which the devices were returned to continue light soaking.
[0117] MPP Tracking: Maximum power point (MPP) tracking testing was conducted using a MPPT system with 32 channels (PAS-GV-32CH) from Enlitech Inc. For each cycle, it continuously measures the J-V curves for 5 times and automatically finds the MPP of each curve. It will select the average efficiency among the 5 J-V curves. And then the load to the device is set based on the measured J-V curves for 2h to make the device to work at MPP point until the next measurement.
[0118] Device encapsulation: All the small solar cells and minimodules were encapsulated with cover glass and epoxy resin (Devcon epoxy Tube 14250) on the Cu side. A LED light was used as the light source for the stability test in air (relative humidity 30-60 %). The temperature of solar cells was measured to be 50-60 °C due to the heating effects of the lamp. The PCEs of the solar cells and minimodules modules monitored by J-V characteristics under simulated AM 1.5G one sun illumination (Oriel Sol3A, Class AAA Solar Simulator).
[0119] Photoluminescence and mapping: The PL signal was detected by the PicoQuant PMA Hybrid single photon counting module with TCSPC technology. PL mapping was conducted with PicoQuant MicroTime 100 and FluoTime 100 system at room temperature. PicoQuant PDL 828 “Sepia II” multichannel diode laser was used as the laser source and 405 nm pulsed laser was used for the measurements.
[0120] Trap density measurement: The standard TAS and DLCP measurements were performed by using an Agilent E4980A precision LCR meter. The DLCP measurement was conducted in the DC bias range of 0 V to 1.2 V (near Voc). While the amplitude of the AC biases was ranging from 20 to 200 mV. For each AC bias, an additional offset DC voltage was applied to keep the maximum forward bias constant. The measured capacitances at each DC bias weregathered with a homemade computer program. For the TAS measurement, the DC bias was fixed at 0 V and the amplitude of the AC bias was 20 mV. The scanning range of the AC frequency was 0.02 - 2000 kHz.
[0121] SEM measurement: SEM images were taken on FEZ Helios 600 Nanolab Dual Beam System. For SEM characterization, the accelerating voltage of electron beam is 5 kV, and the current is 86 pA.
[0122] NMR measurement:1H-NMR spectra were acquired with a Bruker AVANCE III 600 MHz NMR Spectrometer. The NMR liquid samples were prepared as follows: The samples were first prepared on glass substrates and then annealed at 150 °C for 4 min to form perovskite films, and then some powder was collected by scratching the perovskite from glass substrates. These scraped powders were then quickly transferred to NMR tubes filled with deuterium oxide (D2O) and left to stand overnight, so that the soluble substances in the powder could be completely dissolved in D2O.
[0123] Modeling of module efficiency
[0124] The modeling of efficiency, current density, and fill factor as a function of subcell width in minimodules refers to our previous publication (Ref 48). In this work, we improved the laser scribing to shrink the non-working area width (Wd) from 430 pm to 320 pm. The P2 width (WP2) became 110 pm, making the transfer length (LT) 100 pm. The subcell length (L) increased to 55 mm. The JV parameters of the small devices were also improved, including the average Jsc of 25.3 mA cm'2, Voc of 1.17 V, FF of 0.82 and efficiency of 24.1%. The maximum power point (MPP) also changes to (1.00 V, 24.24 mA cm'2). All other parameters used in this model, like sheet resistance of ITO substrate (Rsh and RshP2), busbar width (S), busbar thickness (w) and resistivity of busbar metal material (pmetai), are the same as those in the above publication.
[0125] DFT calculations
[0126] First-principles density functional theory (DFT) calculations were performed using the VASP code with projector augmented-wave potentials. A plane-wave energy cutoff of 500 eV and single T k-point were used for all the surface and interface calculations. The exchangecorrelation interactions were treated with the generalized gradient approximation of the Perdew- Burke-Emzerhof (PBE) parametrization. Grimme’s D3 correction were also included to deal with the van der Waals interactions. The (001) surface with either FAI or Pbh termination of tetragonal FAPbE (a=b=8.95A, c=12.72A) was used for adsorption calculations. Each surface slab wasmodeled with five layers of FAI / Pbb. The top two layers or the two layers near the interface were allowed to relax with force tolerance of 0.01 eV / A on each atom, while other layers were fixed to their bulk positions. The surface and interface slabs were built with lateral dimensions of 17.895 x 17.895 A. A vacuum with thickness of at least 15 A was used for all the slab calculations. Density of states calculations were performed on a 4x4x1 k mesh.Example 1: Passivating the Perovskite-HTL interface.
[0127] One straightforward method to passivate the bottom perovskite-HTLs interface is to blend some passivation species in HTLs. Passivation species generally need to have specific interactions with ions on perovskite surface. Described herein are lead chelation molecules (LCMs) which, while commonly used in water purification or treatments of lead poisoning, have been barely studied for perovskites (25). Fig. 1A illustrates the chelation between LCMs and Pb2at the interface of perovskite films and HTLs which enhances the interaction of HTL with perovskites. The molecular structure of several selected LCMs is shown in Figs. 2-3; these LCMs provide two or more lone pair electrons to chelate with Pb in perovskites, for example, bathocuproine (BCP), p-Toluenesulfonic anhydride (TSA), L-Ascorbic acid (VC), meso-2,3- Dimercaptosuccinic acid (MDSA), and ethylenediaminetetraacetic acid (EDTA). The chelation of LCMs with Pb2+is manifested by the precipitation of lead ions after adding them into perovskite solution. BCP was selected for demonstration because of its low solubility of < 0.2 mg mL'1in 2- ME, the main solvent in perovskite ink solutions used for a fast-blading process. Fig. IB shows the photographs of the solutions for BCP (in 2-ME), formamidinium lead triiodide (FAPbh) in 2- ME / DMSO and the mixture of BCP and FAPbh. When BCP was mixed with FAPbh solution, precipitation was noticed even at a very low BCP concentration of < 0.05 mg mL'1, indicating the reaction product, ostensibly BCP chelated to lead ions, has lower solubility than BCP. The same precipitation phenomenon was observed when TSA was blended with FAPbh (Fig. 4). X-ray diffraction (XRD) pattern of the pale-yellow precipitates is shown in Fig. 1C and Fig. 5 which includes diffraction peaks of multiple compounds and phases including Pbh’BCP (11.06°) and some solvated phases. The diffraction peak in Fig. 1C was assigned to Pbh^BCP, because the same diffraction peak was observed from the precipitates of Pbh and BCP mixture solution (Fig. 6). However, all the peaks corresponding to solvated phases, such as Pbh*DMSO, disappeared after removing DMSO by annealing the precipitates at 100 °C, accompanied with a change ofpowder color to yellow. The presence of the peak corresponding to Pbh’BCP in the annealed powder indicates that the interaction of BCP with Pb2+is even stronger than that of DMSO with Pb2+. Fourier-transform infrared spectroscopy (FTIR) measurement was conducted to study how BCP interacts with perovskite precursors (Fig. 1D-E). The C=N stretch in BCP locates at a smaller wave number of 1622 cm’1than that of FAPbL (1720 cm’1) so that they can be distinguished (26). After mixing with FAPbb, the C=N stretching peak from BCP shifted to a smaller wavenumber of -1606 cm’1, which agrees with the shifting of electron cloud toward Pb2+ions. These data prove that there is a strong interaction between BCP and Pb2+ions. The same FTIR shift was observed when all other LCMs were mixed with FAPbL (Fig. 7), supporting the Pb2+chelation effect of these molecules. The phenanthroline group in BCP has two pyridine rings. Moreover, the C=N FTIR peak completely shifted, rather than splitting into two peaks, indicating that the N atom in both pyridine groups of BCP interacted with Pb2+, resulting in a chelation of Pb2+ions with BCP. The chelation effect results in more robust and stable interaction with perovskites than single pyridine group. The X-ray photoelectron spectroscopy (XPS) study also confirms the interaction of BCP with Pb2+ions, as there was a shift of Pb 4f peak after the perovskite film was covered by a spun thin BCP layer (Fig. IF). The decrease of Pb2+binding energy is consistent with the chelation of BCP with Pb2+due to the sharing of electrons from N atoms (in BCP) with Pb2+. The binding energies of a BCP and a DMSO molecule on Pbb-terminated and FAI-terminated (100) FAPbls perovskite surfaces were calculated. On the PbL termination, the two N atoms of BCP bond to a single Pb atom of FAPbL (Fig. 1G), while for DMSO only a single O-Pb bond forms (Fig. 1H). The binding energy of BCP with FAPbL is 1.71 eV, and it is 0.84 eV for DMSO. For the FAI termination, hydrogen bonding forms between the two N atoms of BCP and one H atom of FA (Fig. II). The binding energy of BCP with FAPbL is 1.41 eV. For DMSO, hydrogen bonding forms between the O atom of DMSO and two H atoms of FA+(Fig. 1 J), resulting in a smaller binding energy of 0.57 eV. It is seen that on both surfaces with Pbb and FAI termination, the binding energy is 2-3 times larger for BCP than for DMSO.Example 2: Addition of Lead Chelating Molecules to Hole Transport Layer (LCMs)
[0128] LCMs were introduced to the poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine (PTAA) layer by mixing them in toluene (TL) at different ratios if the LCMs are soluble in TL, such as BCP and TSA, or blade-coated onto the PTAA layers for insoluble LCMs including VC,MDSA and EDTA (details provided in Methods - Device Fabrication Section). The perovskite composition of FAo.9Cso.1Pbh was used for device fabrication due to its reported high operational stability (5, 27-29). Both HTL and perovskite layers were coated in ambient conditions using nitrogen knife assisted blading (30). Steady-state photoluminescence (PL) and PL lifetime measurements were conducted to understand how LCMs blended in PTAA impact the interfaces of perovskites with HTLs. Several prior studies showed that the embedded perovskite / HTL interface could be even more defective than the top perovskite surface depending on the process conditions (76). When the PL intensity of the perovskite film sandwiched by PTAA to keep charge extraction condition same at both sides were compared, a ~ 40% weaker PL from bottom side (Fig. 8) was observed, indicating that bottom interface is indeed more defective. When incident excitation light came in from the indium tin oxide (ITO) side to examine bottom interface, as illustrated in the inset of Fig. 9A, BCP notably enhanced the steady state PL intensity by 1.7 times (Fig. 9B). The PL lifetime at the bottom of perovskite films was also increased from 195 ns to 452 ns (Fig. 9C), proving that pre-embedded BCP in PTAA reduced the non-radiative recombination defects at the bottom surface of perovskites. However, the PL lifetime improvement may also be caused by the changed crystallinity of the perovskite layer, because HTLs are known to impact the perovskite crystallinity (31). To verify the passivation function of BCP to perovskites, a BCP layer was spun on top of perovskites, as illustrated in the inset of Fig. 9D, to exclude the impact of perovskite crystallinity and measured the PL spectra and PL lifetime changes with light incident from air side. Figs. 9E-9F show that BCP enhanced the PL intensity by 1.2 times, and improved PL lifetime to 1.43 ps, which confirms the passivation effect of BCP to perovskites. To evaluate how uniform the bottom surface of perovskites was passivated, fluorescence lifetime imaging microscopy (FLIM) was used to study optical property of the bottom perovskites. Hereafter the samples or devices with pure PTAA or BCP:PTAA HTLs are referred as control and target samples or devices, respectively. As shown in Fig. 9G-H, the grains can be clearly distinguished in PL mapping showing apparent grain size of 1-2 pm. The PL intensity and lifetime are relatively uniform in both control and target films over a measurement area of 40 pm x 40 pm, but the target film showed 1.5 times stronger PL and 1.1 times longer PL lifetime. The passivation effects of BCP and DMSO were investigated by density function theory (DFT) calculation. It has been found that perfect Pbh- and FAI-terminated surfaces do not form deep gap states. Individual I vacancy also does not form gap states. However, Pb-Pb dimers could form on the surface with an extra Ivacancy, which can be easily formed by loss of iodide. The Pb-Pb dimer induces gap states, due to Pb 5p - Pb 5p bonding. The deep gap states can be eliminated by BCP but not by DMSO. We used the PbL-terminated (100) surface to reveal the effects. Fig. 91 shows that the Pb-Pb dimer caused by the formation of two iodide vacancies create deep gap states. When a BCP molecule presents near the Pb-Pb dimer, the two N atoms bond to one Pb atom of the dimer, breaking the dimer structure (Fig. 9J). This is because the Pb-N bonds formation partly saturates the Pb coordination. As shown in Fig. 9K, the gap states are eliminated after breaking the Pb-Pb dimer. However, DMSO is unable to break the Pb-Pb dimer due to only one Pb-0 bond formation. As shown in Fig. 10A, the Pb-Pb dimer remains after DMSO molecule binds to the Pb-Pb dimer. As a result, the gap states remain as shown in Fig. 10B.Example 3 - Chelation Improves Device Performance
[0129] To evaluate how the LCMs impact perovskite solar cell performance, perovskite solar cells were fabricated with the structure ITO / HTL / perovskite / Ceo / BCP / copper (Cu). As shown in Fig. 11, the stability of all the devices was significantly improved by incorporating LCMs either into or onto HTLs under accelerated light induced degradation test (~200 mW cm'2, at opencircuit condition, ambient condition, 59-65 °C). Among all the LCMs tested, BCP and TSA resulted in higher device efficiency with the improved open circuit voltage (Voc) and fill factor (FF) (Fig. 12). The higher efficiencies can be explained by the better mixing of BCP and TSA with PTAA, because the benzene group in BCP or TSA should induce TT-TT interaction with PTAA (32), facilitating carrier transfer from perovskites to PTAA. Another reason is that BCP and TSA are much less soluble in the solvents of perovskites.
[0130] To verify whether chelation with phenanthroline groups, rather than other functional groups in BCP, dominates the device performance improvement, leads ions’ interaction with other BCP-like molecules was investigated. Fig. 13 shows several molecules with some functional groups of BCP, including bathophenanthroline (BPhen) and 1,10-phenanthroline (OPhen). BCP has three functional groups: methyl, phenyl and phenanthroline groups, while BPhen only has the latter two. As shown by the photocurrent curves and device performance statistic results in Fig. 14, the BCP- and BPhen-based devices exhibited comparable enhancements of device efficiency, which excluded methyl groups as the efficiency-enhancing functional group. Removing the phenyl group of BPhen yields OPhen. OPhen in HTL also increased Voc and PCEof the devices, confirming that the phenanthroline group dominates the PCE enhancement. It is noted that the solubilities of BPhen and OPhen in 2-ME are ~1 mg m ’1and -5 mg mL'1, respectively, much higher than that of BCP. Since embedding BPhen and OPhen in PTAA still enhanced device efficiency, it can be inferred that low solubility reaction products, or chelation products, that retain these functional groups form at bottom interfaces. The best efficiency was still obtained from BCP based devices, indicating a low solubility in 2-ME is very important so that the passivator does not quickly dissolve into perovskite solution.
[0131] To find out what defects were reduced by the introduction of BCP to PTAA, the trap density change of the devices was measured using thermal admittance spectroscopy (TAS) and drive-level capacitance profiling (DLCP). The trap density of state (tDOS) profiles in Fig. 15A showed three distinct trap bands for both control and target devices resembling previous reports for iodide perovskites. These trap bands were assigned to negatively charged iodine interstitials ( / ) and positively charged iodine interstitialsrespectively (33). The density of / did not change obviously in the perovskites, while the / ;+density was reduced by the introduction of BCP into PTAA. DLCP measurement gave consistent results that I~ density did not change throughout the devices, while / ^density reduced notably (Fig. 16). We plotted the change of / + densityIftarget— Ifcontroi I) 'nperovskites across the device from 0,0 to HTL side induced by BCP. As shown in Fig. 15B, BCP mainly reduced / density in perovskites near HTL. Recent study of perovskite with the same perovskite composition showed a similar reduction of / ;+density while unchangeddensity upon thermal annealing of the films in the dark for several hundreds of hours (22). Since it was accompanied with the reduction of amorphous region and appearance of associated voids at the bottom interface close to PTAA, the If may be rich in the amorphous phase at the bottom of the perovskite films, and BCP:PTAA HTL reduced them.
[0132] To verify the hypothesis, scanning electron microscope (SEM) measurement was conducted to examine the voids caused by the recrystallization of the amorphous region in the control perovskite devices using PTAA as HTL. The devices were encapsulated to avoid the impact of moisture and oxygen and soaked under room light for -1000 h to allow recrystallization to occur. The fresh and soaked perovskite films were peeled off from the ITO / PTAA substrate to expose the bottom surfaces, which were then subject to SEM study. As shown in Fig. 15C-15F, the average grain size of these perovskite films was 1-2 pm, agreeing with the PL mapping result.For the fresh samples with or without BCP, there is no notable morphology difference at the bottom of perovskite films. After aging, many shallow voids showed up around the grain boundaries at the bottom of the aged control samples, resembling the result of thermal annealing of such films (22). In contrast, the bottom morphology of the aged target sample was nearly indistinguishable from the fresh target samples, indicating that BCP notably reduced the formation of amorphous phase at the bottom of the perovskite films. We conducted grazing incident X-ray diffraction patterns (GIXRD) measurement to direct examine the crystallinity of perovskites close to the HTL using peeled-off fresh samples. As shown by the GIXRD pattern in Fig. 15G, the peak of the (100) plane is not only 60% stronger but also 8% sharper, confirming the improved crystallinity of the perovskite bottom layer induced by BCP. The reduced amorphous regions should contribute to the / + density reduction at the bottom of perovskite films (Fig. 15A).
[0133] BCP could reduce the amorphous regions. Prior study shows that the trapped solvent DMSO may also cause the amorphous phase in the perovskite bottom and grain boundaries (6). Then we measured the trapped DMSO content in perovskite films after film annealing using hydrogen nuclear magnetic resonance spectroscopy (’H-NMR). Perovskite films fabricated on different HTLs were scraped off from the substrates and dissolved in deuterium oxide. The content of DMSO in the perovskite film was determined by the ratio of the integral area of the characteristic peak ofin DMSO to that of FA+. As shown in Fig. 15H and Fig. 17, the peaks at 7.71 ppm and 2.63 ppm are assigned to -CH in FA+and -CH? in DMSO, respectively (34, 35). The DMSO / FA+atomic ratio in the control sample was 0.13%, while it reduced to 0.08% in the target sample (Table 1). Therefore, BCP in PTAA does reduce the amount of trapped DMSO. It can be explained by the stronger interaction of BCP with Pb2+than DMSO (Fig. 1C). BCP competes with DMSO to coordinate with Pb2+at the bottom region during the film formation process, so BCP:PTAA reduced the amount of DMSO bounded to Pb2+. As a result, less DMSO was trapped, resulting in less amorphous perovskites. The reduction of defective amorphous perovskite by BCP thus improves device efficiency and stability. The trapping of DMSO can be very non-uniform particularly for large area perovskite films coating in production line, depending on the local vapor pressure which could change from location to location dynamically. Reduced trapping of DMSO explains the better uniformity of perovskite films, and thus is expected to enhance perovskite module efficiency.Table 1 DMSO residual ratio in the perovskite films fabricated with and without BCP in PTAA.Example 4 - Optimization of Device Efficiency and Stability
[0134] Considering that the introduction of BCP in PTAA improved efficiency and stability of PSCs simultaneously, BCP was chosen for the device efficiency and stability optimization. As shown in Fig. 18B, the control devices have a short circuit current density (Jsc) of 25.2 mA cm'2, Voc of 1.13 V, FF of 0.80, and PCE of 22.7%, consistent with previous results (5). BCP is broadly used as an electron transport material in organic light emitting diode (36), organic solar cells (37) and particularly p-i-n structure perovskite solar cells (35), and its hole blocking property is often reported 39-41'). Therefore, its loading ratio in PTAA needed to be optimized for optimal hole collection, which was evaluated by the efficiency of the resultant small area perovskite cells. Perovskites have sufficient long carrier diffusion so that photogenerated charges can still be efficiently extracted even some local contacts are blocked, which has been demonstrated by nano-contact perovskite solar cells or those with non-continuous insulating polymer interfacial layers (20. 42-44). As shown by the statistics device performance data in Fig. 18C, a sufficient BCP of -2 weight percent (2 wt%) in PTAA was needed to increase the FF of the perovskite devices. When the BCP loading in PTAA exceeds 2 wt%, the device FF dramatically reduced, which should come from the reduction of hole collection. This is confirmed by the same variation trend of Jsc with that of FF with varied BCP loading ratios. In contrast, the device Voc monotonically increased from 1.13 V to 1.17 V when BCP loading ratio was increased from 0% to 2 wt%, and then Voc saturated with further increased BCP ratio. This is because hole extraction is not needed at Voc condition. The champion target devices with optimal BCP showed a Jsc of 25.5 mA cm'2, Voc of 1.17 V, FF of 0.825, resulting in an efficiency of 24.6%, a new record for p-i-n structure devices. The average PCE was increased to 24.1%, and the photocurrent hysteresis was not obvious in either type of devices. The observed small variation for the efficiency of small-area devices agrees with the uniform distribution of BCP in PTAA and uniform passivation. The average PCE of the control devices is -22.0%, which is consistent with what was reported previously using the same CsI or FAI rich perovskite composition (5). The pre-embedded BCP in PTAA also greatly improved the device stability. Three different light sources were usedfor stability measurement based on the device area and lifetime of light sources (Fig. 19A). The light intensity to the devices from all light sources was controlled to be -100 mW cm’2, determined by a silicon solar cell that is used for solar simulator light intensity calibration, as shown in Fig. 20. The Xenon light source with 400 nm long pass filter (LSI) and the white LED light source (LS2) have more deep blue or UV light and the light emitting plasma light source with 450 nm long pass filter has a stronger infrared component. Deep UV light is filtered to simulate the final PV modules which have a UV absorber such as ZnO coating (45, 46). We also evaluated whether the spectra of these light sources impact solar cell stability. Our study shows that UV light in solar spectrum does accelerates perovskite device degradation, but filtering UV light of solar spectrum made perovskites to be as stable as those measured under white LED light source (Fig. 21). As shown in Fig. 22 the degradation behaviors of these devices are very similar, showing the minor spectral differences of the three light sources do not impact the stability of perovskite solar cells when the deep UV light is filtered. The small area device stability was tested by soaking the devices at open circuit condition by the light source LS2. The devices were heated to 55-61 °C by illumination during the stability testing, and no additional temperature control was applied. Fig. 23 shows typical J-V curves of the devices after light soaking for different durations, and average PCEs over time for the control and target devices are shown in Fig. 18D. For the control devices, the efficiency reduced to 90% of its initial efficiency (T$>o lifetime) after light soaking for 1890 hours (hr). In contrast, the T90 lifetime of the target devices under light soaking was increased to 3010 hr. Previous studies concluded that light soaking stability measured at Voc condition is an even harsher stability testing than the maximum power point (MPP) stability testing, because accumulated photogenerated excess charges accelerate perovskite degradation by enhancing ion migration (47). To verify it for this perovskite composition, we tested the same batch of control devices at the MPP and Voc conditions, showing a much longer T90 lifetime at MPP testing. (Fig.24)
[0135] Prior studies show that non-uniform photocurrent from different subcells would notably reduce the FF of resultant modules (48). BCP:PTAA significantly improved the uniformity of perovskite films, evidenced by the small variation of device performance from batch to batch, which should also improve the module performance. We thus upscaled the 0.08 cm2small-area devices to minimodules with aperture areas of 20-30 cm2defined by the photomask as shown in Fig. 25. The minomodules have a subcell width of 6.0 mm and a dead area width of 320 pm (Fig.26), resulting in a geometry filling factor of 94.7%. The photograph of a typical minimodule is shown in Fig. 18E. As shown by the photocurrent curves in Fig. 18F, the addition of BCP obviously enhanced the FF and Voc of the minimodules. Several minimodules were sent to National Renewable Energy Laboratory (NREL) for efficiency certification. The certified champion aperture PCE of the perovskite minimodules reached 21.8% with an aperture area of 26.9 cm2from J-V scanning (Fig. 27). The stable power output measurement method, i.e., measuring the stabilized photocurrent near the maximum power point, gave a stabilized efficiency of 21.1% (Fig. 18G and Fig. 28). Using the recent established model (48), we calculated the minimal small cell efficiency that is needed to yield the module efficiency of 21.8% (or stabilized PCE of 21.1%) by assuming the perovskite device is perfectly uniform throughout the minimodules. As shown in Fig. 18H, with more details in Fig. 29, the minimal small area cell efficiency needs to be 24.6% (stabilized PCE of 24.1%). This efficiency is very close to the measured average efficiency of small cells, indicating the perovskite films are very uniform. The minimodules with BCP:PTAA HTL have a Voc of 1.17 V, the same as small area cells. The photocurrent density from each 6 mm wide subcell in the minimodule is 23.6 mA cm'2, which is close to the calculated value (Fig. 29A). Notably the minimodule with this large area has a large FF of 0.803, which is also the highest FF reported for perovskite minimodules. Calculation result in Fig. 29B also shows that the FF of 0.803 already reached the theoretical upper limit based on the attainable small area device performance, indicating there is negligible efficiency loss caused by nonuniformity of device performance. This again confirms the excellent uniformity of the perovskites over the whole minimodule area. Benefiting from the stable perovskite small devices, the minimodules are also very stable. The minimodule stability was also evaluated by light-soaking with 5-6 minimodules in ambient condition at Voc condition under light source LS2 with light intensity of -100 mW cm'2. The minimodule temperature was measured to be 56-62 °C and was kept constant during the testing process. Instead of using higher testing temperature, the actual module operation temperature was used to keep the underneath photochemistry to be the same with real operation conditions. Fig. 30 shows typical J-V curves of the control and target minimodules after light soaking for different durations. The average T90 lifetime of the minimodules with BCP:PTAA HTL reached -2130 hr, while the control minimodules only have a T90 lifetime of -1380 hr (Fig. 181).
[0136] The introduction of LCMs into PTAA HTL improved the efficiency, stability, and reproducibility of the p-i-n structure perovskite solar cells. Due to the strong interaction between the phenanthroline group in BCP and Pb2+and the low solubility of BCP’Pbb in 2-ME, BCP stayed at the bottom of perovskite layer during solution coating. With reduced trap density at the bottom of the perovskite layer and charge recombination at the PTAA / perovskite interface, the efficiency of the devices with BCP was increased to 24.1%. With BCP in PTAA layer, the amorphous layer and DMSO residue in perovskite layer were obviously decreased, leading to the reduced void formation around the grain boundaries during light soaking. BCP in PTAA also increased the T90 lifetime from -1890 hr to -3010 hr. The champion minimodules with an aperture area of 26.9 cm2showed a certified efficiency of 21.8% (stabilized at 21.1%).
[0137] Efforts have been made to ensure accuracy with respect to numbers used (e.g., amounts, temperature, etc.) but some experimental errors and deviations should be accounted for.
[0138] One skilled in the art will recognize many methods and materials similar or equivalent to those described herein, which could be used in the practicing the subject matter described herein. The present disclosure is in no way limited to just the methods and materials described.
[0139] Unless defined otherwise, technical, and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this subject matter belongs.
[0140] Throughout this specification and the claims, the words “comprise,” “comprises,” and “comprising” are used in a non-exclusive sense, except where the context requires otherwise. It is understood that embodiments described herein include “consisting of’ and / or “consisting essentially of’ embodiments.
[0141] Where a range of values is provided, it is understood that each intervening value, to the tenth of the unit of the lower limit, unless the context clearly dictates otherwise, between the upper and lower limit of the range and any other stated or intervening value in that stated range, is encompassed. The upper and lower limits of these small ranges which may independently be included in the smaller rangers is also encompassed, subject to any specifically excluded limit in the stated range. Where the stated range includes one or both of the limits, ranges excluding either or both of those included limits are also included.
[0142] Many modifications and other embodiments set forth herein will come to mind to one skilled in the art to which this subject matter pertains having the benefit of the teachings presented in the foregoing descriptions and the associated drawings. Therefore, it is to be understood that the subject matter is not to be limited to the specific embodiments disclosed and that modifications and other embodiments are intended to be included within the scope of the appended claims. Although specific terms are employed herein, they are used in a generic and descriptive sense only and not for purposes of limitation.REFERENCES M. Kim et al., Conformal quantum dot-SnCh layers as electron transporters for efficient perovskite solar cells. Science 375, 302-306 (2022). Y. Zhao et al., Inactive (Pbh^RbCl stabilizes perovskite films for efficient solar cells. Science 377 , 531-534 (2022). H. Min et al., Perovskite solar cells with atomically coherent interlayers on SnCh electrodes. Nature 598, 444-450 (2021). T. Wang etal., Transporting holes stably under iodide invasion in efficient perovskite solar cells. Science 377, 1227-1232 (2022). Y. Deng et al., Defect compensation in formamidinium-caesium perovskites for highly efficient solar mini-modules with improved photostability. Nat. Energy 6, 633-641 (2021). S. Chen et al., Stabilizing perovskite-substrate interfaces for high-performance perovskite modules. Science 373, 902-907 (2021). Y. Deng et al., Reduced Self-Doping of Perovskites Induced by Short Annealing for Efficient Solar Modules. Joule 4, 1949-1960 (2020). T. Bu et al., Lead halide-templated crystallization of methylamine-free perovskite for efficient photovoltaic modules. Science 372, 1327-1332 (2021). Q. Cao et al., Efficient and stable inverted perovskite solar cells with very high fill factors via incorporation of star-shaped polymer. Set. Adv. 7, eabg0633 (2021). Z. Li et al., Organometallic-functionalized interfaces for highly efficient inverted perovskite solar cells. Science 376, 416-420 (2022). X. Li et al., Constructing heterojunctions by surface sulfidation for efficient inverted perovskite solar cells. Science 375, 434-437 (2022). S. Bai et al., Planar perovskite solar cells with long-term stability using ionic liquid additives. Nature 571, 245-250 (2019). S. Tan et al., Stability -limiting heterointerfaces of perovskite photovol taics. Nature 605, 268-273 (2022). Q. Jiang et al., Surface reaction for efficient and stable inverted perovskite solar cells. Nature, (2022). X. Zuo et al., Passivating buried interface via self-assembled novel sulfonium salt toward stable and efficient perovskite solar cells. Chem. Eng. J. 431, 133209 (2022). G. Yang et al., Defect engineering in wide-bandgap perovskites for efficient perovskite- silicon tandem solar cells. Nat. Photonics 16, 588-594 (2022). Y. Yang etal., Dopant free mixture of Spiro-OMeTAD and PTAA with tunable wettability as hole transport layer enhancing performance of inverted CsPbI2Br perovskite solar cells. Org. Electron. 86, 105873 (2020). Brian L. Watson, N. Rolston, K. A. Bush, L. Taleghani, R. H. Dauskardt, Synthesis and use of a hyper-connecting cross-linking agent in the hole-transporting layer of perovskite solar cells. J. Mater. Chem. A 5, 19267-19279 (2017).S. Ye et al., A Breakthrough Efficiency of 19.9% Obtained in Inverted Perovskite Solar Cells by Using an Efficient Trap State Passivator Cu(thiourea)!. JACS 139, 7504-7512 (2017). J. Peng et al., Interface passivation using ultrathin polymer-fullerene films for high- efficiency perovskite solar cells with negligible hysteresis. Energy Environ. Sci. 10, 1792- 1800 (2017). S. Chen et al., Crystallization in one-step solution deposition of perovskite films: Upward or downward? Sci. Adv. 7, eabb2412 (2021). M. Wang, C. Fei, M. A. Uddin, J. Huang, Influence of Voids on the Thermal and Light Stability of Perovskite Solar Cells. Sci. Adv., (2022). S. Yang et al., Stabilizing halide perovskite surfaces for solar cell operation with wide- bandgap lead oxysalts. Science 365, 473-478 (2019). Z. Ni et al., Resolving spatial and energetic distributions of trap states in metal halide perovskite solar cells. Science 367 , 1352-1358 (2020). J. J. Chisolm, The use of chelating agents in the treatment of acute and chronic lead intoxication in childhood. J. Pediatr. 73, 1-38 (1968). V. C. A. Taylor et al., Investigating the Role of the Organic Cation in Formamidinium Lead Iodide Perovskite Using Ultrafast Spectroscopy. J. Phys. Chem. Lett. 9, 895-901 (2018). J. Chen, N.-G. Park, Causes and Solutions of Recombination in Perovskite Solar Cells. Adv. Mater. 31, 1803019 (2019). N. Li et al., Microscopic Degradation in Formamidinium-Cesium Lead Iodide Perovskite Solar Cells under Operational Stressors. Joule 4, 1743-1758 (2020). Y.-H. Lin etal., A piperidinium salt stabilizes efficient metal-halide perovskite solar cells. Science 369, 96-102 (2020). Y. Deng et al., Tailoring solvent coordination for high-speed, room -temperature blading of perovskite photovoltaic films. Sci. Adv. 5, eaax7537 (2019). C. Bi et al., Non-wetting surface-driven high-aspect-ratio crystalline grain growth for efficient hybrid perovskite solar cells. Nat. Commun. 6, 7747 (2015). C.-H. Kuan et al., How can a hydrophobic polymer PTAA serve as a hole- transport layer for an inverted tin perovskite solar cell? Chem. Eng. J. 450, 138037 (2022). Z. Ni et al., Evolution of defects during the degradation of metal halide perovskite solar cells under reverse bias and illumination. Nat. Energy 7, 65-73 (2022). T. Zhu, D. Zheng, M.-N. Rager, T. Pauporte, The Stabilization of Formamidinium Lead Tri-Iodide Perovskite through a Methylammonium-Based Additive for High-Efficiency Solar Cells. Solar RRL 4, 2000348 (2020). T. A. S. Doherty et al., Stabilized tilted-octahedra halide perovskites inhibit local formation of performance-limiting phases. Science 374, 1598-1605 (2021).D. F. O’Brien, M. A. Baldo, M. E. Thompson, S. R. Forrest, Improved energy transfer in electrophosphorescent devices. Appl. Phys. Lett. 74, 442-444 (1999). P. Penmans, V. Bulovic, S. R. Forrest, Efficient photon harvesting at high optical intensities in ultrathin organic double-heterostructure photovoltaic diodes. Appl. Phys. Lett. 76, 2650-2652 (2000). Q. Wang et al., Large fill-factor bilayer iodine perovskite solar cells fabricated by a low- temperature solution-process. Energy Environ. Set. 7, 2359-2365 (2014). R. Tomova, P. Petrova, R. Stoy cheva-Topal ova, Role of bathocuproine as hole-blocking and electron-transporting layer in organic light emitting devices. Phys. Status Solidi C 7, 992-995 (2010). J. Lee et al., Electron transport mechanism of bathocuproine exciton blocking layer in organic photovoltaics. Phys. Chem. Chem. Phys. 18, 5444-5452 (2016). H. Gao et al., Theoretical Characterization of a Typical Hole / Exciton-Blocking Material Bathocuproine and Its Analogues. J. Phys. Chem. A 112, 9097-9103 (2008). J. Peng et al., Nanoscale localized contacts for high fill factors in polymer-passivated perovskite solar cells. Science 371, 390-395 (2021). S.-H. Turren-Cruz, A. Hagfeldt, M. Saliba, Methylammonium-free, high-performance, and stable perovskite solar cells on a planar architecture. Science 362, 449-453 (2018). Q. Wang, Q. Dong, T. Li, A. Gruverman, J. Huang, Thin Insulating Tunneling Contacts for Efficient and Water-Resistant Perovskite Solar Cells. Adv. Mater. 28, 6734-6739 (2016). A. Becheri, M. Diirr, P. Lo Nostro, P. Baglioni, Synthesis and characterization of zinc oxide nanoparticles: application to textiles as UV-absorbers. J. Nanopart. Res. 10, 679-689 (2008). Y. Li et al., Non-fullerene acceptor organic photovoltaics with intrinsic operational lifetimes over 30 years. Nat. Commun. 12, 5419 (2021). Y. Lin et al. , Excess charge-carrier induced instability of hybrid perovskites. Nat. Commun. 9, 4981 (2018). X. Dai et al., Pathways to High Efficiency Perovskite Monolithic Solar Modules. PRX Energy 1, 013004 (2022).
Claims
WHAT IS CLAIMED IS:
1. A multilayer perovskite composite, comprising: i. a hole-transport layer comprising a hole transport material and lead chelating molecules (LCMs), and ii. a polycrystalline perovskite film disposed on top of the hole transport layer wherein the perovskite film comprises a composition of Formula (I):ABX3 (I) wherein A is a cation selected from the group consisting of methylammonium (MA), dimethylammonium (DMA), tetramethylammonium (TMA), formamidinium (FA), cesium (Cs), rubidium (Rb), potassium (K), sodium (NA), butylammonium (BAH), phenylethylammonium (PEA), phenylammonium (PHA), guanidinium (GU), and a combination thereof;B is at least one divalent metal; andX is at least one halide.
2. The multilayer perovskite composite of claim 1, wherein B is selected from the group consisting of lead, tin, cadmium, germanium, zinc, nickel, platinum, palladium, mercury, titanium and silicon, or a combination thereof.
3. The multilayer perovskite composite of claim 2, wherein B is lead or tin, or a combination thereof.
4. The multilayer perovskite composite of claim 3, wherein B is lead.
5. The multilayer perovskite composite of any one of claims 1-4, wherein A comprises a combination of two or more cations selected from the group consisting of methylammonium (MA), dimethylammonium (DMA), tetramethylammonium (TMA), formamidinium (FA), caesium (Cs), rubidium (Rb), potassium (K), sodium (Na), butylammonium (BAH), phenylethylammonium (PEA), phenylammotnium (PHA), and guanidinium (GU).
6. The multilayer perovskite composite of claim 5, wherein A is a combination of two or more cations selected from the group consisting of methylammonium, formamidinium, and cesium.
7. The multilayer perovskite composite of claim 6, wherein A is cesium and formamidinium, wherein the molar ratio of cesium to formamidinium is between 0.05:0.95 and 0.2:0.8.
8. The multilayer perovskite composite of claim 7, wherein A is cesium and formamidinium, wherein the molar ratio of cesium to formamidinium is about 0.08:0.92.
9. The multilayer perovskite composite of any one of claims 1-8, wherein X is selected from group consisting of I, Br, and a combination thereof.
10. The multilayer perovskite composite of claim 9, wherein X is I.
11. The multilayer perovskite composite of claim 1, wherein the perovskite film is selected from group consisting of cesium lead iodide (CsPbh), methylammonium lead iodide (MAPbh), formamidinium lead bromide (FAPbh), methylammonium lead bromide (MAPbBn), cesium formamidinium lead iodide (Cso.1FAo.9PH3), cesium formamidinium methylammonium lead iodide (CS0.05FA0.70MA0.25PH3), cesium formamidinium lead tin iodide (Cso.2FAo.8Pbo5Sno.5I3), cesium formamidinium lead iodide bromide (Cso 2FAo sPb(Io6Bro 4)3), and cesium methylammonium lead iodide bromide (Cso.iMAo.9Pb(Io.9Bro.i)3).
12. The multilayer perovskite composite of any one of claims 1-11, wherein the hole transport layer film comprises hole transport material selected from the group consisting of PTAA, TAA, PF8-TAA, PIF8-TAA, PTB7, PCDTBT, PDPPDBTE, pBBTa-BDTs, PPN, PFT, PTB7, P3HT, PEDOT, graphene oxide, and TSPT.
13. The multilayer perovskite composite of claim 12, wherein the hole transport material is PTAA.
14. The multilayer perovskite composite of any one of claims 1-13, wherein the lead chelating molecules are selected from the group consisting of bathocuproine, dimercaptosuccinic acid, L-Ascorbic acid, alpha lipoic acid, ethylenediaminetetraacetic acid, 2,3- dimercaptopropanesulfonic acid, thiamine tetrahydrofuryl disulfide, p-toluenesulfonic anhydride, and penicillamine, or synthetic derivatives thereof.
15. The multilayer perovskite composite of claim 14, wherein the lead chelating molecules are selected from the group consisting of bathocuproine, dimercaptosuccinic acid, L-Ascorbic acid, and p-toluenesulfonic anhydride, or synthetic derivates thereof.
16. The multilayer perovskite composite of claim 15, wherein the lead chelating molecules are bathocuproine or a synthetic derivative thereof.
17. The multilayer perovskite composite of claim 16, wherein the lead chelating molecules are a synthetic derivative of bathocuproine such as bathophenanthroline (BPhen) or 1,10- phenanthroline (OPhen).
18. The multilayer perovskite composite of claim 16, wherein the lead chelating molecules are bathocuproine.
19. The multilayer perovskite composite of any one of claims 14-18, wherein said lead chelating molecules are present in an amount from about 0.1 to about 90 wt. % of the hole transport layer.
20. The multilayer perovskite composite of claim 19, wherein said lead chelating molecules are present in an amount from about 1.5 to 15 wt. % of the hole transport layer.
21. The multilayer perovskite composite of claim 20, wherein said lead chelating molecules comprise about 2 wt. % of the hole transport layer.
22. A method of preparing the multilayer perovskite composite of any one of claims 1 -21 , comprising: i. disposing a precursor solution comprising the hole transport layer material, the lead chelating molecules, and a solvent onto a substrate using a fast-coating process to form a hole transport film; and ii. disposing a precursor perovskite solution comprising the perovskite material of Formula I and a solvent onto the hole transport film using a fast-coating process to form a perovskite film disposed on the hole transport film.
23. The method of claim 22, wherein the fast-coating process is selected from the group consisting of spin coating, blade coating, slot die coating, shear coating, gravure coating, brush coating, syringe coating, and screen printing.
24. The method of claim 23, wherein the fast-coating process is blade coating.
25. A solar cell comprising: one or more transparent conductive oxide layers; one or more conductive electrode layers; one or more electron transport layers; and an active layer comprising the multilayer perovskite composite of any one of claims 1-21.
26. The solar cell of claim 25, wherein the solar cell comprises: a first transparent conductive oxide layer; an active layer comprising the multilayer perovskite composite of any one of claims 1-21; an electron transport layer; an optional buffer layer; and a conductive electrode layer.
27. The solar cell of claim 26, wherein:the hole transport layer of the multilayer perovskite composite is disposed on the first transparent conductive oxide layer; the perovskite film of the multilayer perovskite composite is disposed on the hole transport layer of the multilayer perovskite composite; the electron transport layer is disposed on the perovskite film; the buffer layer, if present, is disposed on the electron transport layer; and the conductive electrode layer is disposed on the buffer layer.
28. The solar cell of claim 27, wherein: the transparent conductive oxide layer comprises ITO; the hole transport layer of the multilayer perovskite composite comprises PTAA and bathocuproine as lead chelating molecules; the electron transport layer comprises Ceo; and the conductive electrode layer comprises copper.
29. The solar cell of any one of claims 25-28, wherein said solar cell exhibits a Power Conversion Efficiency (PCE) between about 18 to about 26%.
30. The solar cell of claim 29, wherein said solar cell exhibits a PCE of about 22%.
31. The solar cell of any one of claims 25-30, wherein said solar cell is stable.
32. The solar cell of claim 31, wherein said solar cell retains at least 90% of its PCE from about 2000 to about 7000 hours of continuous 1 sun illumination.
33. The solar cell of claim 32, wherein said solar cell retains at least 90% of its PCE for about 3000 hours of continuous 1 sun illumination.
34. The solar cell of claim 32, wherein said solar cell retains at least 95% of its PCE for about 2000 hours of continuous 1 sun illumination.
Citation Information
Patent Citations
Environment-friendly lead-based perovskite composite material, preparation method and solar cell
CN113462111A
High quality, ultra-thin organic-inorganic hybrid perovskite
US9966195B1
Perovskite compositions comprising mixed solvent systems
WO2019195194A1