Preparation and strengthening method for polycrystalline ceramic material

By combining the smelting and cooling method of raw materials such as SiO2, Al2O3, K2CO3, CaF2 and fiber materials, polycrystalline ceramic materials are prepared, which solves the problem of insufficient mechanical and thermodynamic performance of ceramic materials in bearings and other fields, and realizes high-performance ceramic materials Preparation, suitable for high temperature and high strength applications.

WO2024243738A1PCT designated stage expired Publication Date: 2024-12-05WANG JINGRAN +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/096636
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Ceramic materials on the market have problems with poor mechanical and thermodynamic performance in the fields of bearings, and it is difficult to meet the needs of high temperature, high hardness, impact resistance and oxidation resistance.

Method used

The raw materials such as SiO2, Al2O3, K2CO3, CaF2 and NaOH are mixed and sintered and cooled, combined with fiber materials such as carbon fiber and graphite fiber to prepare polycrystalline ceramic materials, and obtain high mechanical and thermodynamic properties through the phase change process of the sintered state. Ceramic material.

Benefits of technology

The obtained polycrystalline ceramic materials are high temperature resistance, high hardness, impact resistance, compression resistance, crack resistance, oxidation resistance and high self-moisture properties. They are suitable for the production of ceramic bearings, turbofan blades and air compressed blades, and their performance is better than traditional ceramic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention relates to the technical field of functional materials, and provides a preparation and strengthening method for a polycrystalline ceramic material. A polycrystalline ceramic material comprises the following raw materials: SiO2, Al2O3, K2CO3, CaF2, and NaOH. The preparation method comprises: mixing the raw materials, melting, and cooling. The polycrystalline ceramic material of the present invention has the characteristics of high temperature resistance, high hardness, high toughness, high impact resistance, high pressure resistance, high crack resistance, high red hardness, high oxidation resistance, and high self-lubricity. According to the preparation method, the polycrystalline ceramic material can be obtained, and the polycrystalline ceramic material can be used for manufacturing ceramic bearings, turbofan blades, air compressor blades and the like.
Need to check novelty before this filing date? Find Prior Art

Description

A preparation and strengthening method of polycrystalline ceramic material Technical Field

[0001] The present invention relates to the technical field of functional materials, and in particular to a method for preparing and strengthening a polycrystalline ceramic material. Background Art

[0002] As a kind of multifunctional material in the future, ceramic materials will be widely used and attract more and more attention from researchers.

[0003] However, the ceramic materials used on the market have more or less defects, and there are still problems with poor mechanical and thermodynamic properties when used in fields such as bearings.

[0004] Summary of the Invention

[0005] The object of the present invention is to provide a method for preparing and strengthening a polycrystalline ceramic material, which can be used to obtain a polycrystalline ceramic material that can be used to make ceramic bearings, turbofan blades, and air compressor blades, etc., and has the characteristics of high temperature resistance, high hardness, high toughness, high impact resistance, high pressure resistance, high crack resistance, high red hardness, high oxidation resistance and high self-lubricating property.

[0006] The present invention solves the technical problem by adopting the following technical solutions.

[0007] The present invention provides a preparation and strengthening method of a polycrystalline ceramic material, which includes the following raw materials: SiO2, Al2O3, K2CO3, CaF2 and NaOH; the preparation method includes the following steps: mixing the raw materials, sintering, and cooling to room temperature.

[0008] The present invention has at least the following beneficial effects:

[0009] In the present invention, by combining various raw materials and gradually cooling them from a molten state, a negligible shrinkage ratio is achieved during the phase transition from liquid to solid, thereby producing a polycrystalline ceramic material with enhanced mechanical and thermodynamic properties. The resulting polycrystalline ceramic material exhibits high temperature resistance, high hardness, high toughness, high impact resistance, high compressive strength, high crack resistance, high red hardness, high oxidation resistance, and high self-lubricating properties. During the sintering process, calcium carbonate and carbon fibers, graphite fibers, graphene, zirconia fibers, or asbestos can also be varied to produce polycrystalline ceramic materials with varying colors, including opaque, transparent, or translucent. Polycrystalline ceramic materials can be used to manufacture ceramic bearings, turbofan blades, and air compressor blades, facilitating widespread utilization. DETAILED DESCRIPTION

[0010] To make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, all are conventional products that can be purchased commercially.

[0011] It should be noted that, in the absence of conflicts, the embodiments and features of the embodiments of the present invention can be combined with each other according to the requirements. The present invention will be described in detail below with reference to specific embodiments.

[0012] A method for preparing and strengthening a polycrystalline ceramic material includes the following raw materials: SiO2, Al2O3, K2CO3, CaF2, and NaOH. The preparation method comprises the following steps: mixing the raw materials, sintering at a temperature of 1300-1700°C, and cooling to room temperature, wherein the room temperature is 22±3°C.

[0013] Specifically, the polycrystalline ceramic material raw materials also include one or more of MgF2, CaO, Na2CO3, SiC, B2O3, Na2O, ZrO2, H3BO3, and NaNO3. These materials are used to produce ceramic materials with diverse mechanical and thermodynamic properties, thereby expanding the application range of the ceramic materials and enabling their application in various fields.

[0014] In detail, the polycrystalline ceramic material raw material further includes one or more of carbon fiber, graphite fiber, graphene, zirconia fiber and asbestos.

[0015] Carbon fiber, graphite fiber, graphene, zirconia fiber or asbestos used in the production of ceramic materials can greatly improve the flexural and thermal shock resistance, improve the brittleness of ceramics, and make ceramic materials have high strength, wear resistance, high temperature resistance and other characteristics, which helps to expand the application range of ceramic materials.

[0016] Specifically, the raw materials of the polycrystalline ceramic material also include stainless steel. Stainless steel is used to make ceramic materials because it has a negligible shrinkage ratio, and adding stainless steel wire, strip stainless steel or sheet stainless steel will not cause peeling or cracking.

[0017] Based on the requirements of polycrystalline ceramic materials, such as temperature resistance and hardness, all of the above compounds can be appropriately combined. Alternatively, some of these compounds can be combined and proportioned based on specific requirements. The proportions are measured by weight. Polycrystalline ceramic materials with varying mechanical and thermodynamic properties are obtained after sintering at a certain temperature and cooling. The appropriate compounds can be used as sintering binders for both soft and hard magnetic materials.

[0018] The polycrystalline ceramic material prepared by the above method exhibits high temperature resistance, high hardness, high toughness, high impact resistance, high compressive strength, high crack resistance, high red hardness, high oxidation resistance, and high self-lubricating properties. Under appropriate proportions, the phase transition from the molten state to the solidified state exhibits negligible shrinkage. Furthermore, high-strength synthetic fiber materials such as carbon fiber, graphene, and zirconia fiber, or metals and their alloys, can be added. These materials have excellent affinity with most metals and alloys, and the addition of these materials can improve the flexural resistance of the polycrystalline ceramic. The resulting polycrystalline ceramic material can be used to replace metal supports in components such as ship blades, gas turbine blades, fan and air compressor blades in front of aircraft engine combustion chambers, turbofan generator casings, and various metal pipelines. Furthermore, due to its excellent mechanical and thermodynamic properties, the polycrystalline ceramic material can also be used in internal combustion engine casings, cylinder blocks, pistons, and other applications, and exhibits excellent cold and hot formability.

[0019] The polycrystalline ceramic material proposed in this invention, due to its inherent advantages, has significantly superior weighted average mechanical properties when cured with carbon fibers compared to epoxy-cured carbon fibers. Because the polycrystalline ceramic material contains no organic matter, it has a higher pyrolysis temperature and more stable properties.

[0020] The features and performance of the present invention are further described in detail below with reference to the embodiments.

[0021] Example 1

[0022] A method for preparing and strengthening a polycrystalline ceramic material comprises the following steps:

[0023] Raw materials: 63kg SiO2, 6kg Al2O3, 10kg K2CO3, 8kg CaF2, 4kg B2O3, 2kg NaNO3, 6kg NaOH, 6kg CaF2, 15kg ZrO2, 5kg H3BO3;

[0024] The raw materials are mixed, sintered at a temperature of 1500°C, and cooled to room temperature to obtain a polycrystalline ceramic material.

[0025] The polycrystalline ceramic material obtained in this embodiment was tested, and the results were as follows: Mohs hardness 7.6, compressive strength 900 MPa, impact toughness 5.7 Kj / cm 2 , flexural strength 150MPa.

[0026] The polycrystalline ceramic material obtained in this embodiment can withstand rapid cooling from >1000°C, either naturally or by forced air cooling, to room temperature without cracking. Bearings made from the polycrystalline ceramic material obtained in this embodiment exhibit self-lubricating properties at temperatures ≤350°C and can operate normally for ≥10 hours at temperatures ≤500°C.

[0027] Example 2

[0028] A method for preparing and strengthening a polycrystalline ceramic material comprises the following steps:

[0029] Raw materials: 65 kg SiO2, 18 kg Al2O3, 15 kg K2CO3, 15 kg CaF2, 5 kg NaOH and 15 kg ZrO2;

[0030] The raw materials are mixed, sintered at a temperature of 1700°C, and cooled to room temperature to obtain a polycrystalline ceramic material.

[0031] The polycrystalline ceramic material obtained in this embodiment was tested, and the results were as follows: Mohs hardness 7.4, compressive strength 880 MPa, impact toughness 5.6 Kj / cm 2 , flexural strength 130MPa.

[0032] The polycrystalline ceramic material obtained in this embodiment can withstand rapid cooling from >1000°C, either naturally or by forced air cooling, to room temperature without cracking. Bearings made from the polycrystalline ceramic material obtained in this embodiment exhibit self-lubricating properties at temperatures ≤350°C and can operate normally for ≥10 hours at temperatures ≤500°C.

[0033] Example 3

[0034] A method for preparing and strengthening a polycrystalline ceramic material comprises the following steps:

[0035] Raw materials: 56kg SiO2, 25kg Al2O3, 12kg K2CO3, 13kg CaF2, 5kg NaOH, 5kg MgF2, 5kg Na2CO3, 7kg SiC, 12kg B2O3, 10kg ZrO2, 12kg H3BO3, 35kg zirconia fiber and 35kg carbon fiber;

[0036] The raw materials are mixed, sintered at a sintering temperature of 1350° C., and cooled to room temperature to obtain a polycrystalline ceramic material.

[0037] The polycrystalline ceramic material obtained in this embodiment was tested, and the results were as follows: Mohs hardness 7.8, compressive strength 1200 MPa, impact toughness 6.9 Kj / cm 2 , flexural strength 530MPa.

[0038] The polycrystalline ceramic material obtained in this embodiment can withstand rapid cooling from >1000°C, either naturally or by forced air cooling, to room temperature without cracking. Bearings made from the polycrystalline ceramic material obtained in this embodiment exhibit self-lubricating properties at temperatures ≤350°C and can operate normally for ≥10 hours at temperatures ≤500°C.

[0039] In summary, the preparation and strengthening method of the polycrystalline ceramic material of the embodiment of the present invention, through the combination of various raw materials, gradually cooling in the molten state, and having a negligible shrinkage ratio during the phase change from liquid to solid, can obtain a polycrystalline ceramic material with stronger mechanical and thermodynamic properties, so that the obtained polycrystalline ceramic material has the characteristics of high temperature resistance, high hardness, high toughness, high impact resistance, high pressure resistance, high crack resistance, high red hardness, high oxidation resistance and high self-lubricating property. Calcium carbonate can also be changed during the sintering process to obtain transparent or translucent polycrystalline ceramic materials of different colors. Polycrystalline ceramic materials can be used to make ceramic bearings, turbofan blades and air compressor blades, which are convenient for promotion and utilization.

[0040] The embodiments described above are some, but not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention as claimed, but rather merely represents selected embodiments of the present invention. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without inventive effort are also within the scope of protection of the present invention.

Claims

1. A method for preparing and strengthening a polycrystalline ceramic material, characterized in that: The raw materials include SiO2, Al2O3, K2CO3, CaF2 and NaOH; The preparation method comprises the following steps: mixing raw materials, melting, and cooling to room temperature.

2. The method for preparing and strengthening a polycrystalline ceramic material according to claim 1, characterized in that: The raw materials also include one or more of MgF2, CaO, Na2CO3, SiC, B2O3, Na2O, ZrO3, H3BO3 and NaNO3.

3. The method for preparing and strengthening a polycrystalline ceramic material according to claim 2, characterized in that: The raw materials also include one or more of carbon fiber, graphite fiber, graphene, zirconium oxide fiber and asbestos.

4. The method for preparing and strengthening a polycrystalline ceramic material according to claim 3, characterized in that: The raw material also includes stainless steel.

5. The method for preparing and strengthening a polycrystalline ceramic material according to claim 1, characterized in that: The sintering temperature is 1300-1700℃.

Citation Information

Patent Citations

  • Kitchen and toilet table surface glass-ceramic and ceramic composite board formula

    CN105621890A

  • Nano-scale microcrystalline glass used in dental department and production method thereof

    CN106966600A

  • High-performance melted casted anti-abrasion brick and melting and casting method thereof

    CN110304910A

  • Anterior tooth facing ceramic material and preparation method thereof

    CN114538780A

  • Low cost molten cast alumina-zirconium dioxide-silicon dioxide product and its appliance

    CN1330053A